Base material reinforcement method and composite body

The method for reinforcing base materials with fiber-reinforced composites using specific adhesive parameters addresses the challenge of achieving both peeling resistance and rigidity, resulting in a structure with enhanced stiffness and reduced material usage.

JP2024146362APending Publication Date: 2024-10-15NIPPON STEEL CHEM & MATERIAL CO LTD

Patent Information

Application Number
JP2023059209
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing methods for reinforcing base materials using fiber-reinforced composite materials (FRP) face challenges in achieving both peeling resistance and rigidity, particularly when using adhesives with high elastic modulus, which can lead to stress concentration and reduced stiffness efficiency.

Method used

A method for reinforcing a base material using a metal member with a fiber-reinforced composite material bonded by an adhesive, adhering to specific formulas involving the elastic modulus, thickness, and bonding length to achieve both peeling resistance and rigidity, utilizing a continuous structure rather than a lap joint.

Benefits of technology

The method enables a reinforced structure with both peeling resistance and rigidity, efficiently imparting stiffness while minimizing material usage and weight, thus enhancing the stiffening efficiency and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146362000001_ABST
    Figure 2024146362000001_ABST
Patent Text Reader

Abstract

To provide a base material reinforcement method capable of achieving both of detachment resistance, and rigidity, exhibiting efficiently, application of the rigidity by a reinforcement material, using a metallic component as a base material and adhering the reinforcement material by an adhesive agent, and a composite body acquired by the same.SOLUTION: There is provided a base material reinforcement method satisfying formulae (1),(2): E1, t1 indicate, an elastic modulus and a thickness of the reinforcement material; E2 and 2t2 indicate, an elastic modulus and a thickness of the base material; G and h indicate, a shear elastic modulus and a thickness of the adhesive layer formed of the adhesive agent. l represents the adhesive half-length between the base material and the reinforcing material.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for reinforcing a base material and a composite obtained thereby, and more specifically, although not particularly limited to, a method for reinforcing a base material by which a composite usable in the manufacture of vehicles or the like can be obtained by bonding a reinforcing material to a base material such as a steel material to reduce weight while ensuring rigidity, and a composite obtained by the method in which a reinforcing material is bonded to a base material. [Background technology]

[0002] Not only structures made of wooden building materials, but also those made of steel or concrete, etc., lose their strength over time due to various causes such as corrosion, salt damage, and load, and develop cracks and distortions. In some cases, this can lead to destruction or collapse.

[0003] To prevent these problems, methods of restraining construction materials using high-strength bolts or splices, or repairing by welding can be adopted. In recent years, however, a method of reinforcing by bonding reinforcing materials made of fiber reinforced plastics (FRP) or the like with an adhesive has been attracting attention (see, for example, Patent Documents 1 to 3).

[0004] In the past, existing metal components have been made stronger and thinner to reduce their weight, but thinning can result in insufficient rigidity against bending. In such cases, in order to ensure rigidity, a multi-material design is considered in which reinforcing materials such as FRP are bonded to the metal components, which is also the reason why the above-mentioned reinforcing methods are adopted.

[0005] In the reinforcing method for bonding such reinforcing materials, epoxy resin, which is heat-resistant and has excellent water resistance, is generally used as an adhesive. Since epoxy resin adhesives have high strength and rigidity, they can fully exert the stiffening effect of the reinforcing materials.

[0006] However, when a reinforcing material is bonded with an adhesive with a high elastic modulus (hardness) such as epoxy resin, when force is applied to the composite obtained by bonding the base material with the reinforcing material, stress is concentrated at the bonding edge, making it easy for peeling to occur. In order to prevent such stress concentration, it is possible to use an elastomer-based low-elasticity adhesive for bonding multi-materials, but although low-elasticity adhesives can be expected to prevent stress concentration at the bonding edge, they are soft materials and therefore have a disadvantage in transmitting stress. Therefore, compared to using an adhesive with a high elastic modulus, this may have a negative effect on the stiffness expression of reinforcing materials such as carbon fiber reinforced composite materials (CFRP). In particular, CFRP with a high specific stiffness has high material costs, so it is ideal to be able to efficiently express stiffness. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2006 / 088184 [Patent Document 2] JP 2009-119607 A [Patent Document 3] International Publication No. 99 / 10168 Summary of the Invention [Problem to be solved by the invention]

[0008] Under these circumstances, the present inventors conducted detailed studies on factors that contribute to the peel resistance and rigidity expression between the base material and the reinforcing material. As a result, they found that a reinforcement structure that achieves both peel resistance and rigidity expression can be realized based on parameters determined by the physical properties of each material used and the dimensions of the resulting composite when bonding the reinforcing material to the base material to obtain the composite, and thus completed the present invention.

[0009] Therefore, an object of the present invention is to provide a method for reinforcing a base material in which a metal component is used as the base material and a reinforcing material is bonded with an adhesive, which method achieves both peel resistance and rigidity and efficiently provides the rigidity provided by the reinforcing material.

