Welding wire, gas-shielded arc welding method, and manufacturing method of weld metal
Patent Information
- Application Number
- JP2023059088
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
【0025】 本発明によれば、優れた電着塗装性を有する溶接ビードを得ることができるとともに、溶接ビード上に塊状スラグが生成されることを抑制し、優れたビード外観を得ることができるガスシールドアーク溶接用の溶接ワイヤ、該溶接ワイヤを用いたガスシールドアーク溶接方法、及び該ガスシールドアーク溶接方法を用いた溶接金属の製造方法を提供することができる。
Smart Images

Figure 2024146286000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a welding wire used in gas-shielded arc welding, a gas-shielded arc welding method using the welding wire, and a method for producing a weld metal using the gas-shielded arc welding method. [Background technology]
[0002] Since automobile suspension parts are exposed to a corrosive environment due to moisture from the road surface and salt damage contained in snow-melting agents, a technology to prevent corrosion is required. Generally, a method of performing electrodeposition coating after arc welding is adopted as a method of protecting suspension parts from a corrosive environment. However, when performing electrodeposition coating after welding, a problem occurs in that an electrodeposition coating film is not formed on the welding slag (hereinafter, also simply referred to as "slag"), which causes coating defects, and corrosion progresses from these defects. There is also a method of suppressing the occurrence of coating defects by, for example, forming a thick electrodeposition coating film, but even if a coating film is formed on the slag, the coating film may peel off together with the slag due to impacts such as hitting a pebble during driving, and corrosion progresses from the peeled part. Thus, in parts manufactured by the conventional method, there was a risk that corrosion would occur due to poor coating on the welding slag, or even if a coating film was formed, corrosion would occur due to slag peeling during driving.
[0003] In response to the above problems, for example, Patent Document 1 proposes a gas-shielded arc welding wire that generates less spatter during welding, does not require processes such as slag removal after welding, has excellent electrodeposition paintability, and can obtain welds with good bead shapes. The welding wire contains, per total mass of the wire, C: 0.01% by mass or more and 0.10% by mass or less, Si: 0.05% by mass or more and 0.55% by mass or less, Mn: 1.60% by mass or more and 2.40% by mass or less, Ti: 0.05% by mass or more and 0.25% by mass or less, Cu: 0.01% by mass or more and 0.30% by mass or less, S: 0.001% by mass or more and 0.020% by mass or less, N: 0.0045% by mass or more and 0.0150% by mass or less, O: 0.0010% by mass or more and 0.0050% by mass or less, Al: 0.10% by mass or less, P: 0.025% by mass or less, the balance being Fe and unavoidable impurities, and 0.1≦[Ti] / [Si]≦3.0. Patent Document 1 describes that when the above-mentioned gas-shielded arc welding wire is used, a thin slag can be uniformly formed at the weld, and excellent electrodeposition paintability can be obtained without the need to remove the slag after welding.
[0004] Patent Document 2 proposes a solid wire for gas-shielded arc welding capable of forming a welded joint having excellent electrocoatability and mechanical properties, and a method for manufacturing a welded joint. The solid wire contains, in mass % relative to the total mass of the wire, C: 0.05-0.20%, Si: 0.01-0.18%, Mn: 1.0-3.0%, Ti: 0.06-0.25%, Al: 0.003-0.10%, B: 0-0.0100%, P: more than 0-0.015%, S: more than 0-0.015%, and optional elements, with the balance being iron and impurities, and satisfies Si×Mn≦0.30 and (Si+Mn / 5) / (Ti+Al)≦3.0, and further has a Ceq of 0.40-0.90%. Patent Document 2 describes that the use of the solid wire for gas-shielded arc welding makes it possible to form a welded joint having excellent electrocoatability and mechanical properties.
[0005] In this way, in the welding wires described in Patent Document 1 and Patent Document 2, the Si content is reduced to suppress the formation of Si, Mn-based slag with extremely low electrical conductivity, which makes it possible to form an excellent electrodeposition coating film even if slag is generated on the weld bead. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2021-74777 [Patent Document 2] Patent Publication No. 2021-3732 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the slag may aggregate depending on the elements added to the welding wire, and this aggregation may result in the formation of thick, lumpy slag. When this lumpy slag is formed, the slag may peel off or be crushed due to the impact generated during travel, as described above, even if an electrodeposition coating film is formed on the slag, resulting in the peeling off of the electrodeposition coating film.
[0008] Although Patent Document 1 describes that thin slag can be uniformly formed, it is difficult to form all the slag on the weld bead thin even if the above welding wire is used. For example, depending on the content of Ti, Si, and Mn, which are deoxidizing elements contained in the welding wire, slag may aggregate in the molten pool or on the surface of the molten pool, and lumpy slag may be generated. Furthermore, Patent Document 2 does not consider lumpy slag at all, and as long as deoxidizing elements such as Ti, Si, and Mn are added to the welding wire, lumpy slag will be generated to a certain extent. Therefore, the weld bead is required to have good electrocoatability and excellent bead appearance so that lumpy slag is not generated on the surface.
[0009] The present invention has been made in consideration of the above problems, and has an object to provide a welding wire for gas-shielded arc welding that can obtain a weld bead having excellent electrodeposition paintability, suppresses the generation of lumpy slag on the weld bead, and provides an excellent bead appearance, a gas-shielded arc welding method using the welding wire, and a method for producing a weld metal using the gas-shielded arc welding method. [Means for solving the problem]
[0010] The above object of the present invention is achieved by the following configuration [1] relating to a welding wire.
[0011] [1] A welding wire used for gas-shielded arc welding, For the total mass of the welding wire, Mn: more than 1.80 mass% and less than 2.20 mass%; Ti: 0.05% by mass or more, 0.23% by mass or less, Contains Al: more than 0.10% by mass and 0.25% by mass or less, Si: 0.45 mass% or less; The content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, When the content of Ti contained in the welding wire is expressed as [Ti] in mass% relative to the total mass of the welding wire, The value M1 calculated by the following formula 1 is 0.45 or less, A welding wire characterized in that a value M2 calculated by the following (Equation 2) is 0.30 or more and 2.50 or less. M1 = [Al] + [Ti] (Eq. 1) M2 = [Ti] / [Al] (equation 2)
[0012] Further, preferred embodiments of the present invention relating to the welding wire relate to the following [2] to [5].
[0013] [2] Furthermore, for the total mass of the welding wire, C: 0.30% by mass or less, Ni: 1.00% by mass or less, Cr: 1.00% by mass or less, Mo: 1.00% by mass or less, Cu: 1.00% by mass or less, Mg: 0.10% by mass or less, Zr: 0.10% by mass or less, Nb: 0.10% by mass or less, V: 0.10% by mass or less, B: 0.0050% by mass or less, Sn: 0.01% by mass or less, Sb: less than 0.01% by mass, P: 0.050% by mass or less, and S: 0.050% by mass or less, The welding wire according to [1], characterized in that the balance is Fe and unavoidable impurities.
