Laminated electronic component

A lattice-like groove pattern on the surface of multilayer ceramic capacitors enhances bonding force, addressing miniaturization and capacity challenges while reducing delamination, resulting in reliable and compact capacitors.

JP2024146696APending Publication Date: 2024-10-15SAMSUNG ELECTRO MECHANICS CO LTD

Patent Information

Application Number
JP2023139985
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-08-30
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing multilayer ceramic capacitors face challenges in achieving miniaturization and high capacity while maintaining reliability, and there is a risk of delamination between the main body and external electrodes due to insufficient bonding force.

Method used

A multilayer electronic component with a lattice-like groove shape on its surface is formed to enhance the interfacial bonding force between the main body and external electrodes, using a laser to create a pattern that increases the surface area for improved adhesion.

Benefits of technology

The solution enables the production of smaller, higher-capacity capacitors with enhanced reliability by reducing the risk of delamination and improving the bonding force between the ceramic body and external electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146696000001_ABST
    Figure 2024146696000001_ABST
Patent Text Reader

Abstract

To achieve miniaturization and higher capacity of laminated electronic components, improve reliability, and prevent delamination or floating between a body and external electrodes.SOLUTION: A laminated electronic component includes a body that includes a dielectric layer and internal electrodes and external electrodes that are arranged on the body. A grid-shaped groove pattern can be formed on at least a portion of a surface of the body, which has multiple grooves arranged in a grid pattern.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer electronic component. [Background technology]

[0002] Multi-layered ceramic capacitors (MLCCs), which are one type of multi-layered electronic component, are chip-type capacitors that are mounted on printed circuit boards of various electronic products such as visual devices such as liquid crystal displays (LCDs) and plasma display panels (PDPs), computers, smartphones, and mobile phones to charge and discharge electricity.

[0003] Such multilayer ceramic capacitors have the advantages of being small yet high capacitance and easy to mount, and can be used as components of various electronic devices. As various electronic devices such as computers and mobile devices become smaller and have higher output, there is an increasing demand for multilayer ceramic capacitors to be smaller and have higher capacitance.

[0004] On the other hand, methods for simultaneously achieving miniaturization and high capacity of multilayer electronic components include using a material with a high dielectric constant, reducing the thickness of the dielectric layer or the internal electrode layer, etc. However, if the thickness of the dielectric layer is reduced too much, problems such as a decrease in the breakdown voltage (BDV) and deterioration in reliability may occur.

[0005] Therefore, by applying a method of thinning the external electrodes, the volume of the portions that are not directly related to the capacitance of the multilayer electronic component can be minimized and the effective volume can be maximized. Methods of thinning the external electrodes include forming the external electrodes with a plating film or applying a thin film deposition method such as sputtering, but when the external electrodes are formed by such methods, the bonding strength with the ceramic body is insufficient, and delamination between the body and the external electrodes may occur.

[0006] To solve these problems, research is being conducted on various pretreatments, such as forming surface roughness on the body or forming other materials on the body to facilitate bonding between the ceramic body and the external electrodes. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Korean Patent Publication No. 10-2021-0033132 [Patent Document 2] Korean Patent Publication No. 10-2022-0063556 Summary of the Invention [Problem to be solved by the invention]

[0008] One of the problems to be solved by the present invention is to achieve miniaturization and high capacity of a multilayer electronic component.

[0009] One of the problems that the present invention aims to solve is to improve the reliability of multilayer electronic components.

[0010] One of the problems that the present invention aims to solve is to suppress the delamination or lifting phenomenon between the main body and the external electrode.

[0011] However, some of the problems that the present invention aims to solve are not limited to the above content, and can be more easily understood in the process of describing specific embodiments of the present invention. [Means for solving the problem]

[0012] A multilayer electronic component according to one embodiment of the present invention includes a body including a dielectric layer and an internal electrode, and an external electrode disposed on the body, and at least a portion of a surface of the body may be formed with a lattice-like groove shape having a plurality of grooves arranged in a lattice pattern. Effect of the Invention

[0013] One of the various effects of the present invention is that it is possible to achieve miniaturization and high capacity of a multilayer electronic component.

[0014] One of the various effects of the present invention is to improve the reliability of the multilayer electronic component.

[0015] One of the many advantages of the present invention is that it improves the interfacial bond between the body and the external electrode.

[0016] However, the various yet significant advantages and effects of the present invention are not limited to the above, and can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0017] [Figure 1] 1 is a schematic perspective view of a multilayer electronic component according to an embodiment of the present invention; [Diagram 2] 2 is a schematic perspective view of the multilayer electronic component of FIG. 1 with external electrodes removed. [Diagram 3] 2 is a schematic exploded perspective view showing a laminated structure of internal electrodes; FIG. [Figure 4] 2 is a schematic cross-sectional view taken along line II' of FIG. 1. [Diagram 5] 2 is a schematic cross-sectional view taken along line II-II' in FIG. 1. [Figure 6] 1 is a schematic cross-sectional view taken along line II' of another embodiment of the present invention; [Figure 7] 1 is a schematic cross-sectional view taken along line II' of another embodiment of the present invention; [Figure 8] 1 is a schematic cross-sectional view taken along line II' of another embodiment of the present invention; [Figure 9] 1 is a schematic cross-sectional view taken along line II' of another embodiment of the present invention; [Figure 10] 5 is a schematic cross-sectional view showing a subdivided II' structure of the external electrode of FIG. 4. [Figure 11] 1A is an image of the body surface of the embodiment taken with a scanning electron microscope (SEM), and FIG. 1B is an image of the body surface of the comparative example taken with a scanning electron microscope (SEM). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, the embodiments of the present invention will be described with reference to specific embodiments and the accompanying drawings. However, the embodiments of the present invention may be modified into several other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those skilled in the art. Therefore, the shapes and sizes of elements in the drawings may be enlarged or reduced (or highlighted or simplified) for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements.

