Carbon dioxide separation membrane and carbon dioxide separation membrane module
The carbon dioxide separation membrane with a copolymer first layer, silicone resin intermediate layer, and porous second layer addresses the challenges of high permeation and separation efficiency, offering a simplified manufacturing process for effective carbon dioxide separation.
Patent Information
- Application Number
- JP2023059313
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing carbon dioxide separation membranes face challenges in achieving high permeation rates and sufficient separation functions while maintaining a simple manufacturing process, with issues such as ionic liquid leakage and complex manufacturing processes in existing technologies.
A carbon dioxide separation membrane comprising a first layer made of a copolymer containing a (meth)acrylic acid ester monomer with a glycidyl group and a (meth)acrylamide monomer, an intermediate layer with a silicone resin, and a porous second layer, utilizing a room temperature molten salt with specific anions and cations to enhance permeation and separation efficiency.
The membrane achieves a high carbon dioxide permeation rate and effective separation function with a simplified manufacturing process, suitable for industrial applications in separating carbon dioxide from mixed gases.
Smart Images

Figure 2024146426000001 
Figure 2024146426000002 
Figure 2024146426000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon dioxide separation membrane and a carbon dioxide separation membrane module. [Background technology]
[0002] In recent years, climate change due to global warming has become a problem. Carbon dioxide is said to be the greenhouse gas that has the greatest impact on global warming, and research is being actively conducted on technologies to separate and capture carbon dioxide from mixed gases that contain it.
[0003] As a technique for separating and recovering carbon dioxide from a mixed gas containing carbon dioxide, a membrane separation method has been developed that can efficiently separate acidic gases while suppressing operating costs. An example of a separation membrane used in the membrane separation method is a composite membrane formed of a layer having a separation function and a porous layer. If the thickness of the separation function layer of this composite membrane is reduced, the permeation rate of acidic gases is improved. In order to further reduce the thickness of the separation function layer, an intermediate layer may be disposed between the separation function layer and the porous support as in Patent Document 1, but there is a demand for further improving the permeation rate without reducing the separation function.
[0004] In addition, ionic liquids (also called room temperature molten salts) have been attracting attention as materials used in layers having a separation function because of their excellent carbon dioxide absorption capacity.
[0005] For example, Patent Document 2 proposes a gas-separating gel membrane obtained by heating and drying a gel-forming composition containing an ionic liquid and polyvinyl alcohol. Although a gel membrane can be obtained from the mixture by a simple operation, there is a problem that the ionic liquid leaks from the formed gel membrane when the concentration of the ionic liquid in the gel-forming composition is high.
[0006] Patent Document 3 proposes a gel-like thin film obtained by drying and dehydrating a hydrogel produced from a gel-forming composition containing two polymers having different reactive functional groups, and immersing the dehydrated product in an ionic liquid. Although the ionic liquid does not leak from the gel-like thin film due to the network structure formed by the reaction of two polymers in the gel-forming composition, the production process of the gel-forming composition is complicated and difficult to control because the two polymers react gradually in the gel-forming composition. In addition, there is a step of drying and dehydrating the hydrogel to form a dehydrated product and a step of immersing the dehydrated product in an ionic liquid, and it is not easy to obtain an ionic liquid gel. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2015-160159 A [Patent Document 2] Patent No. 5877961 [Patent Document 3] JP 2013-60504 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above problems, and has an object to provide a carbon dioxide separation membrane and a carbon dioxide separation membrane module that can be formed by a simple procedure and have sufficient carbon dioxide separation function and carbon dioxide permeation rate. [Means for solving the problem]
[0009] The present inventors conducted extensive research to solve the above problems and arrived at the present invention. That is, the present invention is a carbon dioxide separation membrane comprising a first layer, a porous second layer, and an intermediate layer containing a silicone resin and disposed between the first layer and the second layer, wherein the first layer is a layer containing a copolymer (A) having as essential constituent monomers a (meth)acrylic acid ester-based monomer (a1) having a glycidyl group and having a chemical formula weight of 500 or less, and a (meth)acrylamide-based monomer (a2) having a chemical formula weight of 500 or less, and a room temperature molten salt (B) consisting of an anion and an organic cation, wherein the (meth)acrylamide-based monomer (a2) is at least one amide selected from the group consisting of (meth)acrylamide, N-substituted (meth)acrylamide, and N,N-disubstituted (meth)acrylamide, and the weight of the room temperature molten salt (B) is 95% by weight or less based on the total weight of the copolymer (A) and the room temperature molten salt (B). Effect of the Invention
[0010] According to the present invention, it is possible to provide a carbon dioxide separation membrane and a carbon dioxide separation membrane module that can be formed by a simple procedure and have a sufficient carbon dioxide separation function and carbon dioxide permeation rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment.
[0012] [Carbon dioxide separation membrane] The carbon dioxide separation membrane of the present invention is a carbon dioxide separation membrane comprising a first layer, a porous second layer, and an intermediate layer that is disposed between the first layer and the second layer and contains a silicone resin. Each layer will be described in detail below.
[0013] [First layer] The first layer is a layer containing a copolymer (A) having as essential constituent monomers a (meth)acrylic acid ester monomer (a1) having a glycidyl group and a chemical formula weight of 500 or less, and a (meth)acrylamide monomer (a2) having a chemical formula weight of 500 or less, and a room-temperature molten salt (B) consisting of an anion and an organic cation, the (meth)acrylamide monomer (a2) being at least one amide selected from the group consisting of (meth)acrylamide, N-substituted (meth)acrylamide, and N,N-disubstituted (meth)acrylamide, and the weight of the room-temperature molten salt (B) is 95% by weight or less based on the total weight of the copolymer (A) and the room-temperature molten salt (B). Here, the (meth)acrylic acid ester means a methacrylic acid ester or an acrylic acid ester, and the (meth)acrylamide means a methacrylamide or an acrylamide.
[0014] <(Meth)acrylic acid ester monomer (a1)> The (meth)acrylic acid ester monomer (a1) is a (meth)acrylic acid ester monomer having a glycidyl group and a chemical formula weight of 500 or less. The (meth)acrylic acid ester monomer having a glycidyl group may be a compound having one or more acryloyl groups and one or more glycidyl groups in one molecule, and may be a compound having one each of an acryloyl group and a glycidyl group, or may be a compound having two or more acryloyl groups and two or more glycidyl groups. For example, it may be a diacrylate having two acryloyl groups or a diglycidyl ether having two epoxy groups, and is not particularly limited.