[0014] [3] A welding wire containing flux, Contains an alloy component and a compound contained in the flux, The alloy components include For the total mass of the welding wire, C: 0.30% by mass or less, Ni: 1.00% by mass or less, Cr: 1.00% by mass or less, Mo: 1.00% by mass or less, Cu: 1.00% by mass or less, Mg: 0.10% by mass or less, Zr: 0.10% by mass or less, Nb: 0.10% by mass or less, V: 0.10% by mass or less, B: 0.0050% by mass or less, Sn: 0.01% by mass or less, Sb: less than 0.01% by mass, P: 0.050% by mass or less, and S: 0.050% by mass or less, The balance is Fe and unavoidable impurities. The welding wire according to [1], characterized in that the compound is more than 0 mass % and 5 mass % or less with respect to the total mass of the welding wire.
[0015] [4] The welding wire according to any one of [1] to [3], wherein a value M3 calculated by the following (Equation 3) is less than 0.25, where the content of Si contained in the welding wire is expressed as [Si] in mass% with respect to the total mass of the welding wire, and the content of Mn contained in the welding wire is expressed as [Mn] in mass% with respect to the total mass of the welding wire: M3 = [Si] / [Mn] (Equation 3)
[0016] [5] The welding wire according to any one of [1] to [4], characterized in that, when the content of Mn contained in the welding wire is expressed as [Mn] in mass% with respect to the total mass of the welding wire, a value M4 calculated by the following (Equation 4) is 0.70 or more and 0.95 or less. M4=[Mn] / ([Mn]+[Al]+[Ti]) (Formula 4)
[0017] The above object of the present invention is achieved by the gas shielded arc welding method having the following configuration [6].
[0018] [6] A gas-shielded arc welding method in which welding is performed while supplying a shielding gas using a welding wire, The welding wire has a mass of: Mn: more than 1.80 mass% and less than 2.20 mass%; Ti: 0.05% by mass or more, 0.23% by mass or less, Contains Al: more than 0.10% by mass and 0.25% by mass or less, Si: 0.45 mass% or less; The content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, When the content of Ti contained in the welding wire is expressed as [Ti] in mass% relative to the total mass of the welding wire, The value M1 calculated by the following formula 1 is 0.45 or less, A gas-shielded arc welding method, characterized in that a value M2 calculated by the following (Equation 2) is 0.30 or more and 2.50 or less. M1 = [Al] + [Ti] (Eq. 1) M2 = [Ti] / [Al] (equation 2)
[0019] Further, preferred embodiments of the present invention relating to a gas-shielded arc welding method relate to the following [7] to [9].
[0020] [7] The gas-shielded arc welding method according to [6], characterized in that the shielding gas contains at least one gas selected from Ar and CO2.
[0021] [8] The gas-shielded arc welding method according to [6], characterized in that welding is performed using a feed control method in which the feeding of the welding wire is alternately switched between a forward feed period and a reverse feed period.
[0022] [9] In the above-mentioned feeding control method, A frequency when the forward feed period and the reverse feed period are defined as one cycle is set within a predetermined range, The gas-shielded arc welding method according to [8], characterized in that the welding current supplied to the welding wire is switched between a current suppression period and a current non-suppression period based on at least one of information on a phase representing a feed speed of the welding wire and a phase representing a tip position of the welding wire.
[0023] The above object of the present invention relates to the following
[10] , which relates to a method for producing a weld metal.
[0024]
[10] A method for producing weld metal, comprising the steps of: welding using a welding wire while supplying a shielding gas to produce weld metal, The shielding gas contains at least one gas selected from Ar and CO2, The welding wire has a mass of: Mn: more than 1.80 mass% and less than 2.20 mass%; Ti: 0.05% by mass or more, 0.23% by mass or less, Contains Al: more than 0.10% by mass and 0.25% by mass or less, Si: 0.45 mass% or less; The content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, When the content of Ti contained in the welding wire is expressed as [Ti] in mass% relative to the total mass of the welding wire, The value M1 calculated by the following formula 1 is 0.45 or less, A method for producing a weld metal, characterized in that a value M2 calculated by the following (Equation 2) is 0.30 or more and 2.50 or less. M1 = [Al] + [Ti] (Eq. 1) M2 = [Ti] / [Al] (equation 2) Effect of the Invention
[0025] According to the present invention, it is possible to provide a welding wire for gas-shielded arc welding that can obtain a weld bead having excellent electrodeposition paintability, can suppress the generation of lumpy slag on the weld bead, and can obtain an excellent bead appearance, a gas-shielded arc welding method using the welding wire, and a method for producing a weld metal using the gas-shielded arc welding method. [Brief description of the drawings]
[0026] [Figure 1] FIG. 1 is a waveform diagram illustrating the change over time of the wire feed speed Fw, with the vertical axis representing the wire feed speed Fw and the horizontal axis representing time (phase). [Diagram 2] FIG. 2 is a waveform diagram illustrating the change over time in the wire tip position, where the vertical axis represents the tip position of the welding wire (hereinafter also referred to as "wire tip position") and the horizontal axis represents time (phase). [Diagram 3] FIG. 3 is a diagram showing an example of control of the current setting signal, in which the vertical axis represents the current detection signal Io and the horizontal axis represents time. [Figure 4]FIG. 4 is a schematic diagram showing the welding position during gas shielded arc welding used in this embodiment. [Diagram 5] FIG. 5 is a set of photographs showing the bead appearances after welding, after electro-deposition coating, and after impact for invention examples 1 to 4. [Figure 6] FIG. 6 is a set of photographs showing the bead appearances after welding, after electro-deposition coating, and after impact for invention examples 5 to 8. [Figure 7] FIG. 7 is a set of photographs showing the bead appearances after welding, after electro-deposition coating, and after impact for Comparative Examples 1 to 4. [Figure 8] FIG. 8 is a set of photographs showing the bead appearances after welding, after electrodeposition coating, and after impact for Comparative Examples 5 to 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] The present inventors conducted extensive research to solve the above problems and have come to the following findings: By specifying the combination of deoxidizing elements contained in the welding wire and their contents, it is possible to control the composition of oxides generated in the molten pool or on the molten pool surface and further suppress the generation of non-conductive vitreous oxides. As a result, a weld bead with excellent electrodeposition paintability can be obtained, and by dispersing the oxides, the generation of lumpy slag can be suppressed, resulting in a weld metal with excellent bead appearance.
[0028] Specifically, by making the Si content of the welding wire 0.45 mass% or less with respect to the total mass of the wire, it is possible to suppress the generation of non-conductive glassy oxides and ensure electrodeposition coating properties. In addition, by making the Mn, Ti, and Al contents of the welding wire more than 1.80 mass% and less than 2.20 mass%, Ti more than 0.05 mass% and less than 0.23 mass%, and Al more than 0.10 mass% and less than 0.25 mass%, and specifying the total amount and ratio of Ti and Al, it is possible to generate oxides that are easily dispersed and suppress the formation of lumpy slag on the surface of the weld bead.
