Refreshing fabric and refreshing clothing using the same

A blended yarn fabric with treated natural cellulose and untreated regenerated cellulose fibers, combined with elastic yarns, addresses the slow drying issue of natural fibers and enhances moisture absorption and release, ensuring effective moisture management and comfort in underwear.

JP2024146050APending Publication Date: 2024-10-15KURABO INDUSTRIES LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023058738
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Natural cellulose fibers like cotton absorb moisture slowly and take time to dry, while regenerated cellulose fibers like rayon are difficult to dry once moist, lacking a balanced moisture absorption and release performance suitable for clothing, particularly underwear.

Method used

A blended spun yarn comprising treated natural cellulose fibers with moisture absorption and release properties, and untreated regenerated cellulose fibers, achieving a moisture absorption rate ratio and moisture release rate ratio of 1.05 or more, balanced by incorporating elastic yarns for improved moisture management.

Benefits of technology

The blended yarn fabric exhibits excellent moisture absorption and release properties, maintaining a smooth texture and suitability for underwear, with improved drying performance and durability through balanced moisture management.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146050000001_ABST
    Figure 2024146050000001_ABST
Patent Text Reader

Abstract

To provide a refreshing fabric which is rich in a fiber derived from a natural material, has smooth touch, is excellent in moisture absorbing / releasing properties, and is especially suitable for underwear, and to provide refreshing clothing using the refreshing fabric.SOLUTION: A refreshing fabric contains a blended spun yarn (A) containing a natural cellulosic fiber (a1) subjected to a moisture absorption / desorption process and a regenerated cellulosic fiber (a2) not subjected to the moisture absorption / desorption process. The moisture absorption speed ratio and the moisture desorption speed ratio of the refreshing fabric and a fabric X which is the same as the refreshing fabric except that the fabric X includes a spun yarn composed only of a cotton fiber instead of the blended spun yarn (A) are both 1.05 or more. The blended spun yarn (A) preferably further contains a natural cellulosic fiber (a3) not subjected to the moisture absorption / desorption process.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a refreshing fabric and a refreshing clothing using the same. [Background technology]

[0002] Clothing that comes into direct contact with the skin is expected to have a pleasant texture, be smooth and soft, and be highly hygroscopic and capable of reducing stuffiness, as well as of releasing absorbed moisture.

[0003] Natural cellulose fibers, such as cotton, are environmentally friendly and have excellent texture, dyeability, and water absorption, and are therefore widely used in a variety of clothing. However, cotton fibers have a problem in that the moisture they absorb evaporates slowly, so once they absorb sweat, they take a long time to dry. For this reason, development has been carried out to improve their quick-drying performance.

[0004] Blended spun yarns of regenerated cellulose fibers such as rayon and cotton fibers, and fabrics that mainly contain them, are also known as skin-friendly materials. Regenerated cellulose fibers have moisture absorption properties equal to or greater than cotton, but because the fiber surface is smooth, they feel smoother on the skin and remain smoother than cotton fibers even after repeated washing. In addition, since the material of regenerated cellulose fibers is a natural raw material, unlike synthetic fibers made from petroleum such as polyester and nylon, they can be returned to resources through processing, making them environmentally friendly materials like cotton fibers. However, regenerated cellulose fibers have the problem that they are more difficult to dry than cotton fibers when they absorb moisture.

[0005] Patent Document 1 discloses regenerated cellulose fibers having high moisture absorptive and desorbing properties, in which highly moisture absorptive and desorbing organic fine particles are kneaded into regenerated cellulose fibers. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent Publication No. 2000-290828 Summary of the Invention [Problem to be solved by the invention]

[0007] In recent years, there has been a growing demand for products rich in fibers derived from natural materials. In addition, there is a demand for fabrics that are smooth to the touch and have excellent moisture absorption and release properties, particularly for use in underwear. To provide a refreshing fabric which is rich in fibers derived from natural materials, has a smooth texture and excellent moisture absorption and release properties, and is particularly suitable for use as underwear, and a refreshing clothing using the refreshing fabric. [Means for solving the problem]

[0008] The present invention, in one aspect, comprises: A refreshing fabric comprising a blended spun yarn (A) containing natural cellulosic fibers (a1) that have been subjected to moisture absorption and release processing and regenerated cellulosic fibers (a2) that have not been subjected to moisture absorption and release processing, The present invention relates to a refreshing fabric, in which the moisture absorption rate ratio and the moisture desorption rate ratio between the refreshing fabric and fabric X, which is the same as the refreshing fabric, except that the blended spun yarn (A) is replaced by a spun yarn consisting only of cotton fibers, are both 1.05 or more.

[0009] In one aspect, the present invention relates to a cooling garment comprising the cooling fabric of the present invention. Effect of the Invention

[0010] According to the present invention, it is possible to provide a refreshing fabric that is rich in fibers derived from natural materials, has a smooth texture, has excellent moisture absorption and release properties, and is particularly suitable for use as underwear, and a refreshing clothing using said refreshing fabric. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a front view of an inner garment according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] [Cooling fabric] In one embodiment, the refreshing fabric of the present invention comprises a blended spun yarn (A) containing moisture-absorbing and desorbing natural cellulosic fiber (a1) and non-moisture-absorbing and desorbing regenerated cellulosic fiber (a2) as a main component yarn. The moisture-absorbing and desorbing natural cellulosic fiber (a1) is, for example, a fiber that has been treated to introduce hydrophilic groups such as carboxyl groups into natural cellulosic fiber using a method such as radiation exposure, while the non-moisture-absorbing and desorbing regenerated cellulosic fiber (a2) is a normal regenerated cellulosic fiber that has not been treated. The blended spun yarn (A) may be any of a single yarn, a two-ply yarn, and a three-ply yarn.

