Molecular crystal, electrochemical device, and method for producing molecular crystal

A molecular crystal with a specific sulfolane-to-lithium salt molar ratio of 2.0 to 3.1 forms a hexagonal structure, addressing ionic conductivity limitations and enabling effective use in electrochemical devices.

JP2024145887AActive Publication Date: 2024-10-15TOYOTA JIDOSHA KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023058447
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Conventional molecular crystals have limitations in terms of ionic conductivity.

Method used

A molecular crystal composed of sulfolane and a lithium salt with a molar ratio of 2.0 to 3.1, which can form a hexagonal crystal structure, enhancing ionic conductivity.

Benefits of technology

The molecular crystal exhibits excellent ionic conductivity, suitable for use as a solid electrolyte in electrochemical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145887000013
    Figure 2024145887000013
  • Figure 2024145887000014
    Figure 2024145887000014
  • Figure 2024145887000001
    Figure 2024145887000001
Patent Text Reader

Abstract

To provide a molecular crystal with excellent lithium ion conductivity.SOLUTION: A molecular crystal of the present disclosure includes sulfolane and a lithium salt represented by the following chemical formula, and the molar ratio of the sulfolane to the lithium salt is 2.0 or more and less than 3.0.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application discloses molecular crystals, electrochemical devices and methods for making molecular crystals. [Background technology]

[0002] Patent Document 1 discloses a molecular crystal solid electrolyte containing an electron-donating sulfur-based organic compound and a lithium salt. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-214510 A Summary of the Invention [Problem to be solved by the invention]

[0004] Conventional molecular crystals have room for improvement in terms of ionic conductivity. [Means for solving the problem]

[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A molecular crystal comprising sulfolane and a lithium salt represented by the following chemical formula (1): a molar ratio of the sulfolane to the lithium salt is 2.0 or more and 3.1 or less; Molecular crystal. [ka] <Aspect 2> The molecular crystal of embodiment 1, having a hexagonal crystal structure, Molecular crystal. <Aspect 3> A molecular crystal according to aspect 1 or 2, a molar ratio of the sulfolane to the lithium salt is equal to or greater than 2.0 and less than 3.0; Molecular crystal. <Aspect 4> 1. An electrochemical device comprising an ion conductor, The ion conductor has a molecular crystal according to any one of aspects 1 to 3. Electrochemical devices. <Aspect 5> A method for producing a molecular crystal, comprising the steps of: Mixing sulfolane and a lithium salt represented by the following chemical formula (1) to obtain a solution containing the sulfolane and the lithium salt, and having a molar ratio of the sulfolane to the lithium salt of 2.0 or more and 3.1 or less; cooling the solution to obtain the molecular crystals. A method for producing molecular crystals. [ka] Effect of the Invention

[0006] The molecular crystal of the present disclosure has excellent ionic conductivity. [Brief description of the drawings]

[0007] [Figure 1] 1 shows a schematic diagram of an example of the configuration of an electrochemical device. [Diagram 2] 1 shows the X-ray diffraction patterns of the solid samples of Examples 1 to 5 and Comparative Examples 2, 5 and 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the technology of the present disclosure will be described, but the technology of the present disclosure is not limited to the embodiments described below.

[0009] 1. Molecular Crystals A molecular crystal according to one embodiment includes sulfolane and a lithium salt represented by the following chemical formula (1): The molar ratio of the sulfolane to the lithium salt is 2.0 or more and 3.1 or less. [ka]

[0010] 1.1 Sulfolane The molecular crystal according to the present embodiment includes sulfolane. Sulfolane is a type of electron-donating sulfur-based organic compound and is represented by the following chemical formula (2). In the molecular crystal, the sulfolane represented by the following chemical formula (2) may or may not be chemically bonded to the lithium salt represented by the above chemical formula (1). The molecular crystal according to one embodiment may have a hexagonal structure due to the orientation of each molecule while maintaining the molecular structure of sulfolane and the anion molecular structure of the lithium salt. [ka]

[0011] 1.2 Lithium salts The molecular crystal according to the present embodiment contains a specific lithium salt. The lithium salt is lithium 1,1,2,2,3,3-hexafluoropropane-1,3-disulfonimide represented by the above chemical formula (1). According to the findings of the present inventors, the ionic conductivity of the above sulfolane alone and the above lithium salt alone is difficult to measure due to high resistance. Only when the above sulfolane and the above lithium salt are combined as in the molecular crystal according to the present embodiment, excellent ionic conductivity is exhibited.