[0029] It is believed that the formation of lumpy slag is mainly due to the aggregation of oxides in or on the molten pool. Generally, the worse the wettability between the oxide and the molten metal, the easier it is for the oxide to aggregate and to float to the surface of the molten pool. In other words, the worse the wettability between the oxide and the molten metal, the easier it is for lumpy slag to form on the weld bead. For example, Al2O3, an oxide of Al, has poor wettability with molten steel, so the inclusion of Al in the welding wire is generally avoided. However, the present inventor has found that the slag on the bead surface can be dispersed by intentionally adding an appropriate amount of Al to the welding wire and further adding Mn and Ti. This can be presumed to be because the wettability between the composite oxides formed in or on the molten pool surface and the molten metal is good based on these elements contained in the wire.
[0030] [Welding wire] Below, the embodiment for carrying out the present invention will be described in detail along the above mechanism. The present invention is not limited to the embodiment described below, and can be arbitrarily modified and carried out within the scope of the present invention. Below, the reason for adding the alloy components contained in the welding wire according to this embodiment and the reason for limiting the numerical value will be described in detail. In the following description, the content of each element in the welding wire is specified by the content of the element contained as an alloy component relative to the total mass of the welding wire. In the present invention, as described above, in order to obtain a bead having excellent electrodeposition paintability, suppressing the generation of lumpy slag on the bead surface, and having excellent bead appearance, it is necessary to specify at least Si, Mn, Ti, and Al in the following ranges. However, other alloy elements may be added arbitrarily depending on the base material used and the application. That is, components other than Si, Mn, Ti, and Al do not need to be contained in the wire, and may be 0 mass%.
[0031] The welding wire may be a solid wire made of alloying elements, or a flux-cored wire in which the flux is made only of metal powder (hereinafter also referred to as a metal-based flux-cored wire). Furthermore, the welding wire may be a flux-cored wire in which the flux contains even a small amount of compounds (mainly oxides, fluorides, etc.) (hereinafter also referred to as a slag-based flux-cored wire). In the metal-based flux-cored wire or slag-based flux-cored wire, the alloying elements described below may be contained in either the hoop or the flux.
[0032] (Si: 0.45 mass% or less (including 0 mass%)) Silicon is a deoxidizing agent, and when the welding wire contains silicon, it is possible to obtain an effect of improving the mechanical performance of the weld metal. The amount of silicon can be adjusted appropriately according to the required strength, but in this embodiment, the welding wire does not need to contain silicon, and the amount of silicon may be 0 mass %, as long as the strength can be ensured by other elements.
[0033] On the other hand, SiO2, an oxide of Si, is a non-conductive vitreous oxide, and if it remains as slag on the weld bead, it becomes impossible to form an electrodeposition coating film. Therefore, from the viewpoint of electrodeposition coating, the content of Si needs to be suppressed to 0.45 mass% or less with respect to the total mass of the welding wire. The lower the content of Si, the better, and it is preferably 0.30 mass% or less, and more preferably 0.20 mass% or less.
[0034] (Mn: more than 1.80 mass%, less than 2.20 mass%) Mn, like Si, is a deoxidizer, and when Mn is contained in the welding wire, the effect of improving the mechanical performance of the weld metal can be obtained. In addition, by combining Mn with Ti and Al, which will be described later, it is possible to disperse slag generated on the bead. Furthermore, since MnO has a relatively high electrical conductivity, the higher the Mn content in the welding wire, the better the electrodeposition paintability becomes. If the Mn content in the welding wire is 1.80 mass% or less, the above effect cannot be obtained. Therefore, it is preferable that the Mn content in the welding wire is more than 1.80 mass% and more than 1.90 mass% with respect to the total mass of the welding wire. On the other hand, if the Mn content in the wire is 2.20 mass% or more, excessive deoxidation occurs and the amount of oxygen in the molten pool decreases, which increases the surface tension of the droplets and impairs the bead shape. Therefore, the Mn content in the welding wire should be less than 2.20 mass%, and preferably less than 2.10 mass%, relative to the total mass of the wire.
[0035] (Ti: 0.05 mass% or more, 0.23 mass% or less) Ti is a strong deoxidizing element, and is an element that preferentially forms oxides by deoxidizing action. Therefore, like Mn and Al, Ti is an element that greatly contributes to the composition of slag. As described above, by combining Ti with Mn and Al in the welding wire, it is possible to obtain the effect of dispersing the slag generated on the bead. If the Ti content in the welding wire is less than 0.05 mass%, the above effect cannot be obtained. Therefore, the Ti content in the welding wire is set to 0.05 mass% or more, and preferably 0.08 mass% or more, with respect to the total mass of the welding wire. On the other hand, if Ti is excessively contained in the welding wire in an amount exceeding 0.23 mass%, the composition of the slag changes and the desired slag dispersion effect cannot be obtained. Therefore, the Ti content in the welding wire is set to 0.23 mass% or less, and preferably 0.21 mass% or less, based on the total mass of the wire.
[0036] (Al: more than 0.10 mass%, 0.25 mass% or less) Like Ti, Al is a strong deoxidizing element, and is an element that preferentially forms oxides through its deoxidizing action. Therefore, like Mn and Ti, Al is an element that contributes greatly to the composition of slag. As described above, by combining Al with Mn and Ti in the welding wire, it is possible to obtain the effect of dispersing the slag generated on the bead. If the Al content in the welding wire is 0.10 mass% or less, the above effect cannot be obtained. Therefore, it is preferable that the Al content in the welding wire is more than 0.10 mass% and is 0.12 mass% or more with respect to the total mass of the welding wire. On the other hand, if the Al content in the welding wire is excessively more than 0.25 mass%, the composition of the slag changes and the desired slag dispersion effect cannot be obtained. Therefore, the Al content in the welding wire is set to 0.25 mass% or less, and preferably 0.22 mass% or less, with respect to the total mass of the wire.
[0037] (M1: 0.45 or less, M2: 0.30 or more and 2.50 or less) As described above, in this embodiment, by defining the total amount and ratio of Ti and Al, oxides that are easily dispersed are generated, and the formation of lumpy slag on the surface of the weld bead is suppressed. If the total content of Al and Ti, that is, the value M1 calculated by the following (Equation 1), exceeds 0.45, the amount of slag itself increases and the slag composition changes, making it difficult to obtain the slag dispersion effect. Therefore, M1 is set to 0.45 or less, preferably 0.40 or less, more preferably 0.39 or less, and even more preferably 0.35 or less.
[0038] In this embodiment, the lower limit of the Al content and the Ti content are specified, and even if these are the lower limit, the slag dispersion effect can be sufficiently obtained, so the lower limit of M1 is not particularly limited. However, in order to obtain a further slag dispersion effect, M1 is preferably 0.24 or more, more preferably 0.25 or more, and even more preferably 0.27 or more.
[0039] In this embodiment, it is important to specify the total content of Al and Ti, and also to specify the ratio of the Ti and Al contents, that is, the value M2 calculated by the following (Equation 2). If M2 is less than 0.30, the slag dispersion effect cannot be sufficiently obtained. Therefore, M2 is set to 0.30 or more, and preferably 0.40 or more.
