Method for producing microfibrous cellulose

The method of chemically modifying cellulose fibers with ionic groups, followed by dehydration, washing, and defibration using a sine pump, addresses quality issues in large-scale fine fibrous cellulose production, maintaining consistent product quality and viscosity.

JP2024145179AActive Publication Date: 2024-10-15OJI HLDG CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023057435
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing methods for producing fine fibrous cellulose on a large scale often result in unexpected quality changes, such as chemically modified cellulose or changes in viscosity, which are not adequately addressed by prior technologies.

Method used

A method involving chemical modification of cellulose fibers with ionic groups, followed by a dehydration/washing step, concentration adjustment, and defibration using a mechanical shearing force, utilizing a sine pump for transportation to maintain quality.

Benefits of technology

The method effectively suppresses quality changes during large-scale production of fine fibrous cellulose, ensuring consistent product quality and viscosity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145179000003
    Figure 2024145179000003
  • Figure 2024145179000004
    Figure 2024145179000004
  • Figure 2024145179000001
    Figure 2024145179000001
Patent Text Reader

Abstract

To provide a method for producing microfibrous cellulose in which quality changes are suppressed.SOLUTION: A method for producing microfibrous cellulose includes: a reaction step of performing chemical modification to cellulose fiber to obtain chemically modified cellulose; a dehydrating / cleaning step of performing dehydrating / cleaning of dispersion liquid of the chemically modified cellulose; an adjustment step of adjusting the concentration of the dispersion liquid of the chemically modified cellulose; and a fibrillation step of adding mechanical shearing force to the dispersion liquid of the chemically modified cellulose to fibrillate the liquid, where a sine pump is used for transfer in at least any step of the dispersion liquid of the chemically modified cellulose.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing fine fibrous cellulose. [Background technology]

[0002] Fine fibrous cellulose obtained by defibrating cellulose fibers to a fiber width of 1000 nm or less has excellent strength, elasticity, thermal stability, etc., and is used industrially as a filler for compounding resins and rubbers. In addition, aqueous dispersions of fine fibrous cellulose are used as viscosity adjusters, stabilizers, etc. Fine fibrous cellulose can be obtained by defibrating pulp fibers through a mechanical treatment. In this case, it is said that the energy required for the mechanical treatment can be efficiently reduced by defibrating the pulp fibers after introducing ionic groups into them (see Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-1728 A [Patent Document 2] JP 2010-235679 A Summary of the Invention [Problem to be solved by the invention]

[0004] When various methods for producing fine fibrous cellulose, including the methods described in Patent Documents 1 and 2, are scaled up, unexpected changes in quality, such as chemically modified cellulose or changes in the viscosity of the fine fibrous cellulose, may occur. Therefore, an object of the present invention is to provide a method for producing fine fibrous cellulose in which changes in quality are suppressed. [Means for solving the problem]

[0005] The present invention provides the following [1] to [5]. [1] A method for producing fine fibrous cellulose comprising a reaction step of chemically modifying cellulose fibers to obtain chemically modified cellulose, a dehydration and washing step of dehydrating and washing the dispersion of the chemically modified cellulose, an adjustment step of adjusting the concentration of the dispersion of the chemically modified cellulose, and a defibration step of defibrating the dispersion of the chemically modified cellulose by applying a mechanical shear force, wherein a sine wave pump is used to transport the dispersion of the chemically modified cellulose in at least one of the steps. [2] The method for producing fine fibrous cellulose according to [1], wherein the reaction step is a step of introducing ionic groups into cellulose fibers. [3] The method for producing fine fibrous cellulose according to [2], wherein the ionic group is an anionic group. [4] The method for producing fine fibrous cellulose according to [3], wherein the anionic group is at least one selected from the group consisting of a phosphorus oxoacid group, a sulfur oxoacid group, and a carboxy group. [5] The method for producing fine fibrous cellulose according to [3], wherein the anionic group is a phosphorus oxo acid group. Effect of the Invention

[0006] According to the present invention, there is provided a method for producing fine fibrous cellulose in which changes in quality are suppressed. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a graph showing the relationship between the amount of NaOH dropped onto a slurry containing fibrous cellulose having phosphorus oxoacid groups and pH. [Diagram 2] FIG. 2 is a graph showing the relationship between the amount of NaOH dropped onto a slurry containing fibrous cellulose having a carboxy group and pH. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Method of producing fine fibrous cellulose] The method for producing fine fibrous cellulose in this embodiment includes a reaction step in which cellulose fibers are chemically modified to obtain chemically modified cellulose, a dehydration and washing step in which the dispersion of the chemically modified cellulose is dehydrated and washed, an adjustment step in which the concentration of the dispersion of the chemically modified cellulose is adjusted, and a defibration step in which the dispersion of the chemically modified cellulose is defibrated by applying a mechanical shear force, and a sine wave pump is used to transport the dispersion of the chemically modified cellulose in at least one of the steps.

[0009] [Sine Pump] A sine wave pump is a positive displacement pump that uses a rotor with a sine wave shape. As the single sine wave rotor rotates, four chambers of equal volume are created, and the fluid being pumped is drawn into each chamber in turn through the suction port, and the chambers rotate to discharge the fluid to the discharge port. In addition, as the fluid is discharged, the next fluid is sucked into the chamber, suppressing pulsation. Sine pumps can be used in the production process of fine fibrous cellulose, for circulation in the process of chemically modifying the raw pulp fibers by introducing ionic groups, etc., or for delivering modified reaction solution slurry, as well as for delivering washed reaction solution slurry, and for the high-viscosity fine fibrous cellulose slurry obtained by nano-dispersing chemically modified pulp through high shear.

[0010] Pumps are broadly classified into turbo (non-positive displacement) pumps and positive displacement pumps. Turbo pumps include centrifugal pumps such as volute pumps and diffuser pumps, mixed flow pumps, and axial flow pumps. Positive displacement pumps include reciprocating pumps such as piston pumps, plunger pumps, and diaphragm pumps, as well as gear pumps, vane pumps, and screw pumps. Sine pumps are broadly classified as positive displacement pumps, and as described above, are pumps that transfer fluid by continuously moving the space generated between a rotor and a stator having a sine wave shape. Compared to turbo (non-positive displacement) pumps, which impart kinetic energy to the fluid by rotating an impeller at high speed inside a casing, this type of pump is characterized by the fact that it applies less shear force to the fluid and has extremely little leakage between the rotor and stator, resulting in a high head and the ability to pump fluids with relatively high viscosity.

[0011] The flow rate during transfer by a sine pump is largely dependent on the size of the sine pump, and is not particularly limited. By appropriately selecting the size of the sine pump to be used according to the desired flow rate, it is possible to obtain a flow rate appropriate for the manufacturing process while keeping the shear force applied to the fluid low. Each step will be described in detail below.

[0012] [Reaction step] The reaction step is a step in which cellulose fibers are chemically modified to obtain chemically modified cellulose. In the present invention, the raw material cellulose fiber refers to various forms of materials mainly made of cellulose, and the raw material cellulose fiber is not particularly limited, but examples thereof include wood pulp, non-wood pulp, and deinked pulp. The wood pulp is not particularly limited, but examples thereof include chemical pulps such as hardwood kraft pulp (LBKP), softwood kraft pulp (NBKP), sulfite pulp (SP), dissolving pulp (DP), soda pulp (AP), unbleached kraft pulp (UKP), and oxygen bleached kraft pulp (OKP), semi-chemical pulps such as semi-chemical pulp (SCP) and chemi-ground wood pulp (CGP), and mechanical pulps such as groundwood pulp (GP) and thermomechanical pulp (TMP, BCTMP). The non-wood pulp is not particularly limited, but examples thereof include cotton-based pulps such as cotton linters and cotton lint, and non-wood pulps such as hemp, straw, bamboo, and bagasse. The deinked pulp is not particularly limited, but may be, for example, deinked pulp made from waste paper. The pulp raw material of this embodiment may be one of the above alone or a mixture of two or more of them. Among the cellulose fibers used as the raw material, for example, wood pulp and deinked pulp are preferred from the viewpoint of availability. Furthermore, among wood pulp, for example, chemical pulp is more preferred, and kraft pulp and sulfite pulp are even more preferred, from the viewpoint of a high cellulose ratio and a high yield of fine fibrous cellulose during defibration treatment, and of obtaining long-fiber fine fibrous cellulose with a large axial ratio due to little decomposition of cellulose in the pulp. Note that the viscosity tends to increase when long-fiber fine fibrous cellulose with a large axial ratio is used.

[0013] In the present invention, when a sheet-like cellulose raw material is used, it is preferable to roughly crush it to a size of about 0.5 to 5 cm square. By roughly crushing it to the above size, the cellulose raw material can be efficiently and uniformly modified in the next reaction step. The method of roughly crushing is not particularly limited, but a single-shaft rotary shear type grinder, a double-shaft rotary shear type grinder, a multi-shaft screw type grinder, a shredder, a guillotine cutter, etc. can be used. Among these, the use of a single-shaft rotary shear type grinder or a shredder is preferable from the viewpoint of rough crushing.

[0014] The cellulose fibers are chemically modified to obtain chemically modified cellulose. The chemical modification is preferably performed by introducing an ionic group (ionic substituent). That is, the reaction step is preferably a step of introducing an ionic group into the cellulose fibers. The ionic group may include, for example, either one or both of an anionic group and a cationic group. In this embodiment, it is particularly preferable that the ionic group has an anionic group. In addition, the ionic group is preferably a group that is introduced into the cellulose fibers via an ester bond or an ether bond, and more preferably a group that is introduced into the cellulose fibers via an ester bond. In this case, the ester bond is preferably formed by dehydration condensation of the cellulose fibers and a compound that becomes an ionic group.

