Dissimilar metal material joining method and dissimilar metal material joint structure
By using a conductive current-carrying member to energize the welding wire through a hole in the second member, the method overcomes the insulating coating issue, enabling effective arc welding and strong bonding of dissimilar metals.
Patent Information
- Application Number
- JP2023058879
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing methods for joining dissimilar metal materials, such as steel and aluminum or magnesium alloys, fail due to the insulating electrodeposition coating on steel plates, which prevents arc welding and leads to bonding failures.
A method involving a conductive current-carrying member placed inside a hole in the second member, with a joining auxiliary member, allows arc welding through the insulating layer by energizing the welding wire via the current-carrying member, ensuring the formation of a weld metal between the members.
Enables reliable arc generation and high-quality joining of dissimilar metals despite an insulating layer, preventing bonding defects and ensuring strong, defect-free connections.
Smart Images

Figure 2024146147000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for joining dissimilar metal materials, which is capable of joining plate materials made of different materials with high strength, and to a dissimilar metal joined structure joined by the joining method. [Background technology]
[0002] For transportation equipment, such as automobiles, there is a constant demand for improving fuel efficiency in order to reduce (1) the consumption of petroleum fuel, which is a limited resource, (2) the greenhouse gas CO2 generated by combustion, and (3) driving costs. As a means to achieve this, in addition to improving power system technologies such as the use of electric drive, weight reduction of the vehicle body is also one of the improvement measures. One way to reduce weight is to replace steel, which is currently the main material, with lightweight materials such as aluminum or aluminum alloys, magnesium or magnesium alloys, carbon fiber, resin, and carbon fiber reinforced plastics (CFRP). However, replacing everything with these lightweight materials has issues such as high costs and insufficient strength, and as a solution, a design method called multi-material, which combines steel and lightweight materials in the right places, is attracting attention.
[0003] Patent Document 1 discloses a joint structure in which, for example, a steel material and a non-ferrous metal material that is difficult to weld to the steel material are joined. The joint structure includes a first homogeneous metal material having a protrusion, a second homogeneous metal material, and a dissimilar material having a first penetration portion and sandwiched between the first homogeneous metal material and the second homogeneous metal material. The first protrusion of the first homogeneous metal material is arc-welded in the thickness direction, and the first homogeneous metal material and the second homogeneous metal material are fused and bonded to each other through the first penetration portion, thereby compressing and fixing the dissimilar materials. This fixes the dissimilar materials to the first homogeneous metal material and the second homogeneous metal material.
[0004] Patent Document 2 discloses an arc spot welding method for joining dissimilar materials, which joins a first plate made of an aluminum alloy or magnesium alloy and a second plate made of steel. The welding method described in Patent Document 2 includes the steps of drilling a hole in the first plate, overlapping the first plate and the second plate, inserting a steel auxiliary joining member having a stepped outer shape with an insertion portion and a non-insertion portion and having a hollow portion penetrating the insertion portion and the non-insertion portion into the hole provided in the first plate, and filling the hollow portion of the auxiliary joining member with a weld metal by a specific method, melting the weld metal into the second plate until a back wave appears, and partially melting the insertion portion of the auxiliary joining member without melting its outer circumferential surface, thereby welding the second plate and the auxiliary joining member. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6811380 [Patent Document 2] Patent No. 6461056 Summary of the Invention [Problem to be solved by the invention]
[0006] Meanwhile, in the manufacturing process of automobiles, there is a process of performing electrocoating on the surface of the body material for the purpose of rust prevention. Since this coating film is insulating, the painted steel plate cannot pass electricity, which is essential for arc welding. Therefore, even if an attempt is made to apply a steel plate on which an electrocoating film has been formed to the joining structure described in the above Patent Document 1, an electric current cannot be passed because the electrocoating film is insulating, and an arc cannot be generated. Even with the method using the joining auxiliary member described in the above Patent Document 2, when an attempt is made to perform arc welding after electrocoating the second steel plate, joining is impossible or the joining is poor because the insulating electrocoating film prevents the generation of an arc.