[0010] Another object of the present invention is to provide a composite material which has both peel resistance and rigidity and in which the rigidity is efficiently expressed by the reinforcing material. [Means for solving the problem]

[0011] That is, the gist of the present invention is as follows. [1] A method for reinforcing a base material in which a metal member is used as a base material and a reinforcing material is bonded to at least one surface of the base material with an adhesive to form a composite material, A method for reinforcing a base material, characterized in that the following formulas (1) and (2) are satisfied.

number

number

[10] The composite described in [7], wherein the base material is a flat plate-shaped base material having a front and back surfaces, and the reinforcing material is bonded to one side of the front or back surface of the plate-shaped base material with an adhesive.

[11] The composite described in [7], wherein the base material is a hollow columnar base material having a box-shaped cross section with a hollow portion, and the reinforcing material is bonded with an adhesive to the inner wall surface or the outer wall surface of the hollow portion on one side of the center line of the cross section of the hollow portion along the longitudinal direction of the hollow columnar base material.

[12] The composite according to [7], wherein the base material is made of steel. Effect of the Invention

[0012] By reinforcing a base material using the reinforcing method of the present invention, a reinforced structure that combines peel resistance and rigidity can be realized. Therefore, the rigidity imparted by the reinforcing material can be efficiently realized, and the stiffening efficiency of the base material can be improved. [Brief description of the drawings]

[0013] [Figure 1]FIG. 1 shows an example of a composite in which a reinforcing material is bonded to a plate-shaped base material by the reinforcing method of the present invention, in which (a) is an explanatory cross-sectional (longitudinal cross-sectional) view showing the longitudinal section, and (b) is an explanatory cross-sectional (transverse cross-sectional) view taken along the cutting line AA. [Diagram 2] FIG. 2 shows the shear stress τ and normal stress σy in relation to the position x at the half-length l of the bond between the base material and the reinforcement when the composite of FIG. 1 is subjected to a tensile load P in its longitudinal direction (x-axis direction). [Diagram 3] FIG. 3 is a schematic explanatory diagram showing the concept of determining the stiffness expression rate ξ. [Figure 4] FIG. 4 is a graph showing the relationship between the material parameter cl and the principal stress σ1 of the composite, and the relationship between the material parameter cl and the stiffness expression rate ξ of the composite. [Diagram 5] FIG. 5 shows an example of a composite in which a reinforcing material is bonded to a hollow columnar base material having a square pipe shape by the reinforcing method of the present invention, where (a) is an explanatory oblique view of the hollow columnar base material, and (b) and (c) are explanatory cross-sectional views of the obtained composite (cross-sections taken along the cutting line BB of the hollow columnar base material). [Figure 6] FIG. 6 shows an example of a composite in which a reinforcing material is bonded to a hollow hat-shaped base material, which is formed by bonding a plate-shaped base material to a hat-shaped base material, using the reinforcing method of the present invention. (a) is an explanatory oblique view of the hollow hat-shaped base material, and (b) and (c) are explanatory cross-sectional views of the obtained composite (cross-sections taken along the cutting line CC of the hollow hat-shaped base material). [Figure 7] FIG. 7 is a schematic diagram for explaining a test complex prepared in an example of the present invention, where (a) is a perspective explanatory view, and (b) is a longitudinal sectional explanatory view. [Figure 8] FIG. 8 is a graph plotting the region defined by the relationship equations (1) and (2) for realizing an ideal reinforcement method according to the present invention and the results of test composites in the examples. [Figure 9] FIG. 9 is a conventional example for explaining the shear lag theory, and is an explanatory cross-sectional (longitudinal cross-sectional) view showing a joint having an adhesive layer formed by bonding two adherends with an adhesive. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described in detail below. The present invention relates to a method for reinforcing a base material, in which a metal member is used as a base material, and a reinforcing material is bonded to at least one surface of the base material with an adhesive to form a composite material, It is characterized in that the following expressions (1) and (2) are satisfied.

number

[0015] In the method for reinforcing a base material according to the present invention, a reinforcement structure that combines peel resistance and rigidity can be realized based on the above formulas (1) and (2). Among these, c in formula (2) is used in a differential equation that appears in the Shear lag theory, and is represented by ω in the following formula, for example.

number

[0016] That is, the shear lag theory is that, for example, in the case of the lap joint shown in Figure 9, when two adherends 31, which are assumed to undergo only elongation deformation, are bonded with an adhesive to form a joint having an adhesive layer 12, if the upper and lower adherends 31 and the adhesive layer 12 are both regarded as elastic bodies and a tensile load P is applied in the x-axis direction of these adherends 31 to pull them against each other, a so-called "shear lag" occurs in which no uniform shear stress occurs in the adhesive layer 12. When this "shear lag" occurs, it is thought that shear stress concentrates at the end of the adhesive layer 12, causing peeling.

[0017] The shear lag theory is a theory that deals with the shear stress distribution when different materials are bonded with an adhesive. Therefore, in the present invention, the thickness and elastic modulus of the adhesive layer consisting of the base material, reinforcing material, and adhesive are used as material parameters, as in c in the above-mentioned formula (2). However, unlike the joint of the adherend as shown in Figure 9, the reinforcement method of the present invention relates to a continuous structure of the base material and reinforcing material, in which the reinforcing material is bonded to the base material to form a composite.

