Substrate layer-adding processing method and packaging structure

By setting limit columns on the substrate and grinding and thinning using high-hardness materials and specific grinding wheels, the problem of inaccurate dielectric layer thickness control in substrate layering technology is solved, and accurate control of dielectric layer thickness and product stability are achieved. .

CN114864415BActive Publication Date: 2024-11-08WUXI ZHONGWEI GAOKE ELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210579626.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-26
Publication Date
2024-11-08
Estimated Expiration
2042-05-26

AI Technical Summary

Technical Problem

In the existing substrate layering technology, it is difficult to accurately control the thickness of the dielectric layer after hot pressing and coating, resulting in structural thickness deviations and affecting the connection between layers.

Method used

The carrier plate is equipped with metal through holes and double-sided copper columns. The first coating film covering the double-sided copper columns is formed by hot pressing the film, and a limit column is made on it. The mechanical properties parameters of the selected material are satisfied. The hardness of the 19th century is greater than 3.0, the Young's modulus is higher than 110 GPa and the shear elastic modulus is greater than 49 GPa. The grinding wheels made of specific adhesives and diamonds are ground and thinned until the limit column height is used to control the thickness of the dielectric layer.

Benefits of technology

It effectively reduces the feed speed of the thinning grinding wheel, ensures that the thickness of the dielectric layer conforms to the theoretical thickness, and improves the stability and performance of the structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114864415B_ABST
    Figure CN114864415B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of semiconductor processing technology, and specifically discloses a substrate layer-adding processing method, which includes: providing a carrier; performing hot-pressing coating on one surface of the carrier to form a first coating film covering double-sided copper pillars; performing thinning treatment on the first coating film to expose the double-sided copper pillars; forming a double-sided redistribution layer on the surface of the first coating film away from the carrier; making a plurality of spaced-apart limiting pillars on the double-sided redistribution layer, wherein the mechanical property parameters of the material for making the limiting pillars meet the following conditions: Mohs hardness greater than 3.0, Young's modulus greater than 110GPa, and shear elastic modulus greater than 49GPa; performing opening electroplating on the surface of the double-sided redistribution layer, and making a dielectric layer; performing hot-pressing coating on the surface of the double-sided redistribution layer to form a second coating film covering the dielectric layer and the limiting pillars. The present invention also discloses a packaging structure. The substrate layer-adding processing method provided by the present invention can effectively control the thinning thickness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor processing technology, and in particular to a substrate layer-adding processing method and a packaging structure. Background Art

[0002] FC-BGA (Flip Chip-Ball Grid Array, the packaging format of flip chip ball grid array) substrate layer technology is to use drilling, plating and filling technology to conduct between layers on the coating film, and prepare a single circuit layer on it to achieve circuit connection. At the same time, the circuit layer can also be made and then hot-pressed to fill the entire circuit layer. However, this is done on the premise that the thickness of the dielectric material filled between the metal layers meets the theoretical thickness. At present, the coating thickness is larger than the theoretical dielectric layer thickness, and after the metal layer is hot-pressed, a thinner coating layer will remain on the metal surface, affecting the connection between layers. Therefore, the thinning process after hot-pressing the coating is indispensable, but the problem that follows is that the thickness of the dielectric layer cannot be effectively controlled during the mechanical thinning process, and the thinning amount will be small, or even too much, resulting in a deviation between the overall structure and the theoretical thickness. Therefore, it is necessary to improve the accuracy of the thinning amount to control the overall structure of the plate with a large number of layers. Summary of the invention

[0003] The present invention provides a substrate layer adding processing method and a packaging structure, which solves the problem in the related art that the thinning amount cannot be accurately controlled.

