Resin composition for fiber, and ethylenic fiber using the same

A linear ethylene ionomer resin composition addresses the adhesion and performance issues of conventional polyethylene and ethylene-based ionomers by providing fibers with high-speed spinnability, impact strength, and strong adhesion to polar materials.

JP2024145495APending Publication Date: 2024-10-15JAPAN POLYETHYLENE CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023057870
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional polyethylene resins lack polar groups, leading to poor adhesion with materials like polyethylene terephthalate and polyamide, and fibers produced from ethylene-based ionomers with irregular long and short chain branches have difficulty in achieving high-speed spinnability and impact resistance.

Method used

A resin composition using a substantially linear ethylene ionomer with specific structural units and metal-containing carboxylates, allowing for fibers with improved adhesion to polar materials and enhanced spinnability and impact strength.

Benefits of technology

The fibers exhibit high-speed spinnability, excellent impact strength, and strong adhesion to diverse resins, surpassing the limitations of conventional polyethylene and ethylene-based ionomers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145495000022
    Figure 2024145495000022
  • Figure 2024145495000001
    Figure 2024145495000001
  • Figure 2024145495000002
    Figure 2024145495000002
Patent Text Reader

Abstract

To provide a fiber and a resin composition for a fiber which are excellent in high speed spinning property and impact strength, and have excellent adhesive performances to a dissimilar material having high polarity.SOLUTION: A resin composition for a fiber contains a linear ethylene ionomer which is an ionomer having a phase angle δ at an absolute value G*=0.1 MPa of complex elastic modulus measured by a rotary type rheometer of 50 to 75 degrees.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber resin composition using a novel ethylene-based ionomer, and an ethylene-based fiber using the same. More specifically, the present invention relates to an ethylene-based fiber having excellent adhesion to different resins, high-speed spinnability, and impact resistance. [Background technology]

[0002] Conventional polyethylene resins such as high-density polyethylene and low-density polyethylene can satisfy the required performance in terms of high-speed spinnability and impact resistance if an appropriate resin is selected. However, since conventional polyethylene resins do not have polar groups, there is a problem that they do not have adhesion to resins that have polar groups, such as polyethylene terephthalate and polyamide, making it difficult to form composites.

[0003] Ethylene-based ionomers are resins that use ethylene-unsaturated carboxylic acid copolymers as a base resin and are intermolecularly bonded with metal ions such as sodium and zinc. They are strong, elastic, flexible, abrasion-resistant, and transparent (Patent Document 1). Known commercially available ionomers include sodium and zinc salts of ethylene-methacrylic acid copolymers "PRIMACOR (registered trademark)" sold by SK Chemicals, and "Himilan (registered trademark)" sold by Dow Mitsui Polychemicals.

[0004] Specifically, the ethylene-unsaturated carboxylic acid copolymer used in the conventionally known ethylene-based ionomer is a polar group-containing olefin copolymer obtained by polymerizing ethylene and a polar group-containing monomer such as (meth)acrylic acid by high-pressure radical polymerization. However, the molecular structure of the polar group-containing olefin copolymer produced by high-pressure radical polymerization has many long chain branches and short chain branches irregularly, as shown in the image of Figure 1, and problems include the difficulty of high-speed spinning and low impact resistance.

[0005] Meanwhile, another method for producing a polar-group-containing olefin copolymer that serves as the base resin of an ethylene-based ionomer has been reported in which a copolymer of ethylene and t-butyl acrylate is produced using a late transition metal catalyst, and the resulting polar-group-containing olefin copolymer is modified into an ethylene-acrylic acid copolymer by heat or acid treatment, and then reacted with metal ions to produce a substantially linear binary ionomer as shown in the image diagram in Figure 2 (Patent Document 2).

[0006] In contrast, conventional polyethylene resins such as high-density polyethylene and low-density polyethylene can satisfy the required performance in terms of high-speed spinnability and impact resistance if an appropriate resin is selected. However, as mentioned above, conventional polyethylene resins do not have polar groups, and therefore have the problem that they do not adhere to resins that have polar groups, such as polyethylene terephthalate and polyamide, making it difficult to form composites. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] U.S. Pat. No. 3,264,272 [Patent Document 2] JP 2016-79408 A Summary of the Invention [Problem to be solved by the invention]

[0008] Although the degree of requirements for fibers (spun fibers used for spinning) varies depending on the application, they are generally required to have various properties, such as being able to be spun at high speed, having high strength, such as knot strength, snag strength, and tensile strength, having impact strength that is difficult to break, having flexibility to bend appropriately when molded into processed products such as cloth and nonwoven fabric, and having good adhesion to different materials when composited, either individually or simultaneously. However, since conventional polyethylene resins are nonpolar, they have no adhesion to polyamides or polyesters, making composites difficult. In addition, the present inventors have found that fibers using ionomers with many long chain branches and short chain branches irregularly obtained by conventional high-pressure radical polymerization methods are insufficient in terms of high-speed spinnability and impact strength.

[0009] In view of the above-mentioned state of the art, an object of the present invention is to provide a fiber and a resin composition for fibers which are excellent in high-speed spinnability, impact strength, and excellent adhesive performance to dissimilar materials having high polarity. [Means for solving the problem]

[0010] Means of the Invention The present inventors have conducted extensive research to solve the above problems and have found that molding fibers using a specific ionomer resin provides fibers with sufficient physical properties to meet the performance requirements of the fibers. The ethylene-based ionomer is a novel ethylene-based ionomer that has not been seen before, in which the base resin has a substantially linear structure and also functions as an ionomer, and its physical properties, etc. are significantly different from those of conventional ethylene-based ionomers having a multi-branched molecular structure, and its specific characteristics and suitable applications are also unknown. The present invention was completed based on the discovery that an ethylene-based fiber obtained by molding a resin composition containing a substantially linear ethylene-based ionomer into a fiber has physical properties that cannot be achieved with conventional polyethylene resins or conventional ionomers.

[0011] That is, according to the present invention [1], there is provided a resin composition for fibers containing a linear ethylene ionomer.

[0012] According to the present invention [2], the linear ethylene ionomer has an absolute complex modulus G measured by a rotational rheometer. * The resin composition for fibers according to [1] above is an ionomer having a phase angle δ of 50 degrees to 75 degrees at a pressure of 0.1 MPa.

[0013] The present invention [3] also provides the resin composition for fibers according to the above [1] or [2], in which the linear ethylene ionomer is a copolymer (P) comprising, as essential constituent units, structural units (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms and structural units (B) derived from a monomer having a carboxy group and / or a dicarboxylic acid anhydride group, and at least a portion of the carboxy groups and / or dicarboxylic acid anhydride groups are converted to a metal-containing carboxylate containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table.

[0014] According to the present invention [4], the copolymer (P) 13 The fiber resin composition according to [3] above is characterized in that the number of methyl branches calculated by C-NMR is 5 or less per 1,000 carbon atoms.

[0015] According to the present invention [5], there is provided the resin composition for fibers according to the above [3] or [4], characterized in that the structural unit (A) is a structural unit derived from ethylene.

[0016] According to the present invention [6], there is provided a resin composition for fibers according to any one of the above [3] to [5], characterized in that the copolymer (P) contains the structural unit (B) in an amount of 2 to 20 mol % (the total of all structural units constituting the copolymer being 100 mol %).

[0017] According to the present invention [7], there is provided the resin composition for fibers according to any one of the above [3] to [6], characterized in that the metal ion is a metal ion of Group 1 of the periodic table.

[0018] According to the present invention [8], there is provided the resin composition for fibers according to any one of the above [3] to [6], characterized in that the metal ion is a metal ion of Group 2 of the periodic table.

[0019] The present invention [9] further provides the resin composition for fibers according to any one of the above [3] to [8], wherein the linear ethylene ionomer further contains, as an essential constituent unit, a structural unit (C) which is a compound having one or more carbon-carbon double bonds in its molecular structure, in addition to the structural unit (A) and the structural unit (B).

[0020] According to the present invention

[10] , there is provided the resin composition for fibers according to [9], characterized in that the structural unit (C) in the copolymer (P) is a non-cyclic monomer represented by the following general formula (1) or a cyclic monomer represented by the following general formula (2): [ka] [In general formula (1), T 1 ~T 3 each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, or a cyano group; T 4 is a substituent selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, or a cyano group. [ka] [In general formula (2), R 1 ~R 12 may be the same or different and are selected from the group consisting of a hydrogen atom, a halogen atom, and a hydrocarbon group having 1 to 20 carbon atoms; R 9 and R 10 , and R 11 and R 12 may combine together to form a divalent organic group, R 9 or R 10 And, R 11 or R 12 may form a ring together. In addition, n represents 0 or a positive integer, and when n is 2 or more, R 5 ~R 8 may be the same or different in each repeating unit.

[0021] According to the present invention

[11] , there is provided the resin composition for fibers according to

[10] , characterized in that the structural unit (C) in the copolymer (P) is a non-cyclic monomer represented by the general formula (1).

[0022] According to the present invention

[12] , there is provided the resin composition for fibers according to

[10] , characterized in that the structural unit (C) in the copolymer (P) is a cyclic monomer represented by the general formula (2).

[0023] According to the present invention

[13] , there is provided a resin composition for fibers according to any one of the above [9] to

[12] , characterized in that the copolymer (P) contains the structural unit (C) in an amount of 0.001 mol % to 20,000 mol % when the total of all structural units constituting the copolymer (P) is taken as 100 mol %.

[0024] According to the present invention

[14] , there is provided a resin composition for fibers according to any one of the above [3] to

[13] , characterized in that the copolymer (P) is a copolymer obtained by hydrolysis of a precursor copolymer produced using a transition metal catalyst containing a transition metal of Groups 8 to 11 of the periodic table.

[0025] According to the present invention

[15] , there is provided the fiber resin composition according to

[14] , characterized in that the transition metal catalyst is a transition metal catalyst comprising a phosphorus sulfonic acid or phosphorus phenol ligand and nickel or palladium.

[0026] According to the present invention

[16] , there is provided an ethylene-based fiber formed using the fiber resin composition according to any one of the above [1] to

[15] .

[0027] According to the present invention

[17] , there is provided an ethylene-based fiber, which is a fiber containing an ethylene-based resin as a resin component, and is characterized in that, when measured using a capillograph under the measurement conditions of a temperature of 190°C, an orifice having a length of 8,000 mm and a hole diameter of 2.085 mm, and a piston speed of 10 mm / min, a maximum take-off speed (MDS) of 100 m / min or more is provided.

[0028] According to the present invention

[18] , there is provided an ethylene-based fiber, which contains an ethylene-based resin as a resin component, and is characterized in that the tensile elongation at break is 100% or more when a 30 dtex fiber is subjected to a tensile test with a chuck distance of 65 mm and a tensile speed of 500 mm / min.

[0029] According to the present invention

[19] , there is provided an ethylene-based fiber, which contains an ethylene-based resin as a resin component, and is characterized in that the breaking energy (E) calculated from the stress-strain curve obtained when a 30 dtex fiber is subjected to a tensile test with a chuck distance of 65 mm and a tensile speed of 500 mm / min is 100 J / mm or more.

[0030] According to the present invention

[20] , there is provided a composite fiber formed using any one of the fiber resin compositions [1] to

[15] above and at least one type of resin other than the fiber resin composition.

[0031] According to the present invention

[21] , there is provided an ethylene-based hollow fiber formed using the fiber resin composition according to any one of the above [1] to

[15] . Effect of the Invention

[0032] Fibers using the ethylene-based ionomer having a substantially linear structure according to the present invention are superior in high-speed spinnability, impact strength, and adhesion to different resins, as compared with existing polyethylene fibers or fibers made of ethylene-based ionomer resins having a hyperbranched structure. [Brief description of the drawings]

[0033] [Figure 1] FIG. 1 is a diagram showing stress-strain curves of Examples 6 to 8 and Comparative Examples 3 and 4. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] The present invention relates to a fiber resin composition containing a linear ethylene ionomer and a resin using the same. In particular, the present invention relates to a fiber using an ionomer characterized in that the base resin is a copolymer (P) which contains, as essential structural units, structural units (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms, and structural units (B) derived from a monomer having a carboxy group and / or a dicarboxylic anhydride group, and optionally also contains, as a structural unit, a structural unit (C) which is a compound having one or more carbon-carbon double bonds in its molecular structure, and which is copolymerized, preferably randomly, in a substantially linear manner, and at least a part of the carboxy group and / or dicarboxylic anhydride group of the structural unit (B) is converted into a metal-containing carboxylate containing at least one metal ion selected from Groups 1, 2, or 12 of the periodic table.