[0018] FIG. 1(a) shows an example of a composite obtained by the method for reinforcing a base material according to the present invention. In this composite, a reinforcing material 3 is bonded to one side of the front or back surface of a flat-shaped base material 1 by an adhesive layer 2 made of an adhesive. FIG. 1(b) shows an enlarged view of the adhesive layer end between the base material 1 and the reinforcing material 3 by the adhesive layer 2. FIG. 2 shows the relationship between the shear stress τ and normal stress σy when the composite of FIG. 1 is subjected to a tensile load P in its longitudinal direction (x-axis direction) and the position x in the adhesive half length l between the base material and the reinforcing material. Based on the shear stress distribution of the shear stress distribution of the shear lag theory described above, the shear stress τ is minimum at the adhesive center O (x=0) in the longitudinal direction of the composite, and the shear stress distribution is symmetrical around this adhesive center, with the highest value at both adhesive ends (x=l). On the other hand, the normal stress σy is distributed symmetrically around the center of the adhesive, and the greater the ratio of the stiffness of the reinforcing material to the stiffness of the base material, the greater the normal stress that occurs.

[0019] Therefore, in the present invention, the stiffness ratio r between the base material and the reinforcing material is expressed by the above formula (3), and it is assumed that cl, which is the product of the material parameter c and the half-length of adhesion l between the base material and the reinforcing material, is sufficiently large. Based on these relationships, peel resistance and stiffness were examined from the physical property values ​​of the materials constituting the composite and the dimensions of the structure. In detail, theoretical calculations were performed based on the composite shown in FIG. 1 for the stress at the end of the adhesive layer and the stiffness of the composite as shown in FIG. 2. The details of the theoretical calculation are as described below, but in this theoretical calculation (parametric study), the parameters listed in Table 1 below were used. Specifically, a steel material with a thickness of 0.8 mm was used as the base material, and a CFRP material with a thickness of 0.8 mm having the same width as the base material was used as the reinforcing material, and the materials were bonded together with an adhesive made of polyurea, and the physical property values ​​of each material were applied. In the table, the reinforcing material is referred to as adherend 1, and the base material is referred to as adherend 2. In addition, the half-length L of the bending span in Table 1 represents the distance from the center O of the adhesive of the composite to the chuck position of the base material (▼ in the figure) when a tensile load P acts in the longitudinal direction of the composite, as shown in Figure 1.

[0020] [Table 1]

[0021] First, regarding the peel resistance of the composite, the theoretical calculation of the adhesive layer stress requires the following six components as the stress at the end of the adhesive layer. In the case of the composite of the present invention, however, when considering tension in the longitudinal direction (X direction), it is sufficient to focus on two components, the shear stress σyx (i.e., τ) and the normal stress σyy (i.e., σy), as the main force components acting on the adhesive layer. The other components do not contribute to peeling and are sufficiently small in value that they can be ignored.

number

[0022] Of these, the former shear stress σyx can be expressed by τ(x) in the following formula (5), and the latter normal stress σyy can be expressed by σ y(x). These formulas were derived by rearranging the force balance and moment balance formulas assuming that the position of shear stress in the composite shown in Figure 1 is the center of the adhesive and that the curvature of the base material and the reinforcement backing plate is constant (Reference 1: Mizutani Takeshi et al., Mechanical Properties of Single-Sided Backing Plate-Bonded Steel Plates Subjected to Uniaxial Tension: Proceedings of the Structural Engineering Journal Vol. 65A (2019) p. 755-768).

number

[0023] Here, x represents the distance from the center of the adhesive bond of the composite, as in the case of Fig. 1. In addition, λ, ω, Z1, and W are as follows. In the above formulas (5) and (6), the adhesive width of the composite (width of the patch plate, expressed as b in the above-mentioned Reference 1) is organized as 1, which is a unit width. This is because, in the composite structure of the present invention, the adhesive width is not extremely small compared to the width of the base material, and therefore it can be assumed that the stress distribution is the same at any cross section in the longitudinal direction in the adhesive range.

number

number

[0024] The stress at the end of the adhesive layer related to the peel resistance of the composite can be calculated based on the following equation (7) by combining these shear stress σyx (i.e., τ) and normal stress σyy (i.e., σy) into the principal stress σ1.

number

[0025] On the other hand, the stiffness of a composite can be evaluated by the stiffness development ratio ξ. As shown in the schematic diagram of Figure 3, the stiffness development ratio ξ is a comparison of the displacement of the adhesive layer end when a tensile load is applied to a composite in which a reinforcement material is bonded to a base material, with the displacement when a perfect composite cross section of the base material and reinforcement material is assumed without the adhesive layer. In other words, a perfect composite cross section is a state (conceptually ideal state) in which all cross sections of a component made of multiple materials are effective against tensile and bending forces, there is no slip deformation between the base material and reinforcement material, and they are completely integrated. The stiffness development ratio ξ is calculated by "stiffness of the composite (i) / stiffness of the composite assuming a perfect composite cross section (ii)".