[0040] On the other hand, if M2 exceeds 2.50, the slag dispersion effect cannot be sufficiently obtained. Therefore, M2 is set to 2.50 or less, preferably 1.80 or less, and more preferably 1.30 or less.
[0041] In this way, it is believed that an optimal slag composition can be obtained by controlling the total value of the Al and Ti contents and the Al and Ti contents in the wire within the range of their ratio, and as a result, an excellent slag dispersion effect can be obtained.
[0042] M1 = [Al] + [Ti] (Eq. 1) M2 = [Ti] / [Al] (equation 2) Here, [Al] is a value representing the content of Al contained in the welding wire, expressed as mass % with respect to the total mass of the welding wire, and [Ti] is a value representing the content of Ti contained in the welding wire, expressed as mass %, with respect to the total mass of the welding wire.
[0043] As described above, the welding wire according to the present embodiment has the Si, Mn, Ti, and Al contents regulated, and the M1 and M2 contents appropriately controlled, thereby realizing the electrodeposition coating property on the weld bead and the suppression of the generation of lumpy slag. Therefore, the following elements other than the above elements can be appropriately adjusted according to the base material and the required properties, and may be 0 mass%. Hereinafter, the preferred ranges of the contents of the optional elements in the welding wire according to the present embodiment and the reasons for the limitations will be described in detail. Note that, when the welding wire according to the present embodiment contains elements other than the above Si, Mn, Ti, and Al, it is sufficient that at least one of the following elements is contained within the ranges shown below, and the element to be contained can be selected according to the required properties, etc.
[0044] (C: 0.30% by mass or less (including 0% by mass)) C has a deoxidizing effect, and when C is contained in the welding wire, it is possible to obtain an effect of improving the mechanical performance of the weld metal. The C content can be appropriately adjusted according to the required strength, but in this embodiment, if the strength can be ensured by other elements, the welding wire does not need to contain C, and the C content may be 0 mass %. However, if the welding wire contains an excessive amount of C, the deoxidizing effect becomes large, and CO is generated near the arc, which may cause an explosion, resulting in spatter generation and an increase in the amount of fumes. Therefore, from the viewpoint of welding workability, the C content in the welding wire is preferably 0.30 mass% or less, more preferably 0.10 mass% or less, and even more preferably 0.08 mass% or less, based on the total mass of the welding wire.
[0045] (Ni: 1.00 mass% or less (including 0 mass%)) When the welding wire contains Ni, it is possible to obtain an effect of enhancing the mechanical performance of the weld metal. The Ni content can be appropriately adjusted according to the required strength, but in this embodiment, if the strength can be ensured by other elements, the welding wire does not need to contain Ni, and may contain 0 mass%. In addition, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa steel plates applied to automobile suspension parts, the Ni content is preferably 1.00 mass% or less with respect to the total mass of the welding wire. By suppressing the Ni content as described above, a balance is achieved with other elements that enhance mechanical performance, and it is possible to suppress the weld metal from becoming excessively strong.
[0046] (Cr: 1.00% by mass or less (including 0% by mass)) When the welding wire contains Cr, it is possible to obtain an effect of enhancing the mechanical properties of the weld metal. The Cr content can be appropriately adjusted according to the required strength, but in this embodiment, if the strength can be ensured by other elements, the welding wire does not need to contain Cr, and may contain 0 mass% Cr. In addition, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa class steel plates applied to automobile suspension parts, the Cr content is preferably 1.00 mass% or less with respect to the total mass of the welding wire. By suppressing the Cr content as described above, a balance with other elements that enhance mechanical properties can be achieved, and the weld metal can be suppressed from becoming excessively strong.
[0047] (Mo: 1.00 mass% or less (including 0 mass%)) When the welding wire contains Mo, it is possible to obtain an effect of enhancing the mechanical properties of the weld metal. The content of Mo can be appropriately adjusted according to the required strength, but in this embodiment, if the strength can be ensured by other elements, the welding wire does not need to contain Mo, and may contain 0 mass% Mo. In addition, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa steel plates applied to automobile suspension parts, the Mo content is preferably 1.00 mass% or less with respect to the total mass of the welding wire. By suppressing the Mo content as described above, a balance is achieved with other elements that enhance the mechanical properties, and it is possible to suppress the weld metal from becoming excessively strong.
[0048] (Cu: 1.00 mass% or less (including 0 mass%)) When the welding wire contains Cu, it is possible to obtain an effect of enhancing the mechanical performance of the weld metal. The content of Cu can be appropriately adjusted according to the required strength, but in this embodiment, if the strength can be ensured by other elements, the welding wire may not contain Cu, and may be 0 mass%. Here, the Cu content in this specification also includes Cu in the plating that may be formed on the surface of the welding wire. In addition, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa class steel plates applied to automobile suspension parts, the Cu content in the welding wire including the plating is preferably 1.00 mass% or less with respect to the total mass of the welding wire. By suppressing the Cu content as described above, a balance with other elements that enhance mechanical performance can be achieved, and excessive strength of the weld metal can be suppressed.
[0049] (Mg: 0.10% by mass or less (including 0% by mass)) (Zr: 0.10 mass% or less (including 0 mass%)) Mg and Zr, like Al and Ti, are strong deoxidizing elements and preferentially form oxides due to their deoxidizing action. As the content of Mg and Zr in the welding wire increases, the slag composition changes, and there is a possibility that the slag dispersion effect cannot be obtained. Therefore, if it is desired to obtain a deoxidizing effect by including Mg and Zr in the welding wire without reducing the slag dispersion effect, it is preferable that the Mg content and the Zr content are each 0.10 mass% or less with respect to the total mass of the welding wire.
[0050] (Nb: 0.10 mass% or less (including 0 mass%)) (V: 0.10% by mass or less (including 0% by mass)) When Nb and V are contained in the welding wire, the effect of enhancing the mechanical performance of the weld metal can be obtained. The contents of Nb and V can be appropriately adjusted according to the required strength, but in this embodiment, if the strength can be ensured by other elements, Nb and V do not need to be contained in the welding wire, and may be 0 mass%. In addition, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa class steel plates applied to automobile suspension parts, the Nb content and V content in the welding wire are preferably 0.10 mass% or less, respectively, with respect to the total mass of the welding wire. By suppressing the Nb content and V content as described above, a balance with other elements that enhance mechanical performance can be achieved, and excessive strength of the weld metal can be suppressed.
[0051] (B: 0.0050% by mass or less (including 0% by mass)) When the welding wire contains B, it is possible to obtain an effect of enhancing the mechanical properties of the weld metal. The content of B can be appropriately adjusted according to the required strength, but in this embodiment, if the strength can be ensured by other elements, the welding wire does not need to contain B, and may contain 0 mass%. In addition, when the welding wire according to this embodiment is used in lap fillet welding of 440 to 980 MPa class steel plates applied to automobile suspension parts, the B content is preferably 0.0050 mass% or less with respect to the total mass of the welding wire. By suppressing the B content as described above, a balance with other elements that enhance mechanical properties can be achieved, and the weld metal can be suppressed from becoming excessively strong.