[0019] In addition, in the drawings, parts that are not relevant to the description are omitted in order to clearly explain the present invention, and the size and thickness of each component shown in the drawings are arbitrarily shown for the convenience of explanation, so the present invention is not necessarily limited by the drawings. Furthermore, components having the same function within the same concept may be described using the same reference numerals. Furthermore, throughout the specification, when a part "includes" a certain component, it does not exclude other components, but means that the part may further include other components, unless otherwise specified to the contrary.

[0020] In the drawings, the first direction can be defined as the stacking direction or thickness (T) direction, the second direction can be defined as the length (T) direction, and the third direction can be defined as the width (W) direction.

[0021] Multilayer Electronic Components FIG. 1 is a schematic perspective view of a multilayer electronic component according to one embodiment of the present invention, FIG. 2 is a schematic perspective view of the multilayer electronic component of FIG. 1 excluding external electrodes, FIG. 3 is a schematic separated perspective view showing a laminated structure of internal electrodes, FIG. 4 is a schematic cross-sectional view taken along line I-I' in FIG. 1, FIG. 5 is a schematic cross-sectional view taken along line II-II' in FIG. 1, FIG. 6 is a schematic cross-sectional view taken along line I-I' of another embodiment of the present invention, FIG. 7 is a schematic cross-sectional view taken along line I-I' of another embodiment of the present invention, FIG. 8 is a schematic cross-sectional view taken along line I-I' of another embodiment of the present invention, FIG. 9 is a schematic cross-sectional view taken along line I-I' of another embodiment of the present invention, and FIG. 10 is a schematic cross-sectional view of a subdivided external electrode structure of FIG. 4.

[0022] Hereinafter, a multilayer electronic component according to an embodiment of the present invention will be described in detail with reference to Figures 1 to 11. Although a multilayer ceramic capacitor will be described as an example of a multilayer electronic component, the present invention can also be applied to various electronic products using a dielectric composition, such as an inductor, a piezoelectric element, a varistor, or a thermistor.

[0023] A multilayer electronic component 100 according to one embodiment of the present invention includes a body 110 including a dielectric layer 111 and internal electrodes 121, 122, and external electrodes 131, 132 disposed on the body 110, and a lattice-shaped groove shape 141 having a plurality of grooves arranged in a lattice pattern may be formed on at least a portion of a surface of the body 110.

[0024] The body 110 has dielectric layers 111 and internal electrodes 121 and 122 laminated alternately.

[0025] More specifically, the main body 110 may include a capacitance forming portion Ac that is disposed inside the main body 110 and includes first internal electrodes 121 and second internal electrodes 122 that are alternately arranged facing each other across the dielectric layer 111 to form a capacitance.

[0026] Although there is no particular limitation on the specific shape of the body 110, the body 110 may be hexahedral or a similar shape as shown in the figure. Due to shrinkage of the ceramic powder contained in the body 110 during the firing process, the body 110 may have a substantially hexahedral shape rather than a hexahedral shape having perfectly straight lines.

[0027] The main body 110 may have a first surface 1 and a second surface 2 facing each other in a first direction, a third surface 3 and a fourth surface 4 connected to the first surface 1 and the second surface 2 and facing each other in the second direction, and a fifth surface 5 and a sixth surface 6 connected to the first surface to the fourth surface (1, 2, 3, 4) and facing each other in the third direction.

[0028] The multiple dielectric layers 111 forming the body 110 are in a fired state, and the boundaries between adjacent dielectric layers 111 can be integrated to such an extent that they are difficult to see without the use of a scanning electron microscope (SEM).

[0029] The raw material for forming the dielectric layer 111 is not limited as long as a sufficient capacitance can be obtained. In general, a perovskite (ABO3)-based material can be used, such as a barium titanate-based material, a lead complex perovskite-based material, or a strontium titanate-based material. The barium titanate-based material can include a BaTiO3-based ceramic powder, and examples of the ceramic powder include BaTiO3, BaTiO3 partially solid-dissolved with Ca (calcium), Zr (zirconium), etc. 1-x Ca x )TiO3(0 <x<1)、Ba(Ti 1-y Ca y )O3(0 <y<1)、(Ba 1-x Ca x )(Ti1-y Zr y )O3 (0 < x < 1, 0 < y < 1) or Ba(Ti 1-y Zr y )O3 (0 < y < 1), etc. can be mentioned.

[0030] In addition, as raw materials for forming the dielectric layer 111, various ceramic additives, organic solvents, binders, dispersants, etc. can be added to powders such as barium titanate (BaTiO3) according to the purpose of the present invention.

[0031] The thickness td of the dielectric layer 111 does not particularly need to be limited.

[0032] However, in order to more easily achieve miniaturization and high capacitance of the multilayer electronic component, the thickness of the dielectric layer 111 can be 0.6 μm or less, and more preferably 0.4 μm or less.

[0033] Here, the thickness td of the dielectric layer 111 can mean the thickness td of the dielectric layer 111 disposed between the first internal electrode 121 and the second internal electrode 122.

[0034] On the other hand, the thickness td of the dielectric layer 111 can mean the size of the dielectric layer 111 in the first direction. Note that the thickness td of the dielectric layer 111 can mean the average thickness td of the dielectric layer 111 and can mean the average size of the dielectric layer 111 in the first direction.

[0035] The average size in the first direction of the dielectric layer 111 may be measured by scanning an image of a cross-section in the first and second directions of the body 110 using a scanning electron microscope (SEM) with a magnification of 10,000 times. More specifically, the average size in the first direction of one dielectric layer 111 may mean an average value calculated by measuring the size in the first direction of one dielectric layer 111 at 30 equally spaced points in the second direction in the scanned image. The 30 equally spaced points may be designated as the capacitance forming portion Ac. Furthermore, if such an average measurement is extended to 10 dielectric layers 111 to measure the average value, the average size in the first direction of the dielectric layer 111 may be further generalized.