[0012] 1.3 Molar ratio In the molecular crystal according to the present embodiment, the molar ratio of the sulfolane to the lithium salt (sulfolane / lithium salt) is 2.0 or more and 3.1 or less. That is, the molecular crystal according to the present embodiment contains 2.0 or more and 3.1 or less moles of sulfolane to 1 mole of lithium salt. According to the knowledge of the present inventor, if the molar ratio is too large, a part of the sulfolane becomes liquid and the molecular crystal cannot maintain an appropriate form. In addition, if the molar ratio is too small, the ion conductivity tends to decrease. In the molecular crystal according to the present embodiment, the molar ratio is 2.0 or more and 3.1 or less, so that the ion conductivity is specifically improved. The molar ratio may be 2.0 or more and 3.0 or less, 2.0 or more and less than 3.0, or 2.0 or more and 2.9 or less. The molar ratio of the sulfolane to the lithium salt in the molecular crystal (sulfolane / lithium salt) can be determined by various analytical devices.

[0013] 1.4 Crystal structure The molecular crystal according to the present embodiment may have a specific crystal structure by containing the sulfolane and the lithium salt. For example, the molecular crystal according to the present embodiment may have a hexagonal crystal structure. In the molecular crystal having a hexagonal crystal structure, a Li layer exists in the xy plane direction of the hexagonal crystal structure, and it is considered that there is substantially no component that hinders the diffusion of Li in the xy plane, and Li is easily diffused. As a result, it is considered that excellent ion conductivity is expressed. The molecular crystal according to the present embodiment may be composed of a single phase of a hexagonal crystal structure, or may have other crystal structures in addition to the hexagonal crystal structure. In particular, it is considered that even more excellent ion conductivity is expressed when it is composed of a single phase of a hexagonal crystal structure.

[0014] 1.5 Other 1.5.1 Morphology at room temperature The molecular crystal according to the present embodiment may be, for example, a solid at room temperature (20° C.) in an air atmosphere. That is, the molecular crystal according to the present embodiment may have excellent ion conductivity within the solid.

[0015] 1.5.2 Other ingredients The molecular crystal according to the present embodiment may be composed of only the sulfolane and lithium salt, or may contain some other components in addition to these. In the molecular crystal according to the present embodiment, for example, the total of the sulfolane and lithium salt may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less.

[0016] 1.5.3 Purpose The molecular crystal according to the present embodiment has excellent ion conductivity and can be used for various purposes. The molecular crystal according to the present embodiment may be used, for example, as a solid electrolyte.

[0017] 2. Electrochemical Devices The molecular crystal according to the present embodiment has excellent ionic conductivity and can be used as a constituent material of various electrochemical devices. That is, an electrochemical device according to an embodiment includes an ionic conductor, and the ionic conductor has the molecular crystal according to the present disclosure. Hereinafter, a battery will be exemplified as an electrochemical device, but the molecular crystal according to the present disclosure can also be used in electrochemical devices other than batteries.