[0013] From the viewpoint of achieving both moisture release and moisture absorption, the blended spun yarn (A) preferably further contains natural cellulosic fibers (a3) ​​that have not been moisture-absorbent or desorbent-treated. That is, instead of the regenerated cellulosic fibers (a2) that have not been moisture-absorbent or desorbent-treated, a part of the regenerated cellulosic fibers (a3) ​​that have not been moisture-absorbent or desorbent-treated is preferably used, since this provides a good balance between moisture absorption and moisture release. The refreshing fabric of the present invention is preferably rich in fibers derived from natural materials, and the blended spun yarn (A) is preferably made of only natural cellulosic fibers (a1) that have been moisture-absorbent or desorbent-treated and regenerated cellulosic fibers (a2) that have not been moisture-absorbent or desorbent-treated and regenerated cellulosic fibers (a2) that have not been moisture-absorbent or desorbent-treated and natural cellulosic fibers (a3) ​​that have not been moisture-absorbent or desorbent-treated. When the natural fibers that have not been moisture-absorbent / release-treated contain both the regenerated cellulose fiber (a2) that has not been moisture-absorbent / release-treated and the natural cellulose fiber (a3) ​​that has not been moisture-absorbent / release-treated, both moisture-release and moisture-absorption properties are improved in a well-balanced manner, which is preferable. In other words, a spun yarn obtained by mixing the natural cellulose fiber (a3) ​​that has not been moisture-absorbent / release-treated, the natural cellulose fiber (a1) that has been moisture-absorbent / release-treated, and the regenerated cellulose fiber (a2) that has not been moisture-absorbent / release-treated is preferable because both moisture-release and moisture-absorption properties are improved in a well-balanced manner compared to a spun yarn made only of the natural cellulose fiber (a3) ​​that has not been moisture-absorbent / release-treated.

[0014] In one embodiment, the cool fabric of the present invention may be made only of spun yarn containing the blended spun yarn (A), but in another embodiment, it may contain elastic yarn (B) in addition to the blended spun yarn (A). When the cool fabric of the present invention contains elastic yarn (B) as a constituent yarn, the constituent yarn of the cool fabric of the present invention may be only the blended spun yarn (A) and the elastic yarn (B).

[0015] Regenerated cellulose fibers (a2) such as rayon have inherently high moisture absorption, but when they absorb moisture, they are more difficult to dry than natural cellulose fibers such as cotton. Natural cellulose fibers such as cotton are inherently hygroscopic and heat-generating (Tatsuya Motomiya et al., "Encyclopedia of Fibers," p. 830, left column, March 25, 2002, Maruzen), but their moisture absorption and release properties are improved by moisture absorption and release processing. In the blended spun yarn (A), it is presumed that the moisture release of the regenerated cellulose fibers (a2) is promoted by blending with the moisture absorption and release processed natural cellulose fibers (a1). As a result, the moisture absorption and release properties of the refreshing fabric of the present invention, which contains the blended spun yarn (A) as the main constituent yarn, are excellent, and the moisture absorption and release properties are well balanced. Specifically, the following moisture absorption rate ratio and the following moisture release rate ratio of the refreshing fabric of the present invention are both 1.05 or more. In addition, the refreshing fabric of the present invention contains the regenerated cellulosic fibers (a2), so that it is smooth to the touch and suitable for use as underwear.

[0016] The moisture absorption rate ratio and moisture desorption rate ratio are parameters defined by the evaluation item "Moisture Absorption and Desorption Test (BOKEN Standard: BQE A 034)" established by the General Incorporated Foundation Boken Quality Evaluation Organization, and are calculated from the following (Formula 1) and (Formula 2), respectively. Fabric X is the same fabric as the refreshing fabric, except that it contains 100% by mass of normal cotton fiber spun yarn instead of the blended spun yarn (A). Here, normal cotton fiber means unprocessed cotton fiber that has not been processed for moisture absorption and desorption, nor has it been processed to impart other functions. (Formula 1): The moisture absorption rate ratio (after 1 minute) = the moisture absorption rate of the cooling fabric (per unit area) / the moisture absorption rate of the fabric X (per unit area) (Formula 2): The moisture release rate ratio (after 5 minutes) = the moisture release rate of the cool fabric (per unit mass) / the moisture release rate of the fabric X (per unit mass)

[0017] The moisture absorption rate ratio (per unit area) allows evaluation of the moisture absorption characteristics on the surface, and the moisture desorption rate ratio (per unit mass) allows evaluation of the moisture desorption characteristics up to the inside of the fabric.

[0018] In the present invention, the moisture absorption rate ratio is the moisture absorption rate (μg / cm 2 min) and the moisture absorption rate of fabric X (control product) (μg / cm 2 The moisture release rate ratio is calculated as the ratio of the moisture release rate (mg / g·min) of the refreshing fabric of the present invention to the moisture release rate (mg / g·min) of the fabric X.