[0036] The internal electrodes 121 and 122 may be laminated alternately with the dielectric layers 111 .

[0037] The internal electrodes 121, 122 may include a first internal electrode 121 and a second internal electrode 122, and the first internal electrode 121 and the second internal electrode 122 are alternately arranged to face each other across the dielectric layer 111 that constitutes the main body 110, and may be exposed to the third surface 3 and the fourth surface 4 of the main body 110, respectively.

[0038] More specifically, the first internal electrode 121 may be exposed while being spaced apart from the fourth surface 4 and in contact with the third surface 3, and the second internal electrode 122 may be exposed while being spaced apart from the third surface 3 and in contact with the fourth surface 4. A first external electrode 131 may be disposed on the third surface 3 of the body 110 and connected to the first internal electrode 121, and a second external electrode 132 may be disposed on the fourth surface 4 of the body 110 and connected to the second internal electrode 122.

[0039] That is, the first internal electrode 121 may be connected to the first external electrode 131 without being connected to the second external electrode 132, and the second internal electrode 122 may be connected to the second external electrode 132 without being connected to the first external electrode 131. In this case, the first internal electrode 121 and the second internal electrode 122 may be electrically isolated from each other by the dielectric layer 111 disposed therebetween.

[0040] Meanwhile, the body 110 may be formed by alternately stacking ceramic green sheets on which the first internal electrodes 121 are printed and ceramic green sheets on which the second internal electrodes 122 are printed, and then firing the stacked ceramic green sheets.

[0041] There are no particular limitations on the material forming the internal electrodes 121 and 122, and any material having excellent electrical conductivity can be used. For example, the internal electrodes 121 and 122 can include one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.

[0042] The internal electrodes 121 and 122 may be formed by printing a conductive paste for internal electrodes, which contains at least one of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof, on the ceramic green sheet. The method for printing the conductive paste for internal electrodes may be a screen printing method or a gravure printing method, but the present invention is not limited thereto.

[0043] On the other hand, the thickness te of the internal electrodes 121 and 122 does not need to be particularly limited.

[0044] However, in order to more easily achieve miniaturization and high capacity of the multilayer electronic component, the thickness of the internal electrodes 121, 122 can be 0.6 μm or less, and more preferably 0.4 μm or less.

[0045] Here, the thickness te of the internal electrodes 121, 122 may refer to the size of the internal electrodes 121, 122 in the first direction. In addition, the thickness te of the internal electrodes 121, 122 may refer to the average thickness te of the internal electrodes 121, 122, or may refer to the average size of the internal electrodes 121, 122 in the first direction.

[0046] The average size of the internal electrodes 121, 122 in the first direction may be measured by scanning an image of a cross-section of the body 110 in the first and second directions using a scanning electron microscope (SEM) with a magnification of 10,000 times. More specifically, the average size of one internal electrode in the first direction may be an average value calculated by measuring the size of one internal electrode in the first direction at 30 equally spaced points in the second direction in the scanned image. The 30 equally spaced points may be designated as the capacitance forming portion Ac. Furthermore, if such an average value measurement is extended to 10 internal electrodes 121, 122 to measure the average value, the average size of the internal electrodes 121, 122 in the first direction may be further generalized.

[0047] Meanwhile, the body 110 may include cover portions 112 and 113 disposed on both end surfaces in the first direction of the capacitance forming portion Ac.

[0048] More specifically, it may include an upper cover part 112 disposed on an upper part of the capacitance forming part Ac in the first direction, and a lower cover part 113 disposed on a lower part of the capacitance forming part Ac in the first direction.

[0049] The upper cover part 112 and the lower cover part 113 may be formed by stacking a single dielectric layer 111 or two or more dielectric layers 111 in a first direction on the upper and lower surfaces of the capacitance forming part Ac, respectively, and may basically serve to prevent damage to the internal electrodes 121, 122 due to physical or chemical stress.

[0050] The upper cover part 112 and the lower cover part 113 do not include the internal electrodes 121, 122, and may include the same material as the dielectric layer 111. That is, the upper cover part 112 and the lower cover part 113 may include a ceramic material, for example, a barium titanate (BaTiO3)-based ceramic material.

[0051] On the other hand, the thickness tc of the covers 112 and 113 does not need to be particularly limited.

[0052] However, in order to more easily achieve miniaturization and high capacity of the multilayer electronic component, the thickness tc of the cover parts 112, 113 can be 100 μm or less, preferably 30 μm or less, and more preferably 20 μm or less for ultra-small products.

[0053] Here, the thickness tc of the cover parts 112, 113 may refer to the size of the cover parts 112, 113 in the first direction. In addition, the thickness tc of the cover parts 112, 113 may refer to the average thickness tc of the cover parts 112, 113, or may refer to the average size of the cover parts 112, 113 in the first direction.

[0054] The average size in the first direction of the cover parts 112 and 113 may be measured by scanning an image of a cross section in the first direction and the second direction of the body 110 using a scanning electron microscope (SEM) with a magnification of 10,000 times. More specifically, the average size in the first direction may be calculated by measuring the size in the first direction at 30 points equally spaced in the second direction in an image obtained by scanning one cover part.

[0055] Furthermore, the average size of the cover portion in the first direction measured by the above-mentioned method may be substantially the same as the average size of the cover portion in the first direction in cross-sections of the main body 110 in the first and third directions.

[0056] Meanwhile, side margin parts 114 and 115 may be disposed on both end surfaces of the body 110 in the third direction.

[0057] More specifically, the side margin portions 114, 115 may include a first side margin portion 114 disposed on the fifth surface 5 of the main body 110 and a second side margin portion 115 disposed on the sixth surface 6. That is, the side margin portions 114, 115 may be disposed on both end surfaces of the main body 110 in the third direction.