[0052] (Sn: 0.01 mass% or less (including 0 mass%)) Sn is a low melting point element, and if the welding wire contains Sn in excess of a certain range, hot cracking is likely to occur. Therefore, the Sn content in the welding wire is preferably at the impurity level, and may be 0 mass%. When the welding wire contains Sn, the Sn content in the welding wire is preferably suppressed to less than 0.01 mass% with respect to the total mass of the welding wire.
[0053] (Sb: Less than 0.01% by mass (including 0% by mass)) Sb is an element that affects the physical properties of molten metal, and Sb in the welding wire affects the behavior of the molten pool. Specifically, Sb has a boiling point of 1587°C and is easily vaporized in the molten pool, which causes porosity defects (pits and blowholes) and causes the convection on the molten pool surface to be disturbed by the release of pores. For this reason, if the welding wire contains Sb at a content above a predetermined range, slags may easily collide with each other, and the aggregation of slags may be promoted. Therefore, the Sb content in the welding wire is preferably at the impurity level, and may be 0 mass%. When the welding wire contains Sb, the Sb content in the welding wire is preferably suppressed to less than 0.01 mass% with respect to the total mass of the welding wire.
[0054] (P: 0.050 mass% or less (including 0 mass%)) P is an element that affects the cracking tendency of the weld metal, and the lower the P content in the welding wire, the better the cracking resistance of the weld metal, so the welding wire according to this embodiment does not need to contain P, and may contain 0 mass % P. Note that, when the welding wire contains P, from the viewpoint of cracking resistance, the P content in the welding wire is preferably 0.050 mass % or less with respect to the total mass of the welding wire.
[0055] (S: 0.050% by mass or less (including 0% by mass)) S is an element that reduces the surface tension of molten metal, and when S is contained in a welding wire, it is possible to obtain the effect of forming a flat weld bead. The effect of forming a flat weld bead can be obtained by substituting other surface active elements (oxygen, selenium, tellurium, etc.), so there is no particular lower limit for the S content, and it may be 0 mass%. However, when a flat weld bead is formed by containing S in the welding wire, it is preferable that the S content in the welding wire is 0.001 mass% or more with respect to the total mass of the welding wire. On the other hand, the higher the S content in the welding wire, the more likely it is that sulfides will be generated and the slag composition will change, which may result in the desired slag dispersion effect not being obtained. Therefore, the S content in the welding wire is preferably 0.050 mass% or less with respect to the total mass of the welding wire.
[0056] (The balance of alloying elements is Fe and unavoidable impurities) In this embodiment, the balance of the alloy elements of the wire preferably used is Fe and inevitable impurities. Examples of inevitable impurities include O, N, Li, Bi, and As. The content of each of these inevitable impurities is preferably 0.0100 mass% or less, and more preferably 0.0050 mass% or less, based on the total mass of the wire. In addition, the total content of these inevitable impurities is preferably 0.0200 mass% or less, based on the total mass of the wire.
[0057] The welding wire according to the present embodiment may be a welding wire containing flux, and may contain alloy components and compounds contained in the flux. In this way, in the case of a slag-based flux-cored wire containing compounds in the flux, in addition to the above-mentioned alloy components, the flux may further contain compounds in an amount of more than 0 mass% and 5 mass% or less with respect to the total mass of the wire, more preferably 3 mass% or less of compounds, and even more preferably 1 mass% or less of compounds. Examples of the compounds include oxides, sulfides, carbides, nitrides, fluorides, etc., such as B2O3, Na2O, and K2O. Note that even if the welding wire is a slag-based flux-cored wire, the preferred range of the content of each alloy component is as described above.
[0058] In this embodiment, by specifying the ratio of the Si content to the Mn content in the welding wire, the mechanical properties of the weld metal can be adjusted and a more excellent slag dispersion effect can be obtained. Furthermore, by specifying the values calculated by a specific formula using the contents of Mn, Al, and Ti, a more excellent slag dispersion effect can be obtained. The limited ranges of these values and the reasons therefor will be explained below.
[0059] (M3: Less than 0.25) Since Si is an element that reduces the electrocoatability, it is preferable to reduce the Si content in the welding wire as much as possible. However, since Si is also an element that has the effect of enhancing the mechanical performance of the weld metal, it is necessary to supplement the mechanical performance of the weld metal with another element by reducing the Si content. In this embodiment, the relationship between the Al content and the Ti content is adjusted as described above to control the slag composition and achieve an excellent slag dispersion effect. For this reason, as a method for adjusting the mechanical performance, it is preferable to increase the Mn content and add as few other elements as possible. If the ratio of the Si content to the Mn content, that is, the value M3 calculated by the following (Equation 3), is set to less than 0.25, the mechanical performance and slag dispersion effect of the weld metal can be further improved. Therefore, it is preferable to adjust the Mn content and the Si content so that M3 is less than 0.25, more preferably adjust the Mn content and the Si content so that M3 is 0.20 or less, and more preferably adjust the Mn content and the Si content so that M3 is 0.15 or less.
[0060] M3 = [Si] / [Mn] (Equation 3) Here, [Si] is a value representing the amount of Si contained in the welding wire, expressed as mass % with respect to the total mass of the welding wire, and [Mn] is a value representing the amount of Mn contained in the welding wire, expressed as mass %, with respect to the total mass of the welding wire.
[0061] (M4: 0.70 or more and 0.95 or less) In this embodiment, if the ratio of the Mn content to the total content of Mn, Al, and Ti in the welding wire, that is, the value M4 calculated by the following (Formula 4), is appropriately defined, the slag composition can obtain a more excellent slag dispersion effect. Therefore, M4 is preferably 0.70 or more, and more preferably 0.80 or more. Moreover, M4 is preferably 0.95 or less, and more preferably 0.90 or less.
[0062] M4=[Mn] / ([Mn]+[Al]+[Ti]) (Formula 4) Here, [Mn] is a value representing the amount of Mn contained in the welding wire, expressed as mass %, relative to the total mass of the welding wire; [Al] is a value representing the amount of Al contained in the welding wire, expressed as mass %, relative to the total mass of the welding wire; and [Ti] is a value representing the amount of Ti contained in the welding wire, expressed as mass %, relative to the total mass of the welding wire.
[0063] (Wire diameter) In the welding wire according to the present embodiment, the wire diameter (diameter) is not particularly limited, but a wire having a diameter specified in a welding material standard such as AWS or JIS can be used.
[0064] (Wire manufacturing) In the welding wire according to the present embodiment, the manufacturing method is not particularly limited, and no special manufacturing conditions are required, and the wire can be manufactured by a conventional method. For example, in the case of a solid wire, a steel containing the above alloy elements at a specified content is melted to obtain an ingot. Next, the ingot is subjected to hot forging or the like as necessary, then hot rolling, and further cold wire drawing to form a wire. Thereafter, the obtained wire is annealed at a temperature of about 500 to 900 ° C. as necessary, pickled, copper plated as necessary, and further finish wire drawing as necessary to obtain a target wire diameter. Thereafter, a lubricant is applied as necessary to manufacture the welding wire.