[0019] In this test, a test piece (10cm x 10cm) is conditioned in an initial condition box (25°C, 40%RH), then moved to a moisture absorption box (25°C, 80%RH), and left in the moisture absorption box (25°C, 80%RH) until the mass of the test piece reaches equilibrium. It is then returned to the initial condition box (25°C, 40%RH). After conditioning the moisture in the initial condition box, the test piece is moved from the initial condition box to the moisture absorption box, and the mass of the test piece is measured every 10 seconds until it is returned to the initial condition box and the mass of the test piece reaches equilibrium. The moisture absorption rate of the refreshing fabric of the present invention and that of fabric X (control product) are each expressed as the moisture absorption rate per unit area (μg / cm) 1 minute after the test piece is moved to the moisture absorption box (25°C, 80%RH). 2 The moisture release rate of the cooling fabric of the present invention and that of fabric X (comparison product) are each the moisture release rate per unit mass (mg / g min) 5 minutes after the test piece is returned to the initial condition box.

[0020] The moisture absorption rate ratio is 1.05 or more, preferably 1.10 or more, and from the viewpoint of compatibility with moisture release properties, is preferably 4.00 or less.

[0021] The moisture desorption rate ratio is 1.05 or more, preferably 1.10 or more, and from the viewpoint of compatibility with moisture absorption, is preferably 4.00 or less.

[0022] Since "Fabric X" is "same as the refreshing fabric except that it contains a spun yarn made only of cotton fiber instead of the blended spun yarn (A)," the refreshing fabric of the present invention and Fabric X have the same weaving or knitting structure, the presence or absence of elastic yarn described below, and its content. In addition, when the spun yarn constituting the blended spun yarn (A) is a twisted yarn, the twist coefficient K of the spun yarn constituting the blended spun yarn (A) and the spun yarn constituting Fabric X are equal.

[0023] For example, when the yarn constituting an example of the refreshing fabric of the present invention is 100% by mass of blended spun yarn (A), the yarn constituting the fabric X is 100% by mass of spun yarn consisting of only ordinary cotton fibers. When the yarn constituting an example of the refreshing fabric of the present invention is 5% by mass of elastic yarn and 95% by mass of blended spun yarn (A), the yarn constituting the fabric X is 95% by mass of spun yarn consisting of only 5% by mass of elastic yarn and ordinary cotton fibers.

[0024] When the blended spun yarn (A) is a twisted yarn, the twist factor K of the blended spun yarn (A) is preferably 3.6 or more, more preferably 4.0 or more, from the viewpoint of improving coolness, and is preferably 8.5 or less, more preferably 8.0 or less, from the viewpoint of spun yarn quality. If the blended spun yarn (A) is a hard twisted yarn with a twist factor K of 3.6 or more, the fabric has good skin comfort, which is preferable. The twist factor K can be calculated by the following formula. K=t / √S where t: number of twists per inch (2.54 cm), S: British count (multiples of 840 yards (0.9144 m) at a standard weight of 1 pound (0.4536 kg)).

[0025] When the refreshing fabric of the present invention contains elastic yarn (B), the mass ratio of the two yarns is preferably 85-95% by mass of the blended spun yarn (A) and 5-15% by mass of the elastic yarn (B) when the refreshing fabric is taken as 100% by mass. This allows the realization of a refreshing garment that has appropriate moisture absorption and release properties and is resistant to deformation even after repeated washing. From the same viewpoint, the ratio of the blended spun yarn (A) to the elastic yarn (B) is more preferably 88 (blended spun yarn (A)):12 ​​(elastic yarn (B)) to 95:5, and even more preferably 90:10 to 94:6, in mass %.

[0026] When the cooling fabric is taken as 100% by mass, the mass proportion of the moisture absorbing and releasing processed natural cellulosic fiber (a1) is 3 to 50% by mass, more preferably 3 to 40% by mass, even more preferably 4 to 35% by mass, and even more preferably 5 to 30% by mass, from the viewpoint of good moisture absorbing and releasing properties of the cooling fabric.

[0027] The moisture-absorbing and desorbing processed natural cellulosic fiber (a1) is preferably a natural cellulosic fiber to which a compound containing an ethylenically unsaturated double bond is grafted, and more preferably a cotton fiber to which a compound containing an ethylenically unsaturated double bond is grafted. Examples of the compound containing an ethylenically unsaturated double bond include a compound containing one ethylenically unsaturated double bond and one or two carboxy groups (-COOH). Specifically, at least one carboxylic acid selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid, and fumaric acid, or an ester or salt thereof is preferable. When these compounds are chemically bonded to the surface of natural cellulosic fibers such as cotton, a moisture-absorbing and desorbing function having washability can be imparted.