[0007] The present invention has been made in consideration of such problems, and has an object to provide a method for joining a first member made of steel to a second member made of a material different from the first member by arc welding, which can join the first member and the second member in a simple process without causing joint defects even when an insulating layer is interposed between the first member and the second member, and a joined structure of dissimilar metal materials joined by the above joining method. [Means for solving the problem]
[0008] The above object of the present invention can be achieved by the following configuration [1] relating to a method for joining dissimilar metal materials. [1] A first step of placing a second member having a first hole penetrating in a plate thickness direction and made of a different material from the first member on a first member made of steel; a second step of disposing a conductive current-carrying member that is electrically conductive to the second member in the inside or bottom of the first hole, and inserting a joining auxiliary member having a second hole and having the same main component as the first member into the first hole; and a third step of forming a weld metal having the same main component as that of the first member inside the second hole by arc welding, an insulating layer is interposed between the first member and the second member; the joining auxiliary member includes a flange portion disposed on a surface of the second member opposite to a contact surface with the first member, and a shaft portion inserted into the first hole, the second hole being formed to extend in an axial direction of the shaft portion, a third step of contacting a tip of a welding wire with the current-carrying member, and causing an electric current to flow between the welding wire and the second member via the current-carrying member, thereby generating an arc.
[0009] Further, preferred embodiments of the present invention relating to a method for joining dissimilar metal materials relate to the following [2] to [6]. [2] The method for joining dissimilar metal materials described in [1], characterized in that the insulating layer is an electrocoating coating formed on the surface of the first member. [3] The method for joining dissimilar metal materials described in [1] or [2], characterized in that the current-carrying member is integrated with the auxiliary joining member, the second hole is formed in a bottomed shape, and at least one of the current-carrying member and the auxiliary joining member is in contact with the second member. [4] The current-carrying member and the joining auxiliary member are disposed apart from each other, The method for joining dissimilar metal materials according to [1] or [2], characterized in that the conductive member is in contact with the second member. [5] The method for joining dissimilar metal materials described in [1] or [2], characterized in that the thickness of the current-carrying member is thinner than the thickness of the flange portion of the joining auxiliary member. [6] The method for joining dissimilar metal materials according to [5], characterized in that the thickness of the conductive member is 0.5 mm or less. The above object of the present invention is achieved by the following configuration [7] relating to a dissimilar metal bonded structure.
[0010] [7] A first member made of steel; and A second member is disposed on the first member, has a first hole penetrating in a plate thickness direction, and is made of a material different from that of the first member; an insulating layer interposed between the first member and the second member; a conductive member disposed inside or at a bottom of the first hole and having electrical conductivity; a joining auxiliary member having a flange portion disposed on a surface of the second member opposite to a contact surface with the first member, a shaft portion inserted into the first hole, and a second hole parallel to an axial direction of the shaft portion, the joining auxiliary member having the same main component as the first member; a weld metal formed inside the second hole and having the same main component as the first member.
[0011] Further, preferred embodiments of the present invention relating to a dissimilar metal bonded structure relate to the following items [8] to
[10] . [8] The dissimilar metal joint structure described in [7], characterized in that the insulating layer is an electrocoating coating formed on the surface of the first component. [9] The dissimilar metal joint structure described in [7] or [8], characterized in that the conductive member is integrated with the auxiliary joining member, the second hole is formed in a bottomed shape, and at least one of the conductive member and the auxiliary joining member is in contact with the second member.