[0065] Next, the gas shielded arc welding method according to this embodiment will be described below.
[0066] [Gas shielded arc welding method] The gas-shielded arc welding method according to the present embodiment is a method for performing welding while supplying a shielding gas, using the welding wire according to the present embodiment. The contents of Si, Mn, Ti, and Al in the welding wire, and the values of M1 and M2 calculated based on the Ti content and Al content are as described above. The preferred ranges of the other alloying elements are also as described above.
[0067] (Shielding gas) In the gas-shielded arc welding method according to the present embodiment, the shielding gas to be used is not particularly limited, but it is preferable to use a gas composition that takes the form of globule transition due to the characteristics of the control that is preferable to be used in the present embodiment. Specifically, it is preferable to include at least one gas among carbon dioxide gas, nitrogen gas, hydrogen gas, and oxygen gas, which have a high potential gradient. In addition, from the viewpoint of versatility, it is preferable to use a shielding gas that contains at least one gas selected from Ar and CO2. For example, when using a mixed gas containing argon gas (hereinafter also referred to as "Ar gas"), it is more preferable to use a mixed gas that contains at least 10 volume % or more of carbon dioxide gas. Furthermore, it is preferable to use a mixed gas that contains 90 volume % or more of carbon dioxide gas, and it is particularly preferable to use a shielding gas of carbon dioxide gas alone.
[0068] By performing welding using the gas-shielded arc welding method according to the present embodiment, it is possible to form a weld bead whose surface has excellent electrocoatability and in which the generation of lumpy slag is suppressed.
[0069] In the gas-shielded arc welding method according to the present embodiment, other welding conditions using the welding wire according to the present embodiment and the above-mentioned predetermined shielding gas are not particularly limited. For example, a pulsed MAG welding method or a feed control method may be used, but it is preferable to use the feed control method from the viewpoint of welding workability. The feed control method will be described in detail below.
[0070] (Feeding control method) The feed control method is a method of welding by alternately switching the feed of the welding wire between a forward feed period and a reverse feed period. The feed control method can be further classified into a "short-circuit type feed control method" and a "short-circuit suppression type feed control method". The short-circuit type feed control method is a type of welding in which the feed speed of the welding wire is alternately switched between a forward feed period and a reverse feed period, and a short-circuit transition form that generates a short-circuit period and an arc period is used as a base. The short-circuit suppression type feed control method is a type of welding in which the feed speed of the welding wire is alternately switched between a forward feed period and a reverse feed period, and a globule transition form that suppresses the occurrence of a short-circuit period is used as a base. In the gas-shielded arc welding method according to the present embodiment, it is more preferable to use the short-circuit suppression type feed control method, which can obtain a weld bead having a better appearance and can also improve the welding workability. In addition, when a zinc-plated steel sheet is used as the base material, the occurrence of porosity defects (pits or blowholes), which are a problem in welding of zinc-plated steel sheets, can be suppressed.
[0071] The short circuit suppression type feed control method preferably used in this embodiment will be described in further detail.
[0072] FIG. 1 is a waveform diagram illustrating the change in the wire feed speed Fw over time, with the vertical axis representing the wire feed speed Fw and the horizontal axis representing time (phase). The vertical axis is in meters per minute or revolutions per minute. In FIG. 1, the period during which the speed is higher than the average feed speed Fave is called the "normal feed period T P " and the period when the speed is smaller than the average feed speed Fave is called the "reverse feed period T N In addition, the first half of each delivery period is called the "early period" and the second half is called the "late period." Here, the average feed rate Fave can be regarded as the wire melting rate Fm.
[0073] Fig. 2 is a waveform diagram illustrating the change over time in the wire tip position when the vertical axis represents the tip position of the welding wire (hereinafter also referred to as the "wire tip position") and the horizontal axis represents time (phase). In Fig. 2, the position (height) when the welding wire is fed at the maximum or minimum feed speed is set as the reference distance. Also, in Fig. 2, T0 and T4 represent the times when the tip position of the welding wire is closest to the base metal (hereinafter also referred to as the "bottom end"), and T2 represents the time when the tip position of the welding wire is farthest from the base metal and closest to the power feed tip (hereinafter also referred to as the "top end").
[0074] As shown in FIG. 2, the period during which the tip position of the welding wire approaches the base metal over time, specifically, the period during which the tip position of the welding wire moves from the top end to the bottom end, is called the “normal feeding period T P The period during which the tip position of the welding wire approaches the power feed tip side with the passage of time, specifically, the period during which the tip position of the welding wire moves from the lowermost end to the uppermost end, is called the "reverse feed period T N "
[0075] Also, the points in time corresponding to the reference distance are designated as T1 and T3. T1 is the midpoint from the bottom end, where the tip of the welding wire is closest to the base metal, to the top end, where the tip is closest to the power contact tip. Meanwhile, T3 is the midpoint from the top end to the bottom end. As shown in Figure 2, the range of change from the top end to the bottom end is the "wave height Wh."
[0076] 3 is a diagram showing an example of control of the current setting signal, with the vertical axis representing the current detection signal Io and the horizontal axis representing time. Time points T0, T1, T2, T3, and T4 in the diagram correspond to time points T0, T1, T2, T3, and T4 in FIG. 2, respectively.
[0077] In this embodiment, the welding current supplied to the welding wire is controlled based on at least one of information on a phase representing the feed speed of the welding wire as shown in FIG. 1 (hereinafter also referred to as a "feed speed phase") and information on a phase representing the tip position of the welding wire as shown in FIG. 2 (hereinafter also referred to as a "wire position phase") during a current non-suppression period T IP and current suppression period T IB For example, the welding current is controlled to be switched between the current suppression period T and the current suppression period T based on the wire position phase of 0 to 360 degrees (0 to 2π), with the wire tip position closest to the power feed tip being set to 0 deg and the wire tip position closest to the base metal being set to 180 deg. IB and the current non-suppression period T IP In addition, the current non-suppression period T IP The set current value Ip is also called the peak current, and the current suppression period T IB The set current value Ib is also called the base current. IP The time when the peak current starts is called the peak current start time, and the current non-suppression period T IP The time when the peak current ends can be expressed as the peak current end time.
[0078] As shown in Fig. 3, the timing of the peak current end time is determined by a set period d1 whose start time is the point when the wire position phase becomes 0 deg, and the timing of the peak current start time is determined by a set period d2 whose start time is the peak current end time. This set period is preferably set by phase. For example, if d1 is set to 190° and d2 is set to 120°, the peak current ends when the wire position phase is at 190° (d1) and starts when the wire position phase is at 310° (d1+d2). Note that the current suppression period T IB includes the falling period and the current non-suppression period T IP includes the rise period.
[0079] In the above-mentioned short circuit suppression type feed control method, it is preferable to set the wire forward / reverse frequency, which is the frequency when the forward feed period and the reverse feed period are defined as one cycle, within a predetermined range. For example, it is preferable from the viewpoint of welding workability to set the wire forward / reverse frequency to be in the range of 50 Hz or more and 150 Hz or less, and the wire amplitude indicated by the wave height Wh to be in the range of 3.3 mm or more and 6.3 mm or less.
