Diamond electrode
The diamond electrode with a niobium and carbon-based transition layer enhances adhesion and durability by preventing peeling, ensuring stable performance in acidic environments.
Patent Information
- Application Number
- JP2023057708
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing diamond electrodes suffer from peeling of the conductive diamond film, which compromises their durability, particularly in strong acidic environments.
A diamond electrode with a transition layer composed of microcrystals mainly made of niobium and carbon, and an aggregate of microcrystals mainly composed of niobium and oxygen, is developed to enhance adhesion and durability. This layer includes a porous portion to alleviate thermal expansion differences and a binder effect to prevent peeling.
The solution effectively suppresses peeling of the conductive diamond film, improving the electrode's durability and maintaining performance even in strongly acidic conditions.
Smart Images

Figure 2024145384000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a diamond electrode. [Background technology]
[0002] Conductive diamond has a wide potential window in both aqueous and non-aqueous systems and a small background current, making it known as an electrode material capable of stable electrochemical reactions over a wide potential range.
[0003] For example, Patent Document 1 discloses a method for producing a conductive diamond electrode, which comprises plastically processing at least the surface of an electrode substrate comprising a material selected from a valve metal selected from the group consisting of niobium, tantalum, titanium, and zirconium, and a metal-based alloy thereof, and then heat-treating the electrode substrate in a vacuum or in an inert atmosphere, and forming a conductive diamond film on the heat-treated surface of the electrode substrate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 4456378 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a technique capable of suppressing peeling of a conductive diamond film and improving the durability of a diamond electrode. [Means for solving the problem]
[0006] According to one aspect of the present invention, A substrate made of metal niobium; a conductive diamond film formed on at least one of the main surfaces of the substrate; a transition layer formed between the substrate and the conductive diamond film; A diamond electrode is provided, in which the transition layer is composed of microcrystals mainly composed of niobium and carbon, and an aggregate of microcrystals mainly composed of niobium and oxygen. Effect of the Invention
[0007] According to the present invention, a technique can be provided that can suppress peeling of the conductive diamond film and improve the durability of the diamond electrode. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic diagram showing a cross section of a diamond electrode 10 according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged schematic diagram of the vicinity of the boundary between the transition layer 30 and the conductive diamond film 40 of the diamond electrode 10 according to the embodiment of the present invention. [Diagram 3] FIG. 3 is a flowchart showing an example of a method for manufacturing the diamond electrode 10 according to the embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram illustrating the porous portion forming step S102 according to the embodiment of the present invention. [Diagram 5] FIG. 5 is a flow chart showing an example of a method for manufacturing a diamond electrode 10 according to another embodiment of the present invention. [Figure 6] FIG. 6 is a cross-sectional photograph of Sample 1 according to an embodiment of the present invention. [Figure 7] FIG. 7 is a diagram showing the results of composition analysis of Sample 1 according to the embodiment of the present invention by TEM-EDX. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Inventor's findings> First, the findings of the inventors will be described.
[0010] Diamond electrodes that are made conductive by including boron or the like can be used to generate oxidizing agents such as ozone. Durability is a major issue for such diamond electrodes. Although the technology described in Patent Document 1 and the like has improved the adhesion and peel strength between the substrate and the diamond film, it has been found that it is difficult to obtain a practical level of durability.
[0011] For example, paragraph 0009 of Patent Document 1 states that "if the intermediate layer is made of carbide derived from the substrate, it is expected that the adhesion of the diamond film will be improved due to the relationship between the substrate, the carbide growing from the substrate, and the diamond that generates using the carbide as a nucleus. However, in reality, carbides are often inferior in corrosion resistance to oxides when a potential is applied as an anode in strong acidity. Carbide is likely to form in a substrate that comes into contact with hydrocarbon radicals or diamond at high temperatures, so care must be taken when using it as an anode." From the perspective of improving durability, it was thought that it was preferable to prevent carbide from forming as much as possible in the intermediate layer between the substrate and the diamond film.
[0012] The inventors of the present application have conducted extensive research into the above-mentioned problems. As a result, they have found that by forming an intermediate layer (transition layer) consisting of an aggregate of carbide microcrystals and oxide microcrystals, it is possible to suppress the occurrence of pinholes, and furthermore, to suppress the peeling of the diamond film due to the binder effect of the oxide microcrystals. This makes it possible to further improve the durability of the diamond electrode.
[0013] [Details of the embodiment of the present invention] Next, an embodiment of the present invention will be described below with reference to the drawings. Note that the present invention is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.
[0014] <Embodiments of the present invention> (1) Structure of diamond electrode 10 First, the configuration of the diamond electrode 10 of this embodiment will be described. The diamond electrode 10 of this embodiment can be used, for example, as a diamond electrode 10 for electrochemical reactions (for example, for ozone generation). In this case, it is possible to suppress the deterioration of the diamond electrode 10 due to electrical conduction and improve its durability. In addition, it is possible to suppress the peeling of the conductive diamond film 40 and improve the durability of the diamond electrode 10.
[0015] Fig. 1 is a schematic diagram showing a cross section of a diamond electrode 10 of this embodiment. As shown in Fig. 1, the diamond electrode 10 has, for example, a substrate 20, a transition layer 30, and a conductive diamond film 40. The transition layer 30 has a first transition layer 31 and a second transition layer 32.
[0016] The substrate 20 is, for example, a flat niobium metal plate material for depositing the conductive diamond film 40 and for supporting the conductive diamond film 40. The size and thickness of the main surface of the substrate 20 are not particularly limited, but for example, the main surface has a rectangular shape with one side measuring 20 mm or more and 500 mm or less, and the thickness is 0.5 mm or more and 5 mm or less.
[0017] The transition layer 30 is formed, for example, between the substrate 20 and the conductive diamond film 40, and functions as an intermediate layer for increasing the nucleation density of diamond crystals. The transition layer 30 is made up of an aggregate of microcrystals (niobium carbide microcrystals) mainly composed of niobium and carbon, and microcrystals (niobium oxide microcrystals) mainly composed of niobium and oxygen. The presence of the transition layer 30 can efficiently increase the nucleation density of diamond crystals for forming the conductive diamond film 40. In addition, the microcrystals mainly composed of niobium and oxygen exert a binder effect, which can suppress peeling of the conductive diamond film 40.
[0018] The thickness of the transition layer 30 is preferably, for example, 0.5 μm or more and 10 μm or less (more preferably, 0.8 μm or more and 2.5 μm or less). In other words, it is preferable that the minimum thickness and the maximum thickness of the transition layer 30 are within the range of 0.5 μm or more and 10 μm or less (more preferably, 0.8 μm or more and 2.5 μm or less). If the thickness of the transition layer 30 is less than 0.5 μm, it may be difficult to form a continuous transition layer 30. On the other hand, by setting the thickness of the transition layer 30 to 0.5 μm or more, it is easy to form a continuous transition layer 30. On the other hand, if the thickness of the transition layer 30 exceeds 10 μm, the internal stress becomes large and the diamond electrode 10 may be warped. On the other hand, by setting the thickness of the transition layer 30 to 10 μm or less, the internal stress can be reduced and the warping of the diamond electrode 10 can be reduced.
[0019] The conductive diamond film 40 is, for example, a polycrystalline film having conductivity formed on at least one of the main surfaces of the substrate 20 via the transition layer 30. The conductive diamond film 40 may be either a polycrystalline diamond film or a diamond-like carbon (DLC) film. The conductive diamond film 40 may be, for example, a film having 1×10 19 cm -3 More than 1×10 22 cm -3 It is preferable that it is contained at the following concentration: The thickness of the conductive diamond film 40 is, for example, 0.5 μm or more and 10 μm or less, and from the viewpoint of maintaining a balance between durability and cost, it is preferably 1 μm or more and 5 μm or less.
