Analysis method of metal-containing sample
The method of multiple X-ray CT imaging and normalization addresses the limitations of existing techniques by accurately analyzing metal particle size, shape, and distribution in metal-containing samples, enhancing efficiency and reducing evaluation time.
Patent Information
- Application Number
- JP2023058142
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing methods using MLA and X-ray CT equipment struggle to accurately and efficiently analyze the size, shape, distribution, and abundance ratio of metal particles in metal-containing samples due to limitations in resolution and sample amount variability, leading to inconsistent and inaccurate results.
A method involving multiple X-ray CT imaging at different distances, followed by normalization and threshold setting to integrate particle size distributions, ensuring accurate evaluation of metal particles by adjusting for sample amount and resolution differences.
Enables precise and efficient analysis of metal particles by ensuring accurate detection of a wide range of sizes while minimizing evaluation time and reducing variability, achieving results comparable to chemical analysis.
Smart Images

Figure 2024145687000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for analyzing a metal-containing sample. [Background technology]
[0002] An example of a metal-containing sample is a reduction product obtained when Ni oxide ore such as saprolite is reduced to produce Fe-Ni alloys. This reduction product contains metals (metal particles) such as Fe-Ni alloys and slag (non-metallic substances), with the metals being scattered in the slag as fine particles.
[0003] When recovering fine metal particles scattered in the slag, it is desirable to aggregate the fine metal particles scattered in the slag to make them larger in order to improve smelting efficiency. Therefore, it is useful to obtain information on the size, shape, distribution state, and abundance ratio of metal particles contained in a metal-containing sample. As a method for measuring the ratio of metal components, a method has been proposed in which shape parameters such as the volume, equivalent spherical diameter, and sphericity of particles are analyzed using an automatic mineral analyzer (so-called MLA) and an X-ray CT device (for example, Patent Document 1). In addition, there is also a method for measuring the content of metal components by performing chemical analysis on a metal-containing sample. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-34372 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the method of using MLA and X-ray CT scanners in combination described above, by linking the mineral species data identified by MLA with the brightness data from X-ray CT measurements, information such as the particle volume, equivalent spherical diameter, and sphericity of particles of a specific mineral species in a sample can be obtained by X-ray CT measurements. Methods that employ chemical analysis can measure the metal content, but cannot obtain information such as the size, shape, and distribution of metal particles. Therefore, the method of using MLA and X-ray CT scanners in combination described above can be applied to collect information such as the size, shape, distribution, and abundance ratio of metal particles contained in metal-containing samples.
[0006] However, when fine metal particles are included in X-ray CT measurement, the resolution or pixel size may not allow accurate detection of the fine metal particles. Also, when a small number of coarse metal particles are included, the numerical values indicating the presence ratio, such as the volume ratio, may vary greatly depending on the sample amount and sampling accuracy. In other words, X-ray CT measurement has problems in terms of reducing the detectable particle size and reducing the variation. Therefore, it was sometimes impossible to accurately and efficiently analyze information on metal particles in metal-containing samples, such as the shape, number, distribution state, and position.
[0007] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a technique for accurately and efficiently analyzing information about metal particles contained in a metal-containing sample. [Means for solving the problem]
[0008] The first aspect of the present invention is preparing a metal-containing sample comprising metal particles present in a non-metallic material; an image acquisition step of imaging the metal-containing sample with a plurality of different sample amounts by changing an imaging distance from an X-ray generation source to the metal-containing sample using an X-ray CT device, and acquiring a plurality of CT images having different imaging fields according to the imaging distance; an analysis step of acquiring a plurality of particle size distributions, which indicate a relationship between the particle size and the number of the metal particles contained in the metal-containing sample, from each of the plurality of CT images; A normalization step of normalizing the plurality of particle size distributions by a sample amount that changes according to an imaging distance when acquiring the CT image to obtain a plurality of normalized particle size distributions; an extraction and integration step of comparing one normalized particle size distribution acquired at a predetermined shooting distance with another normalized particle size distribution acquired at a longer shooting distance, setting a particle size threshold with which the number of metal particles correlates, extracting a normalized particle size distribution less than the threshold from the one normalized particle size distribution, and extracting a normalized particle size distribution equal to or greater than the threshold from the other normalized particle size distributions, for each of the plurality of normalized particle size distributions; and evaluating the metal particles contained in the metal-containing sample based on the extracted normalized particle size distribution. A method for analyzing a metal-containing sample is provided.
[0009] The second aspect of the present invention is the method according to the first aspect, In the extraction and integration step, the threshold value is set within a range of three times or more the resolution corresponding to the photographing distance when the other normalized particle size distribution is obtained.
[0010] A third aspect of the present invention relates to a method for producing a composition comprising the steps of: In the extraction and integration step, the threshold value is set from a particle size range in which the ratio of the number of particles in the one normalized particle size distribution to the number of particles in the other normalized particle size distribution is 0.5 to 1.5 times.
