Cation exchange laminate and ion exchange cartridge for electrodialysis
The cation exchange laminate with a thermoplastic resin fiber support and controlled adhesive area addresses membrane deformation and leakage issues, ensuring high cation exchange performance and durability in electrodialysis processes.
Patent Information
- Application Number
- JP2023059236
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Commercially available ion exchange membranes and integrated ion exchange membranes with nonwoven fabrics suffer from membrane deformation and water leakage, leading to reduced ion exchange capacity and inefficiency in electrodialysis processes.
A cation exchange laminate comprising a cation exchange membrane and a support made of thermoplastic resin fibers, with an adhesive area between 2% to 30% of the total area, and an adhesive strength of 2N/4.5 mm to 20N/4.5 mm, ensuring effective bonding and preventing water leakage.
The laminate effectively suppresses membrane deformation and water leakage, maintaining high cation exchange performance and durability, enhancing ion exchange capacity and efficiency in electrodialysis applications.
Smart Images

Figure 2024146378000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to cation exchange laminates and ion exchange cartridges for electrodialysis. [Background technology]
[0002] Generally, ion exchange resins are used for ion exchange. However, the ion exchange capacity of these resins decreases over time. Therefore, from the viewpoint of stability over time, ion exchange membranes that only allow liquid to pass through have attracted attention and are now used.
[0003] Patent Document 1 discloses an ion exchange membrane which is a self-supporting membrane including an anion conductive polymer membrane and a cation conductive polymer membrane and has excellent low membrane resistance, and describes that the ion exchange membrane is used by laminating it with a porous substrate, for example. A nonwoven fabric is used as the porous substrate, and the ion exchange membrane and the nonwoven fabric are sometimes integrated together for use. In addition, as an ion exchange membrane, an ion exchange membrane containing sodium sulfonate styrene-divinylbenzene copolymer impregnated and polymerized into a polyvinyl chloride nonwoven fabric is commercially available. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2021-123648 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, as a result of the inventor's investigation, it was found that in commercially available ion exchange membranes or the ion exchange membrane integrated with the nonwoven fabric described in Patent Document 1, the membrane may be deformed depending on the type of reinforcing nonwoven fabric, and water leakage occurs from the laminate of the porous substrate and the ion exchange membrane. When water leakage occurs, the treatment liquid passes through without passing through the cation exchange membrane, and the ion exchange capacity does not exhibit the expected performance, and it became clear that there is room for improvement.
[0006] An object of the present disclosure is to provide a cation exchange laminate having good cation exchange capacity in which deformation of the membrane and water leakage during use are suppressed, and an ion exchange cartridge for electrodialysis using the cation exchange laminate. [Means for solving the problem]
[0007] Means for solving the above problems include the following embodiments.
[0008] <1> A cation exchange laminate comprising a laminate of a cation exchange membrane and a support including a nonwoven fabric made of thermoplastic resin fibers, the laminate having an ion exchange section consisting of a laminate of the cation exchange membrane and the support, and an adhesive section at the periphery of the ion exchange section where the cation exchange membrane and the support are adhered, and the proportion of the area of the adhesive section to the total area of the laminate in a planar view is 2% or more and less than 30%.
[0009] <2> The average adhesive strength between the cation exchange membrane and the support at the adhesive portion is 2 N / 4.5 mm to 20 N / 4.5 mm. <1> The cation exchange laminate according to claim 1. <3> The adhesive part is an adhesive part in which the cation exchange membrane and the support are laminated with an adhesive, or is a heat-sealed part between the cation exchange membrane and the support. <1> or <2> The cation exchange laminate according to claim 1. <4> The thickness of the cation exchange membrane is 0.01 μm to 5.0 μm. <1> ~ <3> 13. A cation exchange laminate according to claim 12.
[0010] <5> the cation exchange membrane comprises one or more kinds of repeating structural units (A) selected from repeating structural units having an anionic structural group (a2) and a main chain end containing a group containing a Group 16 atom of the periodic table, and a repeating structural unit (B) not having the anionic structural group (a2) and a main chain end containing a group containing a Group 16 atom of the periodic table, the polymer (P) having a content of the anionic structural group (a2) of 5 mol % to 90 mol % relative to the total mass of the cation exchange membrane when the total of the structural units (A) and (B) is taken as 100 mol %, <1> ~ <4> 13. A cation exchange laminate according to claim 12. <6> The polymer (P) is an aromatic polyether resin containing a structural group (I) represented by the following formula (1) and a structural group (2) represented by the following formula (2): <5> The cation exchange laminate according to claim 1.
[0011] [ka]
[0012] [In formula (1) and formula (2), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , and R 10 are each independently H, Cl, F, CF3, or C m H2 m+1 (m is an integer from 1 to 10), and R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 and R 10 At least one of the following is C m H2 m+1(m is an integer from 1 to 10), and R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 and R 10 may be present in two or more aromatic rings, and C m H2 m+1 If there are two or more C m H2 m+1 may be the same or different. X 1 , X 2 , X 3 , X 4 , and X 5 each independently represents H, Cl, F, CF3, a protonic acid group, or a protonic acid salt; X 1 , X 2 , X 3 , X 4 , and X 5 At least one of A represents a protonic acid group or a protonic acid salt. 1 , A 2 , A 3 , A 4 , A 5 , and A 6 each independently represents a single bond, -CH2-, -C(CH3)2-, -C(CF3)2-, -O-, or -CO-; i, j, k, and l each independently represent 0 or 1.
