On machine development type lithographic printing plate original plate, lithographic printing plate dummy plate and generation method of them

The on-press development type lithographic printing plate precursor with an aluminum support and anodized film, incorporating a phosphoric acid compound in cracks, addresses edge stains and setter plate feeding issues, enhancing printing quality and efficiency.

JP2024146709APending Publication Date: 2024-10-15FUJIFILM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023170181
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-09-29
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional lithographic printing plate precursors face issues with edge stains during continuous printing on roll paper and poor setter plate feeding performance due to storage conditions causing plates to stick together.

Method used

The development of an on-press development type lithographic printing plate precursor with an aluminum support and anodized film, featuring a sag-shaped region with cracks containing a phosphoric acid compound, where the P/Al ratio is 0.04 or more, and a controlled solid content difference between edge and non-edge areas to enhance edge stain suppression and setter plate feeding.

Benefits of technology

The solution achieves both excellent edge stain suppression and improved setter plate feeding performance by ensuring the phosphoric acid compound effectively prevents edge stains and facilitates easy plate handling during printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146709000102
    Figure 2024146709000102
  • Figure 2024146709000103
    Figure 2024146709000103
  • Figure 2024146709000104
    Figure 2024146709000104
Patent Text Reader

Abstract

To provide an on-machine development type lithographic printing plate original plate, a lithographic printing plate dummy plate, capable of achieving both of, extremely excellent setter plate feeding performance and excellent edge pollution suppression performance, and a generation method.SOLUTION: There is provided an on-machine development type lithographic printing plate original plate comprising: an aluminum support body having an anodic oxidation coating; and one or more constitution layers including an image recording layer, and comprising a hanging shape region on its end. The hanging shape region comprises: a crack whose deepest part reaches the aluminum support body, in the crack, there is provided a phosphoric acid system. In a surface of the crack region formed in the aluminum support body in the crack, a ratio (P / Al) of elemental phosphorus with respect to an aluminum element measured by FE-AES, is 0.04 or more. When a solid content of the one or more constitution layers on the end of the on-machine development type lithographic printing plate original plate is A, a solid content of one or more constitution layers on a region other than the end of the on-machine development type lithographic printing plate original plate is B, A≥B is satisfied, and A-B being a difference of the A and B is smaller than 0.8 g / m2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an on-press development type lithographic printing plate precursor and a dummy lithographic printing plate, and methods for producing them. [Background technology]

[0002] Generally, a lithographic printing plate consists of an oleophilic image area that accepts ink during the printing process, and a hydrophilic non-image area that accepts dampening water. Lithographic printing utilizes the mutual repulsion properties of water and oil-based ink, making the oleophilic image area of ​​the lithographic printing plate the ink-receptive area and the hydrophilic non-image area the dampening water-receptive area (ink-non-receptive area) to create a difference in ink adhesion on the surface of the lithographic printing plate, and after ink is applied only to the image area, the ink is transferred to the printing material such as paper to print. To prepare such a lithographic printing plate, a lithographic printing plate precursor (PS plate) having an oleophilic photosensitive resin layer (image recording layer) on a hydrophilic support has been widely used. Usually, the lithographic printing plate precursor is exposed to light through an original such as a lithographic film, and then the image areas of the image recording layer are left, while the other unnecessary image recording layer is dissolved and removed with an alkaline developer or organic solvent, exposing the hydrophilic support surface to form non-image areas, thereby obtaining a lithographic printing plate.

[0003] Furthermore, due to growing concern about the global environment, environmental issues related to waste liquids accompanying wet processing such as development processing have come into focus. In response to the above environmental issues, efforts are being made to simplify development or plate making, or to eliminate any processing. One of the simple manufacturing methods is a method called "on-press development." In other words, after exposing a lithographic printing plate precursor to light, it is mounted on a printing press as is, without undergoing conventional development, and unnecessary parts of the image recording layer are removed at an early stage of the normal printing process. In the present invention, a lithographic printing plate precursor that can be used for such on-press development is called an "on-press development type lithographic printing plate precursor".

[0004] When printing using a lithographic printing plate, when printing on paper smaller than the size of the printing plate, as in a normal sheet-fed printing press, the edge of the printing plate is outside the paper surface, so the edge does not affect the print quality. However, when printing continuously on rolled paper using a rotary press, such as in newspaper printing, the edge of the printing plate is within the paper surface, so the ink adhering to the edge is transferred to the paper, causing linear stains (edge ​​stains), which significantly reduces the commercial value of the printed matter.

[0005] Known attempts to suppress the occurrence of edge stains include, for example, a technique in which a liquid containing a component capable of suppressing the occurrence of edge stains is applied to the edge or edge surface of a lithographic printing plate precursor (see Patent Documents 1 and 2), a technique in which a lithographic printing plate precursor having a layer containing a component capable of suppressing the occurrence of edge stains is used for on-press development, thereby dissolving the component capable of suppressing the occurrence of edge stains into printing ink or fountain solution and transferring it to the edge portion of the lithographic printing plate precursor (see Patent Document 3), and a technique in which a treatment liquid containing a hydrophilizing agent is applied to the edge of a lithographic printing plate precursor, the application being performed so that the application means does not come into contact with the plate surface (see Patent Document 4). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Special Publication No. 2020-501936 [Patent Document 2] Patent Publication No. 2021-75268 [Patent Document 3] International Publication No. 2019 / 151447 [Patent Document 4] International Publication No. 2015 / 129504 Summary of the Invention [Problem to be solved by the invention]

[0007] However, there is a demand for further suppression of edge staining compared to conventional lithographic printing plate precursors and dummy lithographic printing plates. In addition, lithographic printing plate precursors and dummy lithographic printing plates are generally supplied by placing a laminate of them on a setter. However, depending on the storage conditions, etc., multiple lithographic printing plate precursors may come into close contact with each other, making it difficult to supply the plates from the setter. Therefore, further improvements in the plate supply performance from the setter (setter plate supply performance) are also expected.

[0008] The present invention has been made in consideration of the above, and its object is to provide an on-press development type lithographic printing plate precursor and a lithographic printing plate dummy plate that can achieve both extremely excellent setter plate feeding performance and extremely excellent edge stain suppression performance, as well as methods for producing the same. [Means for solving the problem]

[0009] Means for solving the above problems are described below.

[0010] [1] An on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, the on-press development type lithographic printing plate precursor having a sagging region at an edge portion, the sagging region has a crack whose deepest portion reaches the aluminum support, Phosphate compounds are present in the cracks, a ratio of phosphorus to aluminum (P / Al) measured by FE-AES on a surface of a crack region formed in the aluminum support inside the crack is 0.04 or more; When the solid content of one or more constituent layers at the end of the on-press development type lithographic printing plate precursor is A and the solid content of one or more constituent layers in the region other than the end of the on-press development type lithographic printing plate precursor is B, A≧B, and the difference between A and B, AB, is 0.8 g / m 2 is less than On-press development type lithographic printing plate precursor.

[0011] [2] The on-press development type lithographic printing plate precursor according to [1], wherein the phosphoric acid compound is at least one compound selected from the group consisting of phosphoric acid, phosphonic acid, phosphinic acid, phosphates, phosphonates, and phosphinates. [3] The on-press development type lithographic printing plate precursor according to [1] or [2], wherein a ratio of phosphorus element to aluminum element (P / Al) is 0.06 or more. [4] AB is 0.6g / m 2 The on-press development type lithographic printing plate precursor according to any one of [1] to [3] below.

[0012] [5] an on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, a sagging region at an end, and a crack in the sagging region, the deepest part of which reaches the aluminum support, inside the crack, A method for producing an on-press development type lithographic printing plate precursor, comprising the step of producing the on-press development type lithographic printing plate precursor according to any one of [1] to [4] above by mist-spraying a liquid containing a phosphoric acid compound.

[0013] [6] The method for preparing an on-press development type lithographic printing plate precursor according to [5], wherein the concentration of the liquid containing the phosphoric acid compound is 0.1 to 50% by mass.

[0014] [7] A method for producing an on-press development type lithographic printing plate precursor according to any one of [1] to [4], comprising spraying water into the inside of the crack of an on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, the on-press development type lithographic printing plate precursor having a sagging region at an edge and a crack in the sagging region whose deepest portion reaches the aluminum support, at least one of the constituent layers including a layer containing a phosphoric acid compound. [8] The amount of mist sprayed was 0.1 g / m 2~50g / m 2 The method for preparing an on-press development type lithographic printing plate precursor according to any one of [5] to [7],

[0015] [9] A method for producing an on-press development type lithographic printing plate precursor according to any one of [1] to [4], comprising exposing an on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, a sagging region at an edge, and a crack in the sagging region whose deepest part reaches the aluminum support, wherein the one or more constituent layers include a layer containing a phosphoric acid compound, to an environment of 60 to 95% RH (relative humidity in a 25°C environment) for 1 minute or more to produce the on-press development type lithographic printing plate precursor described in any one of [1] to [4].

[0016]

[10] The method for preparing an on-press development type lithographic printing plate precursor according to [9], wherein the on-press development type lithographic printing plate precursor is exposed to an environment of 70 to 95% RH as a relative humidity in a 25° C. environment for 1 minute or more.

[11] The method for preparing an on-press development type lithographic printing plate precursor according to [9] or

[10] , wherein the on-press development type lithographic printing plate precursor is exposed to an environment of 80 to 95% RH as a relative humidity in a 25° C. environment for 1 minute or more.

[12] The method for preparing an on-press development type lithographic printing plate precursor according to any one of [5] to

[11] , wherein the phosphoric acid compound is at least one compound selected from the group consisting of phosphoric acid, phosphonic acid, phosphinic acid, phosphates, phosphonates, and phosphinates.

[0017]

[13] A dummy lithographic printing plate having an aluminum support having an anodized film and one or more constituent layers including a polymer layer, and having a sagging region at an edge, the sagging region has a crack whose deepest portion reaches the aluminum support, Phosphate compounds are present in the cracks, the ratio of phosphorus to aluminum (P / Al) measured by FE-AES on the surface of a crack region formed in the aluminum support inside the crack is 0.04 or more, and when the solid content of one or more constituent layers at the end of the dummy lithographic printing plate is A and the solid content of one or more constituent layers in the region other than the end of the dummy lithographic printing plate is B, A≧B, and the difference between A and B, AB, is 0.8 g / m 2 A lithographic printing plate dummy plate that is less than 100 mm.

[0018]

[14] The dummy lithographic printing plate according to

[13] , wherein the phosphoric acid compound is at least one compound selected from the group consisting of phosphoric acid, phosphonic acid, phosphinic acid, phosphates, phosphonates, and phosphinates.

[15] The dummy lithographic printing plate according to

[13] or

[14] , wherein the ratio of phosphorus to aluminum (P / Al) is 0.06 or more.

[16] AB is 0.6g / m 2 The dummy planographic printing plate according to any one of items

[13] to

[15] below.

[0019]

[17] A dummy lithographic printing plate has an aluminum support having an anodized film and one or more constituent layers including a polymer layer, and has a sagging region at an end, and the sagging region has a crack whose deepest part reaches the aluminum support, and inside the crack, A method for producing a dummy lithographic printing plate, comprising producing the dummy lithographic printing plate according to any one of

[13] to

[16] above by misting a liquid containing a phosphoric acid compound.

[0020]

[18] The method for preparing a dummy lithographic printing plate according to

[17] , wherein the concentration of the liquid containing the phosphoric acid compound is 0.1 to 50% by mass.

[0021]

[19] A method for producing a dummy lithographic printing plate according to any one of items

[13] to

[16] , comprising spraying water into the inside of the crack in the dummy lithographic printing plate, the dummy lithographic printing plate having an aluminum support having an anodized film and one or more constituent layers including a polymer layer, a sagging region at an edge, and a crack in the sagging region whose deepest part reaches the aluminum support, wherein at least one of the one or more constituent layers includes a layer containing a phosphoric acid compound.

[20] The amount of mist sprayed was 0.1 g / m 2 ~50g / m 2 The method for producing a dummy lithographic printing plate according to any one of

[17] to

[19] ,

[0022] [twenty one] A method for producing a dummy lithographic printing plate according to any one of items

[13] to

[16] , by exposing a dummy lithographic printing plate having an aluminum support having an anodized film and one or more constituent layers including a polymer layer, a sagging region at an edge, and a crack in the sagging region whose deepest part reaches the aluminum support, wherein at least one of the one or more constituent layers includes a layer containing a phosphoric acid compound, to an environment of 60 to 95% RH in a 25°C environment for one minute or more, thereby producing the dummy lithographic printing plate according to any one of items

[13] to

[16] .

[0023] [twenty two] The method for preparing a dummy lithographic printing plate according to

[21] , further comprising exposing the dummy lithographic printing plate to an environment at 25° C. and a relative humidity of 70 to 95% for 1 minute or more. [twenty three] The method for preparing a dummy lithographic printing plate according to

[21] or

[22] , further comprising exposing the dummy lithographic printing plate to an environment at 25° C. and a relative humidity of 80 to 95% for 1 minute or more. [twenty four] The method for preparing a dummy lithographic printing plate according to any one of

[17] to

[23] , wherein the phosphoric acid compound is at least one compound selected from the group consisting of phosphoric acid, phosphonic acid, phosphinic acid, phosphoric acid salts, phosphonic acid salts, and phosphinic acid salts. Effect of the Invention

[0024] According to the present invention, it is possible to provide an on-press development type lithographic printing plate precursor and a dummy lithographic printing plate, which are capable of achieving both extremely excellent setter plate feeding performance and extremely excellent edge stain suppression performance, and methods for producing them. [Brief description of the drawings]

[0025] [Figure 1] 1 is a graph showing an example of an alternating current waveform used in electrochemical graining treatment. [Diagram 2] FIG. 2 is a side view showing an example of a radial cell in electrochemical graining treatment using an alternating current. [Diagram 3] FIG. 2 is a schematic diagram showing the cross-sectional shape of an edge portion of a planographic printing plate precursor. [Figure 4] FIG. 2 is a conceptual diagram illustrating an example of a cutting section of a slitter device. [Diagram 5] FIG. 2 is a side view showing the concept of a brush graining process used in mechanical roughening treatment in the production of an aluminum support. [Figure 6] FIG. 2 is a schematic diagram of an anodizing treatment device used in anodizing treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The present invention will be described in detail below. The following description of the components may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, the use of "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower limit and upper limit. In addition, in the description of groups (atomic groups) in this specification, descriptions that do not indicate whether they are substituted or unsubstituted include those that have no substituents as well as those that have a substituent. For example, an "alkyl group" includes not only an alkyl group that has no substituents (unsubstituted alkyl groups) but also an alkyl group that has a substituent (substituted alkyl groups). In this specification, "(meth)acrylic" is a term used as a concept including both acrylic and methacrylic, and "(meth)acryloyl" is a term used as a concept including both acryloyl and methacryloyl. In addition, the term "process" in this specification includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. In the present invention, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous. Unless otherwise specified, each component in the composition or each structural unit in the polymer in the present invention may be contained alone or in combination of two or more types. Furthermore, in the present invention, the amount of each component in the composition or each structural unit in the polymer means, when a plurality of substances or structural units corresponding to each component or each structural unit in the polymer are present in the composition, the total amount of the corresponding plurality of substances present in the composition or the corresponding plurality of structural units present in the polymer, unless otherwise specified. Furthermore, in the present invention, combinations of two or more preferred embodiments are more preferred embodiments. In the present invention, unless otherwise specified, the weight average molecular weight (Mw) and number average molecular weight (Mn) are molecular weights detected by a gel permeation chromatography (GPC) analyzer using columns of TSKgel GMHxL, TSKgel G4000HxL, or TSKgel G2000HxL (all of which are product names manufactured by Tosoh Corporation) in a solvent of THF (tetrahydrofuran) and a differential refractometer, and converted using polystyrene as a standard substance. The dummy lithographic printing plate does not necessarily require exposure or development. The dummy lithographic printing plate is a lithographic printing plate precursor that is attached to an unused plate cylinder when, for example, a portion of a page is printed in one color or two colors in color newspaper printing. The present invention will be described in detail below.

[0027] [On-press development type lithographic printing plate original plate] The on-press development type lithographic printing plate precursor according to the present invention (hereinafter, also simply referred to as "lithographic printing plate precursor") is An on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, the on-press development type lithographic printing plate precursor having a sagging region at an edge portion, the sagging region has a crack whose deepest portion reaches the aluminum support, Phosphate compounds are present in the cracks, a ratio of phosphorus to aluminum (P / Al) measured by FE-AES on the surface of a crack region formed in the aluminum support inside the crack is 0.04 or more, and when a solid content of one or more constituent layers at the end of the on-press development type lithographic printing plate precursor is A and a solid content of one or more constituent layers in a region other than the end of the on-press development type lithographic printing plate precursor is B, A≧B, and the difference between A and B, AB, is 0.8 g / m 2 is less than This is an on-press development type lithographic printing plate precursor.

[0028] The dummy planographic printing plate according to the present invention (hereinafter, simply referred to as the dummy planographic printing plate) is A dummy lithographic printing plate having an aluminum support having an anodized film and one or more constituent layers including a polymer layer, and having a sagging region at an edge, the sagging region has a crack whose deepest portion reaches the aluminum support, Phosphate compounds are present in the cracks, a ratio of phosphorus to aluminum (P / Al) measured by FE-AES on a surface of a crack region formed in the aluminum support inside the crack is 0.04 or more; When the solid content of one or more constituent layers at the end of the dummy planographic printing plate is A and the solid content of one or more constituent layers in the region other than the end of the dummy planographic printing plate is B, A≧B, and the difference between A and B, AB, is 0.8 g / m 2 is less than This is a dummy lithographic printing plate.

[0029] According to the on-press development type lithographic printing plate precursor and lithographic printing plate dummy plate of the present invention, by adopting the above-mentioned configuration, it is possible to provide an on-press development type lithographic printing plate precursor and lithographic printing plate dummy plate, as well as a method for producing the same, which can achieve both extremely excellent setter plate feeding performance and extremely excellent edge stain suppression performance. The reason for this is not clear, but is speculated to be as follows.

[0030] First, a lithographic printing plate precursor having an aluminum support with an anodized film and one or more constituent layers including an image recording layer often has a sagging region formed at the edge portion after cutting, etc. Here, when the sagging region is formed, a crack is often formed whose deepest portion reaches the aluminum support (a portion made of aluminum that is deeper than the anodized film, as described later) in the sagging region. It is believed that one of the causes of edge staining is the adhesion of ink to the inside of such cracks during printing, and therefore the above-mentioned conventional technology is known, but as mentioned above, further suppression of edge staining is expected. The on-press development type lithographic printing plate precursor and dummy lithographic printing plate of the present invention are configured such that a phosphorus compound is present in the crack whose deepest portion reaches the aluminum support, and the ratio of phosphorus element to aluminum element (P / Al) measured by FE-AES (field emission Auger electron spectroscopy) on the surface of the crack region formed in the aluminum support inside the crack is 0.04 or more. Furthermore, the method for producing an on-press development type lithographic printing plate precursor and dummy lithographic printing plate of the present invention is a method that can suitably produce the on-press development type lithographic printing plate precursor and dummy lithographic printing plate of the present invention. The above P / Al of 0.04 or more indicates that a certain amount of phosphorus element is present in the deepest part of the crack, and it is considered that a phosphoric acid compound that is expected to suppress edge stains is present even in the deepest part of the crack. That is, in the on-press development type lithographic printing plate precursor and dummy lithographic printing plate of the present invention, it is considered that components that can suppress the occurrence of edge stains are more likely to be present inside the cracks that are considered to be the cause of the occurrence of edge stains, and as a result, it is considered that extremely excellent edge stain suppression performance can be achieved.

[0031] According to the inventors' investigations, it is difficult to achieve the P / Al of 0.04 or more with the above-mentioned technique of applying a liquid containing a component capable of suppressing the occurrence of edge stains to the edge or edge surface of a lithographic printing plate precursor, and the above-mentioned technique of performing on-press development using a lithographic printing plate precursor having a layer containing a component capable of suppressing the occurrence of edge stains, thereby dissolving the component capable of suppressing the occurrence of edge stains into printing ink or fountain solution and transferring it to the edge portion of the lithographic printing plate precursor. Furthermore, for example, in the above-mentioned technique of applying a liquid containing a component capable of suppressing the occurrence of edge stains to the edge or edge surface of a lithographic printing plate precursor, the solid content at the edge tends to increase, leading to an increase in edge thickness. Although lithographic printing plate precursors are generally appropriately removed from a laminate, if the edge thickness increases, the lithographic printing plate precursors come into close contact with each other during storage of the laminate, and when a lithographic printing plate precursor is removed, the underlying lithographic printing plate precursor also needs to be removed, and as described above, it has been found that there is room for improvement in so-called setter plate feeding performance. According to the on-press development type lithographic printing plate precursor and the dummy lithographic printing plate of the present invention, when the solid content of one or more constituent layers at the end of the on-press development type lithographic printing plate precursor is A and the solid content of one or more constituent layers in the region other than the end of the on-press development type lithographic printing plate precursor is B, A≧B, and the difference between A and B, AB, is 0.8 g / m 2 is less than. It is believed that by adjusting the difference in solid content (AB) above, it is possible to remove the lithographic printing plate precursor and the dummy lithographic printing plate from a stack of the lithographic printing plate precursors and the dummy lithographic printing plate placed on a setter while preventing the plates from adhering to each other. From the above, it is presumed that the present invention can achieve both extremely excellent setter plate feeding performance and extremely excellent edge stain suppression performance.

[0032] The method for producing the on-press development type lithographic printing plate precursor and the method for producing the dummy lithographic printing plate according to the present invention will be described later.

[0033] The on-press development type lithographic printing plate precursor according to the present invention will be described in detail below. On-press development is a method in which after image exposure, a lithographic printing plate precursor is mounted directly on a printing press without undergoing conventional wet development processing, and the non-image areas of the image recording layer are removed at an early stage of the normal printing process. A lithographic printing plate precursor that can be subjected to on-press development is an on-press development type lithographic printing plate precursor.

[0034] (lithographic printing plate original plate) First, the on-press development type lithographic printing plate precursor of the present invention will be described. The on-press development type lithographic printing plate precursor according to the present invention is an on-press development type lithographic printing plate precursor having an aluminum support having an anodized film, and one or more constituent layers including an image recording layer, and having a sagging region at an edge portion, the sagging region has a crack whose deepest portion reaches the aluminum support, Phosphate compounds are present in the cracks, the ratio of phosphorus to aluminum (P / AL) measured by FE-AES on the surface of a crack region formed in the aluminum support inside the crack is 0.04 or more, and when the solid content of one or more constituent layers at the end of the on-press development type lithographic printing plate precursor is A and the solid content of one or more constituent layers in the region other than the end of the on-press development type lithographic printing plate precursor is B, A≧B, and the difference between A and B, AB, is 0.8 g / m 2 It is an on-press development type lithographic printing plate precursor having a density of less than 100 nm.

[0035] (Aluminum support) The support is an aluminum support. The aluminum plate used for such an aluminum support is made of a dimensionally stable metal containing aluminum as the main component, i.e., aluminum or an aluminum alloy. It is preferably selected from a pure aluminum plate and an alloy containing aluminum as the main component and a trace amount of other elements.