[0058] As shown, the side margin portions 114, 115 may refer to the areas between both ends of the first internal electrode 121 and the second internal electrode 122 in the third direction and the boundary surface of the body 110, based on the cross-sections of the body 110 in the first and third directions.

[0059] The side margins 114 and 115 essentially serve to prevent damage to the internal electrodes 121 and 122 due to physical or chemical stress.

[0060] The side margin portions 114, 115 can also be formed by forming internal electrodes 121, 122 by applying a conductive paste to the ceramic green sheet except for the areas where the side margin portions 114, 115 are to be formed, and then cutting the laminated internal electrodes 121, 122 so that they are exposed on the fifth surface 5 and the sixth surface 6 of the main body 110 in order to suppress steps caused by the internal electrodes 121, 122, and then stacking a single dielectric layer 111 or two or more dielectric layers 111 in the third direction on both end surfaces in the third direction of the capacitance forming portion Ac.

[0061] The first side margin portion 114 and the second side margin portion 115 do not include the internal electrodes 121, 122, and may include the same material as the dielectric layer 111. That is, the first side margin portion 114 and the second side margin portion 115 may include a ceramic material, for example, a barium titanate (BaTiO3)-based ceramic material.

[0062] On the other hand, the width wm of the first side margin portion 114 and the second side margin portion 115 does not need to be particularly limited.

[0063] However, in order to more easily achieve miniaturization and high capacity of the laminated electronic component 100, the width wm of the first side margin portion 114 and the second side margin portion 115 can be 100 μm or less, preferably 30 μm or less, and for ultra-small products, more preferably 20 μm or less.

[0064] Here, the width wm of the side margin portions 114, 115 may refer to the size in the third direction of each of the side margin portions 114, 115. In addition, the width wm of the side margin portions 114, 115 may refer to the average width wm of the side margin portions 114, 115, or may refer to the average size in the third direction of the side margin portions 114, 115.

[0065] The average size in the third direction of the side margin portions 114, 115 may be measured by scanning an image of a cross-section in the first and third directions of the body 110 using a scanning electron microscope (SEM) with a magnification of 10,000 times. More specifically, it may refer to an average value calculated by measuring the size in the third direction at 10 points equally spaced in the first direction in an image obtained by scanning one side margin portion.

[0066] Meanwhile, methods for simultaneously achieving miniaturization and high capacity of multilayer electronic components include using a material with a high dielectric constant or reducing the thickness of the dielectric layer or internal electrode layer, etc. However, if the thickness of the dielectric layer is reduced too much, problems such as a decrease in breakdown voltage (BDV) and deterioration of reliability may occur.

[0067] Therefore, by applying a method of thinning the external electrodes, it is possible to minimize the volume of the portions that are not directly related to the capacitance of the multilayer electronic component and maximize the effective volume. Methods of thinning the external electrodes include forming the external electrodes with a plating film or applying a thin film deposition method such as sputtering, but when the external electrodes are formed by such methods, the bonding strength with the ceramic body is insufficient, and delamination between the body and the external electrodes may occur.

[0068] In order to solve these problems, research is being conducted on various pretreatments, such as forming surface roughness on the body or forming other materials on the body to facilitate bonding between the ceramic body and the external electrodes.

[0069] As a result, one embodiment of the present invention can improve the interfacial bonding strength with the external electrode by forming a lattice-like groove shape having a plurality of grooves arranged in a lattice pattern on at least a portion of the surface of the main body 110.

[0070] In the present invention, the surface on which the lattice-shaped groove shape 141 is formed can be formed on the first to sixth surfaces (1, 2, 3, 4, 5, 6) of the main body, and when the cover portions 112, 113 are arranged, can be formed on at least a portion of the outer surface of the cover portions 112, 113, and when the side margin portions 114, 115 are arranged, can be formed on at least a portion of the outer surface of the side margin portions 114, 115.

[0071] The lattice-like groove shape 141 includes an outer wall and the groove surrounded by the outer wall, and at this time, the groove may have a shape in which the width narrows toward the inside of the body 110 .

[0072] The lattice-like groove shape may include, for example, one or more of a waffle shape, a wave shape, and a dome shape, but is not limited thereto, and may include any shape in which a repeating pattern of a three-dimensional shape is formed on the surface of the body 110.

[0073] The lattice-like groove shape 141 can be formed by irradiating a laser onto at least a portion of the outer surface of the main body 110 or the outer surface of the side margin portions 114, 115 after firing, but is not limited to this and any method that can form a repeating pattern can be used.

[0074] Meanwhile, when the lattice-like groove shape is formed using a laser, the size and depth can be adjusted by adjusting the intensity, scanning speed, and frequency of the laser, and when a pattern shape having a certain depth or more and a certain width or less is formed, the adhesion between the body and the external electrode can be improved. The specific depth and width of the lattice-like groove shape 141 will be described in more detail below.

[0075] In the present invention, the lattice-like groove shape 141 may mean one lattice-like groove shape 141, or may mean that the lattice-like groove shape 141 has multiple grooves and is formed in a certain area, and the lattice-like groove shape 141 having multiple grooves does not mean that the multiple grooves are completely identical, but may mean that substantially the same shape is repeatedly formed.

[0076] To make it easier to understand the lattice-like groove shape 141, the present invention describes the lattice and the interior of the lattice as a two-dimensional plane, but it can actually be a three-dimensional solid having a surface roughness or a depth, width and height.

[0077] The groove may have a concave shape that narrows toward the inside of the body 110, and the concave shape may have various cross sections such as a square, semicircle, semi-ellipse, triangle, etc., but is not limited thereto.

[0078] In one embodiment of the present invention, when the ten-point average surface roughness of the groove is defined as R2z, R2z≧3 μm can be satisfied.

[0079] There is no particular limitation as long as the ten-point average surface roughness value (R2z) within the lattice is such that the surface bonding strength between the body 110 and the external electrodes 131, 132 can be improved, but the preferred upper limit may be 10 μm or less.