[0013] <7> <1> ~ <6> 13. An ion exchange cartridge for electrodialysis, comprising the cation exchange laminate according to any one of claims 1 to 12 and a support arranged alternately. Effect of the Invention
[0014] According to the present disclosure, there are provided a cation exchange laminate having good cation exchange capacity in which deformation of the membrane and water leakage during use are suppressed, and an ion exchange cartridge for electrodialysis using the cation exchange laminate. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1(A) is a plan view showing an example of a cation exchange laminate having a rectangular shape when viewed from above, and FIG. 1(B) is a plan view showing an example of a cation exchange laminate having a circular shape when viewed from above. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of an ion exchange cartridge incorporating a cation exchange laminate of the present disclosure. [Diagram 3] FIG. 3 is a schematic diagram showing an example of a cation exchange laminate of the present disclosure incorporated into the ion exchange cartridge shown in FIG. 2, and an enlarged schematic cross-sectional view thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present disclosure will now be described in detail with reference to examples of preferred embodiments. These descriptions and examples are merely illustrative of the embodiments and are not intended to limit the scope of the embodiments. In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless otherwise specified, or are considered to be obviously essential in principle, etc. The same applies to the numerical values and their ranges, and they do not limit the present invention. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples. In this specification, the amount of each component in a composition means, when a plurality of substances corresponding to each component are present in the composition, the total amount of the plurality of substances present in the composition, unless otherwise specified. In the present disclosure, "mass%" and "weight%" have the same meaning. In the present disclosure, "%" indicating the amount of a component is based on mass unless otherwise specified. In this specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. In the description of a group (atomic group) in this specification, a description that does not indicate whether it is substituted or unsubstituted includes both a group having no substituent and a group having a substituent. In this disclosure, the term "layer" includes cases where the layer is formed over the entire area when the area in which the layer exists is observed, as well as cases where the layer is formed over only a portion of the area.
[0017] <<Cation exchange laminate>> The cation exchange laminate of the present disclosure (hereinafter also simply referred to as "the laminate of the present disclosure") comprises a laminate of a cation exchange membrane and a support including a nonwoven fabric made of thermoplastic resin fibers, and the laminate has an ion exchange section consisting of a laminate of the cation exchange membrane and the support, and an adhesive section at the periphery of the ion exchange section where the cation exchange membrane and the support are adhered, and the proportion of the area of the adhesive section to the total area of the laminate in a planar view is 2% or more and less than 30%. Hereinafter, one embodiment of the cation exchange laminate of the present disclosure will be described with reference to the drawings.
[0018] Fig. 1(A) is a plan view showing an example of a cation exchange laminate having a rectangular shape in plan view. In Fig. 1(A), a cation exchange laminate 10 is a cation exchange laminate having a rectangular shape in plan view, and includes a laminate 12 of a cation exchange membrane and a nonwoven fabric (not shown). The central part of the laminate 12 is an ion exchange section 14 in which the cation exchange membrane and the nonwoven fabric are not bonded to each other, and an adhesive section 18 is formed on the periphery of the ion exchange section 14. In Fig. 1(A), the region of the adhesive section 18 is indicated by hatching. The area of the adhesive portions 18 indicated by the diagonal lines relative to the total area of the laminate 12 in a plan view is such that the proportion of the adhesive portions 18 to the total area of the laminate 12 is 2% or more and less than 30%. As shown in FIG. 1(A), the adhesive portion 18 need only be present at a position surrounding the periphery of the ion exchange portion 14, and is not necessarily required to be present at the end portion of the laminate 12.
[0019] Fig. 1(B) is a plan view showing an example of a circular cation exchange laminate in plan view. The circular cation exchange laminate 20 shown in Fig. 1(B) has an adhesive part 18 on the circumferential edge part of the circular ion exchange part 14 in plan view. In the embodiment shown in Fig. 1(B), the adhesive part 18 is located at the end part of the laminate 20.
[0020] The proportion of the area of the adhesive portion (the shaded area in Figures 1(A) and 1(B)) to the total area of the cation exchange laminate of the present disclosure in a planar view is 2% or more and less than 30%, preferably 5% or more and 25% or less, and more preferably 10% or more and 20% or less. By having the area of the adhesive portion within the above range, the adhesive strength between the cation exchange membrane and the support is good, the area of the region in the laminate that contributes to cation exchange is sufficiently secured, and water leakage from the ends of the laminate is effectively suppressed.
[0021] To measure the area of the adhesive joint and calculate the area ratio of the adhesive joint, place the laminate on a flat surface and measure the width and length of the adhesive joint with a ruler. From the measured width and length, measure the adhesive area (A) of the adhesive joint. If the laminate is circular, measure the diameter of the circle, and the inner and outer diameters of the adhesive joint to calculate the area. The above area can also be measured from the density difference between the bonded and non-bonded areas using a known image analyzer. Similarly, the total area of the laminate is measured with a ruler to calculate the total area (B). The area (%) of the bonded portion relative to the total area of the laminate in a plan view is calculated by the following formula 1. Three samples are measured, and the average value is calculated to obtain the area ratio of the bonded portion. [Adhesive area of adhesive part (A) / total area (B)] × 100 (%) (Equation 1)
[0022] Although the mechanism of action of the present disclosure is not clear, the cation exchange laminate of the present disclosure includes a laminate of a cation exchange membrane, which is a self-supporting membrane, and a nonwoven fabric as a support, and the laminate has an ion exchange part consisting of a laminate of the cation exchange membrane and the support, and an adhesive part at the periphery of the ion exchange part where the cation exchange membrane and the support are attached, so that the strength of the entire cation exchange laminate is improved and deformation caused by the passage of a fluid is suppressed compared to when the cation exchange membrane is used alone as the ion exchange membrane. Furthermore, the adhesive part effectively suppresses water leakage by the area of the adhesive part being 2% or more and less than 30% of the total area of the ion exchange membrane laminate in a plan view. In addition, in the ion exchange part, which is a non-adhesive part, a constant concentration interface is formed at the interface between the cation exchange membrane and the nonwoven fabric, and it is considered that the ion exchange ability is higher than that of the cation exchange membrane alone. For this reason, it is considered that the cation exchange laminate of the present disclosure has good cation exchange ability.