[0036] The foreign elements contained in the aluminum alloy include silicon, iron, manganese, copper, magnesium, chromium, zinc, bismuth, nickel, titanium, etc. The content of foreign elements in the alloy is 10 mass% or less. Pure aluminum plate is preferable, but since completely pure aluminum is difficult to produce due to smelting technology, an alloy containing a small amount of foreign elements may be used. The composition of the aluminum plate used for the aluminum support is not specified, and conventionally known aluminum plates such as JIS A 1050, JIS A 1100, JIS A 3103, and JIS A 3005 can be appropriately used. The thickness of the support (preferably an aluminum plate) is preferably about 0.1 to 0.6 mm.

[0037] (anodic oxide film) The aluminum support in the present invention has an anodized film. The anodized film refers to an anodized film (preferably an anodized aluminum film) having extremely fine pores (also called micropores) formed on the surface of a support (preferably an aluminum plate) by anodizing treatment. The micropores extend from the surface of the anodized film opposite the support along the thickness direction (support side, depth direction). The average diameter (average opening diameter) of the micropores on the surface of the anodized film is preferably 7 nm to 150 nm, more preferably 10 nm to 100 nm, even more preferably 10 nm to 60 nm, particularly preferably 15 nm to 60 nm, and most preferably 18 nm to 40 nm, from the viewpoints of tone reproducibility, printing durability, and printing stain resistance. The depth of the micropores is preferably from 10 nm to 3,000 nm, more preferably from 10 nm to 2,000 nm, and even more preferably from 10 nm to 1,000 nm.

[0038] The shape of the micropores is usually a substantially straight tube shape (substantially cylindrical shape) in which the diameter of the micropores remains almost constant in the depth direction (thickness direction), but they may also be a cone shape in which the diameter decreases continuously in the depth direction (thickness direction), or a shape in which the diameter decreases discontinuously in the depth direction (thickness direction). An example of a micropore having a diameter that discontinuously decreases in the depth direction (thickness direction) is a micropore composed of a large diameter pore portion extending in the depth direction from the surface of the anodized film and a small diameter pore portion that communicates with the bottom of the large diameter pore portion and extends in the depth direction from the communicating position.

[0039] Specifically, micropores composed of large diameter pores extending 10 nm to 1,000 nm in the depth direction from the surface of the anodized film and small diameter pores that communicate with the bottoms of the large diameter pores and extend a further 20 to 2,000 nm in the depth direction from the communicating position are preferred. The large diameter hole portion and the small diameter hole portion will be described in detail below.

[0040] -Large diameter hole- The average diameter (average opening diameter) of the large diameter pores on the surface of the anodized film is preferably 7 nm to 150 nm, more preferably 10 nm to 100 nm, even more preferably 15 nm to 100 nm, particularly preferably 15 nm to 60 nm, and most preferably 18 nm to 40 nm, from the viewpoints of tone reproducibility, printing durability, and printing stain resistance. The average diameter of the large pores is calculated by observing the surface of the anodized film using a field emission scanning electron microscope (FE-SEM) at a magnification of 150,000 times (N=4), measuring the diameter of the micropores (large pores) present in an area of ​​400 nm x 600 nm in the four obtained images, and calculating the arithmetic mean value of the diameters. If the shape of the large-diameter hole is not circular, the equivalent circle diameter is used. The "equivalent circle diameter" is the diameter of a circle when the shape of the opening is assumed to be a circle having the same projected area as the projected area of ​​the opening.

[0041] The bottoms of the large diameter holes are preferably located at a depth of 70 nm to 1,000 nm (hereinafter also referred to as depth A) from the surface of the anodized film. In other words, the large diameter holes are preferably holes extending 70 nm to 1,000 nm in the depth direction (thickness direction) from the surface of the anodized film. In particular, the depth A is more preferably 90 nm to 850 nm, even more preferably 90 nm to 800 nm, and particularly preferably 90 nm to 600 nm, in terms of superior effects of the manufacturing method for the lithographic printing plate precursor. The depth is calculated as the arithmetic average value by taking a photograph (150,000 times) of the cross section of the anodized film, measuring the depths of 25 or more large diameter holes, and then calculating the depth.

[0042] The shape of the large diameter hole is not particularly limited, and may be, for example, a substantially straight tube shape (substantially cylindrical) or a cone shape with a diameter decreasing in the depth direction (thickness direction), with a substantially straight tube shape being preferred. The shape of the bottom of the large diameter hole is not particularly limited, and may be a curved (convex) or flat surface. The inner diameter of the large pore is not particularly limited, but is preferably about the same as or smaller than the diameter of the opening. The inner diameter of the large pore may differ from the diameter of the opening by about 1 nm to 10 nm.

[0043] -Small diameter hole- The small diameter hole is a hole that communicates with the bottom of the large diameter hole and extends further in the depth direction (thickness direction) from the communicating position. One small diameter hole usually communicates with one large diameter hole, but two or more small diameter holes may communicate with the bottom of one large diameter hole. The average diameter of the small diameter pores at the communicating positions is preferably 15 nm or less, more preferably 13 nm or less, more preferably 11 nm or less, and particularly preferably 10 nm or less. There is no particular lower limit, but a value of 5 nm is preferable.

[0044] The average diameter of the small pores is calculated by observing the surface of the anodized film with an FE-SEM at a magnification of 150,000 times, taking N=4 images, measuring the diameter of the micropores (small pores) present in the range of 400 nm × 600 nm in the four images obtained, and determining the arithmetic mean value of the diameters. If the large pores are deep, the upper part of the anodized film (the area where the large pores are located) may be cut (for example, cut with argon gas) as necessary, and then the surface of the anodized film may be observed with the FE-SEM to determine the average diameter of the small pores. If the shape of the small diameter hole is not circular, the equivalent circle diameter is used. The "equivalent circle diameter" is the diameter of a circle when the shape of the opening is assumed to be a circle with the same projected area as the projected area of ​​the opening.

[0045] The bottoms of the small diameter holes are preferably located at a position extending 20 nm to 2,000 nm in the depth direction from the communicating position with the large diameter hole (corresponding to the above-mentioned depth A). In other words, the small diameter holes are holes extending in the depth direction (thickness direction) from the communicating position with the large diameter hole, and the depth of the small diameter holes is preferably 20 nm to 2,000 nm, more preferably 100 nm to 1,500 nm, and particularly preferably 200 nm to 1,000 nm. The depth is calculated as the arithmetic average value by taking a photograph (150,000 times) of the cross section of the anodized film, measuring the depths of 25 or more small diameter holes, and then calculating the depth.

[0046] The shape of the small diameter hole is not particularly limited, and may be, for example, a substantially straight tube shape (substantially cylindrical) or a cone shape whose diameter decreases in the depth direction, with a substantially straight tube shape being preferred. The shape of the bottom of the small diameter hole is not particularly limited, and may be a curved (convex) or flat surface. The inner diameter of the small hole is not particularly limited, but may be approximately the same as the diameter at the communicating position, or may be smaller or larger than the above diameter. Note that the inner diameter of the small hole may usually differ from the diameter of the opening by about 1 nm to 10 nm.

[0047] The ratio of the average diameter of the large pores on the surface of the anodized film to the average diameter of the small pores at their connecting positions, i.e., (average diameter of the large pores on the surface of the anodized film) / (average diameter of the small pores at their connecting positions), is preferably 1.1 to 13, and more preferably 2.5 to 6.5. The ratio of the depth of the large diameter hole portions to the depth of the small diameter hole portions, (depth of the large diameter hole portions) / (depth of the small diameter hole portions), is preferably 0.005-50, and more preferably 0.025-40.

[0048] The shape of the micropores is generally a substantially straight tube (substantially cylindrical) shape in which the diameter of the micropores remains almost constant in the depth direction (thickness direction), but may also be a cone shape in which the diameter increases continuously in the depth direction (thickness direction), or a shape in which the diameter increases discontinuously in the depth direction (thickness direction). An example of a micropore whose diameter increases discontinuously in the depth direction (thickness direction) is a micropore composed of a small diameter pore portion extending in the depth direction from the surface of the anodized film and a large diameter pore portion that communicates with the bottom of the small diameter pore portion and extends in the depth direction from the communicating position.

[0049] Specifically, micropores composed of small diameter pores extending 10 nm to 1,000 nm in the depth direction from the surface of the anodized film and large diameter pores that communicate with the bottoms of the small diameter pores and extend a further 20 to 2,000 nm in the depth direction from the communicating position are preferred.

[0050] -Small diameter hole- The average diameter (average opening diameter) of the small holes on the surface of the anodized film is not particularly limited, but is preferably 35 nm or less, more preferably 25 nm or less, and particularly preferably 20 nm or less. There is no particular lower limit, but 15 nm is preferred. The average diameter of the small pores is calculated by observing the surface of the anodized film using a field emission scanning electron microscope (FE-SEM) at a magnification of 150,000 times (N=4), measuring the diameter of the micropores (large pores) present in an area of ​​400 nm x 600 nm in the four obtained images, and calculating the arithmetic mean value of the diameters. If the shape of the small diameter hole is not circular, the equivalent circle diameter is used. The "equivalent circle diameter" is the diameter of a circle when the shape of the opening is assumed to be a circle with the same projected area as the projected area of ​​the opening.

[0051] The bottoms of the small holes are preferably located at a depth of 70 nm to 1,000 nm (hereinafter also referred to as depth A') from the surface of the anodized film. In other words, the small holes are preferably holes extending 70 nm to 1,000 nm in the depth direction (thickness direction) from the surface of the anodized film. The depth is calculated as the arithmetic average value by taking a photograph (150,000 times) of the cross section of the anodized film, measuring the depths of 25 or more large diameter holes, and then calculating the depth.

[0052] The shape of the small diameter hole is not particularly limited, and may be, for example, a substantially straight tube shape (substantially cylindrical shape) or a cone shape whose diameter increases in the depth direction (thickness direction), with a substantially straight tube shape being preferred. The shape of the bottom of the small diameter hole is not particularly limited, and may be a curved (convex) shape or a flat shape. The inner diameter of the small hole is not particularly limited, but is preferably about the same as or smaller than the diameter of the opening. The inner diameter of the small hole may differ from the diameter of the opening by about 1 nm to 10 nm.

[0053] -Large diameter hole- The large diameter hole portion is a hole portion that communicates with the bottom of the small diameter hole portion and extends further in the depth direction (thickness direction) from the communicating position. Usually, two or more small diameter holes may communicate with the bottom of one large diameter hole portion. The average diameter of the large diameter pores at the communicating positions is preferably from 20 nm to 400 nm, more preferably from 40 nm to 300 nm, further preferably from 50 nm to 200 nm, and particularly preferably from 50 nm to 100 nm.

[0054] The average diameter of the large pores is calculated by observing the surface of the anodized film with an FE-SEM at a magnification of 150,000 times, taking N=4 images, measuring the diameter of the micropores (large pores) present in the range of 400 nm × 600 nm in the four images obtained, and determining the arithmetic average value of the diameters. If the small pores are deep, the upper part of the anodized film (the area where the small pores are located) may be cut (for example, cut with argon gas) as necessary, and then the surface of the anodized film may be observed with the FE-SEM to determine the average diameter of the large pores. If the shape of the large-diameter hole is not circular, the equivalent circle diameter is used. The "equivalent circle diameter" is the diameter of a circle when the shape of the opening is assumed to be a circle having the same projected area as the projected area of ​​the opening.

[0055] The bottoms of the large diameter holes are preferably located at positions extending 20 nm to 2,000 nm in the depth direction from the positions where the small diameter holes communicate with the large diameter holes (corresponding to the depth A' described above). In other words, the large diameter holes are holes extending in the depth direction (thickness direction) from the positions where the small diameter holes communicate with the large diameter holes, and the depth of the large diameter holes is preferably 20 nm to 2,000 nm, more preferably 100 nm to 1,500 nm, and particularly preferably 200 nm to 1,000 nm. The depth is calculated as the arithmetic average value by taking a photograph (150,000 times) of the cross section of the anodized film, measuring the depths of 25 or more large diameter holes, and then calculating the depth.

[0056] The shape of the large diameter hole is not particularly limited, and may be, for example, a substantially straight tube shape (substantially cylindrical) or a cone shape with a diameter decreasing in the depth direction, with a substantially straight tube shape being preferred. The shape of the bottom of the large diameter hole is not particularly limited, and may be a curved (convex) or flat surface. The inner diameter of the large diameter hole is not particularly limited, but may be approximately the same as the diameter at the communicating position, or may be smaller or larger than the above diameter. Note that the inner diameter of the large diameter hole may usually differ from the diameter of the opening by about 1 nm to 10 nm.

[0057] The support has an anodized coating, The anodized film is formed by sequentially depositing the following layers from the surface of the anodized film in the depth direction: an upper layer having a thickness of 30 to 500 nm and having micropores with an average diameter of 20 to 100 nm; an intermediate layer having a thickness of 100 to 300 nm and having micropores whose average diameter is 1 / 2 to 5 times the average diameter of the micropores in the upper micropore layer; and A lower layer 300-2000 nm thick with micropores with an average diameter of 15 nm or less It is preferred that the compound has the formula:

[0058] In an on-press development type lithographic printing plate precursor, from the viewpoint of improving image visibility, it is useful for the anodized film surface of the support (the surface on which the image recording layer is formed) to have high brightness. In the printing process of a lithographic printing plate, a plate inspection is usually performed to check whether the intended image has been recorded before the printing plate is mounted on a printing press. In the case of an on-press development type lithographic printing plate precursor, it is required to check the image at the stage where the image is exposed, so a means for generating a so-called print-out image in the image-exposed area is applied. A method for quantitatively evaluating the visibility (image visibility) of the image area of ​​an image-exposed on-press development type lithographic printing plate precursor can be to measure the lightness of the image-exposed area and the lightness of the unexposed area and determine the difference between them. Here, the lightness can be the lightness L* value in the CIEL*a*b* color system, and the measurement can be performed using a colorimeter (SpectroEye, manufactured by X-Rite Corporation). The greater the difference between the lightness of the image-exposed area and the lightness of the unexposed area obtained by measurement, the easier the image area is to see. It has been found that in order to increase the difference in brightness between the image-exposed and unexposed areas, it is effective to increase the brightness L* value in the CIEL*a*b* color system of the anodized film surface. In other words, the brightness L* value is preferably 60 to 100.

[0059] If necessary, the support having an anodized coating may have a backcoat layer containing an organic polymer compound described in JP-A-5-45885 or a silicon alkoxy compound described in JP-A-6-35174 on the side opposite to the side on which the constituent layer containing a hydroxy acid compound having two or more hydroxyl groups is formed.

[0060] (Production of aluminum substrate having anodized film) As an example of the support, a method for producing an aluminum support having an anodized film will be described. The aluminum support having an anodized film can be manufactured by a known method. The manufacturing method of the aluminum support having an anodized film is not particularly limited. A preferred embodiment of the manufacturing method of the aluminum support having an anodized film includes a step of roughening an aluminum plate (roughening treatment step), a step of anodizing the roughened aluminum plate (anodizing treatment step), and a step of contacting the aluminum plate having an anodized film obtained in the anodizing treatment step with an acid aqueous solution or an alkali aqueous solution to expand the diameter of the micropores in the anodized film (pore widening treatment step).

[0061] Each step will be described in detail below.

[0062] <Surface roughening process> The surface roughening step is a step of performing a surface roughening treatment, including an electrochemical surface roughening treatment, on the surface of the aluminum plate. The surface roughening step is preferably performed before the anodizing step described below, but may not be performed if the surface of the aluminum plate already has a desired surface shape.

[0063] The surface roughening treatment may be performed by electrochemical surface roughening alone, or may be performed by combining electrochemical surface roughening treatment with at least one of mechanical surface roughening treatment and chemical surface roughening treatment. When mechanical graining and electrochemical graining are combined, it is preferable to carry out the electrochemical graining after the mechanical graining.

[0064] The electrochemical graining treatment is preferably carried out in an aqueous solution of nitric acid or hydrochloric acid.

[0065] Mechanical graining is generally performed for the purpose of making the surface of an aluminum plate have a surface roughness Ra of 0.35 to 1.0 μm. The conditions for the mechanical graining treatment are not particularly limited, but the treatment can be carried out, for example, according to the method described in JP-B-50-40047. The mechanical graining treatment can be carried out by a brush graining treatment using a pumice suspension or by a transfer method. The chemical graining treatment is not particularly limited, and can be carried out according to a known method.

[0066] After the mechanical roughening treatment, it is preferable to carry out the following chemical etching treatment. The chemical etching treatment carried out after the mechanical graining treatment is carried out to smooth the uneven edges of the surface of the aluminum plate, prevent the ink from catching during printing, improve the stain resistance of the lithographic printing plate, and remove unwanted material such as abrasive particles remaining on the surface. Known chemical etching processes include acid etching and alkali etching, but a method that is particularly excellent in terms of etching efficiency is chemical etching using an alkaline solution (hereinafter also referred to as "alkaline etching process").

[0067] The alkaline agent used in the alkaline solution is not particularly limited, but suitable examples include caustic soda, caustic potash, sodium metasilicate, sodium carbonate, sodium aluminate, and sodium gluconate. The alkaline solution may contain aluminum ions. The concentration of the alkaline agent in the alkaline solution is preferably 0.01% by mass or more, more preferably 3% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less. Furthermore, the temperature of the alkaline solution is preferably at least room temperature, more preferably at least 30°C, and is preferably at most 80°C, more preferably at most 75°C.

[0068] The etching amount is 0.01 g / m 2 More than 0.05 g / m is preferable. 2 More preferably, 30 g / m 2 Less than 20 g / m is preferable. 2 The following is more preferred: The treatment time is preferably 2 seconds to 5 minutes depending on the amount of etching, and more preferably 2 to 10 seconds from the viewpoint of improving productivity.

[0069] When an alkaline etching treatment is performed after a mechanical roughening treatment, it is preferable to perform a chemical etching treatment (hereinafter also referred to as a "desmutting treatment") using a low-temperature acidic solution in order to remove products produced by the alkaline etching treatment. The acid used in the acidic solution is not particularly limited, but examples thereof include sulfuric acid, nitric acid, and hydrochloric acid. The concentration of the acidic solution is preferably 1 to 50% by mass. The temperature of the acidic solution is preferably 20 to 80° C. When the concentration and temperature of the acidic solution are within these ranges, the resistance to dot-like staining in a lithographic printing plate using an aluminum support is further improved.

[0070] A preferred embodiment of the surface roughening treatment step will be exemplified below. -Aspect SA- The process shown in (1) to (8) is carried out in this order. (1) Chemical etching treatment using an alkaline aqueous solution (first alkaline etching treatment) (2) Chemical etching treatment using an acidic aqueous solution (first desmutting treatment) (3) Electrochemical roughening treatment using an aqueous solution mainly containing nitric acid (first electrochemical roughening treatment) (4) Chemical etching treatment using an alkaline aqueous solution (second alkaline etching treatment) (5) Chemical etching treatment using an acidic aqueous solution (second desmutting treatment) (6) Electrochemical roughening treatment using an aqueous solution mainly containing hydrochloric acid (second electrochemical roughening treatment) (7) Chemical etching treatment using an alkaline aqueous solution (third alkaline etching treatment) (8) Chemical etching treatment using an acidic aqueous solution (third desmutting treatment)

[0071] -SB- The process shown in (11) to (15) is carried out in this order. (11) Chemical etching treatment using an alkaline aqueous solution (fourth alkaline etching treatment) (12) Chemical etching treatment using an acidic aqueous solution (fourth desmutting treatment) (13) Electrochemical roughening treatment using an aqueous solution mainly containing hydrochloric acid (third electrochemical roughening treatment) (14) Chemical etching treatment using an alkaline aqueous solution (fifth alkaline etching treatment) (15) Chemical etching treatment using an acidic aqueous solution (5th desmutting treatment)

[0072] Before the treatment (1) of the above-mentioned embodiment SA or before the treatment (11) of the embodiment SB, a mechanical graining treatment may be carried out, if necessary.

[0073] The amount of aluminum plate dissolved in the first and fourth alkaline etching treatments was 0.5 g / m 2 ~30g / m 2 is preferred, and 1.0 g / m 2 ~20g / m 2 is more preferred.

[0074] The aqueous solution mainly containing nitric acid for use in the first electrochemical graining treatment in embodiment SA may be an aqueous solution for use in electrochemical graining treatment using direct or alternating current, such as an aqueous solution obtained by adding aluminum nitrate, sodium nitrate, ammonium nitrate, or the like to a 1 g / L to 100 g / L aqueous solution of nitric acid. The aqueous solution mainly containing hydrochloric acid used in the second electrochemical graining treatment in embodiment SA and the third electrochemical graining treatment in embodiment SB includes an aqueous solution used in electrochemical graining treatment using direct or alternating current. For example, an aqueous solution obtained by adding 0 g / L to 30 g / L of sulfuric acid to an aqueous solution of 1 g / L to 100 g / L of hydrochloric acid may be included. Note that this aqueous solution may further include nitrate ions such as aluminum nitrate, sodium nitrate, or ammonium nitrate; or chloride ions such as aluminum chloride, sodium chloride, or ammonium chloride.

[0075] The AC power waveform for the electrochemical graining treatment may be a sine wave, a square wave, a trapezoidal wave, a triangular wave, etc. The frequency is preferably 0.1 Hz to 250 Hz. FIG. 1 is a graph showing an example of an alternating current waveform used in electrochemical surface roughening treatment. In FIG. 1, ta is the anode reaction time, tc is the cathode reaction time, tp is the time from 0 to the peak current, Ia is the current at the peak on the anode cycle side, and Ic is the current at the peak on the cathode cycle side. In the trapezoidal wave, the time tp from 0 to the peak current is preferably 1 msec to 10 msec. The conditions for one cycle of AC used in the electrochemical graining treatment are preferably such that the ratio tc / ta of the anode reaction time ta to the cathode reaction time tc of the aluminum plate is 1 to 20, the ratio Qc / Qa of the quantity of electricity Qc when the aluminum plate is the anode to the quantity of electricity Qa when the aluminum plate is the anode is 0.3 to 20, and the anode reaction time ta is in the range of 5 msec to 1,000 msec. The current density is the peak value of the trapezoidal wave, and both the anode cycle side Ia and the cathode cycle side Ic of the current are 10 to 200 A / dm 2 The ratio Ic / Ia is preferably 0.3 to 20. The total amount of electricity involved in the anodic reaction of the aluminum plate at the time when the electrochemical graining treatment is completed is 25 C / dm 2 ~1,000C / dm 2 is preferred.