[0028] The graft bond is formed by various reactions, such as a reaction of generating radicals (reactive species) on the surface of natural cellulose-based fibers by irradiating with an electron beam, a reaction of contacting a compound having an ethylenically unsaturated double bond containing a functional group (-OH, -NH2, etc.) with the generated radical to graft the compound onto the surface of the natural cellulose-based fibers, and a reaction of reacting the active species with a carboxy group of the compound to form a covalent bond. The compound containing an ethylenically unsaturated double bond is preferably added in a range of 1 to 40% by mass, more preferably 3 to 35% by mass, and even more preferably 5 to 30% by mass, based on the natural cellulose-based fibers. Within the above range, the moisture absorbing and releasing natural cellulose-based fibers (a1) that have been subjected to moisture absorbing and releasing processing can exhibit moisture absorbing and releasing functions even when they are mixed with other fibers that have not been subjected to moisture absorbing and releasing processing, such as regenerated cellulose-based fibers (a2) that have not been subjected to moisture absorbing and releasing processing, or regenerated cellulose-based fibers (a2) that have not been subjected to moisture absorbing and releasing processing and natural cellulose-based fibers (a3) ​​that have not been subjected to moisture absorbing and releasing processing.

[0029] The graft ratio in the moisture absorbing and releasing processed natural cellulosic fibers (a1) is preferably 1 to 40 wt%, more preferably 3 to 35 wt%, and further preferably 5 to 30 wt%. The amount of the compound having an ethylenically unsaturated double bond used in contact with the fibers is preferably such that the graft ratio falls within the above range. The graft ratio (owf%) is the mass increase rate (wt%) calculated from the mass difference before and after processing, and can be calculated by the following formula. owf is an abbreviation for on the weight of fiber. In the following formula, W g is the mass of the natural cellulosic fiber after processing, and W0 is the mass of the natural cellulosic fiber before processing. Graft rate (owf%) = (W g -W0) / W0×100

[0030] In addition, by setting the mass ratio of the moisture absorbing and releasing treated natural cellulosic fibers (a1) in the blended spun yarn (A) to preferably 3 to 50 mass %, damage (strength deterioration) of the natural cellulosic fibers due to the moisture absorbing and releasing treatment can be compensated for by fibers other than the moisture absorbing and releasing treated natural cellulosic fibers (a1) in the blended spun yarn (A). The damage (strength deterioration) of the natural cellulosic fibers occurs with the generation of radicals (C·) due to the cleavage of C—H bonds among double bonds. The fibers in the blended spun yarn (A) other than the moisture-absorbing and desorbing treated natural cellulosic fibers (a1) are, for example, regenerated cellulosic fibers (a2) that have not been treated for moisture absorption and desorption, or regenerated cellulosic fibers (a2) that have not been treated for moisture absorption and desorption and natural cellulosic fibers (a3) ​​that have not been treated for moisture absorption and desorption.

[0031] In the blended spun yarn (A), the moisture absorption / release treated natural cellulosic fiber (a1) is preferably 3-50% by mass, and the non-moisture absorption / release treated regenerated cellulosic fiber (a2) is preferably 50-97% by mass. More preferably, the moisture absorption / release treated natural cellulosic fiber (a1) is 3-40% by mass, and the non-moisture absorption / release treated regenerated cellulosic fiber (a2) is 60-97% by mass. Even more preferably, the moisture absorption / release treated natural cellulosic fiber (a1) is 4-35% by mass, and the non-moisture absorption / release treated regenerated cellulosic fiber (a2) is 65-96% by mass. Even more preferably, the moisture absorption / release treated natural cellulosic fiber (a1) is 5-30% by mass, and the non-moisture absorption / release treated regenerated cellulosic fiber (a2) is 70-95% by mass.

[0032] When the blended spun yarn (A) contains natural cellulosic fibers (a3) ​​that have not been moisture-absorbing / releasing processed, the amount of the moisture-absorbing / releasing processed natural cellulosic fibers (a1) is preferably 3 to 50 mass%, the amount of the non-moisture-absorbing / releasing processed regenerated cellulosic fibers (a2) is preferably 10 to 70 mass%, and the amount of the non-moisture-absorbing / releasing processed natural cellulosic fibers (a3) ​​is preferably 5 to 80 mass% from the viewpoint of improving moisture absorption and release properties. More preferably, the amount of the moisture-absorbing / releasing processed natural cellulosic fibers (a1) is 3 to 40 mass%, the amount of the non-moisture-absorbing / releasing processed regenerated cellulosic fibers (a2) is 15 to 65 mass%, and the amount of the non-moisture-absorbing / releasing processed natural cellulosic fibers (a3) ​​is 10 to 75 mass%. More preferably, the moisture absorption / release treated natural cellulose fiber (a1) is 4-35% by mass, the non-moisture absorption / release treated regenerated cellulose fiber (a2) is 20-65% by mass, and the non-moisture absorption / release treated natural cellulose fiber (a3) ​​is 15-75% by mass. Even more preferably, the moisture absorption / release treated natural cellulose fiber (a1) is 5-30% by mass, the non-moisture absorption / release treated regenerated cellulose fiber (a2) is 20-65% by mass, and the non-moisture absorption / release treated natural cellulose fiber (a3) ​​is 15-70% by mass. Even more preferably, the moisture absorption / release treated natural cellulose fiber (a1) is 5-20% by mass, the non-moisture absorption / release treated regenerated cellulose fiber (a2) is 30-65% by mass, and the non-moisture absorption / release treated natural cellulose fiber (a3) ​​is 15-65% by mass.