[0080] The ten-point average surface roughness (Rz) can mean, for example, that after extracting only a reference length from a roughness curve obtained by measurement in the direction of the average line, the sum of the average value of the absolute values ​​of the elevations of the highest to fifth peaks measured in the longitudinal magnification direction on the average line of this extracted portion and the average value of the absolute values ​​of the elevations of the lowest to fifth valleys measured in the longitudinal magnification direction is calculated. By applying the ten-point average surface roughness, the inside of a grid having different surface roughness can be expressed by a more reliable surface roughness value.

[0081] When the ten-point average surface roughness (R2z) of the grooves is 3 μm or more, the area of ​​the interface between the main body 110 and the external electrodes 131, 132 increases, and the interface bonding strength can be further improved.

[0082] If the ten-point average surface roughness (R2z) of the groove is less than 3 μm, the interface area between the main body 110 and the external electrodes 131, 132 may be insufficient, resulting in insufficient interfacial bonding strength, which may cause peeling between the main body 110 and the external electrodes 131, 132.

[0083] In the present invention, the contents relating to surface roughness such as surface roughness, average surface roughness, maximum surface roughness, and ten-point average surface roughness may be the results of measurement using a surface roughness measuring instrument (Keyence VK-X3000 model), and any measuring instrument capable of measuring surface roughness at fine depths may be used.

[0084] On the other hand, when the maximum length of the lattice-like groove shape is defined as L based on the plan view, L≦10 μm can be satisfied.

[0085] The lower limit of the maximum length (L) of the lattice-like groove shape is not particularly limited, but it is sufficient if the value allows the interior of the lattice to have an area, and can be, for example, 1 μm or more, preferably 3 μm or more, and more preferably 5 μm or more.

[0086] By making the maximum length of the lattice-like groove shape 10 μm or less, the surface area of ​​the main body 110 can be increased, and the interfacial bonding strength between the main body 110 and the external electrodes 131 and 132 can be improved.

[0087] In this case, when the area of ​​the lattice-like groove shape is defined as A based on the plan view, A≦0.5×L 2 can be satisfied.

[0088] When the area of ​​the lattice groove shape is defined as A, A≦0.5×L 2By satisfying the above condition, the surface area of ​​the main body 110 can be increased, and the interfacial bonding strength between the main body 110 and the external electrodes 131 and 132 can be improved.

[0089] In the present invention, the maximum length (L) of the lattice-shaped groove shape based on a plan view may refer to a value measured in the following manner, but is not particularly limited thereto.

[0090] For example, the first surface of the body 110, which is the surface of the body 110 where the lattice-like grooves are located, is exposed through a scanning electron microscope (SEM) or a transmission electron microscope (TEM) with a magnification of 20,000 times, and then an image is obtained by photographing 1 / 4, 2 / 4, and 3 / 4 points of the body based on the third direction. The cross section of the body that can be confirmed in the image photographed at the 1 / 4 point based on the third direction of the body may protrude at a certain distance due to the lattice-like grooves, and in this case, the protruding part can be defined as a floor. The distance between adjacent floors is measured and defined as 1 point, and the distances of 10 points are measured and the average value can be defined as the representative lattice length l1. The representative lattice lengths l2 and l3 measured at 2 / 4 and 3 / 4 points based on the third direction of the body can be obtained using the same method as the above-mentioned measurement method. In this case, the largest value (Max(l1, l2, l3)) among l1, l2, and l3 can be defined as the maximum length (L) of the lattice-like groove shape.

[0091] The area (A) of the lattice-shaped groove shape based on the plan view may refer to a value obtained by measuring the area of ​​the inside of the lattice-shaped groove shape based on the image captured by the above-mentioned method.

[0092] For example, the area of ​​one of the lattice grooves formed on the cross section of the body, which can be seen in an image taken at a 1 / 4 point in the third direction of the body, is measured and defined as 1 point. The average value of the areas measured at 10 points can be defined as the representative lattice area a1. Using the same measurement method as described above, the representative lattice areas a2 and a3 measured at 2 / 4 and 3 / 4 points in the third direction of the body can be obtained. In this case, the largest value (Max(a1, a2, a3)) of a1, a2, and a3 can be defined as the area (A) of the lattice grooves.

[0093] In one embodiment of the present invention, a structure in which the ceramic electronic component 100 has two external electrodes 131, 132 is described, but the number and shapes of the external electrodes 131, 132 can be changed depending on the shape of the internal electrodes 121, 122 and other purposes.

[0094] The external electrodes 131 and 132 may be disposed on the body 110 and connected to the internal electrodes 121 and 122 .

[0095] More specifically, the external electrodes 131, 132 may include a first external electrode 131 and a second external electrode 132 disposed on the third surface 3 and the fourth surface 4 of the body 110, respectively, and connected to the first internal electrode 121 and the second internal electrode 122, respectively. That is, the first external electrode 131 may be disposed on the third surface 3 of the body and connected to the first internal electrode 121, and the second external electrode 132 may be disposed on the fourth surface 4 of the body and connected to the second internal electrode 122.

[0096] The external electrodes 131, 132 may be formed using any material that has electrical conductivity, such as a metal, and the specific material may be determined taking into consideration electrical properties, structural stability, etc., and may further have a multi-layer structure.

[0097] For example, the external electrodes 131 and 132 may include electrode layers 131a and 132a disposed on the body 110, and plating layers 131b, 132b, 131c, 132c, 131d, and 132d disposed on the electrode layers 131a and 132a.

[0098] As a more specific example of the electrode layers 131a and 132a, the electrode layers 131a and 132a may be fired electrodes containing a conductive metal and glass, or resin-based electrodes containing a conductive metal and resin.

[0099] Also, the electrode layers 131a and 132a may be in a form in which a fired electrode and a resin-based electrode are sequentially formed on the body 110.