[0076] For electrochemical roughening treatment using alternating current, the device shown in FIG. 2 can be used. FIG. 2 is a side view showing an example of a radial cell for electrochemical surface roughening treatment using an alternating current. 2, 50 is a main electrolytic cell, 51 is an AC power source, 52 is a radial drum roller, 53a and 53b are main electrodes, 54 is an electrolyte supply port, 55 is an electrolyte, 56 is a slit, 57 is an electrolyte passage, 58 is an auxiliary anode, 60 is an auxiliary anode cell, and W is an aluminum plate. When two or more electrolytic cells are used, the electrolysis conditions may be the same or different. The aluminum sheet W is wound around a radial drum roller 52 immersed in a main electrolytic cell 50, and is electrolyzed by main electrodes 53a and 53b connected to an AC power source 51 during transportation. An electrolyte 55 is supplied from an electrolyte supply port 54 through a slit 56 to an electrolyte passage 57 between the radial drum roller 52 and the main electrodes 53a and 53b. The aluminum sheet W treated in the main electrolytic cell 50 is then electrolyzed in an auxiliary anode cell 60. In this auxiliary anode cell 60, an auxiliary anode 58 is disposed opposite the aluminum sheet W, and the electrolyte 55 is supplied so as to flow through the space between the auxiliary anode 58 and the aluminum sheet W.

[0077] The amount of aluminum plate dissolved in the second alkaline etching treatment is set to 1.0 g / m2 in order to facilitate the production of a desired lithographic printing plate precursor. 2 ~20g / m 2 is preferred, and 2.0 g / m 2 ~10g / m 2 is more preferred.

[0078] The amount of dissolution of the aluminum plate in the third alkaline etching treatment and the fifth alkaline etching treatment is set to 0.01 g / m so as to facilitate the production of a desired lithographic printing plate precursor. 2 ~0.8g / m 2 is preferred, and 0.05 g / m 2 ~0.3g / m 2 is more preferred.

[0079] In the chemical etching treatments (first to fifth desmutting treatments) using an acidic aqueous solution, an acidic aqueous solution containing phosphoric acid, nitric acid, sulfuric acid, chromic acid, hydrochloric acid, or a mixed acid containing two or more of these acids is suitably used. The concentration of the acid in the acidic aqueous solution is preferably 0.5% by mass to 60% by mass.

[0080] <Anodizing process> The anodizing process is a process for forming an aluminum oxide film on the surface of the aluminum plate by anodizing the aluminum plate that has been subjected to the surface roughening process. The anodizing process forms an aluminum anodized film having micropores on the surface of the aluminum plate. The anodizing treatment can be carried out according to a method conventionally known in this field by appropriately setting the production conditions taking into consideration the desired shape of the micropores, etc.

[0081] In the anodizing process, an aqueous solution of sulfuric acid, phosphoric acid, oxalic acid, or the like can be mainly used as the electrolyte. In some cases, an aqueous or non-aqueous solution of chromic acid, sulfamic acid, benzenesulfonic acid, or the like, or a combination of two or more of these, can also be used. When a direct or alternating current is passed through the aluminum plate in the electrolyte, an anodized film can be formed on the surface of the aluminum plate. The electrolyte may contain aluminum ions. The content of aluminum ions is not particularly limited, but is preferably 1 to 10 g / L.

[0082] The conditions for the anodizing treatment are appropriately set depending on the electrolyte used, but generally, the electrolyte concentration is 1 to 80 mass % (preferably 5 to 20 mass %), the solution temperature is 5 to 70°C (preferably 10 to 60°C), and the current density is 0.5 to 60 A / dm 2 (Preferably 5 to 50 A / dm 2 ), a voltage of 1 to 100 V (preferably 5 to 50 V), and an electrolysis time of 1 to 100 seconds (preferably 5 to 60 seconds) are appropriate.

[0083] A preferred example of the anodizing treatment is the method described in British Patent No. 1,412,768, in which anodizing is carried out in sulfuric acid at a high current density.

[0084] The anodizing treatment can be performed multiple times. One or more of the conditions such as the type, concentration, temperature, current density, voltage, and electrolysis time of the electrolyte used in each anodizing treatment can be changed. When the anodizing treatment is performed twice, the first anodizing treatment is sometimes called the first anodizing treatment, and the second anodizing treatment is sometimes called the second anodizing treatment. By performing the first anodizing treatment and the second anodizing treatment, anodized films having different shapes can be formed, making it possible to provide a lithographic printing plate precursor with excellent printing performance. Furthermore, it is also possible to carry out the pore widening treatment described below following the anodizing treatment, and then carry out the anodizing treatment again. In this case, the first anodizing treatment, the pore widening treatment, and the second anodizing treatment are carried out. By utilizing the method of performing the above-mentioned first anodizing treatment, pore widening treatment, and second anodizing treatment, it is possible to form micropores consisting of large diameter pores extending in the depth direction from the surface of the anodized film described above and small diameter pores that communicate with the bottom of the large diameter pores and extend in the depth direction from the communicating position.

[0085] <Pore widening process> The pore widening treatment step is a treatment (pore diameter enlargement treatment) for enlarging the diameter of the micropores present in the anodized film formed by the anodized film treatment step described above. This pore widening treatment enlarges the diameter of the micropores, forming an anodized film having micropores with a larger average diameter.

[0086] The pore widening treatment can be carried out by contacting the aluminum plate obtained by the above-mentioned anodizing treatment step with an acid aqueous solution or an alkaline aqueous solution. The contacting method is not particularly limited, and examples thereof include an immersion method and a spray method. Among these, the immersion method is preferred.

[0087] When an alkaline aqueous solution is used in the pore widening treatment step, it is preferable to use at least one alkaline aqueous solution selected from the group consisting of sodium hydroxide, potassium hydroxide, and lithium hydroxide. The concentration of the alkaline aqueous solution is preferably 0.1 to 5 mass%. It is appropriate to adjust the pH of the alkaline aqueous solution to 11 to 13, and contact the aluminum sheet with the alkaline aqueous solution for 1 to 300 seconds (preferably 1 to 50 seconds) under conditions of 10 to 70°C (preferably 20 to 50°C). In this case, the alkaline treatment liquid may contain metal salts of polyvalent weak acids such as carbonates, borates, and phosphates.

[0088] When an aqueous acid solution is used in the pore widening treatment step, it is preferable to use an aqueous solution of an inorganic acid such as sulfuric acid, phosphoric acid, nitric acid, or hydrochloric acid, or a mixture thereof. The concentration of the aqueous acid solution is preferably 1 to 80% by mass, more preferably 5 to 50% by mass. It is appropriate to contact the aluminum sheet with the aqueous acid solution for 1 to 300 seconds (preferably 1 to 150 seconds) under conditions of a liquid temperature of the aqueous acid solution of 5 to 70°C (preferably 10 to 60°C). The alkaline or acidic aqueous solution may contain aluminum ions. The content of aluminum ions is not particularly limited, but is preferably 1 to 10 g / L.

[0089] The method for producing an aluminum support having an anodized film may include a hydrophilization treatment step in which a hydrophilization treatment is carried out after the pore widening treatment step. For the hydrophilization treatment, a known method described in paragraphs 0109 to 0114 of JP-A-2005-254638 can be used.

[0090] The hydrophilization treatment is preferably carried out by a method of immersing the substrate in an aqueous solution of an alkali metal silicate such as sodium silicate or potassium silicate, or by a method of coating a hydrophilic vinyl polymer or a hydrophilic compound to form a hydrophilic undercoat layer.

[0091] The hydrophilization treatment with an aqueous solution of an alkali metal silicate such as sodium silicate or potassium silicate can be carried out according to the method and procedure described in US Pat. Nos. 2,714,066 and 3,181,461.

[0092] The amount of the anodized film of the anodized film is not particularly limited, but is preferably 3.0 g / m 2 It is preferable that the content is 2.5 g / m or less. 2 More preferably, it is 2.0 g / m or less. 2 It is even more preferable that: The amount of the anodized film of the anodized film is not particularly limited, but is preferably 0.5 g / m 2 More preferably, it is equal to or greater than this.

[0093] The amount of the anodized film of the anodized film is calculated by the following method. The constituent layers of the lithographic printing plate precursor (undercoat layer, image recording layer, protective layer) are removed using a PlasmaReactor PR300 manufactured by Yamato Scientific Co., Ltd. The surface of the anodized film on the exposed aluminum support is measured with a fluorescent X-ray analyzer (ZSX PrimusII manufactured by Rigaku Co., Ltd.), and the anodized film weight (g / m2) of the anodized film is calculated using a separately prepared calibration curve. 2 ) is calculated. A calibration curve was created from the relationship between the Compton scattering intensity obtained from the X-ray fluorescence analyzer and the amount of anodized film calculated by the Mason method. To improve the measurement accuracy of the Mason method, all Mason solutions were new. The conditions for the X-ray fluorescence analysis were as follows: X-ray tube: Rh, measurement spectrum: RhLα, tube voltage: 50 kV, tube current: 60 mA, slit: S2, analyzing crystal: Ge, detector: PC, analysis area: 30 mmφ, peak position (2θ): 89.510 deg., background (2θ): 87.000 deg. and 92.000 deg., accumulation time: 60 seconds / sample.

[0094] As described above, the on-press development type lithographic printing plate precursor of the present invention has an aluminum support having an anodized film, and the sagging region has cracks whose deepest parts reach the aluminum support, but the "aluminum support" in the "aluminum support having an anodized film" is intended not to include the region of the "anodized film" formed on the aluminum support by the above-mentioned treatment or the like. That is, the "aluminum support" in the present invention is intended to mean a portion made of aluminum that is deeper than the anodized film. Therefore, the "crack region formed in the aluminum support inside the crack" in the "ratio of phosphorus element to aluminum element (P / Al) measured by FE-AES on the surface of the crack region formed in the aluminum support inside the crack" in the present invention is intended to mean a crack region formed in a portion made of aluminum that exists at a position deeper than the crack region formed in the anodized film.

[0095] The same applies to the dummy planographic printing plate precursor described below.

[0096] [Phosphate compounds] In the on-press development type lithographic printing plate precursor of the invention, at least one of the one or more constituent layers including the image recording layer may or may not contain a phosphoric acid compound. The phosphoric acid compound preferably does not have an unsaturated double bond group in the molecule, and the content of the phosphoric acid compound is preferably substantially the same in at least one surface of one or more constituent layers including the image recording layer.

[0097] The phosphoric acid compound is not particularly limited, but is a compound containing a phosphorus atom and an acid group such as -PO3H2, -OPO3H2, -PO2H2, etc. The acid group may form a salt. Examples of salts formed by the acid group include alkali metal salts, alkaline earth metal salts, and ammonium salts. The compound preferably does not have an unsaturated double bond group in the molecule. The content of the compound is preferably substantially the same in at least one surface of one or more layers including the image recording layer. Phosphoric acid compounds have the ability to adsorb to the support, and have the property of efficiently adsorbing to cracks during on-press development and making the cracks hydrophilic, thereby contributing to the prevention of edge stains.

[0098] The molecular weight of the phosphoric acid compound is preferably 1,000 or less. By having a molecular weight of 1,000 or less, the compound is easily transferred to the surface of the anodized film during on-machine development, and is also easily transferred to cracks whose deepest parts reach the aluminum support, thereby obtaining an excellent edge stain prevention effect. The molecular weight is preferably 50 to 1,000, more preferably 50 to 800, and even more preferably 50 to 600.

[0099] It is preferable that the phosphoric acid compound does not have an unsaturated double bond group in the molecule. The unsaturated double bond group is a group having polymerizability, and includes ethylenically unsaturated groups such as (meth)acrylic groups, vinyl groups, allyl groups, and styryl groups. Since the phosphoric acid compound does not have an unsaturated double bond group in the molecule, it is possible to prevent the phosphoric acid compound from curing together with at least one of the one or more constituent layers including the image recording layer upon exposure.

[0100] In a preferred embodiment, the phosphoric acid compound includes phosphoric acid, phosphonic acid, and phosphinic acid. The above phosphoric acid, phosphonic acid and phosphinic acid may form a salt. The counter cation in the above phosphate, phosphonate, and phosphinate is not particularly limited, but metal ions, onium ions, etc. are preferably used. Among them, sodium ions, potassium ions, calcium ions, lithium ions, ammonium ions, sulfonium ions, etc. are preferably used as the counter cation in view of ease of handling and solubility in the coating liquid.

[0101] The above salt preferably includes at least one selected from the group consisting of phosphates, phosphonates, and phosphinates.

[0102] Examples of phosphoric acid and phosphates include phosphoric acid, monosodium phosphate, disodium phosphate, trisodium phosphate, monopotassium phosphate, dipotassium phosphate, tripotassium phosphate, monoammonium phosphate, diammonium phosphate, hexametaphosphoric acid, sodium hexametaphosphate, phytic acid, sodium phytate, pyrophosphoric acid, sodium pyrophosphate, polyphosphoric acid, sodium polyphosphate, metaphosphoric acid, and sodium metaphosphate.

[0103] Examples of phosphonic acids and phosphonates include phosphonic acid, ethylphosphonic acid, propylphosphonic acid, i-propylphosphonic acid, butylphosphonic acid, hexylphosphonic acid, octylphosphonic acid, dodecylphosphonic acid, octadecylphosphonic acid, 2-hydroxyethylphosphonic acid, 1,5-pentanediphosphonic acid, aminomethylphosphonic acid, and the sodium, potassium, or ammonium salts of the above compounds. Examples of phosphinates include phosphinic acid, phenylphosphinic acid, diphenylphosphinic acid, and the sodium, potassium, or ammonium salts of the above compounds.

[0104] The phosphoric acid compound of the present invention is preferably at least one compound selected from the group consisting of phosphoric acid, phosphonic acid, phosphinic acid, phosphoric acid salts, phosphonic acid salts, and phosphinic acid salts, and more preferably at least one compound selected from the group consisting of phosphoric acid, phosphonic acid, phosphoric acid salts, and phosphonic acid salts. The above compounds are preferred because they are more easily adsorbed to cracks and have the property of making the cracks hydrophilic, and therefore contribute more to preventing edge stains.

[0105] The phosphoric acid compounds may be used alone or in combination of two or more. The content of the phosphoric acid compound is 10 to 200 mg / m from the viewpoint of suppressing edge staining and printing durability.2 is preferable, and 30 to 150 mg / m 2 More preferably, 50 to 100 mg / m 2 is more preferred.

[0106] In the present invention, it is preferable that the content of the phosphoric acid compound is substantially the same in at least one surface of one or more constituent layers including the image recording layer. Here, "the content of the phosphoric acid compound is substantially the same in at least one surface of one or more layers including the image recording layer" means that the phosphoric acid compound is almost uniformly present in at least one surface of one or more constituent layers including the image recording layer, and there is no substantial difference in the content of the phosphoric acid compound between the center and the edge of the lithographic printing plate precursor. That is, it means that there is no content difference other than the content difference of the phosphoric acid compound in at least one surface of one or more constituent layers including the image recording layer that may usually occur when at least one of the constituent layers including the image recording layer is coated. Therefore, it is preferable that the present invention is different from intentionally applying a phosphoric acid compound only to the edges of a lithographic printing plate precursor, thereby creating a state in which the content of the phosphoric acid compound at the edges is greater than the content of the phosphoric acid compound in areas other than the edges.

[0107] The layer to which the phosphoric acid compound is added is not particularly limited, but from the viewpoint of printing durability, it is preferable to add the phosphoric acid compound to a protective layer. In a preferred embodiment, at least one of the one or more constituent layers including the image recording layer is a protective layer.

[0108] In the lithographic printing plate precursor of the present invention, the "one or more constituent layers including an image recording layer" includes at least an image recording layer. The layer other than the image recording layer is not particularly limited, but examples thereof include an undercoat layer and a protective layer. The undercoat layer is formed on the support, and the protective layer is formed on the image recording layer. The "one or more constituent layers including an image-recording layer" includes the following four embodiments. <1> Image recording layer only <2> Undercoat layer and image recording layer <3> Image recording layer and protective layer <4> Undercoat layer, image recording layer, and protective layer

[0109] At least one of the one or more constituent layers is, for example, at least one layer selected from the group consisting of an image recording layer, an undercoat layer, and a protective layer. Furthermore, at least one of the one or more constituent layers may be, for example, two or more layers selected from the group consisting of an image recording layer, an undercoat layer, and a protective layer.

[0110] The lithographic printing plate precursor of the invention may or may not contain a phosphoric acid compound in at least one of the one or more constituent layers. In a preferred embodiment, the image recording layer contains the above phosphoric acid compound, in which at least one of the one or more layers is an image recording layer. In a preferred embodiment, the lithographic printing plate precursor of the present invention has an undercoat layer on a support, and the undercoat layer contains the above-mentioned phosphoric acid compound. In this case, at least one of the one or more layers is an undercoat layer. Furthermore, in one preferred embodiment, the lithographic printing plate precursor of the present invention has a protective layer on the image recording layer, and the protective layer contains the above phosphoric acid compound. In this case, at least one of the one or more layers is a protective layer.

[0111] The lithographic printing plate precursor of the present invention has one or more constituent layers including an image recording layer. The image recording layer is preferably a negative image recording layer, and more preferably a water-soluble or water-dispersible negative image recording layer. From the viewpoint of on-press developability, the lithographic printing plate precursor used in the invention preferably has an unexposed area of ​​the image recording layer that is removable with at least one of fountain solution and printing ink. The lithographic printing plate precursor of the present invention has an aluminum support and the above-mentioned image recording layer, and any of the following configurations can also be preferably mentioned. (1) The lithographic printing plate precursor has an aluminum support, an image recording layer, and a protective layer in this order. (2) The lithographic printing plate precursor has an aluminum support, an undercoat layer, and an image-recording layer in this order. (3) The lithographic printing plate precursor has an aluminum support, an undercoat layer, an image recording layer, and a protective layer in this order.

[0112] <Image recording layer> In the lithographic printing plate precursor of the invention, the image recording layer preferably contains a polymerizable compound, a polymerization initiator, and an infrared absorbing agent.

[0113] [Polymerizable compound] The image recording layer in the invention preferably contains a polymerizable compound. In the present invention, the polymerizable compound refers to a compound having a polymerizable group. The polymerizable group is not particularly limited and may be any known polymerizable group, but is preferably an ethylenically unsaturated group. The polymerizable group may be either a radically polymerizable group or a cationic polymerizable group, but is preferably a radically polymerizable group. Examples of the radically polymerizable group include a (meth)acryloyl group, an allyl group, a vinylphenyl group, and a vinyl group, and from the viewpoint of reactivity, a (meth)acryloyl group is preferred. The molecular weight of the polymerizable compound (when the polymerizable compound has a molecular weight distribution, the weight average molecular weight) is preferably 50 or more and less than 2,500.

[0114] The polymerizable compound used in the present invention may be, for example, a radically polymerizable compound or a cationic polymerizable compound, but is preferably an addition polymerizable compound having at least one ethylenically unsaturated bond (ethylenically unsaturated compound). The ethylenically unsaturated compound is preferably a compound having at least one terminal ethylenically unsaturated bond, more preferably a compound having two or more terminal ethylenically unsaturated bonds. The polymerizable compound has a chemical form such as a monomer, a prepolymer, i.e., a dimer, a trimer or an oligomer, or a mixture thereof. Among them, from the viewpoint of printing durability, the polymerizable compound preferably contains a trifunctional or more polymerizable compound, more preferably contains a heptafunctional or more polymerizable compound, and even more preferably contains a ten-functional or more polymerizable compound. Furthermore, from the viewpoint of printing durability of the resulting lithographic printing plate, the polymerizable compound preferably contains a trifunctional or more (preferably heptafunctional or more, more preferably ten-functional or more) ethylenically unsaturated compound, and even more preferably contains a trifunctional or more (preferably heptafunctional or more, more preferably ten-functional or more) (meth)acrylate compound.

[0115] Moreover, from the viewpoints of on-machine developability and stain suppression, the polymerizable compound preferably contains a polymerizable compound having two or fewer functionalities, more preferably contains a bifunctional polymerizable compound, and particularly preferably contains a bifunctional (meth)acrylate compound. From the viewpoints of printing durability, on-press developability, and stain suppression, the content of the difunctional or lower polymerizable compound (preferably a difunctional polymerizable compound) is preferably 5% by mass to 100% by mass, more preferably 10% by mass to 100% by mass, and particularly preferably 15% by mass to 100% by mass, relative to the total mass of the polymerizable compounds in the image recording layer.

[0116] -Oligomer- The polymerizable compound contained in the image recording layer preferably contains a polymerizable compound which is an oligomer (hereinafter, also simply referred to as "oligomer"). In the present invention, an oligomer refers to a polymerizable compound having a molecular weight (weight average molecular weight when the molecular weight has a molecular weight distribution) of 600 or more and 40,000 or less and containing at least one polymerizable group. From the viewpoint of excellent chemical resistance and printing durability, the molecular weight of the oligomer is preferably 1,000 or more and 25,000 or less.

[0117] From the viewpoint of improving printing durability, the number of polymerizable groups in one oligomer molecule is preferably 2 or more, more preferably 3 or more, even more preferably 6 or more, and particularly preferably 10 or more. The upper limit of the number of polymerizable groups in the oligomer is not particularly limited, but the number of polymerizable groups is preferably 20 or less.

[0118] From the viewpoints of printing durability and on-press developability, the oligomer preferably has 7 or more polymerizable groups and a molecular weight of 1,000 or more and 40,000 or less, and more preferably has 7 or more polymerizable groups and a molecular weight of 1,000 or more and 25,000 or less. In addition, the oligomer may contain a polymer component that may be generated during the production process of the oligomer.

[0119] From the viewpoints of printing durability, visibility, and on-press developability, the oligomer preferably contains at least one selected from the group consisting of a compound having a urethane bond, a compound having an ester bond, and a compound having an epoxy residue, and more preferably contains a compound having a urethane bond. In the present invention, the epoxy residue refers to a structure formed by an epoxy group, and means, for example, a structure similar to the structure obtained by the reaction of an acid group (such as a carboxylic acid group) with an epoxy group.

[0120] As a compound having a urethane bond, those described in WO 2020 / 262692 can be suitably used.

[0121] Furthermore, as the compound having a urethane bond, a compound in which a polymerizable group is introduced by a polymer reaction into a polyurethane obtained by reacting a polyisocyanate compound with a polyol compound may be used. For example, a compound having a urethane bond may be obtained by reacting a polyurethane oligomer obtained by reacting a polyol compound having an acid group with a polyisocyanate compound, with a compound having an epoxy group and a polymerizable group.

[0122] The number of polymerizable groups in the compound having an ester bond, which is an example of the oligomer, is preferably 3 or more, and more preferably 6 or more.

[0123] As a compound having an epoxy residue, which is an example of an oligomer, a compound containing a hydroxy group within the compound is preferred. The compound having an epoxy residue preferably has 2 to 6 polymerizable groups, and more preferably has 2 to 3 polymerizable groups. The compound having an epoxy residue can be obtained, for example, by reacting a compound having an epoxy group with acrylic acid.

[0124] Specific examples of oligomers are shown in the table below, but the oligomers used in the present invention are not limited to these. As the oligomer, commercially available products may be used, and examples thereof include UA510H, UA-306H, UA-306I, UA-306T (all manufactured by Kyoeisha Chemical Co., Ltd.), UV-1700B, UV-6300B, UV7620EA (all manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), U-15HA (manufactured by Shin-Nakamura Chemical Co., Ltd.), EBECRYL450, EBECRYL657, EBECRYL885, EBECRYL800, EBECRYL3416, EBECRYL860 (all manufactured by Daicel Allnex Corporation), but are not limited thereto.

[0125] From the viewpoint of improving chemical resistance, printing durability, and suppression of on-press development residue, the content of the oligomer is preferably 30% by mass to 100% by mass, more preferably 50% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass, relative to the total mass of the polymerizable compounds in the image recording layer.