[0033] Furthermore, when the blended spun yarn (A) contains natural cellulosic fibers (a3) ​​that have not been treated for moisture absorption and release, from the viewpoint of achieving both improved moisture absorption and release properties and reduced costs, the amount of the natural cellulosic fibers (a1) that have been treated for moisture absorption and release is preferably 5 to 30 mass%, the amount of the regenerated cellulosic fibers (a2) that have not been treated for moisture absorption and release is preferably 25 to 45 mass%, and the amount of the natural cellulosic fibers (a3) ​​that have not been treated for moisture absorption and release is preferably 25 to 70 mass%. Furthermore, when the blended spun yarn (A) contains natural cellulosic fibers (a3) ​​that have been moisture absorbent and desorbent, from the viewpoints of improving moisture absorption and desorbent properties and improving the balance between moisture absorption and desorbent properties, the amount of moisture absorbent and desorbent natural cellulosic fibers (a1) is preferably 5 to 20 mass%, the amount of regenerated cellulosic fibers (a2) that have not been moisture absorbent and desorbent treated is preferably 35 to 65 mass%, and the amount of natural cellulosic fibers (a3) ​​that have not been moisture absorbent and desorbent treated is preferably 20 to 60 mass%.

[0034] When the blended spun yarn (A) contains natural cellulose fibers (a3) ​​that have not been treated for moisture absorption and release, a part of the natural cellulose fibers (a3) ​​that have not been treated for moisture absorption and release may be replaced with synthetic fibers such as polyester.

[0035] In preparing the moisture absorbing and releasing processed natural cellulosic fiber (a1), examples of the natural cellulosic fiber to be subjected to the moisture absorbing and releasing processing include cotton, hemp, etc., and preferably cotton. Examples of the regenerated cellulosic fiber (a2) that has not been subjected to the moisture absorbing and releasing processing include rayon, which may be made from wood pulp or cotton linters, etc. Among rayons, Modal (registered trademark) made from beech pulp is preferable. Examples of the natural cellulosic fiber (a2) that has not been subjected to the moisture absorbing and releasing processing include cotton, hemp, etc., and preferably cotton.

[0036] In the refreshing fabric of the present invention, the content of fibers derived from natural materials is preferably 85% by mass or more, more preferably 88% by mass or more, and even more preferably 90% by mass or more. In addition, since the refreshing fabric of the present invention is a fabric suitable for use in innerwear such as underwear, the total content of natural cellulose-based fibers (including both natural cellulose-based fibers with moisture absorption and release processing and natural cellulose-based fibers without moisture absorption and release processing when natural cellulose-based fibers without moisture absorption and release processing are included) and the content of regenerated cellulose-based fibers in the refreshing fabric is preferably 85% by mass or more, more preferably 88% by mass or more, and even more preferably 90% by mass or more, and the total content of cotton (including both cotton with moisture absorption and release processing and cotton without moisture absorption and release processing) and the content of rayon is preferably 85% by mass or more, more preferably 88% by mass or more, and even more preferably 90% by mass or more.

[0037] In one embodiment, the cool fabric of the present invention may be produced by mixing the blended spun yarn (A) with a normal yarn, that is, by interweaving or interknitting these yarns. For example, one or two normal yarns may be used per blended spun yarn (A). The normal yarn is preferably a spun yarn made of 100% by mass of natural cellulosic fiber (a3) ​​that has not been subjected to moisture absorption / release processing, and more preferably a spun yarn made of 100% by mass of normal cotton fiber.

[0038] The cool fabric of the present invention is preferably a knitted fabric or a woven fabric. Knitted fabrics and woven fabrics are suitable for use as innerwear. Knitted fabrics are particularly stretchy and flexible, making them suitable for use as innerwear. Knitted fabrics include circular knitting, weft knitting, warp knitting (including tricot knitting and raschel knitting), pile knitting, and the like. The cool fabric of the present invention may be any of the following weave structures: plain knitting, jersey knitting, rib knitting, smooth knitting (double-sided knitting), rubber knitting, pearl knitting, Denbigh weave, cord weave, atlas weave, chain weave, insertion weave, and weave structures combining these. Various interlacing methods are used to produce the knitted fabric. Interlacing knitted fabrics may be warp knitting or weft knitting, and examples of these include tricot, raschel, and circular knitting. The knitted structure may be any of the following knitted structures: half knitting, reverse half knitting, double atlas knitting, double Denbigh knitting, and weave structures combining these. Examples of the weave include plain weave, twill weave, satin weave, variegated plain weave, variegated twill weave, variegated satin weave, variegated weave, patterned weave, single layer weave, double weave, multi-layer weave, warp pile weave, weft pile weave, leno weave, and combinations of these. Among these, weft knitted fabrics including circular knitting, and warp knitted fabrics are preferred.

[0039] The mass per unit area of ​​the refreshing fabric of the present invention is 80 to 300 g / m 2 is preferable, and more preferably 90 to 280 g / m 2 and more preferably 100 to 250 g / m 2 If it is in the above range, it is suitable for use as innerwear.

[0040] The elastic yarn is preferably at least one selected from polyurethane yarn and conjugate yarn obtained by conjugating at least two kinds of polymers having different shrinkage rates. The polyurethane elastic yarn may be any one that uses polymer diol and diisocyanate as starting materials, and is not particularly limited. The conjugate yarn is a conjugate yarn obtained by conjugating at least two kinds of polymers having different shrinkage rates, and it exhibits crimp (shrinkage) from the raw yarn stage, but when heat is applied, it exhibits even greater crimp (shrinkage). Specifically, a conjugate yarn (bicomponent yarn) of polyethylene terephthalate (PET) and polytrimethylene terephthalate (PTT) is preferable. Examples of such latent crimp-type stretch yarn include "Lycra T400" manufactured by Toray Opelontex Co., Ltd., "Espandee" manufactured by KB Seiren Co., Ltd., and "Z10" manufactured by Unitika Co., Ltd. The elastic yarn that is usually used is polyurethane yarn.