[0080] (Welding position) In the gas-shielded arc welding method according to the present embodiment, the welding position is not particularly limited. However, the welding wire according to the present embodiment is preferably used for horizontal lap fillet welding, and the welding position is preferably a flat position or a horizontal position.
[0081] (base material) In the gas shielded arc welding method according to the present embodiment, the base material is not particularly limited. The composition of the steel sheet is not particularly limited, and a zinc-plated steel sheet having a steel sheet surface plated with zinc may be used.
[0082] [Method of manufacturing weld metal] The method for producing a weld metal according to this embodiment is a method for producing a weld metal by using the welding wire according to this embodiment described above. The method for producing a weld metal according to this embodiment is also a method for producing a weld metal by using the gas-shielded arc welding method according to this embodiment described above. A specific example of the method for producing a weld metal according to this embodiment is as described in the embodiment relating to the welding wire and the gas-shielded arc welding method. The weld metal produced by the method for producing a weld metal according to this embodiment has excellent electrodeposition paintability on the surface, is free of lumpy slag, and has an excellent appearance.
[0083] [Weld metal] The weld metal obtained by the method for producing a weld metal according to this embodiment preferably contains predetermined components. The composition of the weld metal is affected by the component composition of the welding wire according to this embodiment and the component composition of the base metal, but in this embodiment, it is preferable that the content of each element in the weld metal relative to the total mass of the weld metal is in the following range.
[0084] In other words, the weld metal contains Mn: more than 0.50 mass% and less than 2.00 mass%, Ti: 0.005 mass% or more and 0.10 mass% or less, Al: more than 0.005 mass% and 0.15 mass% or less. Contains, Si: 0.45% by mass or less, C: 0.30% by mass or less, Ni: 1.00% by mass or less, Cr: 1.00% by mass or less, Mo: 1.00% by mass or less, Cu: 1.00% by mass or less. It is preferable that the alloy contains at least one selected from Mg: 0.10 mass% or less, Zr: 0.10 mass% or less, Nb: 0.10 mass% or less, V: 0.10 mass% or less, B: 0.0050 mass% or less, Sn: 0.01 mass% or less, Sb: less than 0.01 mass%, P: 0.050 mass% or less, and S: 0.050 mass% or less, with the balance being Fe and unavoidable impurities. EXAMPLES
[0085] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples, and can be modified within the scope of the present invention, and all of these are included in the technical scope of the present invention. In addition, the welding conditions described here are merely examples, and the present embodiment is not limited to the following welding conditions.
[0086] [Gas shielded arc welding] Gas shielded arc welding was carried out using welding wires having various compositions. Fig. 4 is a schematic diagram showing the welding position during gas-shielded arc welding used in this example. As shown in Fig. 4, steel sheets 1 and 2 were arranged at positions offset from each other, and welding was performed toward a fillet portion formed by the upper surface of steel sheet 1 and the end surface of steel sheet 2 while flowing shielding gas and controlling the feed speed of welding wire 4 with power feed tip 3. The composition of the welding wire used is shown in Table 1 below, and the feed control conditions and other welding conditions are shown below.
[0087] <Feed control conditions> Wire frequency: 70Hz Wave height: 5mm (amplitude ±2.5mm) Current control switching timing: Wire position phase 100~150deg at the end of peak current Wire position phase at the end of base current: 300~360deg
[0088] <Other welding conditions> Steel plate 1, Steel plate 2: Length 200mm x Width 50mm x Thickness 2.3mm, zinc-plated steel plate (SGAH440) Welding position: horizontal lap fillet weld Torch angle (angle between steel plate 1 and welding wire 4) θ: 60° Shielding gas: 100% CO2 gas by volume Average current: 200~250A Average voltage: 19~27V Wire feed rate: 7.0m / min Welding speed: 100cm / min Welding length: 150mm
[0089] <Evaluation test> (Observation of bead appearance after welding) The surface of the obtained weld bead was photographed, and the bead appearance was evaluated. In this embodiment, the bead appearance is measured within a range of 20 mm in the captured image. 2 Slag with an area of 150 mm or more was judged to be lumpy slag, and if even one lump of slag was formed within 150 mm of the weld length, it was deemed to have failed and was marked C. 2If no lumpy slag of an area of 2 mm or more is formed, the test is considered to have passed. 2 Above, 20mm 2 The case where a small slag with an area of less than 2 mm was formed was marked as B. 2 A case in which only lumpy slag of less than 100 mm was formed or no lumpy slag was formed at all was rated as a more favorable result and was designated an A.
[0090] (Bead appearance after electrocoating) Next, the obtained joint was subjected to electrodeposition coating to form an electrodeposition coating film on the surface. In this example, the bead appearance was observed, and when the electrodeposition coating film was formed on the entire surface of the weld bead, it was judged as passing and indicated as "Good." When there was any part where the electrodeposition coating film was not formed, it was judged as failing and indicated as "Bad."
[0091] (Bead appearance after impact) For the joints on which the electrodeposition coating film had been formed, impacts were applied multiple times with a hammer to the back side of the weld bead, and the presence or absence of peeling of the electrodeposition coating film was observed. In this example, the entire surface of the weld bead was observed for the presence or absence of slag peeling, and the case where no slag (electrodeposition coating film) peeling occurred was deemed to have passed and was indicated as "Good." On the other hand, the case where slag (electrodeposition coating film) peeling occurred in even one place was deemed to have failed and was indicated as "Bad."
[0092] (Pit Observation) The surface of the weld metal was visually inspected for the presence or absence of pits. In this example, the case where no pits were observed on a weld length of 150 mm was recorded as "absent," and the case where pits were observed was recorded as "present."
[0093] <Evaluation Results> 5 to 8 are photographs showing the bead appearances after welding, after electrocoating, and after impact for each of the invention examples and comparative examples. The evaluation results obtained from these appearances are shown in Table 2 below.
[0094] The balance other than the components shown in Table 1 below is Fe and inevitable impurities. In addition, in the column of the content of the components in Table 1, "-" indicates that the content was below the detection limit. Furthermore, the values of M2 in Comparative Examples 4 and 5 and the values of M4 in Comparative Examples 6 and 7 were calculated assuming that the contents of Ti and Al were 0 mass%, respectively. The values of M2 in Comparative Examples 6 and 7 could not be calculated, so they were indicated as "-". In addition, in Table 1 below, M1 to M4 are values obtained by the following (Equations 1) to (Equations 4), respectively.
[0095] M1 = [Al] + [Ti] (Eq. 1) M2 = [Ti] / [Al] (equation 2) M3 = [Si] / [Mn] (Equation 3) M4=[Mn] / ([Mn]+[Al]+[Ti]) (Formula 4) Here, [Al] is a value representing the content of Al contained in the welding wire, expressed as mass % with respect to the total mass of the welding wire, and [Ti] is a value representing the content of Ti contained in the welding wire, expressed as mass %, with respect to the total mass of the welding wire. Moreover, [Si] is a value representing the amount of Si contained in the welding wire, expressed as mass %, relative to the total mass of the welding wire, and [Mn] is a value representing the amount of Mn contained in the welding wire, expressed as mass %, relative to the total mass of the welding wire.