[0020] When the surface of the conductive diamond film 40 is observed, for example, using a scanning electron microscope (for example, magnification 5000 times), it is preferable that there are no pinholes reaching the substrate 20 or the transition layer 30 within a field of view of 20 μm × 20 μm. This reduces the risk that the strongly acidic liquid will come into contact with the substrate 20 or the transition layer 30, even if the diamond electrode 10 is used in a strongly acidic liquid, so it is possible to improve the durability of the diamond electrode 10. From the viewpoint of further improving the durability of the diamond electrode 10, it is more preferable that there are no pinholes reaching the substrate 20 or the transition layer 30 within a field of view of 1 mm × 1 mm, and it is particularly preferable that there are no pinholes on the entire surface of the conductive diamond film 40.
[0021] In addition, even when the cross section (longitudinal or transverse section) of the conductive diamond film 40 is observed, for example, using a scanning electron microscope (for example, 5000 times magnification), it is preferable that there are no pinholes reaching the substrate 20 or the transition layer 30 within a field of view of 20 μm×20 μm. In other words, the conductive diamond film 40 has reduced pinholes not only observed from the surface, but also internal pinholes. This makes it possible to further improve the durability of the diamond electrode 10. It is more preferable that there are no pinholes reaching the substrate 20 or the transition layer 30 within a field of view of 1 mm×1 mm in the cross section (longitudinal or transverse section) of the conductive diamond film 40, and it is particularly preferable that there are no pinholes across the entire cross section of the conductive diamond film 40.
[0022] When the cross section of the diamond electrode 10 is observed, for example, using a scanning electron microscope (for example, magnification 5000 times), it is preferable that a continuous transition layer 30 having a thickness of 0.5 μm or more is formed over a width of 20 μm or more (length in the direction parallel to the main surface of the substrate 20). This sufficiently increases the nucleation density of diamond crystals for forming the conductive diamond film 40, and can suppress the occurrence of pinholes. From the viewpoint of further suppressing the occurrence of pinholes, it is more preferable that a continuous transition layer 30 having a thickness of 0.5 μm or more is formed over a width of 1 mm or more, and it is particularly preferable that a continuous transition layer 30 having a thickness of 0.5 μm or more is formed over the entire main surface of the substrate 20.
[0023] It is preferable that the average composition of niobium in the transition layer 30 continuously decreases from the substrate 20 side to the conductive diamond film 40 side. This makes it possible to suppress peeling of the conductive diamond film 40.
[0024] The microcrystals mainly composed of niobium and carbon contained in the transition layer 30 are preferably niobium carbide microcrystals of the chemical formula NbC (hereinafter also referred to as NbC microcrystals) or niobium carbide microcrystals of the chemical formula Nb2C (hereinafter also referred to as Nb2C microcrystals). This makes it possible to efficiently increase the nucleation density of diamond crystals for forming the conductive diamond film 40.
[0025] It is preferable that the first transition layer 31 has a higher content of NbC microcrystals than the content of Nb2C microcrystals, and the second transition layer 32 has a higher content of Nb2C microcrystals than the content of NbC microcrystals. Since the transition layer 30 is carbonized from the surface side, NbC with a high C content is easily formed in the first transition layer 31, which has a large amount of carbon source 22 diffusing from the surface side, and Nb2C with a high Nb content is easily formed in the second transition layer 32, which has a small amount of carbon source 22 diffusing from the surface side. In this way, the first transition layer 31, which is present on the conductive diamond film 40 side of the transition layer 30, has a large C content compared to the second transition layer 32, which is present on the substrate 20 side, and therefore the nucleation density of diamond crystals for forming the conductive diamond film 40 can be sufficiently increased and the occurrence of pinholes can be suppressed.
[0026] The crystallite diameter of the niobium carbide microcrystals contained in the first transition layer 31 is smaller than the crystallite diameter of the niobium carbide microcrystals contained in the second transition layer 32. Specifically, the crystallite diameter of the niobium carbide microcrystals contained in the first transition layer 31 is, for example, 5 nm or more and 100 nm or less, and the crystallite diameter of the niobium carbide microcrystals contained in the second transition layer 32 is, for example, 10 nm or more and 2000 nm or less. The crystallite diameter of each microcrystal can be measured, for example, by the Scherrer method of XRD. When the first transition layer 31 is measured by XRD, peaks such as NbC(111), NbC(200), NbC(222), and NbC(400) are observed, but the peak of NbC(200) is the strongest. Therefore, in this specification, unless otherwise specified, the crystallite diameter of the niobium carbide microcrystals contained in the first transition layer 31 is calculated from the peak of NbC(200) in XRD. Similarly, the crystallite diameter of the niobium carbide microcrystals contained in the second transition layer 32 is calculated from the peak of Nb2C(211) in XRD. Therefore, in this specification, the crystallite diameter of the niobium carbide microcrystals contained in the first transition layer 31 may be rephrased as the crystallite diameter of the NbC microcrystals, and the crystallite diameter of the niobium carbide microcrystals contained in the second transition layer 32 may be rephrased as the crystallite diameter of the Nb2C microcrystals.
[0027] The crystallite diameter of the NbC microcrystals contained in the first transition layer 31 is, for example, preferably 5 nm or more and 100 nm or less, and more preferably 5 nm or more and 60 nm or less. If the crystallite diameter of the NbC microcrystals is outside the above range, it may be difficult to form a continuous transition layer 30 having a thickness of 0.5 μm or more. In contrast, by setting the crystallite diameter of the NbC microcrystals within the above range, it becomes easier to form a continuous transition layer 30 having a thickness of 0.5 μm or more, and as a result, it becomes easier to suppress the occurrence of pinholes. In addition, the crystallite diameter of the Nb2C microcrystals contained in the second transition layer 32 is, for example, preferably 10 nm or more and 2000 nm or less, and more preferably 20 nm or more and 1000 nm or less.
[0028] The microcrystals mainly composed of niobium and oxygen contained in the transition layer 30 are niobium oxide microcrystals (hereinafter also referred to as NbO microcrystals) of the chemical formula NbO, and it is preferable that the NbO microcrystals are mixed in the first transition layer 31. This enhances the binder effect, and peeling of the conductive diamond film 40 can be further suppressed.
[0029] The crystallite diameter of the NbO microcrystals is, for example, preferably 5 nm or more and 100 nm or less, more preferably 5 nm or more and 60 nm or less. By setting the crystallite diameter of the NbO microcrystals within the above range, the binder effect is more effectively exerted, and the peeling of the conductive diamond film 40 can be further suppressed. The crystallite diameter of the NbO microcrystals can also be measured by the Scherrer method of XRD. When the NbO microcrystals are measured by XRD, peaks such as NbO (100), NbO (110), NbO (111), NbO (200), and NbO (220) are observed, but the peak of NbC (111) is the strongest. Therefore, in this specification, unless otherwise specified, the crystallite diameter of the niobium oxide microcrystals contained in the transition layer 30 is calculated from the peak of NbO (111) of XRD.
[0030] The thickness of the first transition layer 31 is, for example, 10 nm or more and 500 nm or less, and the thickness of the second transition layer 32 is, for example, preferably 1 μm or more and 10 μm or less. The thickness of the second transition layer 32 is preferably 1.5 times or more and 10 times or less the thickness of the first transition layer 31. By setting the thicknesses of the first transition layer 31 and the second transition layer 32 within the above ranges, it is easy to form a continuous transition layer 30 and warping of the diamond electrode 10 can be reduced.