[0023] The average adhesive strength between the cation exchange membrane and the support at the adhesive joint is preferably 2 N / 4.5 mm to 20 N / 4.5 mm. From the viewpoint of improving the durability and ion exchange capacity of the laminate, the average adhesive strength is preferably 2N / 4.5mm to 20N / 4.5mm, more preferably 5N / 4.5mm to 20N / 4.5mm, and even more preferably 10N / 4.5mm to 15N / 4.5mm.
[0024] The average adhesive strength is determined by preparing three samples of the laminate as reference material, measuring their peel strength, and taking the arithmetic mean of the measurement results as the average adhesive strength in the following manner. The 180° peel strength when peeling the cation exchange membrane from the nonwoven fabric of the laminate is measured under the following conditions. Measurements are taken at three points for each sample, and the average value is taken as the measured value. [Measurement conditions] Measuring device: TOYOSEIKI Strograph ES type device Measurement speed: 50mm / min Measurement range: 2.5N Sample shape: Width 15mm, length approx. 6cm
[0025] There is no particular limitation on the method for forming the adhesive portion between the cation exchange membrane and the nonwoven fabric in the laminate, and any known adhesive method can be used. The adhesive part may be an adhesive part in which the cation exchange membrane and the support are laminated with an adhesive, or may be a heat-sealed part between the cation exchange membrane and the support.
[0026] 〔glue〕 When the bonding portion is formed via an adhesive, examples of the adhesive include epoxy-based adhesives, acrylic-based adhesives, urethane-based adhesives, silicone-based adhesives, hot melt-based adhesives, etc., and from the viewpoint of adhesive strength, epoxy-based adhesives and acrylic-based adhesives are preferred, with acrylic-based adhesives being more preferred.
[0027] [Heat fusion] When the cation exchange membrane and the support are heat-sealed to form an adhesive joint, the heating temperature is selected taking into consideration the materials of the cation exchange membrane and the nonwoven fabric. The heat fusion can be carried out using a known heat sealer or the like, and the heating temperature can generally be set to 60° C. to 250° C. During heating, the cation exchange membrane and the nonwoven fabric may be pressed together to adhere to each other.
[0028] <Cation exchange membrane> The cation exchange membrane in the cation exchange laminate of the present disclosure can be used without any particular limitation as long as it has cation exchange ability. The cation exchange membrane is preferably a free-standing membrane. From the viewpoint of durability, the cation exchange membrane preferably has a thickness of 0.01 μm to 5.0 μm. The thickness of the cation exchange membrane can be from 0.01 μm to 10.0 μm, preferably from 0.01 μm to 5.0 μm, and more preferably from 0.1 μm to 3.0 μm.
[0029] The thickness of the cation exchange membrane can be measured using a spectrophotometer (ellipsometry) manufactured by JASCO Corporation. Specifically, when light is incident on a film with a refractive index n at a certain angle (θ), light A reflected from the front side of the film and light B reflected from the back side interfere with each other, resulting in a wavy interference spectrum. By counting the number of peaks (mountains or valleys) (Δm) of the interference spectrum within a certain wavelength range (λ1 to λ2), the thickness (d) can be calculated from the following formula (1).
[0030]
number
[0031] The cation exchange membrane according to the present disclosure preferably contains 10 mass% or more of a polymer (P) having an anionic structural group (a2) and selected from repeating structural units whose main chain end is a group containing a Group 16 atom of the periodic table, and a repeating structural unit (B) which does not have the anionic structural group (a2) and whose main chain end is a group containing a Group 16 atom of the periodic table, and in which the content of the anionic structural group (a2) in the total of the structural units (A) and (B) is taken as 100 mol%, based on the total mass of the cation exchange membrane.
[0032] More specifically, the polymer (P) is preferably an aromatic polyether resin containing a structural group (I) represented by the following formula (1) and a structural group (2) represented by the following formula (2).
[0033] [ka]
[0034] In the above formula (1) and formula (2), R 1 ~R 10 are each independently H, Cl, F, CF3, or C m H2 m+1 (m is an integer from 1 to 10), and R 1 ~R 10 At least one of the following is Cm H2 m+1 (m is an integer from 1 to 10), and R 1 ~R 10 may be present in two or more aromatic rings, and C m H2 m+1 If there are two or more C m H2 m+1 may be the same or different from each other. X 1 ~X 5 are each independently H, Cl, F, CF3, a protonic acid group, or a protonic acid salt; X 1 ~X 5 At least one of the groups is a protonic acid group or a protonic acid salt. A 1 ~A 6 each independently represents a single bond, -CH2-, -C(CH3)2-, -C(CF3)2-, -O-, or -CO-; i, j, k, and l each independently represent 0 or 1.
[0035] The cation exchange membrane preferably has a protonic acid group, which is a polar group related to the cationic structure. Examples of the protonic acid group include a sulfonic acid group, a carboxylic acid group, a phosphonic acid group, an alkylsulfonic acid group, an alkylcarboxylic acid group, and an alkylphosphonic acid group, and among these, a sulfonic acid group is preferred. In the present disclosure, a protonic acid salt refers to a salt compound in which the hydrogen atom of a protonic acid group is replaced with a Group 1 or Group 2 element such as lithium, sodium, potassium, calcium, magnesium, etc., an ammonium ion, etc. Among these, the protonic acid salt is preferably a sodium salt or a potassium salt, or may be a mixture thereof. With regard to the content of the protonic acid group or protonic acid salt in the polymer (P), the content of the structural units having a protonic acid group or a protonic acid salt relative to all the structural units contained in the polymer (P) is preferably 8 mol % to 70 mol %, more preferably 10 mol % to 50 mol %, and further preferably 25 mol % to 30 mol %, from the viewpoint of cation exchange ability.
[0036] The structural group (1) represented by the above formula (1) and the structural group (2) represented by the above formula (2) are described in detail in paragraphs
[0033] to
[0054] of JP 2021-123648 A. Among the protonic acid group-containing aromatic polyether resins having the structural groups described therein, those that function as cation exchange membranes are suitably used as the cation exchange membrane in the laminate of the present disclosure.