[0018] As shown in FIG. 1, a battery 100 according to an embodiment includes a positive electrode active material layer 20, an electrolyte layer 30, and a negative electrode active material layer 40. At least one of the positive electrode active material layer 20, the electrolyte layer 30, and the negative electrode active material layer 40 includes the molecular crystal of the present disclosure. That is, in the battery 100, the molecular crystal of the present disclosure can function as a solid electrolyte. In the battery 100, the configuration other than the molecular crystal as a solid electrolyte is the same as that of the conventional battery. For example, the configuration described in JP 2014-186937 A or JP 2021-068556 A can be adopted. As shown in FIG. 1, the battery 100 may include a positive electrode collector 10 electrically connected to the positive electrode active material layer 20, or a negative electrode collector 50 electrically connected to the negative electrode active material layer 40. As the configuration of the collector, a known configuration may be adopted. In addition to the above configuration, the battery 100 may also include a general configuration as a battery. For example, tabs and terminals. The battery 100 may have each of the above-mentioned components housed inside an exterior body. Any known exterior body for a battery may be used as the exterior body. A plurality of batteries 100 may be electrically connected in any manner and stacked in any manner to form a battery pack. The shape of the battery 100 may be, for example, a coin type, a laminate type, a cylindrical type, a square type, and the like. The battery 100 may be a lithium ion battery. The battery 100 may be a primary battery or a secondary battery. The battery 100 may be manufactured, for example, through a process of forming each of the above-mentioned layers in a dry or wet manner.

[0019] 3. Manufacturing method of molecular crystals The molecular crystal of the present disclosure may be produced, for example, by the following method. That is, the method for producing a molecular crystal according to one embodiment includes the steps of: Step S1: mixing sulfolane and a lithium salt represented by the above chemical formula (1) to obtain a solution containing the sulfolane and the lithium salt, and having a molar ratio of the sulfolane to the lithium salt of 2.0 or more and 3.1 or less; Step S2: Cooling the solution to obtain the molecular crystals.

[0020] 3.1 Process S1 In step S1, sulfolane and the lithium salt represented by the above chemical formula (1) are mixed to obtain a solution containing the sulfolane and the lithium salt, and the molar ratio of the sulfolane to the lithium salt is 2.0 to 3.1. For example, a melt of sulfolane is obtained, and then a predetermined amount of lithium salt is added thereto, and the solution is obtained by dissolving the lithium salt in the melt while heating. There is no particular limitation on the mixing conditions, and any conditions may be used as long as the sulfolane and the lithium salt can be appropriately mixed to obtain a solution. During mixing, the sulfolane and the lithium salt may be stirred. For example, the sulfolane and the lithium salt may be uniformly mixed by adding the lithium salt to the melt of sulfolane to dissolve the lithium salt, and then stirring for 1 minute to 10 hours. There is no particular limitation on the stirring means.

[0021] 3.2 Process S2 In step S2, the solution obtained in step S1 is cooled to obtain molecular crystals. There are no particular limitations on the cooling conditions. For example, the solution may be allowed to cool to room temperature in an air atmosphere. EXAMPLES

[0022] As described above, one embodiment of the technology of the present disclosure has been described, but the technology of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the technology. The technology of the present disclosure will be described in more detail below while showing examples, but the technology of the present disclosure is not limited to the following examples.

[0023] 1. Preparation of evaluation samples 1.1 Comparative Example 1 A lithium salt represented by the following chemical formula (1) and sulfolane represented by the following chemical formula (2) were weighed out so that the molar ratio of the sulfolane to the lithium salt was 3.5. The sulfolane was heated to form a molten liquid, and the lithium salt was added thereto. The lithium salt was dissolved by stirring while heating. After stirring for 2 hours, the mixture was allowed to cool to room temperature in the air, thereby obtaining an evaluation sample according to Comparative Example 1. The obtained evaluation sample was a mixed phase of solid and liquid at room temperature (20°C) in the air. [ka]

[0024] 1.2 Example 1 Except for the molar ratio of the sulfolane to the lithium salt being 3.1, an evaluation sample according to Example 1 was obtained in the same manner as in Comparative Example 1. The obtained evaluation sample was a solid at room temperature (20° C.) in an air atmosphere, and was a molecular crystal containing sulfolane and a lithium salt.

[0025] 1.3 Example 2 Except for the molar ratio of the sulfolane to the lithium salt being 3.0, an evaluation sample according to Example 2 was obtained in the same manner as in Comparative Example 1. The obtained evaluation sample was a solid at room temperature (20° C.) in an air atmosphere, and was a molecular crystal containing sulfolane and a lithium salt.

[0026] 1.4 Example 3 Except for the molar ratio of the sulfolane to the lithium salt being 2.9, an evaluation sample according to Example 3 was obtained in the same manner as in Comparative Example 1. The obtained evaluation sample was a solid at room temperature (20° C.) in an air atmosphere, and was a molecular crystal containing sulfolane and a lithium salt.