[0031] In the first transition layer 31, the volumetric abundance ratio of NbO microcrystals to NbC microcrystals is preferably, for example, 50% or more and 100% or less (that is, NbO microcrystals are present in an amount equal to or more than half the amount of NbC microcrystals). If the volumetric abundance ratio of NbO microcrystals is less than 50%, the binder effect is insufficient, and it may be difficult to suppress peeling of the conductive diamond film 40. On the other hand, by setting the volumetric abundance ratio of NbO microcrystals to 50% or more, the binder effect is sufficiently exhibited, and peeling of the conductive diamond film 40 can be further suppressed. On the other hand, if the volumetric abundance ratio of NbO microcrystals exceeds 100%, the nucleation density of diamond crystals for forming the conductive diamond film 40 may decrease. On the other hand, by setting the volumetric abundance ratio of NbO microcrystals to 100% or less, the nucleation density of diamond crystals for forming the conductive diamond film 40 can be efficiently increased.
[0032] 2 is an enlarged schematic diagram of the vicinity of the boundary between the transition layer 30 and the conductive diamond film 40. As shown in FIG. 2, the transition layer 30 preferably has a porous portion 33 having a large number of voids. This reduces the difference in thermal expansion coefficient between niobium and the conductive diamond film 40, and suppresses peeling of the conductive diamond film 40. In other words, it is possible to further improve the durability of the diamond electrode 10.
[0033] 2, the porous portion 33 is preferably present in the vicinity of the boundary between the conductive diamond film 40 inside the transition layer 30 (for example, the first transition layer 31). This can further enhance the effect of reducing the difference in thermal expansion coefficient between niobium and the conductive diamond film 40. In this specification, the vicinity of the boundary between the conductive diamond film 40 inside the transition layer 30 means, for example, a region from the boundary between the transition layer 30 and the conductive diamond film 40 to a depth of 1 μm toward the transition layer 30 side.
[0034] The porosity of the porous portion 33 is preferably, for example, 20% or more and 80% or less. If the porosity of the porous portion 33 is less than 20%, it may be difficult to obtain the effect of reducing the thermal expansion coefficient difference. On the other hand, by making the porosity of the porous portion 33 20% or more, it is possible to obtain a sufficient effect of reducing the thermal expansion coefficient difference. On the other hand, if the porosity of the porous portion 33 exceeds 80%, the strength of the diamond electrode 10 may decrease. On the other hand, by making the porosity 80% or less, it is possible to maintain the strength of the diamond electrode 10. In addition, when measuring the porosity of the porous portion 33, for example, the cross section of the porous portion 33 is observed by a scanning electron microscope, and the total area Sv of voids present in any observation field in the porous portion 33 is calculated by image analysis, and the ratio of the total area Sv of voids to the area S of the observation field is taken as the porosity of the porous portion 33.
[0035] (2) Manufacturing method of diamond electrode 10 Next, a description will be given of a manufacturing method of the diamond electrode 10 of this embodiment. As described above, the diamond electrode 10 of this embodiment can be used as a diamond electrode 10 for electrochemical reactions (for example, for generating ozone).
[0036] Fig. 3 is a flow chart showing an example of the manufacturing method of the diamond electrode 10 of this embodiment. As shown in Fig. 3, the manufacturing method of the diamond electrode 10 of this embodiment includes, for example, a porous portion forming step S102, a carbon source embedding step S103, a niobium carbide layer forming step S105, an oxidation step S106, and a diamond film depositing step S107. In this embodiment, the case of manufacturing the diamond electrode 10 from a substrate 20 made of metal niobium will be described.
[0037] (Porous part formation step S102) Fig. 4 is a schematic diagram illustrating the porous portion forming step S102. As shown in Fig. 4, the porous portion forming step S102 is, for example, a step of forming a porous portion 33 having a large number of voids inside at least one of the main surfaces of the substrate 20. By forming the porous portion 33, the voids in the porous portion 33 relieve distortion caused by the difference in thermal expansion coefficient between niobium and the conductive diamond film 40, so that peeling of the conductive diamond film 40 can be suppressed.
[0038] In the porous portion forming step S102, for example, the main surface of the substrate 20 is subjected to plastic deformation (for example, rough surface pressing) to a depth of 1 μm or more, and then the substrate 20 is heat-treated in a hydrogen atmosphere to form the porous portion 33. The purpose of the plastic deformation is to increase the contact area between the niobium surface and hydrogen, and to promote the diffusion of hydrogen by introducing processing strain into the niobium surface. When the substrate 20 is heat-treated in a hydrogen atmosphere, the metal niobium in the region subjected to the plastic deformation becomes embrittled, and then, in the process of cooling to room temperature, microcracks occur in the embrittled metal niobium, and the microcracks progress to become voids. The number and size of the microcracks (or voids) that occur can be controlled by the heat treatment conditions (temperature, time, cooling rate, etc.). From the viewpoint of efficiently forming a large number of voids in the porous portion 33, the substrate 20 may be further subjected to mechanical processing such as pressing after the heat treatment and cooling. The heat treatment conditions in the porous portion forming step S102 are exemplified as follows. Heat treatment temperature (substrate temperature): 600 to 800 degrees Heat treatment time: 30 to 90 minutes Cooling rate: 10~200 degrees / min In addition, the hydrogen that has bonded to metallic niobium by the above-mentioned embrittlement treatment is removed in the niobium carbide layer formation process S105 described below, so that it does not ultimately remain in large quantities in the substrate 20 and does not adversely affect the strength, etc. of the diamond electrode 10.
[0039] In the porous portion forming step S102, it is preferable to form the porous portion 33 so that the porosity of the porous portion 33 is, for example, 20% or more and 80% or less. If the porosity of the porous portion 33 is less than 20%, it may be difficult to obtain the effect of reducing the thermal expansion coefficient difference. In contrast, by setting the porosity of the porous portion 33 to 20% or more, the effect of reducing the thermal expansion coefficient difference can be sufficiently obtained. On the other hand, if the porosity of the porous portion 33 exceeds 80%, the strength of the diamond electrode 10 may decrease. In contrast, by setting the porosity to 80% or less, the strength of the diamond electrode 10 can be maintained.
[0040] The porous portion forming step S102 may be omitted. In this case, the porous portion 33 is not formed, but the subsequent steps can form the transition layer 30 consisting of an aggregate of microcrystals mainly composed of niobium and carbon, and microcrystals mainly composed of niobium and oxygen, so that the nucleation density of diamond crystals for forming the conductive diamond film 40 can be efficiently increased. In addition, the microcrystals mainly composed of niobium and oxygen exert a binder effect, so that the peeling of the conductive diamond film 40 can be suppressed.
[0041] (Carbon source embedding step S103) The carbon source embedding step S103 is a step of embedding a carbon source 22 made of a solid carbon or carbon compound inside the main surface of the substrate 20. Specifically, for example, the carbon source 22 is sprinkled on the surface of the substrate 20 on which the porous portion 33 has been formed by plastic deformation processing, and the surface is rubbed against a substrate 20 of the same size, etc., to embed the carbon source 22 in the surface of the substrate 20 while crushing the carbon source 22 until it has a size similar to the voids of the porous portion 33 (for example, an average particle size of 200 nm or less). Since the carbon source 22 is a solid, it is possible to introduce carbon atoms into the main surface of the substrate 20 at a higher concentration than a hydrocarbon gas or the like. This makes it easier for the carbon atoms to diffuse into the metal niobium, making it easier to form a continuous transition layer 30.
[0042] As the carbon source 22, for example, graphite, boron carbide, diamond powder, etc. can be used. When diamond powder is used as the carbon source 22, at least the outer periphery of the diamond powder is preferably an amorphous layer (sp 2 It is preferable to use diamond powder covered with carbon (carbon). From the viewpoints of increasing the reactivity with metal niobium and reducing costs, it is preferable to use graphite as the carbon source 22.
[0043] The average particle size of the carbon source 22 is preferably 200 nm or less. This makes it easier to embed the carbon source 22 inside the substrate 20. In addition, the surface area of the carbon source 22 is increased, and the reactivity with metal niobium can be improved. The lower limit of the average particle size of the carbon source 22 is not particularly limited, but is, for example, 5 nm or more.