[0100] In addition, the electrode layers 131a and 132a may be formed by transferring a sheet containing a conductive metal onto the body 110, or may be formed by transferring a sheet containing a conductive metal onto a fired electrode.

[0101] The conductive metal used for the electrode layers 131a and 132a is not particularly limited as long as it can be electrically connected to the internal electrodes 121 and 122 to form capacitance, and may include, for example, at least one selected from the group consisting of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof. The electrode layers 131a and 132a may be formed by applying a conductive paste prepared by adding glass frit to the conductive metal powder, and then firing the paste.

[0102] The electrode layers 131a and 132a may be formed by a thin film deposition method such as sputtering, or a plating method.

[0103] The average thickness of the electrode layers 131a and 132a formed by sputtering or the like can be 1 μm or less, with a preferred lower limit of 0.1 μm or more, and more preferably 0.3 μm or more.

[0104] When the electrode layers 131a, 132a are formed by a thin film deposition method or the like, the electrode layers 131a, 132a can be formed to have a uniform but thin thickness, which makes it possible to simultaneously achieve a miniaturized and high-capacity multilayer electronic component 100.

[0105] The average thickness of the electrode layers 131a and 132a can be measured by, for example, the following method, but is not particularly limited thereto.

[0106] The second-direction size of the electrode layers 131a, 132a formed at the center in the first direction and the second-direction size of the electrode layers 131a, 132a at points spaced apart in the first direction from the center in the first direction, for example, by 3 μm, can be measured and averaged based on the first and second direction cross-sections of the multilayer electronic component 100. The more the measured values ​​of the second-direction size of the electrode layers 131a, 132a measured at regular intervals are, the more the average thickness of the electrode layers 131a, 132 can be generalized.

[0107] The plating layers 131b, 132b, 131c, 132c, 131d, and 132d can serve to improve mounting characteristics.

[0108] The type of plating layers 131b, 132b, 131c, 132c, 131d, and 132d is not particularly limited, and may be a single-layer plating layer containing one or more of copper (Cu), nickel (Ni), tin (Sn), and alloys thereof, or may be formed of multiple layers.

[0109] As a more specific example of the plating layers 131b, 132b, 131c, 132c, 131d, and 132d, the plating layers 131b and 132b may be Ni plating layers or Sn plating layers, and may have a form in which copper (Cu) plating layers 131b and 132b, nickel (Ni) plating layers 131c and 132c, and tin (Sn) plating layers 131d and 132d are sequentially arranged on the electrode layers 131a and 132a.

[0110] The grid-like groove shape according to the present invention may be located on at least a portion of the surface of the body 110 that contacts the external electrodes 131 and 132 .

[0111] In other words, it can mean that the external electrodes 131 and 132 are located on at least a part of the surface of the main body 110, which is the interface where the main body 110 and the external electrodes 131 and 132 are in contact with each other.

[0112] As described above, when the electrode layers 131a and 132a are formed by a sputtering method or the like, glass frit or the like may not be added. This may result in insufficient bonding strength with the ceramic body, which may cause peeling between the body and the electrode layer, but by forming the lattice-like groove shape of the present invention on the surface of the body, the surface area between the body and the electrode layer can be increased, thereby improving the interfacial bonding strength between the body and the electrode layer.

[0113] More specifically, when the first external electrode 131 is disposed on the third surface 3, a part of the first surface 1, and a part of the second surface 2 of the main body, the lattice-like groove shape 141 may also be located on the third surface 3, a part of the first surface 1, and a part of the second surface 2 of the main body. When the second external electrode 132 is disposed on the fourth surface 4, a part of the first surface 1, and a part of the second surface 2 of the main body, the lattice-like groove shape 141 may also be located on the fourth surface 4, a part of the first surface 1, and a part of the second surface 2 of the main body.

[0114] In this case, the area where the lattice-like grooves are formed may be 10% or more of the area of ​​the surface of the body 110 that contacts the external electrodes 131 and 132.

[0115] More specifically, when the first external electrode 131 is arranged on the third surface 3 of the main body, a portion of the first surface 1, and a portion of the second surface 2, the lattice-shaped groove shape 141 can also be located on the third surface 3 of the main body, a portion of the first surface 1, and a portion of the second surface 2.

[0116] Here, when the area where the first external electrode 131 and the body 110 contact each other is defined as S, and the area where the lattice-shaped groove shape 141 is formed on the surface of the body where the first external electrode 131 and the body 110 contact each other is defined as TA, it may mean that TA / S≧10% is satisfied. The description of the first external electrode 131 may be similarly applied to the description of the second external electrode 132.

[0117] By satisfying the requirement that the area of ​​the lattice-like groove shape 141 be 10% or more of the area of ​​the surface of the main body 110 in contact with the external electrodes 131, 132, the interfacial bonding strength between the main body 110 and the external electrodes 131, 132 can be improved, and the occurrence of peeling and floating phenomena can be suppressed.

[0118] In addition, the lattice-like groove shape 141 can also be positioned on the surface of the main body 110 on which the external electrodes 131, 132 are not arranged, thereby improving the bonding strength by solder or the like on the surface of the main body 110 on which the external electrodes are not arranged when mounted on a substrate.

[0119] On the other hand, the lattice-like groove shape 141 may be located on the third surface 3 and the fourth surface 4 of the main body, but the lattice-like groove shape may not be located in the areas where the internal electrodes 121, 122 are in contact with the third surface 3 and the fourth surface 4 of the main body and exposed to the outside.

[0120] This may be because, when the lattice-like groove shape is formed using a laser, the metal of the internal electrode cannot be etched in the region of a specific wavelength band, and only the dielectric layer 111 is etched.

[0121] However, the present invention is not limited to this, and the intensity, frequency, etc. of the laser may be adjusted to form lattice-like grooves 141 in the internal electrodes 121 and 122, thereby contributing to increasing the interfacial bonding strength.