[10] The current-carrying member and the joining auxiliary member are disposed apart from each other, The dissimilar metal joint structure according to [7] or [8], characterized in that the conductive member is in contact with the second member. Effect of the Invention
[0012] According to the present invention, it is possible to provide a method for joining dissimilar metal materials, which can join a first member and a second member in a simple process without causing a joining defect even when an insulating layer is interposed between the first member and the second member, and a joined structure of dissimilar metal materials joined by the above joining method. [Brief description of the drawings]
[0013] [Figure 1A] FIG. 1A is a cross-sectional view showing a first step and a second step of a method for joining dissimilar metal materials according to a first embodiment of the present invention. [Figure 1B] FIG. 1B is a cross-sectional view showing a third step of the method for joining dissimilar metal materials according to the first embodiment of the present invention. [Figure 1C] FIG. 1C is a cross-sectional view showing a dissimilar metal joint structure obtained by the method for joining dissimilar metal materials according to the first embodiment of the present invention. [Figure 2A] FIG. 2A is a cross-sectional view showing a first step and a second step of a method for joining dissimilar metal materials according to a second embodiment of the present invention. [Figure 2B] FIG. 2B is a cross-sectional view showing a third step in the method for joining dissimilar metal materials according to the second embodiment of the present invention. [Figure 3A] FIG. 3A is a top view showing a joining auxiliary member used as an example of the invention. [Figure 3B]FIG. 3B is a cross-sectional view showing the size of the joining auxiliary member shown in FIG. 3A. [Figure 4A] FIG. 4A is a photograph, substituted for a drawing, showing the upper surface side of a dissimilar metal joint structure of Example 1 produced by the method for joining dissimilar metal materials according to the present invention. [Figure 4B] FIG. 4B is a photograph showing the back side of the dissimilar metal bonded structure in FIG. 4A. [Diagram 5] FIG. 5 is a photograph, substituted for a drawing, showing a cross section of the dissimilar metal joint structure of Example 1, cut along a cutting line passing through the center of the weld metal. [Figure 6] FIG. 6 is a photograph, substituted for a drawing, showing the state of the upper surface side of Inventive Examples 2 to 4 after the tensile shear test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The inventors of the present application conducted extensive research into a method for generating an arc when joining a first steel member and a second member made of a different material to the first member by arc welding, even when an insulating layer is present between the first member and the second member.
[0015] One of the reasons for poor joining is that during arc welding, a solidified ball is formed at the tip of the welding wire every time electricity is passed, so even if the tip of the welding wire is brought into contact with the surface of the lower plate, the welding wire cannot penetrate the insulating layer and reach the lower plate, which hinders current flow. If the tip of the welding wire were cut off and sharpened every time welding was performed, the welding wire would penetrate the insulating layer and reach the first member, which is the lower plate, and an arc would be generated.
[0016] However, when considering mass production, it is difficult to cut off the tip of the welding wire every time welding is performed, so further research was conducted on a method for generating an arc more easily. As a result, the inventors of the present application found that an arc can be generated by placing a conductive current-carrying member that conducts current to the second member in a first hole formed in the second member, and by bringing the welding wire into contact with the current-carrying member while a voltage is applied to the welding wire and the second member. The present invention was made based on these findings.
[0017] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail with reference to the drawings. Note that the present invention is not limited to the embodiment described below, and can be modified and implemented as desired without departing from the gist of the present invention.
[0018] [Method of joining dissimilar metal materials] First Embodiment 1A to 1C are schematic cross-sectional views showing a method for joining dissimilar metal materials according to a first embodiment of the present invention in the order of steps.
[0019] (1st step) 1A, first, a steel first member 1 having an electrodeposition coating film (insulating layer) 3 formed on its surface and an aluminum alloy second member 2 having a first hole 2a penetrating in the plate thickness direction are prepared. Then, the second member 2 is placed on top of the surface of the first member 1 perpendicular to the plate thickness direction.
[0020] (2nd process) Next, the steel joint auxiliary member 4 is inserted into the first hole 2a. The joint auxiliary member 4 has a disk-shaped flange portion 4a and a shaft portion 4b having an axis in the same axial direction as the central axis of the disk shape. In addition, the joint auxiliary member 4 has a second hole 4c extending in a direction parallel to the axial direction of the shaft portion 4b from the upper surface of the flange portion 4a toward the shaft portion 4b side. Furthermore, a bottom member (current-carrying member) 5 is integrally formed at the end of the shaft portion 4b side of the joint auxiliary member 4. Therefore, the end of the shaft portion 4b side of the second hole 4c has a closed bottom shape. Note that inserting the joint auxiliary member 4 into the first hole 2a means inserting the shaft portion 4b of the joint auxiliary member 4 into the first hole 2a, and at this time, the flange portion 4a is disposed on the surface of the second member 2 opposite to the contact surface with the first member 1, that is, on the upper surface 2b of the second member 2. In this embodiment, the bottom member 5 and the first member 1 are not in contact with each other and are disposed apart from each other. The bottom member 5 and the first member 1 are in direct contact with the second member 2 or indirectly via the shaft portion 4b, the flange portion 4a, or the like. In other words, at least one of the bottom member 5 and the joining auxiliary member 4 is in contact with the second member 2.