[0126] -Low molecular polymerizable compounds- The polymerizable compound may further contain a polymerizable compound other than the above-mentioned oligomer. From the viewpoint of chemical resistance, the polymerizable compound other than the oligomer is preferably a low molecular weight polymerizable compound. The low molecular weight polymerizable compound may be in a chemical form such as a monomer, a dimer, a trimer, or a mixture thereof. From the viewpoint of chemical resistance, the low molecular weight polymerizable compound is preferably at least one polymerizable compound selected from the group consisting of polymerizable compounds having three or more ethylenically unsaturated groups and polymerizable compounds having an isocyanuric ring structure.

[0127] In the present invention, the low molecular weight polymerizable compound refers to a polymerizable compound having a molecular weight of 50 or more and less than 800 (weight average molecular weight when the compound has a molecular weight distribution). From the viewpoint of excellent chemical resistance, printing durability, and suppression of on-press development residue, the molecular weight of the low molecular weight polymerizable compound is preferably 100 or more and less than 800, more preferably 300 or more and less than 800, and even more preferably 400 or more and less than 800.

[0128] When the polymerizable compound contains a low molecular weight polymerizable compound as a polymerizable compound other than an oligomer (when two or more kinds of low molecular weight polymerizable compounds are contained, the total amount thereof), from the viewpoints of chemical resistance, printing durability, and suppression of on-press development residue, the ratio of the oligomer to the low molecular weight polymerizable compound (oligomer / low molecular weight polymerizable compound) is preferably 10 / 1 to 1 / 10, more preferably 10 / 1 to 3 / 7, and even more preferably 10 / 1 to 7 / 3, by mass.

[0129] In addition, as the low molecular weight polymerizable compound, the polymerizable compounds described in paragraphs 0082 to 0086 of WO 2019 / 013268 can also be suitably used.

[0130] Details of the method of use, such as the structure of the polymerizable compound, whether it is used alone or in combination, and the amount added, can be set arbitrarily. In particular, from the viewpoint of printing durability, it is preferable that the image recording layer contains two or more types of polymerizable compounds. The content of the polymerizable compounds (when two or more types of polymerizable compounds are contained, the total content of the polymerizable compounds) is preferably 5% by mass to 75% by mass, more preferably 10% by mass to 70% by mass, and even more preferably 15% by mass to 60% by mass, based on the total solid content of the image recording layer.

[0131] [Polymerization initiator] The image recording layer in the invention preferably contains a polymerization initiator. Moreover, from the viewpoints of sensitivity, printing durability, on-press developability, and ink receptivity, the polymerization initiator preferably contains an electron-donating polymerization initiator, and more preferably contains an electron-accepting polymerization initiator and an electron-donating polymerization initiator.

[0132] -Electron-accepting polymerization initiator- The image recording layer preferably contains an electron-accepting polymerization initiator as the polymerization initiator. The electron-accepting polymerization initiator is a compound that generates a polymerization initiating species such as a radical by accepting one electron through intermolecular electron transfer when electrons of an infrared absorbing agent are excited by exposure to infrared light. The electron-accepting polymerization initiator used in the present invention is a compound that generates a polymerization initiating species such as a radical or a cation by the energy of light, heat or both, and can be appropriately selected from known thermal polymerization initiators, compounds having a bond with small bond dissociation energy, photopolymerization initiators, etc. As the electron-accepting polymerization initiator, a radical polymerization initiator is preferable, and an onium compound is more preferable. The electron-accepting polymerization initiator is preferably an infrared-sensitive polymerization initiator. Examples of the electron-accepting radical polymerization initiator include (a) organic halides, (b) carbonyl compounds, (c) azo compounds, (d) organic peroxides, (e) metallocene compounds, (f) azide compounds, (g) hexaarylbiimidazole compounds, (i) disulfone compounds, (j) oxime ester compounds, and (k) onium compounds.

[0133] As the (a) organic halide, for example, the compounds described in paragraphs 0022 to 0023 of JP-A No. 2008-195018 are preferable. As the (b) carbonyl compound, for example, the compound described in paragraph 0024 of JP-A-2008-195018 is preferable. As the (c) azo compound, for example, the azo compounds described in JP-A-8-108621 can be used. (d) As the organic peroxide, for example, the compound described in paragraph 0025 of JP-A-2008-195018 is preferable. (e) As the metallocene compound, for example, the compound described in paragraph 0026 of JP-A-2008-195018 is preferable. (f) Examples of the azide compounds include 2,6-bis(4-azidobenzylidene)-4-methylcyclohexanone. (g) Preferred examples of the hexaarylbiimidazole compound include the compounds described in paragraph 0027 of JP-A-2008-195018. (i) Examples of the disulfone compound include the compounds described in JP-A-61-166544 and JP-A-2002-328465. As the (j) oxime ester compound, for example, the compounds described in paragraphs 0028 to 0030 of JP-A No. 2008-195018 are preferable.

[0134] Among the electron-accepting polymerization initiators, preferred are oxime ester compounds and onium compounds from the viewpoint of curability. Among them, preferred are iodonium salt compounds, sulfonium salt compounds and azinium salt compounds from the viewpoint of printing durability, more preferred are iodonium salt compounds and sulfonium salt compounds, and particularly preferred are iodonium salt compounds. Specific examples of these compounds are shown below, but the present invention is not limited to these.

[0135] Preferred examples of the iodonium salt compound include diaryliodonium salt compounds, more preferred are diphenyliodonium salt compounds substituted with electron-donating groups such as alkyl groups or alkoxy groups, and more preferred are asymmetric diphenyliodonium salt compounds. Specific examples include diphenyliodonium hexafluorophosphate, 4-methoxyphenyl-4-(2-methylpropyl)phenyliodonium hexafluorophosphate, 4-(2-methylpropyl)phenyl-p-tolyliodonium hexafluorophosphate, 4-hexyloxyphenyl-2,4,6-trimethoxyphenyliodonium hexafluorophosphate, 4-hexyloxyphenyl-2,4-diethoxyphenyliodonium tetrafluoroborate, 4-octyloxyphenyl-2,4,6-trimethoxyphenyliodonium 1-perfluorobutanesulfonate, 4-octyloxyphenyl-2,4,6-trimethoxyphenyliodonium hexafluorophosphate, and bis(4-t-butylphenyl)iodonium hexafluorophosphate.

[0136] As an example of the sulfonium salt compound, a triarylsulfonium salt compound is preferred, particularly a triarylsulfonium salt compound in which at least a part of the electron-withdrawing group, for example, the group on the aromatic ring, is substituted with a halogen atom, and more preferably a triarylsulfonium salt compound in which the total number of halogen atoms substituted on the aromatic ring is 4 or more. Specific examples include triphenylsulfonium hexafluorophosphate, triphenylsulfonium benzoylformate, bis(4-chlorophenyl)phenylsulfonium benzoylformate, bis(4-chlorophenyl)-4-methylphenylsulfonium tetrafluoroborate, tris(4-chlorophenyl)sulfonium 3,5-bis(methoxycarbonyl)benzenesulfonate, tris(4-chlorophenyl)sulfonium hexafluorophosphate, and tris(2,4-dichlorophenyl)sulfonium hexafluorophosphate.

[0137] As the counter anion of the iodonium salt compound and the sulfonium salt compound, a sulfonamide anion or a sulfonimide anion is preferable, and a sulfonimide anion is more preferable. The sulfonamide anion is preferably an arylsulfonamide anion. The sulfonimide anion is preferably a bisarylsulfonimide anion. Specific examples of sulfonamide anions or sulfonimide anions include those described in WO 2020 / 262692.

[0138] From the viewpoints of developability and printing durability of the resulting lithographic printing plate, the electron-accepting polymerization initiator may contain a compound represented by the following formula (II).

[0139] [ka]

[0140] In formula (II), X A represents a halogen atom, and R A represents an aryl group.

[0141] X in formula (II) A Specific examples of the atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Among these, a chlorine atom or a bromine atom is preferred because of its excellent sensitivity, and a bromine atom is particularly preferred. In addition, in formula (II), R A From the viewpoint of achieving an excellent balance between sensitivity and storage stability, an aryl group substituted with an amide group is preferred.

[0142] As specific examples of the electron-accepting polymerization initiator represented by the above formula (II), those described in WO 2020 / 262692 can be suitably used.

[0143] The lowest unoccupied molecular orbital (LUMO) of the electron-accepting polymerization initiator is preferably −3.00 eV or less, and more preferably −3.02 eV or less, from the viewpoints of improving sensitivity and preventing plate skipping. The lower limit is preferably −3.80 eV or more, and more preferably −3.60 eV or more.

[0144] The electron-accepting polymerization initiator may be used alone or in combination of two or more kinds. The content of the electron-accepting polymerization initiator is preferably 0.1% by mass to 50% by mass, more preferably 0.5% by mass to 30% by mass, and particularly preferably 0.8% by mass to 20% by mass, based on the total solid content of the image recording layer.

[0145] -Electron-donating polymerization initiator- From the viewpoint of contributing to improvement of the chemical resistance and printing durability of the lithographic printing plate, the polymerization initiator preferably contains an electron-donating polymerization initiator, and more preferably contains both the electron-donating polymerization initiator and the above-mentioned electron-donating polymerization initiator. Examples of the electron-donating polymerization initiator include the following five types. (i) Alkyl or aryl ate complexes: It is believed that the carbon-hetero bond is oxidatively cleaved to generate active radicals. Specific examples include borate compounds. (ii) Aminoacetic acid compounds: It is believed that the C-X bond on the carbon adjacent to the nitrogen is cleaved by oxidation to generate an active radical. X is preferably a hydrogen atom, a carboxyl group, a trimethylsilyl group, or a benzyl group. Specific examples include N-phenylglycines (which may have a substituent on the phenyl group), N-phenyliminodiacetic acid (which may have a substituent on the phenyl group), etc. (iii) Sulfur-containing compounds: The above-mentioned aminoacetic acid compounds, in which the nitrogen atom is replaced with a sulfur atom, can generate active radicals by the same action. A specific example is phenylthioacetic acid (the phenyl group may have a substituent). (iv) Tin-containing compounds: Compounds in which the nitrogen atom of the above-mentioned aminoacetic acid compounds is replaced with a tin atom can generate active radicals by the same action. (v) Sulfinates: These can generate active radicals by oxidation. Specific examples include sodium arylsulfinate.

[0146] Among these electron-donating polymerization initiators, the image recording layer preferably contains a borate compound from the viewpoints of printing durability and sensitivity. As the borate compound, a tetraarylborate compound or a monoalkyltriarylborate compound is preferred, and from the viewpoint of compound stability, a tetraarylborate compound is more preferred, and a tetraphenylborate compound is particularly preferred. The counter cation of the borate compound is not particularly limited, but is preferably an alkali metal ion or a tetraalkylammonium ion, and more preferably a sodium ion, a potassium ion, or a tetrabutylammonium ion.

[0147] A specific example of a preferred borate compound is sodium tetraphenylborate.

[0148] Preferred specific examples of the electron-donating polymerization initiator include those described in WO 2020 / 262692.

[0149] Furthermore, from the viewpoints of visibility, printing durability, and stability over time, the image recording layer preferably contains at least one compound selected from the group consisting of an onium compound as the electron-accepting polymerization initiator and a borate compound as the electron-donating polymerization initiator, and more preferably contains an onium compound as the electron-accepting polymerization initiator and a borate compound as the electron-donating polymerization initiator. The image recording layer preferably contains a borate compound as the electron-donating polymerization initiator. In a preferred embodiment, the electron-donating polymerization initiator is a borate compound.

[0150] The electron-donating polymerization initiator may be added either alone or in combination of two or more. The content of the electron-donating polymerization initiator is preferably from 0.01 to 30% by mass, more preferably from 0.05 to 25% by mass, and even more preferably from 0.1 to 20% by mass, based on the total solid content of the image recording layer.

[0151] In addition, one of the preferred embodiments of the present invention is an embodiment in which the electron-accepting polymerization initiator and the electron-donating polymerization initiator form a salt. Specifically, for example, the onium compound may be a salt of an onium ion and an anion in the electron-donating polymerization initiator (e.g., tetraphenylborate anion).More preferably, the onium compound may be an iodonium borate salt compound in which an iodonium cation in the iodonium salt compound (e.g., di-p-tolyliodonium cation) and a borate anion in the electron-donating polymerization initiator form a salt. Specific examples of the embodiment in which the electron-accepting polymerization initiator and the electron-donating polymerization initiator form a salt include those described in WO 2020 / 262692.

[0152] In the present invention, when the image recording layer contains an onium ion and an anion in the above-mentioned electron-donating polymerization initiator, the image recording layer contains an electron-accepting polymerization initiator and the above-mentioned electron-donating polymerization initiator.

[0153] [Infrared absorbing agent] The lithographic printing plate precursor used in the present invention preferably contains an infrared absorbing agent in the image recording layer. The infrared absorbing agent is not particularly limited, and examples thereof include pigments and dyes. As the dye to be used as the infrared absorber, commercially available dyes and known dyes described in literature such as "Dye Handbook" (edited by the Organic Synthesis Chemistry Association, published in 1970) can be used. Specific examples of the dye include azo dyes, metal complex azo dyes, pyrazolone azo dyes, naphthoquinone dyes, anthraquinone dyes, phthalocyanine dyes, carbonium dyes, quinoneimine dyes, methine dyes, cyanine dyes, squarylium dyes, pyrylium salts, and metal thiolate complex dyes.

[0154] Particularly preferred among these dyes are cyanine dyes, squarylium dyes, pyrylium salts, nickel thiolate complexes, and indolenine cyanine dyes.Furthermore, cyanine dyes and indolenine cyanine dyes are also preferred.Of these, cyanine dyes are particularly preferred.

[0155] The infrared absorbing agent is preferably a cationic polymethine dye having an oxygen or nitrogen atom at the meso position. Preferred examples of the cationic polymethine dye include cyanine dyes, pyrylium dyes, thiopyrylium dyes, and azulenium dyes, and from the viewpoints of availability, solubility in a solvent during the introduction reaction, and the like, cyanine dyes are preferred.

[0156] Specific examples of cyanine dyes include the compounds described in paragraphs 0017 to 0019 of JP-A-2001-133969, the compounds described in paragraphs 0016 to 0021 of JP-A-2002-023360, and the compounds described in paragraphs 0012 to 0037 of JP-A-2002-040638, preferably the compounds described in paragraphs 0034 to 0041 of JP-A-2002-278057, and the compounds described in paragraphs 0080 to 0086 of JP-A-2008-195018, and particularly preferably the compounds described in paragraphs 0035 to 0043 of JP-A-2007-90850, and the compounds described in paragraphs 0105 to 0113 of JP-A-2012-206495. In addition, the compounds described in paragraphs 0008 to 0009 of JP-A No. 5-5005 and paragraphs 0022 to 0025 of JP-A No. 2001-222101 can also be preferably used. As the pigment, the compounds described in paragraphs 0072 to 0076 of JP-A No. 2008-195018 are preferred.

[0157] The infrared absorbing agent preferably contains a compound represented by the following formula 4.

[0158] [ka]

[0159] In formula 4, R 14 and R 15 each independently represents a hydrogen atom or an alkyl group; R 14 and R 15 may be linked together to form a ring, R 16 ~R 19 each independently represents a hydrogen atom or an alkyl group; R 20 and R 21 each independently represents an alkyl group or an aryl group; Y3 and Y4 each independently represent an oxygen atom, a sulfur atom, -NR0- or a dialkylmethylene group; R0 represents a hydrogen atom, an alkyl group or an aryl group; Ar3 and Ar4 each independently represent a group forming a benzene ring or a naphthalene ring which may have a group represented by formula 5 described below; A1 is -NR 22 R 23 , -X5-L1 or a halogen atom; R 22 and R 23 Each of X5 and X6 independently represents an alkyl group, an aryl group, an alkoxycarbonyl group, or an arylsulfonyl group, X5 represents an oxygen atom or a sulfur atom, L1 represents a hydrocarbon group or a heteroaryl group, and Za represents a counter ion that neutralizes the charge. In formula 5, X6 is a halogen atom, -C(=O)-X7-R 24 , -C(=O)-NR 25 R 26 , -OC(=O)-R 27 , -CN, -SO2NR 28 R 29 or a perfluoroalkyl group; X7 represents a single bond or an oxygen atom; R24 and R 27 each independently represents an alkyl group or an aryl group; R 25 , R 26 , R 28 and R 29 each independently represents a hydrogen atom, an alkyl group, or an aryl group.

[0160] Ar3 and Ar4 each independently represent a group forming a benzene ring or a naphthalene ring. The benzene ring and the naphthalene ring may have a substituent other than -X6. The substituent may be an alkyl group, an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, or a combination of these groups, and is preferably an alkyl group. In a preferred embodiment, in formula 4, at least one of Ar3 and Ar4 preferably has a group represented by formula 5 above.

[0161] X6 in formula 5 is a halogen atom, -C(=O)-X7-R 24 , -C(=O)-NR 25 R 26 , -OC(=O)-R 27 , -CN, -SO2NR 28 R 29 or a perfluoroalkyl group, and from the viewpoints of printing durability, visibility, and stability over time, a halogen atom, -C(=O)-X7-R 24 , -C(=O)-NR 25 R 26 , -OC(=O)-R 27 , CN, or -SO2NR 28 R 29 is preferably a halogen atom, -C(=O)-OR 24 , -C(=O)-NR 25 R 26 , or -OC(=O)-R 27 is preferably a halogen atom, -C(=O)-OR 24 , or -OC(=O)-R 27More preferably, it is a fluorine atom, a chlorine atom, a bromine atom, or -C(=O)OR 30 It is more preferable that the atom is a chlorine atom or a bromine atom. X6 substituting Ar3 and X6 substituting Ar4 may be the same group or different groups. From the viewpoints of printing durability, visibility, and stability over time, X6 substituting Ar3 and X6 substituting Ar4 are preferably the same group.

[0162] X7 represents a single bond or an oxygen atom, and is preferably an oxygen atom. R 24 and R 27 each independently represents an alkyl group or an aryl group, preferably an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms. R 25 , R 26 , R 28 and R 29 each independently represents a hydrogen atom, an alkyl group, or an aryl group, and is preferably a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an aryl group having 6 to 12 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, and even more preferably an alkyl group having 1 to 12 carbon atoms. R 30 represents an alkyl group or an aryl group, preferably an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms.

[0163] A1 is -NR 22 R 23 , -X5-L1 or a halogen atom, and from the viewpoints of printing durability, visibility and stability over time, -NR 22 R 23 or -X5-L1, and -NR 31 R 32 , -SR 33 It is more preferable that: Furthermore, from the viewpoints of UV plate skipping suppression and UV printing durability, A1 is preferably a halogen atom, more preferably a chlorine atom or a bromine atom, and particularly preferably a chlorine atom. R 22 and R 23 each independently represents an alkyl group, an aryl group, an alkoxycarbonyl group, or an arylsulfonyl group, and is preferably an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms. X5 represents an oxygen atom or a sulfur atom, and when L1 is a hydrocarbon group or a heteroaryl group, X5 is preferably a sulfur atom. L1 represents a hydrocarbon group or a heteroaryl group, and from the viewpoint of printing durability, a hydrocarbon group or a heteroaryl group is preferable, an aryl group or a heteroaryl group is more preferable, and a heteroaryl group is further preferable. R 31 and R 32 each independently represents an aryl group, preferably an aryl group having 6 to 20 carbon atoms, and more preferably a phenyl group. R 33 represents a hydrocarbon group or a heteroaryl group, preferably an aryl group or a heteroaryl group, and more preferably a heteroaryl group.

[0164] L1 and R 33 Preferred examples of the heteroaryl group in the above formula include the following groups.

[0165] [ka]

[0166] R 14 ~R 23 and the alkyl group in R0 is preferably an alkyl group having 1 to 30 carbon atoms, more preferably an alkyl group having 1 to 15 carbon atoms, and further preferably an alkyl group having 1 to 10 carbon atoms. The alkyl group may be linear, branched, or have a ring structure. Specific examples include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a undecyl group, a dodecyl group, a tridecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, an isopropyl group, an isobutyl group, a s-butyl group, a t-butyl group, an isopentyl group, a neopentyl group, a 1-methylbutyl group, an isohexyl group, a 2-ethylhexyl group, a 2-methylhexyl group, a cyclohexyl group, a cyclopentyl group, and a 2-norbornyl group. Among these alkyl groups, a methyl group, an ethyl group, a propyl group, or a butyl group is particularly preferred.

[0167] The alkyl group may have a substituent, for example, an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, an alkyloxycarbonyl group, an aryloxycarbonyl group, or a combination thereof.

[0168] R 22 , R 23 , R 31 , R 32 And the aryl group in R0 is preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and even more preferably an aryl group having 6 to 12 carbon atoms. The aryl group may have a substituent, for example, an alkyl group, an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, an alkyloxycarbonyl group, an aryloxycarbonyl group, or a combination thereof. Specific examples of the aryl group include a phenyl group, a naphthyl group, a p-tolyl group, a p-chlorophenyl group, a p-fluorophenyl group, a p-methoxyphenyl group, a p-dimethylaminophenyl group, a p-methylthiophenyl group, and a p-phenylthiophenyl group. Of these aryl groups, a phenyl group, a p-methoxyphenyl group, a p-dimethylaminophenyl group, or a naphthyl group is preferred.

[0169] R 14 and R 15 are preferably linked to form a ring. R 14 and R 15 When R are linked to form a ring, the ring is preferably a 5- or 6-membered ring, more preferably a 6-membered ring. 14 and R 15 The ring formed by linking is preferably a hydrocarbon ring which may have an ethylenically unsaturated bond.

[0170] Y3 and Y4 each independently represent an oxygen atom, a sulfur atom, -NR0-, or a dialkylmethylene group, preferably -NR0- or a dialkylmethylene group, more preferably a dialkylmethylene group. R0 represents a hydrogen atom, an alkyl group or an aryl group, and is preferably an alkyl group.

[0171] R 20 and R 21 are preferably the same group. Also, R 20 and R 21 are each independently preferably a linear alkyl group or an alkyl group having a terminal sulfonate group, and more preferably a methyl group, an ethyl group, or a butyl group having a terminal sulfonate group. The counter cation of the sulfonate group may be the cation on the nitrogen atom in formula 4, or may be an alkali metal cation or an alkaline earth metal cation. Furthermore, in order to improve the water solubility of the compound represented by formula 4, R 20 and R 21 are each independently preferably an alkyl group having an anionic structure, more preferably an alkyl group having a carboxylate group or a sulfonate group, and further preferably an alkyl group having a sulfonate group at the terminal. In addition, the maximum absorption wavelength of the compound represented by formula 4 is increased, and from the viewpoints of visibility and printing durability of a lithographic printing plate, R 20 and R 21 are each independently preferably an alkyl group having an aromatic ring, more preferably an alkyl group having an aromatic ring at a terminal, and particularly preferably a 2-phenylethyl group, a 2-naphthalenylethyl group, or a 2-(9-anthracenyl)ethyl group.

[0172] R 16 ~R 19 each independently represents a hydrogen atom or an alkyl group, and is preferably a hydrogen atom.