[0044] In the carbon source embedding step S103, when graphite (average particle size 5 to 200 nm) is embedded inside the main surface of the substrate 20 as the carbon source 22, a niobium plate 1 cm 2 It is preferable that the amount of graphite (carbon source 22) used per cm is, for example, 200 μg or more and 1000 μg or less. 2If the amount of the carbon source 22 is less than 200 μg / cm 3 , the carbonization of the metal niobium becomes insufficient, and it may be difficult to form a continuous transition layer 30. 2 If the amount of carbon source 22 used is less than 200 μg / cm, the hydrogen atoms bonded to the metal niobium in the porous portion forming step S102 cannot be completely released, and embrittlement regions may remain, making the diamond film more susceptible to peeling. 2 By setting the amount of carbon source 22 to 1000 μg / cm or more, it is possible to sufficiently carbonize metal niobium, easily form a continuous transition layer 30, and also to remove hydrogen atoms bonded to metal niobium, thereby eliminating embrittled regions of metal niobium. 2 If the amount of carbon source 22 used is more than 1000 μg / cm 2 , a large amount of carbon source 22 will remain after the formation of the transition layer 30, which may adversely affect the deposition of the conductive diamond film 40. 2 or less, it is possible to reduce the amount of residual carbon source 22. Moreover, from the viewpoint of reducing the energy (cost) required for embedding the carbon source 22, it is preferable to embed the carbon source 22 to a depth of 1 μm or less. When checking the carbon source 22 inside the main surface of the substrate 20, for example, a cross-section of the substrate 20 (for example, at a depth of about 1 μm) may be observed using a transmission electron microscope.
[0045] (Niobium carbide layer formation step S105) The niobium carbide layer forming step S105 is a step of forming a niobium carbide layer (which will become the transition layer 30 in a later step) that continuously covers the main surface of the substrate 20 by subjecting the substrate 20 to a heat treatment and reacting the niobium metal with the carbon source 22. This makes it possible to suppress the occurrence of pinholes on the surface of the conductive diamond film 40. In addition, because the niobium carbide layer (transition layer 30) has a porous portion 33, peeling of the conductive diamond film 40 can be suppressed.
[0046] The niobium carbide layer forming step S105 also has the effect of removing hydrogen that has been bonded to metallic niobium by the embrittlement treatment in the porous portion forming step S102 from the substrate 20. In addition, the voids formed in the porous portion forming step S102 can be transformed into a rounded shape by this heat treatment.
[0047] In the niobium carbide layer forming step S105, for example, a hot filament CVD apparatus described below can be used as a heating furnace for heat treatment to form the niobium carbide layer.
[0048] In the niobium carbide layer forming step S105, the heat treatment is preferably performed in an inert atmosphere (for example, a nitrogen atmosphere or a rare gas atmosphere). In an oxidizing atmosphere such as air, the niobium carbide layer may be reduced and converted into a pure niobium layer. In this case, it becomes difficult to uniformly form the conductive diamond film 40. In contrast, by performing the heat treatment in an inert atmosphere, the niobium carbide layer is easily formed, and the conductive diamond film 40 can be formed uniformly.
[0049] The heat treatment conditions in the niobium carbide layer forming step S105 are exemplified as follows. Heat treatment temperature (substrate temperature): 550 to 850 degrees Pressure: 10~50 Torr Heat treatment time: 30 to 120 minutes
[0050] In the niobium carbide layer forming step S105, it is preferable to form the niobium carbide layer so that the crystallite diameter of the NbC crystallites contained in the upper part of the niobium carbide layer (the part that will become the first transition layer 31) is, for example, 1 nm to 100 nm, more preferably 5 nm to 60 nm. This makes it easier to form a continuous niobium carbide layer, making it easier to suppress the occurrence of pinholes. In order to reduce the crystallite diameter of the NbC crystallites contained in the upper part of the niobium carbide layer, it is effective to previously apply plastic deformation processing to the metallic niobium in the region that will become the first transition layer 31 in the porous portion forming step S102 to reduce the crystallite diameter of the metallic niobium.
[0051] (Oxidation step S106) The oxidation step S106 is a step in which the substrate 20 is heat-treated in an atmosphere containing an oxidizing gas, and the metallic niobium (or niobium carbide) of the niobium carbide layer is reacted with oxygen atoms to introduce niobium oxide microcrystals into a part of the niobium carbide layer, and the niobium carbide layer becomes the transition layer 30. Specifically, after the niobium carbide layer forming step S105 is performed in an inert atmosphere, oxygen gas or carbon dioxide gas is introduced into the heating furnace and heat treatment is performed. As a result, the niobium oxide microcrystals exert a binder effect, so that the peeling of the conductive diamond film 40 can be suppressed. Note that, since the use of carbon dioxide does not rapidly oxidize the niobium surface, and the residual strain on the niobium surface can be suppressed, and the subsequent deposition of the conductive diamond film 40 can be performed well, it is preferable to use carbon dioxide gas in the oxidation step S106.
[0052] In the oxidation step S106, it is preferable to control the heat treatment conditions so that NbO crystallites are introduced into the upper part of the niobium carbide layer (the part that becomes the first transition layer 31). This enhances the binder effect, and further suppresses peeling of the conductive diamond film 40.
[0053] In the oxidation step S106, it is preferable to control the heat treatment conditions so that the volume ratio of NbO microcrystals to NbC microcrystals in the upper part of the niobium carbide layer (the part that becomes the first transition layer 31) is 50% or more and 100% or less. This makes it possible to fully exert the binder effect and further suppress peeling of the conductive diamond film 40. In addition, the nucleation density of diamond crystals for forming the conductive diamond film 40 can be efficiently increased.
[0054] In the oxidation step S106, for example, a hot filament CVD apparatus described below can be used as a heating furnace for heat treatment to form the transition layer 30.
[0055] The conditions for the heat treatment in the oxidation step S106 are exemplified as follows. Heat treatment temperature (substrate temperature): 800 to 1000 degrees Pressure: 750 Torr (atmospheric pressure) Oxygen mole fraction (when using oxygen gas): 0.4 (When carbon dioxide gas is used, the amount of carbon dioxide gas should be adjusted so that the oxygen mole fraction is equivalent to 0.4, taking into consideration the reactivity between niobium and carbon dioxide gas.) Heat treatment time: 30 to 120 minutes
[0056] (Diamond film deposition step S107) The diamond film deposition step S107 is, for example, a step of depositing the conductive diamond film 40 on the main surface of the substrate 20 via the transition layer 30. In this embodiment, since the continuous transition layer 30 is formed in the above-mentioned niobium carbide layer formation step S105 and oxidation step S106, the occurrence of pinholes on the surface of the conductive diamond film 40 can be suppressed. In the diamond film deposition step S107, for example, the conductive diamond film 40 can be deposited using a hot filament CVD apparatus. The hot filament CVD apparatus is configured to be able to supply various gases such as hydrogen gas, carbon-containing gas, and boron-containing gas to the growth chamber. As the carbon-containing gas, methane gas or ethane gas can be used. As the boron-containing gas, trimethylboron (TMB) gas, trimethylborate gas, triethylborate gas, or diborane gas can be used. Specifically, for example, after the inside of the hot filament CVD apparatus is evacuated, hydrogen gas, methane gas, and TMB gas can be introduced to deposit the conductive diamond film 40. Moreover, the hot filament CVD apparatus includes a temperature sensor, a tungsten filament, an electrode (for example, a molybdenum electrode), and the like, in an airtight container formed inside the growth chamber.
[0057] The diamond crystal growth conditions in the diamond film deposition step S107 are exemplified as follows. Heat treatment temperature (substrate temperature): 700 to 1000 degrees Pressure: 5~50 Torr Heat treatment time: 1 to 10 hours
[0058] The above steps make it possible to manufacture the diamond electrode 10. Furthermore, a plurality of diamond electrodes 10 may be combined to manufacture a diamond electrode 10 unit.