[0015] Examples of anionic groups as ionic groups include phosphorus oxoacid groups or substituents derived from phosphorus oxoacid groups (sometimes simply referred to as phosphorus oxoacid groups), carboxy groups or substituents derived from carboxy groups (sometimes simply referred to as carboxy groups), sulfur oxoacid groups or substituents derived from sulfur oxoacid groups (sometimes simply referred to as sulfur oxoacid groups), xanthate groups or substituents derived from xanthate groups (sometimes simply referred to as xanthate groups), phosphonic groups or substituents derived from phosphonic groups, phosphine groups or substituents derived from phosphine groups, sulfone groups or substituents derived from sulfone groups, and carboxyalkyl groups. Among them, the anionic group is preferably at least one selected from the group consisting of a phosphorus oxoacid group, a substituent derived from a phosphorus oxoacid group, a carboxy group, a sulfur oxoacid group, a substituent derived from a sulfur oxoacid group, a carboxymethyl group, a carboxyethyl group, and a sulfone group, more preferably at least one selected from the group consisting of a phosphorus oxoacid group, a substituent derived from a phosphorus oxoacid group, a carboxy group, a sulfur oxoacid group, and a substituent derived from a sulfur oxoacid group, and particularly preferably a phosphorus oxoacid group. By introducing a phosphorus oxoacid group as the anionic group, defibration is possible with less energy. Examples of the cationic group as the ionic group include an ammonium group, a phosphonium group, a sulfonium group, etc. Among these, the cationic group is preferably an ammonium group.

[0016] The phosphorus oxoacid group or the substituent derived from the phosphorus oxoacid group is, for example, a substituent represented by the following formula (1). A plurality of substituents represented by the following formula (1) may be introduced into each fibrous cellulose. In this case, the plurality of introduced substituents represented by the following formula (1) may be the same or different.

[0017] [ka]

[0018] In formula (1), a, b, and n are natural numbers, and m is an arbitrary number (where a=b×m). At least one of the n α and α' is O. - and the rest are R or OR. Note that all of α and α' are O - The n α's may all be the same or may be different. b+ is a cation of one or more valences consisting of organic or inorganic substances.

[0019] Each R is a hydrogen atom, a saturated linear hydrocarbon group, a saturated branched hydrocarbon group, a saturated cyclic hydrocarbon group, an unsaturated linear hydrocarbon group, an unsaturated branched hydrocarbon group, an unsaturated cyclic hydrocarbon group, an aromatic group, or a group derived therefrom. In formula (1), n ​​is preferably 1.

[0020] Examples of saturated linear hydrocarbon groups include, but are not limited to, methyl, ethyl, n-propyl, or n-butyl groups. Examples of saturated branched hydrocarbon groups include, but are not limited to, i-propyl or t-butyl groups. Examples of saturated cyclic hydrocarbon groups include, but are not limited to, cyclopentyl or cyclohexyl groups. Examples of unsaturated linear hydrocarbon groups include, but are not limited to, vinyl or allyl groups. Examples of unsaturated branched hydrocarbon groups include, but are not limited to, i-propenyl or 3-butenyl groups. Examples of unsaturated cyclic hydrocarbon groups include, but are not limited to, cyclopentenyl or cyclohexenyl groups. Examples of aromatic groups include, but are not limited to, phenyl or naphthyl groups.

[0021] In addition, the derivative group in R is a carboxy group, a carboxylate group (-COO -), functional groups in which at least one selected from functional groups such as hydroxyl, amino and ammonium groups is added or substituted, but are not particularly limited. The number of carbon atoms constituting the main chain of R is not particularly limited, but is preferably 20 or less, more preferably 10 or less. By setting the number of carbon atoms constituting the main chain of R within the above range, the molecular weight of the phosphorus oxoacid group can be set to an appropriate range, which facilitates penetration into the fiber raw material and increases the yield of fibrous cellulose. When multiple Rs exist in formula (1) or multiple types of substituents represented by the above formula (1) are introduced into the fibrous cellulose, the multiple Rs may be the same or different.

[0022] β b+ is a monovalent or higher cation made of an organic or inorganic substance. An example of the monovalent or higher cation made of an organic substance is an organic onium ion. An example of the organic onium ion is an organic ammonium ion or an organic phosphonium ion. An example of the organic ammonium ion is an aliphatic ammonium ion or an aromatic ammonium ion, and an example of the organic phosphonium ion is an aliphatic phosphonium ion or an aromatic phosphonium ion. An example of the monovalent or higher cation made of an inorganic substance is an ion of an alkali metal such as sodium, potassium, or lithium, an ion of a divalent metal such as calcium or magnesium, a hydrogen ion, an ammonium ion, or the like. In addition, in formula (1), β b+ When a plurality of substituents represented by the above formula (1) are present or when a plurality of substituents represented by the above formula (1) are introduced into the fibrous cellulose, the plurality of β b+ may be the same or different. The organic or inorganic cations of monovalent or higher include β b+ Sodium or potassium ions are preferred because they are less likely to yellow when the fiber raw material containing the cation is heated and are easy to use industrially, but there is no particular limitation.

[0023] More specifically, examples of the phosphorus oxoacid group or the substituent derived from the phosphorus oxoacid group include a phosphoric acid group (-PO3H2), a salt of a phosphoric acid group, a phosphorous acid group (phosphonic acid group) (-PO2H2), and a salt of a phosphorous acid group (phosphonic acid group). In addition, the phosphorus oxoacid group or the substituent derived from the phosphorus oxoacid group may be a group in which a phosphoric acid group is condensed (e.g., a pyrophosphate group), a group in which a phosphonic acid is condensed (e.g., a polyphosphonic acid group), a phosphoric ester group (e.g., a monomethyl phosphate group, a polyoxyethylene alkyl phosphate group), an alkyl phosphonic acid group (e.g., a methyl phosphonic acid group), and the like.

[0024] The sulfur oxoacid group (sulfur oxoacid group or a substituent derived from a sulfur oxoacid group) is, for example, a substituent represented by the following formula (2). A plurality of substituents represented by the following formula (2) may be introduced into each fibrous cellulose. In this case, the plurality of introduced substituents represented by the following formula (2) may be the same or different.

[0025] [ka]

[0026] In the above structural formula, b and n are natural numbers, p is 0 or 1, and m is an arbitrary number (where 1=b×m). When n is 2 or more, the multiple p's may be the same or different. In the above structural formula, β b+is a monovalent or higher cation made of an organic or inorganic substance. Examples of the monovalent or higher cation made of an organic substance include organic onium ions. Examples of the organic onium ions include organic ammonium ions and organic phosphonium ions. Examples of the organic ammonium ions include aliphatic ammonium ions and aromatic ammonium ions, and examples of the organic phosphonium ions include aliphatic phosphonium ions and aromatic phosphonium ions. Examples of the monovalent or higher cation made of an inorganic substance include ions of alkali metals such as sodium, potassium, or lithium, ions of divalent metals such as calcium or magnesium, hydrogen ions, and ammonium ions. When multiple types of substituents represented by the above formula (2) are introduced into the fibrous cellulose, the multiple β b+ may be the same or different. The organic or inorganic cations of monovalent or higher include β b+ Sodium or potassium ions are preferred because they are less likely to yellow when the fiber raw material containing the cation is heated and are easy to use industrially, but there is no particular limitation.

[0027] The amount of ionic groups introduced into the cellulose fibers is, for example, preferably 0.10 mmol / g or more per 1 g (mass) of cellulose fibers, more preferably 0.20 mmol / g or more, even more preferably 0.40 mmol / g or more, and particularly preferably 0.60 mmol / g or more. The amount of ionic groups introduced into the cellulose fibers is, for example, preferably 5.20 mmol / g or less per 1 g (mass) of cellulose fibers, more preferably 3.65 mmol / g or less, even more preferably 3.00 mmol / g or less, even more preferably 2.50 mmol / g or less, even more preferably 2.00 mmol / g or less, even more preferably 1.50 mmol / g or less, and particularly preferably 1.00 mmol / g or less. Here, the denominator in the unit mmol / g is calculated based on the fact that the counter ion of the ionic group is a hydrogen ion (H +By setting the amount of ionic groups introduced within the above range, it is possible to easily refine the fiber raw material and to increase the stability of the cellulose fiber.

[0028] The amount of ionic groups introduced into the cellulose fibers can be measured, for example, by neutralization titration after the cellulose fibers are subjected to a microparticulation treatment. In the measurement by neutralization titration, the amount introduced is measured by determining the change in pH while adding an alkali such as an aqueous sodium hydroxide solution to a slurry containing the obtained cellulose fibers.

[0029] 1 is a graph showing the relationship between the amount of NaOH dropped onto a dispersion of fine fibrous cellulose having phosphorus oxo acid groups and pH. The amount of phosphorus oxo acid groups introduced into the cellulose fibers is measured, for example, as follows. First, ion-exchanged water is added to the cellulose fiber to prepare a slurry with a solid content of 0.2% by mass. This slurry is treated four times with a wet pulverizer (Starburst, manufactured by Sugino Machine Co., Ltd.) at a pressure of 200 MPa to obtain a fine fibrous cellulose dispersion (slurry) containing fine fibrous cellulose. The fine fibrous cellulose dispersion is then treated with a strong acid ion-exchange resin. Next, the change in pH is observed while adding the aqueous sodium hydroxide solution, and a titration curve such as that shown in the upper part of Figure 1 is obtained. In the titration curve shown in the upper part of Figure 1, the measured pH is plotted against the amount of alkali added, and in the titration curve shown in the lower part of Figure 1, the increment (derivative value) of pH (1 / mmol) against the amount of alkali added is plotted. In this neutralization titration, two points are confirmed in the curve plotting the measured pH against the amount of alkali added, where the increment (derivative value of pH against the amount of alkali added) is maximum. Of these, the first maximum point of the increment obtained after starting to add the alkali is called the first endpoint, and the next maximum point of the increment is called the second endpoint. The amount of alkali required from the start of titration to the first end point is equal to the amount of the first dissociated acid of the fibrous cellulose contained in the slurry used for titration, the amount of alkali required from the first end point to the second end point is equal to the amount of the second dissociated acid of the fibrous cellulose contained in the slurry used for titration, and the amount of alkali required from the start of titration to the second end point is equal to the total amount of dissociated acid of the fibrous cellulose contained in the slurry used for titration. The value obtained by dividing the amount of alkali required from the start of titration to the first end point by the solid content (g) in the slurry to be titrated is the amount of phosphorus oxoacid group introduced (mmol / g). Note that when simply referring to the amount of phosphorus oxoacid group introduced (or the amount of phosphorus oxoacid group), it refers to the amount of the first dissociated acid. In FIG. 1, the region from the start of titration to the first end point is called the first region, and the region from the first end point to the second end point is called the second region. For example, when the phosphorus oxoacid group is a phosphate group and this phosphate group undergoes condensation, the amount of weak acid groups in the phosphorus oxoacid group (also referred to as the second dissociated acid amount in this specification) appears to decrease, and the amount of alkali required in the second region becomes smaller than the amount of alkali required in the first region. On the other hand, the amount of strong acid groups in the phosphorus oxoacid group (also referred to as the first dissociated acid amount in this specification) is equal to the amount of phosphorus atoms regardless of the presence or absence of condensation. In addition, when the phosphorus oxoacid group is a phosphorous acid group, the phosphorus oxoacid group no longer has weak acid groups, so the amount of alkali required in the second region becomes smaller or may become zero. In this case, there is only one point on the titration curve where the pH increment is maximum.