[0021] (3rd step) Then, a weld metal 9 having the same main component as that of the first member 1 is formed inside the second hole 4c by arc welding. Specifically, as shown in FIG. 1B, a welding wire 7 held by a welding nozzle 6 is placed on the joining assistant member 4, and a power source 11 is connected to the welding wire 7 and the second member 2 to apply a voltage. Then, the tip of the welding wire 7 is brought into contact with the bottom member 5 to generate an arc. At this time, a solidified ball 8 may be formed at the tip of the welding wire 7, but it is not necessary to cut it off.
[0022] Thereafter, the second hole 4c is filled with molten metal while melting the welding wire 7. As a result, as shown in Fig. 1C, at least a part of the first member 1 having the electrodeposition coating film 3, at least a part of the bottom member 5, and at least a part of the joining auxiliary member 4 melt to form a steel weld metal 9, and a dissimilar metal joining structure 10 is obtained.
[0023] As described above, in the conventional joining method, when the first steel member 1 has an electrodeposition coating film 3 on its surface, electricity is not passed between the welding wire 7 and the first member 1, and an arc may not be generated. If the solidified ball 8 formed at the tip of the welding wire 7 is cut off after each welding and the tip is sharpened, the welding wire 7 can penetrate the electrodeposition coating film 3, and electricity can be passed between the welding wire 7 and the first member 1. However, cutting the tip of the welding wire 7 after each welding increases the number of steps, which causes an increase in manufacturing costs and a decrease in yield.
[0024] In contrast, in this embodiment, since the welding wire 7 and the second member 2 are energized through the bottom member 5, an arc can be reliably generated even when an insulating layer is interposed between the first member 1 and the second member 2, such as the electrodeposition coating film 3. In addition, the joining auxiliary member 4 and the welding wire 7 are both made of steel, and the weld metal 9 is made of a material that can be joined to the first member 1. Since the weld metal 9 includes at least a part of the first member 1 having the electrodeposition coating film 3, at least a part of the bottom member 5, and at least a part of the joining auxiliary member 4, the joining auxiliary member 4 and the first member 1 are firmly fixed by the weld metal 9. Furthermore, the second member 2 is physically fixed to the first member 1 by the flange portion 4a of the joining auxiliary member 4. Therefore, the first member 1 having the electrodeposition coating film 3 and the second member 2 made of a material different from the first member 1 can be easily joined in a high-quality state.
[0025] In this embodiment, an example has been shown in which an aluminum alloy plate is used as the second member 2, but the second member 2 is not particularly limited as long as it is made of a material different from that of the first member 1. As the second member 2, various conductive materials can be used, and specifically, aluminum or aluminum alloy material, magnesium alloy, etc. can be used. Since the auxiliary joining member 4 needs to be made of a material that can form the weld metal 9 together with the first member 1, the auxiliary joining member 4 and the first member 1 have the same main components. Therefore, the obtained weld metal 9 also has the same main components as the first member 1.
[0026] In addition, in the present invention, the shapes of the first member 1 and the second member 2 are not particularly limited. In particular, as long as the region where the first hole 2a is formed is plate-shaped, the other regions of the second member 2 may have any shape, and may be freely selected from shapes that are partially bent, shapes that have partially different thicknesses, and the like. In other words, the "plate thickness direction" of the second member 2 in this specification refers to the thickness direction of the plate-shaped portion in the region of the second member 2 that is joined to the first member 1.