[0027] 1.5 Example 4 Except for the molar ratio of the sulfolane to the lithium salt being 2.5, an evaluation sample according to Example 4 was obtained in the same manner as in Comparative Example 1. The obtained evaluation sample was a solid at room temperature (20° C.) in an air atmosphere, and was a molecular crystal containing sulfolane and a lithium salt.

[0028] 1.6 Example 5 Except for the molar ratio of the sulfolane to the lithium salt being 2.0, an evaluation sample according to Example 5 was obtained in the same manner as in Comparative Example 1. The obtained evaluation sample was a solid at room temperature (20° C.) in an air atmosphere, and was a molecular crystal containing sulfolane and a lithium salt.

[0029] 1.7 Comparative Example 2 Except for the molar ratio of the sulfolane to the lithium salt being 1.5, an evaluation sample according to Comparative Example 2 was obtained in the same manner as in Comparative Example 1. The obtained evaluation sample was a solid at room temperature (20° C.) in an air atmosphere, and was a molecular crystal containing sulfolane and a lithium salt.

[0030] 1.8 Comparative Example 3 LiPF6 as a lithium salt and sulfolane represented by the above chemical formula (2) were weighed out so that the molar ratio of the sulfolane to the lithium salt was 4.0. The sulfolane was heated to form a molten liquid, and the lithium salt was added thereto. The lithium salt was dissolved by stirring while heating. After stirring for 2 hours, the mixture was allowed to cool to room temperature in the air, thereby obtaining an evaluation sample according to Comparative Example 3. The obtained evaluation sample was a mixed phase of solid and liquid at room temperature (20°C) in the air.

[0031] 1.9 Comparative Example 4 Lithium bis(fluorosulfonyl)imide (LiFSI (also referred to as lithium bis(fluorosulfonyl)amide, LiFSA)) as a lithium salt and sulfolane represented by the above chemical formula (2) were weighed out so that the molar ratio of the sulfolane to the lithium salt was 1.5. The sulfolane was heated to form a molten liquid, and the lithium salt was added thereto. The lithium salt was dissolved by stirring while heating. After stirring for 2 hours, the mixture was allowed to cool to room temperature in the air, thereby obtaining an evaluation sample according to Comparative Example 4. The obtained evaluation sample was a mixed phase of solid and liquid at room temperature (20° C.) in the air.

[0032] 1.10 Comparative Example 5 Except for the molar ratio of the sulfolane to the lithium salt being 1.0, an evaluation sample according to Comparative Example 5 was obtained in the same manner as in Comparative Example 4. The obtained evaluation sample was a solid at room temperature (20° C.) in an air atmosphere, and was a molecular crystal containing sulfolane and a lithium salt.

[0033] 1.11 Comparative Example 6 Lithium bis(trifluoromethanesulfonyl)imide (LiFSI (also referred to as lithium bis(trifluoromethanesulfonyl)amide, LiTFSA)) as a lithium salt and sulfolane represented by the above chemical formula (2) were weighed out so that the molar ratio of the sulfolane to the lithium salt was 2.0. The sulfolane was heated to form a molten liquid, and the lithium salt was added thereto. The lithium salt was dissolved by stirring while heating. After stirring for 2 hours, the mixture was allowed to cool to room temperature in the air, thereby obtaining an evaluation sample according to Comparative Example 6. The obtained evaluation sample was liquid at room temperature (20° C.) in the air.

[0034] 1.12 Comparative Example 7 A sample for evaluation according to Comparative Example 7 was obtained in the same manner as in Comparative Example 6, except that the molar ratio of the sulfolane to the lithium salt was 1.5. The obtained sample for evaluation was a mixed phase of solid and liquid at room temperature (20° C.) in the air.

[0035] 1.13 Comparative Example 8 A sample for evaluation according to Comparative Example 8 was obtained in the same manner as in Comparative Example 6, except that the molar ratio of the sulfolane to the lithium salt was 1.0. The obtained sample for evaluation was a solid at room temperature (20° C.) in an air atmosphere, and was a molecular crystal containing sulfolane and a lithium salt.