[0173] Za represents a counter ion that neutralizes the charge, and examples of an anion species include a sulfonate ion, a carboxylate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a chloride ion, a perchlorate ion, a sulfonamide anion, and a sulfonimide anion. Examples of a cationic species include an alkali metal ion, an alkaline earth metal ion, an ammonium ion, a pyridinium ion, or a sulfonium ion, more preferably a sodium ion, a potassium ion, an ammonium ion, a pyridinium ion, or a sulfonium ion, further preferably a sodium ion, a potassium ion, or an ammonium ion, and particularly preferably a sodium ion, a potassium ion, or a trialkylammonium ion. R 14 ~R 21 , R0, A1, Ar3, Ar4, Y3 and Y4 may have an anionic structure or a cationic structure, R 14 ~R 21 If R, A, Ar, Ar, Y, and Y are all neutral groups, Za is a monovalent counter anion. 14 ~R 21 When R0, A1, Ar3, Ar4, Y3 and Y4 have two or more anion structures, Za can also be a counter cation. In addition, in formula 4, if the moieties other than Za are electrically neutral, Za may be omitted.

[0174] The infrared absorbing agent may be used alone or in combination of two or more kinds. Also, a pigment and a dye may be used in combination as the infrared absorbing agent. The total content of the infrared absorbing agent in the image recording layer is preferably from 0.1% by mass to 10.0% by mass, and more preferably from 0.5% by mass to 5.0% by mass, based on the total solid content of the image recording layer.

[0175] 〔particle〕 From the viewpoint of printing durability, the image recording layer preferably contains particles. The particles may be organic particles or inorganic particles, but from the viewpoint of printing durability, it is preferable that the toner contains organic particles, and it is more preferable that the toner contains polymer particles. As the inorganic particles, known inorganic particles can be used, and metal oxide particles such as silica particles and titania particles can be suitably used.

[0176] The polymer particles are preferably selected from the group consisting of thermoplastic resin particles, thermoreactive resin particles, polymer particles having a polymerizable group, microcapsules containing a hydrophobic compound, and microgels (crosslinked polymer particles). Among them, polymer particles or microgels having a polymerizable group are preferred. In a particularly preferred embodiment, the polymer particles contain at least one ethylenically unsaturated group. The presence of such polymer particles provides the effect of increasing the printing durability of the exposed area and the on-press developability of the unexposed area. From the viewpoints of printing durability and on-press developability, the polymer particles are preferably thermoplastic resin particles.

[0177] Preferred examples of the thermoplastic resin particles include thermoplastic polymer particles described in Research Disclosure No. 33303 published in January 1992, JP-A Nos. 9-123387, 9-131850, 9-171249, and 9-171250, and European Patent No. 931647. Specific examples of the polymer constituting the thermoplastic resin particles include homopolymers or copolymers of monomers such as ethylene, styrene, vinyl chloride, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, vinylidene chloride, acrylonitrile, vinylcarbazole, acrylates or methacrylates having a polyalkylene structure, or mixtures thereof. Preferred examples include copolymers containing polystyrene, styrene and acrylonitrile, or polymethyl methacrylate. The average particle size of the thermoplastic resin particles is preferably 0.01 μm to 3.0 μm.

[0178] The heat-reactive resin particles include polymer particles having a heat-reactive group, which form a hydrophobic region by crosslinking through a heat reaction and by the change in functional group.

[0179] The thermally reactive group in the polymer particles having a thermally reactive group may be a functional group that undergoes any reaction as long as a chemical bond is formed, but is preferably a polymerizable group, and preferred examples thereof include ethylenically unsaturated groups that undergo radical polymerization reactions (e.g., acryloyl groups, methacryloyl groups, vinyl groups, allyl groups, etc.), cationic polymerizable groups (e.g., vinyl groups, vinyloxy groups, epoxy groups, oxetanyl groups, etc.), isocyanato groups or blocked groups thereof that undergo addition reactions, epoxy groups, vinyloxy groups, and functional groups having active hydrogen atoms that are their reaction partners (e.g., amino groups, hydroxy groups, carboxy groups, etc.), carboxy groups and their reaction partners, hydroxy groups or amino groups that undergo condensation reactions, and acid anhydrides and their reaction partners, amino groups or hydroxy groups, that undergo ring-opening addition reactions.

[0180] As the microcapsules, for example, as described in JP-A-2001-277740 and JP-A-2001-277742, at least a part of the components of the image recording layer is encapsulated in the microcapsules. The components of the image recording layer can also be contained outside the microcapsules. In a preferred embodiment, the image recording layer containing the microcapsules has a hydrophobic component encapsulated in the microcapsules and a hydrophilic component contained outside the microcapsules.

[0181] The microgel (crosslinked polymer particle) can contain a part of the components of the image recording layer on at least one of the surface or the inside thereof. In particular, a reactive microgel having a radical polymerizable group on its surface is preferred from the viewpoints of the sensitivity of the resulting lithographic printing plate precursor and the printing durability of the resulting lithographic printing plate.

[0182] The components of the image recording layer can be microencapsulated or microgelled by known methods.

[0183] From the viewpoint of the printing durability, stain resistance and storage stability of the resulting lithographic printing plate, the polymer particles are preferably those obtained by reacting a polyisocyanate compound, which is an adduct of a polyphenol compound having two or more hydroxy groups in the molecule and isophorone diisocyanate, with a compound having active hydrogen. The polyhydric phenol compound is preferably a compound having a plurality of benzene rings each having a phenolic hydroxy group. The compound having active hydrogen is preferably a polyol compound or a polyamine compound, more preferably a polyol compound, and even more preferably at least one compound selected from the group consisting of propylene glycol, glycerin, and trimethylolpropane. Preferred examples of resin particles obtained by reacting a polyisocyanate compound, which is an adduct of a polyphenol compound having two or more hydroxy groups in the molecule and isophorone diisocyanate, with a compound having active hydrogen include the polymer particles described in paragraphs 0032 to 0095 of JP2012-206495A.

[0184] Furthermore, from the viewpoint of the printing durability and solvent resistance of the resulting lithographic printing plate, it is preferable that the polymer particles have a hydrophobic main chain and contain both i) a constituent unit having a pendant cyano group directly bonded to the hydrophobic main chain, and ii) a constituent unit having a pendant group that includes a hydrophilic polyalkylene oxide segment. A preferred example of the hydrophobic main chain is an acrylic resin chain. Preferred examples of the pendant cyano group include -[CH2CH(C≡N)]- or -[CH2C(CH3)(C≡N)]-. Furthermore, the structural unit having a pendant cyano group can be easily derived from an ethylenically unsaturated monomer, such as acrylonitrile or methacrylonitrile, or a combination thereof. The alkylene oxide in the hydrophilic polyalkylene oxide segment is preferably ethylene oxide or propylene oxide, and more preferably ethylene oxide. The number of repeating alkylene oxide structures in the hydrophilic polyalkylene oxide segment is preferably 10-100, more preferably 25-75, and even more preferably 40-50. Preferred examples of resin particles having a hydrophobic main chain and including both i) a constituent unit having a pendant cyano group directly bonded to the hydrophobic main chain, and ii) a constituent unit having a pendant group containing a hydrophilic polyalkylene oxide segment include those described in paragraphs 0039 to 0068 of JP2008-503365A.

[0185] In addition, from the viewpoints of printing durability and on-press developability, the polymer particles preferably have a hydrophilic group. The hydrophilic group is not particularly limited as long as it has a structure having hydrophilicity, and examples of the hydrophilic group include acid groups such as a carboxy group, a hydroxy group, an amino group, a cyano group, and a polyalkylene oxide structure. Among these, from the viewpoints of on-press developability and printing durability, a polyalkylene oxide structure is preferred, and a polyethylene oxide structure, a polypropylene oxide structure, or a polyethylene / propylene oxide structure is more preferred. From the viewpoint of on-press developability and suppression of development residue during on-press development, the polyalkylene oxide structure preferably has a polypropylene oxide structure, and more preferably has a polyethylene oxide structure or a polypropylene oxide structure. From the viewpoints of printing durability, ink receptivity, and on-press developability, the hydrophilic group preferably contains a structural unit having a cyano group or a group represented by the following formula Z, more preferably contains a structural unit represented by the following formula (AN) or a group represented by the following formula Z, and particularly preferably contains a group represented by the following formula Z. *-QWY formula Z In formula Z, Q represents a divalent linking group, W represents a divalent group having a hydrophilic structure or a divalent group having a hydrophobic structure, Y represents a monovalent group having a hydrophilic structure or a monovalent group having a hydrophobic structure, either W or Y has a hydrophilic structure, and * represents a bonding site with another structure.

[0186] [ka]

[0187] In formula (AN), R AN represents a hydrogen atom or a methyl group.

[0188] From the viewpoint of printing durability, the polymer contained in the polymer particles preferably contains a structural unit formed from a compound having a cyano group. The cyano group is preferably introduced into the resin as a structural unit containing a cyano group by using a compound (monomer) having a cyano group. Examples of the compound having a cyano group include acrylonitrile compounds, and (meth)acrylonitrile is preferred. The structural unit having a cyano group is preferably a structural unit formed from an acrylonitrile compound, and more preferably a structural unit formed from (meth)acrylonitrile, that is, a structural unit represented by the above formula (AN). When the above polymer includes a polymer having a structural unit having a cyano group, the content of the structural unit having a cyano group, preferably the structural unit represented by the above formula (AN), in the polymer having a structural unit having a cyano group is, from the viewpoint of printing durability, preferably 5% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, and particularly preferably 30% by mass to 60% by mass, relative to the total mass of the polymer having a structural unit having a cyano group.

[0189] Moreover, from the viewpoints of printing durability, ink receptivity, and on-press developability, the polymer particles preferably contain polymer particles having a group represented by the formula Z above.

[0190] Q in the above formula Z is preferably a divalent linking group having 1 to 20 carbon atoms, and more preferably a divalent linking group having 1 to 10 carbon atoms. Furthermore, Q in the above formula Z is preferably an alkylene group, an arylene group, an ester bond, an amide bond, or a group consisting of a combination of two or more of these, and more preferably a phenylene group, an ester bond, or an amide bond.

[0191] The divalent group having a hydrophilic structure in W of the above formula Z is a polyalkyleneoxy group or a polyalkyleneoxy group having -CH2CH2NR at one end. W It is preferable that R W represents a hydrogen atom or an alkyl group. The divalent group having a hydrophobic structure in W of the above formula Z is -R WA-, -OR WA -O-, -R W NR WA -NR W -, -OC(=O)-R WA -O- or -OC(=O)-R WA It is preferable that R is —O—. WA each independently represents a linear, branched, or cyclic alkylene group having 6 to 120 carbon atoms, a haloalkylene group having 6 to 120 carbon atoms, an arylene group having 6 to 120 carbon atoms, an alkylylene group having 6 to 120 carbon atoms (a divalent group obtained by removing one hydrogen atom from an alkylaryl group), or an aralkylene group having 6 to 120 carbon atoms.

[0192] The monovalent group having a hydrophilic structure in Y of the above formula Z is -OH, -C(=O)OH, a polyalkyleneoxy group having a hydrogen atom or an alkyl group at the end, or a polyalkyleneoxy group having a hydrogen atom or an alkyl group at the other end, and -CH2CH2NR W It is preferably a group with a - bonded thereto. The monovalent group having a hydrophobic structure for Y in the above formula Z is a linear, branched or cyclic alkyl group having 6 to 120 carbon atoms, a haloalkyl group having 6 to 120 carbon atoms, an aryl group having 6 to 120 carbon atoms, an alkaryl group (alkylaryl group) having 7 to 120 carbon atoms, an aralkyl group having 7 to 120 carbon atoms, -OR WB , -C(=O)OR WB , or -OC(=O)R WB It is preferable that R WB represents an alkyl group having 6 to 20 carbon atoms.

[0193] From the viewpoints of printing durability, ink receptivity, and on-press developability, it is more preferable that in the polymer particles having a group represented by the above formula Z, W is a divalent group having a hydrophilic structure, Q is a phenylene group, an ester bond, or an amide bond, W is a polyalkyleneoxy group, and Y is a polyalkyleneoxy group whose terminal is a hydrogen atom or an alkyl group.

[0194] From the viewpoints of printing durability and on-press developability, the polymer particles preferably contain polymer particles having a polymerizable group, and more preferably contain polymer particles having a polymerizable group on the particle surface. Furthermore, from the viewpoint of printing durability, the polymer particles preferably contain polymer particles having a hydrophilic group and a polymerizable group. The polymerizable group may be a cationically polymerizable group or a radically polymerizable group, but from the viewpoint of reactivity, it is preferably a radically polymerizable group. The polymerizable group is not particularly limited as long as it is a polymerizable group, but from the viewpoint of reactivity, an ethylenically unsaturated group is preferred, a vinylphenyl group (styryl group), a (meth)acryloxy group, or a (meth)acrylamide group is more preferred, and a (meth)acryloxy group is particularly preferred. The polymer in the polymer particles having a polymerizable group preferably has a structural unit having a polymerizable group. Furthermore, polymerizable groups may be introduced onto the surfaces of the polymer particles by a polymer reaction.

[0195] In addition, from the viewpoints of printing durability and on-press developability, the image recording layer preferably contains, as the polymer particles, addition polymerization type resin particles having a dispersible group, and it is more preferable that the dispersible group contains a group represented by the above formula Z.

[0196] In addition, from the viewpoints of printing durability, ink receptivity, on-press developability, and suppression of development residue during on-press development, the polymer particles preferably contain a resin having a urea bond. Suitable examples of the resin having the urea bond include those described in WO 2020 / 262692.

[0197] From the viewpoints of printing durability and on-press developability, the image recording layer preferably contains thermoplastic resin particles. The thermoplastic resin contained in the thermoplastic resin particles is not particularly limited, and examples thereof include polyethylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polymethyl (meth)acrylate, polyethyl (meth)acrylate, polybutyl (meth)acrylate, polyacrylonitrile, polyvinyl acetate, copolymers thereof, etc. The thermoplastic resin may be in a latex state. The thermoplastic resin according to the present invention is preferably a resin that forms all or part of the hydrophobic film that forms the recording layer by melting or softening the thermoplastic resin due to the heat generated in the exposure process described below.

[0198] From the viewpoints of ink receptivity and printing durability, the thermoplastic resin preferably contains a resin having a structural unit formed from an aromatic vinyl compound and a structural unit having a cyano group. Suitable examples of resins having a structural unit formed by an aromatic vinyl compound and a structural unit having a cyano group include those described in WO 2020 / 262692.

[0199] The thermoplastic resin contained in the thermoplastic resin particles preferably has a hydrophilic group from the viewpoints of printing durability and on-press developability. The hydrophilic group is not particularly limited as long as it has a structure having hydrophilicity, and examples thereof include acid groups such as a carboxy group, a hydroxy group, an amino group, a cyano group, and a polyalkylene oxide structure. From the viewpoints of printing durability and on-press developability, the hydrophilic group is preferably a group having a polyalkylene oxide structure, a group having a polyester structure, or a sulfonic acid group, more preferably a group having a polyalkylene oxide structure or a sulfonic acid group, and even more preferably a group having a polyalkylene oxide structure.

[0200] From the viewpoint of on-press developability, the polyalkylene oxide structure is preferably a polyethylene oxide structure, a polypropylene oxide structure, or a poly(ethylene oxide / propylene oxide) structure. From the viewpoint of on-press developability, the hydrophilic group preferably has a polypropylene oxide structure as the polyalkylene oxide structure, and more preferably has a polyethylene oxide structure or a polypropylene oxide structure. The number of alkylene oxide structures in the polyalkylene oxide structure is preferably 2 or more, more preferably 5 or more, further preferably 5 to 200, and particularly preferably 8 to 150, from the viewpoint of on-press developability.

[0201] From the viewpoint of on-press developability, the hydrophilic group is preferably a group represented by the formula Z.

[0202] The glass transition temperature (Tg) of the thermoplastic resin is preferably 60°C to 150°C, more preferably 80°C to 140°C, and even more preferably 90°C to 130°C, from the viewpoints of printing durability and ink receptivity. When the thermoplastic resin particles contain two or more types of thermoplastic resins, the value obtained by the FOX equation described below is referred to as the glass transition temperature of the thermoplastic resin.

[0203] In the present invention, the glass transition temperature of the resin can be measured by differential scanning calorimetry (DSC). A specific measurement method is performed in accordance with the method described in JIS K 7121 (1987) or JIS K 6240 (2011). In this specification, the glass transition temperature is the extrapolated glass transition onset temperature (hereinafter, sometimes referred to as Tig). The method for measuring the glass transition temperature will now be described more specifically. When determining the glass transition temperature, the temperature is held at about 50°C lower than the expected Tg of the resin until the apparatus stabilizes, then the material is heated at a heating rate of 20°C / min to a temperature about 30°C higher than the temperature at which the glass transition ends, and a differential thermal analysis (DTA) curve or DSC curve is prepared. The extrapolated glass transition onset temperature (Tig), i.e., the glass transition temperature Tg in this specification, is determined as the temperature at the intersection of a straight line extending from the low-temperature side baseline of a DTA curve or DSC curve to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the stepwise change in the glass transition is maximum.

[0204] When the thermoplastic resin particles contain two or more types of thermoplastic resins, the Tg of the thermoplastic resin contained in the thermoplastic resin particles is determined as follows. When the Tg of the first thermoplastic resin is Tg1(K), the mass fraction of the first thermoplastic resin relative to the total mass of the thermoplastic resin components in the thermoplastic resin particle is W1, the second Tg is Tg2(K), and the mass fraction of the second resin relative to the total mass of the thermoplastic resin components in the thermoplastic resin particle is W2, the Tg0(K) of the thermoplastic resin particle can be estimated according to the following FOX formula. FOX formula: 1 / Tg0=(W1 / Tg1)+(W2 / Tg2) Furthermore, when the thermoplastic resin particles contain three types of resins or when three types of thermoplastic resin particles containing different types of thermoplastic resins are contained in the pretreatment liquid, the Tg of the thermoplastic resin particles can be estimated according to the following formula, as described above, where Tg of the nth resin is Tgn(K) and the mass fraction of the nth resin relative to the total mass of the resin components in the thermoplastic resin particles is Wn. FOX formula: 1 / Tg0=(W1 / Tg1)+(W2 / Tg2)+(W3 / Tg3)... +(Wn / Tgn)

[0205] As a differential scanning calorimeter (DSC), for example, EXSTAR6220 from SII NanoTechnology, Inc. can be used.

[0206] From the viewpoint of printing durability, the arithmetic mean particle size of the thermoplastic resin particles is preferably 1 nm or more and 200 nm or less, more preferably 3 nm or more and less than 80 nm, and even more preferably 10 nm or more and 49 nm or less.

[0207] The arithmetic mean particle size of the thermoplastic resin particles in the present invention refers to a value measured by dynamic light scattering (DLS) unless otherwise specified. The arithmetic mean particle size of the thermoplastic resin particles by DLS is measured using Brookhaven BI-90 (manufactured by Brookhaven Instrument Company) according to the manual of the above instrument.

[0208] The weight average molecular weight of the thermoplastic resin contained in the thermoplastic resin particles is preferably 3,000 to 300,000, and more preferably 5,000 to 100,000.

[0209] The method for producing the thermoplastic resin contained in the thermoplastic resin particles is not particularly limited, and the thermoplastic resin can be produced by a known method. For example, it can be obtained by polymerizing a styrene compound, an acrylonitrile compound, and, if necessary, at least one compound selected from the group consisting of the N-vinyl heterocyclic compound, the compound used to form the structural unit having an ethylenically unsaturated group, the compound used to form the structural unit having an acidic group, the compound used to form the structural unit having a hydrophobic group, and the compound used to form the other structural units, by a known method.

[0210] Specific examples of the thermoplastic resin contained in the thermoplastic resin particles include those described in WO 2020 / 262692.

[0211] The average particle size of the above particles is preferably 0.01 μm to 3.0 μm, more preferably 0.03 μm to 2.0 μm, and even more preferably 0.10 μm to 1.0 μm. Within this range, good resolution and stability over time can be obtained. The average primary particle size of the above particles in the present invention is measured by a light scattering method, or by taking an electron micrograph of the particles, measuring the particle sizes of a total of 5,000 particles on the photograph, and calculating the average value. For non-spherical particles, the particle size is the particle size of a spherical particle having the same particle area as the particle area on the photograph. In the present invention, the average particle size is a volume average particle size unless otherwise specified.

[0212] The image recording layer may contain one type of particles, particularly polymer particles, or may contain two or more types. Furthermore, from the viewpoints of on-press developability and printing durability, the content of particles, particularly polymer particles, in the image recording layer is preferably 5% by mass to 90% by mass, more preferably 10% by mass to 90% by mass, even more preferably 20% by mass to 90% by mass, and particularly preferably 50% by mass to 90% by mass, relative to the total solid content of the image recording layer. From the viewpoints of on-press developability and printing durability, the content of the polymer particles in the image recording layer is preferably 20% by mass to 100% by mass, more preferably 35% by mass to 100% by mass, even more preferably 50% by mass to 100% by mass, and particularly preferably 80% by mass to 100% by mass, relative to the total mass of components having a molecular weight of 3,000 or more in the image recording layer.

[0213] [Binder Polymer] The image recording layer may contain a binder polymer. The polymer particles do not fall under the category of the binder polymer, that is, the binder polymer is a polymer that is not in a particulate form. The binder polymer is preferably a (meth)acrylic resin, a polyvinyl acetal resin, or a polyurethane resin.

[0214] Among them, the binder polymer may suitably be a known binder polymer used in the image recording layer of a lithographic printing plate precursor. As an example, a binder polymer used in an on-press development type lithographic printing plate precursor (hereinafter also referred to as an on-press development binder polymer) will be described in detail. The binder polymer for on-press development is preferably a binder polymer having an alkylene oxide chain. The binder polymer having an alkylene oxide chain may have a poly(alkylene oxide) moiety in the main chain or in the side chain. In addition, the binder polymer may be a graft polymer having a poly(alkylene oxide) in the side chain, or a block copolymer of a block composed of a poly(alkylene oxide)-containing repeating unit and a block composed of a non-(alkylene oxide)-containing repeating unit. When the main chain has a poly(alkylene oxide) moiety, polyurethane resin is preferred. When the main chain has a poly(alkylene oxide) moiety in the side chain, examples of the polymer of the main chain include (meth)acrylic resin, polyvinyl acetal resin, polyurethane resin, polyurea resin, polyimide resin, polyamide resin, epoxy resin, polystyrene resin, novolac type phenolic resin, polyester resin, synthetic rubber, and natural rubber, and (meth)acrylic resin is particularly preferred.

[0215] Another preferred example of the binder polymer is a polymer compound (hereinafter also referred to as a star-shaped polymer compound) having a 6- to 10-functional polyfunctional thiol core, a polymer chain bonded to the core via a sulfide bond, and the polymer chain having a polymerizable group. From the viewpoint of curability, the star-shaped polymer compound preferably has a polymerizable group such as an ethylenically unsaturated group in the main chain or side chain, more preferably in the side chain. Examples of star-shaped polymer compounds include those described in JP 2012-148555 A or WO 2020 / 262692 A.