[0011] A fourth aspect of the present invention is the method according to any one of the first to third aspects, In the image acquiring step, the ratio between the two sample amounts at close shooting distances is set to be 3 to 100 times the sample amount at the relatively long shooting distance.
[0012] A fifth aspect of the present invention is the method according to any one of the first to third aspects, In the normalization step, when the amount of sample in the CT image captured at the maximum shooting distance is A and the amount of sample in the CT image captured at the other shooting distances is B, the particle size distributions acquired at the other shooting distances are normalized by multiplying the number by A / B. Effect of the Invention
[0013] According to the present invention, information on metal particles contained in a metal-containing sample can be analyzed accurately and efficiently. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a flow chart showing a method for analyzing a metal-containing sample according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram for explaining the imaging field of view when a CT image is taken using an X-ray CT apparatus. [Diagram 3] FIG. 3 shows a particle size distribution obtained in the analysis step in one embodiment of the present invention. [Figure 4] FIG. 4 shows the normalized particle size distribution obtained in the normalization step in one embodiment of the present invention. [Diagram 5] FIG. 5 shows the normalized particle size distribution obtained for sample 1. [Figure 6] FIG. 6 shows the normalized particle size distribution obtained for sample 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <One embodiment of the present invention> Hereinafter, a method for analyzing a metal-containing sample according to one embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a flow chart showing a method for analyzing a metal-containing sample according to one embodiment of the present invention. Fig. 2 is a diagram for explaining the imaging field of view when a CT image is captured using an X-ray CT device.
[0016] (Preparation process S1) First, as shown in FIG. 1, a metal-containing sample to be evaluated is prepared.
[0017] A metal-containing sample is composed of metal particles present (or scattered) in a non-metallic substance. The metal-containing sample is, for example, a reduction product obtained by reduction of Ni oxide ore such as saprolite. The metal particles contained in the reduction product are metals such as Fe-Ni alloys. The non-metallic substance contained in the reduction product is slag, and the compound form is, for example, Fe 2 O 3 , Al 2 O 3 , CaO, MgO, SiO 2 And so on.
[0018] The shape of the metal-containing sample may be either a lump or a powder, as long as it does not interfere with the X-ray CT measurement. However, a powder is preferable in order to fill a specified sample container and obtain a specified field of view. The particle size of the metal-containing sample in powder form varies depending on the manufacturing process, origin, and source of the metal-containing sample, and the information to be obtained by the X-ray CT measurement. For example, if the metal-containing sample is a reduction product obtained by reducing Ni oxide ore such as saprolite, and information such as the size, shape, distribution, and abundance ratio of fine metal particles scattered in the slag is to be known, the necessary information cannot be obtained if the metal particles are pulverized to such an extent that the size and shape of the metal particles cannot be determined. In such a case, air-cooled slag that has been crushed to a maximum of about 6 mm is used. For example, if the granular slag is produced by the water granulation shot method, i.e., by dropping a molten material into a jet water stream, there are cases where crushing or pulverization is not necessary. When the metal-containing sample is in powder form, if there are too many voids, the air layer may become a permeable layer and interfere with precise measurement, so it is necessary to adjust the apparent density by tapping. In other words, it is preferable for the particle size of the metal-containing sample to be 6 mm or less.
[0019] (Image acquisition step S2) Next, the above-mentioned metal-containing sample is placed in a container (capsule) for X-ray CT measurement, and the capsule containing the metal-containing sample is introduced into the X-ray CT device.
[0020] An X-ray CT (Computed Tomography) apparatus irradiates an object sample with X-rays while rotating it 360 degrees, and evaluates the internal structure of a substance in a non-destructive and three-dimensional manner by utilizing the difference in the amount of X-ray absorption for each material of each part of the sample. As shown in FIG. 2, the X-ray CT apparatus 1 is configured to include an X-ray source 10, a detector 20, and a stage (not shown) on which a capsule is placed. The X-ray source 10 is configured to irradiate X-rays by expanding them in a cone shape, for example, using a cone beam method. The detector 20 can be, for example, a flat panel detector, and can obtain a transmission image by detecting X-rays that pass through a metal-containing sample. The stage is disposed between the X-ray source 10 and the detector 20, and is configured to be rotatable and movable between the X-ray source 10 and the detector 20. In the X-ray CT apparatus 1, the stage is moved to a predetermined position, and then the metal-containing sample in the capsule is irradiated with X-rays, and the transmission image is obtained by detecting the X-rays that pass through the metal-containing sample. The capsule is then rotated and X-rays are irradiated to obtain multiple radiographs, and finally a three-dimensional CT image is obtained from these multiple radiographs.