[0015] Examples of the (meth)acrylic acid ester monomer (a1) having a glycidyl group include glycidyl (meth)acrylate {chemical formula weight: 128 (142)}, glycidyloxyalkyl (meth)acrylate [2-hydroxyethyl (meth)acrylate glycidyl ether {chemical formula weight: 172 (186)}, 3-hydroxypropyl (meth)acrylate glycidyl ether {chemical formula weight: 186 (200)}, 2-hydroxypropyl (meth)acrylate glycidyl ether {chemical formula weight: 186 (200)}, 4-hydroxybutyl (meth)acrylate glycidyl ether {chemical formula weight: 200 (214)}, 2-hydroxybutyl (meth)acrylate glycidyl ether {chemical formula weight: 200 (214)}, 5-hydroxypropyl ... -hydroxypentyl (meth)acrylate glycidyl ether {chemical formula weight: 214 (228)}, 6-hydroxyhexyl (meth)acrylate glycidyl ether {chemical formula weight: 228 (242)}, 3-hydroxy-3-methylbutyl (meth)acrylate glycidyl ether {chemical formula weight: 214 (228)}, 2-hydroxy-3-phenoxypropyl (meth)acrylate glycidyl ether {chemical formula weight: 278 (292)}, etc.], pentaerythritol tri(meth)acrylate glycidyl ether {chemical formula weight: 354 (398)}, (meth)acrylic acid ester monomers represented by the following general formula (2), and (meth)acrylic acid ester monomers represented by the following general formula (3). The chemical formula weights of the acrylate and methacrylate are listed next to the compound name, and the chemical formula weight of the methacrylate is listed in parentheses.
[0016] CH2=CR 3 -C(O)O-(R 4 O)nX 1 (2)
[0017] In the general formula (2), R 3 is H or CH3, R 3 As the radical, H is preferable.
[0018] X 1 represents a glycidyl group.
[0019] R 4 is CH2CH2 or CH2CH(CH3), n is an integer of 2 or more, and there are two or more R 4 may all be the same or different. 4 When all are CH2CH2, the upper limit of n is 8, and R 4 When all are CH2CH(CH3), the upper limit of n is 6. 4 When CH2CH2 and CH2CH(CH3) are included as a cyclic group, the upper limit of n is the number of R 4 R is CH2CH(CH3) 4 Except when there are 6 and 7 O's, it is 8. n is preferably 2 or 3.
[0020] R 4 When CH2CH2 and CH2CH(CH3) are included, R 4 There is no limitation on the mode of bonding between the ethyleneoxy group and the propyleneoxy group represented by O, and they may be bonded regularly (block bond, alternating bond, etc.) or randomly. R 4 When CH2CH2 and CH2CH(CH3) are included as the substituent, the bond is preferably random.
[0021] R 4 When CH2CH2 and CH2CH(CH3) are contained as the alkyl group, the number of CH2CH2 and CH2CH(CH3) is preferably 1 or 2, respectively.
[0022] R 4 is preferably CH2CH2.
[0023] Examples of the (meth)acrylic acid ester monomer represented by the general formula (2) include glycidyl ether diethylene glycol (meth)acrylate {chemical formula weight: 216, (230)}, glycidyl ether triethylene glycol (meth)acrylate {chemical formula weight: 260, (274)}, glycidyl ether dipropylene glycol (meth)acrylate {chemical formula weight: 244, (258)}, and glycidyl ether tripropylene glycol (meth)acrylate {chemical formula weight: 302, (316)}. The chemical formula weights of the acrylate and methacrylate are listed in succession following the compound name, and the chemical formula weight of the methacrylate is listed in parentheses.
[0024] Glycidyl ether diethylene glycol (meth)acrylate is represented by the general formula (2), 3 is H or CH3, R 4 is CH2CH2, n is 2, X 1 Glycidyl ether triethylene glycol (meth)acrylate is represented by the chemical formula (2), where R 3 is H or CH3, R 4 is CH2CH2, n is 3, X 1 Glycidyl ether dipropylene glycol (meth)acrylate is represented by the chemical formula (2) in which R 3 is H or CH3, R 4 is CH2CH(CH3), n is 2, X 1 Glycidyl ether tripropylene glycol (meth)acrylate is represented by the chemical formula (2), where R 3 is H or CH3, R 4 is CH2CH(CH3), n is 3, X 1 is represented by the chemical formula:
[0025] CH2=CR 5 -C(O)O-(R 6 O)p-[R 7 O]qX 2 (3)
[0026] In the general formula (3), R 5 is H or CH3, R 5 As the radical, H is preferable.
[0027] X 2 represents a glycidyl group.
[0028] R 6 is CH2CH2. p is an integer between 1 and 3. As p, 1 or 2 is preferable.
[0029] R 7 is CH2CH2CH2CH2. q is an integer between 1 and 3. q is preferably 1 or 2.
[0030] Examples of the (meth)acrylic acid ester monomer represented by general formula (3) include glycidyl ether butylene glycol ethylene glycol ether (meth)acrylate {chemical formula weight: 244, (258)}, glycidyl ether dibutylene glycol ethylene glycol ether (meth)acrylate {chemical formula weight: 316, (330)}, and glycidyl ether butylene glycol diethylene glycol ether (meth)acrylate {chemical formula weight: 288, (302)}. The chemical formula weights of the acrylate and methacrylate are listed in succession following the compound name, and the chemical formula weight of the methacrylate is listed in parentheses.
[0031] Glycidyl ether butylene glycol ethylene glycol ether (meth)acrylate is a compound represented by the general formula (3), in which p is 1, q is 1, and X 2 Glycidyl ether dibutylene glycol ethylene glycol ether (meth)acrylate is represented by the chemical formula (3) where p is 1, q is 2, and X is a glycidyl group. 2 Glycidyl ether butylene glycol diethylene glycol ether (meth)acrylate is represented by the chemical formula (3) where p is 2, q is 1, and X is a glycidyl group. 2is represented by the chemical formula:
[0032] From the viewpoints of carbon dioxide separation function and carbon dioxide permeation rate, the chemical formula weight of the (meth)acrylic acid ester monomer (a1) is preferably 128 to 500, and more preferably 128 to 400. The chemical formula weight of the (meth)acrylic acid ester monomer (a1) can be calculated from the chemical formula of the (meth)acrylic acid ester monomer (a1).
[0033] Among them, from the viewpoint of carbon dioxide separation function and carbon dioxide permeation rate, the (meth)acrylic acid ester monomer (a1) is preferably glycidyl (meth)acrylate, {chemical formula weight: 128 (142)}, 2-hydroxyethyl (meth)acrylate glycidyl ether {chemical formula weight: 172 (186)}, 3-hydroxypropyl (meth)acrylate glycidyl ether {chemical formula weight: 186 (200)}, 2-hydroxypropyl (meth)acrylate glycidyl ether {chemical formula weight: 186 (200)}, 4-hydroxybutyl (meth)acrylate glycidyl ether {chemical formula weight: 200 (214)}, 2-hydroxybutyl (meth)acrylate glycidyl ether {chemical formula weight: 200 (214)}, and a compound represented by general formula (2), and more preferably glycidyl (meth)acrylate {chemical formula weight: 128 (142)}. As the (meth)acrylic acid ester monomer (a1), one type may be used alone, or two or more types may be used in combination.