[0059] (3) Effects of this embodiment According to this embodiment, one or more of the following advantages are achieved.
[0060] (a) The diamond electrode 10 of this embodiment has a transition layer 30 consisting of microcrystals mainly composed of niobium and carbon, and an aggregate of microcrystals mainly composed of niobium and oxygen. This makes it possible to efficiently increase the nucleation density of diamond crystals for forming the conductive diamond film 40. In addition, the microcrystals mainly composed of niobium and oxygen exert a binder effect, so that peeling of the conductive diamond film 40 can be suppressed.
[0061] (b) In the diamond electrode 10 of this embodiment, it is preferable that the average composition of niobium in the transition layer 30 continuously decreases from the substrate 20 side to the conductive diamond film 40 side. This makes it possible to suppress peeling of the conductive diamond film 40.
[0062] (c) In the diamond electrode 10 of this embodiment, the microcrystals mainly composed of niobium and carbon contained in the transition layer 30 are preferably NbC microcrystals or Nb2C microcrystals. This makes it possible to efficiently increase the nucleation density of diamond crystals for forming the conductive diamond film 40.
[0063] (d) In the diamond electrode 10 of this embodiment, the transition layer 30 has a first transition layer 31 in which the abundance ratio of NbC microcrystals is greater than that of Nb2C microcrystals, and a second transition layer 32 in which the abundance ratio of Nb2C microcrystals is greater than that of NbC microcrystals, and it is preferable that the first transition layer 31 is present on the conductive diamond film 40 side, and the second transition layer 32 is present on the substrate 20 side. The first transition layer 31 present on the conductive diamond film 40 side has a higher C component than the second transition layer 32 present on the substrate 20 side, so that the nucleation density of diamond crystals for forming the conductive diamond film 40 can be sufficiently increased and the occurrence of pinholes can be suppressed.
[0064] (e) In the diamond electrode 10 of this embodiment, the microcrystals mainly composed of niobium and oxygen contained in the transition layer 30 are NbO microcrystals, and it is preferable that the NbO microcrystals are mixed in the first transition layer 31. This enhances the binder effect, and further suppresses peeling of the conductive diamond film 40.
[0065] (f) In the diamond electrode 10 of this embodiment, the crystallite diameter of the NbC microcrystals contained in the first transition layer 31 is, for example, preferably 5 nm or more and 100 nm or less, more preferably 5 nm or more and 60 nm or less. If the crystallite diameter of the NbC microcrystals is outside the above range, it may be difficult to form a continuous transition layer 30 with a thickness of 0.5 μm or more. On the other hand, by setting the crystallite diameter of the NbC microcrystals within the above range, it becomes easier to form a continuous transition layer 30 with a thickness of 0.5 μm or more, and as a result, it becomes easier to suppress the occurrence of pinholes.
[0066] (g) In the diamond electrode 10 of the present embodiment, the crystallite diameter of the NbO microcrystals is, for example, preferably 5 nm or more and 100 nm or less, more preferably 5 nm or more and 60 nm or less. By setting the crystallite diameter of the NbO microcrystals within the above range, the binder effect is more effectively exerted, and the peeling of the conductive diamond film 40 can be further suppressed.
[0067] (h) In the diamond electrode 10 of this embodiment, the thickness of the first transition layer 31 is, for example, 10 nm or more and 500 nm or less, and the thickness of the second transition layer 32 is, for example, 1 μm or more and 10 μm or less. The thickness of the second transition layer 32 is preferably 1.5 times or more and 10 times or less the thickness of the first transition layer 31. By setting the thicknesses of the first transition layer 31 and the second transition layer 32 within the above ranges, it is easy to form a continuous transition layer 30 and the warping of the diamond electrode 10 can be reduced.
[0068] (i) In the diamond electrode 10 of this embodiment, the volumetric abundance ratio of NbO microcrystals to NbC microcrystals in the first transition layer 31 is preferably, for example, 50% or more and 100% or less. If the volumetric abundance ratio of NbO microcrystals is less than 50%, the binder effect is insufficient, and it may be difficult to suppress the peeling of the conductive diamond film 40. On the other hand, by making the volumetric abundance ratio of NbO microcrystals 50% or more, the binder effect is sufficiently exhibited, and the peeling of the conductive diamond film 40 can be further suppressed. On the other hand, if the volumetric abundance ratio of NbO microcrystals exceeds 100%, the nucleation density of diamond crystals for forming the conductive diamond film 40 may decrease. On the other hand, by making the volumetric abundance ratio of NbO microcrystals 100% or less, the nucleation density of diamond crystals for forming the conductive diamond film 40 can be efficiently increased.
[0069] (j) In the diamond electrode 10 of this embodiment, it is preferable to provide a porous portion 33 having a large number of voids near the boundary with the conductive diamond film 40 inside the transition layer 30. This can reduce the difference in thermal expansion coefficient between niobium and the conductive diamond film 40, and suppress peeling of the conductive diamond film 40. In other words, it is possible to further improve the durability of the diamond electrode 10.
[0070] (k) In the diamond electrode 10 of this embodiment, when the surface of the conductive diamond film 40 is observed using, for example, a scanning electron microscope, it is preferable that there are no pinholes reaching the substrate 20 or the transition layer 30 within a field of view of 20 μm×20 μm. As a result, even if the diamond electrode 10 is used in, for example, a strongly acidic liquid, the risk of the strongly acidic liquid coming into contact with the substrate 20 or the transition layer 30 can be reduced, so that the durability of the diamond electrode 10 can be improved. From the viewpoint of further improving the durability of the diamond electrode 10, it is more preferable that there are no pinholes reaching the substrate 20 or the transition layer 30 within a field of view of 1 mm×1 mm, and it is particularly preferable that there are no pinholes on the entire surface of the conductive diamond film 40. Specifically, for example, when the diamond electrode 10 of this embodiment is used as a diamond electrode 10 for generating ozone water, the current deterioration of the diamond electrode 10 can be suppressed and the peeling of the conductive diamond film 40 can be prevented. That is, it is possible to improve the durability of the diamond electrode 10.
[0071] <Other embodiments of the present invention> Although the embodiment of the present invention has been specifically described above, the present invention is not limited to the above-mentioned embodiment, and various modifications can be made without departing from the gist of the present invention.
[0072] FIG. 5 is a flow chart showing an example of a method for manufacturing a diamond electrode 10 according to another embodiment of the present invention. In the above-mentioned embodiment, each step of the method for manufacturing a diamond electrode 10 has been described. For example, as shown in the flow chart of FIG. 5, the unevenness forming step S101 may be performed before the porous portion forming step S102, and the seeding step S104 may be performed before the niobium carbide layer forming step S105. In this case, as in the above-mentioned embodiment, a continuous transition layer 30 may be formed, and pinholes in the conductive diamond film 40 may be suppressed. In addition, peeling of the conductive diamond film 40 may be suppressed. Hereinafter, the unevenness forming step S101 and the seeding step S104 will be described.
[0073] (Irregularity forming step S101) The unevenness forming step S101 is, for example, a step of processing at least one of the main surfaces of the substrate 20 to form uneven undulations. This can suppress peeling caused by the difference in thermal expansion coefficient between the substrate 20 and the conductive diamond film 40. In other words, the peel strength of the diamond electrode 10 can be further improved. In the unevenness forming step S101, it is preferable to form unevenness so that the arithmetic mean roughness Ra (see JIS B0601-2001) of the main surface is 0.5 μm or more and 10 μm or less. For the processing to form unevenness, for example, known methods such as grinding, blasting, wet etching, dry etching, etc. can be used.
