Self-leveling hydraulic composition and mortar thereof
A self-smoothing hydraulic composition with specific thickeners and additives addresses fluidity and surface finish issues, ensuring smoothness and reducing cracking in large floor areas.
Patent Information
- Application Number
- JP2023057280
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing self-leveling materials face issues with fluidity and surface finish, leading to material separation and cracking during drying, especially in large floor areas, necessitating improved workability and aesthetics.
A self-smoothing hydraulic composition comprising cement, fine aggregate, and multiple types of thickeners with specific viscosities, along with other additives like water reducing agents and antifoaming agents, to achieve optimal fluidity and surface finish.
The composition ensures good fluidity and excellent surface finish upon curing, reducing material separation and cracking, thus enhancing work efficiency and shortening construction time.
Smart Images

Figure 2024145048000001 
Figure 2024145048000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a self-smoothing hydraulic composition and a mortar thereof. [Background technology]
[0002] In recent years, there has been a shortage of plasterers and an increasing demand for structures with large floor areas, such as logistics warehouses, and there is a demand for shortening construction time and improving productivity to open the floors quickly after finishing. There is a method of pouring a cement-based self-leveling material, which uses cement as a binder, into the base concrete floor as a finishing material to ensure the levelness of the floor surface. When using a self-leveling material, the easiest way to shorten construction time and improve workability is to increase the amount of mixing water to improve fluidity. However, on the other hand, as the amount of water increases, problems such as material separation and cracks during the drying process become more likely to occur. By adding a dispersant, etc., it is possible to prevent the cement particles from agglomerating and improve fluidity without increasing the amount of water.
[0003] For example, Patent Document 1 discloses a self-smoothing mortar using a mixed water-reducing agent of a polyether-based water-reducing agent and a polycarboxylic acid-based water-reducing agent. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-123026 A Summary of the Invention [Problem to be solved by the invention]
[0005] Self-leveling materials intended for floor finishing need to have sufficient fluidity to ensure smoothness, but also enough viscosity to prevent the material from separating, and so moderate fluidity that balances these two is required. In addition, from the viewpoint of aesthetics, it is also important that the surface finish of the self-leveling material is good when it hardens.
[0006] Therefore, an object of the present invention is to provide a self-smoothing hydraulic composition having good fluidity capable of exerting smoothness and having an excellent surface finish when hardened, and a mortar made therefrom. [Means for solving the problem]
[0007] As a result of intensive research into the above-mentioned problems, the present inventors have found that a self-smoothing hydraulic composition and a mortar therewith that exhibit excellent fluidity and surface finish can be obtained by using two or more types of thickeners, including a thickener having a specific viscosity.
[0008] That is, the present invention is as follows. [1] A self-smoothing hydraulic composition comprising cement, fine aggregate, a thickening agent, an expansive agent and a water-reducing agent, wherein the thickening agent is two or more types including at least one thickening agent having a viscosity of 3000-6000 mPa s in a 2% by mass aqueous solution at 20°C, and the content of the thickening agent is 0.06-1 part by mass in terms of solid content per 100 parts by mass of cement. [2] The self-smoothing hydraulic composition according to [1], further comprising an antifoaming agent. [3] A self-smoothing mortar comprising the self-smoothing hydraulic composition according to [1] or [2] and water, the water content being 55 to 105 parts by mass per 100 parts by mass of cement. [4] A self-smoothing mortar according to [3], having a flow time of 10 to 40 seconds using a J10 funnel as measured in accordance with the Japan Society of Civil Engineers standard "Test method for fluidity of PC grout (draft)" JSCE-F531:2018. Effect of the Invention
[0009] According to the present invention, it is possible to provide a self-smoothing hydraulic composition having good fluidity capable of exerting smoothness and having an excellent surface finish when hardened, and a mortar made from the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, one embodiment of the present invention will be described in detail.
[0011] The self-smoothing hydraulic composition of the present embodiment contains cement, fine aggregate, a thickening agent, an expansive agent, and a water-reducing agent.
[0012] Various types of cement can be used, for example, various types of Portland cement such as ordinary, early strength, ultra-early strength, low heat and moderate heat, ecocement, ultra-rapid hardening cement, fly ash cement, etc. One type of cement may be used alone, or two or more types may be used in combination.
[0013] Examples of fine aggregate include river sand, silica sand, crushed sand, kansui stone, limestone sand, and slag aggregate. Of these, it is preferable to use aggregate such as silica sand or limestone adjusted to a grain size that does not contain fine powder or coarse aggregate. One type of fine aggregate may be used alone, or two or more types may be used in combination. It is preferable to use fine aggregate with a grain size of less than 1.2 mm (passing a 1.2 mm sieve), which is commonly used.