[0034] <(Meth)acrylamide monomer (a2)> The (meth)acrylamide monomer (a2) has a chemical formula weight of 500 or less.
[0035] The (meth)acrylamide monomer (a2) includes at least one selected from the group consisting of (meth)acrylamide, N-substituted (meth)acrylamide, and N,N-disubstituted (meth)acrylamide.
[0036] Examples of N-substituted (meth)acrylamides include compounds represented by the following general formula (4).
[0037] CH2=CR 8 -C(O)-NH(R 9 ) (4)
[0038] In general formula (4), R 8 is H or CH3, R 9 represents an alkyl group having 1 to 28 carbon atoms or an aryl group having 6 to 28 carbon atoms.
[0039] R 9 Examples of the alkyl group having 1 to 28 carbon atoms represented by the formula (1) include a methyl group, an ethyl group, a linear alkyl group having 3 to 28 carbon atoms, and a branched alkyl group having 3 to 28 carbon atoms, and examples of the linear alkyl group include a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the branched alkyl group include an isopropyl group, a sec-butyl group, an isobutyl group, a tert-butyl group, an isopentyl group, a tert-pentyl group, and a 2,2-dimethylpropyl ... having 3 to 6 carbon atoms are preferable from the viewpoint of the carbon dioxide separation function and the carbon dioxide permeation rate, and a methyl group, an ethyl group, and a isopropyl group are more preferable.
[0040] R 9 Examples of the aryl group having 6 to 28 carbon atoms represented by the formula (I) include a phenyl group, a substituted phenyl group (a hydrocarbon group having one phenyl group), a hydrocarbon group having two or more phenyl groups (excluding a phenyl group and a substituted phenyl group), and a condensed polycyclic aromatic hydrocarbon group. Examples of the substituted phenyl group include a methylphenyl group and a dimethylphenyl group, and examples of the hydrocarbon group having two or more phenyl groups include a biphenyl group and a triphenylmethyl group. Examples of the condensed polycyclic aromatic hydrocarbon group include a naphthyl group and a phenanthrene group. From the viewpoint of carbon dioxide separation function and carbon dioxide permeation rate, a phenyl group and a substituted phenyl group having 6 to 12 carbon atoms are preferred, and a phenyl group and a methylphenyl group are more preferred.
[0041] Examples of compounds that can be represented by general formula (4) include N-methyl(meth)acrylamide {chemical formula weight: 85, (99)}, N-ethyl(meth)acrylamide {chemical formula weight: 99, (113)}, and N-isopropyl(meth)acrylamide {chemical formula weight: 113, (127)}. The chemical formula weights of the acrylate and methacrylate are listed following the compound name, with the chemical formula weight of the methacrylate listed in parentheses.
[0042] Examples of N,N-disubstituted (meth)acrylamides include compounds represented by the following formula (5).
[0043] CH2=CR 10 -C(O)-NR 11 (R 12 ) (5)
[0044] In general formula (5), R 10 is H or CH3, R 11 and R 12 each represents an alkyl group having 1 to 27 carbon atoms or an aryl group having 6 to 27 carbon atoms, R 11 The number of carbon atoms and R 12 The total number of carbon atoms is 2 to 28.
[0045] R 11 and R 12 Examples of the alkyl group having 1 to 27 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a linear alkyl group having 3 to 27 carbon atoms, and a branched alkyl group having 3 to 27 carbon atoms. Examples of the linear alkyl group include a propyl group, a butyl group, a pentyl group, and a hexyl group. Examples of the branched alkyl group include an isopropyl group, a sec-butyl group, an isobutyl group, a tert-butyl group, an isopentyl group, a tert-pentyl group, and a 2,2-dimethylpropyl group. From the viewpoint of the carbon dioxide separation function and the carbon dioxide permeation rate, R 11 and R 12are preferably a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, and a branched alkyl group having 3 to 6 carbon atoms, respectively, and more preferably a methyl group, an ethyl group, and an isopropyl group.
[0046] R 11 and R 12 Examples of the aryl group having 6 to 27 carbon atoms represented by the formula (I) include a phenyl group, a substituted phenyl group (a hydrocarbon group having one phenyl group), a hydrocarbon group having two or more phenyl groups (excluding a phenyl group and a substituted phenyl group), and a condensed polycyclic aromatic hydrocarbon group. Examples of the substituted phenyl group include a methylphenyl group and a dimethylphenyl group, and examples of the hydrocarbon group having two or more phenyl groups include a biphenyl group and a triphenylmethyl group. Examples of the condensed polycyclic aromatic hydrocarbon group include a naphthyl group and a phenanthrene group. Among these, from the viewpoint of carbon dioxide separation function and carbon dioxide permeation rate, a phenyl group and a substituted phenyl group having 6 to 12 carbon atoms are preferred, and a phenyl group and a methylphenyl group are more preferred.
[0047] Examples of N,N-disubstituted (meth)acrylamides represented by general formula (5) include N,N-dimethyl(meth)acrylamide {chemical formula weight: 99, (113)} and N,N-diethyl(meth)acrylamide {chemical formula weight: 127, (141)}. The chemical formula weights of the acrylate and methacrylate are listed in succession following the compound name, with the chemical formula weight of the methacrylate listed in parentheses.
[0048] The chemical formula weight of the (meth)acrylamide monomer (a2) is preferably from 71 to 500, and more preferably from 71 to 400, from the viewpoints of the carbon dioxide separating function and the carbon dioxide permeation rate.
[0049] From the viewpoint of carbon dioxide separation function and carbon dioxide permeation rate, the (meth)acrylamide-based monomer (a2) having a chemical formula weight of 500 or less is preferably (meth)acrylamide {chemical formula weight: 71, (85)}, N-isopropyl(meth)acrylamide {chemical formula weight: 113, (127)}, and N,N-dimethyl(meth)acrylamide {chemical formula weight: 99, (113)}, and more preferably N,N-dimethyl(meth)acrylamide {chemical formula weight: 99, (113)}. As the (meth)acrylamide monomer (a2), one type may be used alone, or two or more types may be used in combination.
[0050] <Copolymer (A)> Copolymer (A) contains, as essential constituent monomers, a (meth)acrylic acid ester monomer (a1) having a glycidyl group and a chemical formula weight of 500 or less, and a (meth)acrylamide monomer (a2) having a chemical formula weight of 500 or less. In addition, there is no limitation on the order of bonding of the monomers constituting copolymer (A), and it may be a block polymer or a random polymer.