[0030] The above-mentioned amount of phosphorus oxoacid groups introduced (mmol / g) indicates the amount of phosphorus oxoacid groups possessed by the acid-type fibrous cellulose (hereinafter referred to as the amount of phosphorus oxoacid groups (acid type)), since the denominator indicates the mass of the acid-type fibrous cellulose. On the other hand, when the counter ion of the phosphorus oxoacid group is replaced with an arbitrary cation C so as to be the charge equivalent, the amount of phosphorus oxoacid groups possessed by the fibrous cellulose in which the cation C is the counter ion (hereinafter referred to as the amount of phosphorus oxoacid groups (C type)) can be obtained by converting the denominator to the mass of the fibrous cellulose when the cation C is the counter ion. That is, it is calculated according to the following formula. Amount of phosphorus oxoacid group (C type) = Amount of phosphorus oxoacid group (acid type) / {1+(W-1)×A / 1000} A [mmol / g]: total amount of anions derived from phosphorus oxoacid groups in fibrous cellulose (total amount of dissociated acid from phosphorus oxoacid groups) W: Formula weight per valence of cation C (e.g., Na is 23, Al is 9)

[0031] 2 is a graph showing the relationship between the amount of NaOH dropped onto a dispersion of fine fibrous cellulose having a carboxy group as an ionic group and pH. The amount of carboxy group introduced into the cellulose fibers is measured, for example, as follows. First, ion-exchanged water is added to the cellulose fiber to prepare a slurry with a solid content of 0.2% by mass. This slurry is treated four times with a wet pulverizer (Starburst, manufactured by Sugino Machine Co., Ltd.) at a pressure of 200 MPa to obtain a fine fibrous cellulose dispersion (slurry) containing fine fibrous cellulose. The fine fibrous cellulose dispersion is then treated with a strong acid ion-exchange resin. Next, the change in pH is observed while adding the aqueous sodium hydroxide solution, and a titration curve as shown in the upper part of FIG. 2 is obtained. In the titration curve shown in the upper part of FIG. 2, the measured pH is plotted against the amount of added alkali, and in the titration curve shown in the lower part of FIG. 2, the increment (differential value) (1 / mmol) of pH against the amount of added alkali is plotted. In this neutralization titration, one point where the increment (differential value of pH against the amount of added alkali) is maximum is confirmed in the curve plotting the measured pH against the amount of added alkali, and this maximum point is called the first end point. Here, the region from the start of titration to the first end point in FIG. 2 is called the first region. The amount of alkali required in the first region is equal to the amount of carboxyl groups in the dispersion used for titration. The amount of alkali required in the first region of the titration curve (mmol) is divided by the solid content (g) in the dispersion containing the fibrous cellulose to be titrated to calculate the amount of carboxyl groups introduced (mmol / g).

[0032] The above-mentioned amount of carboxyl groups introduced (mmol / g) indicates the amount of carboxyl groups in the acid-type fibrous cellulose (hereinafter referred to as the amount of carboxyl groups (acid type)) since the denominator is the mass of the acid-type fibrous cellulose. On the other hand, when the counter ion of the carboxyl group is replaced with any cation C so as to be the charge equivalent, the amount of carboxyl groups in the fibrous cellulose in which the cation C is the counter ion (hereinafter referred to as the amount of carboxyl groups (C type)) can be obtained by converting the denominator to the mass of the fibrous cellulose when the cation C is the counter ion. That is, it is calculated by the following formula. Carboxylic acid amount (C type) = Carboxylic acid amount (acid type) / {1 + (W-1) x (Carboxylic acid amount (acid type)) / 1000} W: Formula weight per valence of cation C (e.g., Na is 23, Al is 9)

[0033] In measuring the amount of ionic groups by titration, if the amount of sodium hydroxide solution dropped is too large or the titration interval is too short, the amount of ionic groups may be lower than the actual amount, and an accurate value may not be obtained. For example, an appropriate amount of drop and titration interval may be, for example, 10 μL to 50 μL of 0.1N sodium hydroxide solution titrated for 5 to 30 seconds. In addition, in order to eliminate the influence of carbon dioxide dissolved in the fine fibrous cellulose dispersion, it is preferable to measure while blowing an inert gas such as nitrogen gas into the slurry from 15 minutes before the start of titration until the end of titration.

[0034] The amount of sulfur oxoacid and sulfonic acid groups introduced into the fibrous cellulose was measured by wet ashing the obtained fibrous cellulose using perchloric acid and concentrated nitric acid, diluting it at an appropriate ratio, and measuring the amount of sulfur by ICP atomic emission spectrometry. The amount of sulfur thus determined was divided by the bone dry mass of the fibrous cellulose tested, and this value was taken as the amount of sulfur oxoacid groups and sulfonic groups (unit: mmol / g).

[0035] In order to obtain chemically modified cellulose having an ionic group introduced therein, it is preferable to have an ionic group introduction step in which an ionic group is introduced into the above-mentioned cellulose-containing fiber raw material (cellulose fiber), and examples of the ionic group introduction step include a phosphorus oxo acid group introduction step, a carboxyl group introduction step, a sulfur oxo acid group introduction step, a xanthate group introduction step, a phosphonic or phosphine group introduction step, a sulfonic group introduction step, and a cationic group introduction step. Each of these steps will be described below.

[0036] <Phosphorus oxo acid group introduction step> When obtaining chemically modified cellulose having ionic groups, it is preferable to provide a reaction step for introducing ionic groups prior to the defibration step. An example of the reaction step is a phosphorus oxoacid group introduction step. The phosphorus oxoacid group introduction step is a step of reacting at least one compound (hereinafter also referred to as "compound A") selected from compounds capable of introducing phosphorus oxoacid groups by reacting with hydroxyl groups possessed by cellulose fibers with the cellulose fibers as raw material. This step results in the production of cellulose fibers having phosphorus oxoacid groups (chemically modified cellulose).

[0037] In the phosphorus oxoacid group introduction step according to this embodiment, the reaction between the cellulose fiber and compound A may be carried out in the presence of at least one selected from urea and its derivatives (hereinafter also referred to as "compound B"). Alternatively, the reaction between the cellulose fiber and compound A may be carried out in the absence of compound B.

[0038] An example of a method for acting compound A on cellulose fibers in the presence of compound B includes a method of mixing compound A and compound B with cellulose fibers in a dry state, a wet state, or a slurry state. Of these, it is preferable to use cellulose fibers in a dry state or a wet state, and it is particularly preferable to use cellulose fibers in a dry state, because the reaction is highly uniform. The form of the cellulose fibers is not particularly limited, but is preferably, for example, cotton-like or thin sheet-like. Compound A and compound B may be added to the fiber raw material in a powder form, a solution form dissolved in a solvent, or a melted state by heating to a melting point or higher. Of these, it is preferable to add compound A and compound B in a solution form dissolved in a solvent, especially in an aqueous solution form, because the reaction is highly uniform. Compound A and compound B may be added to cellulose fibers simultaneously, separately, or as a mixture. The method of adding compound A and compound B is not particularly limited, but when compound A and compound B are in a solution form, the cellulose fibers may be immersed in the solution to absorb the liquid and then removed, or the solution may be dropped or sprayed onto the cellulose fibers. Alternatively, the required amounts of compound A and compound B may be added to the cellulose fibers, or excess amounts of compound A and compound B may be added to the cellulose fibers, and then the excess compound A and compound B may be removed by squeezing or filtration.

[0039] Compound A used in this embodiment may be any compound having a phosphorus atom and capable of forming an ester bond with cellulose, and may include, but is not limited to, phosphoric acid or a salt thereof, phosphorous acid or a salt thereof, dehydrated condensed phosphoric acid or a salt thereof, and anhydrous phosphoric acid (diphosphorus pentoxide). Phosphoric acid may be used with various purities, for example, 100% phosphoric acid (orthophosphoric acid) or 85% phosphoric acid. Phosphorous acid may be 99% phosphorous acid (phosphonic acid). Dehydrated condensed phosphoric acid is a phosphoric acid in which two or more molecules are condensed by a dehydration reaction, and examples of such include pyrophosphoric acid and polyphosphoric acid. Phosphates, phosphites, and dehydrated condensed phosphates include lithium salts, sodium salts, potassium salts, and ammonium salts of phosphoric acid, phosphorous acid, or dehydrated condensed phosphoric acid, and these may be neutralized to various degrees. Among these, from the viewpoints of high efficiency of introduction of phosphate groups, easier improvement of defibration efficiency in the defibration step described below, low cost, and ease of industrial application, phosphoric acid, sodium salt of phosphoric acid, potassium salt of phosphoric acid, ammonium salt of phosphoric acid, or phosphorous acid, sodium salt of phosphorous acid, potassium salt of phosphorous acid, or ammonium salt of phosphorous acid are preferred, and phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, ammonium dihydrogen phosphate, or phosphorous acid and sodium phosphite are more preferred.

[0040] The amount of compound A added to the cellulose fibers is not particularly limited, but for example, when the amount of compound A added is converted into the amount of phosphorus atoms, the amount of phosphorus atoms added to the cellulose fibers (bone dry mass) is preferably 0.5% by mass or more and 100% by mass or less, more preferably 1% by mass or more and 50% by mass or less, and even more preferably 2% by mass or more and 30% by mass or less. By setting the amount of phosphorus atoms added to the cellulose fibers within the above range, the yield of fine fibrous cellulose can be further improved. On the other hand, by setting the amount of phosphorus atoms added to the cellulose fibers to the above upper limit or less, a balance can be achieved between the effect of improving the yield and the cost.