[0035] The ionomer of the present invention will be described in detail below for each item. In this specification, "(meth)acrylic acid" means acrylic acid or methacrylic acid. In this specification, "to" indicating a numerical range is used to mean that the numerical values ​​before and after it are included as the lower and upper limits. In this specification, the copolymer (P) means a binary or higher copolymer containing at least one structural unit (A) and at least one structural unit (B). In this specification, the ionomer also means an ionomer of a ternary or higher copolymer that contains the structural unit (A), a structural unit (B') in which at least a portion of the structural unit (B) is converted to a metal-containing carboxylate, and the structural unit (C), and may further contain the structural unit (B).

[0036] 1. Linear ethylene ionomer The linear ethylene ionomer of the present invention refers to an ethylene ionomer in which an ethylene copolymer, which is the basic structure of the ethylene ionomer before neutralization with ions, has a linear molecular structure and is ionomerized. Specifically, the copolymer (P) contains, as a base resin, a structural unit (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms, and a structural unit (B) derived from a monomer having a carboxy group and / or a dicarboxylic anhydride group, as essential structural units, and optionally also contains a structural unit (C) which is a compound having one or more carbon-carbon double bonds in its molecular structure, and these are copolymerized, preferably randomly, in a substantially linear manner, and is characterized in that at least a portion of the carboxy group and / or dicarboxylic anhydride group of the structural unit (B) is converted to a metal-containing carboxylate containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table.

[0037] (1) Structural unit (A) The structural unit (A) is derived from one or more monomers selected from ethylene and α-olefins having 3 to 20 carbon atoms. The α-olefins of the present invention have the structural formula: CH2=CHR1 is an α-olefin having 3 to 20 carbon atoms (R 1 is a hydrocarbon group having 1 to 18 carbon atoms, which may have a linear structure or may be branched.) The α-olefin more preferably has 3 to 12 carbon atoms.

[0038] Specific examples of the structural unit (A) include structural units derived from ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 3-methyl-1-butene, and 4-methyl-1-pentene, and may be a structural unit derived from ethylene. The structural unit (A) may be of one type or of multiple types. Combinations of the two types include structural units derived from ethylene-propylene, ethylene-1-butene, ethylene-1-hexene, ethylene-1-octene, propylene-1-butene, propylene-1-hexene, and propylene-1-octene. Examples of combinations of the three types include structural units derived from ethylene-propylene-1-butene, ethylene-propylene-1-hexene, ethylene-propylene-1-octene, propylene-1-butene-hexene, and propylene-1-butene-1-octene.

[0039] In the present invention, the structural unit (A) preferably essentially contains a structural unit derived from ethylene, and may further contain, as necessary, one or more structural units derived from an α-olefin having 3 to 20 carbon atoms. The amount of the structural unit derived from ethylene in the structural unit (A) may be 65 to 100 mol % or 70 to 100 mol % based on the total moles of the structural unit (A). From the standpoint of impact resistance, the structural unit (A) may be a structural unit derived from ethylene.

[0040] (2) Structural unit (B) The structural unit (B) is a structural unit derived from a monomer having a carboxy group and / or a dicarboxylic anhydride group.

[0041] Specific examples of monomers having a carboxy group include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, norbornene dicarboxylic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid. Examples of monomers having a dicarboxylic acid anhydride group include maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, 3,6-epoxy-1,2,3,6-tetrahydrophthalic anhydride, and tetracyclo[6.2.1.1 3,6 .0 2,7 ] Unsaturated dicarboxylic acid anhydrides such as dodec-9-ene-4,5-dicarboxylic acid anhydride and 2,7-octadien-1-yl succinic acid anhydride are exemplified. As the structural unit derived from a monomer having a carboxy group and / or a dicarboxylic acid anhydride group, from the viewpoint of industrial availability, preferably, a structural unit derived from acrylic acid, methacrylic acid, or 5-norbornene-2,3-dicarboxylic acid anhydride is mentioned, and in particular, a structural unit derived from acrylic acid may be used. Furthermore, the structural unit derived from a monomer having a carboxy group and / or a dicarboxylic anhydride group may be of one type or of multiple types.

[0042] In addition, the dicarboxylic anhydride group may react with moisture in the air to open the ring and become a part of the dicarboxylic acid, but the dicarboxylic anhydride group may be in a ring-opened state as long as it does not deviate from the gist of the present invention.

[0043] (3) Structural unit (C) The copolymer (P) used in the present invention may be a binary copolymer consisting of only the structural unit (A) and the structural unit (B), or a multi-component copolymer containing the structural unit (A), the structural unit (B), and a structural unit (C) other than these. The monomer that gives the structural unit (C) may be any monomer that is not included in the monomers that give the structural unit (A) and the structural unit (B), and is not limited as long as it is a compound having one or more carbon-carbon double bonds in the molecular structure. Examples of the monomer that gives the structural unit (C) include acyclic monomers represented by the general formula (1) shown below and cyclic monomers represented by the general formula (2). Compared to a binary copolymer consisting of only the structural unit (A) and the structural unit (B), by using a ternary or higher multi-component copolymer containing the structural unit (C) as the base resin of the ionomer, it is possible to obtain an ionomer with a low melting point and a low degree of crystallinity, and when made into a film, it is possible to obtain a film with a dramatically improved balance between rigidity and toughness, outstanding transparency and gloss, and excellent low-temperature heat sealability. The structural unit (C) may be based on one type of monomer, or two or more types of monomers may be used in combination.

[0044] [ka] [In general formula (1), T 1 ~T 3 each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, and a cyano group; T 4is a substituent selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, and a cyano group.

[0045] T 1 ~T 4 The carbon skeleton of the hydrocarbon group, alkoxy group, aryl group, ester group, and silyl group may have a branch, a ring, and / or an unsaturated bond. The number of carbon atoms in the ester group (-COOR) includes the number of carbon atoms in the carbonyl group. The number of carbon atoms in the hydrocarbon group having a substituent includes the number of carbon atoms in the substituent. T 1 ~T 4 The lower limit of the number of carbon atoms in the hydrocarbon group may be 1 or more, and the upper limit may be 20 or less, or may be 10 or less. T 1 ~T 4 The lower limit of the number of carbon atoms in the alkoxy group may be 1 or more, and the upper limit may be 20 or less, or may be 10 or less. T 1 ~T 4 The lower limit of the number of carbon atoms in the aryl group in the above formula may be 6 or more, and the upper limit may be 20 or less, or may be 11 or less. T 1 ~T 4 The lower limit of the number of carbon atoms in the ester group may be 2 or more, and the upper limit may be 20 or less, or may be 10 or less. T 1 ~T 4The number of carbon atoms in the silyl group in the above formula may be 3 or more, and may be 18 or less, or may be 12 or less. Examples of the silyl group include a trimethylsilyl group, a triethylsilyl group, a tri-n-propylsilyl group, a triisopropylsilyl group, a dimethylphenylsilyl group, a methyldiphenylsilyl group, and a triphenylsilyl group.

[0046] In the copolymer of the present invention, from the viewpoint of ease of production, T 1 and T 2 may be a hydrogen atom, T 3 may be a hydrogen atom or a methyl group, T 1 ~T 3 However, each of them may be a hydrogen atom. In addition, in terms of impact resistance and adhesiveness, 4 may be an ester group having 2 to 20 carbon atoms.

[0047] Specific examples of the acyclic monomer include T 4 is an ester group having 2 to 20 carbon atoms. T 4 is an ester group having 2 to 20 carbon atoms, the acyclic monomer may be a monomer having the structural formula: CH2=C(R 21 )CO2(R 22 ) where R 21 R is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, which may have a branch, a ring, and / or an unsaturated bond. 22 is a hydrocarbon group having 1 to 19 carbon atoms, which may have a branch, a ring, and / or an unsaturated bond. 22 It may contain a heteroatom at any position within the group. Structural formula: CH2=C(R 21 )CO2(R 22 ) as a compound represented by R 21 is a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms. 21 is a hydrogen atom, or R 21 Methacrylate esters in which the alkyl group is a methyl group are also included. Structural formula: CH2=C(R 21 )CO2(R 22 Specific examples of the compound represented by the formula (1) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, and benzyl (meth)acrylate. From the viewpoints of flexibility and impact resistance, acrylic esters are preferred. 22 Examples of the acrylate ester include acrylate esters having 1 to 8 carbon atoms, and specific examples of the compound include at least one selected from the group consisting of methyl acrylate, ethyl acrylate, n-butyl acrylate (nBA), isobutyl acrylate (iBA), t-butyl acrylate (tBA), and 2-ethylhexyl acrylate, and in particular at least one selected from the group consisting of n-butyl acrylate (nBA) and isobutyl acrylate (iBA). Examples of the acyclic monomer include 5-hexen-1-ol, allyl methyl ether, ethyl-4-pentenoate, 4-chloro-1-butene, methyl vinyl ether, styrene, vinyltrimethylsilane, vinyl chloride, and (meth)acrylonitrile. The non-cyclic monomer may be of one type or of multiple types.

[0048] Cyclic Monomers [ka] [In general formula (2), R 1 ~R 12may be the same or different and are selected from the group consisting of a hydrogen atom, a halogen atom, and a hydrocarbon group having 1 to 20 carbon atoms; R 9 and R 10 , and R 11 and R 12 may combine together to form a divalent organic group, R 9 or R 10 And, R 11 or R 12 may form a ring together. In addition, n represents 0 or a positive integer, and when n is 2 or more, R 5 ~R 8 may be the same or different in each repeating unit. Examples of the cyclic monomer include norbornene-based olefins, such as norbornene, vinylnorbornene, ethylidenenorbornene, norbornadiene, tetracyclododecene, tricyclo[4.3.0.1 2,5 ], Tricyclo[4.3.0.1 2,5 ]dec-3-ene, and other compounds having a cyclic olefin skeleton. 3,6 .0 2,7 ]dodec-4-ene and the like.

[0049] (4) Copolymer (P) The copolymer (P) used in the present invention as the base resin of the ionomer contains, as essential constituent units, a structural unit (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms, and a structural unit (B) derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group, and may further contain an arbitrary structural unit (C) other than the above (A) and (B), and these structural units are copolymerized substantially linearly, preferably randomly. "Substantially linear" refers to a state in which the copolymer has no branch or the frequency of branched structures is low, and the copolymer can be considered to be linear. Specifically, it refers to a state in which the phase angle δ of the copolymer is 50 degrees or more under the conditions described below.

[0050] The copolymer (P) according to the present invention must contain at least one type of structural unit (A) and at least one type of structural unit (B), that is, at least two types of monomer units in total. It may contain any structural unit (C) other than the above-mentioned (A) and (B). However, it is preferable that the copolymer (P) is a multicomponent copolymer containing such a structural unit (C). The structural units and the amounts of the structural units in the copolymer according to the present invention will be described below. A structure derived from one molecule each of ethylene and / or an α-olefin having 3 to 20 carbon atoms (A), a monomer (B) having a carboxy group and / or a dicarboxylic anhydride group, and any monomer (C) other than (A) and (B) is defined as one structural unit in the copolymer. The amount of structural units is the ratio of each structural unit expressed in mol % when all structural units in the copolymer are taken as 100 mol %.

[0051] Amount of structural units (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms: The structural unit amount of the structural unit (A) according to the present invention is selected from the following: the lower limit is 60.000 mol% or more, preferably 70.000 mol% or more, more preferably 80.000 mol% or more, even more preferably 85.000 mol% or more, even more preferably 90.000 mol% or more, and particularly preferably 91.200 mol% or more, and the upper limit is 97.999 mol% or less, preferably 97.990 mol% or less, more preferably 97.980 mol% or less, even more preferably 96.980 mol% or less, even more preferably 96.900 mol% or less, and particularly preferably 92.700 mol% or less. If the amount of structural units derived from ethylene and / or the α-olefin (A) having 3 to 20 carbon atoms is less than 60.000 mol %, the toughness of the copolymer will be poor, and if it is more than 97.999 mol %, the adhesion to different resins may be poor.

[0052] Amount of structural units of monomer (B) having a carboxy group and / or a dicarboxylic anhydride group: The amount of the structural unit (B) according to the present invention is selected from the following: the lower limit is 2.0 mol% or more, preferably 2.9 mol% or more, and more preferably 5.2 mol% or more, and the upper limit is 20.0 mol% or less, preferably 15.0 mol% or less, more preferably 10.0 mol% or less, even more preferably 8.0 mol% or less, and particularly preferably 5.4 mol% or less. If the amount of structural units derived from monomer (B) having a carboxy group and / or a dicarboxylic anhydride group is less than 2.0 mol%, the copolymer may not have sufficient adhesion to highly polar dissimilar materials, and if it exceeds 20.0 mol%, the copolymer may not have sufficient mechanical properties. Furthermore, the monomer having a carboxy group and / or a dicarboxylic anhydride group to be used may be used alone or in combination of two or more kinds.