[0051] The copolymer (A) may contain at least one (meth)acrylic acid ester monomer (a1) and at least one (meth)acrylamide monomer (a2) as monomers, and two or more types of each of the (meth)acrylic acid ester monomer (a1) and the (meth)acrylamide monomer (a2) may be used.
[0052] The copolymer (A) may contain another monomer (a3) as a monomer. Preferred examples of the other monomer (a3) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate.
[0053] In the copolymer (A) of the present invention, the polymerization ratio of the (meth)acrylic acid ester monomer (a1) based on the total weight of the (meth)acrylic acid ester monomer (a1) and the (meth)acrylamide monomer (a2) is preferably 5 to 30% by weight, and more preferably 15 to 20% by weight, from the viewpoints of carbon dioxide separation function and carbon dioxide permeation rate.
[0054] When the copolymer (A) contains another monomer (a3) as a monomer, the weight proportion of the other monomer (a3) is preferably 0.1 to 10% by weight based on the total weight of the (meth)acrylic acid ester monomer (a1), the (meth)acrylamide monomer (a2) and the other monomer (a3).
[0055] Examples of the copolymer (A) include poly(N,N-dimethyl(meth)acrylamide-co-glycidyl(meth)acrylate), poly(N-isopropyl(meth)acrylamide-co-glycidyl(meth)acrylate), poly((meth)acrylamide-co-glycidyl(meth)acrylate), poly(N,N-dimethyl(meth)acrylamide-co-4-hydroxybutyl(meth)acrylate glycidyl ether), poly(N-isopropyl(meth)acrylamide-co-4-hydroxybutyl(meth)acrylate glycidyl ether), and poly(( From the viewpoint of suppressing the exudation of the room-temperature molten salt (B) from the gel, preferred are poly(N,N-dimethyl(meth)acrylamide-co-glycidyl(meth)acrylate), poly(N-isopropyl(meth)acrylamide-co-glycidyl(meth)acrylate), and poly((meth)acrylamide-co-glycidyl(meth)acrylate), and more preferred are poly(N,N-dimethylacrylamide-co-glycidyl methacrylate).
[0056] In the copolymer (A), it is preferable that the (meth)acrylic acid ester monomer (a1) is glycidyl (meth)acrylate, and the (meth)acrylamide monomer (a2) is N,N-dimethyl (meth)acrylamide. The copolymer (A) may be a copolymer containing only glycidyl (meth)acrylate and N,N-dimethyl (meth)acrylamide as constituent monomers.
[0057] When the copolymer (A) is poly(N,N-dimethylacrylamide-co-glycidyl methacrylate), the weight proportion of glycidyl methacrylate, which is the (meth)acrylic acid ester monomer (a1), is preferably 5 to 30% by weight based on the total weight of N,N-dimethylacrylamide and glycidyl methacrylate.
[0058] The weight average molecular weight of the copolymer (A) of the present invention is preferably 50,000 to 5,000,000, and more preferably 100,000 to 2,000,000, from the viewpoints of carbon dioxide separation function and carbon dioxide permeation rate. The weight average molecular weight of the copolymer (A) can be measured by gel permeation chromatography (GPC) under the following conditions, and in the examples, Mw was determined by GPC under the following measurement conditions.
[0059] <Measurement conditions for weight average molecular weight (Mw) of copolymer (A)> Equipment: "HLC-8320" [Tosoh Corporation] Column: "TSK GEL α-M" [manufactured by Tosoh Corporation] Measurement temperature: 40℃ Sample solution: 0.25% by weight N,N-dimethylformamide solution (insoluble matter was filtered off using a glass filter) Solution injection volume: 100μl Detector: Refractive index detector Reference material: 12 standard polystyrenes (TSKstandard POLYSTYRENE) (molecular weight: 500, 1,050, 2,800, 5,970, 9,100, 18,100, 37,900, 96,400, 190,000, 355,000, 1,090,000, 2,890,000) [manufactured by Tosoh Corporation]
[0060] The copolymer (A) can be produced by a known method, among which a solution polymerization method is preferred.
[0061] An example of the solution polymerization method is a method in which a monomer composition (a monomer composition containing a (meth)acrylic acid ester monomer (a1), a (meth)acrylamide monomer (a2), and other monomers (a3) used as necessary) and a polymerization initiator (azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile, etc.) are dropped into a solvent such as ethyl acetate to polymerize. The polymerization temperature is preferably 60 to 230°C, more preferably 70 to 180°C, from the viewpoint of protecting the glycidyl group.
[0062] <Room temperature molten salt (B)> The gel-forming composition of the present invention contains an ambient-temperature molten salt (B). The room-temperature molten salt (B) comprises an anion and an organic cation.
[0063] The organic cation is preferably a cation represented by the following general formula (1).
[0064] [ka]
[0065] In general formula (1), R 1 and R 2 each independently represents an alkyl group having 1 to 6 carbon atoms.
[0066] R 1 and R 2Examples of the alkyl group having 1 to 6 carbon atoms represented by the formula (1) include linear alkyl groups having 1 to 6 carbon atoms and branched alkyl groups having 3 to 6 carbon atoms, and examples of the linear alkyl groups include methyl, ethyl, propyl, butyl, pentyl, and hexyl groups, and examples of the branched alkyl groups include isopropyl, sec-butyl, isobutyl, tert-butyl, isopentyl, tert-pentyl, and 2,2-dimethylpropyl groups. Among these, the methyl group, ethyl group, and branched alkyl groups having 3 to 4 carbon atoms are preferred from the viewpoints of carbon dioxide separation function and carbon dioxide permeation rate, and the methyl group and the ethyl group are more preferred.
[0067] Examples of the cation include 1,3-dimethyl-imidazolium cation, 1,3-diethyl-imidazolium cation, 1-ethyl-3-methylimidazolium cation, 1-propyl-3-methylimidazolium cation, 1-butyl-3-methylimidazolium cation, and 1-hexyl-3-methylimidazolium cation. Among these, from the viewpoints of carbon dioxide separation function and carbon dioxide permeation rate, the 1-ethyl-3-methylimidazolium cation, the 1,3-dimethyl-imidazolium cation, the 1,3-diethyl-imidazolium cation and the 1-butyl-3-methylimidazolium cation are preferred, and the 1-ethyl-3-methylimidazolium cation is more preferred.
[0068] There are no particular limitations on the anion, so long as it can form a room-temperature molten salt in combination with an organic cation.