[0027] <Second embodiment> 2A and 2B are schematic cross-sectional views showing the process steps of a method for joining dissimilar metal materials according to a second embodiment of the present invention. In the second embodiment shown in Fig. 2A and 2B, the same components as those in the first embodiment shown in Fig. 1A to 1C are denoted by the same reference numerals, and detailed descriptions thereof will be omitted or simplified.
[0028] (1st step) As shown in FIG. 2A, a second member 2 made of an aluminum alloy and having a first hole 2a is placed on top of a first member 1 made of steel.
[0029] (2nd process) Next, an aluminum alloy foil 15 is placed on the first member 1 at the bottom of the first hole 2a as a conductive member so as to contact the second member 2. Then, a steel joint auxiliary member 14 is inserted into the first hole 2a. In this embodiment, the joint auxiliary member 14 has a disk-shaped flange portion 14a and a shaft portion 14b having an axis in the same axial direction as the central axis of the disk. In addition, a second hole 14c is formed in the joint auxiliary member 14, penetrating in a direction parallel to the axial direction of the shaft portion 14b from the upper surface of the flange portion 14a toward the shaft portion 14b side. That is, in this embodiment, the joint auxiliary member 14 and the aluminum alloy foil 15 as the conductive member are not integrated, but are placed separately. The aluminum alloy foil 15 may be placed so as to be fitted into the first hole 2a, or may be placed so as to be sandwiched between the electrodeposition coating film 3 of the first member 1 and the second member 2.
[0030] (3rd step) Then, a weld metal having the same main component as the first member 1 is formed inside the second hole 14c by arc welding. Specifically, as shown in FIG. 2B, a power source 11 is connected to the welding wire 7 and the second member 2, and a voltage is applied. Then, the tip of the welding wire 7 is brought into contact with the aluminum alloy foil 15, and an electric current is passed between the welding wire 7 and the second member 2 through the aluminum alloy foil 15 to generate an arc. Then, while melting the welding wire 7, the molten metal is filled into the second hole 14c. As a result, as in FIG. 1C, a weld metal 9 is formed that joins the first member 1 and the second member 2 through the joining auxiliary member 14, and a dissimilar metal joining structure 10 is obtained.
[0031] In the second embodiment described above, as in the first embodiment, an arc can be reliably generated, thereby making it possible to easily join a first member 1 having an electrocoating coating 3 to a second member 2 made of a different material from the first member 1 in a high-quality state.
[0032] In the first embodiment, the bottom member (current-carrying member) 5 and the auxiliary joining member 4 are integrated, and the bottom member 5 is disposed apart from the first member 1. In the second embodiment, the aluminum alloy foil (current-carrying member) 15 and the auxiliary joining member 14 are separate members, and are disposed apart from each other. Thus, in the present invention, the bottom member 5 and the aluminum alloy foil 15, which are current-carrying members, may be disposed inside the first hole 2a in the second member 2, or may be disposed at the bottom.
[0033] In addition, the bottom member 5 and the aluminum alloy foil 15, which are the current-carrying members, do not need to cover the entire surfaces of the second holes 4c and 14c in the direction perpendicular to the axial direction, and may have a hole partially formed therein. In other words, it is sufficient that the welding wire 7 can be easily brought into contact with the current-carrying members, and at this time, the current-carrying members are directly or indirectly connected to the second member 2, and electricity is conducted between the current-carrying members and the second member 2.
[0034] Furthermore, in the above first and second embodiments, an example was shown in which the second member 2 having the electrodeposition coating film 3 formed on its surface was used, but the insulating layer is not limited to the electrodeposition coating film 3. The present invention can also be applied to a state in which an insulating plate or film, such as a fluororesin sheet or resin coating, is interposed between the first member 1 and the second member 2.