[0053] Amount of structural units of any monomer (C): When the constituent elements of the ionomer according to the present invention contain an arbitrary monomer (C) other than the above (A) or (B), the structural unit amount of the structural unit (C) according to the present invention is selected from the following: the lower limit is 0.001 mol% or more, preferably 0.010 mol% or more, more preferably 0.020 mol% or more, even more preferably 0.100 mol% or more, still more preferably 2.000 mol% or more, particularly preferably 1.900 mol% or more, and the upper limit is 20.000 mol% or less, preferably 15.000 mol% or less, more preferably 10.000 mol% or less, even more preferably 5.000 mol% or less, particularly preferably 3.600 mol% or less. When the amount of the structural unit derived from any monomer (C) is 0.001 mol % or more, the flexibility of the copolymer tends to be sufficient, and when it is 20.000 mol % or less, the mechanical properties of the copolymer tend to be sufficient. Furthermore, any of the monomers used may be used alone or in combination of two or more kinds.

[0054] 2. Resin properties of copolymer (P) (1) Number of branches per 1,000 carbon atoms in a polymer In the copolymer according to the present invention, in order to increase the elastic modulus and obtain sufficient mechanical properties, 13 The number of methyl branches calculated by C-NMR may be 50 or less, 5.0 or less, 1.0 or less, or 0.5 or less per 1,000 carbons, with no particular limit on the lower limit, and the smaller the better. The number of ethyl branches may be 3.0 or less, 2.0 or less, 1.0 or less, or 0.5 or less per 1,000 carbons, with no particular limit on the lower limit, and the smaller the better. The number of butyl branches may be 7.0 or less, 5.0 or less, 3.0 or less, or 0.5 or less per 1,000 carbons, with no particular limit on the lower limit, and the smaller the better.

[0055] (2) Method for measuring the amount of structural units derived from monomers having a carboxy group and / or a dicarboxylic anhydride group and non-cyclic monomers in the copolymer, and the number of branches The amount of structural units derived from monomers having a carboxy group and / or a dicarboxylic anhydride group and non-cyclic monomers in the copolymer of the present invention, and the number of branches per 1,000 carbon atoms are 13 It can be determined using C-NMR spectroscopy. 13 C-NMR is measured by the following method. 200-300 mg of sample is placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of a mixed solvent of o-dichlorobenzene (C6H4Cl2) and deuterated bromide benzene (C6D5Br) (C6H4Cl2 / C6D5Br = 2 / 1 (volume ratio)) and hexamethyldisiloxane, a chemical shift standard substance, and the tube is sealed after replacing with nitrogen. It is heated and dissolved to prepare a homogeneous solution, which is used as the NMR measurement sample. NMR measurements are performed at 120°C using an AV400M NMR instrument from Bruker Japan Ltd. equipped with a 10 mmφ cryoprobe. 13 C-NMR was measured using the inverse gate decoupling method with a sample temperature of 120°C, a pulse angle of 90°, a pulse interval of 51.5 seconds, and an accumulation count of 512 or more. The chemical shifts are those of hexamethyldisiloxane. 13 The C signal was set at 1.98 ppm, and the other 13 The chemical shifts of the C signals are based on this. Obtained 13 In C-NMR, the signals specific to the monomers or branches of the multicomponent copolymer are identified and their intensities are compared, so that the amount of structural units of each monomer in the multicomponent copolymer and the number of branches can be analyzed. The positions of the signals specific to the monomers or branches can be referred to publicly known materials, or can be independently identified depending on the sample. Such an analysis method is commonly known to those skilled in the art.

[0056] (3) Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) The weight average molecular weight (Mw) of the copolymer of the present invention has a lower limit of usually 1,000 or more, preferably 6,000 or more, more preferably 10,000 or more, and an upper limit of usually 2,000,000 or less, preferably 1,500,000 or less, more preferably 1,000,000 or less, even more preferably 800,000 or less, and most preferably 100,000 or less. If Mw is less than 1,000, the mechanical properties and impact resistance of the copolymer are insufficient, and if Mw exceeds 2,000,000, the melt viscosity of the copolymer becomes high, making it difficult to spin the copolymer at high speed.

[0057] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the copolymer according to the present invention is usually in the range of 1.5 to 4.0, preferably 1.6 to 3.5, and more preferably 1.9 to 2.3. If Mw / Mn is less than 1.5, the copolymer may have insufficient processability, including molding, whereas if it exceeds 4.0, the copolymer may have poor mechanical properties. In this specification, (Mw / Mn) may be expressed as a molecular weight distribution parameter.

[0058] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the copolymer according to the present invention are determined by gel permeation chromatography (GPC). The molecular weight distribution parameter (Mw / Mn) is calculated by determining the number average molecular weight (Mn) by gel permeation chromatography (GPC) and then calculating the ratio of Mw to Mn, Mw / Mn.

[0059] An example of the GPC measurement method of the present invention is as follows. (Measurement conditions) Machine used: Waters 150C Detector: FOXBORO MIRAN1A IR detector (measurement wavelength: 3.42 μm) Measurement temperature: 140℃ Solvent: orthodichlorobenzene (ODCB) Column: Showa Denko AD806M / S (3 columns) Flow rate: 1.0mL / min Injection volume: 0.2mL (Sample preparation) A 1 mg / mL solution of the sample is prepared using ODCB (containing 0.5 mg / mL BHT (2,6-di-t-butyl-4-methylphenol)), and dissolved at 140° C. for about 1 hour. (Calculation of molecular weight (M)) The standard polystyrene method is used, and the conversion from retention volume to molecular weight is performed using a calibration curve prepared in advance using standard polystyrene. All of the standard polystyrenes used are Tosoh Corporation brands (F380, F288, F128, F80, F40, F20, F10, F4, F1, A5000, A2500, A1000). A calibration curve is created by injecting 0.2 mL of a solution in which each of the polystyrenes is dissolved in ODCB (containing 0.5 mg / mL BHT) so that the concentration is 0.5 mg / mL. The calibration curve uses a cubic equation obtained by approximating with the least squares method. The viscosity equation [η] = K × Mα used for conversion to molecular weight (M) uses the following values. Polystyrene (PS): K = 1.38 x 10 -4 , α=0.7 Polyethylene (PE): K = 3.92 x 10 -4 , α=0.733 Polypropylene (PP): K = 1.03 x 10 -4 , α=0.78

[0060] (4) Melting point (Tm, °C) The melting point of the copolymer according to the present invention is indicated by the maximum peak temperature of the endothermic curve measured by a differential scanning calorimeter (DSC). When multiple peaks are shown in the endothermic curve obtained by DSC measurement, with heat flow (mW) on the vertical axis and temperature (°C) on the horizontal axis, the maximum peak temperature refers to the temperature of the peak with the maximum height from the baseline among the multiple peaks, or when there is only one peak, the maximum peak temperature refers to the temperature of that peak. From the viewpoint of heat resistance, the melting point of the copolymer of the present invention is preferably at least 50°C, more preferably at least 60°C, and even more preferably at least 70°C. From the viewpoint of obtaining sufficient adhesion to different materials having high polarity, the melting point of the copolymer of the present invention is preferably at most 140°C, more preferably at most 110°C, even more preferably at most 100°C, even more preferably at most 98°C, and particularly preferably at most 96°C. In the present invention, the melting point can be determined from the absorption curve obtained by, for example, using a DSC (DSC7020) manufactured by SII Nano Technology Inc., packing about 5.0 mg of a sample into an aluminum pan, heating it to 200°C at 10°C / min, holding it isothermally at 200°C for 5 minutes, lowering it to 20°C at 10°C / min, holding it isothermally at 20°C for 5 minutes, and then heating it again to 200°C at 10°C / min.

[0061] (5) Molecular structure of copolymer The molecular chain terminal of the copolymer according to the present invention may be a structural unit (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms, a structural unit (B) derived from a monomer having a carboxy group and / or a dicarboxylic anhydride group, or a structural unit (C) derived from a non-cyclic monomer.

[0062] The copolymer according to the present invention may be a random copolymer, block copolymer, graft copolymer, etc., of a structural unit (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms, a structural unit (B) derived from a monomer having a carboxy group and / or a dicarboxylic anhydride group, and a structural unit (C) derived from a non-cyclic monomer. Among these, a random copolymer that can contain a large amount of the structural unit (B) may be used. An example of the molecular structure of a typical ternary copolymer (1) is shown below. A random copolymer is a copolymer in which the probability of finding each of the structural units (A), (B), and (C) at any position in a molecular chain is independent of the type of adjacent structural unit, as shown in the following molecular structure example (1).

[0063] [ka]

[0064] As an example of a graft copolymer, a molecular structure example (2) of a multicomponent copolymer into which a structural unit (B) derived from a monomer having a carboxy group and / or a dicarboxylic anhydride group is introduced by graft modification is also shown for reference. In the molecular structure example (2), a part of the copolymer of the structural unit (A) and the structural unit (C) is graft modified with the structural unit (B).

[0065] [ka]

[0066] In addition, the random copolymerization of a copolymer can be confirmed by various methods, but a method for determining the random copolymerization from the relationship between the comonomer content and melting point of a copolymer is described in detail in JP 2015-163691 A and JP 2016-079408 A. From the above documents, it can be determined that the randomness is low when the melting point (Tm, °C) of a multicomponent copolymer is higher than -3.74 × [Z] + 130 (where [Z] is the comonomer content / mol%).

[0067] The copolymer of the present invention, which is a random copolymer, preferably has a melting point (Tm, °C) measured by differential scanning calorimetry (DSC) and a total content [Z] (mol %) of the structural unit (B) derived from a monomer having a carboxy group and / or a dicarboxylic anhydride group and the structural unit (C) derived from an arbitrary monomer, which satisfy the following formula (I): 50 <Tm<-3.74×[Z]+130···(I) If the melting point of the copolymer (Tm, °C) is higher than -3.74 × [Z] + 130 (°C), the random copolymerization property is low, so there is a risk that the mechanical properties such as impact strength will be poor. If the melting point is lower than 50°C, there is a risk that the heat resistance will be poor.

[0068] Furthermore, the copolymer according to the present invention is preferably produced in the presence of a transition metal catalyst, from the viewpoint of making the molecular structure linear. It is known that the molecular structure of the copolymer varies depending on the production method, such as polymerization by a high-pressure radical polymerization process or polymerization using a metal catalyst. The difference in molecular structure can be controlled by selecting the production method, but the molecular structure can also be estimated from the complex modulus measured with a rotational rheometer, as described in JP 2010-150532 A, for example.

[0069] (6) Absolute value of complex elastic modulus G * Phase angle δ at =0.1MPa In the copolymer of the present invention, the absolute value of the complex modulus G measured by a rotational rheometer * It is preferable that the phase angle δ at pressure = 0.1 MPa is 50 to 75 degrees. The lower limit of the phase angle δ may be 51 degrees or more, and the upper limit of the phase angle δ may be 64 degrees or less. More specifically, the absolute value of the complex modulus G measured by a rotational rheometer * = Phase angle δ at 0.1 MPa (G *=0.1 MPa) is 50 degrees or more, the molecular structure of the copolymer is a linear structure containing no long chain branches or a substantially linear structure containing a small amount of long chain branches that does not affect the mechanical strength. In addition, the absolute value of the complex modulus G measured by a rotational rheometer * = Phase angle δ at 0.1 MPa (G * = 0.1 MPa) is lower than 50 degrees, the molecular structure of the copolymer will contain excessive long chain branches, and the mechanical strength may be inferior. Absolute value of complex modulus G measured by a rotational rheometer * The phase angle δ at G = 0.1 MPa is affected by both the molecular weight distribution and long chain branching. However, for copolymers with Mw / Mn ≦ 4, more preferably Mw / Mn ≦ 3, it is an index of the amount of long chain branching, and the more long chain branches there are in the molecular structure, the lower the δ(G * If the Mw / Mn of the copolymer is 1.5 or more, the δ(G * =0.1MPa) value never exceeds 75 degrees.

[0070] In the present invention, the method for measuring the complex elastic modulus is as follows. The sample is placed in a 1.0 mm thick mold for hot pressing, preheated for 5 minutes in a hot press machine with a surface temperature of 180°C, and then the residual gas in the sample is degassed by repeatedly applying and depressurizing pressure, and then pressurized to 4.9 MPa and held for 5 minutes. The sample is then transferred to a press machine with a surface temperature of 25°C and cooled by holding at a pressure of 4.9 MPa for 3 minutes to create a pressed plate made of a sample with a thickness of approximately 1.0 mm. The pressed plate made of the sample is processed into a circle with a diameter of 25 mm to serve as a measurement sample, and a Rheometrics ARES type rotational rheometer is used as a measurement device for dynamic viscoelastic properties, and dynamic viscoelasticity is measured under the following conditions in a nitrogen atmosphere. Plate: φ25mm parallel plate ·Temperature: 160℃ Distortion: 10% Measurement angular frequency range: 1.0×10 -2~1.0×10 2 rad / s Measurement interval: 5 points / decade Absolute value of complex elastic modulus G * Common logarithm logG of (Pa) * Plot the phase angle δ against logG * = 5.0, the value of δ (degrees) at the point * = 0.1MPa). * If there is no point corresponding to =5.0, logG * Using two points around =5.0, logG * The δ value at logG = 5.0 is calculated by linear interpolation. * <5, logG * Using the three largest values, we plot logG on a quadratic curve. * = 5.0.