[0216] The molecular weight of the binder polymer is preferably a weight average molecular weight (Mw) of 2,000 or more, more preferably 5,000 or more, and further preferably 10,000 to 300,000, as calculated as polystyrene by the GPC method.

[0217] If necessary, a hydrophilic polymer such as polyacrylic acid or polyvinyl alcohol described in JP-A-2008-195018 can be used in combination. Also, a lipophilic polymer and a hydrophilic polymer can be used in combination.

[0218] In addition, from the viewpoints of printing durability and on-press developability, the image recording layer preferably contains a polymer having a structural unit formed by an aromatic vinyl compound, and more preferably contains a polymer having a structural unit formed by an aromatic vinyl compound and an infrared absorbing agent that decomposes upon exposure to infrared rays.

[0219] Furthermore, the binder polymer used in the present invention preferably has a glass transition temperature (Tg) of 50° C. or higher, more preferably 70° C. or higher, even more preferably 80° C. or higher, and particularly preferably 90° C. or higher, from the viewpoint of suppressing deterioration of on-press developability over time. The upper limit of the glass transition temperature of the binder polymer is preferably 200° C. or lower, and more preferably 120° C. or lower, from the viewpoint of ease of penetration of water into the image recording layer.

[0220] As the binder polymer having the above glass transition temperature, polyvinyl acetal is preferred from the viewpoint of further suppressing the deterioration of on-press developability over time. Polyvinyl acetal is a resin obtained by acetalizing the hydroxyl groups of polyvinyl alcohol with an aldehyde. In particular, polyvinyl butyral obtained by acetalizing (that is, butyralizing) the hydroxyl groups of polyvinyl alcohol with butylaldehyde is preferred. In addition, from the viewpoint of improving printing durability, the polyvinyl acetal preferably has an ethylenically unsaturated group. Suitable examples of polyvinyl acetals include those described in WO 2020 / 262692.

[0221] The image recording layer in the invention preferably contains a resin having a fluorine atom, and more preferably contains a fluoroaliphatic group-containing copolymer. By using a resin having a fluorine atom, in particular a fluoroaliphatic group-containing copolymer, it is possible to suppress surface quality abnormalities due to foaming during the formation of the image recording layer, improve the coating surface condition, and further improve the ink receptivity of the formed image recording layer. Furthermore, an image recording layer containing a fluoroaliphatic group-containing copolymer provides high gradation, for example, high sensitivity to laser light, and provides a lithographic printing plate with good resistance to fogging caused by scattered light, reflected light, etc., and excellent printing durability.

[0222] As the fluoroaliphatic group-containing copolymer, those described in WO 2020 / 262692 can be suitably used.

[0223] In the image recording layer used in the present invention, the binder polymer may be used alone or in combination of two or more kinds. The binder polymer can be contained in any amount in the image recording layer, but the content of the binder polymer is preferably 1% by mass to 90% by mass, and more preferably 5% by mass to 80% by mass, based on the total solid content of the image recording layer.

[0224] [Acid color former] The image recording layer may contain an acid color former. The term "acid color former" used in the present invention means a compound that has the property of developing or decolorizing a color and changing the color of the image recording layer when heated in a state in which it accepts an electron-accepting compound (e.g., a proton of an acid, etc.). As the acid color former, a colorless compound having a partial skeleton such as lactone, lactam, sultone, spiropyran, ester, amide, etc., and in which the partial skeleton is rapidly opened or cleaved when it comes into contact with an electron-accepting compound is particularly preferred.

[0225] Specific examples of acid color formers include those described in WO 2020 / 158138.

[0226] Among these, from the viewpoint of color development, the acid color former used in the present invention is preferably at least one compound selected from the group consisting of spiropyran compounds, spirooxazine compounds, spirolactone compounds, and spirolactam compounds. From the viewpoint of visibility, the hue of the dye after color development is preferably green, blue or black.

[0227] From the viewpoints of color development and visibility, the acid color former preferably contains a leuco dye. The leuco dye is not particularly limited as long as it has a leuco structure, but it preferably has a spiro structure, and more preferably has a spirolactone ring structure. From the viewpoints of color development and visibility of exposed areas, the leuco dye is preferably a leuco dye having a phthalide structure or a fluoran structure. Furthermore, from the viewpoints of color development and visibility of exposed areas, the leuco dye having the above-mentioned phthalide structure or fluoran structure is preferably a compound represented by any one of the following formulas (Le-1) to (Le-3), and more preferably a compound represented by the following formula (Le-2).

[0228] [ka]

[0229] In formulae (Le-1) to (Le-3), ERG each independently represents an electron donating group, X1 to X4 each independently represent a hydrogen atom, a halogen atom or a dialkylanilino group, X5 to X 10 each independently represents a hydrogen atom, a halogen atom, or a monovalent organic group; Y1 and Y2 each independently represent C or N; when Y1 is N, X1 is not present; and when Y2 is N, X4 is not present; Ra1 represents a hydrogen atom, an alkyl group, or an alkoxy group; and Rb1 to Rb4 each independently represent a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group.

[0230] The electron-donating group in ERG of formulae (Le-1) to (Le-3) is preferably an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group, more preferably an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, an alkoxy group, or an aryloxy group, further preferably a monoalkylmonoarylamino group, a diarylamino group, a diheteroarylamino group, or a monoarylmonoheteroarylamino group, and particularly preferably a monoalkylmonoarylamino group. In addition, from the viewpoints of color development and visibility of exposed areas, the electron-donating group in the above ERG is preferably a di-substituted amino group having an aryl group having a substituent at at least one ortho position or a heteroaryl group having a substituent at at least one ortho position, more preferably a di-substituted amino group having a phenyl group having a substituent at at least one ortho position and an electron-donating group at the para position, still more preferably an amino group having a phenyl group having a substituent at at least one ortho position and an electron-donating group at the para position, and an aryl group or a heteroaryl group, and particularly preferably an amino group having a phenyl group having a substituent at at least one ortho position and an electron-donating group at the para position, and an aryl group having an electron-donating group or a heteroaryl group having an electron-donating group. In the present invention, the ortho position in an aryl group or heteroaryl group other than a phenyl group refers to the bonding position adjacent to the bonding position 1 (e.g., the 2nd position, etc.) when the bonding position of the aryl group or heteroaryl group to another structure is defined as the 1st position.

[0046] Furthermore, from the viewpoints of color development and visibility of exposed areas, the electron-donating group contained in the aryl group or heteroaryl group is preferably an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group, more preferably an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group, and particularly preferably an alkoxy group.

[0231] In formulae (Le-1) to (Le-3), X1 to X4 each independently represent preferably a hydrogen atom or a chlorine atom, and more preferably a hydrogen atom, from the viewpoints of color development and visibility of exposed areas. X5 to X in formula (Le-2) or formula (Le-3) 10 are each independently, from the viewpoints of color development and visibility of the exposed area, preferably a hydrogen atom, a halogen atom, an alkyl group, an aryl group, an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, a hydroxy group, an alkoxy group, an aryloxy group, a heteroaryloxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, a heteroaryloxycarbonyl group, or a cyano group, more preferably a hydrogen atom, a halogen atom, an alkyl group, an aryl group, an alkoxy group, or an aryloxy group, further preferably a hydrogen atom, a halogen atom, an alkyl group, or an aryl group, and particularly preferably a hydrogen atom. In the formulae (Le-1) to (Le-3), from the viewpoints of color development and visibility of exposed areas, at least one of Y1 and Y2 is preferably C, and it is more preferable that both Y1 and Y2 are C. From the viewpoints of color development and visibility of exposed areas, Ra1 in formulae (Le-1) to (Le-3) is preferably an alkyl group or an alkoxy group, more preferably an alkoxy group, and particularly preferably a methoxy group. In formulae (Le-1) to (Le-3), Rb1 to Rb4 each independently represent, from the viewpoints of color development and visibility of exposed areas, preferably a hydrogen atom or an alkyl group, more preferably an alkyl group, and particularly preferably a methyl group.

[0232] From the viewpoints of color development and visibility of exposed areas, the leuco dye having a phthalide structure or a fluoran structure is more preferably a compound represented by any one of the following formulas (Le-4) to (Le-6), and even more preferably a compound represented by the following formula (Le-5).

[0233] [ka]

[0234] In formulae (Le-4) to (Le-6), ERG each independently represents an electron donating group, X1 to X4 each independently represent a hydrogen atom, a halogen atom, or a dialkylanilino group, Y1 and Y2 each independently represent C or N, and when Y1 is N, X1 does not exist, and when Y2 is N, X4 does not exist, Ra1 represents a hydrogen atom, an alkyl group, or an alkoxy group, and Rb1 to Rb4 each independently represent a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group.

[0235] In formulae (Le-4) to (Le-6), ERG, X1 to X4, Y1, Y2, Ra1, and Rb1 to Rb4 have the same meanings as ERG, X1 to X4, Y1, Y2, Ra1, and Rb1 to Rb4 in formulae (Le-1) to (Le-3), respectively, and preferred embodiments are also the same.

[0236] Furthermore, from the viewpoints of color development and visibility of exposed areas, the leuco dye having the phthalide structure or the fluoran structure is more preferably a compound represented by any one of the following formulas (Le-7) to (Le-9), and particularly preferably a compound represented by the following formula (Le-8).

[0237] [ka]

[0238] In formulae (Le-7) to (Le-9), X1 to X4 each independently represent a hydrogen atom, a halogen atom, or a dialkylanilino group; Y1 and Y2 each independently represent C or N; when Y1 is N, X1 does not exist; when Y2 is N, X4 does not exist; Ra1 to Ra4 each independently represent a hydrogen atom, an alkyl group, or an alkoxy group; Rb1 to Rb4 each independently represent a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group; and Rc1 and Rc2 each independently represent an aryl group or a heteroaryl group.

[0239] X1 to X4, Y1 and Y2 in formulae (Le-7) to (Le-9) have the same meanings as X1 to X4, Y1 and Y2 in formulae (Le-1) to (Le-3), and preferred embodiments are also the same. In formula (Le-7) or formula (Le-9), Ra1 to Ra4 are each independently preferably an alkyl group or an alkoxy group, more preferably an alkoxy group, and particularly preferably a methoxy group, from the viewpoints of color development and visibility of the exposed area. In formulae (Le-7) to (Le-9), Rb1 to Rb4 each independently represent, from the viewpoints of color development and visibility of the exposed area, preferably a hydrogen atom, an alkyl group, or an aryl group substituted with an alkoxy group, more preferably an alkyl group, and particularly preferably a methyl group. In formula (Le-8), Rc1 and Rc2 each independently represent, from the viewpoints of color development and visibility of exposed areas, preferably a phenyl group or an alkylphenyl group, and more preferably a phenyl group. In addition, in terms of color development and visibility of exposed areas, Rc1 and Rc2 in formula (Le-8) are each preferably an aryl group having a substituent at at least one ortho position, or a heteroaryl group having a substituent at at least one ortho position, more preferably an aryl group having a substituent at at least one ortho position, even more preferably a phenyl group having a substituent at at least one ortho position, and particularly preferably a phenyl group having a substituent at at least one ortho position and an electron-donating group at the para position. Examples of the substituents in Rc1 and Rc2 include the substituents described below. In formula (Le-8), from the viewpoints of color development and visibility of exposed areas, it is preferable that X1 to X4 are hydrogen atoms, and Y1 and Y2 are C. Furthermore, in formula (Le-8), from the viewpoints of color development and visibility of exposed areas, it is preferred that Rb1 and Rb2 each independently represent an aryl group substituted with an alkyl group or an alkoxy group. Furthermore, in formula (Le-8), from the viewpoints of color development and visibility of the exposed area, it is preferable that Rb1 and Rb2 are each independently an aryl group or a heteroaryl group, more preferably an aryl group, still more preferably an aryl group having an electron-donating group, and particularly preferably a phenyl group having an electron-donating group at the para position. In addition, from the viewpoints of color development and visibility of the exposed area, the electron-donating group in Rb1, Rb2, Rc1, and Rc2 is preferably an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group, more preferably an alkoxy group, an aryloxy group, a heteroaryloxy group, or an alkyl group, and particularly preferably an alkoxy group.

[0240] In addition, from the viewpoints of color development and visibility of exposed areas, it is preferable that the acid color former contains a compound represented by the following formula (Le-10).

[0241] [ka]

[0242] In formula (Le-10), each Ar1 independently represents an aryl group or a heteroaryl group, and each Ar2 independently represents an aryl group having a substituent at at least one ortho position, or a heteroaryl group having a substituent at at least one ortho position.

[0243] Ar1 in formula (Le-10) has the same meaning as Rb1 and Rb2 in formulae (Le-7) to (Le-9), and preferred embodiments are also the same. Ar2 in formula (Le-10) has the same meaning as Rc1 and Rc2 in formulae (Le-7) to (Le-9), and preferred embodiments are also the same.

[0244] In addition, from the viewpoints of color development and visibility of exposed areas, it is preferable that the acid color former contains a compound represented by the following formula (Le-11).

[0245] [ka]

[0246] In formula (Le-11), ERG each independently represents an electron donating group, n11 represents an integer of 1 to 5, X1 to X4 each independently represent a hydrogen atom, a halogen atom, or a dialkylanilino group, Y1 and Y2 each independently represent C or N, and when Y1 is N, X1 is not present, and when Y2 is N, X4 is not present, and Rb2 and Rb4 each independently represent a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group.

[0247] ERG, X1 to X4, Y1, Y2, Rb2, and Rb4 in formula (Le-11) have the same meanings as ERG, X1 to X4, Y1, Y2, Rb2, and Rb4 in formulas (Le-1) to (Le-3), respectively, and preferred embodiments are also the same. In the formula (Le-11), n11 is preferably an integer of 1 to 3, and more preferably 1 or 2.

[0248] The alkyl group in the formula (Le-1) to the formula (Le-9) or the formula (Le-11) may be linear, branched, or have a ring structure. In addition, the number of carbon atoms in the alkyl group in formula (Le-1) to formula (Le-9) or formula (Le-11) is preferably 1 to 20, more preferably 1 to 8, even more preferably 1 to 4, and particularly preferably 1 or 2. The aryl group in formulae (Le-1) to (Le-11) preferably has 6 to 20 carbon atoms, more preferably 6 to 10 carbon atoms, and particularly preferably 6 to 8 carbon atoms. Specific examples of the aryl group in the formulae (Le-1) to (Le-11) include a phenyl group, a naphthyl group, an anthracenyl group, and a phenanthrenyl group, each of which may have a substituent. Specific examples of the heteroaryl group in the formulae (Le-1) to (Le-11) include a furyl group, a pyridyl group, a pyrimidyl group, a pyrazoyl group, and a thiophenyl group, each of which may have a substituent.

[0249] In addition, each group such as a monovalent organic group, an alkyl group, an aryl group, a heteroaryl group, a dialkylanilino group, an alkylamino group, and an alkoxy group in the formulae (Le-1) to (Le-11) may have a substituent. Examples of the substituent include an alkyl group, an aryl group, a heteroaryl group, a halogen atom, an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, a hydroxy group, an alkoxy group, an aryloxy group, a heteroaryloxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, a heteroaryloxycarbonyl group, and a cyano group. In addition, these substituents may be further substituted with these substituents.

[0250] In addition, from the viewpoints of color development and visibility of exposed areas, the acid color former preferably contains a compound represented by any one of the following formulas 3a and 3b. In a preferred embodiment, the acid color former is a compound represented by either formula 3a or 3b below.

[0251] [ka]

[0252] In formula (3a), Ar1 and Ar2 each independently represent an aryl group or a heteroaryl group; R 10 , R 11 each independently represents a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group. In formula (3b), ERG each independently represents an electron donating group, n represents an integer of 1 to 5, X1 to X4 each independently represent a hydrogen atom, a halogen atom or a monovalent organic group, Y1 and Y2 each independently represent C or N, and when Y1 is N, X1 does not exist, and when Y2 is N, X4 does not exist, and R 12 and R 13each independently represents a hydrogen atom, an alkyl group, an aryl group, or a heteroaryl group.

[0253] The alkyl group in formula (3a) to formula (3b) may be linear, branched, or have a ring structure. In addition, the alkyl group in formulae (3a) and (3b) preferably has 1 to 20 carbon atoms, more preferably 1 to 8 carbon atoms, further preferably 1 to 4 carbon atoms, and particularly preferably 1 or 2 carbon atoms. The aryl group in formulae (3a) and (3b) preferably has 6 to 20 carbon atoms, more preferably 6 to 10 carbon atoms, and particularly preferably 6 to 8 carbon atoms. Specific examples of the aryl group in formulae (3a) and (3b) include a phenyl group, a naphthyl group, an anthracenyl group, and a phenanthrenyl group, each of which may have a substituent. Specific examples of the heteroaryl group in formulae (3a) and (3b) include a furyl group, a pyridyl group, a pyrimidyl group, a pyrazoyl group, and a thiophenyl group, each of which may have a substituent. ERG in formula (3b) has the same meaning as ERG in formulae (Le-1) to (Le-3), and preferred embodiments are also the same. In formula (3b), n is preferably an integer of 1 to 3, and more preferably 1 or 2. The monovalent organic group in formula (3b) is X5 to X in formulas (Le-2) to (Le-3). 10 The same applies to the preferred embodiments.

[0254] In addition, each group such as the monovalent organic group, the alkyl group, the aryl group, and the heteroaryl group in the formulas (3a) to (3b) may have a substituent. Examples of the substituent include an alkyl group, an aryl group, a heteroaryl group, a halogen atom, an amino group, an alkylamino group, an arylamino group, a heteroarylamino group, a dialkylamino group, a monoalkylmonoarylamino group, a monoalkylmonoheteroarylamino group, a diarylamino group, a diheteroarylamino group, a monoarylmonoheteroarylamino group, a hydroxy group, an alkoxy group, an aryloxy group, a heteroaryloxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, a heteroaryloxycarbonyl group, and a cyano group. In addition, these substituents may be further substituted with these substituents.

[0255] As the leuco dye having a phthalide structure or a fluoran structure that is preferably used, the following compounds can be mentioned.

[0256] [ka]

[0257] [ka]

[0258] [ka]

[0259] [ka]

[0260] [ka]

[0261] [ka]

[0262] [ka]

[0263] [ka]

[0264] [ka]

[0265] [ka]

[0266] [ka]

[0267] In addition, as a preferred embodiment, the acid color former preferably contains a compound (specific dye compound) having a decomposable group that is decomposed by an acid and a structure that opens a ring or leaves a leaving group upon decomposition of the decomposable group.

[0268] From the viewpoints of color development and visibility of exposed areas, the decomposable group is preferably a group that is decomposed by an acid to generate an amino group or a hydroxy group, and more preferably a group that is decomposed by an acid to generate an amino group. In addition, the amino group generated by decomposition of the above-mentioned decomposable group may be an unsubstituted amino group or a mono-substituted amino group. From the viewpoints of color development and visibility of exposed areas, however, a mono-substituted amino group is preferable, and an alkylamino group is more preferable. From the viewpoints of color development and visibility of exposed areas, the decomposable group is preferably a group represented by the following formula 2a or 2b, and more preferably a group represented by the following formula 2a.

[0269] [ka]

[0270] In formula 2a and formula 2b, R a represents a hydrogen atom or an alkyl group, R b represents a hydrogen atom, an alkyl group, an aryl group, a heteroaryl group, an alkoxy group, or an aryloxy group; R c represents a protecting group for a hydroxy group, and the wavy line portion represents the bonding position to other structures.

[0271] R a From the viewpoints of color development and visibility of exposed areas, is preferably an alkyl group, more preferably an alkyl group having 1 to 8 carbon atoms, even more preferably an alkyl group having 1 to 4 carbon atoms, and particularly preferably a methyl group or an ethyl group. R b From the viewpoints of color development and visibility of exposed areas, is preferably an alkoxy group or an aryloxy group, more preferably an alkoxy group, and even more preferably a tertiary alkoxy group, an arylmethoxy group, or a 2-trialkylsilylethoxy group. R c From the viewpoints of color development and visibility of exposed areas, is preferably an acetal protecting group, an oxycarbonyl protecting group, an acyl group, or a silyl group, more preferably a tetrahydrofuranyl group, a tetrahydropyranyl group, a 1-alkoxyalkyl group, a tertiary alkoxycarbonyl group, an acyl group, or a trialkylsilyl group, still more preferably a tetrahydrofuranyl group, a tetrahydropyranyl group, a 1-alkoxyalkyl group, a tertiary alkoxycarbonyl group, or a trialkylsilyl group, and particularly preferably a tetrahydrofuranyl group, a tetrahydropyranyl group, or a trialkylsilyl group.

[0272] The specific dye compound may have one or more decomposable groups, but from the viewpoint of color development, the number of decomposable groups in the specific dye compound is preferably 1 to 4, more preferably 1 or 2, and particularly preferably 1. From the viewpoints of color development and visibility of exposed areas, the decomposable group is preferably a group having at least one structure selected from the group consisting of a urethane bond and a carbonate bond.

[0273] Furthermore, the group generated by decomposition of the decomposable group preferably has a Hammett value of 0 or less, more preferably -0.3 or less, and even more preferably -1.0 or more and -0.5 or less. The method for calculating the Hammett value of a group in the present invention is based on Chem. Rev., 1991, 97, 165-195. For example, the para and meta positions in each core structure described below are defined as follows.

[0274] [ka]

[0275] When calculating the Hammett value of a group not described in the above literature, the value is calculated simply from the following formula using the equilibrium constant pKx of the corresponding substituted benzoic acid at 25°C and the equilibrium constant pKH of unsubstituted benzoic acid = 4.201 (J. Org. Chem., 1958, 23(3), pp. 420-427). σ = pKx - pKH As the value of the substituted benzoic acid, a literature value may be used, or it may be experimentally calculated by the following method. Add the corresponding substituted benzoic acid to a 50 / 50 ethanol / water solution, titrate with 0.1N NaOH aqueous solution at 25°C, and calculate the pKx from the pH at the half-neutralization point. Since it is a weak acid, the pH at the half-neutralization point can be calculated as pH=pKx.

[0276] Specific examples of the decomposable group include, from the viewpoints of color development and visibility of exposed areas, preferably a group represented by any one of the following formulae D-1 to D-5, more preferably a group represented by any one of the following formulae D-1 to D-4, still more preferably a group represented by any one of the following formulae D-1 to D-3, and preferably a group represented by the following formula D-1. The wavy line portion indicates the bonding position to other structures.

[0277] [ka]

[0278] In formulas D-1 to D-5, R D1 represents an alkyl group, R D2 represents an alkyl group or an aryl group, R D3 represents an alkyl group, R D4 represents a hydrogen atom or an alkyl group, R D5 represents an alkyl group, R D4 and R D5 may be bonded to form a ring, R D6 each independently represents an alkyl group or an aryl group; R D7 represents an alkyl group or an aryl group.