[0041] The compound B used in this embodiment is at least one selected from urea and its derivatives as described above. Examples of compound B include urea, biuret, 1-phenylurea, 1-benzylurea, 1-methylurea, and 1-ethylurea. From the viewpoint of improving the uniformity of the reaction, it is preferable to use compound B as an aqueous solution. In addition, from the viewpoint of further improving the uniformity of the reaction, it is preferable to use an aqueous solution in which both compound A and compound B are dissolved.

[0042] The amount of compound B added relative to the cellulose fiber (bone dry mass) is not particularly limited, but is preferably, for example, 1 mass% or more and 500 mass% or less, more preferably 10 mass% or more and 400 mass% or less, and even more preferably 100 mass% or more and 350 mass% or less.

[0043] In the reaction of a fiber raw material containing cellulose with compound A, in addition to compound B, for example, amides or amines may be included in the reaction system. Examples of amides include formamide, dimethylformamide, acetamide, and dimethylacetamide. Examples of amines include methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, triethylamine in particular is known to act as a good reaction catalyst.

[0044] In the phosphorus oxo acid group introduction step, it is preferable to add or mix compound A or the like to the cellulose fiber, and then heat-treat the cellulose fiber. It is preferable to select a temperature for the heat treatment that allows efficient introduction of phosphorus oxo acid groups while suppressing thermal decomposition and hydrolysis of the fiber. The heat treatment temperature is, for example, preferably 50°C or higher and 300°C or lower, more preferably 100°C or higher and 250°C or lower, and even more preferably 130°C or higher and 200°C or lower. In addition, for the heat treatment, equipment having various heat media can be used, such as a stirring dryer, a rotary dryer, a disk dryer, a roll-type heater, a plate-type heater, a fluidized bed dryer, a band-type dryer, a filtration dryer, a vibration fluidized dryer, an airflow dryer, a reduced pressure dryer, an infrared heater, a far-infrared heater, a microwave heater, or a high-frequency dryer.

[0045] In the heat treatment according to the present embodiment, for example, a method of adding compound A to a thin sheet-like cellulose fiber by a method such as impregnation and then heating the fiber, or a method of heating the fiber while kneading or stirring the cellulose fiber and compound A in a kneader or the like can be adopted. This makes it possible to suppress unevenness in the concentration of compound A in the cellulose fiber and introduce phosphorus oxoacid groups more uniformly onto the surface of the cellulose fiber. This is believed to be due to the fact that when water molecules move to the surface of the cellulose fiber as it is dried, the dissolved compound A is attracted to the water molecules by surface tension and similarly moves to the surface of the cellulose fiber (i.e., unevenness in the concentration of compound A is caused).

[0046] In addition, the heating device used in the heat treatment is preferably a device that can constantly discharge, for example, the moisture held by the slurry and the moisture generated by the dehydration condensation (phosphorylation) reaction between compound A and hydroxyl groups contained in cellulose and the like in the cellulose fibers, outside the device system. Examples of such heating devices include ovens that use a blowing system. By constantly discharging the moisture within the device system, it is possible to suppress the hydrolysis reaction of phosphate ester bonds, which is the reverse reaction of phosphate esterification, and also to suppress acid hydrolysis of the sugar chains in the cellulose fibers. This makes it possible to obtain fine fibrous cellulose with a high axial ratio.

[0047] The time for the heat treatment is, for example, preferably from 1 second to 300 minutes after the moisture has been substantially removed from the cellulose fibers, more preferably from 1 second to 1000 seconds, and even more preferably from 10 seconds to 800 seconds. In this embodiment, the introduction amount of phosphorus oxo acid groups can be kept within a preferred range by setting the heating temperature and heating time within appropriate ranges.

[0048] The phosphorus oxo acid group introduction step may be carried out at least once, but may also be carried out twice or more. By carrying out the phosphorus oxo acid group introduction step twice or more, a large number of phosphorus oxo acid groups can be introduced into the fiber raw material.

[0049] The amount of phosphorus oxoacid groups introduced into the cellulose fibers is, for example, preferably 0.10 mmol / g or more per 1 g (mass) of cellulose fibers, more preferably 0.20 mmol / g or more, even more preferably 0.50 mmol / g or more, and particularly preferably 1.00 mmol / g or more. The amount of phosphorus oxoacid groups introduced into the cellulose fibers is, for example, preferably 5.20 mmol / g or less per 1 g (mass) of cellulose fibers, more preferably 3.65 mmol / g or less, and even more preferably 3.00 mmol / g or less. By setting the amount of phosphorus oxoacid groups introduced within the above range, it is possible to facilitate the fineness of the cellulose fibers in the fineness treatment step and to increase the stability of the fine fibrous cellulose.

[0050] <Carboxy group introduction step> The ionic group introduction step may include a carboxyl group introduction step, which is carried out by subjecting the cellulose fiber to an oxidation treatment such as ozone oxidation, oxidation by the Fenton method, or TEMPO oxidation treatment, or by treating the cellulose fiber with a compound having a carboxylic acid-derived group or a derivative thereof, or an acid anhydride of a compound having a carboxylic acid-derived group or a derivative thereof.

[0051] Examples of compounds having a group derived from a carboxylic acid include, but are not limited to, dicarboxylic acid compounds such as maleic acid, succinic acid, phthalic acid, fumaric acid, glutaric acid, adipic acid, and itaconic acid, and tricarboxylic acid compounds such as citric acid and aconitic acid. Examples of derivatives of compounds having a group derived from a carboxylic acid include, but are not limited to, imidized products of acid anhydrides of compounds having a carboxy group, and derivatives of acid anhydrides of compounds having a carboxy group. Examples of imidized products of acid anhydrides of compounds having a carboxy group include, but are not limited to, imidized products of dicarboxylic acid compounds such as maleimide, succinimide, and phthalimide.

[0052] The acid anhydride of a compound having a group derived from a carboxylic acid is not particularly limited, but examples thereof include acid anhydrides of dicarboxylic acid compounds such as maleic anhydride, succinic anhydride, phthalic anhydride, glutaric anhydride, adipic anhydride, itaconic anhydride, etc. Furthermore, the derivative of an acid anhydride of a compound having a group derived from a carboxylic acid is not particularly limited, but examples thereof include acid anhydrides of compounds having a carboxy group such as dimethylmaleic anhydride, diethylmaleic anhydride, diphenylmaleic anhydride, etc., in which at least a part of the hydrogen atoms is substituted with a substituent such as an alkyl group or a phenyl group.

[0053] When a TEMPO oxidation treatment is performed in the carboxyl group introduction step, the treatment is preferably performed under conditions of pH 6 or more and 8 or less. Such a treatment is also called a neutral TEMPO oxidation treatment. The neutral TEMPO oxidation treatment can be performed, for example, by adding cellulose fibers, a nitroxy radical such as TEMPO (2,2,6,6-tetramethylpiperidine-1-oxyl) as a catalyst, and sodium hypochlorite as a sacrificial reagent to a sodium phosphate buffer solution (pH = 6.8). By further allowing sodium chlorite to coexist, aldehydes generated during the oxidation process can be efficiently oxidized to carboxyl groups. The TEMPO oxidation treatment may also be performed under conditions of pH 10 or more and 11 or less. Such a treatment is also called an alkaline TEMPO oxidation treatment. The alkaline TEMPO oxidation treatment can be performed, for example, by adding a nitroxy radical such as TEMPO as a catalyst, sodium bromide as a cocatalyst, and sodium hypochlorite as an oxidizing agent to cellulose fibers.

[0054] The amount of carboxyl groups introduced into cellulose fibers varies depending on the type of the substituent, but for example, when carboxyl groups are introduced by TEMPO oxidation, it is preferably 0.10 mmol / g or more per 1 g (mass) of cellulose fibers, more preferably 0.20 mmol / g or more, even more preferably 0.40 mmol / g or more, and particularly preferably 0.60 mmol / g or more. The amount of carboxyl groups introduced into cellulose fibers is preferably 3.65 mmol / g or less, more preferably 3.00 mmol / g or less, even more preferably 2.50 mmol / g or less, even more preferably 2.00 mmol / g or less, even more preferably 1.50 mmol / g or less, and particularly preferably 1.00 mmol / g or less. In addition, when the substituent is a carboxymethyl group, the amount of carboxyl groups introduced may be 5.8 mmol / g or less per 1 g (mass) of cellulose fibers. By setting the amount of carboxyl groups introduced within the above range, it is possible to facilitate the fine pulverization of cellulose fibers in the fine pulverization treatment step and to increase the stability of fine fibrous cellulose.

[0055] <Sulfonic group introduction step> The ionic group introduction step may include a sulfonic group introduction step, in which a hydroxyl group of the cellulose fiber reacts with a sulfur oxoacid to obtain a cellulose fiber having a sulfonic group (sulfonic group-introduced fiber).

[0056] In the sulfonic group introduction step, instead of the compound A in the above-mentioned <phosphorus oxo acid group introduction step>, at least one compound (hereinafter also referred to as "compound C") selected from compounds capable of introducing sulfonic groups by reacting with hydroxyl groups possessed by cellulose fibers is used. Compound C may be any compound having a sulfur atom and capable of forming an ester bond with cellulose, and may include, but is not limited to, sulfuric acid or its salt, sulfurous acid or its salt, and sulfuric acid amide. As sulfuric acid, those of various purities may be used, for example, 96% sulfuric acid (concentrated sulfuric acid). As sulfurous acid, 5% sulfurous acid water may be used. As sulfates or sulfites, lithium salts, sodium salts, potassium salts, ammonium salts of sulfates or sulfites may be used, and these may be neutralized to various degrees. As sulfuric acid amides, sulfamic acid or the like may be used. In the sulfonic group introduction step, it is preferable to use compound B in the above-mentioned <phosphorus oxo acid group introduction step> in the same manner.

[0057] In the sulfonic group introduction step, it is preferable to mix the cellulose fiber with an aqueous solution containing sulfur oxoacid and urea and / or a urea derivative, and then heat-treat the cellulose fiber. It is preferable to select a heat-treatment temperature that allows efficient introduction of sulfonic groups while suppressing thermal decomposition and hydrolysis of the fiber. The heat-treatment temperature is preferably 100°C or higher, more preferably 120°C or higher, and even more preferably 150°C or higher. The heat-treatment temperature is preferably 300°C or lower, more preferably 250°C or lower, and even more preferably 200°C or lower.