[0096] [Table 1]
[0097] [Table 2]
[0098] 5 to 8, in the columns showing the appearance of the bead after welding, the black areas indicate the formation of lumpy slag, and in the columns showing the appearance of the bead after impact application, the white areas indicate the peeling of the electrodeposition coating film.
[0099] As shown in Figures 5 to 8 and Tables 1 and 2, in Examples 1 to 8, the contents of Mn, Ti, Al, and Si in the welding wire and the values of M1 and M2 were within the ranges specified in the present invention, so that the electrodeposition paintability of the surface was excellent, no lumpy slag was formed, and a weld bead with excellent appearance could be obtained. Therefore, even when an impact was applied after the electrodeposition paint, the slag did not peel off, and an excellent joint could be obtained.
[0100] On the other hand, in Comparative Examples No. 1 to 7, at least one of the contents of Mn, Ti, Al, and Si in the welding wire and the values of M1 and M2 is outside the range specified in the present invention. Therefore, although the electrodeposition coatability of the surface was excellent, lumpy slag was formed, and when an impact was applied after the electrodeposition coating, the electrodeposition coating film peeled off together with the slag. [Explanation of symbols]
[0101] 1, 2 steel plate 3 Power supply chip 4 Welding Wire
Claims
1. A welding wire used for gas shielded arc welding, For the total mass of the welding wire, Mn: more than 1.80 mass% and less than 2.20 mass%; Ti: 0.05% by mass or more and 0.23% by mass or less, Contains Al: more than 0.10% by mass and 0.25% by mass or less, Si: 0.45% by mass or less; The content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, When the content of Ti contained in the welding wire is expressed as [Ti] in mass% with respect to the total mass of the welding wire, The value M1 calculated by the following (Equation 1) is 0.45 or less, A welding wire, characterized in that a value M2 calculated by the following (Equation 2) is 0.30 or more and 2.50 or less. M1=[Al]+[Ti]...(Formula 1) M2=[Ti] / [Al]...(Formula 2)
2. Furthermore, with respect to the total mass of the welding wire, C: 0.30% by mass or less, Ni: 1.00% by mass or less, Cr: 1.00% by mass or less, Mo: 1.00% by mass or less, Cu: 1.00% by mass or less, Mg: 0.10% by mass or less, Zr: 0.10% by mass or less, Nb: 0.10% by mass or less, V: 0.10% by mass or less, B: 0.0050% by mass or less, Sn: 0.01% by mass or less, Sb: less than 0.01% by mass, P: 0.050% by mass or less, and S: 0.050% by mass or less, The welding wire according to claim 1 , wherein the balance is Fe and unavoidable impurities.
3. A welding wire including a flux, Contains an alloy component and a compound contained in the flux, The alloy components include For the total mass of welding wire, C: 0.30% by mass or less, Ni: 1.00% by mass or less, Cr: 1.00% by mass or less, Mo: 1.00% by mass or less, Cu: 1.00% by mass or less, Mg: 0.10% by mass or less, Zr: 0.10% by mass or less, Nb: 0.10% by mass or less, V: 0.10% by mass or less, B: 0.0050% by mass or less, Sn: 0.01% by mass or less, Sb: less than 0.01% by mass, P: 0.050% by mass or less, and S: 0.050% by mass or less, The balance is Fe and inevitable impurities. The welding wire according to claim 1 , wherein the compound is more than 0 mass % and 5 mass % or less with respect to a total mass of the welding wire.
4. The welding wire according to any one of claims 1 to 3, characterized in that, when a content of Si contained in the welding wire is expressed as [Si] in mass % with respect to a total mass of the welding wire, and a content of Mn contained in the welding wire is expressed as [Mn] in mass % with respect to a total mass of the welding wire, a value M3 calculated by the following (Equation 3) is less than 0.
25. M3=[Si] / [Mn]...(Formula 3)
5. The welding wire according to any one of claims 1 to 3, characterized in that, when a content of Mn contained in the welding wire is expressed as [Mn] in mass% with respect to a total mass of the welding wire, a value M4 calculated by the following (Equation 4) is 0.70 or more and 0.95 or less. M4=[Mn] / ([Mn]+[Al]+[Ti])...(Formula 4)
6. A gas-shielded arc welding method for performing welding using a welding wire while supplying a shielding gas, comprising the steps of: The welding wire has a mass of: Mn: more than 1.80 mass% and less than 2.20 mass%; Ti: 0.05% by mass or more and 0.23% by mass or less, Contains Al: more than 0.10% by mass and 0.25% by mass or less, Si: 0.45% by mass or less; The content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, When the content of Ti contained in the welding wire is expressed as [Ti] in mass% with respect to the total mass of the welding wire, The value M1 calculated by the following (Equation 1) is 0.45 or less, A gas-shielded arc welding method, characterized in that a value M2 calculated by the following (Equation 2) is 0.30 or more and 2.50 or less. M1=[Al]+[Ti]...(Formula 1) M2=[Ti] / [Al]...(Formula 2)
7. The shielding gas is Ar and CO 2 7. The gas-shielded arc welding method according to claim 6, further comprising at least one gas selected from the group consisting of:
8. 7. The gas-shielded arc welding method according to claim 6, wherein welding is performed using a feed control method in which the feeding of the welding wire is alternately switched between a forward feed period and a reverse feed period.
9. In the feed control method, A frequency when the forward feed period and the reverse feed period are defined as one cycle is set within a predetermined range, 9. The gas-shielded arc welding method according to claim 8, characterized in that the welding current supplied to the welding wire is switched between a current suppression period and a current non-suppression period based on at least one of information on a phase representing a feed speed of the welding wire and a phase representing a tip position of the welding wire.
10. A method for producing a weld metal, comprising the steps of: welding using a welding wire while supplying a shielding gas to produce a weld metal, The shielding gas is Ar and CO 2 At least one gas selected from The welding wire has a mass of: Mn: more than 1.80 mass% and less than 2.20 mass%; Ti: 0.05% by mass or more and 0.23% by mass or less, Contains Al: more than 0.10% by mass and 0.25% by mass or less, Si: 0.45% by mass or less; The content of Al contained in the welding wire is expressed as [Al] in mass% relative to the total mass of the welding wire, When the content of Ti contained in the welding wire is expressed as [Ti] in mass% with respect to the total mass of the welding wire, The value M1 calculated by the following (Equation 1) is 0.45 or less, A method for producing a weld metal, characterized in that a value M2 calculated by the following (Equation 2) is 0.30 or more and 2.50 or less. M1=[Al]+[Ti]...(Formula 1) M2=[Ti] / [Al]...(Formula 2)
Citation Information
Patent Citations
Solid wire for gas shield arc welding, and method for producing weld joint
JP2021003732A
Wire for gas shield arc welding
JP2021074777A