[0041] In the case of weft-knitted and circular-knitted fabrics, it is preferable to insert a bare spandex yarn (elastic yarn) as a plating yarn for loop yarns, and in the case of warp-knitted fabrics, the bare spandex yarn (elastic yarn) is inserted by insertion weaving or weft insertion. In the case of so-called innerwear, circular knitting is usually adopted, and an elastic yarn, especially a polyurethane elastic yarn, is used as a plating yarn for loop yarns. The polyurethane elastic yarn is usually inserted as a plating yarn in a state where a yarn of 20 to 40 decitex is stretched to about 2.5 times its original length.

[0042] The moisture absorbing and releasing fabric of the present invention is preferably a so-called one-way stretch fabric, which allows the elastic yarns in the clothing produced using the fabric to be arranged along the circumferential direction of the body. The circumferential direction of the body refers to the circumferential direction of the torso and the circumferential direction of the arms. By arranging the elastic yarns in this way, the inner clothing becomes comfortable to wear and does not easily lose its shape even after repeated washing. Specifically, the clothing is preferably a shirt or pants. The refreshing clothing of the present invention is preferably an inner clothing that is smooth to the touch and gentle on the skin, with the total content of cotton and rayon being preferably 85% by mass or more, more preferably 88% by mass or more, and even more preferably 90% by mass or more.

[0043] [How to make cool fabric] Next, the method for producing the refreshing fabric of the present invention will be described by taking as an example the case where cotton is used as the natural cellulosic fiber and rayon is used as the regenerated cellulosic fiber.

[0044] The moisture absorbing and releasing treatment for natural cellulosic fibers can be carried out, for example, as follows. In the case of the continuous method, the cotton sliver for spinning is irradiated with an electron beam under a nitrogen atmosphere to generate radicals on the surface of the cotton fiber, and immediately thereafter, the compound containing an ethylenically unsaturated double bond is continuously brought into contact with the surface of the cotton fiber. The reason why the compound containing an ethylenically unsaturated double bond is brought into contact with the surface of the cotton fiber immediately after the electron beam irradiation is to prevent the radicals generated by the electron beam irradiation from decaying. Since the radicals have a high tendency to decay over time, it is preferable to bring the compound containing an ethylenically unsaturated double bond into contact with the surface of the cotton fiber immediately after the electron beam irradiation. In addition, the reason why the compound containing an ethylenically unsaturated double bond is continuously brought into contact with the surface of the cotton fiber after the electron beam irradiation is that the compound containing an ethylenically unsaturated double bond can be effectively brought into contact with the radicals generated on the surface of the cotton fiber. The continuous process is convenient for treating a long sliver for spinning. The irradiation with an electron beam under a nitrogen atmosphere is preferable because the generated radicals are less likely to be deactivated.

[0045] The method for contacting the surface of cotton fibers with the compound containing an ethylenically unsaturated double bond may be any method such as immersion or spraying. For example, a method is preferred in which an aqueous solution of the compound containing an ethylenically unsaturated double bond is prepared, and the sliver is immersed in the aqueous solution or sprayed onto the sliver.

[0046] In the present invention, for example, a sliver of cotton for spinning that has been processed to absorb and release moisture and a rayon that has not been processed to absorb and release moisture, or a sliver of cotton for spinning that has been processed to absorb and release moisture and a rayon that has not been processed to absorb and release moisture and a cotton that has not been processed to absorb and release moisture are mixed in a cotton mixer and spun at a desired mixing ratio according to a conventional method. Specifically, these are mixed in a cotton mixer, opened, and made into a carded sliver with little unevenness and good uniformity (carding process), and then, a certain number of carded slivers are stretched while being combined, the fibers are made parallel, and the unevenness is further reduced to make a drawn sliver. Next, the drawn sliver is stretched and thinned, and after passing through a roving process in which a roving is made, the roving is stretched and twisted to make a yarn (spinning process). Blending can also be performed in a roving process or a fine spinning process, and blending can be performed by aligning a plurality of webs, slivers, fleeces, or rovings and stretching them at a predetermined ratio. In the roving and fine spinning processes, the constituent fibers can be mixed due to migration during twisting.

[0047] In this way, after blending the moisture-absorbing / releasing cotton and the non-moisture-absorbing / releasing rayon, or the moisture-absorbing / releasing cotton, the non-moisture-absorbing / releasing rayon, and the non-moisture-absorbing / releasing cotton, the yarn is twisted as necessary according to a conventional method to obtain a blended spun yarn (A). A cool fabric is produced by using only the blended spun yarn (A), the blended spun yarn (A) and the elastic yarn (B), or the blended spun yarn (A) and the normal yarn in a predetermined amount each. This fabric can be optionally subjected to post-processing such as bleaching, dyeing, and softening according to a conventional method.