[0036] 1.14 Comparative Example 9 The lithium salt represented by the above chemical formula (1) and ethyl methyl sulfone represented by the following chemical formula (3) were weighed out so that the molar ratio of the ethyl methyl sulfone to the lithium salt was 1.0. The ethyl methyl sulfone was heated to form a molten liquid, and the lithium salt was added thereto. The lithium salt was dissolved by stirring while heating. After stirring for 2 hours, the mixture was allowed to cool to room temperature in the air, thereby obtaining an evaluation sample according to Comparative Example 9. The obtained evaluation sample was liquid at room temperature (20°C) in the air. [ka]

[0037] 1.15 Comparative Example 10 The lithium salt represented by the above chemical formula (1) and 3-methylsulfolane represented by the following chemical formula (4) were weighed out so that the molar ratio of the 3-methylsulfolane to the lithium salt was 1.5. The 3-methylsulfolane was heated to form a molten liquid, and the lithium salt was added thereto. The lithium salt was dissolved by stirring while heating. After stirring for 2 hours, the mixture was allowed to cool to room temperature in the air, thereby obtaining an evaluation sample according to Comparative Example 10. The obtained evaluation sample was a mixed phase of solid and liquid at room temperature (20°C) in the air. [ka]

[0038] 1.16 Comparative Example 11 The lithium salt represented by the above chemical formula (1) and 1,4-butane sultone represented by the following chemical formula (5) were weighed out so that the molar ratio of the 1,4-butane sultone to the lithium salt was 2.0. The 1,4-butane sultone was heated to form a melt, and the lithium salt was added thereto. The mixture was stirred while being heated to dissolve the lithium salt. After stirring for 2 hours, the mixture was allowed to cool to room temperature in the air, thereby obtaining an evaluation sample according to Comparative Example 11. The obtained evaluation sample was a mixed phase of solid and liquid at room temperature (20°C) in the air. [ka]

[0039] 1.17 Comparative Example 12 The lithium salt represented by the above chemical formula (1) and 1,3-propane sultone represented by the following chemical formula (6) were weighed out so that the molar ratio of the 1,3-propane sultone to the lithium salt was 2.0. The 1,3-propane sultone was heated to form a molten liquid, and the lithium salt was added thereto. The lithium salt was dissolved by stirring while heating. After stirring for 2 hours, the mixture was allowed to cool to room temperature in the air, thereby obtaining an evaluation sample according to Comparative Example 12. The obtained evaluation sample was a mixed phase of solid and liquid at room temperature (20°C) in the air. [ka]

[0040] 2. Ionic Conductivity Measurement Among the above evaluation samples, the evaluation samples according to Examples 1 to 5 and Comparative Examples 2, 5, and 8, which were solid at room temperature, were placed in a press cell and pressed to prepare blocking cells. The blocking cells were subjected to AC impedance measurement to obtain resistance values ​​associated with ion conduction, and ion conductivity was calculated from the cell shape. The measurement conditions were a temperature of 25°C, an amplitude of 10 mV, and a frequency of 1 MHz to 10 mHz.

[0041] 3.Crystal structure analysis Of the above evaluation samples, the evaluation samples according to Examples 1 to 5 and Comparative Examples 2, 5, and 8, which were solid at room temperature, were subjected to X-ray diffraction measurement using CuKα radiation by using an X-ray diffractometer. The measurement conditions were a scan speed of 2° / min and a step width of 0.01°.

[0042] 4. Evaluation Results The evaluation results are shown in the following Table 1. Moreover, the X-ray diffraction patterns of the evaluation samples of Examples 1 to 5 and Comparative Examples 2, 5 and 8 are shown in FIG.