[0071] 3. Method for producing copolymer (P) The method for producing the ionomer according to the present invention is not particularly limited as long as it is a method that can produce the ionomer according to the present invention. For example, a method for producing the ionomer of the present invention includes a step of preparing a copolymer (P) containing, as essential components, structural units (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms and structural units (B) derived from a monomer having a carboxy group and / or a dicarboxylic anhydride group, and optionally containing other structural units (C) represented by the general formula (1) or (2); and a conversion step of reacting at least a part of the carboxyl groups and / or dicarboxylic anhydride groups of the structural unit (B) of the copolymer (P) with a compound containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table to convert them into a metal-containing carboxylate.

[0072] (1) A step of preparing a copolymer (P) There is no particular limitation on the method for introducing a carboxy group and / or a dicarboxylic anhydride group into the copolymer according to the present invention. Carboxy groups and / or dicarboxylic anhydride groups can be introduced by various methods within the scope of the present invention. Examples of methods for introducing a carboxy group and / or a dicarboxylic anhydride group include a method of directly copolymerizing a monomer having a carboxy group and / or a dicarboxylic anhydride group, and a method of copolymerizing another monomer and then introducing a carboxy group and / or a dicarboxylic anhydride group by modification. Examples of the method for introducing a carboxy group and / or a dicarboxylic anhydride group by modification after copolymerizing other monomers include, for example, when introducing a carboxy group, a method in which a (meth)acrylic acid ester is copolymerized and then hydrolyzed to convert it to a carboxy group, and a method in which t-butyl (meth)acrylate is copolymerized and then thermally decomposed to convert it to a carboxy group.

[0073] Therefore, a copolymer precursor (Pp) containing, as essential constituent units, a structural unit (Bp) derived from a monomer having a carboxylate group, which becomes the structural unit (B) by thermal decomposition or hydrolysis, and a structural unit (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms, and optionally containing other structural units (C) represented by the general formula (1) or (2), may be prepared, and the carboxylate group of the structural unit (Bp) in the copolymer precursor (Pp) may be converted to a carboxy group by thermal decomposition or hydrolysis to obtain the copolymer (P).

[0074] (2) Polymerization catalyst The copolymer (P) may be produced in the presence of a transition metal catalyst in order to make its molecular structure linear. The type of polymerization catalyst used in producing the multicomponent copolymer (P) or the copolymer precursor (Pp) is not particularly limited as long as it is capable of copolymerizing the structural unit (A), the structural unit (B), and the structural unit (C), or the structural unit (A), the structural unit (Bp), and the structural unit (C). For example, a Group 5 to 11 transition metal complex having a chelating ligand can be used.

[0075] Specific examples of preferred transition metals include vanadium atom, niobium atom, tantalum atom, chromium atom, molybdenum atom, tungsten atom, manganese atom, iron atom, platinum atom, ruthenium atom, cobalt atom, rhodium atom, nickel atom, palladium atom, copper atom, etc. Among these, preferred are transition metals of Groups 8 to 11, more preferred are transition metals of Group 10, and particularly preferred are nickel (Ni) and palladium (Pd). These metals may be used alone or in combination.

[0076] Chelating ligands have at least two atoms selected from the group consisting of P, N, O, S, As, and Sb, and include ligands that are bidentate or multidentate, and are electronically neutral or anionic. Exemplary chelating ligand structures are given in the review by Brookhart et al. (Chem. Rev., 2000, 100, 1169). The chelating ligand preferably includes a bidentate anionic P, O ligand. Examples of the bidentate anionic P, O ligand include phosphorus sulfonic acid, phosphorus carboxylic acid, phosphorus phenol, and phosphorus enolate. Other examples of the chelating ligand include a bidentate anionic N, O ligand. Examples of the bidentate anionic N, O ligand include salicylaldimine and pyridine carboxylic acid. Other examples of the chelating ligand include a diimine ligand, a diphenoxide ligand, and a diamide ligand.

[0077] Examples of metal complexes obtained from chelating ligands include metal complexes represented by the following general formula (101) or (102) in which an arylphosphine compound, an arylarsine compound, or an arylantimony compound, which may have a substituent, is coordinated.

[0078] [ka]

[0079] [ka]

[0080] [In general formula (101) and general formula (102), M represents a transition metal belonging to any one of Groups 5 to 11 of the periodic table. X 1 represents oxygen, sulfur, -SO3-, or -CO2-. Y 1 represents carbon or silicon. n represents an integer of 0 or 1. E 1 represents phosphorus, arsenic or antimony. R 53 and R 54 each independently represents hydrogen or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 55 each independently represents hydrogen, halogen, or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 56 and R 57 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom, OR 52 , CO2R 52 , CO2M', C(O)N(R 51 )2, C(O)R 52 , S.R. 52 , SO2R 52 , SOR 52 , OSO2R 52 , P(O)(OR 52 ) 2-y (R 51 ) y , C.N., N.H.R. 52 , N(R 52 )2, Si(OR 51 ) 3-x (R 51 ) x , OSi(OR 51 ) 3-x (R 51 ) x , NO2, SO3M', PO3M'2, P(O)(OR 52)2M' or an epoxy-containing group. R 51 represents hydrogen or a hydrocarbon group having 1 to 20 carbon atoms. R 52 represents a hydrocarbon group having 1 to 20 carbon atoms. M′ represents an alkali metal, an alkaline earth metal, ammonium, a quaternary ammonium or a phosphonium; x represents an integer of 0 to 3; and y represents an integer of 0 to 2. In addition, R 56 and R 57 may be linked to each other to form an alicyclic ring, an aromatic ring, or a heterocyclic ring containing a heteroatom selected from oxygen, nitrogen, or sulfur, in which case the ring has 5 to 8 members and may or may not have a substituent on the ring. L 1 represents a ligand coordinated to M. Also, R 53 and L 1 may be bonded to each other to form a ring. More preferably, it is a transition metal complex represented by the following general formula (103).

[0081] [ka]

[0082] [In the general formula (103), M represents a transition metal belonging to any one of Groups 5 to 11 of the periodic table. X 1 represents oxygen, sulfur, -SO3-, or -CO2-. Y 1 represents carbon or silicon. n represents an integer of 0 or 1. E 1 represents phosphorus, arsenic or antimony. R 53 and R 54 each independently represents hydrogen or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 55each independently represents hydrogen, halogen, or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 58 , R 59 , R 60 and R 61 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom, OR 52 , CO2R 52 , CO2M', C(O)N(R 51 )2, C(O)R 52 , S.R. 52 , SO2R 52 , SOR 52 , OSO2R 52 , P(O)(OR 52 ) 2-y (R 51 ) y , C.N., N.H.R. 52 , N(R 52 )2, Si(OR 51 ) 3-x (R 51 ) x , OSi(OR 51 ) 3-x (R 51 ) x , NO2, SO3M', PO3M'2, P(O)(OR 52 )2M' or an epoxy-containing group. R 51 represents hydrogen or a hydrocarbon group having 1 to 20 carbon atoms. R 52 represents a hydrocarbon group having 1 to 20 carbon atoms. M′ represents an alkali metal, an alkaline earth metal, ammonium, a quaternary ammonium or a phosphonium; x represents an integer of 0 to 3; and y represents an integer of 0 to 2. In addition, R 58 ~R 61 may be bonded to each other to form an alicyclic ring, an aromatic ring, or a heterocyclic ring containing a heteroatom selected from oxygen, nitrogen, or sulfur. In this case, the number of ring members is 5 to 8, and the ring may or may not have a substituent. L 1 represents a ligand coordinated to M. Also, R 53 and L 1 may be bonded to each other to form a ring.

[0083] In the general formulae (101) to (103), M can be any of the transition metals mentioned above. X 1 Among them, is preferably oxygen or -SO3-. Y 1 Of these, carbon is preferred. Among these, n preferably represents 0. E 1 Of these, phosphorus is preferred. L 1 represents a ligand coordinated to M. In the present disclosure, the ligand L 1 Examples of the compound include hydrocarbon compounds having 1 to 20 carbon atoms and containing oxygen, nitrogen, or sulfur as an atom capable of forming a coordinate bond. 1 As L, a hydrocarbon compound having a carbon-carbon unsaturated bond capable of coordinating with a transition metal (which may contain a heteroatom) can also be used. 1 The number of carbon atoms of is 1 to 16, and more preferably 1 to 10. 1 As the charge-discharging agent, a compound having no electric charge is preferable. Preferred L 1 As the preferred L in the general formula (D) of WO2010 / 050256, 1 It may be similar to: Preferred R 53 As the preferred R in the general formula (D) of WO2010 / 050256, 3 It may be similar to: Preferred R 54 As the preferred R in the general formula (D) of WO2010 / 050256, 4 It may be similar to: In addition, R 53 and L 1 may be bonded to each other to form a ring, an example of which is a cyclooct-1-enyl group.

[0084] Representative catalysts of Group 5 to 11 transition metal complexes having a chelating ligand include so-called SHOP catalysts and Drent catalysts. The SHOP catalyst includes a catalyst in which a phosphorus-based ligand having an aryl group which may have a substituent is coordinated to nickel metal, and can be used by referring to, for example, WO2010 / 050256. Furthermore, examples of the Drent-based catalyst include catalysts in which a phosphorus-based ligand having an aryl group which may have a substituent is coordinated to palladium metal, and can be used by referring to, for example, JP-A-2010-202647.

[0085] (3) Polymerization cocatalyst In the production of the copolymer according to the present invention, the polymerization activity can be further increased by contacting a monomer with a small amount of an organometallic compound and then copolymerizing the structural unit (A), the structural unit (B), and the structural unit (C), or the structural unit (A), the structural unit (Bp), and the structural unit (C), in the presence of the transition metal catalyst. The organometallic compound is an organometallic compound containing a hydrocarbon group which may have a substituent, and can be represented by the following general formula (104). R 30 n M 30 X 30 m-n General formula (104) (In general formula (104), R 30 represents a hydrocarbon group having 1 to 12 carbon atoms which may have a substituent, M 30 is a metal selected from the group consisting of groups 1, 2, 12 and 13 of the periodic table; X 30 represents a halogen atom or a hydrogen atom, and m represents M 30 The valence, n, is 1 to m.

[0086] Examples of the organometallic compound represented by the above general formula (104) include alkylaluminums such as tri-n-butylaluminum, tri-n-hexylaluminum, tri-n-octylaluminum, and tri-n-decylaluminum, and alkylaluminum halides such as methylaluminum dichloride, ethylaluminum dichloride, dimethylaluminum chloride, diethylaluminum chloride, and diethylaluminum ethoxide, and preferably, trialkylaluminums are selected. As the organometallic compound, trialkylaluminum having a hydrocarbon group with 4 or more carbon atoms is more preferably selected, trialkylaluminum having a hydrocarbon group with 6 or more carbon atoms is even more preferably selected, and tri-n-hexylaluminum, tri-n-octylaluminum, and tri-n-decylaluminum are even more preferably selected, with tri-n-octylaluminum being particularly preferably used. The organometallic compound has a molar ratio of 10 to the comonomer. -5 ~0.9, preferably 10 -4 ~0.2, more preferably 10 -4 From the viewpoints of polymerization activity and cost, it is preferable to contact the catalyst in an amount of 1 to 0.1.

[0087] Residual amount of aluminum (Al) The copolymer (P) according to the present invention preferably has a small amount of aluminum (Al) remaining in the copolymer. The amount of aluminum (Al) remaining in 1 g of copolymer (P) is preferably 100,000 μg Al / g or less, more preferably 70,000 μg Al / g or less, even more preferably 20,000 μg Al / g or less, even more preferably 10,000 μg Al / g or less, particularly preferably 5,000 μg Al / g or less, particularly preferably 1,000 μg Al / g or less, and most preferably 500 μg Al / g or less. If it is more than this, the mechanical properties of the copolymer may decrease, and the polymerization product may discolor or deteriorate. The amount of aluminum (Al) remaining is preferably as small as possible, and may be, for example, as small as 1 μg Al / g or 0 μg Al / g (not included). Note that "μg Al / g" means the amount of aluminum (Al) contained in 1 g of multi-component copolymer expressed in μg units.

[0088] · Calculation method for residual aluminum (Al) amount The amount of aluminum (Al) contained in the copolymer (P) according to the present invention can be calculated by dividing the amount of aluminum contained in the alkylaluminum subjected to polymerization by the yield of the obtained copolymer (P).