[0069] The anion is PF6 - , BF4 - , BF3(CF3) - , F - , Cl - , Br - , I - , AlCl4 - , Al2Cl7 - , NO3 - , (NC)2N - , (FSO2)2N -, (CF3SO2)2N - , (CF3CF2SO2)2N - , (CF3SO2)3C - , CH3COO - , CH3CH2COO - , (CH3)3CCOO - , (CH3O)CH2COO - , CF3COO - , CF3CF2CF2COO - , CF3SO3 - , CF3(CF2)3SO3 - , AsF6 - , and SbF6 - etc.
[0070] From the viewpoint of carbon dioxide separation function and carbon dioxide permeation rate, the anion is preferably BF4 - , (NC)2N - , (FSO2)2N - , (CF3SO2)2N - , (CF3CF2SO2)2N - , (CF3SO2)3C - , CH3COO - , CH3CH2COO - , (CH3)3CCOO - , and (CH3O)CH2COO - and more preferably BF4 - [Tetrafluoroborate], (FSO2)2N - [Bis(fluorosulfonyl)imide], (NC)2N - [Dicyanamide] and CH3CH2COO - [Propionate].
[0071] As the room-temperature molten salt (B), from the viewpoints of carbon dioxide separation function and carbon dioxide permeation rate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium dicyanamide, and 1-ethyl-3-methylimidazolium propionate are preferred. The composition for absorbing acidic gas of the present invention may contain two or more kinds of room-temperature molten salts (B).
[0072] The room-temperature molten salt (B) can be produced by a known method, for example, the alkyl halide method, the dialkyl carbonate method, the direct alkylation method, or the like.
[0073] <Other ingredients (C)> The first layer may contain components other than the copolymer (A) and the room temperature molten salt (B) (hereinafter, other components (C)). Examples of other components (C) include crosslinking agents, thickeners, crosslinking reaction catalysts, solvents, and other additives. The crosslinking agent referred to here is a polyfunctional compound that reacts with two or more glycidyl groups.
[0074] Examples of the crosslinking agent include ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, oxalic acid, succinic acid, adipic acid, azelaic acid, and dodecanedioic acid. From the viewpoints of carbon dioxide separation function and carbon dioxide permeation rate, preferred crosslinking agents are ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and pentaethylenehexamine, and preferably pentaethylenehexamine.
[0075] Thickening agents include polyvinyl alcohol, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, xanthan gum, and the like.
[0076] Crosslinking reaction catalysts include salicylic acid, glycolic acid, and 1,8-diazabicyclo[5.4.0]-7-undecene.
[0077] Examples of the solvent include ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, etc. From the viewpoint of the solubility of the gel-forming composition in the solvent, preferred solvents are ethyl acetate, methanol, ethanol, 1-propanol, 2-propanol, and 1-butanol, and more preferred are ethyl acetate, 2-propanol, and methanol.
[0078] Other additives include wetting agents, etc. Examples of wetting agents include KP-112 (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0079] In the first layer, the weight of the room-temperature molten salt (B) is 95% by weight or less based on the total weight of the copolymer (A) and the room-temperature molten salt (B). The weight of the room-temperature molten salt (B) is preferably 80% by weight or more and 95% by weight or less based on the total weight of the copolymer (A) and the room-temperature molten salt (B).
[0080] In the first layer, the weight of the copolymer (A) is 5% by weight or more based on the total weight of the copolymer (A) and the room-temperature molten salt (B). The weight of the copolymer (A) is preferably 5% by weight or more and 20% by weight or less based on the total weight of the copolymer (A) and the room-temperature molten salt (B).
[0081] The thickness of the first layer is not particularly limited, but from the viewpoints of the carbon dioxide separation function and the carbon dioxide permeation rate, it is preferably 20 μm or less.
[0082] [Second layer] The second layer is a porous thin film and supports the first layer through an intermediate layer. Examples of the second layer include ultrafiltration membranes, nonwoven fabrics, porous polytetrafluoroethylene, aromatic polyamide fibers, porous metals, sintered metals, porous ceramics, porous polyesters, porous nylons, activated carbon fibers, latex, silicones, silicone rubbers, permeable (porous) polymers, open or closed cell metal foams, open or closed cell polymer foams, silica, porous glass, mesh screens, etc. The second layer may be a combination of two or more of these.
[0083] The permeable (porous) polymer may be at least one selected from the group consisting of polyvinyl fluoride, polyvinylidene fluoride, polyurethane, polypropylene, polyethylene, polystyrene, polycarbonate, polysulfone, polyether ether ketone, polyacrylonitrile, polyimide, and polyphenylene oxide.
[0084] The thickness of the second layer is not particularly limited and is, for example, 10 μm or more, preferably 20 μm or more, and more preferably 50 μm or more. The thickness of the second layer is, for example, 300 μm or less, preferably 200 μm or less, and more preferably 150 μm or less.
[0085] The pore size of the second layer is preferably 0.001 to 1.0 μm, and more preferably 0.01 to 0.4 μm. If the pore size is smaller than 0.001 μm, gas permeability is hindered, and if the pore size is larger than 1.0 μm, the intermediate layer may penetrate into the pores of the second layer.
[0086] [Middle layer] The intermediate layer includes a silicone resin. Examples of the silicone resin include silicone rubber, silicone adhesive, and polytrimethylsilylpropyne (PTMSP). In this specification, silicon-containing polyacetylene such as polytrimethylsilylpropyne (PTMSP) is also included in the silicone resin.
[0087] The thickness of the intermediate layer is not particularly limited, and is, for example, less than 50 μm, preferably 40 μm or less, and more preferably 30 μm or less. The thickness of the intermediate layer is, for example, 0.5 μm or more, and may be 1 μm or more.
[0088] [Method of manufacturing carbon dioxide separation membrane] An example of a method for producing a carbon dioxide separation membrane is described below. The method for producing a carbon dioxide separation membrane is not limited to the following method, and any method may be used as long as the above-mentioned carbon dioxide separation membrane can be obtained. First, a 6 wt% decane solution of silicone resin (YSR3022 manufactured by Momentive Performance Materials) was applied onto the porous support. The porous support will be the second layer of the carbon dioxide separation membrane of the present invention. An ultrafiltration membrane (NTU-3175M manufactured by Nitto Denko Corporation) was used as the porous support. The decane solution was applied using a roll coater, adjusting the thickness so that the film thickness of the intermediate layer after drying would be a desired value. Next, the obtained coating film was dried at 130°C for 5 minutes. This resulted in a laminate consisting of the intermediate layer and the second layer. Next, a coating liquid containing the material of the first layer was prepared. The coating liquid was applied onto the film consisting of the intermediate layer and the second layer to obtain a coating film. The method of applying the coating liquid is not particularly limited, and for example, a spin coating method can be used. The thickness of the first layer formed from the coating film can be adjusted by adjusting the rotation speed of the spin coater, the concentration of the material of the first layer in the coating liquid, and the like. Next, the coating film was dried to form the first layer. The drying of the coating film can be performed, for example, under heating conditions. The heating temperature of the coating film is, for example, not less than 50° C. The heating time of the coating film is, for example, not less than 120 minutes, and may be not less than 300 minutes.