[0014] The particle size of the fine aggregate is not particularly limited, and can be adjusted within the required particle size range of the fine aggregate. The particle size of the fine aggregate can be considered from the coarse particle ratio defined by JIS A 1102:2014 "Sieving test method for aggregates". From the viewpoint of easily obtaining better fluidity and easily suppressing bleeding, the coarse particle ratio of the fine aggregate is preferably 1 to 3, more preferably 1.1 to 2.5, and even more preferably 1.2 to 2.
[0015] The content of the fine aggregate is preferably 100 to 300 parts by mass, more preferably 120 to 250 parts by mass, and even more preferably 140 to 200 parts by mass, relative to 100 parts by mass of cement. If the amount of the fine aggregate added is within the above range, it is easy to ensure sufficient fluidity and compressive strength as a self-leveling material.
[0016] The thickener according to the present embodiment is two or more types including at least one type of thickener having a viscosity of 3000 to 6000 mPa·s in a 2% by mass aqueous solution at 20°C. If the viscosity of the thickener is outside the above range or if only one type of thickener is used, the fluidity indicated by the spread and flow time of the mortar is insufficient, and the surface finish is also not excellent. From the viewpoint of easily obtaining a suitable fluidity and further improving the surface finish, the viscosity of the thickener in a 2% by mass aqueous solution at 20°C is preferably 3500 to 5500 mPa·s, more preferably 4000 to 5000 mPa·s. In this specification, the viscosity of the thickener is a value measured by using a rotational viscometer in an environment of 20°C for an aqueous solution of the thickener prepared to have a concentration of 2% by mass. A commonly used rotational viscometer can be used, for example, an inner cylinder rotational viscometer or an outer cylinder rotational viscometer can be used.
[0017] The type of thickener is not particularly limited, and examples thereof include cellulose-based thickeners, acrylic-based thickeners, guar gum-based thickeners, and starch-based thickeners. As the thickener, cellulose-based thickeners are preferred. As the cellulose-based thickener, for example, methylcellulose-based thickeners such as carboxymethylcellulose, methylcellulose, hydroxyethylmethylcellulose, and hydroxypropylmethylcellulose, hydroxyethylcellulose, and hydroxypropylcellulose are included. As the acrylic thickener, an acrylamide-based thickener is included. As the guar gum-based thickener, a hydroxypropyl guar gum-based thickener is included. As the starch-based thickener, a hydroxypropyl starch ether-based thickener is included. As the thickener, it is preferable to combine different types of thickeners from the viewpoint of easily obtaining a fluidity suitable for ensuring smoothness and further improving the surface finish, and it is more preferable to combine multiple types of thickeners having a viscosity of 3000 mPa·s or more in a 2% by mass aqueous solution at 20°C.
[0018] The content of the thickener is 0.06 to 1 part by mass in terms of solid content relative to 100 parts by mass of cement. If the content of the thickener is outside the above range, the fluidity of the mortar is not stable, and the surface finish upon hardening is not excellent. From the viewpoint of easily obtaining a fluidity suitable for ensuring smoothness, the content of the thickener is preferably 0.08 to 0.8 parts by mass, more preferably 0.1 to 0.6 parts by mass in terms of solid content relative to 100 parts by mass of cement.
[0019] The water reducing agent includes a high-performance water reducing agent, a high-performance AE water reducing agent, an AE water reducing agent, and a superplasticizer. Examples of such water reducing agents include those specified in JIS A 6204:2011 "Chemical admixtures for concrete". Examples of the water reducing agent include polycarboxylic acid water reducing agents, naphthalene sulfonic acid water reducing agents, lignin sulfonic acid water reducing agents, and melamine water reducing agents. Among these, polycarboxylic acid water reducing agents are preferred. The water reducing agents may be used alone or in combination of two or more types.
[0020] The content of the water reducing agent is preferably 0.1 to 5 parts by mass, more preferably 0.3 to 3 parts by mass, and even more preferably 0.4 to 1.5 parts by mass, in terms of solid content, relative to 100 parts by mass of cement. If the content of the water reducing agent is within the above range, better fluidity is likely to be obtained when the mortar is made.
[0021] The self-smoothing hydraulic composition of the present embodiment may contain an expansive material. The expansive material may be any JIS-compliant expansive material (JIS A 6202:2008) that is generally used as an expansive material for concrete. Examples of the expansive material include expansive materials containing free quicklime as the main component (quicklime-based expansive materials), expansive materials containing Irwin as the main component (ettringite-based expansive materials), and composite expansive materials containing free quicklime and ettringite-forming substances. One type of expansive material may be used alone, or two or more types may be used in combination. The expansive material may have a Blaine specific surface area of 2000 to 6000 cm. 2 It is preferable to use one having a molecular weight of 1 / g.