[0279] R D1 From the viewpoints of color development and visibility of exposed areas, is preferably an alkyl group having 1 to 8 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and particularly preferably a methyl group or an ethyl group. R D2 From the viewpoints of color development and visibility of exposed areas, is preferably an alkyl group, and more preferably a tertiary alkyl group, an arylmethyl group, or a 2-trialkylsilylethyl group. R D3 From the viewpoints of color development and visibility of exposed areas, is preferably a tertiary alkyl group. R D4 and R D5From the viewpoints of color development and visibility of exposed areas, they are preferably bonded to form a ring, and more preferably bonded to form a 5- or 6-membered ring. In addition, from the viewpoint of color development and visibility of exposed areas, R D4 is a hydrogen atom, and R D5 is also a preferred embodiment in which the group is an alkyl group. R D6 are each independently preferably an alkyl group, and particularly preferably a methyl group, from the viewpoints of color development and visibility of exposed areas. R D7 From the viewpoints of color development and visibility of exposed areas, is preferably an alkyl group, more preferably an alkyl group having 1 to 4 carbon atoms, and even more preferably a methyl group.

[0280] The structure which opens a ring upon decomposition of the decomposable group or from which a leaving group is eliminated is preferably a structure which opens a ring upon decomposition of the decomposable group from the viewpoint of color development. In addition, from the viewpoints of color development and visibility of exposed areas, the specific dye compound is preferably a compound having a quaternary carbon atom to which three carbon atoms and one heteroatom (preferably a nitrogen atom or an oxygen atom, more preferably an oxygen atom) are bonded as the moiety that opens the ring or from which the leaving group is eliminated.

[0281] As the structure that opens a ring or from which a leaving group is eliminated by decomposition of the decomposable group, from the viewpoints of color development and inhibition of fading over time, a structure represented by any one of the following formulae 1a to 1d is preferable, a structure represented by any one of the following formulae 1a to 1c is more preferable, and a structure represented by the following formula 1a is particularly preferable. In a preferred embodiment, the acid color former has a structure that undergoes ring-opening or a leaving group is eliminated by decomposition of the decomposable group, and the structure that undergoes ring-opening or a leaving group is eliminated by decomposition of the decomposable group is preferably a structure represented by any one of the following formulas 1a to 1d.

[0282] [ka]

[0283] In formulas 1a to 1d, R 1 and R 2 represents a portion linked to the core structure of the acid color former (e.g., a specific dye compound), R 3 and R 4 represents an aryl group or a heteroaryl group; R 5 represents a hydrocarbon group, and X represents the above-mentioned leaving group.

[0284] R 3 and R 4 From the viewpoint of color development, is preferably an aryl group having 6 to 12 carbon atoms or a heteroaryl group having 2 to 12 carbon atoms, more preferably an aryl group having 6 to 12 carbon atoms, and further preferably a phenyl group. R 5 From the viewpoint of color development, is preferably an alkyl group or an aryl group, more preferably an aryl group, further preferably an aryl group having 6 to 12 carbon atoms, and particularly preferably a phenyl group. X is not particularly limited as long as it is a group that can be eliminated by decomposition of the decomposable group, but is preferably an acyloxy group, more preferably an acyloxy group having 1 to 8 carbon atoms, and even more preferably an acetyloxy group.

[0285] From the viewpoint of color development, the acid color former (preferably the specific dye compound) preferably has a structure represented by any one of the following formulas 2a to 2f as a mother structure, and more preferably has a structure represented by the following formula 2a.

[0286] [ka]

[0287] In formulae 2a to 2f, structure b represents a structure that opens upon decomposition of the decomposable group, and R1 to R9 each independently represent a hydrogen atom, an alkyl group, or an alkoxy group. The structures represented by Formulae 2a to 2f have one or more decomposable groups on the aromatic ring in Formulae 2a to 2f.

[0288] The alkyl group of R1 to R9 is not particularly limited, but is more preferably an alkyl group having 1 to 8 carbon atoms, further preferably an alkyl group having 1 to 4 carbon atoms, and particularly preferably a methyl group or an ethyl group. The alkoxy group of R1 to R9 is not particularly limited, but is more preferably an alkoxy group having 1 to 8 carbon atoms, even more preferably an alkoxy group having 1 to 4 carbon atoms, and particularly preferably an alkoxy group having 1 or 2 carbon atoms.

[0289] In Formulae 2a to 2f, Structure b represents a structure that opens upon decomposition of the decomposable group, and the structures represented by Formulae 2a to 2f have one or more of the decomposable groups on the aromatic ring in Formulae 2a to 2f.

[0290] From the viewpoints of color development and visibility of exposed areas, the structure b is preferably a structure represented by any one of formulae 1a to 1d. The structures represented by the above formulae 2a to 2f have one or more of the above decomposable groups on the aromatic ring in formulae 2a to 2f, and may further have a substituent on the aromatic ring. Preferred examples of the substituent include an alkyl group, an aryl group, an alkoxy group, an aryloxy group, a dialkylamino group, a diarylamino group, an alkylarylamino group, an arylamino group, and an alkylamino group. Among these, it is preferable that the compound has at least one dialkylamino group as a substituent from the viewpoints of color development and visibility of exposed areas.

[0291] From the viewpoints of color development and visibility of exposed areas, the specific dye compound is particularly preferably a compound represented by the following formula D-6.

[0292] [ka]

[0293] In formula D-6, R D8 represents the decomposable group, R D9 each independently represents an alkyl group or an aryl group; R D10 each independently represents an alkyl group or an aryl group, and each nd independently represents an integer of 0 to 3.

[0294] R D9 are each independently, from the viewpoints of color development and visibility of exposed areas, preferably an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, a benzyl group or a phenyl group, and further preferably an alkyl group having 1 to 4 carbon atoms. R D10 is preferably an alkyl group, more preferably a methyl group. Each nd is preferably independently 0 or 1, and more preferably 0.

[0295] As preferred specific examples of the specific dye compound, the following compounds are shown below, but it goes without saying that the compounds are not limited to these: In addition, Ph represents a phenyl group.

[0296] [ka]

[0297] [ka]

[0298] [ka]

[0299] [ka]

[0300] [ka]

[0301] [ka]

[0302] [ka]

[0303] The method for producing the specific dye compound is not particularly limited, and the specific dye compound can be produced by referring to known methods for producing leuco dyes and methods for introducing decomposable groups.

[0304] Commercially available products can be used as acid colorants, including ETAC, RED500, RED520, CVL, S-205, BLACK305, BLACK400, BLACK100, BLACK500, H-7001, GREEN300, NIRBLACK78, BLUE220, H-3035, BLUE203, ATP, H-1046, H-2114 (all manufactured by Fukui Yamada Chemical Industry Co., Ltd.), ORANGE-DCF, and Vermilio. Examples of such dyes include n-DCF, PINK-DCF, RED-DCF, BLMB, CVL, GREEN-DCF, TH-107 (all manufactured by Hodogaya Chemical Co., Ltd.), ODB, ODB-2, ODB-4, ODB-250, ODB-BlackXV, Blue-63, Blue-502, GN-169, GN-2, Green-118, Red-40, Red-8 (all manufactured by Yamamoto Chemical Industry Co., Ltd.), and crystal violet lactone (manufactured by Tokyo Chemical Industry Co., Ltd.). Among these commercially available products, ETAC, S-205, BLACK305, BLACK400, BLACK100, BLACK500, H-7001, GREEN300, NIRBLACK78, H-3035, ATP, H-1046, H-2114, GREEN-DCF, Blue-63, GN-169, and crystal violet lactone are preferred because the films formed have good visible light absorptance.

[0305] These acid color formers may be used alone or in combination of two or more kinds. The content of the acid color former is 5 to 100 mg / m from the viewpoint of visibility and printing durability. 2 is preferable, and 10 to 70 mg / m 2 More preferably, 15 to 50 mg / m 2 is more preferred.

[0306] [Chain transfer agent] The image recording layer used in the present invention may contain a chain transfer agent, which contributes to improving the printing durability of the lithographic printing plate. The chain transfer agent is preferably a thiol compound, more preferably a thiol compound having 7 or more carbon atoms from the viewpoint of boiling point (difficulty of volatilization), and further preferably a compound having a mercapto group on an aromatic ring (aromatic thiol compound).The thiol compound is preferably a monofunctional thiol compound. Specific examples of chain transfer agents include those described in WO 2020 / 262692.

[0307] The chain transfer agent may be added alone or in combination of two or more kinds. The content of the chain transfer agent is preferably from 0.01 to 50% by mass, more preferably from 0.05 to 40% by mass, and even more preferably from 0.1 to 30% by mass, based on the total solid content of the image recording layer.

[0308] [Oil Sensitizer] The image recording layer preferably further contains an oil sensitizer in order to improve ink receptivity. Examples of the oil sensitizer include onium compounds, nitrogen-containing low molecular weight compounds, and ammonium compounds such as ammonium group-containing polymers. In particular, when the protective layer contains an inorganic layer compound, the compound functions as a surface coating agent for the inorganic layer compound, and can suppress a decrease in ink receptivity during printing caused by the inorganic layer compound.

[0309] From the viewpoint of ink receptivity, the oil sensitizer is preferably an onium compound. Examples of the onium compound include phosphonium compounds, ammonium compounds, and sulfonium compounds. From the above viewpoint, the onium compound is preferably at least one selected from the group consisting of phosphonium compounds and ammonium compounds. Preferred examples of the ammonium compound include nitrogen-containing low molecular weight compounds and ammonium group-containing polymers. Specific examples of the sensitizer include those described in WO 2020 / 262692.

[0310] The content of the oil sensitizer is preferably from 1 to 40.0% by mass, more preferably from 2 to 25.0% by mass, and even more preferably from 3 to 20.0% by mass, based on the total solid content of the image recording layer.

[0311] The image recording layer may contain one type of oil sensitizer alone, or two or more types may be used in combination. One of the preferred embodiments of the image recording layer used in the present invention is an embodiment containing two or more compounds as oil sensitizers. Specifically, from the viewpoint of achieving both on-press developability and ink receptivity, the image recording layer used in the present invention preferably uses, as the oil sensitizer, a phosphonium compound, a nitrogen-containing low molecular weight compound, and an ammonium group-containing polymer in combination, and more preferably uses a phosphonium compound, a quaternary ammonium salt, and an ammonium group-containing polymer in combination.

[0312] [Development Accelerator] The image recording layer used in the present invention preferably further contains a development accelerator. The development accelerator preferably has a polarity term SP value of 6.0 to 26.0, more preferably 6.2 to 24.0, further preferably 6.3 to 23.5, and particularly preferably 6.4 to 22.0.

[0313] The SP value in the present invention (solubility parameter, unit: (cal / cm 3 ) 1 / 2 The value of the polar term in (3) is the value of the polar term δp in the Hansen solubility parameter. The Hansen solubility parameter is a solubility parameter introduced by Hildebrand, which is divided into three components, the dispersion term δd, the polar term δp, and the hydrogen bond term δh, and is expressed in a three-dimensional space. In the present invention, the polar term δp is used. δp[cal / cm 3 ] is the Hansen solubility parameter dipole-dipole term, V[cal / cm 3 ] is the molar volume, μ[D] is the dipole moment. For δp, the following formula simplified by Hansen and Beerbower is generally used:

[0314]

number

[0315] The development accelerator is preferably a hydrophilic high molecular weight compound or a hydrophilic low molecular weight compound. In the present invention, "hydrophilic" means that the value of the polar term of the SP value is 6.0 to 26.0, "hydrophilic polymer compound" means a compound having a molecular weight (weight average molecular weight when there is a molecular weight distribution) of 3,000 or more, and "hydrophilic low molecular weight compound" means a compound having a molecular weight (weight average molecular weight when there is a molecular weight distribution) of less than 3,000.

[0316] Examples of the hydrophilic polymer compound include cellulose compounds, and the like, with cellulose compounds being preferred. The cellulose compound includes cellulose and a compound in which cellulose is at least partially modified (modified cellulose compound), and the modified cellulose compound is preferred. Preferred examples of modified cellulose compounds include compounds in which at least a portion of the hydroxy groups of cellulose are substituted with at least one group selected from the group consisting of alkyl groups and hydroxyalkyl groups. The degree of substitution of the compound in which at least a portion of the hydroxy groups of the cellulose is substituted with at least one group selected from the group consisting of alkyl groups and hydroxyalkyl groups is preferably 0.1 to 6.0, and more preferably 1 to 4. The modified cellulose compound is preferably an alkyl cellulose compound or a hydroxyalkyl cellulose compound, more preferably a hydroxyalkyl cellulose compound. A preferred example of the alkyl cellulose compound is methyl cellulose. A preferred example of the hydroxyalkyl cellulose compound is hydroxypropyl cellulose.

[0317] The molecular weight of the hydrophilic polymer compound (weight average molecular weight when the compound has a molecular weight distribution) is preferably from 3,000 to 5,000,000, and more preferably from 5,000 to 200,000.

[0318] Examples of the hydrophilic low molecular weight compound include glycol compounds, polyol compounds, organic amine compounds, organic sulfonic acid compounds, organic sulfamine compounds, organic sulfuric acid compounds, organic phosphonic acid compounds, organic carboxylic acid compounds, and betaine compounds, and polyol compounds, organic sulfonic acid compounds, and betaine compounds are preferred.

[0319] Examples of the glycol compound include glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, and tripropylene glycol, and ether or ester derivatives of these compounds. Examples of the polyol compound include glycerin, pentaerythritol, and tris(2-hydroxyethyl)isocyanurate. The organic amine compound includes triethanolamine, diethanolamine, monoethanolamine, and the like, and salts thereof. Examples of the organic sulfonic acid compound include alkylsulfonic acid, toluenesulfonic acid, benzenesulfonic acid, and salts thereof, and preferable examples include alkylsulfonic acids in which the alkyl group has 1 to 10 carbon atoms. The organic sulfamine compounds include alkylsulfamic acids and their salts. The organic sulfate compound includes alkyl sulfates, alkyl ether sulfates, and salts thereof. The organic phosphonic acid compounds include phenylphosphonic acid and salts thereof. The organic carboxylic acid compound includes tartaric acid, oxalic acid, citric acid, malic acid, lactic acid, gluconic acid, and the like, and salts thereof. Examples of the betaine compound include a phosphobetaine compound, a sulfobetaine compound, and a carboxybetaine compound, and a preferred example is trimethylglycine.

[0320] The molecular weight of the hydrophilic low-molecular-weight compound (weight average molecular weight when the compound has a molecular weight distribution) is preferably 100 or more and less than 3,000, and more preferably 300 to 2,500.

[0321] The development accelerator is preferably a compound having a cyclic structure. The cyclic structure is not particularly limited, but examples thereof include a glucose ring in which at least a portion of a hydroxy group may be substituted, an isocyanuric ring, an aromatic ring which may have a heteroatom, and an aliphatic ring which may have a heteroatom, and is preferably a glucose ring or an isocyanuric ring. Examples of the compound having a glucose ring include the above-mentioned cellulose compounds. The compound having an isocyanuric ring includes the above-mentioned tris(2-hydroxyethyl)isocyanurate. Examples of the compound having an aromatic ring include the above-mentioned toluenesulfonic acid and benzenesulfonic acid. Examples of the compound having an aliphatic ring include the above-mentioned alkyl sulfate in which the alkyl group has a ring structure.

[0322] The compound having a cyclic structure preferably has a hydroxy group. Preferred examples of the compound having a hydroxy group and a cyclic structure include the above-mentioned cellulose compound and the above-mentioned tris(2-hydroxyethyl)isocyanurate.

[0323] The development accelerator is preferably an onium compound. The onium compound includes ammonium compounds and sulfonium compounds, and the ammonium compounds are preferred. The onium compound development accelerator includes trimethylglycine. Moreover, the onium compound in the above electron-accepting polymerization initiator is a compound in which the value of the polarity term of the SP value is not from 6.0 to 26.0, and is not included in the development accelerator.

[0324] The image recording layer may contain one type of development accelerator alone, or two or more types may be used in combination. One of the preferred embodiments of the image recording layer used in the present invention is an embodiment containing two or more compounds as development accelerators. Specifically, from the viewpoints of on-machine developability and ink receptivity, the image recording layer used in the present invention preferably contains, as a development accelerator, the above-mentioned polyol compound and the above-mentioned betaine compound, the above-mentioned betaine compound and the above-mentioned organic sulfonic acid compound, or the above-mentioned polyol compound and the above-mentioned organic sulfonic acid compound.

[0325] The content of the development accelerator relative to the total solid content of the image recording layer is preferably from 0.1 to 20% by mass, more preferably from 0.5 to 15% by mass, and even more preferably from 1 to 10% by mass.

[0326] [Color-forming compounds having a group cleavable by exposure to heat or infrared rays] The image recording layer used in the present invention may or may not contain a color-forming compound having a group that is cleaved by exposure to heat or infrared light. The color-forming compound having a group that is cleaved by exposure to heat or infrared rays may be a compound having a group that is cleaved by directly absorbing heat or infrared rays, or may be a compound having a group that is cleaved by heat or the like generated when an infrared absorbing agent contained separately absorbs infrared rays. Furthermore, the color-forming compound having a group that is cleaved by exposure to heat or infrared rays is a compound that develops color by cleavage of the above group. In the present invention, color development refers to the coloring or absorption of light having a shorter wavelength and having absorption in the visible light region after heating or exposure, more strongly than before heating or exposure. Among these, the color-forming compound having a group that is cleaved by heat or infrared exposure is preferably a decomposable infrared absorber from the viewpoints of edge stain suppression, color development, color development over time, on-machine developability, and chemical resistance, and is more preferably a compound represented by the following formula (A):

[0327] [ka]

[0328] In formula A, + Y A1 = the following structure:

[0329] [ka]

[0330] is displayed by one of Y A2 - has the following structure:

[0331] [ka]

[0332] n is 0, 1, 2 or 3; p and q are each independently 0, 1 or 2; R A1 and R A2each independently represents a hydrocarbon group, or R A1 , R A2 , R Ad and R Aa two of R comprise the atoms necessary to form a cyclic structure together; Ad At least one of the R is generated by a chemical reaction induced by exposure to infrared radiation or heat. Ad represents a group that is converted into a group that is a stronger electron donor, or R Aa At least one of the R is generated by a chemical reaction induced by exposure to infrared radiation or heat. Aa Represents a group that is converted to a group that is a stronger electron donor, and other R Ad and R Aa are each independently a hydrogen atom, a halogen atom, or -R Ae , -OR Af , -SR Ag and -NR Au R Av R represents a group selected from the group consisting of Ae , R Af , R Ag , R Au and R Av each independently represents an aliphatic hydrocarbon group, an aryl group, or a heteroaryl group, and the above conversion is a conversion that imparts an increase in light absorption in the wavelength range of 400 nm to 700 nm. Also, R A1 and R A2 Hydrocarbon groups in R Ae , R Af , R Ag , R Au and R Av The aliphatic hydrocarbon group, aryl group or heteroaryl group in may have a substituent.

[0333] In addition, the above R Ad is preferably any one of the groups shown below.

[0334] [ka]

[0335] In the above formula, Aa, Ab, Ac and Ad each independently represent 0 or 1; A - represents a bonding group, R A17 represents a hydrogen atom, an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group or an optionally substituted heteroaryl group, or R A17 and R A3 , R A17 and R A5 , or R A17 and R A11 R comprises the atoms necessary to form a ring structure together; A4 -OR A10 , -NR A13 R A14 or -CF3, R A10 represents an optionally substituted aryl group, an optionally substituted heteroaryl group, or an α-branched aliphatic hydrocarbon group; R A13 and R A14 each independently represents a hydrogen atom, an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, or an optionally substituted heteroaryl group, or R A13 and R A14 R comprises the atoms necessary to form a ring structure together; A3 is a hydrogen atom, an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, or an optionally substituted heteroaryl group, or R A3 R A10 , R A13 and R A14 R A6 represents an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, an optionally substituted heteroaryl group, -OR A10 , -NR A13 R A14 or -CF3, where R A10 , RA13 and R A14 R A4 has the same meaning as in R A5 represents a hydrogen atom, an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, or an optionally substituted heteroaryl group, or R A5 R A10 , R A13 and R A14 R A11 , R A15 and R A16 each independently represents a hydrogen atom, an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, or an optionally substituted heteroaryl group, or R A15 and R A16 R comprises the atoms necessary to form a ring structure together; A12 represents an optionally substituted aliphatic hydrocarbon group, an optionally substituted aryl group, or an optionally substituted heteroaryl group; R A7 and R A9 each independently represents a hydrogen atom or an optionally substituted aliphatic hydrocarbon group; R A8 -COO- or -COOR A8’ where R A8’ represents a hydrogen atom, an alkali metal cation, an ammonium ion, or a mono-, di-, tri-, or tetra-alkylammonium ion; R A18 represents an optionally substituted aryl group, an optionally substituted heteroaryl group, or an α-branched aliphatic hydrocarbon group.

[0336] As the color-forming compound having a group that is cleaved by exposure to heat or infrared rays, from the viewpoints of edge stain suppression, color development, color development over time, on-machine developability, and chemical resistance, it is particularly preferable to use a compound represented by the following formula (1):

[0337] [ka]

[0338] In formula (1), M 1 is a group that is cleaved by exposure to heat or infrared light; R 2 and R 3 each independently represents a hydrogen atom or an alkyl group; R 2 and R 3 may be linked together to form a ring, Ar 1 and Ar 2 each independently represents a group forming a benzene ring or a naphthalene ring; Y 1 and Y 2 each independently represents an oxygen atom, a sulfur atom, or -NR 0 - or a dialkylmethylene group; R 4 and R 5 each independently represents an aliphatic hydrocarbon group; R 6 ~R 9 each independently represents a hydrogen atom or an alkyl group; R 0 represents a hydrogen atom, an alkyl group or an aryl group, and Za represents a counter ion that neutralizes the charge.

[0339] The compound represented by the above formula (1) is preferably a compound that decomposes upon exposure to heat or infrared rays to generate a compound having a maximum absorption wavelength in the range of 500 nm to 600 nm. The color-developing mechanism of the compound represented by formula (1) is as follows: 1 The color develops when the cleavage occurs. For example, M 1 R 1 The present inventors presume that in the case of -O-, the cleaved oxygen atom forms a carbonyl group as shown below, resulting in the production of a merocyanine dye, which is a color-developing substance, and thus color development. In addition, to produce a merocyanine dye, R, which is cleaved by exposure to heat or infrared rays, is required. 1 The present inventors presume that it is important that the cyanine dye structure is bonded to the cyanine dye structure via an oxygen atom.

[0340] [ka]

[0341] M in formula (1) 1 A preferred embodiment of the above will be described later. Also, R 2 ~R 9 , R 0 , Ar 1 and Ar 2 may have a substituent such as a hydrophilic group described later. Examples of the substituent include an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, an alkyloxycarbonyl group, an aryloxycarbonyl group, a phosphonic acid group, a phosphonate group, and a group combining these groups. When the above group is an anionic group, it may form a salt, and the counter cation may be a cation of a cyanine dye structure, a proton, a metal cation, an onium, or the like.

[0342] R in formula (1) 2 ~R 9 and R 0 The alkyl group in is preferably an alkyl group having 1 to 30 carbon atoms, more preferably an alkyl group having 1 to 15 carbon atoms, and further preferably an alkyl group having 1 to 10 carbon atoms. The alkyl group may be linear, branched, or have a ring structure. Specific examples include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a undecyl group, a dodecyl group, a tridecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, an isopropyl group, an isobutyl group, a s-butyl group, a t-butyl group, an isopentyl group, a neopentyl group, a 1-methylbutyl group, an isohexyl group, a 2-ethylhexyl group, a 2-methylhexyl group, a cyclohexyl group, a cyclopentyl group, and a 2-norbornyl group. Among these alkyl groups, a methyl group, an ethyl group, a propyl group, or a butyl group is particularly preferred.