[0089] [Carbon dioxide transmission rate] The carbon dioxide separation membrane of the present invention can efficiently separate gases, and therefore can easily increase the carbon dioxide permeation rate. The carbon dioxide permeation rate Q is, for example, 50 GPU or more, and preferably 80 GPU or more. -6 ·cm 3(STP) / (sec cm 2 cm 3 (STP) means the volume of carbon dioxide at 1 atmosphere and 0° C. The carbon dioxide permeation rate Q is calculated by the following method.
[0090] First, a mixed gas consisting of carbon dioxide and hydrogen is supplied to a space adjacent to one side of the separation membrane (e.g., the main surface of the first layer side of the separation membrane). As a result, a permeated fluid that has permeated the separation membrane is obtained in a space adjacent to the other side of the separation membrane (e.g., the main surface of the second layer of the separation membrane). The weight of the permeated fluid, as well as the volume ratio of carbon dioxide and the volume ratio of hydrogen in the permeated fluid are measured. From the measurement results, the permeation rate Q can be calculated using formula (1) described in the examples. In the above operation, the concentration of carbon dioxide in the mixed gas is 50 vol% under standard conditions (0°C, 1 atm). The mixed gas supplied to the space adjacent to one side of the separation membrane has a temperature of 30°C and a pressure of 0.1 MPa.
[0091] [Carbon dioxide separation membrane module] The carbon dioxide separation membrane module of the present invention has the carbon dioxide separation membrane of the present invention. The shape of the carbon dioxide separation membrane module is not particularly limited, and may be a spiral type formed by winding a flat separation membrane in a spiral shape.
[0092] The present specification discloses the following:
[0093] The present disclosure (1) is a carbon dioxide separation membrane comprising a first layer, a porous second layer, and an intermediate layer containing a silicone resin and disposed between the first layer and the second layer, wherein the first layer is a layer containing a copolymer (A) having, as essential constituent monomers, a (meth)acrylic acid ester-based monomer (a1) having a glycidyl group and a chemical formula weight of 500 or less, and a (meth)acrylamide-based monomer (a2) having a chemical formula weight of 500 or less, and a room temperature molten salt (B) composed of an anion and an organic cation, wherein the (meth)acrylamide-based monomer (a2) is at least one amide selected from the group consisting of (meth)acrylamide, N-substituted (meth)acrylamide, and N,N-disubstituted (meth)acrylamide, and the weight of the room temperature molten salt (B) is 95% by weight or less based on the total weight of the copolymer (A) and the room temperature molten salt (B).
[0094] The present disclosure (2) is the carbon dioxide separation membrane according to the present disclosure (1), wherein the organic cation is a cation represented by the following general formula (1): [In general formula (1), R 1 and R 2 each independently represents an alkyl group having 1 to 6 carbon atoms.] [ka]
[0095] The present disclosure (3) is the carbon dioxide separation membrane according to the present disclosure (1) or (2), in which the (meth)acrylic acid ester-based monomer (a1) is glycidyl (meth)acrylate, and the (meth)acrylamide-based monomer (a2) is N,N-dimethyl(meth)acrylamide.
[0096] The present disclosure (4) is the carbon dioxide separation membrane according to any one of the present disclosures (1) to (3), in which the polymerization ratio of the (meth)acrylic acid ester-based monomer (a1) is 5 to 30 weight % based on the total weight of the (meth)acrylic acid ester-based monomer (a1) and the (meth)acrylamide-based monomer (a2).
[0097] The present disclosure (5) is the carbon dioxide separation membrane according to any one of the present disclosures (1) to (4), wherein the weight of the room temperature molten salt (B) is 80% by weight or more and 95% by weight or less with respect to the total weight of the copolymer (A) and the room temperature molten salt (B).
[0098] The present disclosure (6) is the carbon dioxide separation membrane according to any one of the present disclosures (1) to (5), wherein the first layer has a thickness of 20 μm or less.
[0099] The present disclosure (7) is a carbon dioxide separation membrane module having the carbon dioxide separation membrane according to any one of the present disclosures (1) to (6). EXAMPLES
[0100] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples unless it deviates from the gist of the present invention. In the following description, "parts" means parts by weight unless otherwise specified.
[0101] <Production Example 1: Production of Copolymer (A-1)> A reaction vessel equipped with a thermometer, a stirrer, a reflux condenser, and a nitrogen inlet was charged with 140 parts of ethyl acetate, and the air in the reaction vessel was replaced with nitrogen gas while stirring, and then the mixture was heated to reflux. Next, a mixture of 89.3 parts of N,N-dimethylacrylamide, 15.7 parts of glycidyl methacrylate, 112 parts of ethyl acetate, and 0.1 parts of 2,2'-azobis(2-methylbutyronitrile) was added dropwise over 3 hours to polymerize. The reaction was continued for 2 hours while heating to reflux. The solvent was removed under reduced pressure, and poly(N,N-dimethylacrylamide-co-glycidyl methacrylate) (weight average molecular weight: about 1 million) was obtained.
[0102] <Production Example 2: Production of Copolymer (A-2)> A reaction vessel equipped with a thermometer, a stirrer, a reflux condenser, and a nitrogen inlet was charged with 140 parts of ethyl acetate, and the air in the reaction vessel was replaced with nitrogen gas while stirring, and then the mixture was heated to reflux. Next, a mixture of 84 parts of N,N-dimethylacrylamide, 21 parts of glycidyl methacrylate, 112 parts of ethyl acetate, and 0.1 parts of 2,2'azobis(2-methylbutyronitrile) was added dropwise over 3 hours to polymerize. The reaction was continued for another 2 hours while heating to reflux. The solvent was then removed under reduced pressure, and poly(N,N-dimethylacrylamide-co-glycidyl methacrylate) (weight average molecular weight: about 1 million) was obtained.