[0058] In the heat treatment step, it is preferable to heat until substantially no moisture is present. For this reason, the heat treatment time varies depending on the amount of moisture contained in the cellulose fiber and the amount of the aqueous solution containing sulfur oxoacid and urea and / or a urea derivative added, but is preferably, for example, 10 seconds or more and 10,000 seconds or less. For the heat treatment, various devices having a heat medium can be used, such as a hot air dryer, a stirring dryer, a rotary dryer, a disk dryer, a roll type heater, a plate type heater, a fluidized bed dryer, a band type dryer, a filtration dryer, a vibration fluidized dryer, an air flow dryer, a reduced pressure dryer, an infrared heater, a far infrared heater, a microwave heater, and a high frequency dryer.

[0059] The amount of sulfonic groups introduced into the cellulose fibers is preferably 0.05 mmol / g or more, more preferably 0.10 mmol / g or more, even more preferably 0.20 mmol / g or more, even more preferably 0.40 mmol / g or more, and particularly preferably 0.50 mmol / g or more. The amount of sulfonic groups introduced into the cellulose fibers is preferably 5.00 mmol / g or less, more preferably 3.00 mmol / g or less. By setting the amount of sulfonic groups introduced within the above range, it is possible to facilitate the fineness of the cellulose fibers in the fineness treatment step and to increase the stability of the fine fibrous cellulose.

[0060] <Oxidation step using a chlorine-based oxidizing agent (second carboxyl group introduction step)> The ionic group introduction step may include an oxidation step using a chlorine-based oxidizing agent, in which the chlorine-based oxidizing agent is added to wet or dry cellulose fibers having hydroxyl groups to cause a reaction, thereby introducing carboxyl groups into the cellulose fibers.

[0061] Examples of chlorine-based oxidizing agents include hypochlorous acid, hypochlorites, chlorous acid, chlorites, chloric acid, chlorates, perchloric acid, perchlorates, and chlorine dioxide. In terms of the efficiency of introducing a substituent, and therefore the efficiency of defibration, cost, and ease of handling, the chlorine-based oxidizing agent is preferably sodium hypochlorite, sodium chlorite, or chlorine dioxide. When adding a chlorine-based oxidizing agent, it may be added to the fiber raw material as it is as a reagent (solid or liquid), or it may be added after dissolving in an appropriate solvent.

[0062] The concentration of the chlorine-based oxidizing agent in the solution in the oxidation step using the chlorine-based oxidizing agent is, for example, preferably 1% by mass to 1,000% by mass, more preferably 5% by mass to 500% by mass, and even more preferably 10% by mass to 100% by mass. The amount of the chlorine-based oxidizing agent added per 100 parts by mass of cellulose fibers is preferably 1 part by mass to 100,000 parts by mass, more preferably 10 parts by mass to 10,000 parts by mass, and even more preferably 100 parts by mass to 5,000 parts by mass.

[0063] The reaction time with the chlorine-based oxidizing agent in the oxidation step using the chlorine-based oxidizing agent may vary depending on the reaction temperature, but is preferably from 1 minute to 1,000 minutes, more preferably from 10 minutes to 500 minutes, and even more preferably from 20 minutes to 400 minutes. The pH during the reaction is preferably from 5 to 15, more preferably from 7 to 14, and even more preferably from 9 to 13. At the start of the reaction, the pH during the reaction is preferably kept constant (for example, pH 11) by appropriately adding hydrochloric acid or sodium hydroxide. After the reaction, excess reaction reagents, by-products, etc. may be washed and removed with water by filtration or the like.

[0064] <Xanthate group introduction process> The process for producing fine fibrous cellulose may include a xanthate group introduction process as a reaction process. In the xanthate group introduction process, hydroxyl groups of cellulose fibers are replaced with xanthate groups represented by the following formula (3), thereby obtaining cellulose fibers having xanthate groups (xanthate group-introduced fibers). -OCSS - M + ……(3) Here, M + is at least one selected from a hydrogen ion, a monovalent metal ion, an ammonium ion, and an aliphatic or aromatic ammonium ion.

[0065] In the xanthate group introduction step, the cellulose fiber is first treated with an alkali solution to obtain alkali cellulose. Examples of the alkali solution include an alkali metal hydroxide aqueous solution and an alkaline earth metal hydroxide aqueous solution. Among them, the alkali solution is preferably an alkali metal hydroxide aqueous solution such as sodium hydroxide or potassium hydroxide, and is particularly preferably an aqueous sodium hydroxide solution. When the alkali solution is an alkali metal hydroxide aqueous solution, the alkali metal hydroxide concentration in the alkali metal hydroxide aqueous solution is preferably 4% by mass or more, more preferably 5% by mass or more. In addition, the alkali metal hydroxide concentration in the alkali metal hydroxide aqueous solution is preferably 9% by mass or less. By setting the alkali metal hydroxide concentration to the above lower limit value or more, the mercerization of cellulose can be sufficiently promoted, the amount of by-products generated during the subsequent xanthation can be reduced, and as a result, the yield of xanthate group-introduced fiber can be increased. This makes it possible to more effectively perform the defibration treatment described below. Furthermore, by setting the alkali metal hydroxide concentration to the above upper limit or less, it is possible to prevent the aqueous alkali metal hydroxide solution from penetrating into the crystalline regions of cellulose while allowing mercerization to proceed, which makes it easier to maintain the cellulose type I crystal structure and further increases the yield of fine fibrous cellulose.

[0066] The alkali treatment time is preferably 30 minutes or more, more preferably 1 hour or more. The alkali treatment time is preferably 6 hours or less, more preferably 5 hours or less. By setting the alkali treatment time within the above range, the final yield can be increased, and the productivity can be improved.

[0067] The alkali cellulose obtained by the above-mentioned alkali treatment is preferably subjected to solid-liquid separation to remove as much aqueous solution as possible. This can reduce the water content during the subsequent xanthate treatment, and can promote the reaction. As a method for solid-liquid separation, for example, a general dehydration method such as centrifugation or filtration can be used. In addition, the concentration of alkali metal hydroxide contained in the alkali cellulose after solid-liquid separation is preferably 3% by mass or more and 8% by mass or less with respect to the total mass of the alkali cellulose after solid-liquid separation.

[0068] In the xanthate group introduction process, a xanthate formation process is carried out after the alkali treatment. In the xanthate formation process, carbon disulfide (CS2) is reacted with alkali cellulose to form (-O - Na + ) group to (-OCSS - Na + In the above, the metal ions introduced into the alkali cellulose are typically Na + However, similar reactions occur with other alkali metal ions.

[0069] In the xanthate treatment, it is preferable to supply 10% by mass or more of carbon disulfide based on the absolute dry mass of cellulose in the alkali cellulose. In addition, in the xanthate treatment, the time for which carbon disulfide and alkali cellulose are in contact is preferably 30 minutes or more, more preferably 1 hour or more. Although the xanthate formation proceeds quickly when carbon disulfide contacts alkali cellulose, it takes time for carbon disulfide to penetrate into the inside of alkali cellulose, so it is preferable to set the reaction time to the above range. On the other hand, the time for which carbon disulfide contacts alkali cellulose may be 6 hours or less, which allows sufficient penetration into the mass of alkali cellulose after dehydration, and allows the reaction-ready xanthate formation to be almost completed.

[0070] The reaction temperature in the xanthate treatment is preferably 46° C. or less. By setting the reaction temperature within the above range, it is easy to suppress the decomposition of the alkali cellulose. In addition, by setting the reaction temperature within the above range, it is easy to react uniformly, so that the generation of by-products can be suppressed, and further, the removal of the generated xanthate group can be suppressed.

[0071] The amount of xanthate group introduced in the xanthate group introduction step is preferably 0.60 mmol / g or more per 1 g (mass) of cellulose fiber, more preferably 0.70 mmol / g or more, even more preferably 0.80 mmol / g or more, even more preferably 1.00 mmol / g or more, and particularly preferably 1.20 mmol / g or more. The amount of xanthate group introduced is preferably 5.00 mmol / g or less per 1 g (mass) of cellulose fiber, more preferably 3.00 mmol / g or less. By setting the amount of xanthate group introduction within the above range, a fine fibrous cellulose having excellent defibration properties and excellent transparency can be obtained.

[0072] <Phosphonic or Phosphine Group Introduction Step (Phosphoalkylation Step)> The ionic group introduction step may include a phosphonic or phosphine group introduction step (phosphoalkylation step). In the phosphoalkylation step, a compound having a reactive group and a phosphonic or phosphine group (compound E A ), an optional alkaline compound, and compound B selected from the above-mentioned urea and its derivatives are added to a wet or dry fiber raw material having hydroxyl groups and reacted to introduce phosphonic or phosphine groups into the cellulose fiber.

[0073] Examples of the reactive group include a halogenated alkyl group, a vinyl group, and an epoxy group (glycidyl group). Compound E A Examples of the compound E include vinyl phosphonic acid, phenyl vinyl phosphonic acid, and phenyl vinyl phosphinic acid. From the viewpoints of the efficiency of introducing the substituent, the defibration efficiency, the cost, and the ease of handling, the compound E A is preferably vinylphosphonic acid. Furthermore, as an optional component, it is also preferable to use compound B in the above-mentioned <Phosphorus oxo acid group introduction step> in the same manner, and the amount added is also preferably as described above.

[0074] Compound E A When adding, it may be added to the cellulose fiber as a reagent (solid or liquid) as it is, or it may be dissolved in an appropriate solvent and added. It is preferable that the cellulose fiber is converted into alkali cellulose in advance or simultaneously with the reaction. The method of conversion into alkali cellulose is as described above.

[0075] The temperature during the reaction is, for example, preferably 50°C or higher and 300°C or lower, more preferably 100°C or higher and 250°C or lower, and even more preferably 130°C or higher and 200°C or lower.

[0076] Compound E AThe amount of the additive per 100 parts by mass of cellulose fibers is preferably 1 part by mass or more and 100,000 parts by mass or less, more preferably 2 parts by mass or more and 10,000 parts by mass or less, and even more preferably 5 parts by mass or more and 1,000 parts by mass or less.

[0077] The reaction time may vary depending on the reaction temperature, but is preferably, for example, from 1 minute to 1,000 minutes, more preferably from 10 minutes to 500 minutes, and even more preferably from 20 minutes to 400 minutes. After the reaction, excess reaction reagents, by-products, etc. may be washed and removed with water by filtration or the like.