[0089] The amount of aluminum (Al) contained in the copolymer (P) may be calculated from the amount of alkyl aluminum charged for polymerization, but may also be measured by X-ray fluorescence analysis or inductively coupled plasma emission (ICP) analysis. When X-ray fluorescence analysis or ICP analysis is used, the amount of aluminum (Al) may be measured by, for example, the following X-ray fluorescence analysis or inductively coupled plasma emission (ICP) analysis.

[0090] 1) X-ray fluorescence analysis Weigh out 3 to 10 g of the sample and heat and press it in a hot press to make a flat plate sample with a diameter of 45 mm. Measurements are performed on the central part of the flat plate sample, 30 mm in diameter, using a scanning X-ray fluorescence analyzer "ZSX100e" (Rh tube 4.0 kW) manufactured by Rigaku Electric Industries Co., Ltd., under the following conditions. X-ray output: 50kV-50mA ·Spectroscopic crystal: PET Detector: PC (proportional counter) Detection line: Al-Kα line The aluminum content can be calculated from a previously prepared calibration curve and the results of measurements under the above conditions. The calibration curve can be prepared by measuring the aluminum content of multiple polyethylene resins by ICP analysis, and then subjecting those polyethylene resins to X-ray fluorescence analysis under the above conditions.

[0091] 2) Inductively Coupled Plasma (ICP) Analysis The sample, 3 ml of special grade nitric acid, and 1 ml of hydrogen peroxide solution (hydrogen peroxide content 30% by weight) are placed in a Teflon (registered trademark) container, and the sample is dissolved by heating and decomposing at a maximum of 500 W using a microwave decomposition device (MLS-1200MEGA, manufactured by Milestone General Co., Ltd.). The aluminum content can be measured by subjecting the dissolved sample to an ICP emission spectrometer (IRIS-AP, manufactured by Thermo Jarrell Ash Co., Ltd.). The aluminum content is quantified using a calibration curve created using a standard solution with a known aluminum element concentration.

[0092] (4) Polymerization method The method for polymerizing the copolymer (P) or the multicomponent copolymer precursor (Pp) according to the present invention is not limited. Examples of the polymerization method include slurry polymerization in which at least a portion of the produced polymer becomes a slurry in a medium, bulk polymerization in which the liquefied monomer itself is used as the medium, gas phase polymerization in vaporized monomer, and high pressure ionic polymerization in which at least a portion of the produced polymer is dissolved in monomer liquefied at high temperature and pressure. The polymerization method may be any of batch polymerization, semi-batch polymerization, and continuous polymerization. Furthermore, living polymerization may be carried out, or polymerization may be carried out while simultaneously causing chain transfer. Furthermore, during polymerization, a so-called chain shuttling agent (CSA) may be used in combination to carry out a chain shuttling reaction or coordinate chain transfer polymerization (CCTP). The specific manufacturing process and conditions may be appropriately selected, and reference may be made to, for example, JP-A-2010-260913 and JP-A-2010-202647.

[0093] When the carboxylate group of the structural unit (Bp) in the copolymer precursor (Pp) is converted to a carboxyl group by thermal decomposition or hydrolysis to obtain the copolymer (P), a conventionally known acid-base catalyst may be used as an additive for promoting the reaction during hydrolysis or thermal decomposition. The acid-base catalyst is not particularly limited, and examples of the acid-base catalyst that can be used include, for example, hydroxides of alkali metals or alkaline earth metals such as sodium hydroxide, potassium hydroxide, or lithium hydroxide, alkali metals or carbonates of alkaline earth metals such as sodium hydrogencarbonate or sodium carbonate, solid acids such as montmorillonite, inorganic acids such as hydrochloric acid, nitric acid, or sulfuric acid, and organic acids such as formic acid, acetic acid, benzoic acid, citric acid, paratoluenesulfonic acid, trifluoroacetic acid, or trifluoromethanesulfonic acid. From the viewpoints of reaction promotion effect, cost, equipment corrosivity, etc., sodium hydroxide, potassium hydroxide, sodium carbonate, paratoluenesulfonic acid, and trifluoroacetic acid are preferred, and paratoluenesulfonic acid and trifluoroacetic acid are more preferred.

[0094] 4. Ionomer manufacturing method The method for producing an ionomer according to the present invention includes a step of converting at least a portion of the carboxyl groups and / or dicarboxylic anhydride groups of the structural unit (B) of the copolymer (P) into a metal-containing carboxylate by reacting the carboxyl groups and / or dicarboxylic anhydride groups of the structural unit (B) with a compound containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table. The conversion step may be a conversion step of converting the carboxylate groups of the structural unit (Bp) in the copolymer precursor (Pp) into carboxy groups by thermal decomposition or hydrolysis to form a copolymer (P), and at the same time converting at least a part of the carboxy groups and / or dicarboxylic anhydride groups of the structural unit (B) of the copolymer (P) into a metal-containing carboxylate by reacting them with a compound containing at least one kind of metal ion selected from Group 1, Group 2, or Group 12 of the periodic table.

[0095] The metal ion-containing compound may be an oxide, hydroxide, carbonate, bicarbonate, acetate, formate, etc., of a metal from Groups 1, 2, or 12 of the Periodic Table. The compound containing metal ions may be supplied to the reaction system in the form of particles or fine powder, or may be dissolved or dispersed in water or an organic solvent and then supplied to the reaction system, or a master batch may be prepared using an ethylene / unsaturated carboxylic acid copolymer or an olefin copolymer as a base polymer and then supplied to the reaction system. In order to ensure smooth reaction, a method in which a master batch is prepared and a compound containing metal ions is supplied to the reaction system is preferred.

[0096] The reaction with the compound containing metal ions may be carried out by melt kneading using various types of equipment such as a vent extruder, a Banbury mixer, a roll mill, etc., and the reaction may be a batch or continuous method. Since the reaction can be carried out smoothly by discharging water and carbon dioxide gas by-produced by the reaction using a degassing device, it is preferable to carry out the reaction continuously using an extruder equipped with a degassing device such as a vent extruder. In the reaction with the compound containing metal ions, a small amount of water may be injected to promote the reaction.

[0097] When converting the carboxylate group of the structural unit (Bp) in the copolymer precursor (Pp) into a carboxylate group by thermal decomposition to obtain the copolymer (P), the temperature at which the copolymer precursor (Pp) is heated may be a temperature at which the carboxylate group is converted into a carboxylate group. If the heating temperature is too low, the carboxylate group is not converted into a carboxylate group, and if the heating temperature is too high, decarbonylation or decomposition of the copolymer may proceed. Therefore, the heating temperature is preferably 60°C to 350°C, more preferably 70°C to 340°C, even more preferably 80°C to 330°C, even more preferably 100°C to 330°C, particularly preferably 150°C to 320°C, and most preferably 200°C to 320°C. The reaction time varies depending on the heating temperature, the reactivity of the ester group portion, etc., but is usually 1 minute to 50 hours, more preferably 2 minutes to 30 hours, even more preferably 2 minutes to 10 hours, still more preferably 2 minutes to 5 hours, and particularly preferably 3 minutes to 4 hours.

[0098] Heating is also preferred when at least a portion of the carboxyl groups and / or dicarboxylic anhydride groups of the structural unit (B) of the copolymer (P) is reacted with a compound containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table. The heating temperature is preferably in the range of 80°C to 350°C, more preferably 100°C to 340°C, even more preferably 150°C to 330°C, and even more preferably 200°C to 320°C. The reaction time varies depending on the heating temperature, reactivity, etc., but is usually 1 minute to 50 hours, more preferably 2 minutes to 30 hours, even more preferably 2 minutes to 10 hours, still more preferably 2 minutes to 5 hours, and particularly preferably 3 minutes to 4 hours.

[0099] In the above conversion step, the reaction atmosphere is not particularly limited, but it is generally preferred to carry out the reaction under a flow of an inert gas, such as nitrogen, argon, or carbon dioxide, and a small amount of oxygen or air may be mixed in.

[0100] The reactor used in the above conversion step is not particularly limited, and any method can be used as long as it can substantially uniformly stir the copolymer. A glass vessel or autoclave (AC) equipped with a stirrer may be used, or any conventionally known kneader such as a Brabender plastograph, a single-screw or twin-screw extruder, a high-intensity screw-type kneader, a Banbury mixer, a kneader, or a roll may be used.

[0101] 5. Additives The ionomer of the present invention may be used as an ionomer resin material by blending with additives such as conventionally known antioxidants, ultraviolet absorbers, lubricants, antistatic agents, colorants, pigments, crosslinking agents, foaming agents, nucleating agents, flame retardants, conductive materials, and fillers, within the scope of the gist of the present invention.

[0102] 6. Fiber (1) Manufacturing method The method for producing fibers (spun fibers) using the fiber resin composition containing the ionomer according to the present invention can be selected optimally according to production efficiency, fiber shape, and application. Examples include melt spinning, wet spinning, and dry spinning, and melt spinning is preferred. The lower limit of the molding temperature is preferably equal to or higher than the melting point of the ionomer, and the upper limit is preferably a temperature at which the ionomer does not deteriorate before being extruded from the spinneret. For example, it is 100°C to 250°C, preferably 110°C to 230°C, and more preferably 120°C to 210°C.

[0103] (2) Compounding The ionomer according to the present invention may be combined with a material different from the ionomer to produce a composite fiber. There is no particular limitation on the material to be used in combination with the ionomer, and examples of the material include polyethylene, polypropylene, polyvinyl chloride, polyester resin, polyamide resin, acrylic resin, polycarbonate resin, phenol resin, epoxy resin, urea resin, melamine resin, urea resin, polyurethane, polyoxymethylene, polytetrafluoroethylene, acetyl cellulose, and rayon. The shape of the composite fiber is not particularly limited, but examples include a conjugate type, a core-sheath type, a split type, and an island-in-the-sea type.

[0104] (3) Blend The fibers using the ionomer according to the present invention can be blended to satisfy the required functions. The ionomer according to the present invention may be combined with a different material to produce a composite fiber. There is no particular restriction on the different materials used, but examples thereof include polyethylene, polypropylene, polyvinyl chloride, polyester resins, polyamide resins, acrylic resins, polycarbonate resins, phenolic resins, epoxy resins, urea resins, melamine resins, urea resins, polyurethane, polyoxymethylene, polytetrafluoroethylene, acetyl cellulose, and rayon. There is also no particular restriction on the blending ratio, and the materials can be blended at any ratio to satisfy the required functions.

[0105] (4) Hollowing The fibers using the ionomer according to the present invention can be hollowed out to satisfy the required functions. The ionomer hollow fibers may have a structure having a hollow portion and micropores penetrating from the fiber surface to the hollow portion. Methods for producing hollow fibers having such micropores include a method of first producing a hollow fiber and then stretching it to obtain micropores, and a method of spinning a mixture of a different material soluble in alkali or acid and the ionomer according to the present invention as a composite fiber, and then treating the obtained fiber with an alkali or acid to remove the different material. Any of these methods can be appropriately selected.

[0106] 7. Fiber properties (1) Adhesion performance to different materials Fibers spun using the ionomer according to the present invention have excellent adhesion performance to different materials having high polarity. Specific examples of different materials having high polarity according to the present invention that can exhibit excellent adhesion performance include polyethylene resins such as ethylene-vinyl acetate copolymer and ethylene-acrylic acid ester copolymer, vinyl polymers such as polyvinyl chloride, polyvinylidene chloride, polystyrene, polyacrylate, and polyacrylonitrile, polyamide resins such as nylon 6, nylon 66, nylon 10, nylon 11, nylon 12, nylon 610, and polymetaxylylene adipamide, polyester resins such as polyethylene terephthalate, polyethylene terephthalate / isophthalate, polybutylene terephthalate, polylactic acid, polybutylene succinate, and aromatic polyesters, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polycarbonate, and the like. Examples of the material include thermosetting resins such as carbonate resins, adhesive fluororesins, phenolic resins, epoxy resins, urea resins, melamine resins, urea resins, alkyd resins, unsaturated polyesters, polyurethanes, and thermosetting polyimides; thermoplastic resin films or sheets (stretched or printed products thereof) having film-forming ability such as cellulose-based polymers such as cellophane; metal foils or metal plates such as aluminum, iron, copper, or alloys containing these as main components; vapor-deposited films of inorganic oxides such as silica-deposited plastic films and alumina-deposited plastic films; vapor-deposited films of metals such as gold, silver, and aluminum, or compounds other than the oxides of these metals; papers such as fine paper, craft paper, paperboard, glassine paper, and synthetic paper; cellophane, woven fabrics, and nonwoven fabrics.