[0074] The unevenness forming step S101 is preferably performed, for example, before the porous portion forming step S102. If a process for forming unevenness is performed on the surface on which the porous portion 33 is formed, there is a possibility that the porous portion 33 will be removed. In contrast, by performing the unevenness forming step S101 before the porous portion forming step S102, the subsequent steps can be performed in a state in which the porous portion 33 remains.
[0075] As in the above embodiment, the unevenness forming step S101 may be omitted. Even if the unevenness forming step S101 is omitted, the transition layer 30 can be formed by performing the niobium carbide layer forming step S105 and the oxidation step S106, and the peeling of the conductive diamond film 40 can be suppressed.
[0076] (Seeding process S104) The seeding step S104 is, for example, a step of seeding diamond particles on the main surface of the substrate 20 (for example, the main surface on which the porous portion 33 is formed). In a typical seeding step S104, diamond particles are attached (seeded) to the surface of the substrate 20 on which the transition layer 30 is formed by a method such as rubbing, immersion, or blasting immediately before the diamond film deposition step S107. By thus interposing diamond particles at the interface between the transition layer 30 and the conductive diamond film 40, the energy barrier required for initial nucleation to form the conductive diamond film 40 can be lowered.
[0077] The seeding step S104 can be carried out, for example, before the formation of the transition layer 30 (i.e., before the niobium carbide layer forming step S105). That is, the seeding step S104 and the above-mentioned carbon source embedding step S103 can be carried out simultaneously. This is made possible by using the same diamond particles as the carbon source 22 used in the carbon source embedding step S103 and the diamond particles used in the seeding step S104. As described above, the carbon source 22 can be sp 2 It is preferable that the diamond structure (sp 3 The core of the structure is surrounded by an amorphous layer (sp 2 The diamond particles (e.g., nanodiamond particles obtained by detonation) covered with sp 2 Carbon is exhausted and sp 3 The core of the structure can be left as seeded diamond particles, which allows the niobium carbide layer formation step S105, the oxidation step S106, and the diamond film deposition step S107 to be performed consecutively in the same apparatus.
[0078] As in the above embodiment, the seeding step S104 may be omitted. Even if the seeding step S104 is omitted, by performing the above carbon source embedding step S103, the main surface of the substrate 20 is continuously covered with the transition layer 30 in the niobium carbide layer forming step S105 and the oxidation step S106, which promotes nucleation when depositing the diamond film, and therefore the occurrence of pinholes in the conductive diamond film 40 can be suppressed.
[0079] In the above embodiment, the carbon source 22 is embedded in the main surface of the substrate 20 in the carbon source embedding step S103. However, the carbon source 22 does not necessarily have to be embedded in the main surface of the substrate 20. For example, by making the crystallite diameter of the metal niobium in the main surface of the substrate 20 sufficiently small (for example, 20 nm or less), a large number of grain boundaries in which crystal defects are densely assembled and arranged can be formed. This ensures a sufficient diffusion path for the carbon source 22 and a sufficiently large surface area of the metal niobium that contributes to the carbonization reaction. Therefore, even if the carbon source 22 is not embedded in the main surface of the substrate 20 and is introduced so as to be in contact with the surface of the substrate 20, the transition layer 30 can be formed. Even if the carbon source 22 is not embedded in the main surface of the substrate 20, it diffuses from the grain boundaries of the metal niobium to the inside, and therefore it is possible to obtain the transition layer 30 having a thickness according to the diffusion length. However, from the viewpoint of facilitating the formation of a continuous transition layer 30 having a sufficient thickness (eg, 0.5 μm or more), it is preferable to embed the carbon source 22 inside the main surface of the substrate 20 as in the above embodiment.
[0080] In the above embodiment, the conductive diamond film 40 has a single layer structure, but the conductive diamond film 40 may have a laminated structure in which a plurality of conductive diamond layers are laminated. However, according to the present invention, even if the conductive diamond film 40 has a single layer structure as in the above embodiment, it is possible to suppress the occurrence of pinholes and the peeling of the conductive diamond film 40. EXAMPLES
[0081] Next, examples of the present invention will be described. These examples are merely examples of the present invention, and the present invention is not limited to these examples.
[0082] (1) Manufacturing of diamond electrode 10 (Sample 1) First, the diamond electrode 10 of Sample 1 was manufactured by the following procedure.
[0083] A substrate 20 made of metal niobium with a size of 50 mm×50 mm and a thickness of 1 mm was prepared, and a main surface was subjected to plastic deformation processing by pressing. Specifically, a cemented carbide die with a rough surface (Ra of about 1 μm) was used, and the surface of the substrate 20 was subjected to plastic deformation processing by pressing at a pressure of 60 t.
[0084] After the plastic deformation process, the substrate 20 was subjected to a heat treatment in a hydrogen atmosphere at 600 degrees for 60 minutes, and then cooled to room temperature to form the porous portion 33. When the porous portion 33 was observed with a scanning electron microscope, the porosity of the porous portion 33 was found to be 70%.
[0085] Graphite (particle size: 1 to 2 μm) was applied as the carbon source 22 at a concentration of approximately 1 mg / cm on the main surface of the substrate 20 on which the porous portion 33 was formed. 2 The amount of graphite embedded in the main surface of the substrate 20 was calculated from the amount of carbon source 22 recovered after the rubbing operation, and the inside of the main surface of the substrate 20 was found to be about 300 μg / cm 2 It was confirmed that graphite (grain size 5 to 70 nm) was embedded in the sintered material.
[0086] In the present examples, the crystallite sizes were calculated from the results of wide-angle X-ray diffraction measurements using an X-ray diffractometer (RINT2500HLB) manufactured by Rigaku Corporation. The measurement conditions were as follows: Measurement wavelength: CuKα (0.15418nm) X-ray output: 50kV-250mA Optical system: Parallel beam with monochromator Divergence slit (DS): 0.5°+10mmH Scattering slit (SS): 0.5° Receiving slit (RS): 0.15 mm Scan axis: 2θ / θ Scanning method: Continuous scanning Scanning range: 5°≦2θ≦100° Scanning speed: 0.5° / min Sampling: 0.01°
[0087] The substrate 20 with the graphite embedded therein was placed in a hot filament CVD apparatus, and the formation of the transition layer 30 (niobium carbide layer formation step S105 and oxidation step S106) and the deposition of the conductive diamond film 40 (diamond film deposition step S107) were performed continuously. Specifically, nitrogen gas was introduced, the pressure was set to 20 to 50 Torr, and the substrate temperature was held at 600 to 700°C for 60 minutes to form the niobium carbide layer. Next, carbon dioxide gas was introduced, and the substrate temperature was held at 800°C for 60 minutes at atmospheric pressure (equivalent to oxygen molar partial pressure of 0.4), to form the transition layer 30. After that, the inside of the apparatus was evacuated to remove the oxidizing gas, and then methane gas was introduced and a voltage (120 to 150 V) was applied to the 40 cm filament, and the filament was carbonized and held until the resistance became constant. Thereafter, hydrogen gas, methane gas, and TMB gas were introduced, the pressure was set to 20 to 50 Torr, the filament voltage was increased to 175 V, and the filament temperature was kept at 2200 to 2400°C and the substrate temperature was kept at 700 to 800°C for 180 minutes to deposit a conductive diamond film 40.
[0088] The diamond electrode 10 was removed from the hot filament CVD apparatus, and it was confirmed that a conductive diamond film 40 with a thickness of 3.21 μm had been deposited. In addition, when the diamond electrode 10 was measured by XRD from the conductive diamond film 40 side, the crystallite diameter of niobium carbide (NbC) was 30.8 nm, and the crystallite diameter of niobium oxide (NbO) was 43.4 nm.
[0089] (Sample 2) Moreover, the diamond electrode 10 of Sample 2 was manufactured by the following procedure.
[0090] A substrate 20 made of metal niobium was prepared, and similarly to sample 1, a main surface was subjected to plastic deformation processing by pressing.