[0035] In the first and second embodiments, the thickness of the current-carrying member represented by the bottom member 5 or the aluminum alloy foil 15 is not particularly limited, and may be such that the welding wire 7 and the second member 2 can be electrically connected through the current-carrying member. However, as shown in the first embodiment, when the bottom member 5 as the current-carrying member is integrated with the joining auxiliary member 4, if the joining auxiliary member 4 is to be produced by drawing a plate material, the thickness of the flange portion 4a and the thickness of the bottom member 5 will be approximately the same thickness. In this way, if the thickness of the bottom member 5 becomes as thick as the thickness of the flange portion 4a, heat is required to melt the current-carrying member, and it may be difficult to sufficiently melt the first member 1. Therefore, the thickness of the current-carrying member is preferably thinner than the thickness of the flange portion of the joining auxiliary member, more preferably 0.5 mm or less, even more preferably 0.3 mm or less, and particularly preferably 0.1 mm or less.
[0036] Next, a dissimilar metal joint structure 10 joined by the method for joining dissimilar metal materials according to the above embodiment will be described.
[0037] [Dissimilar metal bonded structure] As shown in FIG. 1C, the dissimilar metal joint structure 10 according to this embodiment includes a first member 1 made of steel, a second member 2 made of a material different from the first member 1, an electrocoating coating 3 interposed between the first member 1 and the second member 2, a bottom member (conductive member) 5 having electrical conductivity, a joint auxiliary member 4 having the same main component as the first member 1, and a weld metal 9 having the same main component as the first member 1. The second member 2 is arranged on top of the first member 1 and has a first hole 2a penetrating in the plate thickness direction. The joint auxiliary member 4 has a flange portion 4a arranged on the surface of the second member 2 opposite to the contact surface with the first member 1, a shaft portion 4b inserted into the first hole 2a, and a second hole 4c parallel to the axial direction of the shaft portion 4b. The bottom member 5 is integrated with the joint auxiliary member 4, and the second hole 4c is formed in a bottomed shape, and at least one of the bottom member 5 and the joint auxiliary member 4 is in contact with the second member 2. The weld metal 9 is formed inside the second hole 4c and includes a molten portion in which at least a part of the first member 1, at least a part of the electrocoating coating 3, at least a part of the bottom member 5, and at least a part of the joining auxiliary member 4 are melted.
[0038] The dissimilar metal joined structure 10 of this embodiment is obtained by the above-mentioned method capable of generating an arc even if an electrocoating coating 3 is formed on the surface of the first member 1, and therefore the first member 1 and the second member 2 are reliably joined by the weld metal 9 and the joining auxiliary member 4.
[0039] As described in the above-mentioned joining method section, the above-mentioned dissimilar metal joint structure 10 is an example in which the first member 1 having the electrodeposition coating film 3 formed on its surface is used, but the insulating layer in the present invention is not limited to the electrodeposition coating film 3. For example, the present invention also includes a case in which an insulating plate or film, such as a fluororesin sheet or resin coating, is interposed between the first member 1 and the second member 2. In addition, the bottom member 5 does not need to be integrated with the joining auxiliary member 4. As shown in FIG. 2B, the present invention includes various cases, such as a case in which the joining auxiliary member 14 and a current-carrying member such as the aluminum alloy foil 15 are separated from each other, a case in which the current-carrying member and the first member 1 are separated from each other, and a case in which the current-carrying member is sandwiched between the first member 1 and the second member 2. That is, the current-carrying member such as the bottom member 5 or the aluminum alloy foil 15 may be arranged inside or at the bottom of the second hole 4c so as to be directly or indirectly conducted to the second member 2. EXAMPLES
[0040] Hereinafter, examples of the method for joining dissimilar metal materials according to this embodiment will be specifically described.
[0041] [Manufacturing of dissimilar metal bonded structures] As shown in Figs. 1A to 1C, a second member 2 made of an aluminum alloy and having a first hole 2a was placed on top of a first member 1 made of steel having an electrodeposition coating film 3 formed on its surface. Next, a joining auxiliary member 4 made of steel was inserted into the first hole 2a. After that, a power source 11 was connected to the welding wire 7 and the second member 2, and then the tip of the welding wire 7 was brought into contact with the bottom member 5 to generate an arc and perform arc welding, thereby filling the second hole 4c with molten metal. As a result, a dissimilar metal joined structure 10 was obtained in which the first member 1 and the second member 2 were joined by the joining auxiliary member 4 and the weld metal 9.