[0107] (2) High-speed spinning performance The fibers spun using the ionomer according to the present invention have high-speed spinning performance. That is, they can be spun while being wound at high speed. Compared with the multi-branched ionomers produced by the conventional high-pressure radical polymerization method, the ionomers having a substantially linear structure according to the present invention have fewer branches, and therefore the number of entanglements between molecular chains is smaller, and it is possible to avoid stress concentration at the entanglement points when the molten body is wound at high speed. A specific index is the maximum take-up speed (MDS) using a capillograph. The value of MDS is not particularly limited, but when measured using a capillograph under the measurement conditions of a temperature of 190°C, an orifice with a length of 8.000 mm and a hole diameter of 2.085 mm, and a piston speed of 10 mm / min, the value of MDS is 100 to 200 m / min, preferably 125 to 200 m / min, and more preferably 150 to 200 m / min.

[0108] (3) Impact resistance The fibers spun using the ionomer according to the present invention have superior impact resistance compared to conventional hyperbranched ionomers. The ionomer according to the present invention is substantially linear, and this is because there are few molecular chain ends that are the starting point of breakage. A specific index of impact resistance is the breaking energy (E) represented by the area of ​​the stress-strain curve. The breaking energy value of the fiber is not particularly limited, but the breaking energy (E) calculated from the stress-strain curve obtained when a 30 dtex fiber is subjected to a tensile test with a chuck distance of 50 mm and a tensile speed of 500 mm / min is 100 J / mm or more, preferably 110 J / mm or more, and more preferably 120 J / mm or more. There is no particular upper limit, and the larger the value of E, the better. EXAMPLES

[0109] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. The physical properties in the examples and comparative examples were measured and evaluated by the methods described below. In the table, "no data" means that no measurement was performed, "not detected" means that the measurement was below the detection limit, and "non break" means that no break occurred and the measurement was above the upper limit of the measuring device.

[0110] <Measurement and Evaluation> 1. Absolute value of complex elastic modulus G * = Phase angle δ at 0.1 MPa (G * =0.1MPa) (1) Sample preparation and measurement The sample was placed in a 1.0 mm thick mold for hot pressing, preheated in a hot press machine with a surface temperature of 180°C for 5 minutes, and then repeatedly pressurized and depressurized to remove residual gas from the sample. The sample was then pressurized to 4.9 MPa and held for 5 minutes. The sample was then transferred to a press machine with a surface temperature of 25°C and cooled by holding at a pressure of 4.9 MPa for 3 minutes to produce a pressed plate made of a sample with a thickness of approximately 1.0 mm. The pressed plate made of the sample was processed into a circular shape with a diameter of 25 mm to serve as a measurement sample. A Rheometrics ARES type rotational rheometer was used as a measurement device for dynamic viscoelastic properties, and dynamic viscoelasticity was measured under the following conditions in a nitrogen atmosphere. (2) Measurement conditions Plate: φ25mm (diameter) parallel plate ·Temperature: 160℃ Distortion: 10% Measurement angular frequency range: 1.0×10 -2 ~1.0×10 2 rad / s Measurement interval: 5 points / decade Absolute value of complex elastic modulus G * Common logarithm logG of (Pa) * Plot the phase angle δ against logG * = 5.0, the value of δ (degrees) at the point * = 0.1MPa). * If there is no point corresponding to =5.0, logG * Using two points around =5.0, logG * The δ value at logG = 5.0 was calculated by linear interpolation. * <5, logG* Using the three largest values, we plot logG on a quadratic curve. * The δ value at =5.0 was extrapolated.

[0111] 2. Measurement of weight average molecular weight (Mw) and molecular weight distribution parameter (Mw / Mn) The weight average molecular weight (Mw) was determined by gel permeation chromatography (GPC). The molecular weight distribution parameter (Mw / Mn) was calculated from the ratio of Mw to Mn, Mw / Mn, obtained by further determining the number average molecular weight (Mn) by gel permeation chromatography (GPC). The measurements were carried out according to the following procedures and conditions.

[0112] (1) Sample pretreatment When the sample contained a carboxyl group, it was subjected to an esterification treatment, such as methyl esterification using diazomethane or trimethylsilyl (TMS) diazomethane, before the measurement. When the sample contained a carboxyl group, it was subjected to an acid treatment to modify the carboxyl group to a carboxyl group, and then subjected to the above-mentioned esterification treatment before the measurement.

[0113] (2) Preparation of sample solution 3 mg of sample and 3 mL of o-dichlorobenzene were weighed into a 4 mL vial, and the vial was capped with a screw cap and a Teflon (registered trademark) septum, and then shaken for 2 hours at 150°C using a Senshu Scientific SSC-7300 high-temperature shaker. After shaking, it was visually confirmed that there were no insoluble components.

[0114] (3) Measurement A Waters Alliance GPCV2000 was connected to Showa Denko's high-temperature GPC columns Showdex HT-G x 1 and HT-806M x 2, and GPC measurements were performed using o-dichlorobenzene as the eluent at a temperature of 145°C and a flow rate of 1.0 mL / min.

[0115] (4) Calibration curve The column was calibrated using monodisperse polystyrene (S-7300, S-3900, S-1950, S-1460, S-1010, S-565, S-152, S-66.0, S-28.5, S-5.05, each 0.07 mg / ml solution) manufactured by Showa Denko, n-eicosane and n-tetracontane were measured under the same conditions as above, and the elution time and the logarithm of the molecular weight were approximated by a fourth-order equation. PS ) and polyethylene molecular weight (M PE The following formula was used to convert M PE =0.468×M PS

[0116] 3.Melt Flow Rate (MFR) The MFR was measured in accordance with Table 1-Condition 7 of JIS K-7210 (1999) at a temperature of 190°C and a load of 21.18N.

[0117] 4. Tensile test of pressed sheet A sheet with a thickness of 1 mm was prepared from the sample by the method described in JIS K7151 (1995) (cooling method A), and this was punched out to prepare a small 5B type test piece described in JIS K7162 (1994). A tensile test was performed at a temperature of 23°C according to JIS K7161 (1994) to measure the tensile modulus of elasticity, tensile stress at break, tensile elongation at break, and tensile impact strength. The test speed was 10 mm / min.

[0118] 5. Haze The haze was measured in accordance with JIS K 7136.

[0119] 6. Melting point and crystallinity The melting point is indicated by the peak temperature of the endothermic curve measured by a differential scanning calorimeter (DSC). The measurement was performed using a DSC (DSC7020) manufactured by SII Nano Technology Co., Ltd. under the following measurement conditions. Approximately 5.0 mg of the sample was placed in an aluminum pan, heated to 200°C at 10°C / min, held at 200°C for 5 minutes, and then cooled to 30°C at 10°C / min. After holding at 30°C for 5 minutes, the sample was heated again at 10°C / min. The maximum peak temperature in the absorption curve was taken as the melting point Tm, and the heat of fusion (ΔH) was calculated from the area of ​​the melting endothermic peak. The degree of crystallinity (%) was calculated by dividing the heat of fusion by the heat of fusion of perfect crystals of high density polyethylene (HDPE), 293 J / g.

[0120] 7. Method for measuring the amount of structural units derived from monomers having a carboxy group and / or a dicarboxylic anhydride group, and non-cyclic monomers, and the number of branches per 1,000 carbons The amount of structural units derived from monomers having a carboxy group and / or a dicarboxylic anhydride group and non-cyclic monomers in the copolymer of the present invention, and the number of branches per 1,000 carbon atoms are 13 It can be determined using C-NMR spectroscopy. 13 C-NMR was measured by the following method. 200-300 mg of sample was placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of a mixed solvent of o-dichlorobenzene (C6H4Cl2) and deuterated bromide benzene (C6D5Br) (C6H4Cl2 / C6D5Br = 2 / 1 (volume ratio)) and hexamethyldisiloxane, a chemical shift standard substance, and the tube was purged with nitrogen, sealed, and heated to dissolve and prepare a homogeneous solution to be used as the NMR measurement sample. NMR measurements were performed at 120°C using an AV400M NMR instrument from Bruker Japan equipped with a 10 mmφ cryoprobe. 13 C-NMR was measured using the inverse gate decoupling method with a sample temperature of 120°C, a pulse angle of 90°, a pulse interval of 51.5 seconds, and an accumulation number of 512 or more. The chemical shifts are those of hexamethyldisiloxane. 13 The C signal was set to 1.98 ppm, and the other 13 The chemical shifts of the C signals were based on this.

[0121] (1) Sample pretreatment When the sample contained a carboxylate group, the sample was subjected to an acid treatment to convert the carboxylate group to a carboxyl group before the measurement. When the sample contained a carboxyl group, an esterification treatment such as methyl esterification using diazomethane or trimethylsilyl (TMS) diazomethane may be appropriately performed.

[0122] (2) Calculation of the amount of structural units derived from monomers having a carboxy group and / or a dicarboxylic anhydride group, and non-cyclic monomers <e tba> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 It is detected at 79.6 to 78.8 in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I(tBA) × 100 / 〔I(tBA) + I(E)〕 Here, I(tBA) and I(E) are the quantities shown in the following formulas. I(tBA)=I 79.6~78.8 I(E)=(I 180.0~135.0 +I 120.0~5.0 -I(tBA) × 7) / 2

[0123] <e tba nba> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The methylene signal of the butoxy group of nBA was detected at 64.1 to 63.4 ppm in the C-NMR spectrum and 79.6 to 78.8 ppm in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I(tBA) × 100 / 〔I(tBA) + I(nBA) + I(E)〕 Total amount of nBA (mol%)=I(nBA)×100 / [I(tBA)+I(nBA)+I(E)] Here, I(tBA), I(nBA), and I(E) are quantities expressed by the following formulas, respectively. I(tBA)=I 79.6~78.8 I(nBA)=I 64.1~63.4 I(E)=(I 180.0~135.0 +I 120.0~5.0 -I(nBA) x 7 -I(tBA) x 7) / 2

[0124] <e tba iba> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The methylene signal of the isobutoxy group of iBA is detected at 70.5 to 69.8 ppm, and the methyl signal of the isobutoxy group is detected at 19.5 to 18.9 ppm in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I(tBA) × 100 / 〔I(tBA) + I(iBA) + I(E)〕 Total amount of iBA (mol%)=I(iBA)×100 / [I(tBA)+I(iBA)+I(E)] Here, I(tBA), I(iBA), and I(E) are quantities expressed by the following formulas, respectively. I(tBA)=I 79.6~78.8 I(iBA) = (I 70.5~69.8 +I 19.5~18.9 ) / 3 I(E)=(I 180.0~135.0 +I 120.0~5.0 -I(iBA) x 7 -I(tBA) x 7) / 2

[0125] <e tba nb> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The methine carbon signal of NB was detected at 41.9 to 41.1 ppm in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I(tBA) × 100 / 〔I(tBA) + I(NB) + I(E)〕 Total amount of NB (mol%) = I(NB) × 100 / 〔I(tBA) + I(NB) + I(E)〕 Here, I(tBA), I(NB), and I(E) are quantities expressed by the following formulas. I(tBA)=I 79.6~78.8 I(NB)=(I 41.9~41.1 ) / 2 I(E)=(I 180.0~135.0 +I 120.0~5.0 -I(NB) x 7 -I(tBA) x 7) / 2

[0126] In addition, when the structural unit amount of each monomer is indicated by "<0.1" including an inequality sign, it means that it is present as a structural unit in the multi-component copolymer, but the amount is less than 0.1 mol %, taking into account significant digits.

[0127] (3) Calculation of the number of branches per 1,000 carbon atoms Copolymers come in three types: isolated types, in which a branch exists alone in the main chain, complex types (face-to-face types in which branches face each other via the main chain, branched-branch types, in which there are branches within a branched chain, and chain types). The following is an example of the structure of an ethyl branch. In the example of the facing type, R represents an alkyl group.

[0128] [ka]

[0129] The number of branches per 1,000 carbons is calculated by substituting either I(B1), I(B2), or I(B4) below into the I (branch) term in the following formula. B1 represents methyl branches, B2 represents ethyl branches, and B4 represents butyl branches. The number of methyl branches is calculated using I(B1), the number of ethyl branches using I(B2), and the number of butyl branches using I(B4). Number of branches (per 1,000 carbons) = I (branches) x 1000 / I (total) Here, I(total), I(B1), I(B2), and I(B4) are quantities expressed by the following formulas. I(total)=I 180.0~135.0 +I 120.0~5.0 I(B1)=(I 20.0~19.8 +I 33.2~33.1 +I 37.5~37.3 ) / 4 I(B2)=I 8.6~7.6 +I 11.8~10.5 I(B4)=I 14.3~13.7 -I 32.2~32.0 Here, I is the integrated intensity, and the subscripts of I indicate the range of chemical shifts. For example, I 180.0~135.0 was detected between 180.0 ppm and 135.0 ppm. 13 C The integrated intensity of the signal is shown. The attribution was based on the non-patent literature Macromolecules 1984, 17, 1756-1761 and Macromolecules 1979, 12, 41. In addition, when each branch number is indicated by "<0.1" including an inequality sign, it means that it exists as a structural unit in the multi-component copolymer, but the amount is less than 0.1 mol% considering significant figures. Also, "not detected" means below the detection limit.