[0091] After the plastic deformation process, the main surface of the substrate 20 was subjected to a heat treatment in a hydrogen atmosphere at 600 degrees for 60 minutes, and then cooled to room temperature to form the porous portion 33. When the porous portion 33 was observed with a scanning electron microscope, the porosity of the porous portion 33 was 68%.
[0092] In sample 2, the carbon source 22 was not embedded, and the surface of the substrate 20 on which the porous portion 33 was formed was seeded by applying a suspension containing fine diamond powder, and then sufficiently dried. The substrate 20 was then placed in a hot filament CVD apparatus, and heat-treated under the same conditions as in sample 1, to deposit a conductive diamond film 40.
[0093] The diamond electrode 10 was taken out of the hot filament CVD apparatus, and it was confirmed that a conductive diamond film 40 with a thickness of 2.72 μm had been deposited thereon.
[0094] (Sample 3) Moreover, the diamond electrode 10 of Sample 3 was manufactured by the following procedure.
[0095] A substrate 20 made of metal niobium was prepared, and similarly to sample 1, a main surface was subjected to plastic deformation processing by pressing.
[0096] In sample 3, the porous portion 33 was not formed, and graphite (grain size 1 to 2 μm) was applied as the carbon source 22 at a concentration of 1 mg / cm on the main surface of the substrate 20 that had been subjected to plastic deformation processing. 2 The amount of embedded graphite was measured before and after embedding, and the inside of the main surface of the substrate 20 contained 50 μg / cm 2 It was confirmed that graphite (grain size 5 to 70 nm) was embedded in the sintered material.
[0097] The substrate 20 after grinding was placed in a hot filament CVD apparatus, and under the same conditions as those for sample 1, the formation of the transition layer 30 and the deposition of the conductive diamond film 40 were carried out successively.
[0098] The diamond electrode 10 was removed from the hot filament CVD apparatus, and it was confirmed that a conductive diamond film 40 with a thickness of 2.94 μm had been deposited. In addition, when the diamond electrode 10 was measured by XRD from the conductive diamond film 40 side, the crystallite diameter of the niobium carbide was 49.0 nm, and the crystallite diameter of the niobium oxide was 38.7 nm.
[0099] (Sample 4) Moreover, the diamond electrode 10 of Sample 4 was manufactured by the following procedure.
[0100] The porous portion 33 was formed and the carbon source 22 was embedded under the same conditions as those of Sample 1. Thereafter, the substrate 20 was placed in a hot filament CVD apparatus, and the formation of the niobium carbide layer and the deposition of the conductive diamond film 40 were performed consecutively. That is, in Sample 4, the oxidation step S106 was not performed, and NbO microcrystals were not introduced into a part of the niobium carbide layer. The formation of the niobium carbide layer and the deposition of the conductive diamond film 40 were performed under the same conditions as those of Sample 1.
[0101] (2) Evaluation of diamond electrodes 10 The cross sections of Samples 1 to 4 were observed using a scanning electron microscope (SEM). In Sample 2, in which the carbon source 22 was not embedded, niobium carbide formed in islands was observed at the interface between the substrate 20 and the conductive diamond film 40, and no continuous transition layer 30 was formed. In contrast, in Samples 1 and 3, in which the carbon source 22 was embedded inside the main surface of the substrate 20, it was confirmed that a continuous transition layer 30 was formed at the interface between the substrate 20 and the conductive diamond film 40. In Sample 4, it was confirmed that a continuous niobium carbide layer was formed at the interface between the substrate 20 and the conductive diamond film 40. It was also confirmed that the transition layer 30 of Sample 1 and the niobium carbide layer of Sample 4 had a porous portion 33 near the boundary with the conductive diamond film 40. A cross-sectional photograph of Sample 1 is shown in FIG. 6.
[0102] Furthermore, the surface of the conductive diamond film 40 of Samples 1 to 4 was observed using an SEM. In Sample 2 in which the carbon source 22 was not embedded, pinholes were observed on the surface of the conductive diamond film 40. In contrast, in Samples 1, 3, and 4 in which the carbon source 22 was embedded inside the main surface of the substrate 20, no pinholes were observed on the surface of the conductive diamond film 40.
[0103] From the above, it was confirmed that a continuous transition layer 30 (or a niobium carbide layer) can be formed by embedding the carbon source 22 inside the main surface of the substrate 20. It was also confirmed that the formation of a continuous transition layer 30 (or a niobium carbide layer) can suppress the occurrence of pinholes on the surface of the conductive diamond film 40.
[0104] In addition, composition analysis was performed by TEM-EELS and TEM-EDX on the cross section around the transition layer 30 of sample 1. TEM-EELS confirmed that oxygen was continuously distributed in the transition layer 30 (first transition layer 31) of sample 1. FIG. 7 shows the results of the composition analysis of sample 1 by TEM-EDX. As shown in FIG. 7, it was confirmed that the first transition layer 31 of sample 1 contains oxygen. In other words, it was confirmed that NbO microcrystals are mixed in the first transition layer 31. It was also confirmed that the average composition of niobium in the transition layer 30 continuously decreases from the substrate 20 side to the conductive diamond film 40 side.
[0105] In this example, cross-sectional SEM observation and TEM-EELS and TEM-EDX compositional analysis were performed according to the following procedures. (a) A sample containing the area to be observed was cut to an appropriate size using a low-speed rotating diamond cutter. (b) The sample in (a) was embedded in epoxy resin and cured by heating at 120°C for 1 hour in an atmospheric oven. (c) The cross section of the sample (b) near the observation target area was roughened using a rotary polisher, and then buffed using polishing diamond paste (grain size 0.3 μm). (d) The cross section near the target observation area was finished using an ion milling device, ArBlade5000, manufactured by Hitachi High-Technologies Corporation. This resulted in a flat observation surface, making it easier to observe the fine structure. (e) The sample (d) was subjected to a conductive treatment using a Pt sputter coating device manufactured by JEOL Ltd. (f) SEM observation was performed on the sample in (e). The accelerating voltage during observation was 5 kV. The SEM used was a Hitachi High-Tech S-4800. (g) Thin film samples for TEM observation were prepared for the samples observed with the SEM in (f). The thin film samples were processed using the focused ion beam (FIB) method. The equipment used was the NB5000 manufactured by Hitachi High-Technologies Corporation. The processing conditions were an accelerating voltage of 40 kV. The thin film samples in (h) and (g) were subjected to TEM observation and elemental analysis by TEM-EELS and TEM-EDX. The TEM equipment used was a Hitachi High-Tech HD-2700 with an accelerating voltage of 200 kV. For TEM-EELS, an EELS equipment (GATAN Enfinium) manufactured by Ametech was used. For TEM-EDX, an EDX equipment (EDAX Octane T Ultra W) manufactured by Ametech was used.
[0106] (3) Durability test of diamond electrode 10 A durability test was conducted to generate ozone water using the diamond electrodes 10 of samples 1 to 4 as the anode and cathode, respectively. The durability test was conducted by using tap water (flow rate 200 mL / min) as the raw water, driving the anode and cathode fixed with a polymer electrolyte membrane between them at a voltage drive of 12 V for 1 minute and resting for 4 minutes, and repeating this cycle 10,000 times. The polymer electrolyte membrane used was Nafion324 (manufactured by Du Pont). The results of checking the current values and the generated ozone water concentrations before and after the above 10,000 cycles, as well as the area ratio of peeled off conductive diamond film 40 after 10,000 cycles, are shown in Table 1.