[0042] FIG. 3A is a top view showing the auxiliary joining member 4 used as an example of the invention, and FIG. 3B is a cross-sectional view showing the size of the auxiliary joining member shown in FIG. 3A. As shown in FIG. 3A and FIG. 3B, the auxiliary joining member 4 used had a disk-shaped flange portion 4a, a shaft portion 4b having an axis in the same axial direction as the central axis of the disk, and a second hole 4c extending in a direction parallel to the axial direction of the shaft portion 4b from the upper surface of the flange portion 4a toward the shaft portion 4b side. The end of the second hole 4c on the shaft portion 4b side was blocked by a bottom member 5, and this bottom member 5 corresponds to the current-carrying member in the present invention. Other welding conditions are shown below.
[0043] (Size of auxiliary joining parts) Outer diameter of flange part 4a: 12.4 mm Thickness of flange part 4a: 1.8 mm Axial length of shaft portion 4b: 1.9 mm Outer diameter of shaft 4b: 8.4 mm Inner diameter of shaft 4b: 6.4 mm Thickness of bottom member 5: 0.3 mm
[0044] (Other welding conditions) Type of first component 1: galvannealed 980MPa-class high-tensile steel plate (with electrochemical coating) Plate thickness of first component 1: 1.4 mm Type of second component 2: A6022-T4 tempered plate material Plate thickness of second member 2: 2.0 mm Material of the auxiliary joint part 4 (and bottom part 5): SS400 Welding wire type 7: JIS Z3317 G 55A-1CM3 Diameter of welding wire 7: 1.2mm Shielding gas type and flow rate: 100% CO2, 25 liters / min Welding power source: Pulse MAG / MIG welding power source P500L (manufactured by Daihen Corporation) Welding mode: Wire feed control mode Upslope initial setting current: 50A Upslope initial setting voltage: 18.0V Upslope Time: 0.2 seconds Main current setting: 190A Main power supply voltage: 19.6V Main arc time: 1.4 seconds Average current: 155~165A Average voltage: 16.5~17.0V Total Arc Time: 1.6 seconds
[0045] [Arc occurrence and appearance evaluation] Fig. 4A is a drawing substitute photograph showing the top side of a dissimilar metal joint structure of Example 1 produced by the method for joining dissimilar metal materials according to the present invention, and Fig. 4B is a drawing substitute photograph showing the back side. Fig. 5 is a drawing substitute photograph showing a cross section of the dissimilar metal joint structure of Example 1 cut along a cutting line passing through the center of the weld metal 9. The cutting line is parallel to the short side direction of the first member 1 and the second member 2. In Figs. 4A and 4B, a hole 20 formed in the first member 1 is a hanging hole for forming an electrodeposition coating film 3.
[0046] In Example 1, A6022-T4 tempered plate material was used as the second member 2. As shown in Figures 4A and 4B, according to the joining method of the present invention, an arc can be reliably generated during arc welding, and sufficient penetration can be ensured even when a steel plate having an electrodeposition coating film 3 is used.
[0047] [Evaluation by tensile shear test] A dissimilar metal joint structure was manufactured by joining a first member 1 made of steel and a second member 2 made of an aluminum alloy in the same manner as in the above-mentioned invention example 1. Next, a tensile shear test was carried out on the obtained dissimilar metal joint structure in accordance with "Test piece dimensions and test method for shear test of resistance spot and projection welded joints" described in JIS Z 3136:1999, and the tensile shear strength (TSS) was evaluated. Note that the welding of invention examples 2, 3, and 4 was carried out using the same materials and the same welding condition settings as the above-mentioned invention example 1.
[0048] Figure 6 is a photograph showing the state of the upper surface after the tensile shear test for Examples 2 to 4. The effective values of the current and voltage during welding and the measurement results of the tensile shear test are shown in the table below. Note that since Figure 6 shows the state after the tensile shear test, the first member 1 (left side in the figure) and the second member 2 (right side in the figure) are divided, but the reference numerals are omitted.