[0130] 8. Aluminum (Al) adhesive strength The aluminum (Al) adhesive strength was measured by making a laminate by overlapping the sample processed into a press plate and an aluminum sheet, hot pressing them, and then performing a peel test. The methods for making the press plate and the laminate, and the method for measuring the adhesive strength are explained in order.

[0131] (1) Method for preparing the sample press plate The sample was placed in a heat press mold with dimensions: 50 mm x 60 mm, thickness: 0.5 mm, preheated for 5 minutes in a heat press machine with a surface temperature of 180°C, and then the residual gas in the sample was degassed by repeatedly applying and depressurizing pressure, and the sample was then pressurized to 4.9 MPa and held for 3 minutes.The sample was then transferred to a press machine with a surface temperature of 25°C and cooled by holding the pressure at 4.9 MPa for 3 minutes to produce a press plate with a thickness of approximately 0.5 mm.

[0132] (2) Method for preparing a laminate of a sample and an aluminum (Al) sheet The sample press plate obtained by the press plate preparation method and a commercially available 50 μm thick aluminum sheet (manufactured by UACJ Corporation, 1N30_H18_B1-1 (1N30 standard, hard double-sided gloss specification)) were cut to dimensions of 50 mm x 60 mm. The surfaces of the sample press plate and aluminum sheet were wiped with a cloth soaked in ethanol, and the sample press plate and aluminum sheet were overlapped on each wiped surface, placed in a heat press mold with dimensions: 50 mm x 60 mm, thickness 0.5 mm, and pressed at 4.9 MPa for 5 minutes using a heat press machine with a surface temperature of 180 ° C. Then, it was transferred to a press machine with a surface temperature of 25 ° C. and cooled by holding it at a pressure of 4.9 MPa for 3 minutes to prepare a laminate of the sample press plate and aluminum sheet.

[0133] (3) Method for measuring adhesive strength of laminate The laminate obtained by the laminate preparation method was cut into 10 mm widths, and the adhesive strength was measured by T-peeling at a speed of 50 mm / min using a Tensilon (manufactured by Toyo Seiki Co., Ltd.) tensile tester. The adhesive strength was expressed in units of N / 10 mm. If the adhesive strength was very strong, the sample layer or the base layer would yield and even break during the peel test. This is a phenomenon that occurs because the adhesive strength of the laminate shows a higher strength than the lower tensile breaking strength of the sample layer or the base layer, and it can be judged that the adhesiveness is very high. If the adhesive strength cannot be measured due to this phenomenon, the adhesive strength measurement result is written as "not peelable," and it is judged that the adhesive strength is more highly bonded than the adhesive strength value measured. If the laminate can be easily peeled off by hand, or peeled off when the laminate is removed from the press mold, it is judged that there is no adhesion, and the adhesive strength measurement result is written as 0 N.

[0134] 9.Method of measuring maximum take-off speed (MDS) Using a Toyo Seiki Capillograph, the resin, which had been heated and stabilized at 190°C in the furnace, was extruded from an orifice with an inner diameter of 2.095 mm and a length of 8 mm at a piston speed of 10 mm / min, and the extruded molten resin was pulled at a speed of 4 m / min to obtain the initial test state. After that, the take-up speed was increased at a rate of 1.67 m / sec, and the take-up speed at which the resin broke was measured. This was repeated at least twice, and the average value was taken as the MDS.

[0135] 10.Fineness, average diameter Using a Toyo Seiki Capillograph, the resin inside the furnace was heated and stabilized at 190℃ and extruded from an orifice with an inner diameter of 2.095 mm and a length of 8 mm at a piston speed of 5 mm / min, and the extruded molten resin was pulled at a speed of 10 m / min to obtain a fiber with a length of 10 m. Four of these were made, and the weights of each were measured using an electronic balance, and the fineness was calculated based on the average value. The average diameter is the average value of the thread diameters of each sample used in the tensile test described later. The thread diameter of each sample was measured at three points using a dial gauge and the average value was used.

[0136] 11. Fiber Tensile Measurement With reference to JIS L 1013, the samples were measured with a sample length of 10 cm, n=5, using an ORIENTECH tensile tester, RTC-1210A, under the measurement conditions of a chuck distance of 50 mm and a tensile speed of 500 mm / min. The elongation at break was the break elongation, and the load at break was the tensile break load to calculate the tensile break elongation and tensile break strength. The area of ​​the obtained stress-strain curve was also calculated, and this was taken as the break energy (E).

[0137] <Synthesis of metal complexes> Synthesis of B-423 / Ni complex 1) Ligand B-423: Synthesis of 2-bis(2,6-dimethoxyphenyl)phosphano-6-(2,6-diisopropylphenyl)phenol

[0138] [ka] Ligand B-423 was synthesized according to the following scheme. In the following chemical formulas, -OMOM represents a methoxymethoxy group (-OCH2OCH3).

[0139] [ka]

[0140] (i) Synthesis of Compound 2 It was synthesized according to patent document WO2010 / 050256.

[0141] (ii) Synthesis of Compound 3 To a solution of compound 2 (2.64 g, 10.0 mmol) in THF (5.0 ml) was added iso-PrMgCl (2 M, 5.25 ml) at 0° C. The reaction mixture was stirred at 25° C. for 1 h, and then PCl3 (618 mg, 4.50 mmol) was added at −78° C. The reaction mixture was warmed to 25° C. over 3 hours to give a yellow suspension. The solvent was removed under reduced pressure to give a yellow solid. This mixture was used in the next reaction without purification.

[0142] (iii) Synthesis of Compound 5 To a solution of compound 4 (30 g, 220 mmol) in THF (250 ml), n-BuLi (2.5 M, 96 ml) was added at 0° C. and stirred at 30° C. for 1 hour. i Pr)3 (123 g, 651 mmol) was added at -78°C, and the mixture was stirred at 30°C for 2 hours to give a white suspension. Hydrochloric acid (1M) was added to adjust the pH to 6 to 7, and the organic layer was concentrated to obtain a mixture. The resulting mixture was washed with petroleum ether (80 ml) to give 26 g of compound 5.

[0143] (iv) Synthesis of Compound 7 Compound 5 (5.00 g, 27.5 mmol), compound 6 (4.42 g, 18.3 mmol), Pd2(dba)3 (168 mg, 0.183 mmol), s-Phos(2-Dicyclohexylphosphino-2',6'-dimethoxybiphenyl) (376 mg, 0.916 mmol), and K3PO4 (7.35 g, 34.6 mmol) were weighed into a reaction vessel, and toluene (40 ml) was added. This solution was reacted at 110°C for 12 hours to obtain a black suspension. H2O (50 ml) was added and extracted with EtOAc (55 ml x 3). The organic layer was washed with brine (20 ml) and dried over Na2SO4. The organic layer was filtered, the solvent was distilled off under reduced pressure, and the residue was purified using a silica gel column to obtain 1.3 g of an oily substance.

[0144] (v) Synthesis of compound 8 To a solution of compound 7 (6.5 g, 22 mmol) in THF (40 ml), n-BuLi (2.5 M, 9.15 ml) was added dropwise at 0° C., the temperature was raised to 30° C., and the mixture was stirred for 1 hour. The reaction solution was cooled to −78° C., CuCN (2.1 g, 23 mmol) was added, and the mixture was stirred at 30° C. for 1 hour. The reaction solution was cooled to -78°C, and a solution of compound 3 (6.7 g, 20 mmol) in THF (40 ml) was added, followed by stirring at 30°C for 12 hours to obtain a white suspension. To the suspension was added H2O (50 ml) resulting in a white precipitate. The white precipitate was collected by filtration, dissolved in dichloromethane (20 ml), and aqueous ammonia (80 ml) was added thereto, followed by stirring for 3 hours. The product was extracted with dichloromethane (50 ml x 3), dehydrated with Na2SO4, and concentrated to obtain a yellow oily substance, which was purified with a silica gel column to obtain 2.9 g of compound 8.

[0145] (vi) Synthesis of B-423 To a solution of compound 8 (2.9 g, 4.8 mmol) in dichloromethane (20 ml) was added HCl / EtOAc (4 M, 50 ml) at 0° C., and the mixture was stirred at 30° C. for 2 hours to give a pale yellow solution. The solvent was removed under reduced pressure, and dichloromethane (50 ml) was added. Washing with saturated aqueous NaHCO3 solution (100 ml) gave 2.5 g of B-423. The NMR assignment values ​​of the obtained ligand B-423 are shown below. [NMR] 1 H NMR (CDCl3, δ, ppm): 7.49 (t, 1H), 7.33 (t, 1H), 7.22 (m, 4H), 6.93 (d, 1H), 6.81 (t, 1H), 6.49(dd, 4H), 6.46(br, 1H), 3.56(s, 12H), 2.63(sept, 2H), 1.05(d, 6H), 1.04(d, 6H); 31 P NMR(CDCl3, δ, ppm):-61.6(s).

[0146] 2) Synthesis of B-423 / Ni complex All the following operations were carried out under a nitrogen atmosphere. Hereinafter, nickel acetylacetone will be referred to as Ni(acac)2. Ni(acac)2 (90.0 mg, 0.35 mol) was dissolved in toluene (30 mL) and added as a ligand to the B-423 (200 mg, 0.36 mmol) obtained above. The reaction solution was stirred at room temperature for 10 minutes, and the solvent was then removed under reduced pressure to give a deep red-purple solid. The product was washed with hexane (10 mL x 2) and dried under reduced pressure to obtain a reddish purple solid (yield: 247 g, 99%). The NMR assignment values ​​of the obtained metal complex are shown below. [NMR] 1 HNMR(C6D6,δ,ppm):7.65(d,1H), 7.25-7.35(m,3H), 7.07(t,2H), 6.97(d,1H), 6.51(t,1H), 6.2 6(d,4H), 4.83(brs,1H), 3.44(s,12H), 3.14(sept,2H), 1.44(d,6H), 1.29(s,6H), 1.21(d,6H).

[0147] <(Production Examples 1 to 3): Production of Copolymer Precursor (Pp)> A copolymer precursor (Pp) was produced using a transition metal complex (B-423 / Ni complex). The copolymer was produced with reference to Production Example 1 or Production Example 3 described in JP 2016-79408 A. The production conditions and production results, which were appropriately changed such as the metal catalyst type, metal catalyst amount, trioctyl aluminum (TNOA) amount, toluene amount, comonomer type, comonomer amount, ethylene partial pressure, polymerization temperature, and polymerization time, are shown in Table 1, and the physical properties of the obtained copolymer are shown in Table 2.

[0148] [Table 1]

[0149] [Table 2]

[0150] <(Production Examples 4 to 6): Production of Ionomer-Based Resins> Internal volume 1.6m 3 In a SUS316L autoclave equipped with an agitator, 100 kg of the copolymer of Production Example 1, 2.0 kg of paratoluenesulfonic acid monohydrate, and 173 L of toluene were added and stirred at 105°C for 4 hours. 173 L of ion-exchanged water was added, stirred, and allowed to stand, and then the aqueous layer was extracted. Thereafter, the addition and withdrawal of ion-exchanged water was repeated until the pH of the extracted aqueous layer reached 5 or more. The remaining solution was added to a twin-screw extruder (L / D=42) equipped with a 42 mmφ vent device, and the solvent was distilled off by drawing a vacuum through the vent. Furthermore, the resin extruded continuously in the form of a strand from the die at the tip of the extruder was cooled in water and cut with a cutter to obtain resin pellets. In the IR spectrum of the obtained resin, the 850 cm -1 The disappearance of the peak near 1730 cm -1 The decrease in the peak near 1700 cm originates from the carbonyl group of the carboxylic acid (dimer). -1 An increase in the peak near As a result, the decomposition of t-Bu ester and the generation of carboxylic acid were confirmed, and an ionomer base resin was obtained. The physical properties of the obtained resin are shown in Tables 3 and 4. In the following tables, "E", "AA", and "NB" are abbreviations for "ethylene", "acrylic acid", and "norbornene", respectively, as structural units contained in the base resin.

[0151] [Table 3]

[0152] [Table 4]

[0153] <Ionomer production> (1) Preparation of Na ion source A Na ion source was prepared by adding 22 g of ethylene / methacrylic acid (MAA) copolymer (Mitsui Dow Polychemicals, brand: Nucrel N1050H) and 18 g of sodium carbonate to a Labo Plastomill (Roller Mixer R60) manufactured by Toyo Seiki Co., Ltd., equipped with a small mixer with a capacity of 60 ml, and kneading the mixture at 180°C and 40 rpm for 3 minutes.