[0021] In this embodiment, the imaging distance from the X-ray source to the capsule (metal-containing sample) is changed, imaging is performed with a plurality of different sample amounts, and a plurality of CT images having different imaging fields according to the imaging distance are obtained. In this embodiment, as shown in FIG. 2, an example will be described in which imaging is performed at three imaging distances d1 to d3, and three CT images P1 to P3 are obtained. <d2<d3となる。
[0022] The CT image P1 obtained at the shooting distance d1 has the shortest shooting distance and the highest magnification. Therefore, the CT image P1 has a small shooting field of view (hereinafter also referred to as FOV (Field Of View)) and the observed sample amount is the smallest. On the other hand, the magnification of the CT image P1 is high, so the minimum pixel size is small and the resolution is the highest. In other words, the CT image obtained at the short shooting distance d1 can display a small sample amount with high resolution. Here, the FOV indicates the size of the shooting area observed at a specified distance, and is indicated by the diameter of the shooting area displayed as a cylinder in FIG. 2, for example. The sample amount indicates the weight or volume of a part of the sample contained in the capsule that is photographed by the penetration of X-rays. The sample amount varies in response to the change in the shooting distance and the change in the penetration area of X-rays.
[0023] On the other hand, as the shooting distance becomes longer, such as d2 and d3, the magnification ratio becomes smaller. Therefore, the FOV of CT image P2 and CT image P3 becomes larger according to the shooting distance, and the amount of the observed sample also increases. On the other hand, the resolution decreases in response to the shooting distance becoming longer, and the resolution is the lowest at shooting distance d3. In other words, as the shooting distance becomes longer, the resolution decreases, but the amount of the observed sample can be increased.
[0024] According to the study by the present inventors, the CT image P1 acquired at a short shooting distance d1 has a high resolution, so that even fine metal particles contained in a metal-containing sample can be captured. However, the grain size of metal particles in a metal-containing sample may vary, and if the amount of sample to be captured is too small, the grain size of the entire metal particles in the metal-containing sample may not be evaluated accurately. For example, when one coarse metal particle is included in the CT image P1, it is not clear whether the metal particle is present uniformly throughout the entire metal sample or locally, and the grain size distribution of the metal particles may not be evaluated accurately. In order to improve the evaluation accuracy, it is necessary to increase the amount of sample, and it is necessary to repeatedly capture the CT image P1 at a short shooting distance d1. In this case, the evaluation time is long, and the workability is significantly reduced.
[0025] On the other hand, for example, in the case of CT image P3 acquired at a long shooting distance d3, since the amount of sample is large, it is not necessary to repeatedly acquire CT images as in the case of CT image P1, and the decrease in workability can be suppressed. However, the resolution of CT image P3 is low, and among the metal particles contained in the metal-containing sample, fine metal particles that are below the resolution cannot be observed. Therefore, neither CT image P1 nor CT image P3 can accurately evaluate the metal particles contained in the metal-containing sample over a wide range of particle sizes.
[0026] For example, in a CT image with an FOV of 30 mm, the amount of sample observed is 20 g, whereas in a CT image with an FOV of 7 mm, the amount of sample observed is 0.2 g. When the FOV is 7 mm, CT images must be acquired 100 times to ensure the same amount of sample as when the FOV is 30 mm. In addition, when the FOV is 30 mm, the resolution is about 90 μm, and metal particles smaller than 90 μm may not be detected.
[0027] In this way, using only one CT image acquired at a given shooting distance can result in a significant reduction in workability due to a small sample amount, or an inability to perform an accurate evaluation due to low resolution, depending on the shooting distance.
[0028] For this reason, in this embodiment, three CT images having different imaging fields are obtained by changing the imaging distance. Then, the analysis step S3, the normalization step S4, the extraction and integration step S5, and the evaluation step S6 are performed on these CT images.
[0029] In the image acquisition step S2, the multiple shooting distances may be appropriately changed according to the range of particle sizes that metal particles contained in the metal-containing sample can have. From the viewpoint of performing the extraction and integration step S5 described later with high accuracy, the ratio of the sample amounts of the two samples with close shooting distances is preferably set to 3 times or more and 100 times or less, and more preferably 3 times or more and 25 times or less, of the sample amount of the relatively long shooting distance, and more preferably 3 times or more and 25 times or less. For example, the sample amount of the sample at the shooting distance d2 may be set to 3 times or more and 100 times or less, and the sample amount of the sample at the shooting distance d3 may be set to 3 times or more and 100 times or less, and the sample amount of the sample at the shooting distance d2 may be set to 3 times or more and 100 times or less, and the sample amount of the sample at the shooting distance d3 may be set to 3 times or more and 100 times or less, of the sample amount at the shooting distance d2. From the viewpoint of performing the extraction and integration step S5 described later with high accuracy, it is preferable that the sample amount at the maximum shooting distance is set to 3 times or more and 100 times or less, of the sample amount at the minimum shooting distance, among the sample amounts at the multiple shooting distances.