[0107] [Table 1]
[0108] As shown in Table 1, in sample 2 in which the carbon source 22 was not embedded, the ozone water concentration at 10,000 cycles was significantly lower than that at the first cycle, and degradation due to current flow was confirmed, and extensive peeling of the conductive diamond film 40 was confirmed. In addition, in sample 3 in which the porous portion 33 was not formed, a decrease in the ozone water concentration at 10,000 cycles was observed, and partial peeling of the conductive diamond film 40 was confirmed. In addition, in sample 4 in which the NbO microcrystals were not introduced, a decrease in the ozone water concentration at 10,000 cycles was observed, and partial peeling of the conductive diamond film 40 was confirmed. In contrast, in sample 1 in which the porous portion 33 was formed, the carbon source 22 was embedded inside the main surface of the substrate 20, and the NbO microcrystals were introduced, the ozone water concentration at the first cycle was higher than that of samples 2 to 4, and an ozone water concentration at the 10,000 cycles was similar to that at the first cycle (90% or more at the first cycle). In addition, almost no peeling of the conductive diamond film 40 was confirmed.
[0109] From the above, it was confirmed that by forming the transition layer 30 consisting of microcrystals mainly composed of niobium and carbon, and an aggregate of microcrystals mainly composed of niobium and oxygen, it is possible to suppress electrical deterioration and prevent peeling of the conductive diamond film 40. In other words, it was confirmed that the durability of the diamond electrode 10 can be improved. In addition, it was confirmed that the durability of the diamond electrode 10 can be further improved by forming the porous portion 33 in the transition layer 30.
[0110] <Preferred embodiment of the present invention> Preferred embodiments of the present invention will be described below.
[0111] (Appendix 1) According to one aspect of the present invention, a conductive diamond film formed on at least one of the main surfaces of the substrate; a transition layer formed between the substrate and the conductive diamond film; A diamond electrode is provided, in which the transition layer is composed of microcrystals mainly composed of niobium and carbon, and an aggregate of microcrystals mainly composed of niobium and oxygen.
[0112] (Appendix 2) 2. The diamond electrode according to claim 1, The average composition of niobium in the transition layer continuously decreases from the substrate side to the conductive diamond film side.
[0113] (Appendix 3) 2. The diamond electrode according to claim 1, The niobium and carbon based crystallites are niobium carbide crystallites of the formula NbC or Nb2C.
[0114] (Appendix 4) 4. The diamond electrode according to claim 3, The transition layer has a first transition layer in which the abundance ratio of niobium carbide microcrystals of the chemical formula NbC is greater than the abundance ratio of niobium carbide microcrystals of the chemical formula Nb2C, and a second transition layer in which the abundance ratio of niobium carbide microcrystals of the chemical formula Nb2C is greater than the abundance ratio of niobium carbide microcrystals of the chemical formula NbC, The first transition layer is present on the conductive diamond film side, and the second transition layer is present on the substrate side.
[0115] (Appendix 5) 5. The diamond electrode according to claim 4, The microcrystals containing niobium and oxygen as main components are niobium oxide microcrystals having a chemical formula of NbO, and the niobium oxide microcrystals are mixed in the first transition layer.
[0116] (Appendix 6) 5. The diamond electrode according to claim 4, The crystallite diameter of the niobium carbide microcrystals of the chemical formula NbC contained in the first transition layer is 5 nm or more and 100 nm or less, and the crystallite diameter of the niobium carbide microcrystals of the chemical formula Nb2C contained in the second transition layer is 10 nm or more and 2000 nm or less.
[0117] (Appendix 7) 6. The diamond electrode according to claim 5, The crystallite size of the niobium oxide microcrystals of the chemical formula NbO is 5 nm or more and 100 nm or less.
[0118] (Appendix 8) 5. The diamond electrode according to claim 4, The first transition layer has a thickness of 10 nm to 500 nm, and the second transition layer has a thickness of 1 μm to 10 μm.
[0119] (Appendix 9) 6. The diamond electrode according to claim 5, In the first transition layer, the volumetric abundance ratio of the niobium oxide microcrystals having the chemical formula NbO to the niobium carbide microcrystals having the chemical formula NbC is 50% or more and 100% or less.
[0120] (Appendix 10) 2. The diamond electrode according to claim 1, A porous portion having voids is present within the transition layer near the boundary with the conductive diamond film.
[0121] (Appendix 11) 11. A diamond electrode according to any one of claims 1 to 10, When the surface of the conductive diamond film is observed using a scanning electron microscope, no pinholes reaching the substrate or the transition layer are present within a field of view of 20 μm×20 μm. Preferably, there are no pinholes within a 1 mm x 1 mm field of view that reach down to the substrate or the transition layer. It is particularly preferable that the entire surface of the conductive diamond film is free of pinholes reaching the substrate or the transition layer. [Explanation of symbols]
[0122] 10 Diamond electrode 20 Substrate 22 Carbon Source 30 Transition layer 31 1st transition layer 32 Second transition layer 33 Porous part 40 Conductive diamond film S101 Irregularity forming process S102 Porous part formation process S103 Carbon source embedding process S104 Seeding process S105 Niobium carbide layer formation process S106 Oxidation process S107 Diamond film deposition process
Claims
1. A substrate made of metal niobium; a conductive diamond film formed on at least one of the main surfaces of the substrate; a transition layer formed between the substrate and the conductive diamond film; The diamond electrode, wherein the transition layer is composed of microcrystals mainly composed of niobium and carbon, and an aggregate of microcrystals mainly composed of niobium and oxygen.
2. 2. The diamond electrode according to claim 1, wherein the average composition of niobium in the transition layer decreases continuously from the substrate side to the conductive diamond film side.
3. The niobium and carbon-based microcrystals have the chemical formula NbC or Nb 2 The diamond electrode according to claim 1, which is a niobium carbide microcrystal of C.
4. The transition layer has a niobium carbide crystallite content of NbC, the content of which is Nb 2 A first transition layer having a higher content of niobium carbide microcrystals than that of C, and a chemical formula of Nb 2 A second transition layer in which the proportion of niobium carbide crystallites of formula C is greater than the proportion of niobium carbide crystallites of formula NbC; The diamond electrode according to claim 3 , wherein the first transition layer is present on the conductive diamond film side, and the second transition layer is present on the substrate side.
5. The diamond electrode according to claim 4, wherein the microcrystals mainly composed of niobium and oxygen are niobium oxide microcrystals having the chemical formula NbO, and the niobium oxide microcrystals are mixed in the first transition layer.
6. The crystallite size of the niobium carbide microcrystals of the chemical formula NbC contained in the first transition layer is 5 nm or more and 100 nm or less, and the crystallite size of the niobium carbide microcrystals of the chemical formula NbC contained in the second transition layer is 5 nm or more and 100 nm or less. 2 The diamond electrode according to claim 4, wherein the crystallite size of the niobium carbide microcrystals of C is 10 nm or more and 2000 nm or less.
7. The diamond electrode according to claim 5, wherein the crystallite size of the niobium oxide microcrystals of the chemical formula NbO is 5 nm or more and 100 nm or less.
8. The diamond electrode according to claim 4, wherein the thickness of the first transition layer is 10 nm or more and 500 nm or less, and the thickness of the second transition layer is 1 μm or more and 10 μm or less.
9. The diamond electrode according to claim 5, wherein the volumetric abundance ratio of the niobium oxide microcrystals of the chemical formula NbO to the niobium carbide microcrystals of the chemical formula NbC in the first transition layer is 50% or more and 100% or less.
10. 2. The diamond electrode according to claim 1, wherein a porous portion having voids is present inside the transition layer near the boundary with the conductive diamond film.
11. A diamond electrode described in any one of claims 1 to 10, wherein when the surface of the conductive diamond film is observed using a scanning electron microscope, there are no pinholes reaching the substrate or the transition layer within a field of view of 20 μm x 20 μm.
Citation Information
Patent Citations
BDD membrane electrode material and preparation method thereof
CN108486546A
Boron doped diamond electrode and preparation method thereof
CN109750291A
JP1973099080A
Electrode for electrolysis and electrolytic cell using this electrode
JP1997268395A
Electrically conductive diamond electrode and its production method