[0048] [Cool clothing] 1 is a front view of an inner garment 1 according to one embodiment of the present invention. The inner garment 1 is an example of a long-sleeved shirt. Elastic yarns are arranged in the circumferential direction of the body, i.e., in the circumferential direction of the torso (arrow 2) and in the circumferential direction of the arms (arrow 3). EXAMPLES

[0049] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0050] <Moisture absorption / desorption test> The moisture absorption and desorption test was carried out by the Boken Quality Evaluation Organization (BOKEN Standard: BQE A 034). The details are as follows: After conditioning the moisture in the initial condition box (25°C, 40% RH), the test piece (10cm x 10cm) is moved to the moisture absorption box (25°C, 80% RH) and left in the moisture absorption box (25°C, 80% RH) until the mass of the test piece reaches equilibrium. It is then returned to the initial condition box (25°C, 40% RH), and measurement of the mass of the test piece is stopped when the mass of the test piece reaches equilibrium. During this time, the mass of the test piece is measured every 10 seconds. From the measurement results, the moisture absorption amount ratio below, moisture absorption rate ratio below, moisture absorption rate difference below, moisture absorption rate ratio per unit area after 1 minute, and moisture desorption rate ratio per unit mass after 5 minutes were calculated, and are shown in Table 1. In addition, moisture absorption ratio, moisture absorption rate ratio, moisture absorption rate difference, moisture absorption rate (μg / cm 2 The control material used to calculate the moisture release rate (mg / g·min) ratio and the moisture release rate (mg / g·min) ratio was a normal 100% cotton knit fabric prepared in the same manner as each test piece.

[0051] (moisture absorption ratio) Moisture absorption ratio = Moisture absorption of knitted fabrics in the following Examples and Comparative Examples / Moisture absorption of 100% cotton knitted fabric The amount of moisture absorption is calculated by placing a test piece in a moisture absorption box (25°C / 80%RH) and calculating the mass of the test piece when the mass of the test piece reaches equilibrium. (Moisture absorption rate ratio) Moisture absorption rate ratio = Moisture absorption rate of knitted fabrics in the following Examples and Comparative Examples / Moisture absorption rate of normal 100% cotton knitted fabric The moisture absorption rate (%) is calculated from the following formula. Moisture absorption rate (%) = Place the test piece in a moisture absorption box (25℃・80%RH), and the amount of moisture absorbed when the mass of the test piece reaches equilibrium (g) / weight of the test piece (initial condition) × 100 (Moisture absorption rate difference) Moisture absorption rate difference = (Moisture absorption rates of the knitted fabrics in the Examples and Comparative Examples below) - (Moisture absorption rate of normal 100% cotton knitted fabric)

[0052] <Sliver processing> Cotton sliver (mass per unit length, unit grain: 25.0 g / 6 yd (4.6 g / m)) was irradiated with electron beams at a dose of 40 kGy and an acceleration voltage of 200 kV under a nitrogen atmosphere using an electron beam irradiation device EC250 / 30 / 90L (manufactured by Iwasaki Electric Co., Ltd.). The sliver irradiated with the electron beam was immediately immersed in a 16% by mass aqueous solution of acrylic acid (manufactured by Nacalai Tesque Co., Ltd.) containing 0.5% by weight of a penetrant, and squeezed with a mangle to obtain a pickup rate of about 100% by mass relative to the weight of the sliver. Thereafter, the sliver was washed with water to continuously remove unreacted acrylic acid, dried at 80°C, and coiled and stored in a container. The acrylic acid-grafted cotton sliver thus obtained is hereinafter referred to as "grafted cotton". 16% by mass of acrylic acid was bonded to this grafted cotton. The above cotton sliver (mass per unit length, unit grain: 25.0 g / 6 yd (4.6 g / m)) is called "normal cotton".

[0053] <Yarn production & fabric creation for evaluation> Example 1 The cooling knitted fabric of Example 1 was produced as follows. The grafted cotton, the regular cotton, and rayon (staple, fineness 0.9 dtex, fiber length 38 mm) were mixed in a cotton blender, and spun yarn was produced using a quick spin. The mass ratio of the grafted cotton in the blended spun yarn was 10 mass%, the mass ratio of the rayon was 40 mass%, and the mass ratio of the regular cotton was 50 mass%. A circular knitted fabric was made from the above spun yarn, bleached with soda ash and hydrogen peroxide, and then acid-treated and alkali-substituted. Specifically, for the acid treatment, a 4.0 g / L citric acid aqueous solution was used, and the knitted fabric was immersed in this aqueous solution at a bath ratio of 1:15, treated at 40°C for 20 minutes, and then repeatedly washed with water at room temperature for 5 minutes twice. For the alkali substitution, the knitted fabric was immersed in an aqueous solution containing 9.0 g / L sodium bicarbonate and 0.5 g / L of a chelating agent (diethylenetriaminepentaacetic acid (DTPA)) at a bath ratio of 1:15, treated at 40°C for 20 minutes, and then repeatedly washed with water at room temperature for 5 minutes twice. The mass per unit area of ​​the obtained knitted fabric was 195 g / m 2 It was.

[0054] Example 2 A spun yarn was produced in the same manner as in Example 1, except that the mass ratio was 15 mass% grafted cotton, 45 mass% regular cotton, and 40 mass% rayon. A circular knit fabric (20 gauge) was produced from the spun yarn, and after bleaching treatment, acid treatment and alkali substitution were performed in the same manner as in Example 1, to obtain a mass per unit area of ​​191 g / m 2 A knitted fabric was obtained.