[0037] The polymer has a rigid main chain structure including a cyclic structure, and contains a predetermined amount of protonic acid groups, so that the polymer functions as a cation exchange membrane having both excellent strength and properties as a cation exchange membrane.
[0038] For example, the structural group (1) having a protonic acid group and represented by the above formula (1) may be the following structural unit (1-2) or (1-3).
[0039] [ka]
[0040] The structural group (2) represented by the above formula (2) having no protonic acid group may be the following structural unit (2-2) or (2-3).
[0041] [ka]
[0042] The cation exchange laminate of the present disclosure preferably contains the structural unit (1-2) or (1-3) having a sulfonic acid group in an amount of 25 mol % to 30 mol % relative to 100 mol of all structural units constituting the polymer (P). The method for producing the cation exchange membrane will be described in detail in the Examples.
[0043] <Nonwoven fabric> An example of the cation exchange laminate of the present disclosure includes a laminate of the above-mentioned cation exchange membrane and a nonwoven fabric. As the nonwoven fabric that can be used in the ion exchange membrane of the present disclosure, a nonwoven fabric made of thermoplastic resin fibers is preferable. The thermoplastic resin constituting the nonwoven fabric preferably contains one or more selected from the group consisting of polypropylene, polyethylene, ethylene-α-olefin copolymer, and polyethylene terephthalate, and more preferably contains polyester. Polyesters include, for example, polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate.
[0044] [Preferable physical properties of nonwoven fabric] The preferred physical properties of nonwoven fabric are a basis weight of 1 g / m 2 ~50g / m 2 The weight is in the range of 5g / m 2 ~20g / m 2 It is more preferable that the range is . The thickness of the nonwoven fabric is preferably from 15 μm to 1000 μm, more preferably from 15 μm to 500 μm, and even more preferably from 20 μm to 50 μm.
[0045] Other preferred physical properties of the nonwoven fabric are that it has an air permeability of 100 m as measured by the A method (Fragile method) described in JIS L 1096:2010 from the viewpoint of imparting necessary strength to the laminate without reducing the ion exchange capacity. 3 / cm 2 / s~400m 3 / cm 2 / s is preferred, and 100m 3 / cm 2 / s~400m 3 / cm 2 / s is more preferable. The air permeability is measured as follows based on Method A (Fragile type method) described in JIS L 1096:2010. Attach a 20cm x 20cm test piece to the testing machine, adjust the intake fan and air holes so that the inclined barometer reads 125 Pa, and measure the pressure indicated by the vertical barometer. Using the measured pressure and the type of air hole, calculate the amount of air passing through the test piece using the conversion table attached to the testing machine.
[0046] The nonwoven fabric and the cation exchange membrane may be laminated together via an adhesive or pressure-sensitive adhesive, or the nonwoven fabric and the cation exchange membrane may be laminated together and the periphery of the ion exchange portion sandwiched between a frame material to fix them. Since the laminate of the present disclosure has an adhesive portion around the periphery of the ion exchange portion, a preferred embodiment is one in which the nonwoven fabric and the cation exchange membrane are laminated together, the ion exchange portion, i.e., the nonwoven fabric and the cation exchange membrane are not adhered to each other, and an adhesive portion is formed around the periphery of the ion exchange portion. In addition, when the nonwoven fabric and the cation exchange membrane are bonded together via an adhesive or pressure-sensitive adhesive, the ion exchange capacity may decrease if the openings in the nonwoven fabric are blocked, so it is preferable to apply the adhesive or pressure-sensitive adhesive only to the fibers that make up the nonwoven fabric.
[0047] The laminate of the present disclosure, in which a cation exchange membrane and a nonwoven fabric are laminated, has a configuration in which each of the constituent materials is substantially independent, and therefore, compared to a configuration in which a porous substrate is impregnated with an ion exchange resin, such as a commercially available ion exchange membrane, peeling of the ion exchange resin due to deterioration of the porous substrate is suppressed, and an additional effect of improving the durability of the laminate is also achieved.
[0048] The laminate of the present disclosure is, for example, appropriately cut into an appropriate size and then used or sold. The laminate of the present disclosure can be used for known applications without any restrictions. Applications include, for example, electrodialysis membranes, diffusion dialysis membranes, reverse electrodialysis membranes, fuel cells (eg, methanol fuel cells), as well as electrolyte membranes for solid polymer membrane cells and various secondary cells. For example, in the case of electrodialysis membranes, the cation exchange laminate of the present disclosure is a low-resistance membrane, so that a reduction in running costs can be expected. In addition, in the case of diffusion dialysis membranes, even if the cation exchange membrane is a thin layer, the durability is good and water leakage is suppressed, so that a dramatic improvement in ion permeation flux can be expected. In the case of reverse electrodialysis membranes, the ion exchange membrane has a high transport number and a low membrane resistance, so that an improvement in output performance can be expected. In the case of electrolyte membranes for fuel cells, a dramatic improvement in proton conductivity can be expected for the same reason.
[0049] <<Ion exchange cartridges for electrodialysis>> The laminate of the present disclosure is suitably used in an ion exchange cartridge for electrodialysis. The ion exchange cartridge for electrodialysis according to the present disclosure is an ion exchange cartridge for electrodialysis in which the above-described cation exchange laminates according to the present disclosure and supports are alternately arranged.