[0004] As a first aspect of the present invention, a substrate layer adding processing method is provided, which comprises:

[0005] Providing a carrier board, wherein the carrier board is provided with metal through holes and double-sided copper pillars;

[0006] Performing hot-pressed coating on one surface of the carrier to form a first coating film covering the double-sided copper column;

[0007] Performing a thinning process on the first coating film to expose the double-sided copper pillar;

[0008] forming a double-sided redistribution layer on a surface of the first coating film facing away from the carrier;

[0009] Opening electroplating is performed on the double-sided redistribution layer, and a plurality of spaced limiting posts are manufactured, wherein the plurality of spaced limiting posts are on the double-sided redistribution layer and are distributed in a ring shape along the periphery, the height of the limiting posts is greater than the preset height of the dielectric layer to be manufactured, and the difference between the height of the limiting posts and the preset height of the dielectric layer is within a preset range, and the mechanical property parameters of the manufacturing material of the limiting posts meet the following conditions: Mohs hardness greater than 3.0, Young's modulus greater than 110 GPa, and shear elastic modulus greater than 49 GPa;

[0010] Performing opening electroplating on the surface of the double-sided redistribution layer and manufacturing a dielectric layer, wherein the actual height of the dielectric layer is greater than the preset height of the dielectric layer, and the difference between the actual height of the dielectric layer and the preset height of the dielectric layer is within a preset range;

[0011] Performing hot-pressing coating on the surface of the double-sided redistribution layer to form a second coating film covering the dielectric layer and the limiting pillars, wherein the thickness of the second coating film is greater than the height of the dielectric layer and the height of the limiting pillars;

[0012] The second coating film is ground and thinned at a preset grinding feed speed until it is ground to the height of the limiting pillar, and then the preset grinding feed speed is passively reduced until the grinding is stopped to obtain a dielectric layer of the preset height.

[0013] Furthermore, the shape of the limiting column includes a cylindrical shape.

[0014] Furthermore, the diameter of the limiting column is between 300 μm and 500 μm.

[0015] Furthermore, the limiting pillar is made of a material including any one of Ni, Cr and Mo or a combination of multiple thereof.

[0016] Furthermore, the height of the double-sided redistribution layer is between 40 μm and 100 μm.

[0017] Furthermore, the thickness of the carrier plate is between 400 μm and 800 μm.

[0018] Furthermore, the second coating film is ground and thinned by a grinding wheel according to a preset grinding feed speed until it is ground to the height of the limit column, and the preset grinding feed speed is passively reduced until the grinding is stopped to obtain a medium layer of the preset height, wherein the grinding wheel includes a grinding wheel with a mesh size between 500 and 800 and a concentration between 75 and 125.

[0019] As another aspect of the present invention, a packaging structure is provided, wherein the packaging structure is manufactured by the substrate layer-building processing method described above.

[0020] The substrate layer adding processing method provided by the present invention forms a limiting column, and the mechanical properties of the limiting column selected from the material meet the requirements of Mohs hardness greater than 3.0, Young's modulus greater than 110GPa, and shear elastic modulus greater than 49GPa. When the coating film is thinned, the hardness of the limiting column is high, so the feed speed of the thinning grinding wheel can be reduced, thereby effectively controlling the thinning thickness. In addition, by thinning the coating film, a grinding wheel made of a specific adhesive and diamond is used to grind the coating layer, which can ensure that the grinding wheel has differences in grinding the copper column and the limiting column. When grinding to the height of the limiting column, the grinding wheel feed speed is greatly reduced, thereby ensuring that the thickness of the dielectric layer meets the theoretical thickness, and ensuring the stability and performance of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0022] Figure 1 The present invention provides a flow chart of the substrate layer adding method.

[0023] Figure 2 This is a schematic diagram of the carrier structure provided by the present invention.

[0024] Figure 3 This is a schematic diagram of the structure of the carrier provided by the present invention after hot pressing, coating and grinding.

[0025] Figure 4 This is a schematic diagram of the structure after a double-sided redistribution layer is performed on the coating film provided by the present invention.

[0026] Figure 5 A schematic diagram of the structure of preparing limit posts on the double-sided redistribution layer provided by the present invention.

[0027] Figure 6 The present invention provides a schematic structural diagram of a dielectric layer prepared on a double-sided redistribution layer.

[0028] Figure 7 This is a schematic diagram of the structure after the double-sided redistribution layer provided by the present invention is heat-pressed and coated.

[0029] Figure 8 This is a schematic diagram of the structure of the coating film after grinding provided by the present invention.

[0030] Fig. 9 A schematic top view of the distribution of the limiting posts provided by the present invention on the carrier plate. DETAILED DESCRIPTION

[0031] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0032] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work should fall within the scope of protection of the present invention.