[0026] Regarding the "composite rigidity (i)" mentioned above, first, the tensile stress generated in the bonded length of the base material can be expressed by the following formula (8).

number

[0027] By dividing this by the elastic modulus (modulus of elasticity) of the base material, the strain at position x of the base material can be calculated. Furthermore, by integrating this strain over the entire bonded range in the length direction, the average strain and elongation over the bonded length of the base material can be calculated. The average strain of the composite has the same meaning as the average strain over the bonded length of the base material, and the apparent elastic modulus (modulus of elasticity) of the composite can be calculated as "tensile force P / cross-sectional area of ​​composite (t1 + t2) / average strain of composite". Multiplying this by the cross-sectional area of ​​the composite gives the "rigidity of the composite (i)".

[0028] In addition, the above "rigidity of the composite when a completely composite cross section is assumed (ii)" can be calculated from "rigidity of the reinforcing material + rigidity of the base material."

[0029] Figure 4 shows a graph of the relationship between cl, one of the material parameters of the composite, and the principal stress σ1 of the composite, and the relationship between the material parameter cl and the stiffness expression rate ξ of the composite. In Figure 4, the filled markers indicate the relationship between cl and the stiffness expression rate ξ. Also, the unfilled markers indicate the relationship between cl and the principal stress σ1. In both cases, the horizontal axis indicates cl, the left vertical axis indicates the value of the stiffness expression rate ξ, and the right vertical axis indicates the principal stress σ1 when a tensile stress of 200 MPa is applied to the steel material. Also, in these graphs, r, which indicates the stiffness ratio between the base material and the reinforcement material, is shown for r=0.33, r=0.66, r=1, and r=1.31.

[0030] In the present invention, since it is desired to increase the rigidity of the composite as much as possible while preventing peeling at the end of the adhesive layer, the conditions for the principal stress σ1, which is an index of peel resistance, and the rigidity expression rate ξ, which is an index of rigidity, are set as follows. That is, regarding the rigidity expression rate ξ, in general, in an adhesive structure, since the rigidity of the adhesive is lower than that of the base material, the rigidity of the reinforcing material is not fully expressed, and it can be said that sufficient rigidity is guaranteed if the rigidity expression rate ξ is 50% or more. In addition, it can be said that the principal stress σ1 satisfies peel resistance if it is 10 or less. Incidentally, when a reinforcing material is bonded with an adhesive with a high elastic modulus (hard) such as epoxy resin, it is generally difficult to achieve a principal stress σ1 of 10 or less.

[0031] According to Fig. 4, the stiffness expression rate ξ does not vary with the material parameter cl, but is determined by the stiffness ratio r between the base material steel and the reinforcing material CFRP. In other words, it can be seen that the stiffness expression rate ξ is 50% or more when r≦0.66, as shown in formula (1) above.

[0032] In addition, the value of the principal stress σ1 increases with an increase in the material parameter cl. As supplemented in Figure 4, when the adhesive is changed to change the adhesive layer shear modulus G, which is one of the parameters that make up cl, σ1 increases in proportion to cl. Incidentally, σ1 does not change much even if other parameters are changed to change the value of cl.

[0033] On the other hand, the relationship between the stiffness ratio r between the base material and the reinforcement and the principal stress σ1 at the end of the adhesive layer is such that the higher the stiffness ratio r, the larger the value of the principal stress σ1. The principal stress σ1 also changes depending on the adhesive layer shear modulus G, and if r=0.66, then σ1 is 10MPa or less when G≦131MPa, and this condition is expressed in terms of cl, which is cl≦4.9. Similarly, if r=0.33, then the condition for σ1 to be 10MPa or less is G≦1800MPa, and this condition is expressed in terms of cl, which is cl≦26.0. In this way, the condition for σ1≦10MPa can be expressed by the relationship between r and cl. The condition for σ1≦10MPa can be expressed by an approximate equation consisting of the stiffness ratio r and the material parameter cl, as shown in the following equation (2).

number

[0034] In other words, assuming that the ideal state in the base material reinforcing method of the present invention is a stiffness expression rate ξ of 50% or more and a principal stress σ1 of 10 or less, and solving the equations in the graphs shown in FIG. 4 (both r and cl are 0 or more), it is necessary to satisfy the conditions of the above-mentioned equations (1) and (2) in order to obtain the above-mentioned ideal state.

[0035] Here, taking into consideration the types of base material and reinforcing material used in the base material reinforcing method of the present invention, as well as their thicknesses, it is practical for the rigidity ratio r to be 0.05 or more. Therefore, in order to more reliably realize an ideal reinforcing method that can increase the rigidity of the composite as much as possible while preventing peeling at the ends of the adhesive layer, it is preferable that r≦0.5 in formula (1) and more preferably 0.1≦r≦0.4. Similarly, it is preferable that cl / (2.5r-1.9 )≦0.95, and more preferably 0.1≦cl / (2.5r -1.9 )≦0.3. The meanings of the symbols in the formula are as described above.

[0036] In the present invention, there are no particular limitations on the base material to be reinforced, and it can be used in any structure that requires reinforcement, and examples of such base materials include steel, aluminum (including aluminum alloy materials, the same applies below), titanium (titanium alloys), magnesium (magnesium alloys), and the like, with steel being particularly preferred.