[0078] <Sulfone Group Introduction Step (Sulfoalkylation Step) (Second Sulfone Group Introduction Step)> The ionic group introduction step may include a sulfone group introduction step (sulfoalkylation step). In the sulfoalkylation, a compound having a reactive group and a sulfone group (compound E B ) and, as an optional component, an alkali compound, and compound B selected from the above-mentioned urea and its derivatives are added to wet or dry cellulose fibers having hydroxyl groups and reacted to introduce sulfone groups into the cellulose fibers.

[0079] Examples of the reactive group include a halogenated alkyl group, a vinyl group, and an epoxy group (glycidyl group). Compound E B Examples of suitable sulfonates include sodium 2-chloroethanesulfonate, sodium vinylsulfonate, sodium p-styrenesulfonate, and 2-acrylamido-2-methylpropanesulfonic acid. Among these, compound E is particularly preferred in terms of the efficiency of introducing substituents, and therefore the defibration efficiency, cost, and ease of handling. B is preferably sodium vinyl sulfonate. Furthermore, as an optional component, it is also preferable to use compound B in the above-mentioned <Phosphorus oxo acid group introduction step> in the same manner, and the amount added is also preferably as described above.

[0080] Compound EB When adding, it may be added to the cellulose fiber as a reagent (solid or liquid) as it is, or it may be dissolved in an appropriate solvent and added. It is preferable that the cellulose fiber is converted into alkali cellulose in advance or simultaneously with the reaction. The method of conversion into alkali cellulose is as described above.

[0081] The temperature during the reaction is, for example, preferably 50°C or higher and 300°C or lower, more preferably 100°C or higher and 250°C or lower, and even more preferably 130°C or higher and 200°C or lower.

[0082] Compound E B The amount of the additive per 100 parts by mass of cellulose fibers is preferably 1 part by mass or more and 100,000 parts by mass or less, more preferably 2 parts by mass or more and 10,000 parts by mass or less, and even more preferably 5 parts by mass or more and 1,000 parts by mass or less.

[0083] The reaction time may vary depending on the reaction temperature, but is preferably, for example, from 1 minute to 1,000 minutes, more preferably from 10 minutes to 500 minutes, and even more preferably from 15 minutes to 400 minutes. After the reaction, excess reaction reagents, by-products, etc. may be washed and removed with water by filtration or the like.

[0084] <Carboxyalkylation step (third carboxy group introduction step)> The reaction step may include a carboxyalkylation step. As an essential component, a compound having a reactive group and a carboxy group (compound E C ), an optional alkaline compound, and compound B selected from the above-mentioned urea and its derivatives are added to wet or dry cellulose fibers having hydroxyl groups and reacted to introduce carboxyl groups into the cellulose fibers.

[0085] Examples of the reactive group include a halogenated alkyl group, a vinyl group, and an epoxy group (glycidyl group). Compound E CAs the chloropropionic acid, monochloroacetic acid, sodium monochloroacetate, 2-chloropropionic acid, 3-chloropropionic acid, sodium 2-chloropropionate, and sodium 3-chloropropionate are preferred from the standpoint of efficiency of introducing substituents, and therefore defibration efficiency, cost, and ease of handling. Furthermore, as an optional component, it is also preferable to use compound B in the above-mentioned <Phosphorus oxo acid group introduction step> in the same manner, and the amount added is also preferably as described above.

[0086] Compound E C When adding, it may be added to the cellulose fiber as a reagent (solid or liquid) as it is, or it may be dissolved in an appropriate solvent and added. It is preferable that the cellulose fiber is converted into alkali cellulose in advance or simultaneously with the reaction. The method of conversion into alkali cellulose is as described above.

[0087] The temperature during the reaction is, for example, preferably 50°C or higher and 300°C or lower, more preferably 100°C or higher and 250°C or lower, and even more preferably 130°C or higher and 200°C or lower.

[0088] Compound E C The amount of the additive per 100 parts by mass of cellulose fibers is preferably 1 part by mass or more and 100,000 parts by mass or less, more preferably 2 parts by mass or more and 10,000 parts by mass or less, and even more preferably 5 parts by mass or more and 1,000 parts by mass or less.

[0089] The reaction time may vary depending on the reaction temperature, but is preferably, for example, from 1 minute to 1,000 minutes, more preferably from 3 minutes to 500 minutes, and even more preferably from 5 minutes to 400 minutes. After the reaction, excess reaction reagents, by-products, etc. may be washed and removed with water by filtration or the like.

[0090] <Cationic group introduction step (cationization step)> As an essential component, a compound having a reactive group and a cationic group (compound E D), an optional alkaline compound, and compound B selected from the above-mentioned urea and its derivatives are added to wet or dry cellulose fibers having hydroxyl groups and reacted to introduce cationic groups into the cellulose fibers.

[0091] Examples of the reactive group include a halogenated alkyl group, a vinyl group, and an epoxy group (glycidyl group). Examples of the cationic group include an ammonium group, a phosphonium group, a sulfonium group, etc. Among these, the cationic group is preferably an ammonium group. Compound E D As the alkyl group, glycidyl trimethyl ammonium chloride, 3-chloro-2-hydroxypropyl trimethyl ammonium chloride, etc. are preferred from the viewpoints of the efficiency of introducing a substituent, and therefore the defibration efficiency, cost, and ease of handling. Furthermore, as an optional component, it is also preferable to use the compound B in the above-mentioned <Phosphorus oxo acid group introduction step> in the same manner. The amount of addition is also preferably as described above.

[0092] Compound E D When adding, it may be added to the cellulose fiber as a reagent (solid or liquid) as it is, or it may be dissolved in an appropriate solvent and added. It is preferable that the cellulose fiber is converted into alkali cellulose in advance or simultaneously with the reaction. The method of conversion into alkali cellulose is as described above.

[0093] The temperature during the reaction is, for example, preferably 50°C or higher and 300°C or lower, more preferably 100°C or higher and 250°C or lower, and even more preferably 130°C or higher and 200°C or lower.

[0094] Compound E D The amount of the additive per 100 parts by mass of cellulose fibers is preferably 1 part by mass or more and 100,000 parts by mass or less, more preferably 2 parts by mass or more and 10,000 parts by mass or less, and even more preferably 5 parts by mass or more and 1,000 parts by mass or less.

[0095] The reaction time may vary depending on the reaction temperature, but is preferably, for example, from 1 minute to 1,000 minutes, more preferably from 5 minutes to 500 minutes, and even more preferably from 10 minutes to 400 minutes. After the reaction, excess reaction reagents, by-products, etc. may be washed and removed with water by filtration or the like.

[0096] After the reaction step as described above, it is preferable to have a dehydration / washing step, an alkali treatment step (neutralization step), and a defibration treatment step in this order, and in addition to the washing step, an acid treatment step may be included. [Dehydration and washing process] The dehydration and washing step is a step in which the obtained dispersion of chemically modified cellulose is washed with water or an organic solvent after the dehydration treatment, and is an essential step for obtaining fine fibrous cellulose with few impurities. Washing is preferably carried out with water. In addition, the dehydration / washing step may be carried out after each step described below, and the number of washing steps carried out in each washing step is not particularly limited. In this step, dehydration devices of the centrifugal separation type, vacuum dehydration type, and pressurized dehydration type can be used. Specifically, centrifugal separation type (Tanabe Willtec centrifuge, Kokusan centrifuge, etc.), vacuum dehydration type (drum type vacuum dehydrator, Tsukishima Kikai horizontal belt filter, etc.), pressurized dehydration type (filter press, tube press), centrifugal separation type (Tanabe Willtec centrifuge, Kokusan centrifuge, etc.), and vacuum dehydration type (drum type vacuum dehydrator, Tsukishima Kikai horizontal belt filter) are preferred, since they can perform dehydration without applying strong shear force to the dehydrated raw material. In addition, a combination of these types can also be used.

[0097] In addition, an alkali treatment step or an acid treatment step may be performed between the above-mentioned dehydration / washing step and the preparation step described below, and the above-mentioned dehydration / washing step may be performed before or after the alkali treatment step or the acid treatment step. <Alkaline treatment process> An alkali treatment step may be provided between the reaction step and the adjustment step. The method of the alkali treatment is not particularly limited, but may be, for example, a method of immersing chemically modified cellulose, preferably chemically modified cellulose having an ionic group introduced therein (ionic group-introduced cellulose), in an alkali solution.

[0098] The alkaline compound contained in the alkaline solution is not particularly limited, and may be an inorganic alkaline compound or an organic alkaline compound. In this embodiment, it is preferable to use, for example, sodium hydroxide or potassium hydroxide as the alkaline compound because of its high versatility. The solvent contained in the alkaline solution may be either water or an organic solvent. Among them, the solvent contained in the alkaline solution is preferably a polar solvent including water or a polar organic solvent exemplified by alcohol, and more preferably an aqueous solvent including at least water. As the alkaline solution, for example, an aqueous sodium hydroxide solution or an aqueous potassium hydroxide solution is preferable because of its high versatility.

[0099] The temperature of the alkaline solution in the alkaline treatment step is not particularly limited, but is preferably, for example, from 5° C. to 80° C., and more preferably from 10° C. to 60° C. The immersion time of the chemically modified cellulose in the alkaline solution in the alkaline treatment step is not particularly limited, but is, for example, preferably from 5 minutes to 30 minutes, and more preferably from 10 minutes to 20 minutes. The amount of the alkaline solution used in the alkaline treatment is not particularly limited, but is, for example, preferably from 100% by mass to 100,000% by mass, and more preferably from 1,000% by mass to 10,000% by mass, based on the absolute dry mass of the chemically modified cellulose.

[0100] In order to reduce the amount of alkaline solution used in the alkaline treatment step, the chemically modified cellulose may be washed with water or an organic solvent after the reaction step and before the alkaline treatment step. From the viewpoint of improving handleability, it is preferable to wash the alkaline-treated chemically modified cellulose with water or an organic solvent after the alkaline treatment step and before the defibration step.

[0101] <Acid treatment process> In the reaction step, an acid treatment step may be provided between the step of introducing an ionic group and the adjustment step. For example, the reaction step, acid treatment, alkali treatment, and defibration treatment may be performed in this order.