[0050] Fig. 2 is a schematic diagram of an ion exchange cartridge for electrodialysis according to the present disclosure. An ion exchange cartridge for electrodialysis 30 is formed by alternately stacking 6 to 20 layers of the cation exchange laminate 26 according to the present disclosure and a known anion exchange laminate 28, and providing a pair of electrodes 32A, 32B at the ends. In Fig. 2, the solid lines indicate the flow paths of the concentrated water lines, and the dashed lines indicate the flow paths of the dilute water lines. Fig. 3 is a schematic diagram and an enlarged schematic cross-sectional view of an example of a cation exchange laminate 26 of the present disclosure incorporated in Fig. 2. As shown in the enlarged schematic cross-sectional view, the laminate 26 shown in Fig. 3 has a laminate structure in which a cation exchange membrane 22 is sandwiched between two nonwoven fabrics 24, and has an adhesive part 18 on the periphery of the laminate structure. The cation exchange laminate 26 shown in Fig. 3 has adhesive parts 18 on its periphery, and therefore, when incorporated into the ion exchange cartridge 30 for electrodialysis shown in Fig. 2, it does not obstruct the flow path of the concentrated water line shown by the solid line in Fig. 2, and furthermore, water leakage from the cation exchange membrane 22 sandwiched between the nonwoven fabrics 24 and the gaps in the nonwoven fabrics 24 is suppressed. Note that, although the direction of water leakage is indicated by the dashed arrow in Fig. 2, the ion exchange cartridge 30 for electrodialysis shown in Fig. 2 suppresses water leakage from the cation exchange laminate, which usually occurs frequently, and therefore suppresses leakage of untreated liquid due to water leakage, thereby exhibiting efficient cation exchange capacity. EXAMPLES
[0051] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to examples. Note that the present disclosure is not limited to the description of these examples.
[0052] The abbreviations used in the present examples and comparative examples are as follows.
[0053] (1) Solvent DMSO: Dimethyl sulfoxide NMP: N-methyl-2-pyrrolidone DMF: N,N-dimethylformamide (2) Components of aromatic polyether DFBP: 4,4'-difluorobenzophenone DSDFBP: 5,5'-carbonylbis(sodium 2-fluorobenzenesulfonate) TMBPF: 3,3',5,5'-tetramethyl-4,4'-dihydroxydiphenylmethane BPA: 4,4'-(2,2-propanediyl)diphenol The water used in this example was purified using Millipore's MQ Academic A10 system.
[0054] <How to measure film thickness> The thickness of the cation exchange membrane was measured using a spectrophotometer (ellipsometry) manufactured by JASCO Corporation. Specifically, when light is incident on a film with a refractive index n at a certain angle (θ), light A reflected from the front side of the film and light B reflected from the back side interfere with each other, resulting in a wavy interference spectrum. By counting the number of peaks (mountains or valleys) (Δm) of the interference spectrum within a certain wavelength range (λ1 to λ2), the thickness (d) was calculated using the following formula (1).
[0055]
number
[0056] <Method of measuring adhesive strength> In a laminate of a cation exchange membrane and a nonwoven fabric, the 180° peel strength when peeling the cation exchange membrane from the nonwoven fabric was measured under the following conditions, and this was taken as the adhesive strength. Each sample is measured at three points and the average value is taken as the measured value. [Measurement conditions] Measuring device: TOYOSEIKI Strograph ES type device Measurement speed: 50mm / min Measurement range: 2.5N Sample shape: Width 15mm, length approx. 6cm
[0057] <Method for measuring the adhesive area ratio> The area measurement of the adhesive part and the calculation of the area ratio of the adhesive part were performed by placing the laminate on a flat surface, measuring the width and length of the adhesive part with a ruler, and calculating the adhesive area (A) of the adhesive part from the measured width and length. Similarly, the total area of the laminate was measured with a ruler to calculate the total area (B). The area (%) of the adhesive portion relative to the total area of the laminate in a plan view was calculated by the following formula 1. Three samples were measured, and the average value was calculated to obtain the area ratio of the adhesive portion. [Adhesive area of adhesive part (A) / total area (B)] × 100 (%) (Equation 1)
[0058] <Electrodialysis performance evaluation and leakage measurement> The electrodialysis performance was evaluated using a benchtop electrodialysis device (Micro Asilazer S3) manufactured by Astom Co., Ltd. One cation exchange membrane of the Example or Comparative Example and ASM manufactured by Astom Co., Ltd. were used as a pair of units, and the evaluation was performed using a two-chamber electrodialysis device of six units. Effective membrane area: 330cm 2 The electrode solution was 500 mL of a 5 mass% aqueous sodium nitrate solution, the dilute side solution was 500 mL of a 0.5 mol / % aqueous sodium chloride solution, and the concentrated side solution was 500 mL of a 0.5 mol / % aqueous sodium chloride solution. Electrodialysis was performed at 25°C, an average current of 1.0 A, and a voltage of 10 V, and the electrodialysis performance was evaluated from the ratio of the molar concentration of the dilute side solution to the molar concentration of the concentrated side solution (molar concentration of concentrated side solution / molar concentration of dilute side solution) 60 minutes after the start of electrodialysis. The higher this value, the higher the electrodialysis performance (cation exchange capacity) is evaluated to be. Meanwhile, the amount of liquid that flowed out 60 minutes after the start of electrodialysis was taken as the amount of liquid leakage, and this amount was measured after the evaluation of the electrodialysis performance was completed.
[0059] [Synthesis Example 1: Synthesis of Resin 1] (1. Synthesis of Monomer 1 (DSDFBP)) According to the method described in paragraph
[0061] (Synthesis Example 1) of JP2014-533A, white crystals of Monomer 1 (DSDFBP) having the following structure were obtained. The yield was 155.2 g (0.386 mol, 70% yield).
[0060] [ka]
[0061] 2. Synthesis of Resin 1 In a five-necked reactor equipped with a nitrogen inlet tube, a thermometer, a reflux condenser, and a stirrer, 40.1 g (0.095 mol) of DSDFBP, 62.2 g (0.285 mol) of DFBP, 97.4 g (0.380 mol) of TMBPF, and 65.7 g (0.475 mol) of potassium carbonate were weighed out as the monomer 1 obtained above. 783.4 g of DMSO and 261.1 g of toluene were added thereto, and the mixture was stirred under a nitrogen atmosphere and heated at 130° C. for 12 hours. The water generated was removed from the system, and then the toluene was distilled off.