[0037] Examples of the steel material include iron and iron-based alloys including stainless steel, but iron and iron-based alloys are preferred, and iron and iron-based alloys are more preferred, with steel materials having a higher elastic modulus than other metals. Examples of such steel materials include, for example, cold-rolled steel sheets for general use, drawing or ultra-deep drawing, cold-rolled high-tensile steel sheets for automobiles, hot-rolled steel sheets for general use or processing, hot-rolled steel sheets for automobile structures, and hot-rolled high-tensile steel sheets for automobile structures. Examples of the steel materials include carbon steel, alloy steel, high-tensile steel, etc., used for general structures or machine structures. The components of such steel materials are not particularly limited, but may contain one or more of Si, Mn, S, P, Al, N, Cr, Mo, Ni, Cu, Ca, Mg, Ce, Hf, La, Zr, and Sb in addition to Fe and C. One or more of these additive elements may be appropriately selected in order to obtain the desired material strength and formability, and the content may also be appropriately adjusted.

[0038] The various steel materials as described above preferably have a tensile strength of 590 MPa or more, and more preferably have a tensile strength of 980 MPa or more.

[0039] The steel material may be subjected to any surface treatment. Examples of surface treatment include, but are not limited to, various plating treatments such as zinc plating and aluminum plating, chemical conversion treatments such as chromate treatment and non-chromate treatment, and physical surface roughening treatments such as sandblasting or chemical surface roughening treatments such as chemical etching. In addition, the steel material may be subjected to alloying of plating or a plurality of types of surface treatments. As the surface treatment, it is preferable that at least a treatment for the purpose of imparting rust prevention is performed.

[0040] The type of plating applied to the steel material is not particularly limited, and various known platings such as zinc-based plating can be used. For example, as the plated steel sheet (steel material), hot-dip galvanized steel sheet, alloyed hot-dip galvanized steel sheet, Zn-Al-Mg alloy-plated steel sheet, aluminum-plated steel sheet, electrolytic galvanized steel sheet, electrolytic Zn-Ni alloy-plated steel sheet, etc. can be used.

[0041] In addition, there are no particular limitations on the structures that require reinforcement, and examples of such structures include transportation and transport equipment such as automobiles, trains, ships, and airplanes, as well as general industrial structures such as unmanned aerial vehicles such as drones, industrial robot components in manufacturing factories for liquid crystal displays, bridges for rivers, roads, and railways, as well as buildings such as buildings, houses, and livestock sheds, and constructions such as signs, and various other structures and structures. The thickness of the base material is not particularly limited, but for example, in the case of steel materials that constitute these structures, it is generally within the range of 0.8 to 9 mm.

[0042] The reinforcing material is not particularly limited, and various known materials can be used, such as woven, knitted or nonwoven fabrics using reinforcing fibers such as glass fibers or carbon fibers, unidirectional materials (UD materials) in which fibers are aligned in one direction, impregnated with resin and cured, materials obtained by dispersing short reinforcing fibers in resin, fiber-reinforced composite materials using continuous fibers, etc. Among these, fiber-reinforced composite materials (FRP) in which resins such as epoxy resins or phenolic resins are combined with fibers such as glass fibers or carbon fibers to improve strength are preferable.

[0043] Among these, fiber materials (reinforcing fiber materials) used in FRP include glass fiber, carbon fiber, aramid fiber, basalt fiber, ceramic fiber, etc., but in the present invention, glass fiber and carbon fiber are preferred, and carbon fiber is particularly preferred.

[0044] In addition, it is preferable that the reinforcing material such as FRP is in the form of a plate. In producing the reinforcing material, any of the generally known methods can be used without particular limitation, such as a method of heating and pressurizing laminated FRP molding prepregs (autoclave method, hot press method), a method of injecting liquid resin into a reinforcing fiber substrate placed in a mold and then impregnating and curing the substrate (RTM method), a method of impregnating continuous fibers with resin and drawing the resin into a mold to heat and harden the substrate (pultrusion molding method), and a method of melting a resin material containing short reinforcing fibers and injecting the melted resin material into a mold to mold the substrate (injection molding method).

[0045] In addition, the elastic modulus of the reinforcing material is preferably 20 GPa or more, and more preferably 50 GPa or more, considering that the purpose is to reinforce metal members. The width of the reinforcing material varies depending on the type of reinforcing material, the use of the composite obtained, the purpose of reinforcement, etc., so it is difficult to specify it in general, but generally, the width when viewed in a cross section perpendicular to the longitudinal direction of the composite is about 10 to 300 mm. Similarly, the thickness of the reinforcing material also varies depending on the type and purpose of reinforcement, but for example, when it is made of the above-mentioned fiber-reinforced composite material, it is generally within the range of 1 to 20 mm.

[0046] Furthermore, there are no particular limitations on the resin (matrix resin) that forms the reinforcing material, and it may be a thermosetting resin such as an epoxy resin or a vinyl ester resin, or a thermoplastic resin such as nylon, polyphenylene sulfide (PPS) resin, or a phenoxy resin.

[0047] Furthermore, there is no particular limitation on the adhesive used in the present invention, and a commonly used thermosetting resin or thermoplastic resin can be used. For example, as the thermosetting resin, a room temperature curing type or a thermosetting type epoxy resin, a vinyl ester resin, an MMA resin, an acrylic resin, an unsaturated polyester resin, or a phenolic resin is preferably used, while as the thermoplastic resin, a thermoplastic polyester, a polyolefin, a polyamide, an ethylene vinyl acetate, a phenoxy resin, a polyurea, a polyurethane, a thermoplastic elastomer, or the like can be preferably used. The resin used as the adhesive may be a combination of two or more of the above-mentioned resins, such as a blend or lamination, and may be the same as the resin used in the fiber-reinforced composite material used as the reinforcing material, or different resins may be used.