[0030] In the image acquisition step S2, the shortest shooting distance is not particularly limited as long as it can detect fine metal particles contained in the metal-containing sample on the CT image, and may be changed appropriately depending on the size of the fine metal particles to be detected. The lower limit of detection is the better, but it cannot be determined in general because it depends on the performance of the device. In general, it is recommended to set the shooting distance to a value that realizes a resolution that can detect fine metal particles with a particle size of 7 μm or more.
[0031] The magnification ratio indicates the ratio of the distance from the focal point of the X-ray source 10 to the capsule (metal-containing sample) relative to the distance from the focal point of the X-ray source 10 to the detector 20. The minimum pixel size indicates the value obtained by dividing the pixel size originating from the detector 20 by the magnification ratio.
[0032] (Analysis process S3) Next, each of the three acquired CT images is analyzed to obtain multiple particle size distributions that show the relationship between the particle size and number of metal particles contained in the metal-containing sample.
[0033] In CT images, the amount of X-ray absorption differs depending on the material of the metallic particles and non-metallic substances in a metal-containing sample. In a metal-containing sample, the greater the density, thickness, atomic number, etc. of the component, the lower the intensity of the transmitted X-rays, and vice versa. In CT images, metal particles in a metal-containing sample are denser than non-metallic substances, such as slag, and therefore appear with high brightness. Slag has a relatively low density and therefore appears with low brightness.
[0034] In this embodiment, for example, voxels that are displayed with high brightness are extracted from the CT images, and the particle size and number of metal particles are obtained to obtain a particle size distribution. In this embodiment, the particle size distribution is obtained for each of three CT images having different shooting fields.
[0035] Specifically, each particle size distribution indicates the number of metal particles with particle sizes x1 to x11, as shown in Fig. 3. Fig. 3 shows the particle size distribution acquired in the analysis step S3 in one embodiment of the present invention, with the horizontal axis indicating the particle size of the metal particles and the vertical axis indicating the number of metal particles. Since the sample amounts of the three CT images differ depending on the shooting distance, the particle size distributions obtained from each CT image are information based on different sample amounts. For example, the particle size distribution obtained from CT image P3 with a large sample amount tends to have a larger number of particles with the same particle size than CT image P1 with a small sample amount.
[0036] (Standardization process S4) Next, the three particle size distributions are normalized by the sample amount.
[0037] In this embodiment, in order to eliminate differences in sample amounts for each particle size distribution, multiple particle size distributions are normalized by the sample amount. This results in multiple normalized particle size distributions in which differences in sample amounts have been eliminated. Each normalized particle size distribution has the same sample amount due to normalization, and differences in sample amounts are eliminated.
[0038] Although the normalization method is not particularly limited, when the sample amount in the CT image captured at the maximum shooting distance is A, and the sample amount in the CT image captured at the other shooting distance is B, it is preferable to normalize the particle size distribution acquired at the other shooting distance by multiplying the number by A / B. In this embodiment, when the sample amount in the CT image P3 captured at the maximum shooting distance d3 is A, the sample amount in the CT image P1 is B1, and the sample amount in the CT image P2 is B2, it is preferable to multiply the number by A / B1 for the particle size distribution obtained from the CT image P1, and the number by A / B2 for the particle size distribution obtained from the CT image P2. This makes it possible to correct the particle size distribution obtained from the CT image P1 or the CT image P2, which has a relatively small sample amount, to have the same sample amount as the CT image P3.
[0039] The normalized particle size distribution based on each CT image is, for example, as shown in Fig. 4. Fig. 4 shows the normalized particle size distribution obtained in the normalization step in one embodiment of the present invention, where the horizontal axis indicates the particle size of the metal particles, and the vertical axis indicates the number of metal particles.
[0040] (Extraction / integration step S5) Next, the particle size range that can guarantee the accuracy of the count is identified and extracted from the three normalized particle size distributions. In normalized particle size distributions, the longer the shooting distance, the lower the resolution, so the greater the sample amount in CT images P2 and P3, the lower the accuracy of the count in the small particle size range. On the other hand, the shorter the shooting distance and the smaller the sample amount, the greater the variation in large particle sizes, so it becomes more difficult to guarantee the accuracy of the count in the large particle size range in CT images P2 and P1, the smaller the sample amount. Therefore, the particle size range that can guarantee the accuracy of the count is identified and extracted from each normalized particle size distribution.
[0041] The method for identifying the range of particle sizes that can guarantee the accuracy of the number is to compare one normalized particle size distribution obtained at a predetermined shooting distance with another normalized particle size distribution obtained at a longer shooting distance, and set a particle size threshold value with which the number of metal particles correlates. In this embodiment, the normalized particle size distributions obtained at the closest shooting distance are compared to each other, and the correlation of the number distribution at each particle size is confirmed.