[0102] The method of acid treatment is not particularly limited, but for example, a method of immersing chemically modified cellulose in an acidic solution containing an acid can be mentioned. The concentration of the acidic solution used is not particularly limited, but for example, it is preferably 10% by mass or less, more preferably 5% by mass or less. The pH of the acidic solution used is not particularly limited, but for example, it is preferably 0 to 4, more preferably 1 to 3. For example, inorganic acids, sulfonic acids, carboxylic acids, etc. can be used as the acid contained in the acidic solution. For example, inorganic acids, sulfonic acids, carboxylic acids, etc. can be mentioned as inorganic acids, for example, sulfuric acid, nitric acid, hydrobromic acid, hydroiodic acid, hypochlorous acid, chlorous acid, chloric acid, perchloric acid, phosphoric acid, boric acid, etc. can be mentioned as inorganic acids. For example, sulfonic acids can be mentioned as methanesulfonic acid, ethanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, trifluoromethanesulfonic acid, etc. can be mentioned as carboxylic acids. For example, formic acid, acetic acid, citric acid, gluconic acid, lactic acid, oxalic acid, tartaric acid, etc. can be mentioned as carboxylic acids. Among these, it is particularly preferable to use hydrochloric acid or sulfuric acid.

[0103] The temperature of the acid solution in the acid treatment is not particularly limited, but is preferably, for example, 5° C. to 100° C., and more preferably, 20° C. to 90° C. The immersion time in the acid solution in the acid treatment is not particularly limited, but is, for example, preferably, 5 minutes to 120 minutes, and more preferably, 10 minutes to 60 minutes. The amount of the acid solution used in the acid treatment is not particularly limited, but is, for example, preferably, 100 mass% to 100,000 mass%, and more preferably, 1000 mass% to 10,000 mass%, based on the absolute dry mass of the chemically modified cellulose.

[0104] [Adjustment process] In this embodiment, in order to efficiently carry out the subsequent defibration step, the concentration of the dispersion liquid of chemically modified cellulose is adjusted. In the preparation step, for example, the chemically modified cellulose is preferably diluted with a dispersion medium to form a slurry. As the dispersion medium, one or more selected from water and organic solvents such as polar organic solvents can be used. The polar organic solvent is not particularly limited, but for example, alcohols, polyhydric alcohols, ketones, ethers, esters, aprotic polar solvents, etc. are preferable. As the alcohols, for example, methanol, ethanol, isopropanol, n-butanol, isobutyl alcohol, etc. are mentioned. As the polyhydric alcohols, for example, ethylene glycol, propylene glycol, glycerin, etc. are mentioned. As the ketones, acetone, methyl ethyl ketone (MEK), etc. are mentioned. As the ethers, for example, diethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono n-butyl ether, propylene glycol monomethyl ether, etc. are mentioned. As the esters, for example, ethyl acetate, butyl acetate, etc. are mentioned. Aprotic polar solvents include dimethylsulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAc), and N-methyl-2-pyrrolidinone (NMP). Of these, it is preferable to use water.

[0105] The solids concentration of the dispersion of the chemically modified cellulose in the preparation step can be appropriately set. The solids concentration of the dispersion of chemically modified cellulose is preferably 0.1% by mass or more and 10% by mass or less. The solids concentration of the dispersion of chemically modified cellulose is more preferably 0.2% by mass or more, even more preferably 0.3% by mass or more, and is preferably 10% by mass or less, more preferably 6% by mass or less. If the solids concentration is too low, the amount of liquid becomes too large for the amount of chemically modified cellulose to be treated, resulting in poor efficiency, and if the solids concentration is too high, the flowability becomes poor. The dispersion of chemically modified cellulose may contain solid matter other than the pulp into which an ionic group has been introduced, such as urea having hydrogen bonding properties.

[0106] [Defibration process] In this embodiment, the defibration step is a step of applying a mechanical shear force to a dispersion of chemically modified cellulose to defibrate the chemically modified cellulose. In the defibration step, for example, a defibration treatment device can be used. The defibration treatment device is not particularly limited, but for example, a high-speed defibrator, a grinder (stone mill type grinder), a high-pressure homogenizer, an ultra-high-pressure homogenizer, a high-pressure collision type grinder, a ball mill, a bead mill, a disk type refiner, a conical refiner, a biaxial kneader, a vibration mill, a homomixer under high-speed rotation, an ultrasonic disperser, or a beater can be used. Among the above defibration treatment devices, it is more preferable to use a high-speed defibrator, a high-pressure homogenizer, or an ultra-high-pressure homogenizer, which are less affected by the grinding media and have less risk of contamination.

[0107] The defibration step may be carried out in one stage using the above-mentioned defibration processing device, or may be carried out in two stages consisting of a rough defibration step and a fine defibration step. When the defibration process is carried out in two stages, it is preferable to use a refiner to perform defibration in the rough defibration process, and the refiner performs preliminary defibration of the chemically modified cellulose. The refiner is a device that beats the chemically modified cellulose, and by beating the chemically modified cellulose under load, a shear force is applied to the chemically modified cellulose, causing fluffing in the chemically modified cellulose and softening the fibers, thereby performing preliminary defibration.

[0108] The refiner is not particularly limited as long as it can beat the chemically modified cellulose, and any known refiner can be used. As the refiner, a conical type, a double disc refiner (DDR), or a single disc refiner (SDR) is preferable because it can efficiently apply a shear force to the chemically modified cellulose and advance preliminary defibration.

[0109] In the fine defibration step, it is preferable to use a high-pressure homogenizer. The high-pressure homogenizer is used to finely pulp the chemically modified cellulose in the slurry, and is used as a dispersing machine that discharges the slurry or the like from fine holes at high pressure. The high-pressure homogenizer is a homogenizer capable of discharging the slurry at a pressure of, for example, 10 MPa or more, preferably 100 MPa or more. By treating the ionic group-introduced pulp with the high-pressure homogenizer, the chemically modified cellulose fibers collide with each other, the pressure difference, microcavitation, etc., and defibration occurs effectively. This allows the number of treatments in the fine defibration step to be reduced (shortened), and the production efficiency of the fine fibrous cellulose to be further improved.

[0110] <Fine fibrous cellulose> The fine fibrous cellulose obtained by the production method of this embodiment is a fibrous cellulose having a fiber width of 1,000 nm or less. The fiber width of the fibrous cellulose can be measured, for example, by observation under an electron microscope. The fiber width of the fine fibrous cellulose is 1,000 nm or less. The fiber width of the fine fibrous cellulose is, for example, preferably 2 nm or more and 1,000 nm or less, more preferably 2 nm or more and 100 nm or less, even more preferably 2 nm or more and 50 nm or less, and particularly preferably 2 nm or more and 10 nm or less. By making the fiber width of the fine fibrous cellulose 2 nm or more, it is possible to suppress dissolution of the cellulose molecules in water, and to more easily realize the effect of improving the strength, rigidity, and dimensional stability of the fine fibrous cellulose.

[0111] The average fiber width of the fine fibrous cellulose is, for example, 1,000 nm or less. The average fiber width of the fine fibrous cellulose is preferably 2 nm or more and 1,000 nm or less, more preferably 2 nm or more and 100 nm or less, even more preferably 2 nm or more and 50 nm or less, and particularly preferably 2 nm or more and 10 nm or less. By making the average fiber width of the fine fibrous cellulose 2 nm or more, it is possible to suppress dissolution of the cellulose molecules in water, and to more easily realize the effect of improving the strength, rigidity, and dimensional stability of the fine fibrous cellulose. The fine fibrous cellulose is, for example, a single-fiber cellulose.

[0112] The average fiber width of fine fibrous cellulose is measured, for example, using an electron microscope as follows. First, an aqueous suspension of fibrous cellulose with a concentration of 0.05% by mass or more and 0.1% by mass or less is prepared, and this suspension is cast on a hydrophilically treated carbon film-coated grid to prepare a sample for TEM observation. When wide fibers are included, an SEM image of the surface cast on glass may be observed. Next, observation is performed using an electron microscope image at a magnification of 1,000x, 5,000x, 10,000x, or 50,000x depending on the width of the fiber to be observed. However, the sample, observation conditions, and magnification are adjusted to satisfy the following conditions. (1) A straight line X is drawn at any point within the observed image, and 20 or more fibers intersect with the straight line X. (2) Within the same image, draw a line Y that intersects the line perpendicularly, and have 20 or more fibers intersect with the line Y.

[0113] For observation images that satisfy the above conditions, the width of the fibers that intersect with lines X and Y is visually read. In this manner, three or more sets of observation images of at least the surface portions that do not overlap each other are obtained. Next, for each image, the width of the fibers that intersect with lines X and Y is read. In this manner, the width of at least 20 fibers x 2 x 3 = 120 fibers is read. The average value of the read fiber widths is then determined as the average fiber width of the fibrous cellulose.

[0114] The fiber length of the fine fibrous cellulose is not particularly limited, but is preferably 0.1 μm or more and 1,000 μm or less, more preferably 0.1 μm or more and 800 μm or less, and even more preferably 0.1 μm or more and 600 μm or less. By setting the fiber length within the above range, destruction of the crystalline region of the fine fibrous cellulose can be suppressed. In addition, it is also possible to set the slurry viscosity of the fine fibrous cellulose to an appropriate range. The fiber length of the fine fibrous cellulose can be determined by image analysis using, for example, TEM, SEM, or AFM.

[0115] The fine fibrous cellulose preferably has a type I crystal structure. The fact that the fine fibrous cellulose has a type I crystal structure can be identified from a diffraction profile obtained from a wide-angle X-ray diffraction photograph using CuKα (λ=1.5418 Å) monochromated with graphite. Specifically, it can be identified from the presence of typical peaks at two positions, around 2θ=14° to 17° and around 2θ=22° to 23°. The proportion of I-type crystal structure in the fine fibrous cellulose is, for example, preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more. This is expected to provide even better performance in terms of heat resistance and low linear thermal expansion coefficient. The degree of crystallinity is determined by measuring an X-ray diffraction profile and using the pattern in a conventional manner (Seagal et al., Textile Research Journal, Vol. 29, p. 786, 1959).

[0116] The axial ratio (fiber length / fiber width) of the fine fibrous cellulose is not particularly limited, but is preferably, for example, 20 to 10,000, and more preferably 50 to 1,000. By setting the axial ratio to the above lower limit or more, a sheet containing the fine fibrous cellulose can be easily formed. In addition, sufficient viscosity can be easily obtained when a solvent dispersion is prepared. By setting the axial ratio to the above upper limit or less, it is preferable in that, for example, when the fine fibrous cellulose is treated as an aqueous dispersion, handling such as dilution is facilitated.