[0048] The shear modulus G of the adhesive is preferably 10 to 1200 MPa, and more preferably 10 to 400 MPa, taking into consideration the need for a minimum rigidity that can transmit the stress acting on the base material to the reinforcing material, and the need for flexibility to prevent stress concentration by moderate shearing, etc. The thickness of the adhesive layer formed by these adhesives is generally within the range of 0.1 to 5 mm.

[0049] In the method for reinforcing a base material in the present invention, a metal member is used as the base material, and a reinforcing material is bonded to at least one surface of the base material with an adhesive to form a composite. In the case where the base material is a flat plate-shaped base material having a front and back surfaces, an example of such a form of reinforcement is a method in which a reinforcing material is bonded to one of the front or back surfaces of the plate-shaped base material with an adhesive, as shown in Fig. 1 above. Note that any form of adhesive can be used, such as varnish, film, powder, etc., as long as it forms a layer after bonding.

[0050] In addition, when the base material is a hollow columnar base material 11 having a box-shaped cross section with a hollow portion 4 in the shape of a square pipe as shown in Fig. 5(a), a method of adhering a reinforcing material 3 via an adhesive layer 2 to the inner wall surface 11a of the hollow portion on one side of the center line M of the cross section of the hollow portion along the longitudinal direction of the hollow columnar base material 11 as shown in Fig. 5(b) can be used. In addition, as shown in Fig. 5(c), the reinforcing material 3 may be adhered to the outer wall surface 11b of the hollow portion.

[0051] Furthermore, as shown in Fig. 6(a), in the case of a hollow hat-shaped base material 23 having a box-shaped cross section with a hollow portion 4 formed by combining a flat plate material 22 and a hat-shaped material 21, a method of adhering a reinforcing material 3 via an adhesive layer 2 to the inner wall surface 21a of the hollow portion on one side of the center line M of the cross section of the hollow portion along the longitudinal direction of the hollow hat-shaped base material 23 can be used, as shown in Fig. 6(b). Also, as shown in Fig. 6(c), the reinforcing material 3 may be adhered to the outer wall surface 21b of the hollow portion.

[0052] It should be noted that the present invention also covers cases where the width of the reinforcing material does not match the width of the base material, as in the examples of Figures 5 and 6; that is, it also covers reinforcement methods in which the width of the reinforcing material 3 shown in Figure 5(b) does not match the width of the base material 11, and in which the width of the reinforcing material 3 shown in Figure 6(b) does not match the width of the base material 23; in such cases, the present invention applies to the adhesion area where the reinforcing material is adhered to the base material.

[0053] As described above, the method for reinforcing a base material in the present invention can be applied to the reinforcement of transportation equipment such as automobiles, trains, and aircraft, the reinforcement of structural members in general industrial structures such as industrial robots and drones, and the reinforcement of construction structures such as bridges, buildings, and buildings, as well as to the reinforcement of base materials such as light metals such as steel and aluminum used in various structures. It can also be applied to the case where a reinforcing material is bonded to a base material to obtain a composite material while ensuring rigidity and reducing weight. That is, for example, it can be suitably used in the case where a reinforcing material is bonded to a steel material to obtain a composite material that can be used in the manufacture of vehicles such as trains and automobiles, or a composite material that can be used for the arms of industrial robots and structural members of drones.

[0054] In this case, it is sufficient to satisfy the above-mentioned formulas (1) and (2), and the present invention can be effectively used in the selection of materials such as the base material, reinforcing material, and adhesive that forms the adhesive layer, and in the design of forming a composite using these materials, etc. In addition, the present invention can be applied not only to the case of forming a new composite, but also to the case of repairing and reinforcing an existing metal member. EXAMPLES

[0055] In order to verify the effect of the method for reinforcing a base material according to the present invention, the following experimental examples were carried out. However, the present invention is not limited to the contents thereof.

[0056] Example 1 A test composite was prepared using a base material, a reinforcing material, and an adhesive. As shown in FIG. 1, this test composite is a plate-shaped base material 1 having a thickness t2=1.6 mm, a width w=25 mm, and a length 2L=600 mm, and a reinforcing material 3 having a thickness t1=2.4 mm, a width w=25 mm, and a length 2l=300 mm is bonded to the surface (upper surface) of the plate-shaped base material 1 through an adhesive layer 2 having a thickness h=0.2 mm. FIG. 7(a) shows a perspective view of the test composite according to Example 1, and FIG. 7(b) shows a longitudinal cross-sectional view of the test composite. The length 2L of the plate-shaped base material 1 represents the chuck distance excluding the clamping portion (chuck).