[0122] When the side margin portions 114, 115 are arranged on the fifth surface 5 and the sixth surface 6 of the main body and the external electrodes 131, 132 are arranged on the side margin portions 114, 115, a lattice-shaped groove shape 141 can be located on at least a portion of the outer surface of the side margin portions 114, 115.

[0123] For example, when the first side margin portion 114 is disposed on the fifth surface 5 of the main body, a lattice-shaped groove may be located in an area of ​​the outer surface of the first side margin portion 114 parallel to the fifth surface 5 of the main body where the external electrodes are disposed. When both end surfaces in the second direction of the first side margin portion 114 are on the same plane as the third surface 3 and the fourth surface 4 of the main body, a lattice-shaped groove may be located in at least a part of both end surfaces, which are the outer surfaces in the second direction of the first side margin portion 114. The description of the first side margin portion 114 may be similarly applied to the second side margin portion 115.

[0124] In other words, by positioning the lattice-like groove shape 141 in the area in contact with the external electrodes 131, 132, peeling or floating of the external electrodes 131, 132 can be suppressed, and the multilayer electronic component can be made smaller and have a higher capacity, resulting in excellent reliability.

[0125] The size of the multilayer electronic component 100 does not need to be particularly limited.

[0126] However, in order to simultaneously achieve miniaturization and high capacity, it is necessary to reduce the thickness of the dielectric layers and internal electrodes and increase the number of layers, so the effects of the present invention can be more pronounced in a multilayer electronic component 100 having a size of 1005 (length x width: 1.0 mm x 0.5 mm) or less.

[0127] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment and the accompanying drawings, but is defined by the appended claims. Therefore, various substitutions, modifications and changes can be made by a person having ordinary skill in the art within the scope of the technical idea of ​​the present invention described in the claims, and these also belong to the scope of the present invention.

[0128] The present invention will be described in more detail below with reference to examples. However, these examples are intended to aid in the specific understanding of the present invention, and the scope of the present invention is not limited to these examples.

[0129] (Example) The following describes the results of evaluating the interfacial bonding strength of Test Example 1, in which a lattice-like groove shape was formed on the surface of the main body, and Test Example 2, in which a lattice-like groove shape was not formed.

[0130] In test example 1, a lattice-like groove shape was formed in the ceramic region of the third surface of a chip using a laser with an intensity of 1.5 watts (W), and then a copper (Cu) electrode layer was formed to a thickness of 0.5 μm using a sputtering method. After this, a copper (Cu) electrolytic plating layer was plated to a thickness of 3 μm on the copper (Cu) electrode layer, and a tape test, which is a type of adhesion evaluation, was performed. After the tape test described below, the maximum length (L) measured from an image of the lattice-like groove shape taken with a scanning electron microscope (SEM) was 10 μm, and the area (A) was 48 μm. 2 It was.

[0131] Test example 2 was produced in the same manner as test example 1, except that the lattice-like grooves were not formed on the surface of the main body.

[0132] The tape test involves repeatedly attaching and detaching an adhesive tape material to an external electrode that includes a copper (Cu) electrode layer, and evaluating whether or not the copper (Cu) electrode layer of the external electrode peels off.

[0133] Twenty-five sample chips were produced for each of Test Examples 1 and 2, and then a tape test was performed in which the chips were attached and detached 10 times. As a result, in Test Example 1, none of the 25 sample chips experienced peeling of the copper (Cu) electrode layer, whereas in Test Example 2, peeling of the copper (Cu) electrode layer occurred in five of the 25 sample chips.

[0134] This shows that by forming a lattice-like groove shape to increase the surface area of ​​the main body, peeling between the main body and the external electrode can be suppressed.

[0135] Next, the measured data regarding the optimum maximum length (L), area (A), average surface roughness (Ra), ten-point average surface roughness (Rz) and surface area of ​​the lattice-like groove shape will be described.

[0136] The maximum length (L) of the lattice groove shape means the maximum length that can be measured in the lattice groove shape in the image taken by a scanning electron microscope (SEM), and the area (A) means the internal area of ​​one lattice groove shape in the image taken by a scanning electron microscope (SEM). The average surface roughness (Ra) and the ten-point average surface roughness (Rz) are measured by a surface roughness measuring instrument, and the surface area growth rate (Sdr) means the growth rate of the actual three-dimensional area of ​​one lattice groove shape, and the larger the surface area, the higher the fineness level.

[0137] Test example 3 is a sample chip in which no lattice-like grooves are formed on the main body surface of the sample chip, and the manufacturing method is the same as that of test example 2 described above.

[0138] In Test Example 4, after completing the surface roughness measurement of Test Example 3, a laser with an intensity of 1.5 watts (W) was irradiated onto the body surface of the sample chip to form a lattice-like groove shape, and the surface roughness was measured again. The fabrication method was the same as in the above-mentioned Test Example 1. Figure 11 (a) is an image taken using a scanning electron microscope (SEM) to measure the maximum length (L) and area (A) of the lattice-like groove shape formed on the surface of the body of Test Example 4.

[0139] In Test Example 5, a lattice-like groove shape was formed on the body surface of a new sample chip by irradiating a 1.0 watt (W) laser, and the surface roughness was measured. Except for the laser intensity, the fabrication method was the same as in Test Example 1. Figure 11 (b) is an image taken using a scanning electron microscope (SEM) to measure the maximum length (L') and area (A') of the lattice-like groove shape formed on the body surface of Test Example 5.

[0140] [Table 1]

[0141] In the case of test example 3, in which no lattice-shaped grooves were formed, it could be evaluated as having a typical surface roughness of the main body, with the average surface roughness (Ra) being 0.181 μm, the ten-point average surface roughness (Rz) being 1.750 μm, and the surface area growth rate (Sdr) being 0.03753.