[0117] In this embodiment, the above-mentioned sine wave pump is used to transport the dispersion liquid of chemically modified cellulose. The sine wave pump may be used to transport the dispersion liquid of chemically modified cellulose in the dehydration / washing process, or may be used to transport the dispersion liquid in the above-mentioned alkali treatment process or acid treatment process. Furthermore, in the adjustment process for adjusting the concentration of the dispersion of chemically modified cellulose after washing, the separator may be used for transporting the dispersion of chemically modified cellulose to a tank storing the dispersion of chemically modified cellulose to be used in the defibration process, or for transporting the dispersion from the tank to a defibrator, or for transporting the dispersion of chemically modified cellulose defibrated by the defibrator, and is not particularly limited. Among these, it is particularly preferable to use it for transfer in the dehydration / washing process and for transfer in the defibration process. Among the transfers in the defibration process, it is particularly preferable to use it when transferring a dispersion of chemically modified cellulose or a dispersion of fine fibrous cellulose to the defibrator. Note that the treatment with the defibrator may be performed multiple times, and in the first treatment, a dispersion of chemically modified cellulose is transferred to the defibrator, but in the second and subsequent treatments, the dispersion contains defibrated fine fibrous cellulose and undefibrated or partially defibrated chemically modified cellulose. EXAMPLES

[0118] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0119] The raw material, cellulose fiber, was softwood kraft pulp (solid content 93% by mass, basis weight 245 g / m) manufactured by Oji Paper Co., Ltd. 2 A sheet-like product with a Canadian Standard Freeness (CSF) of 700 mL when disintegrated and measured in accordance with JIS P 8121-2:2012 was used.

[0120] The cellulose fibers were subjected to phosphorus oxo-oxidation treatment as follows. First, a mixed aqueous solution of ammonium dihydrogen phosphate and urea was added to 100 parts by mass (bone dry mass) of the cellulose fibers to adjust the composition to 45 parts by mass of ammonium dihydrogen phosphate, 120 parts by mass of urea, and 150 parts by mass of water, to obtain a chemical-impregnated pulp. Next, the obtained chemical-impregnated pulp was heated in a hot air dryer at 165°C for 250 seconds to introduce phosphoric acid groups into the cellulose fibers, and a phosphorylated pulp, which is a chemically modified cellulose, was obtained.

[0121] The resulting chemically modified cellulose (phosphorylated pulp) was then washed by pouring 20 L of ion-exchanged water into 400 g (bone dry weight) of phosphorylated pulp to obtain a pulp dispersion, stirring the resulting pulp to uniformly disperse the pulp, and then pumping the resulting solution to a vacuum dehydrator at a flow rate of 10 L / min using a Watson-Marlow SPS sine pump, and repeatedly filtering and dehydrating the solution.

[0122] Next, the washed phosphorylated pulp was subjected to neutralization treatment as follows: First, 15 L of a 1.0% by mass aqueous sodium hydroxide solution was poured onto the washed phosphorylated pulp, which was then dehydrated, and 30 L of ion-exchanged water was poured in again, followed by dehydration, to wash away excess sodium hydroxide and obtain neutralized phosphorylated pulp.

[0123] The infrared absorption spectrum of the phosphorylated pulp was measured using FT-IR. -1 Absorption due to the P=O of the phosphate group was observed near the 2θ=14° to 17° position, and it was confirmed that the phosphate group was added to the pulp. In addition, when the obtained phosphorylated pulp was analyzed using an X-ray diffraction device, typical peaks were confirmed at two positions, near 2θ=14° to 17° and near 2θ=22° to 23°, and it was confirmed that it had cellulose type I crystals. The amount of phosphate groups (amount of first dissociated acid) measured by the measurement method described later in [Measurement of the amount of phosphorus oxo acid groups] was 1.6 mmol / g.

[0124] <Example 1> Ion-exchanged water was added to the obtained phosphorylated pulp to prepare a slurry with a solid content concentration of 2% by mass (preparation step). The slurry was placed in a 10 L hopper, and the flow rate was adjusted to a discharge pressure of 0.4 MPa or more using a Watoson-Marlow Co., Ltd. sine pump SPS model, and the liquid was sent to a wet pulverizer (Starburst, Sugino Machine Co., Ltd.). The pressure of the wet pulverizer was set to 200 MPa, and the treatment was carried out twice to obtain a fine fibrous cellulose dispersion 1 containing fine fibrous cellulose. The treatment speed of the wet pulverizer was 30 L / h. The viscosity measured by the measurement method described later in [Measurement of viscosity of 0.4% by mass fine fibrous cellulose dispersion] was 33,000 mPa·s.

[0125] <Comparative Example 1> Ion-exchanged water was added to the obtained phosphorylated pulp to prepare a slurry with a solid content concentration of 2% by mass (preparation step). The slurry was placed in a 10 L hopper, and the flow rate was adjusted to a discharge pressure of 0.4 MPa or more using a twin-screw pump SQ type manufactured by Futora Metal Industries Co., Ltd., and the liquid was sent to a wet type pulverizer (Starburst manufactured by Sugino Machine Co., Ltd.). The pressure of the wet type pulverizer was set to 200 MPa, and the treatment was carried out twice to obtain a fine fibrous cellulose dispersion 2 containing fine fibrous cellulose. The treatment speed of the wet type pulverizer was 30 L / h. The viscosity measured by the measurement method described later in [Measurement of viscosity of 0.4% by mass fine fibrous cellulose dispersion] was 27,000 mPa·s.

[0126] <Measurement> [Measurement of phosphorus oxoacid group content] The amount of phosphorus oxoacid groups in the fine fibrous cellulose was measured by treating a fibrous cellulose-containing slurry with an ion exchange resin after diluting a fine fibrous cellulose dispersion containing the target fine fibrous cellulose with ion exchange water to a content of 0.2 mass%, and then titrating the slurry with an alkali. Treatment with ion exchange resin was carried out by adding 1 / 10 by volume of a strongly acidic ion exchange resin (Amberjet 1024; Organo Corporation, conditioned) to the above fibrous cellulose-containing slurry, shaking for 1 hour, and then pouring onto a mesh with 90 μm openings to separate the resin and the slurry. The titration using alkali was performed by adding 10 μL of 0.1N sodium hydroxide solution every 5 seconds to the fibrous cellulose-containing slurry after the ion exchange resin treatment, while measuring the change in the pH value of the slurry. Nitrogen gas was blown into the slurry 15 minutes before the start of the titration. In this neutralization titration, two points were observed where the increment (the derivative value of pH with respect to the amount of alkali added) was maximum on the curve plotting the measured pH against the amount of alkali added. Of these, the first maximum point of the increment obtained after the start of the alkali addition is called the first end point, and the second maximum point of the increment obtained next is called the second end point (Figure 1). The amount of alkali required from the start of the titration to the first end point is equal to the amount of first dissociated acid in the slurry used for the titration. The amount of alkali required from the start of the titration to the second end point is equal to the total amount of dissociated acid in the slurry used for the titration. The amount of alkali (mmol) required from the start of titration to the first end point was divided by the solid content (g) in the slurry to be titrated, and this value was taken as the amount of phosphorus oxoacid groups (mmol / g).

[0127] [Measurement of viscosity of 0.4% by mass fine fibrous cellulose dispersion] The viscosity of the fine fibrous cellulose dispersion obtained in Example 1 and Comparative Example 1 was measured as follows. First, the fine fibrous cellulose dispersion was diluted with ion-exchanged water so that the solid content concentration was 0.4% by mass, and then stirred in a disperser at 4000 rpm for 5 minutes. The obtained dispersion was subjected to a degassing treatment using a rotation-revolution type super mixer (ARE-250, manufactured by Thinky Corporation). Next, the viscosity of the dispersion thus obtained was measured using a B-type viscometer (analog viscometer T-LVT, manufactured by BLOOKFIELD). The measurement conditions were a rotation speed of 3 rpm, and the viscosity value 3 minutes after the start of the measurement was taken as the viscosity of the dispersion.

[0128] From the results of the Examples and Comparative Examples, in Example 1, in which a sine wave pump was used for transportation, the viscosity was 33,000 mPa s, whereas in Comparative Example 1, in which a twin screw pump was used for transportation, the viscosity was 27,000 mPa s. The decrease in viscosity in Comparative Example 1 is believed to have occurred due to unexpected micronization, and it can be said that the quality has changed in Comparative Example 1. In other words, it can be seen that the use of a sine wave pump suppressed the unexpected change in quality. In Example 1, in which a sine pump was used for transportation, the change in quality was suppressed compared to Comparative Example 1, in which a twin-screw pump was used for transportation, and fine fibrous cellulose of higher quality was produced.

Claims

1. A reaction step of chemically modifying cellulose fibers to obtain chemically modified cellulose; a dehydration and washing step of dehydrating and washing the dispersion of the chemically modified cellulose; adjusting the concentration of the dispersion of the chemically modified cellulose; a defibration step of defibrating the dispersion of the chemically modified cellulose by applying a mechanical shear force; A method for producing fine fibrous cellulose comprising the steps of: A sine wave pump is used for transporting the dispersion of the chemically modified cellulose in at least one of the steps. A method for producing fine fibrous cellulose.

2. The method for producing fine fibrous cellulose according to claim 1 , wherein the reaction step is a step of introducing ionic groups into cellulose fibers.

3. The method for producing fine fibrous cellulose according to claim 2, wherein the ionic group is an anionic group.

4. The method for producing fine fibrous cellulose according to claim 3, wherein the anionic group is at least one selected from the group consisting of a phosphorus oxoacid group, a sulfur oxoacid group, and a carboxy group.

5. The method for producing fine fibrous cellulose according to claim 3, wherein the anionic group is a phosphorus oxoacid group.

Citation Information

Patent Citations

  • Method for producing cellulose nano-fiber

    JP2018135421A

  • Method for producing hydrogen gas-containing material and device for producing hydrogen gas-containing material

    WO2018131559A1

  • Method for producing anionically modified cellulose nanofibers

    WO2019059079A1

  • Fine cellulose fiber

    JP2008001728A

  • Method for manufacturing cellulose nano-fiber

    JP2010235679A