[0057] As shown in Table 2, the members forming this test composite were a high-tensile steel plate with an elastic modulus E2 of 206,000 MPa and a yield stress of 299 MPa as the plate-shaped base material 1. As the reinforcement material 3, a PAN-based pseudo-isotropically reinforced CFRP ([(0 / 45 / 90 / -45)s]3) with an elastic modulus E1 of 51,000 MPa and an epoxy resin matrix was used (referred to as PAN-based CFRP-1 in the table). The carbon fiber of this CFRP was a PAN-based carbon fiber (TR50S, manufactured by Mitsubishi Chemical). Furthermore, as the adhesive, a polyurea-based adhesive with a shear modulus G of 20 MPa (polyurea-based adhesive FU-Z, manufactured by Nippon Steel Chemical & Material Co., Ltd.) was used (referred to simply as polyurea-based in Table 2).

[0058] To obtain the test composite, the adhesive surfaces of the plate-shaped base material 1 and the reinforcing material 3 were polished with #120 sandpaper, degreased, and then the reinforcing material 3 was bonded to the surface of the plate-shaped base material 1 with an adhesive, and cured for 7 days at a constant temperature of 20°C to ensure that curing proceeded smoothly. The dimensions, elastic modulus, and shear modulus of the test composite described above are all those after curing. These values ​​are summarized in Table 2 below.

[0059] For the above test composite, the stiffness ratio r between the base material and the reinforcement material was calculated based on the above-mentioned formula (3), and the material parameter cl was calculated based on the formula (4). The test composite was evaluated by the method described below. These are summarized in Table 2. In addition, in FIG. 8, the area consisting of the relational expressions [formulas (1) and (2)] for realizing the above-mentioned ideal reinforcement method is illustrated as surrounded by a dashed line, and the corresponding part of the test composite of this embodiment is plotted. In addition, in the graph of FIG. 8 including the following examples and comparative examples, when the stiffness expression rate is 50% or more and the peeling evaluation is "◎", it is plotted with "●", and when the stiffness expression rate is 50% or more and the peeling evaluation is "○", it is plotted with "○". In addition, when the stiffness expression rate ξ is less than 50% and the peeling evaluation is "◎" or "○", it is plotted with "▲", and when the peeling test is peeling before yield, it is plotted with "×".

[0060] [Evaluation of peeling in the elastic range of steel] A tensile test on the test composite obtained above was performed using a universal testing machine (Instron Model 5985 Universal Testing Machine) under displacement control at a test speed of 2 mm / min, and the evaluation was performed by comparing it with the yield strength of the steel material (299 MPa) in a tensile test of the steel material alone used as the plate-shaped base material 1 performed in the same manner. That is, using the yield strength of the steel material alone as the standard, the case where there was no peeling of the adhesive layer 2 from the test composite was evaluated as "◎", the case where the peel strength of the adhesive layer 2 was higher than the yield strength of the steel material alone was evaluated as "○", and the case where the peel strength of the adhesive layer 2 was lower than the yield strength of the steel material alone was evaluated as "×".

[0061] [Rigidity development rate ξ] As described above, the stiffness expression rate ξ (%) is calculated from "stiffness of the composite (i) / stiffness of the composite when a completely composite cross section is assumed (ii)", and in this embodiment, it was evaluated by FEM analysis (simulation). That is, MSC Software's Marc was used as the analysis software, and a test composite having the same material and shape as the base material, reinforcing material, and adhesive in this embodiment was modeled, and a tensile load was applied in the x-axis direction (longitudinal direction), and (ii) the stiffness of the composite when the base material and reinforcing material are integrated without an adhesive layer (completely composite) and (i) the stiffness of the composite in the test composite in this embodiment were calculated, and the value of (i) was divided by the value of (ii) to calculate the stiffness expression rate ξ (%). It should be noted that a stiffness expression rate ξ of 50% or more was considered to be good.

[0062] (Comparative Examples 1 to 4) Test composites according to Comparative Examples 1 to 4 were obtained in the same manner as in Example 1, except that the reinforcing material and adhesive among the members used were changed to those shown in Table 2, and the thickness h of the adhesive layer was changed as shown in Table 2. Here, the reinforcing material used in Comparative Examples 1 to 4 was a pitch-based pseudo-isotropically reinforced CFRP ([(0 / 45 / 90 / -45)s]3) with an elastic modulus E1 = 137000 MPa with an epoxy resin matrix (referred to as pitch-based CFRP in the table), and the carbon fiber of this CFRP was a pitch-based carbon fiber (XN-80 manufactured by Nippon Graphite Fiber Co., Ltd.). On the other hand, as for the adhesive, the same polyurea-based adhesive as that used in Example 1 was used in Comparative Examples 1 and 2, and a bisphenol A-based epoxy resin adhesive (AW136N / HY994 manufactured by Nagase ChemteX Corporation) with a shear elastic modulus G = 1154 MPa was used in Comparative Examples 3 and 4 (simply referred to as epoxy-based in Table 2).

[0063] [Table 2]

[0064] [Table 3]

[0065] Example 2 As shown in Table 4, the length of the plate-shaped base material 1 was 2L = 160 mm, the bonding length was 2l = 120 mm, and the reinforcing material 3 was changed to the following CFRP, but the same procedure was followed as in Example 1 to produce a test composite. That is, the CFRP was a PAN-based unidirectional reinforced CFRP with an elastic modulus E1 = 135,000 MPa and an epoxy resin matrix, and the carbon fiber of this CFRP was a PAN-based carbon fiber (TR50S manufactured by Mitsubishi Chemical Corporation) (referred to as PAN-based CFRP-2 in the table). The reinforcing material had a thickness t1 = 0.8 mm, a width w = 25 mm, and a length 2l = 120 mm.