[0062] The reaction was continued at 160°C for 12 hours to obtain a viscous polymer solution. The obtained solution was diluted with 570g of toluene and then poured into 2400g of methanol. The precipitated polymer powder was filtered, washed, and then dried at 150°C for 4 hours to obtain 171.6g of polyetherketone powder (Resin 1).
[0063] The resin (1) has a structure represented by the following (1-3) as the structural unit (1).
[0064] [ka] Moreover, the resin (1) has a structure represented by the following (2-3) as the structural unit (2).
[0065] [ka]
[0066] Resin 1 has a content of the structural unit (1) of 25 mol % (the total of the structural unit (1) and the structural unit (2) is 100 mol %).
[0067] <Synthesis Example 2: Synthesis of Resin 2> The resin raw materials and solvent were 80.2 g (0.190 mol) of DSDFBP, 41.5 g (0.190 mol) of DFBP, 97.4 g (0.380 mol) of TMBPF, 65.7 g (0.475 mol) of potassium carbonate, as well as 876.4 g of DMSO and 292.1 g of toluene. Except for this, 174.6 g of polymer powder (resin 2) was obtained in the same manner as in the synthesis example of resin 1. Resin 2 has a content of the structural unit (1) of 50 mol % (the total of the structural unit (1) and the structural unit (2) is 100 mol %).
[0068] <Synthesis Example 3: Synthesis of Resin 3> In a five-necked reactor equipped with a nitrogen inlet tube, a thermometer, a reflux condenser, and a stirrer, 40.2 g (0.095 mol) of DSDFBP obtained in the synthesis of monomer 1, 62.2 g (0.285 mol) of DFBP, 86.8 g (0.380 mol) of BPA, and 65.7 g (0.475 mol) of potassium carbonate were weighed out. 756.2 g of DMSO and 302.1 g of toluene were added thereto, stirred under a nitrogen atmosphere, heated at 130°C for 12 hours, and the generated water was removed from the system, and then the toluene was distilled off.
[0069] The reaction was continued for 12 hours at 160°C to obtain a viscous polymer solution. The obtained solution was diluted with 570g of toluene and then poured into 2400g of methanol. The precipitated polymer powder was filtered, washed, and then dried at 150°C for 4 hours to obtain 160.6g of polyetherketone powder (resin 3).
[0070] The resin (3) contains the following structural unit (1-2) as the structural unit (1).
[0071] [ka]
[0072] The structural unit (2) includes the following structural unit (2-2).
[0073] [ka]
[0074] Resin 3 has a content of the structural unit (1) of 25 mol % (the total of the structural unit (1) and the structural unit (2) is 100 mol %).
[0075] For Resin 1, Resin 2 and Resin 3, the constituent materials and sulfonic acid unit contents of the synthesized polymers are shown in Table 1 below.
[0076] [Table 1]
[0077] [Example 1] Resin 1 obtained in Synthesis Example 1 was dissolved in a mixed solvent of DMF and toluene (DMF / toluene = 50 / 50 (weight ratio)) to prepare a varnish. This varnish was cast onto a PET substrate having a release agent layer (A4160 manufactured by Toyobo Co., Ltd.) and dried at 110°C for 3 minutes to obtain a film of Resin 1. This was peeled off from the PET substrate to obtain a free-standing film 1.
[0078] Next, the air permeability measured by the A method (Fragile method) described in JIS L 1096:2010 is 266 m 3 / cm 2 Two sheets of polyester nonwoven fabric (05TH-12 (product name), manufactured by Hirose Paper Co., Ltd.) with a length of 1 / s and a thickness of 43 μm were prepared, and the self-supporting membrane 1 was sandwiched between these nonwoven fabrics to integrate them.Then, using a stand sealer (NL-453PS-5, manufactured by Ishizaki Electric Manufacturing Co., Ltd.), they were thermally bonded at 120°C with an area ratio of 2% to form an adhesive joint, thereby obtaining the cation exchange laminate of Example 1. The adhesive portion was formed on the periphery of the rectangular free-standing film.
[0079] [Example 2] The self-supporting membrane 1 prepared in the same manner as in Example 1 had an air permeability of 266 m as measured by the A method (Fragile type method) described in JIS L 1096:2010.3 / cm 2 Two sheets of polyester nonwoven fabric (05TH-12 (product name), manufactured by Hirose Paper Co., Ltd.) with a length of 1 / s and a thickness of 43 μm were prepared, and the self-supporting membrane 1 was sandwiched between these nonwoven fabrics to integrate them.Then, using a stand sealer (NL-453PS-5, manufactured by Ishizaki Electric Manufacturing Co., Ltd.), they were thermally bonded at an area ratio of 10% at approximately 120°C to form an adhesive joint, thereby obtaining the cation exchange laminate of Example 2. The adhesive portion was formed on the periphery of the rectangular free-standing film.
[0080] [Example 3] The self-supporting membrane 1 prepared in the same manner as in Example 1 had an air permeability of 266 m as measured by the A method (Fragile type method) described in JIS L 1096:2010. 3 / cm 2 Two sheets of polyester nonwoven fabric (05TH-12 (product name), manufactured by Hirose Paper Co., Ltd.) with a length of 1 / s and a thickness of 43 μm were prepared, and the self-supporting membrane 1 was sandwiched between these nonwoven fabrics to integrate them.Then, using a stand sealer (NL-453PS-5, manufactured by Ishizaki Electric Manufacturing Co., Ltd.), they were thermally bonded at an area ratio of 20% at approximately 120°C to form an adhesive joint, thereby obtaining the cation exchange laminate of Example 3. The adhesive portion was formed on the periphery of the rectangular free-standing film.