[0022] The content of the expansive agent is preferably 0.1 to 15 parts by mass, more preferably 1 to 10 parts by mass, and even more preferably 2 to 8 parts by mass, relative to 100 parts by mass of cement. If the content of the expansive agent is within the above range, the compressive strength tends to be excellent and cracks tend to be reduced.
[0023] The self-smoothing hydraulic composition of the present embodiment may contain fibers. The fibers are not limited as long as they improve crack resistance and bending strength. Examples of the fibers include organic fibers such as vinylon fibers, polypropylene fibers, and nylon fibers; steel fibers; and inorganic fibers such as glass fibers. From the viewpoint of better dispersibility, the fibers are preferably organic fibers, and more preferably polyester fibers. The fibers may be used alone or in combination of two or more types.
[0024] The length of the fibers is preferably 1 to 10 mm, more preferably 1.2 to 8 mm, and most preferably 1.5 to 5 mm. If the length of the fibers is within the above range, it is easy to suppress cracks during hardening while ensuring fluidity.
[0025] The content of the fibers is preferably 0.01 to 3 parts by mass, more preferably 0.05 to 1 part by mass, and even more preferably 0.1 to 0.5 parts by mass, relative to 100 parts by mass of cement. If the content of the fibers is within the above range, it is easy to suppress cracks during hardening while ensuring fluidity.
[0026] The self-smoothing hydraulic composition of the present embodiment may contain an antifoaming agent. The antifoaming agent is not particularly limited as long as it is an antifoaming agent used in general concrete, and examples thereof include mineral oil-based antifoaming agents, ester-based antifoaming agents, amine-based antifoaming agents, amide-based antifoaming agents, polyether-based antifoaming agents, and silicone-based antifoaming agents.
[0027] The amount of the defoaming agent added is preferably 0.01 to 3 parts by mass, more preferably 0.03 to 1 part by mass, and even more preferably 0.05 to 0.5 parts by mass, relative to 100 parts by mass of cement. If the amount of the defoaming agent added is within the above range, it is easy to exert an effect on the defoaming of the mixed air, and the surface finish when hardened is also more excellent.
[0028] The self-smoothing hydraulic composition of the present embodiment may contain various admixtures (materials) within the range that does not impair the effects of the present invention. Examples of the admixtures (materials) include waterproofing agents, rust inhibitors, shrinkage reducing agents, water retention agents, pigments, water repellents, and efflorescence inhibitors.
[0029] The method for producing the self-smoothing hydraulic composition of the present embodiment can be carried out by mixing the above-mentioned components with a commonly used kneading tool, which is not particularly limited. Examples of the kneading tool include a grout mixer, a Hobart mixer, a hand mixer, a tilting mixer, and a twin-shaft mixer.
[0030] The self-smoothing hydraulic composition of the present embodiment can be prepared as a self-smoothing mortar by mixing with water, and the water content may be appropriately adjusted depending on the application. The water content is preferably 55 to 105 parts by mass, more preferably 65 to 95 parts by mass, and even more preferably 70 to 90 parts by mass, relative to 100 parts by mass of the cement component. If the water content is within the above range, it is easy to ensure fluidity and easy to suppress the occurrence of material separation and the decrease in strength development.
[0031] The method for producing the self-smoothing mortar of the present embodiment can use the same kneading equipment as that used for ordinary self-smoothing hydraulic compositions, and is not particularly limited. Examples of the kneading equipment include a grout mixer, a Hobart mixer, a hand mixer, a tilting mixer, and a twin-shaft mixer.
[0032] The self-smoothing mortar has a flow value of preferably 230 to 290 mm, more preferably 240 to 280 mm, and even more preferably 250 to 275 mm, as specified in the Architectural Institute of Japan standard "Quality Standard for Self-Leveling Materials" JASS 15M-103:2019. If the flow value of the self-smoothing mortar is within the above range, there is a tendency that smoothness can be ensured while further suppressing material separation.
[0033] The self-smoothing mortar preferably has a flow time of 10 to 40 seconds, more preferably 15 to 38 seconds, and even more preferably 20 to 36 seconds, in a J10 funnel measured in accordance with the Japan Society of Civil Engineers standard "PC Grout Fluidity Test Method (Draft)" JSCE-F531:2018. If the flow time of the self-smoothing mortar is within the above range, there is a tendency that material separation can be further suppressed while smoothness can be ensured.