[0049] [Table 1]
[0050] As shown in Fig. 6, good weld metal was obtained in all of Examples 2 to 4, and the weld metal did not come out of the first member in the tensile shear test. Furthermore, as shown in Table 1, excellent tensile shear strength was obtained in all of Examples 2 to 4.
[0051] In this way, it has been shown that by using the method for joining dissimilar metal materials according to the present invention, an arc can be reliably generated even when an insulating layer such as an electrocoating coating 3 is interposed between the first member 1 and the second member 2, and the first member 1 and the second member 2 can be joined with high quality. [Explanation of symbols]
[0052] 1 First member 2 Second member 2a 1st hole 3 Electrochemical coating 4, 14 Joining auxiliary parts 4a, 14a Flange part 4b, 14b shaft part 4c, 14c 2nd hole 5 Bottom member 7 Welding Wire 9 Welding metal 10 Dissimilar metal bonded structure 11 Power supply 15 Aluminum alloy foil
Claims
1. A first step of disposing a second member having a first hole penetrating in a plate thickness direction and made of a material different from that of the first member on a first member made of steel; a second step of disposing a conductive current-carrying member that is electrically conductive to the second member in the inside or bottom of the first hole, and inserting a joining auxiliary member having a second hole and having the same main component as the first member into the first hole; and a third step of forming a weld metal having the same main component as that of the first member inside the second hole by arc welding, an insulating layer is interposed between the first member and the second member; the joining auxiliary member includes a flange portion disposed on a surface of the second member opposite to a contact surface with the first member, and a shaft portion inserted into the first hole, the second hole being formed to extend in an axial direction of the shaft portion, a third step of contacting a tip of a welding wire with the current-carrying member, and causing an electric current to flow between the welding wire and the second member via the current-carrying member, thereby generating an arc.
2. 2. The method for joining dissimilar metal materials according to claim 1, wherein the insulating layer is an electrodeposition coating film formed on the surface of the first member.
3. 3. The method for joining dissimilar metal materials according to claim 1 or 2, characterized in that the conductive member is integrated with the auxiliary joining member, the second hole is formed in a bottomed shape, and at least one of the conductive member and the auxiliary joining member is in contact with the second member.
4. The current-carrying member and the joining auxiliary member are disposed apart from each other, 3. The method for joining dissimilar metal materials according to claim 1, wherein the current-carrying member is in contact with the second member.
5. 3. The method for joining dissimilar metal materials according to claim 1, wherein the current-carrying member has a thickness smaller than a thickness of the flange portion of the joining auxiliary member.
6. 6. The method for joining dissimilar metal materials according to claim 5, wherein the current-carrying member has a thickness of 0.5 mm or less.
7. A first member made of steel; A second member is disposed on the first member, has a first hole penetrating in a plate thickness direction, and is made of a material different from that of the first member; an insulating layer interposed between the first member and the second member; a conductive member disposed inside or at a bottom of the first hole and having electrical conductivity; a joining auxiliary member having a flange portion disposed on a surface of the second member opposite to a contact surface with the first member, a shaft portion inserted into the first hole, and a second hole parallel to an axial direction of the shaft portion, the joining auxiliary member having the same main component as the first member; a weld metal formed inside the second hole and having the same main component as the first member.
8. 8. The dissimilar metal joint structure according to claim 7, wherein the insulating layer is an electrodeposition coating film formed on the surface of the first member.
9. 9. The dissimilar metal joint structure according to claim 7 or 8, characterized in that the conductive member is integrated with the auxiliary joining member, the second hole is formed in a bottomed shape, and at least one of the conductive member and the auxiliary joining member is in contact with the second member.
10. The current-carrying member and the joining auxiliary member are disposed apart from each other, 9. The dissimilar metal joint structure according to claim 7, wherein the current-carrying member is in contact with the second member.
Citation Information
Patent Citations
Rivet joint structure and method of manufacturing the same
JP2014226698A
Dissimilar material jointing spot welding method, joint auxiliary member, and dissimilar material welding coupling
JP2018051570A
Battery case and method for manufacturing battery case
JP2023035000A
Solid-state image sensor
JP1989061056A
Joint structure
JP6811380B2