[0066] (Examples 3 to 5) Test composites according to Examples 3 to 5 were obtained in the same manner as in Example 2, except that the adhesive and adhesive thickness of the members used were changed to those shown in Table 4.

[0067] [Table 4]

[0068] The obtained test complex was evaluated in the same manner as in Example 1. The results are shown in Table 3 and Figure 8. In addition, in the plot of Figure 8, the position of the test complex corresponding to each Example and Comparative Example is plotted, and the method of plotting at that time is as described above.

[0069] As can be seen from the above results, the test composites according to Comparative Examples 1 to 4 either showed peeling in the previous peeling evaluation or had a stiffness expression rate ξ that did not reach 50%, and these test composites were outside the region defined by formulas (1) and (2) of the present invention, as shown in Fig. 8. In contrast, the test composites according to Examples 1 to 5 did not show peeling in the deformation region up to the yielding of the steel material in the peeling evaluation, and also showed stiffness expression rates ξ of 50% or more (specifically, 60% or more), and all of these were included in the region defined by formulas (1) and (2) of the present invention.

[0070] Therefore, according to the present invention, a reinforced structure that has both peel resistance and rigidity can be realized. Moreover, the amount of material used for reinforcement can be reduced to a minimum while increasing the stiffening efficiency, which is advantageous in terms of cost and workability, and the weight of the resulting composite can be reduced. [Explanation of symbols]

[0071] 1: base material, 2: adhesive layer, 3: reinforcing material, 4: hollow portion, 11: base material, 21: hat-shaped material, 22: flat plate material, 23: hollow hat-shaped base material, 31: adherend.

Claims

1. A method for reinforcing a base material, comprising the steps of: bonding a reinforcing material to at least one surface of a base material made of a metal member with an adhesive to form a composite material, the method comprising the steps of: A method for reinforcing a base material, characterized in that the following formulas (1) and (2) are satisfied. [0010] E 1 and 1 represents the elastic modulus and thickness of the reinforcement material. E 2 and 2t 2 represents the elastic modulus and thickness of the base material. G and h represent the shear modulus and thickness of the adhesive layer made of the adhesive. l represents the half-length of adhesion between the base material and the reinforcing material.

2. The method for reinforcing a base material according to claim 1 , wherein the reinforcing material has an elastic modulus of 20 GPa or more.

3. 2. The method for reinforcing a base material according to claim 1, wherein the reinforcing material is made of a fiber-reinforced composite material using continuous fibers.

4. 2. The method for reinforcing a base material according to claim 1, wherein the base material is a flat plate-shaped base material having a front and back surface, and the reinforcing material is bonded to one of the front surface or the back surface of the plate-shaped base material with an adhesive.

5. 2. The method for reinforcing a base material as described in claim 1, wherein the base material is a hollow columnar base material having a box-shaped cross section with a hollow portion, and the reinforcing material is adhered with an adhesive to the inner wall surface or the outer wall surface of the hollow portion on one side of the center line of the cross section of the hollow portion along the longitudinal direction of the hollow columnar base material.

6. The method for reinforcing a base material according to claim 1 , wherein the base material is made of steel.

7. A composite body having a metal member as a base material and a reinforcing material bonded to at least one surface of the base material with an adhesive, A composite comprising a base material and a reinforcing material bonded to the base material, the composite satisfying the following formulas (1) and (2): [0025] E 1 and 1 represents the elastic modulus and thickness of the reinforcement material. E 2 and 2t 2 represents the elastic modulus and thickness of the base material. G and h represent the shear modulus and thickness of the adhesive layer made of the adhesive. l represents the half-length of adhesion between the base material and the reinforcing material.

8. 8. The composite of claim 7, wherein the reinforcing material has an elastic modulus of 20 GPa or greater.

9. 8. The composite of claim 7, wherein the reinforcing material comprises a fiber-reinforced composite material using continuous fibers.

10. 8. The composite according to claim 7, wherein the base material is a flat plate-shaped base material having a front and back surface, and the reinforcing material is bonded to one side of the front surface or the back surface of the plate-shaped base material with an adhesive.

11. 8. The composite according to claim 7, wherein the base material is a hollow columnar base material having a box-shaped cross section with a hollow portion, and the reinforcing material is bonded with an adhesive to the inner wall surface or the outer wall surface of the hollow portion on one side of the center line of the cross section of the hollow portion along the longitudinal direction of the hollow columnar base material.

12. 8. The composite of claim 7, wherein said matrix comprises steel.

Citation Information

Patent Citations

  • Method for manufacturing stiffening insert and stiffening insert manufactured by the method

    JP2009119607A

  • Light metal / CFRP structural member

    WO1999010168A1

  • Reinforcement for building structure, reinforced building structure, and method of reinforcing building structure

    WO2006088184A1

Cited By

  • Reinforcing structure for building structure

    JP2025088357A

  • Reinforcement structures for building structures

    JP7785369B2