[0033] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so as to describe the embodiments of the present invention described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0034] In this embodiment, a substrate layer adding processing method is provided. Figure 1 is a flow chart of a substrate layer adding method provided according to an embodiment of the present invention. Figure 1 As shown, including:

[0035] S110, providing a carrier board, wherein the carrier board is provided with metal through holes and double-sided copper pillars;

[0036] It should be understood that after the carrier 101 is produced and processed, multiple metallized through holes are filled therein, and double-sided copper pillars of a certain height grow on the surface of the through holes, as shown in the specific schematic diagram. Figure 2 shown.

[0037] like Figure 2 , which is a schematic diagram of a carrier 101. It should be understood that the carrier 101 is provided with a metal through hole 103 and a double-sided copper column (Bump) 102, and the double-sided copper column 102 is provided here so as to achieve double-sided growth.

[0038] In the embodiment of the present invention, the thickness of the carrier 101 is between 400 μm and 800 μm.

[0039] S120, performing hot-pressing coating on one surface of the carrier to form a first coating film covering the double-sided copper column;

[0040] like Figure 3 As shown, Figure 3 Taking the direction shown as an example, a hot-pressed coating film is applied on the upper surface of the carrier 101 to the double-sided copper pillars covering the surface, thereby forming a first coating film 104 covering the double-sided copper pillars.

[0041] S130, performing a thinning process on the first coating film to expose the double-sided copper pillar;

[0042] The first coating film 104 is thinned. Specifically, the thickness of the thinning can be determined according to the height of the double-sided copper pillar 102, that is, the thinning is performed until the double-sided copper pillar 102 is exposed. The specific operation is well known to those skilled in the art and will not be described in detail here.

[0043] S140, forming a double-sided redistribution layer on the surface of the first coating film facing away from the carrier board;

[0044] like Figure 4 As shown, taking the direction shown in the figure as an example, a double-sided redistribution layer 105 is formed on the upper surface of the first coating film 104, and the double-sided redistribution layer 105 is opened and electroplated with a copper layer of a specific height.

[0045] In the embodiment of the present invention, the height of the double-sided redistribution layer 105 is between 40 μm and 100 μm.

[0046] S150 is required, opening electroplating is performed on the double-sided redistribution layer 105, and a plurality of spaced-apart limiting posts 106 are manufactured, wherein the plurality of spaced-apart limiting posts 106 are on the double-sided redistribution layer 105 and are distributed in a ring shape along the periphery, the height of the limiting posts 106 is greater than the preset height of the dielectric layer 107 to be manufactured, and the difference between the height of the limiting posts 106 and the preset height of the dielectric layer 107 is within a preset range, and the mechanical property parameters of the manufacturing material of the limiting posts 106 meet the following conditions: Mohs hardness is greater than 3.0, Young's modulus is higher than 110 GPa, and shear elastic modulus is greater than 49 GPa;

[0047] It should be understood that if Figure 5 As shown, taking the direction shown in the figure as an example, opening electroplating is performed on the double-sided redistribution layer 105 to prepare limiting columns 106 of hard materials with high Young's modulus such as Ni. The height of the limiting columns 106 is slightly higher than the preset height of the dielectric layer 107 by 5μm. Specifically, it can be understood that the difference between the height of the limiting columns 106 and the preset height of the dielectric layer 107 is about 5μm, that is, the preset range can be ±5μm.

[0048] like Fig. 9 As shown, it is a top view of the layout of the limit posts 106 on the double-sided redistribution layer 105. It can be seen from the figure that the limit posts 106 are arranged along the periphery of the wafer, and the dielectric layer 107 is surrounded by the limit posts 106 on the periphery. When the grinding wheel 109 thins the limit posts 106, since the hardness and other mechanical properties of the material making the limit posts 106 are higher than those of copper, the resistance formed is relatively large, thereby effectively reducing the thinning speed of the grinding wheel, that is, reducing the feed speed of the grinding wheel, achieving effective control of the thinning thickness, and obtaining a dielectric layer thickness that meets the requirements.

[0049] In the embodiment of the present invention, the shape of the limiting pillar 106 is not limited in the embodiment of the present invention, and a cylindrical shape with a regular shape and easy processing is preferably selected. Specifically, the diameter of the limiting pillar 106 is between 300 μm and 500 μm.