[0034] The self-smoothing hydraulic composition and mortar thereof of the present embodiment have good fluidity to provide smoothness and provide an excellent surface finish when hardened, so that by pouring the composition onto a floor surface, the smoothness of the floor surface can be ensured, and work efficiency can be improved and construction time can be shortened. Therefore, the self-smoothing hydraulic composition and mortar thereof of the present embodiment can be suitably used for structures with large floor areas. EXAMPLES
[0035] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. All tests were carried out at 20°C.
[0036] [material] Cement: Ordinary Portland cement Expansion material: quicklime-based expansion material Fine aggregate: silica sand, particle size adjusted product (particle size 0.01mm~0.4mm, coarse grain ratio 1.37) Thickener: Thickener A: Hydroxypropyl methylcellulose-based thickener (2% by weight aqueous solution viscosity at 20°C: 4000 mPa s) Thickener B: Hydroxyethyl methylcellulose-based thickener (2% by weight aqueous solution viscosity at 20°C: 4500 mPa s) Thickener C: Hydroxypropyl guar gum thickener (2% by weight aqueous solution viscosity at 20°C: 8000 mPa s) Thickener D: Acrylamide-based thickener (2% by weight aqueous solution at 20°C: viscosity 10,000 mPa s) Thickener E: Hydroxypropyl starch ether thickener (2% by weight aqueous solution viscosity at 20°C: 60 mPa s) Fiber: Polyester fiber, fiber length 2mm · Defoamer: Silicone-based defoamer Water reducing agent: Polycarboxylic acid water reducing agent
[0037] [Preparation of Self-Leveling Composition] The mixture was designed with 100 parts by mass of cement, cement, expansive agent, fine aggregate, thickener, fiber and antifoaming agent in the proportions shown in Table 1. All the mixtures are calculated on a solids basis.
[0038] [Table 1]
[0039] [Preparation of self-smoothing mortar] The self-smoothing mortar was prepared by adding the self-smoothing composition and water to a cylindrical container and kneading for 90 seconds with a hand mixer. Water was added in a ratio of 72 parts by mass to 100 parts by mass of cement.
[0040] [Evaluation method] Fluidity (flow test, flow down test) The flow value was measured in accordance with JASS-15M-103:2019 (quality standard for self-leveling materials) of the Architectural Institute of Japan. The flow time is based on the Japan Society of Civil Engineers standard "PC Grout Fluidity Test Method (Draft)" JSCE-F531:2018. 10 The measurements were made using a funnel tester. The measurement was carried out 0 hours after mixing the self-smoothing mortar. · Surface finish after curing The self-smoothing mortar prepared in an environment of 20°C and 80% humidity was poured into a plastic container with inner dimensions of 13.5 cm length x 18.5 cm width x 2.5 cm height to a thickness of 1 cm. One day after molding, the surface of the hardened self-smoothing mortar was visually inspected and evaluated as follows. "Good": No cracks or brittle layers due to material separation are observed, and the surface is smooth. "△": Smoothness is lost due to cracks or unevenness "X": Cracks have occurred, and at the same time, unevenness has appeared and smoothness cannot be confirmed.
[0041] [Table 2]
[0042] The self-smoothing mortars of the Examples had flow values and flow times within appropriate ranges, and showed adequate fluidity without excessive spreading, which is suitable for demonstrating self-smoothing properties. Furthermore, the self-smoothing mortars of the Examples did not show any material separation, and the surface finish was good even after hardening. On the other hand, the self-smoothing mortars of the Comparative Examples sometimes had too high or too low fluidity, and the surface finish after hardening was not excellent.
Claims
1. Contains cement, fine aggregate, thickener, expansive material and water reducer. The thickener is two or more types including at least one thickener having a viscosity of 3000 to 6000 mPa s in a 2% by mass aqueous solution at 20°C, The self-smoothing hydraulic composition has a thickening agent content of 0.06 to 1 part by mass in terms of solid content per 100 parts by mass of the cement.
2. The self-leveling hydraulic composition of claim 1 further comprising an antifoaming agent.
3. A self-smoothing hydraulic composition according to claim 1 or 2, and water, The self-smoothing mortar has a water content of 55 to 105 parts by mass per 100 parts by mass of the cement.
4. The self-smoothing mortar according to claim 3, wherein the flow time of a J10 funnel measured in accordance with the Japan Society of Civil Engineers standard "PC Grout Fluidity Test Method (Draft)" JSCE-F531:2018 is 10 to 40 seconds.
Citation Information
Patent Citations
Self-leveling mortar
JP2018123026A