[0055] Example 3 A spun yarn was produced in the same manner as in Example 1, except that the mass ratio was 10 mass% grafted cotton, 60 mass% regular cotton, and 30 mass% rayon. A circular knit fabric (20 gauge) was produced from the spun yarn, and after bleaching treatment, acid treatment and alkali substitution were performed in the same manner as in Example 1, to obtain a mass per unit area of ​​222 g / m. 2 A knitted fabric was obtained.

[0056] Comparative Example 1 A spun yarn was produced in the same manner as in Example 3, except that the mass ratio was 70 mass% of the normal cotton and 30 mass% of the rayon. A circular knit fabric (20 gauge) was produced from the spun yarn, and after bleaching treatment, it was subjected to acid treatment and alkali substitution in the same manner as in Example 3 to obtain a mass per unit area of ​​216 g / m. 2 A knitted fabric was obtained.

[0057] Comparative Example 2 A spun yarn was produced in the same manner as in Example 3, except that the mass ratio was 10 mass% of the grafted cotton and 90 mass% of the normal cotton. A circular knit fabric (20 gauge) was produced from the spun yarn, and after bleaching treatment, acid treatment and alkali substitution were performed in the same manner as in Example 3 to obtain a mass per unit area of ​​163 g / m 2 A knitted fabric was obtained.

[0058] [Table 1]

[0059] As is clear from Table 1, in the case of a blend of only normal cotton and rayon, the moisture absorption rate is somewhat improved compared to a fabric containing 100% normal cotton by mass, but the moisture release rate is not improved (Comparative Example 1). When normal cotton is blended with grafted cotton (Comparative Example 2), the moisture release rate is improved compared to a fabric containing 100% normal cotton by mass, but the moisture absorption rate is not significantly improved. When a three-kind blend of grafted cotton, normal cotton, and rayon is performed, the inclusion of rayon makes the fabric smooth to the touch, and the moisture absorption rate and moisture release rate are improved, and the moisture absorption and release properties are well balanced. In particular, when the grafted cotton is 5 to 20% by mass, the rayon is 30 to 65% by mass, and the normal cotton is 20 to 60% by mass, the moisture absorption rate and moisture release rate are significantly improved. [Industrial Applicability]

[0060] The refreshing fabric of the present invention and the refreshing clothing using the same are suitable for innerwear such as shirts, pants, etc. Also, since it is gentle on the skin, it is suitable for T-shirts, etc. [Explanation of symbols]

[0061] 1 Cool clothing 2. Around the fuselage 3 Arm circumference

Claims

1. A refreshing fabric comprising a blended spun yarn (A) containing natural cellulosic fibers (a1) that have been subjected to moisture absorption and release processing and regenerated cellulosic fibers (a2) that have not been subjected to moisture absorption and release processing, The refreshing fabric has a moisture absorption rate ratio and a moisture release rate ratio of 1.05 or more between the refreshing fabric and a fabric X which is the same as the refreshing fabric except that it contains a spun yarn consisting only of cotton fibers instead of the blended spun yarn (A).

2. The refreshing fabric according to claim 1, wherein the blended spun yarn (A) further contains natural cellulosic fibers (a3) ​​that have not been subjected to moisture absorption / release treatment.

3. The refreshing fabric according to claim 1, wherein the content of the moisture absorbing and releasing processed natural cellulosic fiber (a1) is 3% by mass or more and 50% by mass or less, when the refreshing fabric is taken as 100% by mass.

4. The refreshing fabric according to claim 1, wherein the blended spun yarn (A) contains the moisture-absorbing and desorbing processed natural cellulosic fiber (a1) in an amount of 3% by mass or more and 50% by mass or less.

5. The refreshing fabric according to claim 2, wherein the blended spun yarn (A) contains the non-moisture-absorbing and non-releasing regenerated cellulosic fiber (a2) in a blended ratio of 10% by mass or more and 70% by mass or less.

6. The refreshing fabric according to claim 1, wherein the moisture absorbing and releasing processed natural cellulosic fiber (a1) is a fiber in which a compound containing an ethylenically unsaturated double bond is graft-bonded to a natural cellulosic fiber.

7. The refreshing fabric according to claim 6, wherein the graft rate of the moisture-absorbing and desorbing processed natural cellulosic fiber (a1) is 1% or more and 40% or less.

8. The cooling fabric according to claim 1 , further comprising an elastic yarn.

9. The cooling fabric according to claim 8, wherein the content of the elastic yarn in the cooling fabric is 15% by mass or less.

10. A refreshing clothing comprising the refreshing fabric according to any one of claims 1 to 9.

11. The refreshing clothing according to claim 10, wherein the refreshing clothing is an inner garment, and is a shirt or pants.

Citation Information

Patent Citations

  • Cellulosic fiber or cellulosic textile product reduced in stuffy feeling in light exercise and method for processing the same

    JP2002030570A

  • Fabric having moisture-absorbing exothermic property / moisture-releasing cooling property

    JP2002088653A

  • Hygroscopic and exothermic fabric and hygroscopic and exothermic clothing using the same

    JP2021025135A

  • Natural knit fabric with a cool feel upon contact.

    JP3192709U

  • Regenerated cellulose having high moisture-absorbing and releasing property, and pyrogenicity and its production

    JP2000290828A