[0050] In the embodiment of the present invention, the material of the limiting column 106 can be selected from metal materials such as Ni, which has a higher Young's modulus than copper and is easy to electroplate, or alloys. Specifically, the material of the limiting column includes any one of Ni, Cr and Mo or a combination of multiple thereof.

[0051] It should be understood that the materials used to make the limit column include materials with high mechanical properties such as Mohs hardness greater than 3.0, Young's modulus greater than 110 GPa, and shear elastic modulus greater than 49 GPa, such as Ni, Cr, Mo and their alloys and other metal materials.

[0052] S160, performing opening electroplating on the surface of the double-sided redistribution layer, and manufacturing a dielectric layer 107, wherein the actual height of the dielectric layer is greater than the preset height of the dielectric layer, and the difference between the actual height of the dielectric layer and the preset height of the dielectric layer is within a preset range;

[0053] In the embodiment of the present invention, Figure 6 As shown, the dielectric layer 107 is prepared by opening electroplating on the upper surface of the double-sided redistribution layer 105 , wherein the actual height of the prepared dielectric layer 107 is higher than the preset height of the dielectric layer 107 .

[0054] S170, performing hot-pressing coating on the surface of the double-sided redistribution layer 105 to form a second coating film 108 covering the dielectric layer 107 and the limiting pillars 106, wherein the thickness of the second coating film 108 is greater than the height of the dielectric layer 107 and the height of the limiting pillars 106;

[0055] It should be understood that if Figure 7As shown, hot pressing and coating is performed on the surface of the double-sided redistribution layer 105 to form a second coating film 108 , wherein the second coating film 108 can completely cover the dielectric layer 107 and the limiting pillars 106 .

[0056] S180, grinding and thinning the second coating film at a preset grinding feed speed until it is ground to the height of the limiting pillar, and then the preset grinding feed speed is passively reduced until the grinding is stopped to obtain a dielectric layer of the preset height.

[0057] In the embodiment of the present invention, Figure 8 As shown, the second coating film is ground and thinned by a grinding wheel according to a preset grinding feed speed until it is ground to the height of the limiting column, and the preset grinding feed speed is passively reduced until the grinding is stopped to obtain a medium layer of the preset height, wherein the grinding wheel includes a grinding wheel with a mesh size between 500 and 800 and a concentration between 75 and 125.

[0058] It should be understood that when the grinding wheel is ground and thinned to the height of the limiting column according to the preset grinding feed speed, the preset grinding feed speed of the grinding wheel will gradually passively reduce the grinding feed speed due to the increased resistance, that is, the grinding wheel will be worn out due to the increased resistance until the grinding feed speed is reduced to 0, and the time to reduce to 0 here is related to the mutual resistance between the grinding wheel and the material. For example, the preset grinding feed speed is 0.1μm / s, then before grinding to the height of the limiting column, due to the influence of the hardness of the material, the grinding wheel will suffer certain losses, and the actual grinding feed speed will be slightly less than 0.1, and after reaching the height of the limiting column, due to the higher hardness of the material thereafter, the grinding wheel will suffer greater losses, and the grinding feed speed will be further reduced until it drops to 0, and then the grinding will stop.

[0059] It should be noted that the grinding wheel can be specifically made of a specific adhesive and an appropriate amount of diamond. The second coating film is ground and thinned by the grinding wheel. After grinding to the height of the limiting column 106, the feed speed of the grinding wheel is reduced and the thinning is stopped, thereby obtaining a dielectric layer 107 that meets the preset height.

[0060] It should also be noted that the type of binder used to prepare the grinding wheel should be suitable for grinding copper pillars with small diameters and coatings, but has little effect on thinning hard metals.

[0061] In the embodiment of the present invention, the binder mainly includes resin binder, ceramic binder and metal binder. The selection of suitable resin binder is beneficial to the grinding of copper columns with small diameters and coating films, but has no obvious effect on the thinning of hard metals. In addition, the particle size and quantity of diamonds selected in the grinding wheel must also meet such requirements to achieve suitable effects.

[0062] It should be understood that Figure 4 To prepare a double-sided redistribution layer on the coating film, a metal material with a high Young's modulus is then electroplated on the double-sided redistribution layer. The number is 16 or more, distributed around the 12-inch or 8-inch Core material, such as Figure 8 As shown, the double-sided redistribution layer is then electroplated with a bump to ensure the connection between the layers. The coating film is then hot-pressed to fill the pores in the metal layer and insulate the metal layer to protect the circuit. Figure 7 A special grinding wheel is used for thinning. During the thinning process, the grinding wheel feed speed is slowed down and the thinning is stopped to reduce the copper to the target thickness.