[0081] [Example 4] Resin 2 obtained in Synthesis Example 2 was dissolved in a mixed solvent of DMF and toluene (DMF / toluene = 50 / 50 (weight ratio)) to prepare a varnish. This varnish was cast onto a PET substrate having a release agent layer (A4160 manufactured by Toyobo Co., Ltd.) and dried at 110°C for 3 minutes to obtain a film of Resin 2. This was peeled off from the PET substrate to obtain a free-standing film 2.
[0082] Next, the air permeability measured by the A method (Fragile method) described in JIS L 1096:2010 is 266 m 3 / cm 2Two sheets of polyester nonwoven fabric (05TH-12 (product name), manufactured by Hirose Paper Co., Ltd.) with a length of 1 / s and a thickness of 43 μm were prepared, and the obtained free-standing membrane 2 was sandwiched between the nonwoven fabrics to integrate them. After that, using a stand sealer (NL-453PS-5, manufactured by Ishizaki Electric Manufacturing Co., Ltd.), they were thermally bonded at an area ratio of 20% at approximately 120°C to form an adhesive joint, and a cation exchange laminate of Example 4 was obtained. The adhesive portion was formed on the periphery of the rectangular free-standing film.
[0083] [Example 5] Resin 3 obtained in Synthesis Example 3 was dissolved in a mixed solvent of DMF and toluene (DMF / toluene = 50 / 50 (weight ratio)) to prepare a varnish. This varnish was cast onto a PET substrate (A4160 manufactured by Toyobo Co., Ltd.) having a release agent layer, and dried at 110°C for 3 minutes to obtain a film of Resin 3. This was peeled off from the PET substrate to obtain a free-standing film 3.
[0084] Next, the air permeability measured by the A method (Fragile method) described in JIS L 1096:2010 is 266 m 3 / cm 2 Two sheets of polyester nonwoven fabric (05TH-12 (product name), manufactured by Hirose Paper Co., Ltd.) with a length of 1 / s and a thickness of 43 μm were prepared, and the self-supporting membrane 3 was sandwiched between the nonwoven fabrics to integrate them.Then, using a stand sealer (NL-453PS-5, manufactured by Ishizaki Electric Manufacturing Co., Ltd.), they were thermally bonded at an area ratio of 20% at approximately 120°C to form an adhesive joint, thereby obtaining the cation exchange laminate of Example 5. The adhesive portion was formed on the periphery of the rectangular free-standing film.
[0085] [Example 6] A free-standing film 1 was prepared in the same manner as in Example 1. Next, the air permeability measured by the A method (Fragile method) described in JIS L 1096:2010 is 330 m 3 / cm 2Two sheets of polypropylene nonwoven fabric (Syntex (registered trademark) PK-108, manufactured by Mitsui Chemicals, Inc.) with a length of 1 / s and a thickness of 380 μm were prepared, and the self-supporting membrane 1 was sandwiched between the nonwoven fabrics to integrate them. After that, using a stand sealer (NL-453PS-5, manufactured by Ishizaki Electric Works, Ltd.), they were thermally bonded at a temperature of approximately 100°C at an area ratio of 20% to form an adhesive joint, thereby obtaining the cation exchange laminate of Example 6. The adhesive portion was formed on the periphery of the rectangular free-standing film.
[0086] [Example 7] A free-standing film 1 was prepared in the same manner as in Example 1. Next, the air permeability measured by the A method (Fragile method) described in JIS L 1096:2010 is 266 m 3 / cm 2 Two sheets of polyester nonwoven fabric (05TH-12 (product name), manufactured by Hirose Paper Co., Ltd.) with a length of 1 / s and a thickness of 43 μm were prepared, and an adhesive (CAT-I300S, manufactured by Teikoku Ink Co., Ltd.) was applied to the nonwoven fabric with an adhesive area ratio of 20%, and then the free-standing membrane 1 was sandwiched between them to integrate them.Then, the sheets were dried in an oven at a temperature of 80°C for 10 minutes to form an adhesive portion, and the cation exchange laminate of Example 7 was obtained. The adhesive portion was formed on the periphery of the rectangular free-standing film.
[0087] [Comparative Example 1] A free-standing film 1 was prepared in the same manner as in Example 1. Next, the air permeability measured by the A method (Fragile method) described in JIS L 1096:2010 is 266 m 3 / cm 2 Two sheets of polyester nonwoven fabric (05TH-12 (product name), manufactured by Hirose Paper Co., Ltd.) with a length of 1 / s and a thickness of 43 μm were prepared, and the free-standing membrane 1 was sandwiched between the nonwoven fabrics to be integrated. Thereafter, a cation exchange laminate of Comparative Example 1 was obtained that was not thermally bonded and had no adhesive part.
[0088] [Comparative Example 2] A free-standing film 1 was prepared in the same manner as in Example 1. Next, the air permeability measured by the A method (Fragile method) described in JIS L 1096:2010 is 330 m 3 / cm 2 Two sheets of polypropylene nonwoven fabric (Syntex (registered trademark) PK-108, manufactured by Mitsui Chemicals, Inc.) with a length of 1 / s and a thickness of 380 μm were prepared, and the free-standing membrane 1 was sandwiched between the nonwoven fabrics to be integrated. Thereafter, a cation exchange laminate of Comparative Example 2 was obtained which was not thermally bonded and had no adhesive part.
[0089] [Comparative Example 3] A free-standing film 1 was prepared in the same manner as in Example 1. Next, the air permeability measured by the A method (Fragile method) described in JIS L 1096:2010 is 266 m 3 / cm 2 Two sheets of polyester nonwoven fabric (05TH-12 (product name), manufactured by Hirose Paper Co., Ltd.) with a length of 1 / s and a thickness of 43 μm were prepared, and the self-supporting membrane 1 was sandwiched between the nonwoven fabrics to integrate them. Thereafter, a stand sealer (NL-453PS-5, manufactured by Ishizaki Electric Co., Ltd.) was used to thermally bond the two at a temperature of about 120° C. and an area ratio of 60% to form a bonded portion, thereby obtaining a cation exchange laminate of Comparative Example 3. The adhesive portion was formed on the periphery of the rectangular free-standing film.