[0142] In the case of Test Example 4 in which a lattice-shaped groove shape was formed, the average surface roughness (Ra) was 0.655 μm, the ten-point average surface roughness (Rz) was 4.070 μm, the surface area growth rate (Sdr) was 0.08183, the maximum length (L) was 10 μm, and the area (A) was 48 μm. 2 was measured.

[0143] In the case of Test Example 5, in which a lattice-like groove shape different from Test Example 4 was formed, the average surface roughness (Ra) was 0.201 μm, the ten-point average surface roughness (Rz) was 1.390 μm, the surface area growth rate (Sdr) was 0.06056, the maximum length (L) was 12 μm, and the area (A) was 66.5 μm. 2 was measured.

[0144] The surface area growth rate (Sdr) of Test Example 4 was 0.08183, which is 2.18 times higher than the surface area growth rate (Sdr) of 0.03753 of Test Example 3, where the lattice-shaped groove shape was not formed. If the surface area growth rate increases by more than two times, it is predicted that the interfacial adhesion strength between the body and the external electrode can be increased, and therefore it can be seen that the lattice-shaped groove shape of Test Example 4 is the optimal condition.

[0145] The surface area growth rate (Sdr) of Test Example 5 was 0.06056, which is 1.61 times higher than the surface area growth rate (Sdr) of 0.03753 of Test Example 3, which does not have a lattice-shaped groove shape. Although the surface area growth rate increases, it can be seen that the characteristics are somewhat worse than those of Test Example 4.

[0146] The expression "one embodiment" used in this specification does not mean the same embodiment as each other, but is provided to emphasize and describe each unique feature. However, the above-mentioned one embodiment does not exclude being realized in combination with the features of another embodiment. For example, even if the matter described in a specific embodiment is not described in another embodiment, it can be understood as a description related to the other embodiment, unless there is a description that is opposite or contradictory to the matter in the other embodiment.

[0147] The terms used in this specification are merely used to describe one embodiment and are not intended to limit the present disclosure. In this case, the singular expression includes the plural expression unless otherwise clearly indicated in the context. [Explanation of symbols]

[0148] 100 Multilayer electronic components 110 Main unit 111 Dielectric layer 112, 113 Cover part 114, 115 Side margin 121, 122 Internal electrode 131, 132 External electrode

Claims

1. a body including a dielectric layer and an internal electrode; an external electrode disposed on the body; A multilayer electronic component, wherein a lattice-like groove shape having a plurality of grooves arranged in a lattice pattern is formed on at least a portion of a surface of the main body.

2. The lattice-like groove shape includes an outer wall and a groove surrounded by the outer wall, 2. The multilayer electronic component according to claim 1, wherein the groove has a shape in which its width narrows toward the inside of the main body.

3. The multilayer electronic component according to claim 2 , wherein the lattice-like groove shape includes at least one of a waffle shape, a wave shape, and a dome shape.

4. 2. The multilayer electronic component according to claim 1, wherein when the ten-point average surface roughness of the grooves is defined as R2z, R2z ≥ 3 μm is satisfied.

5. 2. The multilayer electronic component according to claim 1, wherein, when a maximum length of the lattice-like groove shape is defined as L with respect to a plan view, L≦10 μm is satisfied.

6. When the area of ​​the lattice-like groove shape is defined as A based on the plan view, A≦0.5×L 2 The multilayer electronic component according to claim 5 , which satisfies the above.

7. 2. The multilayer electronic component according to claim 1, wherein the lattice-like grooves are formed on at least a portion of a surface of the main body that contacts the external electrodes.

8. 8. The multilayer electronic component according to claim 7, wherein an area in which the lattice-like grooves are formed is 10% or more of an area of ​​the surface of the main body in contact with the external electrodes.

9. 8. The multilayer electronic component according to claim 7, wherein the lattice-like groove shape is further formed on a surface of the main body on which the external electrodes are not disposed.

10. the body includes a capacitance forming portion including the dielectric layer and the internal electrodes arranged alternately in a first direction with the dielectric layer therebetween, and cover portions respectively arranged on both end faces of the capacitance forming portion in the first direction, the body including a first surface and a second surface facing each other in the first direction, a third surface and a fourth surface connected to the first surface and the second surface and facing each other in the second direction, and a fifth surface and a sixth surface connected to the first surface to the fourth surface and facing each other in the third direction, The multilayer electronic component according to claim 1 , further comprising side margin portions disposed on fifth and sixth surfaces of the main body, respectively.

11. the internal electrodes include a first internal electrode in contact with a third surface of the body and a second internal electrode in contact with a fourth surface of the body; The multilayer electronic component according to claim 10 , wherein the lattice-like groove shape is not formed on one surface of the first internal electrode in contact with the third surface and on one surface of the second internal electrode in contact with the fourth surface.

12. The multilayer electronic component according to claim 10 , wherein the lattice-like groove shape is further formed on at least a part of an outer surface of the side margin portion.

13. the external electrode includes an electrode layer disposed on the body and connected to the internal electrode; 2. The multilayer electronic component according to claim 1, wherein the electrode layers have an average thickness of 1 μm or less.

14. The laminated electronic component according to claim 13 , wherein the electrode layers contain copper (Cu).

15. The external electrode further includes a plating layer disposed on the electrode layer, The multilayer electronic component according to claim 13 , wherein the plating layer includes at least one of a copper (Cu) plating layer, a nickel (Ni) plating layer, and a tin (Sn) plating layer.

16. The multilayer electronic component according to claim 15 , wherein the plating layers are arranged in the following order: a copper (Cu) plating layer, a nickel (Ni) plating layer, and a tin (Sn) plating layer.

Citation Information

Patent Citations

  • Multilayered electronic component

    KR1020210033132A

  • Multilayered capacitor and board having the same mounted thereon

    KR1020220063556A

Cited By

  • Multilayer ceramic electronic component

    WO2026004910A1