[0042] Specifically, first, the normalized particle size distributions obtained from the CT image P1 with the shortest shooting distance and the CT image P2 with the shortest shooting distance are compared. Then, a particle size range with a small discrepancy in number is identified. For example, in FIG. 4, since there is a correlation between the numbers of particles in the CT image P1 and the CT image P2 when the particle size is x6 or more, the particle size x6 is set as the threshold T1 with which the number of metal particles correlates between the CT image P1 and the CT image P2. In the particle size range less than x6 (x5 or less), the normalized particle size distribution obtained from the CT image P1 reflects the particle size distribution of metal particles with higher accuracy, and in the particle size range of x6 or more, the normalized particle size distribution obtained from the CT image P2 reflects the particle size distribution of metal particles with higher accuracy. Next, the same operation is performed on the normalized particle size distributions obtained from the CT image P3 and the CT image P2 with the shortest shooting distance. 4, since there is a correlation between the numbers of metal particles in CT image P2 and CT image P3 for particle sizes of x9 or more, particle size x9 is set as threshold value T2 at which the numbers of metal particles in CT image P2 and CT image P3 correlate. In the particle size range less than x9 (x8 or less), the normalized particle size distribution obtained from CT image P2 reflects the particle size distribution of metal particles with higher accuracy, and in the particle size range of x9 or more, the normalized particle size distribution obtained from CT image P3 reflects the particle size distribution of metal particles with higher accuracy.
[0043] In this way, after setting a particle size threshold value that can ensure the accuracy of the number for each normalized particle size distribution from a comparison of each normalized particle size distribution, a number distribution is extracted from each normalized particle size distribution.
[0044] In addition, in the extraction and integration step S5, it is preferable to set the particle size threshold based on the resolution according to the shooting distance of the CT image, that is, the pixel size. Specifically, for one normalized particle size distribution acquired at a predetermined shooting distance and another normalized particle size distribution with a longer shooting distance, it is preferable to set the particle size threshold from a range of three times or more the resolution (pixel size) of the other normalized particle size distribution. For example, in the case of FIG. 4, for the normalized particle size distribution acquired from the CT image P1 and the CT image P2, it is preferable to set the threshold from a range of three times or more the resolution (pixel size) of the CT image P2. Also, for the normalized particle size distribution acquired from the CT image P2 and the CT image P3, it is preferable to set the threshold from a range of three times or more the resolution (pixel size) of the CT image P3. According to the study by the present inventors, it was found that even particles with a particle size equal to or larger than the resolution (pixel size) of metal particles cannot be detected with high accuracy. On the other hand, it was found that particles with a particle size equal to or larger than the resolution (pixel size) can be detected with high accuracy.
[0045] In addition, in the extraction and integration step S5, when setting a threshold value for the particle size with which the number of metal particles correlates, it is advisable to set the threshold value from within a particle size range in which the ratio of the number of particles in one given normalized particle size distribution to that of another normalized particle size distribution with a longer shooting distance is 0.5 to 1.5 times. If the ratio of the number of particles is within the above range, the deviation of the normalized particle size distribution is small, and the accuracy of the number of particles can be ensured within the range above the threshold value.
[0046] (Evaluation step S6) Next, the metal particles contained in the metal-containing sample are evaluated based on the extracted and integrated normalized particle size distribution. For this evaluation, for example, the weight ratio of the metal particles contained in the metal-containing sample can be determined from the particle size and number of the metal particles. In addition to the weight ratio, the shape and distribution state of the metal particles and their shape and position can also be evaluated and analyzed based on the particle size threshold value that correlates with the number of metal particles set above.
[0047] In this way, information on metal particles contained in a metal-containing sample can be evaluated.
[0048] <Effects of this embodiment> According to this embodiment, one or more of the following advantages are achieved.
[0049] For comparison, when evaluating metal particles contained in a metal-containing sample based on a CT image acquired at a single shooting distance, the following problem occurs.
[0050] For example, when evaluating metal particles from a particle size distribution obtained based on a CT image acquired at a short shooting distance, the resolution is high and it is possible to detect even fine metal particles. However, since the amount of sample is small, if one coarse metal particle is included, it may not be possible to determine whether it reflects the original particle size distribution of the metal-containing sample. In other words, the accuracy of the number of metal particles with large diameters may not be guaranteed. To solve this, it is possible to increase the amount of sample by evaluating multiple times at the same shooting distance, but this will increase the time required for evaluation and reduce workability.
[0051] On the other hand, when evaluating metal particles from a particle size distribution obtained based on a CT image taken at a long shooting distance, it is possible to obtain the original particle size distribution of the metal-containing sample in the coarse particle size range because of the large sample amount. However, the resolution of the CT image is low in that particle size distribution, and fine metal particles cannot be detected accurately, so the accuracy of the number of small metal particles may not be guaranteed.