[0154] (2) Preparation of Zn ion source A Zn ion source was prepared by adding 21.8 g of ethylene / methacrylic acid (MAA) copolymer (Mitsui Dow Polychemicals, brand: Nucrel N1050H) to a Toyo Seiki Co., Ltd. Labo Plastomill: Roller Mixer R60 equipped with a 60 ml small mixer, 18 g of zinc oxide, and 0.2 g of zinc stearate, and kneading at 180 °C and 40 rpm for 3 minutes.

[0155] Example 1: Preparation of E / AA / iBA-based Na ternary ionomer 40 g of the base resin described in Production Example 4 was added to a Labo Plastomill (Roller Mixer R60) manufactured by Toyo Seiki Co., Ltd., equipped with a small mixer with a capacity of 60 ml, and dissolved by kneading for 3 minutes at 160°C and 40 rpm. Thereafter, a Na ion source was added so as to achieve a desired degree of neutralization, and kneading was continued for 5 minutes at 250°C and 40 rpm. In the IR spectrum of the obtained resin, the 1700 cm -1 The peak at 1560 cm originating from the carbonyl group of the carboxylate group decreased. -1 The peak around 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) increased. -1 From the reduction in the peak in the vicinity, it was confirmed that an ionomer with the desired degree of neutralization had been produced. The production results of the obtained ionomer are shown in Table 5, and the pressed sheet physical properties are shown in Table 6.

[0156] Example 2: Preparation of E / AA / iBA-based Zn ternary ionomer Except for the fact that the amount of the Zn ion source was appropriately adjusted and added so as to obtain the desired degree of neutralization, the procedure was the same as in Example 1. The production results of the obtained ionomer are shown in Table 5, and the physical properties of the pressed sheet are shown in Table 6.

[0157] (Example 3): Preparation of E / AA-based Na binary ionomer The base resin and Na ion source described in Production Example 5 were continuously fed into a Toshiba Machine 26 mmφ vented twin-screw extruder (L / D=65) at a blending ratio to obtain a predetermined degree of neutralization, and extrusion was performed under kneading conditions of barrel set temperature 200°C and screw rotation speed 150 rpm, while injecting water at a ratio of 4 parts per 100 parts of the resin fed and removing gas and water generated during kneading from the vent part with a vacuum pump. Furthermore, the resin continuously extruded in the form of strands from the die at the tip of the extruder was cooled in water and cut with a cutter to obtain ionomer pellets. In the IR spectrum of the obtained resin, the 1700 cm -1 The peak at 1560 cm originating from the carbonyl group of the carboxylate group decreased. -1 The peak around 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) increased. -1 From the reduction in the peak in the vicinity, it was confirmed that an ionomer with the desired degree of neutralization had been produced. The production results of the obtained ionomer are shown in Table 5, and the pressed sheet physical properties are shown in Table 6.

[0158] (Example 4): Preparation of E / AA-based Na binary ionomer The same procedure was followed as in Example 3, except that the base resin described in Production Example 6 was used as the base resin, and the amount of the Na ion source was appropriately adjusted and added so as to obtain the desired degree of neutralization. The production results of the obtained ionomer are shown in Table 5, and the pressed sheet physical properties are shown in Table 6.

[0159] (Example 5): Preparation of E / AA-based Zn binary ionomer The same procedure was followed as in Example 3, except that the base resin described in Production Example 6 was used as the base resin, and the amount of the Zn ion source was appropriately adjusted and added so as to obtain the desired degree of neutralization. The production results of the obtained ionomer are shown in Table 5, and the pressed sheet physical properties are shown in Table 6.

[0160] (Comparative Examples 1 and 2): Polyethylene resin composition A polyethylene resin composition obtained by copolymerizing ethylene and an α-olefin by a gas phase method (manufactured by Japan Polyethylene Co., Ltd., brand: Harmolex NC596A (Comparative Example 1)) and a polyethylene resin composition obtained by copolymerizing ethylene and an α-olefin by a slurry method (manufactured by Japan Polyethylene Co., Ltd., brand: Novatec HD HY340 (Comparative Example 2)) were prepared. The physical properties of the press sheets are shown in Table 6.

[0161] [Table 5]

[0162] [Table 6]

[0163] <Creating ionomer fibers> Example 6 The ionomer described in Example 1 was used to prepare fibers using a Capillograph manufactured by Toyo Seiki Seisakusho Co., Ltd. The resin, which had been heated and stabilized at 190°C in a furnace, was extruded from an orifice with an inner diameter of 2.095 mm and a length of 8 mm at a piston speed of 5 mm / min, and the extruded molten resin was taken up at a speed of 10 m / min to prepare ionomer fibers. The physical properties of the ionomer fibers are shown in Table 7.

[0164] Example 7 The same as Example 6 was used, except that the ionomer described in Example 2 was used. The physical properties of the ionomer fiber are shown in Table 7.

[0165] Example 8 The same procedure was followed as in Example 6, except that the ionomer described in Example 3 was used. The physical properties of the ionomer fiber are shown in Table 7.

[0166] Comparative Example 3 An E / AA-based bifunctional hyperbranched ionomer resin (manufactured by Mitsui DuPont Polychemicals Co., Ltd., brand: HIMILAN HIM1605) was prepared, which is a copolymer of ethylene, methacrylic acid, and sodium methacrylate, and was produced by a high-pressure radical process. The physical properties of the ionomer fiber are shown in Table 7.

[0167] Comparative Example 4 An E / AA-based bifunctional hyperbranched ionomer resin (SK Chemical Co., Ltd., brand: PRIMACOR IO 1706) produced by a high-pressure radical process was prepared. The physical properties of the ionomer fiber are shown in Table 7.

[0168] [Table 7]

[0169] <Consideration of the results of the Examples and Comparative Examples> Haze Looking at the Examples and Comparative Examples in Table 6, the haze values ​​of all the Examples are 35 or less, while the Comparative Examples are all over 70, meaning that the Examples have higher transparency. From this, it can be said that the ionomers of the present invention have clear coloring and excellent transparency when made into fibers and textiles. ·Al adhesive strength Looking at the Examples and Comparative Examples in Table 6, all of the Examples have adhesive strength to aluminum sheets, but none of the Comparative Examples adhere to aluminum sheets. In other words, this suggests that the ionomer of the present invention has adhesive properties with different materials, and when compounded, it maintains its shape more easily than conventional polyethylene resins, and when used as a blend, it suggests that it can impart the flexibility and cold impact resistance of polyethylene due to its high affinity with different resins. Maximum take-off speed (MDS) Looking at the Examples and Comparative Examples in Table 7, all of the Examples have MDS values ​​of 100 m / min or more, and more specifically, MDS values ​​of 190 m / min or more, which are almost at the upper limit (200 m / min) of MDS measurement. On the other hand, the Comparative Examples have MDS values ​​of less than 50 m / min. In terms of production efficiency, it is preferable that the fibers do not break even at high take-up speeds, and it can be said that the higher the MDS value, the better. From this, it can be said that the ionomers related to the present invention have higher MDS values ​​and therefore are superior in high-speed spinnability. Breaking energy (E) Looking at the Examples and Comparative Examples in Table 7, the Examples all have breaking energies exceeding 100 J / mm, while the Comparative Examples have E values ​​of 100 J / mm or less. Since E is the area of ​​the stress-strain curve, it can be considered as the energy required for breaking, that is, impact strength. Since a larger E value indicates better impact strength, it can be said that the ionomers of the present invention have better impact strength. [Industrial Applicability]

[0170] The ionomer of the present invention has superior high-speed spinning performance and impact resistance, and has superior adhesive performance to heterogeneous materials with high polarity, compared to conventional polyethylene resins and ionomers with a hyperbranched structure. In addition, it has the inherent advantages of polyethylene resins, such as light weight, water resistance, superior cold impact resistance compared to ester-based resins and amide-based resins, and flexibility. By utilizing these characteristics, it is expected to be used in a wide range of applications, for example, as a nonwoven fabric to replace paper, or to develop materials with flexibility and cold impact resistance by combining with ester-based resins or amide-based resins.< / e> < / e> < / e> < / e>

Claims

1. A fiber resin composition containing a linear ethylene ionomer.

2. The linear ethylene ionomer has an absolute complex modulus G measured by a rotational rheometer. * The fiber resin composition according to claim 1, which is an ionomer having a phase angle δ at σ = 0.1 MPa of 50 degrees to 75 degrees.

3. 2. The resin composition for fibers according to claim 1, wherein the linear ethylene ionomer is a copolymer (P) comprising, as essential constituent units, structural units (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms, and structural units (B) derived from a monomer having a carboxy group and / or a dicarboxylic acid anhydride group, and at least a portion of the carboxy groups and / or dicarboxylic acid anhydride groups in the copolymer (P) are converted to a metal-containing carboxylate containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table.

4. The copolymer (P) 13 4. The fiber resin composition according to claim 3, wherein the number of methyl branches calculated by C-NMR is 5 or less per 1,000 carbon atoms.

5. The resin composition for fibers according to claim 3, wherein the structural unit (A) is a structural unit derived from ethylene.

6. The resin composition for fibers according to claim 3, characterized in that the copolymer (P) contains the structural unit (B) in an amount of 2 to 20 mol % (the total of all structural units constituting the copolymer is taken as 100 mol %).

7. 4. The fiber resin composition according to claim 3, wherein the metal ion is a metal ion of Group 1 of the periodic table.

8. 4. The fiber resin composition according to claim 3, wherein the metal ion is a metal ion of Group 2 of the periodic table.

9. The resin composition for fibers according to claim 3, wherein the linear ethylene ionomer further contains, in addition to the structural unit (A) and the structural unit (B), a structural unit (C) which is a compound having one or more carbon-carbon double bonds in its molecular structure, as an essential structural unit.

10. The fiber resin composition according to claim 9, wherein the structural unit (C) in the copolymer (P) is a non-cyclic monomer represented by the following general formula (1) or a cyclic monomer represented by the following general formula (2): [Formula 1] [In general formula (1), T 1 ~T 3 each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, or a cyano group; T 4 is a substituent selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, or a cyano group. [chemical 2] [In general formula (2), R 1 ~R 12 may be the same or different and are selected from the group consisting of a hydrogen atom, a halogen atom, and a hydrocarbon group having 1 to 20 carbon atoms; R 9 and R 10 , and R 11 and R 12 may combine together to form a divalent organic group, R 9 Or R 10 And, R 11 Or R 12 may form a ring together. In addition, n represents 0 or a positive integer, and when n is 2 or more, R 5 ~R 8 may be the same or different in each repeating unit.

11. 11. The resin composition for fibers according to claim 10, wherein the structural unit (C) in the copolymer (P) is a non-cyclic monomer represented by the general formula (1).

12. 11. The fiber resin composition according to claim 10, wherein the structural unit (C) in the copolymer (P) is a cyclic monomer represented by the general formula (2).

13. The resin composition for fibers according to claim 9, characterized in that the copolymer (P) contains the structural unit (C) in an amount of 0.001 mol % to 20.000 mol % when the total of all structural units constituting the copolymer (P) is taken as 100 mol %.

14. The fiber resin composition according to claim 3, wherein the copolymer (P) is a copolymer obtained by hydrolysis of a precursor copolymer produced using a transition metal catalyst containing a transition metal of Groups 8 to 11 of the periodic table.

15. 15. The fiber resin composition according to claim 14, wherein the transition metal catalyst is a transition metal catalyst comprising a phosphorus sulfonic acid or phosphorus phenol ligand and nickel or palladium.

16. An ethylene-based fiber formed using the fiber resin composition according to any one of claims 1 to 15.

17. An ethylene-based fiber, comprising an ethylene-based resin as a resin component, characterized in that the maximum take-off speed (MDS) is 100 m / min or more when measured using a capillograph under measurement conditions of a temperature of 190°C, an orifice having a length of 8,000 mm and a hole diameter of 2.085 mm, and a piston speed of 10 mm / min.

18. An ethylene-based fiber, comprising an ethylene-based resin as a resin component, characterized in that a tensile breaking elongation of 100% or more is obtained when a 30 dtex fiber is subjected to a tensile test with a chuck distance of 65 mm and a tensile speed of 500 mm / min.

19. The ethylene-based fiber is a fiber containing an ethylene-based resin as a resin component, characterized in that the breaking energy (E) calculated from a stress-strain curve obtained when a 30 dtex fiber is subjected to a tensile test with a chuck distance of 65 mm and a tensile speed of 500 mm / min is 100 J / mm or more.

20. A composite fiber formed by using the fiber resin composition according to claim 1 and at least one resin other than said fiber resin composition.

21. 2. An ethylene-based hollow fiber molded from the fiber resin composition according to claim 1.

Citation Information

Patent Citations

  • Conjugate fiber

    JP1995238420A

  • Method for producing fiber material

    JP2012219402A

  • Method for producing ethylenic ionomer, and the ethylenic ionomer

    JP2016079408A

  • Poly(phenylene ether) fiber, method of production, and article made from same

    JP2017502179A

  • Multinary polar group-containing olefin copolymer

    JP2019112623A