[0063] In summary, the substrate layer-adding processing method provided by the embodiment of the present invention forms a limiting column, and the mechanical properties of the limiting column selected from the material satisfy the Mohs hardness greater than 3.0, the Young's modulus greater than 110GPa, and the shear elastic modulus greater than 49GPa. When the coating film is thinned, due to the high hardness of the limiting column, the feed speed of the thinning grinding wheel can be reduced, thereby effectively controlling the thinning thickness. In addition, by thinning the coating film and using a grinding wheel made of a specific adhesive and diamond to grind the coating layer, it can be ensured that the grinding wheel has differences in grinding the copper column and the limiting column. When grinding to the height of the limiting column, the grinding wheel feed speed is greatly reduced, thereby ensuring that the thickness of the dielectric layer meets the theoretical thickness and ensuring the stability and performance of the product.

[0064] As another embodiment of the present invention, a packaging structure is provided, which is manufactured by using the substrate layer-adding processing method described above. The specific schematic diagram of the packaging structure can be as follows: Figure 8 shown.

[0065] The specific detailed structure of the packaging structure of the embodiment of the present invention can refer to the description of the substrate layer-building processing method mentioned above, which will not be repeated here.

[0066] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A substrate layer-adding processing method, characterized in that: include: Providing a carrier board, wherein the carrier board is provided with metal through holes and double-sided copper pillars; Performing hot-pressed coating on one surface of the carrier to form a first coating film covering the double-sided copper column; Performing a thinning process on the first coating film to expose the double-sided copper pillar; forming a double-sided redistribution layer on a surface of the first coating film facing away from the carrier; Opening electroplating is performed on the double-sided redistribution layer, and a plurality of spaced limiting posts are manufactured, wherein the plurality of spaced limiting posts are on the double-sided redistribution layer and are distributed in a ring shape along the periphery, the height of the limiting posts is greater than the preset height of the dielectric layer to be manufactured, and the difference between the height of the limiting posts and the preset height of the dielectric layer is within a preset range, and the mechanical property parameters of the manufacturing material of the limiting posts meet the following conditions: Mohs hardness greater than 3.0, Young's modulus greater than 110 GPa, and shear elastic modulus greater than 49 GPa; Performing opening electroplating on the surface of the double-sided redistribution layer and manufacturing a dielectric layer, wherein the actual height of the dielectric layer is greater than the preset height of the dielectric layer, and the difference between the actual height of the dielectric layer and the preset height of the dielectric layer is within a preset range; Performing hot-pressing coating on the surface of the double-sided redistribution layer to form a second coating film covering the dielectric layer and the limiting pillars, wherein the thickness of the second coating film is greater than the height of the dielectric layer and the height of the limiting pillars; The second coating film is ground and thinned at a preset grinding feed speed until it is ground to the height of the limiting pillar, and then the preset grinding feed speed is passively reduced until the grinding is stopped to obtain a dielectric layer of the preset height.

2. The method according to claim 1, characterized in that The shape of the limiting column includes a cylindrical shape.

3. The method according to claim 1, characterized in that The diameter of the limiting column is between 300 μm and 500 μm.

4. The method according to claim 1, characterized in that: The limiting pillar is made of a material including any one of Ni, Cr and Mo or a combination of multiple thereof.

5. The method according to claim 1, characterized in that The height of the double-sided redistribution layer is between 40 μm and 100 μm.

6. The method according to claim 1, characterized in that The thickness of the carrier plate is between 400 μm and 800 μm.

7. The method according to any one of claims 1 to 6, characterized in that: The second coating film is ground and thinned by a grinding wheel at a preset grinding feed speed until it is ground to the height of the limiting column, and the preset grinding feed speed is passively reduced until the grinding is stopped to obtain a medium layer of the preset height, wherein the grinding wheel includes a grinding wheel with a mesh size between 500 and 800 and a concentration between 75 and 125.

8. A packaging structure, characterized in that: The method is manufactured by the substrate layer adding method described in any one of claims 1 to 7.