[0090] [Comparative Example 4] A free-standing film 1 was prepared in the same manner as in Example 1. Next, the air permeability measured by the A method (Fragile method) described in JIS L 1096:2010 is 266 m 3 / cm 2 Two sheets of polyester nonwoven fabric (05TH-12 (product name), manufactured by Hirose Paper Co., Ltd.) with a length of 1 / s and a thickness of 43 μm were prepared, and the self-supporting membrane 1 was sandwiched between the nonwoven fabrics to integrate them. Thereafter, a stand sealer (NL-453PS-5, manufactured by Ishizaki Electric Co., Ltd.) was used to thermally bond the two sheets at a temperature of about 120° C. and an area ratio of 1% was used to form a bonded portion, and a cation exchange laminate of Comparative Example 4 was obtained. The adhesive portion was formed on the periphery of the rectangular free-standing film.
[0091] For the obtained cation exchange laminates of each Example and Comparative Example, the adhesive strength between the cation exchange membrane and the nonwoven fabric, the area ratio of the adhesive part (referred to as the adhesive area ratio in the table), the amount of liquid leakage, and the molar concentration ratio of ions after 60 minutes of electrodialysis treatment, which indicates the cation exchange capacity (electrodialysis performance) of the cation exchange laminate, were measured by the methods described above. The results are shown in Tables 2 and 3 below.
[0092] [Table 2]
[0093] [Table 3]
[0094] The cation exchange laminates of Examples 1 to 7 showed no liquid leakage even after 60 minutes of electrodialysis, and the molar concentration ratio exceeded 10, confirming that they exhibited cation exchange capacity that is acceptable for practical use. On the other hand, in the cation exchange laminates of Comparative Examples 1 and 2, which had no adhesive parts, and Comparative Example 4, in which the area of the adhesive parts was too small, liquid leakage was observed, and as a result, the cation exchange capacity was inferior to that of each Example. In addition, in the cation exchange laminate of Comparative Example 3, which had adhesive parts but had too large an area, liquid leakage was suppressed, but the area of the ion exchange parts was relatively small, so the cation exchange capacity was inferior to that of each Example. [Explanation of symbols]
[0095] 10 Cation exchange laminate 12 Laminate 14 Ion exchange section 18 Adhesive part 20 Cation exchange laminate 22 Cation exchange membrane 24 Nonwoven fabric 26 Cation exchange laminate 28 Anion exchange laminate 30 Ion exchange cartridge for electrodialysis 32A, 32B electrode
Claims
1. A cation exchange membrane; A laminate comprising a support including a nonwoven fabric made of thermoplastic resin fibers, The laminate includes an ion exchange portion including a laminate of the cation exchange membrane and the support, and an adhesive portion between the cation exchange membrane and the support is provided on the periphery of the ion exchange portion; A cation exchange laminate, wherein the ratio of the area of the adhesive portion to the total area of the laminate in a plan view is 2% or more and less than 30%.
2. 2. The cation exchange laminate according to claim 1, wherein the average adhesive strength between the cation exchange membrane and the support at the adhesive joint is from 2 N / 4.5 mm to 20 N / 4.5 mm.
3. The cation exchange laminate according to claim 1 , wherein the adhesive portion is an adhesive portion formed by laminating the cation exchange membrane and the support with an adhesive, or a heat-sealed portion between the cation exchange membrane and the support.
4. 2. The cation exchange laminate according to claim 1, wherein the cation exchange membrane has a thickness of 0.01 μm to 5.0 μm.
5. The cation exchange membrane comprises one or more repeating structural units (A) selected from repeating structural units having an anionic structural group (a2) and having a main chain terminal which is a group containing an atom of Group 16 of the periodic table; a repeating structural unit (B) which does not have the anionic structural group (a2) and whose main chain end is a group containing an atom of Group 16 of the periodic table, 2. The cation exchange laminate according to claim 1, wherein the polymer (P) has a content of the anionic structural group (a2) of 5 mol % to 90 mol % relative to the total of the structural units (A) and (B), where the total of the structural units (A) and (B) is taken as 100 mol %, in an amount of 10 mass % or more relative to the total mass of the cation exchange membrane.
6. The cation exchange laminate according to claim 5, wherein the polymer (P) is an aromatic polyether resin containing a structural group (I) represented by the following formula (1) and a structural group (2) represented by the following formula (2). 【Chemistry 1】 [In formula (1) and formula (2), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , and R 10 are each independently H, Cl, F, or CF 3 , or C m H2 m+1 (m represents an integer of 1 to 10), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 and R 10 At least one of the following is C m H2 m+1 (m is an integer from 1 to 10), and R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 and R 10 may be present in two or more aromatic rings, and C m H2 m+1 If there are two or more C m H2 m+1 may be the same or different from each other. X 1 , X 2 , X 3 , X 4 , and X 5 are each independently H, Cl, F, or CF 3 , a protonic acid group or a protonic acid salt; X 1 , X 2 , X 3 , X 4 , and X 5 At least one of represents a protonic acid group or a protonic acid salt. A 1 , A 2 , A 3 , A 4 , A 5 , and A 6 each independently represents a single bond, -CH 2 -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 It represents -, -O- or -CO-. i, j, k and l each independently represent 0 or 1.
7. 7. An ion exchange cartridge for electrodialysis, comprising the cation exchange laminate according to any one of claims 1 to 6 and a support arranged alternately.
Citation Information
Patent Citations
Ion exchange membrane and method for producing the same
JP2012040508A
Polymer functional film, and production method, laminate, and device thereof
JP2016137434A
Medical signal processing device, cap member, and medical signal processing method
JP2021129648A
Ceramic Anion Exchange Materials
JP2022535132A
Particulate filter and method of use
US20100218595A1