[0052] In this way, when evaluating metal-containing samples by acquiring CT images at a single shooting distance, the resolution of the CT image is inversely proportional to the amount of sample, making it difficult to obtain an accurate particle size distribution over a wide range of particle sizes in a short period of time.
[0053] (a) In this embodiment, first, in the image acquisition step S2 and the analysis step S3, particle size distributions are obtained from three CT images P1 to P3 captured at three different shooting distances (d1 to d3). Then, since these particle size distributions are information based on the sample amount according to the shooting distance, each particle size distribution is normalized by the sample amount in the normalization step S4. As a result, normalized particle size distributions normalized to the same sample amount are obtained. Since the normalized particle size distributions have different shooting distances, the particle size ranges that can ensure the accuracy of the number of metal particles are different. Therefore, in the extraction and integration step S5, the three normalized particle size distributions with the closest shooting distances are compared with each other, and a particle size threshold value with which the number of metal particles is correlated is set. For example, as shown in FIG. 4, the normalized particle size distribution with the shooting distance d1 is compared with the normalized particle size distribution with the shooting distance d2, and the particle size range with which the number of metal particles is correlated is identified, and the threshold value T1 is set. Similarly, the normalized particle size distribution at the shooting distance d2 is compared with the normalized particle size distribution at the shooting distance d3, and the particle size threshold T2 is set. Next, a particle size range that can ensure the accuracy of the number of metal particles is extracted from each normalized particle size distribution. Specifically, less than the threshold T1 is extracted from the normalized particle size distribution at the shooting distance d1, more than the threshold T1 and less than the threshold T2 is extracted from the normalized particle size distribution at the shooting distance d2, and more than the threshold T2 is extracted from the normalized particle size distribution at the shooting distance d3. By extracting from each normalized particle size distribution in this way, the accuracy of the number of metal particles at each particle size can be maintained high, so that the metal-containing sample can be accurately evaluated from fine metal particles to coarse metal particles in the evaluation step S6. Moreover, even if the CT image is acquired three times, information on the largest sample amount corresponding to the longest shooting distance d3 can be acquired. In other words, it is possible to shorten the evaluation time while increasing the sample amount for accurate evaluation.
[0054] (b) In the extraction and integration step S5, it is preferable to compare one normalized particle size distribution acquired at a predetermined shooting distance with another normalized particle size distribution acquired at a longer and closest shooting distance, and set the particle size threshold from a range of three times or more the resolution of the other normalized particle size distribution, i.e., the pixel size. In this embodiment, the particle size threshold T1 for the normalized particle size distribution acquired at shooting distances d1 and d2 may be selected from a range of three times or more the resolution (pixel size) of the CT image P2 at the shooting distance d2. Similarly, the particle size threshold T2 for the normalized particle size distribution acquired at shooting distances d2 and d3 may be selected from a range of three times or more the resolution (pixel size) of the CT image P3 at the shooting distance d3. This makes it possible to obtain information on the number of metal particles with higher accuracy from each normalized particle size distribution.
[0055] (c) In addition, in the extraction and integration step S5, it is preferable to set a threshold value from the range of particle diameters in which the ratio of the number of metal particles is 0.5 to 1.5 times when comparing one normalized particle size distribution with another normalized particle size distribution. If the ratio of the number is within the above range, the correlation of the number between one normalized particle size distribution and another normalized particle size distribution becomes higher, so that it is possible to obtain information on the number of metal particles with higher accuracy.
[0056] (d) In the image acquisition step S2, it is preferable that the ratio of the two sample amounts at close shooting distances is such that the sample amount at the relatively long shooting distance is 3 to 100 times the sample amount at the relatively short shooting distance. This makes it possible to more reliably extract a particle size range with guaranteed accuracy in number from each normalized particle size distribution in the extraction and integration step S5, and to more accurately evaluate metal particles in the evaluation step S6.
[0057] (e) In the normalization step S4, when the amount of sample in the CT image taken at the maximum shooting distance is A and the amount of sample in the CT image taken at the other shooting distances is B, it is preferable to normalize the particle size distributions obtained at the other shooting distances by multiplying the number by A / B. This allows the metal particles to be evaluated more accurately in the evaluation step S6.
[0058] <Other embodiments> Although an embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the spirit of the present invention.