[0103] <Production Example 3: Production of Room Temperature Molten Salt (B-2)> A mixture of 18 parts by weight of glyoxal (40% aqueous solution) and 10 parts by weight of formalin (37% aqueous solution) was charged into a reaction flask equipped with a stirrer, a thermometer, a dropping funnel, a reflux condenser, and a nitrogen gas inlet tube, and the mixture was stirred to form a homogeneous solution, and heated to 40° C. while flowing a small amount of nitrogen gas. After that, a mixture of 64 parts by weight of ethylamine (70% aqueous solution) and 61 parts by weight of ammonia (28% aqueous solution) was dropped from the dropping funnel while maintaining the reaction temperature at 35 to 45° C. Next, 35 minutes after the start of the dropwise addition of the mixed solution of ethylamine and ammonia, a mixed solution of 127 parts by weight of glyoxal (40% aqueous solution) and 71 parts by weight of formalin (37% aqueous solution) was dropped from another dropping funnel over 4 hours. The mixed solution of ethylamine and ammonia was dropped over 4 hours and 35 minutes, and the drop start time was shifted so that the drop of the mixed solution of glyoxal and formalin was completed at the same time as the drop of the mixed solution of ethylamine and ammonia was completed. After the dropwise addition was completed, the reaction was continued for another hour at 40°C. Next, the temperature was kept at 80°C, and the pressure was gradually reduced from normal pressure to a reduced pressure of 5.3 kPa to perform dehydration, and crude 1-ethylimidazole was obtained. Next, the mixture was purified by simple distillation at a temperature of 100°C and a reduced pressure of 0.7 kPa to obtain 1-ethylimidazole. Next, 96 parts by weight of the obtained 1-ethylimidazole, 135 parts by weight of dimethyl carbonate, and 192 parts by weight of methanol were charged into a stainless steel autoclave equipped with a reflux condenser and dissolved uniformly. The temperature was then raised to 150°C. The reaction was carried out at a pressure of about 0.8 MPa for 70 hours to obtain a reaction product. 1 H-NMR analysis revealed that 1-ethyl-3-methylimidazolium monomethyl carbonate was produced. 423 parts by weight of the resulting reaction product (salt purity 44% by weight) was placed in a flask, and 74 parts by weight of propionic acid was gradually added dropwise at room temperature over about 30 minutes while stirring. Carbon dioxide bubbles were generated during the dropwise addition. After the dropwise addition was completed and the generation of bubbles subsided, the reaction liquid was transferred to a rotary evaporator and the entire amount of the solvent was distilled off. 184 parts by weight of a colorless, transparent liquid was obtained in the flask. This liquid 1 H-NMR analysis revealed that the compound was 1-ethyl-3-methylimidazolium propionate.
[0104] <Example 1> A 6 wt% decane solution of silicone resin (YSR3022 manufactured by Momentive Performance Materials) was applied onto the porous support. The porous support will be the second layer of the carbon dioxide separation membrane. An ultrafiltration membrane (NTU-3175M manufactured by Nitto Denko Corporation) was used as the porous support. The decane solution was applied using a roll coater, with the thickness adjusted so that the film thickness of the intermediate layer after drying would be 0.6 μm. Next, the resulting coating film was dried at 130 ° C for 5 minutes. This resulted in a laminate consisting of the intermediate layer and the second layer. Next, a coating solution containing the material of the first layer listed in Table 1 was prepared. The coating solution was applied onto the laminate consisting of the intermediate layer and the second layer, and the solution was applied by spin coating. The rotation speed of the spin coater was set to 1000 rpm. Next, the film coated with the material of the first layer was dried at 60 ° C for 300 minutes to harden the material of the first layer to form the first layer, and a carbon dioxide separation membrane was obtained. In Example 1, a carbon dioxide separation membrane was obtained in which the first layer had a thickness of 1.7 μm after curing.
[0105] <Example 2> A separation membrane was obtained in the same manner as in Example 1, except that the coating conditions for the first layer (the rotation speed of the spin coater) in Example 1 was changed to 500 rpm. In Example 2, a carbon dioxide separation membrane having a thickness of 1.9 μm after the first layer was cured was obtained.
[0106] <Example 3> A separation membrane was obtained in the same manner as in Example 1, except that the coating conditions for the first layer (the rotation speed of the spin coater) in Example 1 was changed to 200 rpm. In Example 3, a carbon dioxide separation membrane was obtained in which the first layer had a thickness of 3.4 μm after curing.
[0107] <Example 4> A separation membrane was obtained in the same manner as in Example 1, except that the curing conditions for the first layer in Example 1 were changed to drying at 80° C. for 60 minutes and then drying at 150° C. for 60 minutes. In Example 4, a carbon dioxide separation membrane having a membrane thickness of 1.3 μm after the first layer was cured was obtained.
[0108] <Example 5> A separation membrane was obtained in the same manner as in Example 1, except that the solvent for the first layer in Example 1 was changed to methanol and ethyl acetate in the amounts shown in Table 1. In Example 5, a carbon dioxide separation membrane having a first layer with a thickness of 2.1 μm after curing was obtained.
[0109] <Example 6> A 6 wt% decane solution of silicone resin (YSR3022 manufactured by Momentive Performance Materials) was applied onto the porous support. The porous support will be the second layer of the carbon dioxide separation membrane. An ultrafiltration membrane (NTU-3175M manufactured by Nitto Denko Corporation) was used as the porous support. The decane solution was applied using a roll coater, with the thickness adjusted so that the thickness of the intermediate layer after drying would be 2.0 μm. Next, the resulting coating film was dried at 130 ° C for 5 minutes. This resulted in a laminate consisting of the intermediate layer and the second layer. Next, a coating solution containing the material of the first layer listed in Table 1 was prepared. The coating solution was applied onto the laminate consisting of the intermediate layer and the second layer, and the solution was applied by spin coating. The rotation speed of the spin coater was set to 1000 rpm. Next, the film coated with the material of the first layer was dried at 80 ° C for 60 minutes, and then dried at 150 ° C for 60 minutes to harden the material of the first layer, thereby forming the first layer, and a carbon dioxide separation membrane was obtained. In Example 6, a carbon dioxide separation membrane was obtained in which the first layer had a thickness of 2.0 μm after curing.
[0110] <Example 7> A separation membrane was obtained in the same manner as in Example 6, except that the material of the first layer in Example 6 was changed to that shown in Table 1. In Example 7, a carbon dioxide separation membrane having a first layer with a thickness of 1.9 μm after curing was obtained.
[0111] <Example 8> A separation membrane was obtained in the same manner as in Example 6, except that the material of the first layer in Example 6 was changed to that shown in Table 1. In Example 8, a carbon dioxide separation membrane having a first layer with a thickness of 1.2 μm after curing was obtained.
[0112] <Example 9> A separation membrane was obtained in the same manner as in Example 6, except that the material of the first layer in Example 6 was changed to that shown in Table 1 and the coating conditions for the first layer (spin coater rotation speed) was changed to 500 rpm. In Example 9, a carbon dioxide separation membrane was obtained in which the first layer had a thickness of 1.8 μm after curing.
[0113] <Example 10> A separation membrane was obtained in the same manner as in Example 1, except that the material of the first layer in Example 1 was changed to that shown in Table 1. In Example 10, a carbon dioxide separation membrane was obtained in which the first layer had a thickness of 0.4 μm after curing.