[0043] [Table 1]

[0044] The results shown in Table 1 and FIG. 2 reveal the following: When sulfolane and the lithium salt represented by the chemical formula (1) were used, the evaluation sample according to Comparative Example 1, in which the molar ratio of sulfolane to lithium salt was 3.5, did not form a solid single phase and could not be used as a molecular crystal. In contrast, the evaluation samples according to Examples 1 to 5, in which the molar ratio of sulfolane to lithium salt was 2.0 or more and 3.1 or less, did not form a solid single phase and could not be used as a molecular crystal. -7 The evaluation samples according to Examples 3 to 5, which exhibit an ionic conductivity of more than 1.0×10 S / cm and in particular have a molar ratio of 2.0 or more and less than 3.0 (in particular, 2.9 or less), -6 The ionic conductivity of the evaluation sample according to Comparative Example 2, in which the molar ratio is 1.5, was lower than that of Examples 1 to 5. In addition to a monoclinic crystal structure, an X-ray diffraction peak derived from the lithium salt raw material was confirmed in the evaluation sample according to Comparative Example 2. On the other hand, the evaluation samples according to Examples 1 to 5, which showed high ionic conductivity, were composed of a single phase of a hexagonal crystal structure. It is believed that the hexagonal crystal structure has a path through which Li can diffuse in the xy plane direction, which is thought to have increased the ionic conductivity in the solid. The evaluation sample according to Comparative Example 3, which used LiPF6 as the lithium salt, did not become a solid single phase at any molar ratio up to 4.0. When the lithium salt concentration was higher than that, the lithium salt did not dissolve, and molecular crystals could not be obtained. The evaluation samples according to Comparative Examples 4 and 5, which used LiFSA as the lithium salt, were solid single phase at a molar ratio of 1.0, but the crystal structure was monoclinic and the ionic conductivity was 10 -8 The value was low, on the order of S / cm. The evaluation samples according to Comparative Examples 6 to 8, which used LiTFSA as the lithium salt, were solid single phase at a molar ratio of 1.0, but the crystal structure was monoclinic and the ionic conductivity was 10 -8 The value was low, on the order of S / cm. The evaluation samples according to Comparative Examples 9 to 12, which used an electron donor organic compound other than sulfolane, did not form a solid single phase and could not be used as molecular crystals. This is thought to be because none of them had a stable structure that could become a crystal.

[0045] From the above results, it can be said that the molecular crystals having the following configurations (A) and (B) have excellent ionic conductivity. (A) The molecular crystal contains sulfolane and a lithium salt represented by the above chemical formula (1). (B) The molar ratio of the sulfolane to the lithium salt is 2.0 or more and 3.1 or less. [Explanation of symbols]

[0046] 100 batteries 10 Positive electrode current collector 20 Cathode active material layer 30 Electrolyte layer 40 Negative electrode active material layer 50 Negative electrode current collector

Claims

1. A molecular crystal comprising sulfolane and a lithium salt represented by the following chemical formula (1): a molar ratio of the sulfolane to the lithium salt is 2.0 or more and 3.1 or less; Molecular crystal. [Formula 1]

2. 2. The molecular crystal of claim 1 , having a hexagonal crystal structure, Molecular crystal.

3. 2. The molecular crystal of claim 1 , a molar ratio of the sulfolane to the lithium salt is 2.0 or more and less than 3.0; Molecular crystal.

4. 1. An electrochemical device comprising an ion conductor, The ionic conductor has the molecular crystal according to any one of claims 1 to 3. Electrochemical devices.

5. A method for producing a molecular crystal, comprising the steps of: Mixing sulfolane and a lithium salt represented by the following chemical formula (1) to obtain a solution containing the sulfolane and the lithium salt, and having a molar ratio of the sulfolane to the lithium salt of 2.0 or more and 3.1 or less; and cooling the solution to obtain the molecular crystals. A method for producing molecular crystals. [chemical 2]

Citation Information

Patent Citations

  • Preparation method of high-performance lithium salt

    CN107987035A

  • Preparation method and purification method of compound comprising at least one cyclic ligand structure

    CN109467539A

  • Cyclic perfluoroalkanebis(sulfonyl)imides and methods for preparing such novel four-membered cyclic imides

    JP2000506132A

  • Nonaqueous secondary battery

    JP2015185401A

  • Lithium secondary battery and electrolytic solution

    JP2020017362A