[0059] In the above embodiment, the case where CT images are acquired at three different shooting distances has been described, but CT images may be acquired at two different shooting distances, and the analysis step S3 to the evaluation step S6 may be performed in the same manner as in the above embodiment. In this case, it is preferable that the maximum shooting distance is 3 to 100 times the minimum shooting distance. Note that four or more different shooting distances may be selected. There is no particular limit to the upper limit, but since the evaluation time increases as the shooting distance increases, it is preferable to set it appropriately within a range that does not significantly deteriorate workability. EXAMPLES
[0060] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0061] (Sample 1) In Sample 1, a crushed material obtained by crushing the reduction product obtained by the reduction treatment of Ni oxide ore (saprolite) was prepared as a metal-containing sample. This crushed material is mainly composed of slag containing metal oxides, and metals are present in particulate form within it. This crushed material was crushed so that it would pass through a 2 mm sieve.
[0062] Next, the crushed material was placed in a container (capsule) for X-ray CT measurement and introduced into an X-ray CT device ("CTLabHX130" manufactured by Rigaku Corporation). For sample 1, the shooting distance between the X-ray source and the metal-containing sample was changed, and images were taken so that the field of view (FOV) size was 7 mm, 20 mm, and 30 mm, and three CT images with different shooting fields were obtained. Hereinafter, if the FOV size is 7 mm, it will be written as "FOV7". The amount of each sample was 0.2 g for FOV7, 5 g for FOV20, and 20 g for FOV30. The resolution, i.e., pixel size, in each CT image was 7.1 μm for FOV7, 20 μm for FOV20, and 30 μm for FOV30.
[0063] Next, each acquired CT image was analyzed, and the particle size and number of metal particles contained in the metal-containing sample were measured to obtain a particle size distribution. Next, each particle size distribution was normalized to the sample amount of FOV30. Specifically, the number was multiplied by 100 (20 / 0.2) for the particle size distribution of FOV7, and by 4 (20 / 5) for the particle size distribution of FOV20. As a result, three normalized particle size distributions were obtained. The normalized particle size distributions obtained are shown in Figure 5. Figure 5 shows the normalized particle size distribution obtained in sample 1, with the horizontal axis indicating the particle size [μm] and the vertical axis indicating the logarithm of the number.
[0064] Next, each normalized particle size distribution was compared, and a particle size threshold value with which the number of metal particles correlated was set. When the normalized particle size distributions of FOV7 and FOV20 were compared, the correlation of the number of particles was high in the particle size range of 63 μm or more, so the threshold value for FOV7 and FOV20 was set to 63 μm. Similarly, when the normalized particle size distributions of FOV20 and FOV30 were compared, the correlation of the number of particles was high in the particle size range of 90 μm or more, so the threshold value for FOV20 and FOV30 was set to 90 μm. The particle size threshold value was set from a particle size range that was 3 times or more the resolution of each FOV, that is, the pixel size, and in which the ratio of the number of particles in the normalized particle size distributions to be compared was 0.5 times or more and 1.5 times or less.
[0065] Next, particle size distributions were extracted based on the particle size thresholds set for each normalized particle size distribution. Specifically, the particle size range of 8.1 μm to 53 μm was extracted for the normalized particle size distribution of FOV7, the particle size range of 63 μm to 75 μm for the normalized particle size distribution of FOV20, and the particle size range of 90 μm or more for the normalized particle size distribution of FOV30, and then integrated into one.
[0066] Next, the metal particles contained in the metal-containing sample were evaluated based on the extracted and integrated normalized particle size distribution. For sample 1, the content (weight ratio) of metal particles contained in the metal-containing sample was analyzed as information on metal particles. Specifically, the weight ratio of metal (metal) contained in the metal-containing sample was evaluated based on the particle size and number of metal particles. As a result, it was confirmed that the content of metal contained in the metal-containing sample was 10.7% by weight.
[0067] (Sample 2) In sample 2, the metal-containing sample was evaluated by performing the same operations as sample 1, except that CT images were obtained by capturing images at two shooting distances to be FOV7 and FOV30. The normalized particle size distribution obtained in sample 2 is shown in Figure 6. Figure 6 shows the normalized particle size distribution obtained in sample 2, with the horizontal axis indicating particle size [μm] and the vertical axis indicating the logarithm of the number of particles. In sample 2, the normalized particle size distributions of FOV7 and FOV30 were compared, and since the correlation of the number of particles was high in the particle size range of 90 μm or more, the threshold value for FOV7 and FOV30 was set to 90 μm. Then, the metal sample was evaluated based on the extracted normalized particle size distribution, and it was confirmed that the content of the metal contained in the metal sample in sample 2 was 11.1 wt% by weight.
[0068] (Sample 3) For sample 3, the particle size distribution was obtained from a CT image taken at a single shooting distance so that the FOV was 7, and the metal sample was evaluated in the same manner as for sample 1, except that normalization was omitted. As a result, it was confirmed that the content of metals in the metal-containing sample for sample 3 was 22.0% by weight.
[0069] (Sample 4) For sample 4, the particle size distribution was obtained from a CT image taken at a single shooting distance so that the FOV was 30, and the metal sample was evaluated in the same manner as for sample 1, except that normalization was omitted. As a result, it was confirmed that the content of metals in the metal-containing sample for sample 4 was 7.5% by weight.