[0114] <Comparative Example 1> A coating solution containing the material of the first layer shown in Table 1 was prepared. Next, the coating solution was applied onto an ultrafiltration membrane (NITTO DENKO CORPORATION NTU-3175M) by spin coating. The rotation speed of the spin coater was set to 1000 rpm. Next, the membrane was dried at 60°C for 300 minutes to form a first layer. The film thickness of the first layer after curing was 15 μm. The separation membrane of Comparative Example 1 does not include an intermediate layer.
[0115] <Comparative Example 2> A coating solution containing the material for the first layer shown in Table 1 was prepared. Next, a frame made of silicone rubber was placed on a release-treated PET film (SG2 manufactured by PANAC Corporation) and the solution was poured into the inside. It was dried at 60°C for 300 minutes to produce a sheet consisting of only the first layer. The film thickness of the first layer after curing was set to 210 μm.
[0116] <Comparative Example 3> A sheet consisting of only a first layer was produced in the same manner as in Comparative Example 2, except that the thickness of the first layer after curing was changed to 302 μm.
[0117] <Comparative Example 4> A sheet consisting of only a first layer was produced in the same manner as in Comparative Example 2, except that the thickness of the first layer after curing was changed to 318 μm.
[0118] [Measurement and Evaluation] For each of Examples 1 to 10 and Comparative Examples 1 to 4, the initial separation performance (permeation rate, permeation coefficient, gas selectivity) was evaluated and is shown in Table 1. The permeation coefficient and selectivity are calculated as follows.
[0119] <Gas permeability test> First, the separation membrane was set in the metal cell and sealed with an O-ring to prevent leakage. Next, the mixed gas was injected into the metal cell so that the mixed gas contacted one main surface of the separation membrane. The mixed gas was substantially composed of only carbon dioxide and hydrogen. The concentration of carbon dioxide in the mixed gas was 50 vol% under standard conditions. The mixed gas injected into the metal cell had a temperature of 30°C and a pressure of 0.1 MPa. Next, the space in the metal cell adjacent to the other main surface of the separation membrane was depressurized by a vacuum pump. At this time, the pressure in this space was depressurized so that the pressure in the space was 0.1 MPa lower than the atmospheric pressure in the measurement environment. As a result, a permeated fluid was obtained from the other main surface of the separation membrane. The permeation coefficient and separation coefficient were calculated based on the composition of the obtained permeated fluid, the weight of the permeated fluid, and the like.
[0120] <Permeation rate and permeation coefficient> The amount of gas permeated N was calculated from the gas concentration in the permeation side gas flowing through the gas chromatography, and the CO2 permeation rate Q was calculated from the following formulas (1) and (2). CO2 and H2 permeation rate Q H2 was calculated.
number
number
number
number
number
number
[0121] <Gas selectivity> The separation factor α was calculated by the following formula (7).
number
[0122] [Table 1]
[0123] In addition to Production Examples 1, 2 and 3, the chemicals used in the Examples and Comparative Examples shown in Table 1 are as follows. <Room temperature molten salt (B)> Room temperature molten salt (B-1): 1-ethyl-3-methylimidazolium dicyanamide (BASF) <Crosslinking agent> Pentaethylenehexamine (Tokyo Chemical Industry Co., Ltd.) <Solvent> Ethyl acetate (Tokyo Chemical Industry Co., Ltd.) Methanol (Tokyo Chemical Industry Co., Ltd.) 2-Propanol (Tokyo Chemical Industry Co., Ltd.) <Wetting agent> KP-112 (Shin-Etsu Chemical Co., Ltd.)
[0124] As shown in Table 1, the separation membranes according to the examples had a higher gas selectivity for carbon dioxide and a higher carbon dioxide permeation rate than the comparative examples, and therefore separated a larger amount of carbon dioxide efficiently. [Industrial Applicability]
[0125] According to the present invention, a carbon dioxide separation membrane and a carbon dioxide separation membrane module having a sufficient carbon dioxide separation function and carbon dioxide permeation rate can be obtained by a simple procedure. Therefore, the carbon dioxide separation membrane and carbon dioxide separation membrane module of the present invention can be used for separating acidic gases such as carbon dioxide contained in exhaust gases from chemical plants, steelworks, etc., producing energy resources (natural gas, biogas, synthetic gas) by removing carbon dioxide, and removing carbon dioxide from distributed emission sources such as automobiles, but are not limited to these exemplified fields.
Claims
1. The first layer, a porous second layer; disposed between the first layer and the second layer, and an intermediate layer containing a silicone resin. the first layer is a copolymer (A) containing, as essential constituent monomers, a (meth)acrylic acid ester monomer (a1) having a glycidyl group and a chemical formula weight of 500 or less, and a (meth)acrylamide monomer (a2) having a chemical formula weight of 500 or less; a room-temperature molten salt (B) composed of an anion and an organic cation; The (meth)acrylamide monomer (a2) is at least one amide selected from the group consisting of (meth)acrylamide, N-substituted (meth)acrylamide, and N,N-disubstituted (meth)acrylamide, A carbon dioxide separation membrane, wherein the weight of the room temperature molten salt (B) is 95% by weight or less based on the total weight of the copolymer (A) and the room temperature molten salt (B).
2. The carbon dioxide separation membrane according to claim 1 , wherein the organic cation is a cation represented by the following general formula (1): [In general formula (1), R 1 and R 2 each independently represents an alkyl group having 1 to 6 carbon atoms. 【Chemistry 1】
3. The carbon dioxide separation membrane according to claim 1, wherein the (meth)acrylic acid ester monomer (a1) is glycidyl (meth)acrylate, and the (meth)acrylamide monomer (a2) is N,N-dimethyl(meth)acrylamide.
4. The (meth)acrylic acid ester monomer (a1) has a polymerization ratio of 5 to 30% by weight based on the total weight of the (meth)acrylic acid ester monomer (a1) and the (meth)acrylamide monomer (a2). The carbon dioxide separation membrane according to claim 1.
5. 2. The carbon dioxide separation membrane according to claim 1, wherein the weight of the room temperature molten salt (B) is 80% by weight or more and 95% by weight or less with respect to the total weight of the copolymer (A) and the room temperature molten salt (B).
6. 2. The carbon dioxide separation membrane according to claim 1, wherein the first layer has a thickness of 20 μm or less.
7. A carbon dioxide separation membrane module comprising the carbon dioxide separation membrane according to any one of claims 1 to 6.
Citation Information
Patent Citations
V belt type stepless transmission
JP1983077961A
Ionic liquid-containing gelatinous composition, gelatinous thin film, and method for manufacturing the same
JP2013060504A
Gas separation membrane and manufacturing method
JP2015160159A