[0070] (Evaluation Results) In order to compare the evaluation results of Samples 1 to 4, the metal content of the metal-containing sample was measured by chemical analysis, and it was confirmed that the metal content was 15.4% by weight. This confirmed that Samples 1 and 2 can evaluate metal samples with an accuracy close to that of chemical analysis while shortening the evaluation time compared to Samples 3 and 4.
[0071] In sample 3, which was evaluated based only on the CT image from FOV7, the metal content was confirmed to be higher than that of the chemical analysis. This is presumably because the imaging distance was short and the imaging field of view had a small sample amount, and coarse metal particles were included, so the particle size distribution did not accurately reflect the original particle size distribution of the metal sample.
[0072] Additionally, it was confirmed that sample 4, which was evaluated based only on the CT image with FOV30, had a lower metal content than the chemical analysis. This is presumably because the CT image with FOV30 has low resolution and cannot accurately detect the number of minute metal particles.
[0073] On the other hand, in samples 1 and 2, which were extracted and integrated from multiple CT images and evaluated, the detectable particle size was reduced and the variation in analysis due to coarse metal particles was suppressed, so it is presumed that the metal samples were evaluated more accurately than samples 3 and 4. According to the analysis method for metal-containing samples of the present invention, the particle size distribution of metal particles scattered in non-metallic substances can be obtained accurately and efficiently, and further, it was found that the weight ratio of metal particles can be rapidly evaluated, although only as a guideline. Incidentally, in general chemical analysis, all metal elements are quantified regardless of whether they are in the form of a compound or a simple substance, so in order to quantify only those in the form of simple metals, a special analysis method is required, which requires a lot of time and effort.
[0074] As described above, by taking multiple CT images of a metal-containing sample at different shooting distances, obtaining a particle size distribution from the multiple CT images, normalizing it, and appropriately extracting a specified particle size range based on the normalized particle size distribution, it is possible to evaluate metal particles contained in the metal-containing sample with high accuracy while shortening the measurement time. [Explanation of symbols]
[0075] 1 X-ray CT device 10 X-ray source 20 Detector
Claims
1. preparing a metal-containing sample comprising metal particles present in a non-metallic material; an image acquisition step of imaging the metal-containing sample with a plurality of different sample amounts by changing an imaging distance from an X-ray generation source to the metal-containing sample using an X-ray CT device, and acquiring a plurality of CT images having different imaging fields according to the imaging distance; an analyzing step of acquiring a plurality of particle size distributions, which indicate a relationship between the particle size and the number of the metal particles contained in the metal-containing sample, from each of the plurality of CT images; A normalization step of normalizing the plurality of particle size distributions by a sample amount that changes according to an imaging distance when the CT image is acquired, to obtain a plurality of normalized particle size distributions; an extraction and integration process for each of the plurality of normalized particle size distributions, in which one normalized particle size distribution obtained at a predetermined shooting distance is compared with another normalized particle size distribution obtained at a longer shooting distance, a threshold value of particle size with which the number of metal particles is correlated is set, and a normalized particle size distribution less than the threshold value is extracted from the one normalized particle size distribution, and a normalized particle size distribution equal to or greater than the threshold value is extracted from the other normalized particle size distributions; and evaluating the metal particles contained in the metal-containing sample based on the extracted normalized particle size distribution. Methods for the analysis of metal-containing samples.
2. In the extraction and integration step, the threshold value is set within a range of three or more times the resolution corresponding to the shooting distance when the other normalized particle size distribution is obtained. The method for analyzing a metal-containing sample according to claim 1 .
3. In the extraction and integration step, the threshold value is set from a particle size range in which the ratio of the number of particles in the one normalized particle size distribution to the number of particles in the other normalized particle size distribution is 0.5 to 1.5 times. The method for analyzing a metal-containing sample according to claim 1 .
4. In the image acquisition step, a ratio of the two sample amounts at close shooting distances is set to 3 times or more and 100 times or less of the sample amount at a relatively long shooting distance. A method for analyzing a metal-containing sample according to any one of claims 1 to 3.
5. In the normalization step, when the amount of sample in the CT image taken at the maximum shooting distance is A and the amount of sample in the CT image taken at the other shooting distance is B, the particle size distributions obtained at the other shooting distances are normalized by multiplying the number by A / B. A method for analyzing a metal-containing sample according to any one of claims 1 to 3.
Citation Information
Patent Citations
Multi-resolution CT imaging system and method
CN114199907A
Grain image analysis device
JP1996136439A
Apparatus and method for producing high-resolution CT reproductions of a target including important target regions.
JP2011510313A
Particle size distribution measurement method and system for granular material
JP2013257188A
Sample analysis method
JP2020034372A