[0343] R 0 The aryl group in is preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and further preferably an aryl group having 6 to 12 carbon atoms. The aryl group may have a substituent, for example, an alkyl group, an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, an alkyloxycarbonyl group, an aryloxycarbonyl group, or a combination thereof. Specific examples include a phenyl group, a naphthyl group, a p-tolyl group, a p-chlorophenyl group, a p-fluorophenyl group, a p-methoxyphenyl group, a p-dimethylaminophenyl group, a p-methylthiophenyl group, and a p-phenylthiophenyl group. Of these aryl groups, a phenyl group, a p-methoxyphenyl group, a p-dimethylaminophenyl group, and a naphthyl group are preferred.

[0344] R 2 and R 3 are preferably linked to form a ring. R 2 and R 3 When they are linked to form a ring, the ring is preferably a 5- or 6-membered ring, and more preferably a 6-membered ring.

[0345] Y 1 and Y 2 each independently represents an oxygen atom, a sulfur atom, or -NR 0 - or a dialkylmethylene group, -NR 0 - or a dialkylmethylene group is preferred, and a dialkylmethylene group is more preferred. R 0 represents a hydrogen atom, an alkyl group or an aryl group, and is preferably an alkyl group.

[0346] R4 and R 5 are preferably the same group. 4 and R 5 When R has an anionic group, 4 and R 5 is preferably the same group except that it has an anionic group and has or does not have a counter cation. Also, R 4 and R 5 are each independently preferably a linear alkyl group or an alkyl group having a terminal sulfonate group, and more preferably a methyl group, an ethyl group, or a butyl group having a terminal sulfonate group. The counter cation of the sulfonate group may be the quaternary ammonium group in formula (1), or an alkali metal cation or an alkaline earth metal cation. Furthermore, from the viewpoint of improving the water solubility of the compound represented by formula (1), R 4 and R 5 are each independently preferably an alkyl group having an anionic structure, more preferably an alkyl group having a carboxylate group or a sulfonate group, and further preferably an alkyl group having a sulfonate group at the terminal. In addition, the maximum absorption wavelength of the compound represented by formula (1) is increased, and from the viewpoints of color development and printing durability of a lithographic printing plate, R 4 and R 5 are each independently preferably an alkyl group having an aromatic ring, more preferably an alkyl group having an aromatic ring at a terminal, and particularly preferably a 2-phenylethyl group, a 2-naphthalenylethyl group, or a 2-(9-anthracenyl)ethyl group.

[0347] R 6 ~R 9 each independently represents a hydrogen atom or an alkyl group, and is preferably a hydrogen atom. Ar 1 and Ar 2Each independently represents a group forming a benzene ring or a naphthalene ring. The benzene ring and the naphthalene ring may have a substituent. Examples of the substituent include an alkyl group, an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, an alkyloxycarbonyl group, an aryloxycarbonyl group, and a combination of these groups, and the like, but is preferably an alkyl group. In addition, the maximum absorption wavelength of the compound represented by formula (1) is increased, and from the viewpoints of color development and printing durability of a lithographic printing plate, Ar 1 and Ar 2 are each independently preferably a group forming a naphthalene ring or a benzene ring having an alkyl group or an alkoxy group as a substituent, more preferably a group forming a naphthalene ring or a benzene ring having an alkoxy group as a substituent, and particularly preferably a group forming a naphthalene ring or a benzene ring having a methoxy group as a substituent.

[0348] Za represents a counter ion that neutralizes the charge, and when it represents an anion species, examples thereof include a sulfonate ion, a carboxylate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a p-toluenesulfonate ion, a perchlorate ion, etc., and a hexafluorophosphate ion is particularly preferred.When it represents a cation species, an alkali metal ion, an alkaline earth metal ion, an ammonium ion, a pyridinium ion, or a sulfonium ion is preferred, a sodium ion, a potassium ion, an ammonium ion, a pyridinium ion, or a sulfonium ion is more preferred, and a sodium ion, a potassium ion, or an ammonium ion is even more preferred. R 1 ~R 9 , R 0 , Ar 1 , Ar 2 , Y 1 and Y 2 may have an anionic or cationic structure, R 1 ~R 9 , R0 , Ar 1 , Ar 2 , Y 1 and Y 2 If all of the groups are charge-neutral, Za is a monovalent counter anion. For example, R 1 ~R 9 , R 0 , Ar 1 , Ar 2 , Y 1 and Y 2 When the compound has two or more anion structures, Za can also be a counter cation.

[0349] In formula (1), Ar 1 Or Ar 2 is preferably a group forming a group represented by the following formula (8).

[0350] [ka]

[0351] In formula (8), R 19 represents an alkyl group having 1 to 12 carbon atoms or a group represented by any of the formulae (2) to (4) described below, n3 represents an integer of 1 to 4, and * represents a bonding site.

[0352] From the viewpoints of edge stain suppression, on-press developability, and chemical resistance, R 4 , R 5 , M 1 , Ar 1 and Ar 2 It is preferable that at least one group selected from the group consisting of has a hydrophilic group, and R 4 , R 5 and M 1 It is more preferable that at least one group selected from the group consisting of has a hydrophilic group, and R 4 and R 5 It is further preferred that at least one group selected from the group consisting of has a hydrophilic group, and R 4 and R 5 It is particularly preferable that each of the groups independently has a hydrophilic group.

[0353] Examples of the hydrophilic group include a polyalkyleneoxy group, an acid group, a salt of an acid group, an alkoxy group, and a hydroxy group. Among these, from the viewpoints of edge stain suppression, on-press developability, and chemical resistance, the hydrophilic group is preferably a group represented by any one of the following formulas (2) to (5), more preferably a group represented by either the following formula (2) or formula (5), and particularly preferably a group represented by the following formula (2).

[0354] [ka]

[0355] In formulas (2) to (5), R 10 represents an alkylene group having 2 to 6 carbon atoms; W 1 represents a single bond or an oxygen atom, n1 represents an integer of 1 to 45, R 11 represents an alkyl group having 1 to 12 carbon atoms or an acyl group having 2 to 12 carbon atoms, R 12 and R 13 each independently represents a single bond, or an alkylene group or alkyleneoxy group having 1 to 12 carbon atoms; M represents a hydrogen atom, a Na atom, a K atom, or an onium group; and when the charge can be neutralized by the entire compound represented by formula (1), M may not be present; m1 represents 1, 2, 3, or 4; X 1 represents -O-, -S- or -CH2-, and the wavy line represents the bonding position to other structures.

[0356] R 10 Specific examples of the alkylene group represented by the formula (I) include an ethylene group, an n-propylene group, an isopropylene group, an n-butylene group, an isobutylene group, an n-pentylene group, an isopentylene group, an n-hexyl group, an isohexyl group, and the like. Of these, an ethylene group, an n-propylene group, an isopropylene group, or an n-butylene group is preferred, and an n-propylene group is particularly preferred. n1 is preferably 1 to 10, more preferably 1 to 5, and particularly preferably 1 to 3. R11 Specific examples of the alkyl group represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, an n-hexyl group, an n-octyl group, and an n-dodecyl group. Of these, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, or a tert-butyl group is preferable, a methyl group or an ethyl group is more preferable, and a methyl group is particularly preferable. R 11 Specific examples of the acyl group in include an acetyl group, a propionyl group, a pivaloyl group, etc. Among these, an acetyl group is preferred.

[0357] Specific examples of the group represented by formula (2) are shown below, but the present invention is not limited thereto. In the following structural formula, Me represents a methyl group, Et represents an ethyl group, and * represents a bonding site.

[0358] [ka]

[0359] In formula (3) or formula (4), R 12 or R 13 Specific examples of the alkylene group represented by the formula (I) include a methylene group, an ethylene group, an n-propylene group, an isopropylene group, an n-butylene group, an isobutylene group, an n-pentylene group, an isopentylene group, an n-hexyl group, an isohexyl group, an n-octylene group, and an n-dodecylene group. An ethylene group, an n-propylene group, an isopropylene group, or an n-butylene group is preferred, and an ethylene group or an n-propylene group is particularly preferred. The group represented by formula (3) or formula (4) is Ar 1 Or Ar 2 When present in a group represented by R 12 or R 13 is preferably a single bond. The group represented by formula (3) or formula (4) is M of the compound represented by formula (1). 1If present in R 4 or R 5 When present as a group represented by R 12 or R 13 is preferably an alkylene group. In formula (4), the two M's may be the same or different.

[0360] In formula (3) or (4), specific examples of the onium group represented by M include an ammonium group, an iodonium group, a phosphonium group, and a sulfonium group.

[0361] The ammonium group includes a group represented by the following formula (A1).

[0362] [ka]

[0363] In formula (A1), R a ~R d R each independently represents a hydrogen atom or an aryl group, an alkyl group, an alkenyl group, or an alkynyl group having 20 or less carbon atoms. The aryl group, the alkyl group, the alkenyl group, or the alkynyl group may have a substituent. Examples of the substituent include an alkyl group having 1 to 12 carbon atoms, an alkenyl group having 1 to 12 carbon atoms, an alkynyl group having 1 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an aryloxy group having 6 to 12 carbon atoms, a halogen atom, an alkylamino group having 1 to 12 carbon atoms, a dialkylamino group having 2 to 12 carbon atoms, an alkylamide group or an arylamide group having 2 to 12 carbon atoms, a carbonyl group, a carboxy group, a cyano group, a sulfonyl group, a thioalkyl group having 1 to 12 carbon atoms, a thioaryl group having 6 to 12 carbon atoms, and a hydroxy group. a ~R d is preferably a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an aryl group having 6 carbon atoms.

[0364] Specific examples of the ammonium group are shown below, but the present invention is not limited to these. In the following structural formulas, Me represents a methyl group, and Et represents an ethyl group.

[0365] [ka]

[0366] The iodonium group includes a group represented by the following formula (B1):

[0367] [ka]

[0368] In formula (B1), R e ~R f each independently represents R in formula (A1) a ~R d The preferred R e ~R f Examples of the group include aryl groups having 6 to 20 carbon atoms.

[0369] Specific examples of the iodonium group are shown below, but the present invention is not limited to these.

[0370] [ka]

[0371] The phosphonium group includes a group represented by the following formula (C1):

[0372] [ka]

[0373] In formula (C1), R g ~R j each independently represents R in formula (A1) a ~Rd The preferred R g ~R j Examples of the group include aryl groups having 6 to 20 carbon atoms.

[0374] Specific examples of the phosphonium group are shown below, but the present invention is not limited to these.

[0375] [ka]

[0376] The sulfonium group includes a group represented by the following formula (D1).

[0377] [ka]

[0378] In formula (D1), R k ~R m each independently represents R in formula (A1) a ~R d A preferred example is an aryl group having 6 to 20 carbon atoms. k ~R m Examples of the group include aryl groups having 6 to 20 carbon atoms.

[0379] Specific examples of the sulfonium group are shown below, but the present invention is not limited to these.

[0380] [ka]

[0381] Of the above onium groups, ammonium groups are preferred. When the compound represented by formula (1) contains an onium group, M may be the above-mentioned onium group. The onium group may be present as an intramolecular onium salt.

[0382] Specific examples of the group represented by formula (3) are shown below, but the present invention is not limited thereto. In the following structural formula, Et represents an ethyl group, and * represents a bonding site.

[0383] [ka]

[0384] Specific examples of the group represented by formula (4) are shown below, but the present invention is not limited thereto. In the following structural formula, Et represents an ethyl group, and * represents a binding site.

[0385] [ka]

[0386] Specific examples of the group represented by formula (5) are shown below, but the present invention is not limited to these. In the following structural formula, * represents a binding site.

[0387] [ka]

[0388] The compound represented by formula (1) may have one or more groups represented by any one of formulas (2) to (5). The upper limit of the number of groups represented by any one of formulas (2) to (5) is preferably 5. The number of groups represented by any one of formulas (2) to (5) is preferably 1 to 5, more preferably 2 to 3. The group represented by any one of formulas (2) to (5) is R 4 or R 5 or M 1 , Ar 1 Or Ar 2 may be present in a group represented by the formula: The group represented by any one of formulas (2) to (5) is R 4 and R 5 It is particularly preferable that the group represented by any one of formulas (2) to (5) is Ar 1 and Ar 2 It is preferred that the aryl group is present in a group represented by the formula:

[0389] M in the above formula (1) 1 From the viewpoints of edge stain suppression, color development, and color development over time, -NR a R b , -NR c (SO2R d ) or -NR e (CO2R f ) is preferred. However, R a and R b each independently represents an aryl group; R c , R e and R f each independently represents an alkyl group or an aryl group; R d is an alkyl group, an aryl group, or -NR d1 R d2 R d1 and R d2 each independently represents a hydrogen atom, an alkyl group, or an aryl group.

[0390] R c ~R f , R d1 and R d2 The alkyl group in is preferably an alkyl group having 1 to 20 carbon atoms. Also, R a ~R f , R d1 and R d2 The aryl group in is preferably an aryl group having 6 to 20 carbon atoms. R a ~R f , R d1 and R d2The alkyl group and the aryl group in may have a substituent. Examples of the substituent include an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a carboxylate group, a sulfo group, a sulfonate group, an alkyloxycarbonyl group, an aryloxycarbonyl group, a phosphonic acid group, a phosphonate group, and a group combining these groups. In addition, when the above group is an anionic group, it may form a salt, and the counter cation may be a cation of a cyanine dye structure, a proton, a metal cation, an onium, or the like.

[0391] In addition, M in the above formula (1) 1 From the viewpoints of edge stain suppression, color development, and color development over time, -OR 1 It is preferable that: However, R 1 is destroyed by heat or infrared exposure. 1 Represents a group in which the -O bond is cleaved.

[0392] From the viewpoint of color development, R 1 is preferably a group represented by any one of the following formulas 1-1 to 1-7, and more preferably a group represented by any one of the following formulas 1-1 to 1-3.

[0393] [ka]

[0394] In formulas 1-1 to 1-7, ● represents a bonding site with an oxygen atom, and R 20 each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, -OR 24 , -NR 25 R 26 or -SR 27 R 21 each independently represents a hydrogen atom, an alkyl group, or an aryl group; R 22 is an aryl group, -OR 24 , -NR 25 R 26 , -SR27 , -C(=O)R 28 , -OC(=O)R 28 or a halogen atom, R 23 represents an aryl group, an alkenyl group, an alkoxy group, or an onium group; R 24 ~R 27 each independently represents a hydrogen atom, an alkyl group, or an aryl group; R 28 each independently represents an alkyl group, an aryl group, or -OR 24 , -NR 25 R 26 or -SR 27 represents Z 1 represents a counter ion that neutralizes the charge.

[0395] R 20 , R 21 and R 24 ~R 28 In a preferred embodiment, when R is an alkyl group, 2 ~R 9 and R 0 The preferred embodiments of the alkyl group are the same as those in the above. R 20 and R 23 The alkenyl group in preferably has 1 to 30 carbon atoms, more preferably 1 to 15 carbon atoms, and further preferably 1 to 10 carbon atoms. R 20 ~R 28 In a preferred embodiment, when R is an aryl group, 0 The preferred embodiments are the same as those of the aryl group in the above.

[0396] From the viewpoint of color development, R in Formula 1-1 20 is an alkyl group, an alkenyl group, an aryl group, -OR 24 , -NR 25 R 26 or -SR 27 is preferably an alkyl group, -OR 24 , -NR 25 R 26 or -SR 27 More preferably, it is an alkyl group or -OR 24 More preferably, -OR 24It is particularly preferred that: In addition, R in Formula 1-1 20 When is an alkyl group, the alkyl group is preferably an alkyl group having an arylthio group or an alkyloxycarbonyl group at the α-position. R in Formula 1-1 20 -OR 24 If R 24 is preferably an alkyl group, more preferably an alkyl group having 1 to 8 carbon atoms, further preferably an isopropyl group or a t-butyl group, and particularly preferably a t-butyl group.

[0397] From the viewpoint of color development, R in Formula 1-2 21 is preferably a hydrogen atom. In addition, from the viewpoint of color development, R 22 is -C(=O)OR 24 , -OC(=O)OR 24 or a halogen atom, preferably -C(=O)OR 24 Or -OC(=O)OR 24 It is more preferable that R in Formula 1-2 is 22 -C(=O)OR 24 Or -OC(=O)OR 24 If R 24 is preferably an alkyl group.

[0398] From the viewpoint of color development, R in Formula 1-3 21 are each preferably independently a hydrogen atom or an alkyl group, and at least one R 11 However, it is more preferably an alkyl group. Also, R 21 The alkyl group in is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 3 to 10 carbon atoms. Furthermore, R 21The alkyl group in is preferably an alkyl group having a branch containing a ring structure, more preferably a secondary or tertiary alkyl group, and further preferably an isopropyl group, a cyclopentyl group, a cyclohexyl group, or a t-butyl group. In addition, from the viewpoint of color development, R 23 is preferably an aryl group, an alkoxy group or an onium group, more preferably a p-dimethylaminophenyl group or a pyridinium group, and further preferably a pyridinium group. R 23 In the above formula, examples of the onium group include a pyridinium group, an ammonium group, and a sulfonium group. The onium group may have a substituent. Examples of the substituent include an alkyl group, an alkoxy group, an aryloxy group, an amino group, an alkylthio group, an arylthio group, a halogen atom, a carboxy group, a sulfo group, an alkyloxycarbonyl group, an aryloxycarbonyl group, and a combination of these groups. However, an alkyl group, an aryl group, and a combination of these groups are preferred. Among these, pyridinium groups are preferred, and examples thereof include N-alkyl-3-pyridinium groups, N-benzyl-3-pyridinium groups, N-(alkoxypolyalkyleneoxyalkyl)-3-pyridinium groups, N-alkoxycarbonylmethyl-3-pyridinium groups, N-alkyl-4-pyridinium groups, N-benzyl-4-pyridinium groups, N-(alkoxypolyalkyleneoxyalkyl)-4-pyridinium groups, and N-alkoxycarbonylmethyl-4-pyridinium groups. An N-alkyl-3,5-dimethyl-4-pyridinium group or an N-alkyl-3-pyridinium group is more preferred, an N-alkyl-3-pyridinium group or an N-alkyl-4-pyridinium group is even more preferred, an N-methyl-3-pyridinium group, an N-octyl-3-pyridinium group, an N-methyl-4-pyridinium group or an N-octyl-4-pyridinium group is particularly preferred, and an N-octyl-3-pyridinium group or an N-octyl-4-pyridinium group is most preferred. Also, R 23When is a pyridinium group, examples of the counter anion include a sulfonate ion, a carboxylate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a p-toluenesulfonate ion, a perchlorate ion, and the like, with the p-toluenesulfonate ion and the hexafluorophosphate ion being preferred.

[0399] From the viewpoint of color development, R in Formula 1-4 20 is preferably an alkyl group or an aryl group, and two R 20 It is more preferable that one of them is an alkyl group and the other is an aryl group. From the viewpoint of color development, R in Formula 1-5 20 is preferably an alkyl group or an aryl group, more preferably an aryl group, and further preferably a p-methylphenyl group. From the viewpoint of color development, R in Formula 1-6 20 are each independently preferably an alkyl group or an aryl group, and more preferably a methyl group or a phenyl group. From the viewpoint of color development, Z in formula 1-7 1 is a counter ion that neutralizes the charge, and the compound as a whole may be included in the above Za. Z 1 is preferably a sulfonate ion, a carboxylate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a p-toluenesulfonate ion, or a perchlorate ion, and more preferably a p-toluenesulfonate ion or a hexafluorophosphate ion.

[0400] From the viewpoint of color development, R 1 is a group represented by the following formula (6).

[0401] [ka]

[0402] In formula (6), R15 and R 16 each independently represents a hydrogen atom, an alkyl group or an aryl group, E represents an onium group, and the wavy line portion represents the bonding position to the oxygen atom.

[0403] R 15 or R 16 The alkyl group represented by R 2 ~R 9 and R 0 The alkyl group in R 2 ~R 9 and R 0 The preferred embodiments of the alkyl group are the same as those in the above. R 15 or R 16 The aryl group represented by R 0 The same applies to the aryl group in R 0 The preferred embodiments are the same as those of the aryl group in the above. The onium group represented by E is R 23 The same as the onium group in R 23 The preferred embodiments are the same as those of the onium group in the above.

[0404] From the viewpoint of color development, E in the above formula (6) is preferably a pyridinium group represented by the following formula (7).

[0405] [ka]

[0406] In formula (7), R 17 represents a halogen atom, an alkyl group, an aryl group, a hydroxyl group, or an alkoxy group; R 17 If there are multiple R 17 may be the same or different, or may be multiple R 17 may be linked to form a ring, n2 represents an integer of 0 to 4, and R 18 represents an alkyl group, an aryl group, or a group represented by the following formulae (2) to (5), and Zb represents a counter ion for neutralizing the charge.

[0407] [ka]

[0408] In formulas (2) to (5), R 10 represents an alkylene group having 2 to 6 carbon atoms; W 1 represents a single bond or an oxygen atom, n1 represents an integer of 1 to 45, R 11 represents an alkyl group having 1 to 12 carbon atoms, R 12 and R 13 each independently represents a single bond, or an alkylene group or alkyleneoxy group having 1 to 12 carbon atoms; M represents a hydrogen atom, a Na atom, a K atom, or an onium group; and when the charge can be neutralized by the entire compound represented by formula (1), M may not be present; m1 represents 1, 2, 3, or 4; X 1 represents -O-, -S- or -CH2-, and the wavy line represents the bonding position to other structures.

[0409] R 17 or R 18 The alkyl or aryl group represented by R 2 ~R 9 and R 0 The alkyl group or R 0 The same as the aryl group in R 2 ~R 9 and R 0 The alkyl group or R 0 The preferred embodiments are the same as those of the aryl group in the above. R 17 The alkoxy group represented by the formula (I) is preferably an alkoxy group having 1 to 10 carbon atoms, and examples thereof include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, and a tert-butoxy group. n2 is preferably 0. The counter ion for neutralizing the charge represented by Zb is Z in formula (1-7). 1 The preferred embodiment is also the same as Z 1 This is similar to the preferred embodiment of the above. In addition, R in Eq. (7) 18 The groups represented by formulae (2) to (5) in the formula (1) have the same meanings as the groups represented by formulae (2) to (5) described above, and preferred embodiments are also the same.

[0410] Below is R 1 However, the present invention is not limited to these examples. - represents a tosylate anion, and ● represents a bonding site with an oxygen atom.

[0411] [ka]

[0412] [ka]

[0413] [ka]

[0414] [ka]

[0415] [ka]

[0416] [ka]

[0417] [ka]

[0418] [ka]

[0419] [ka]

[0420] Specific examples of the color-forming compound are shown below, but the present invention is not limited thereto. In the following structural formula, Me represents a methyl group, TsO - represents a tosylate anion.

[0421] [ka]

[0422] [ka]

[0423] [ka]

[0424] [ka]

[0425] [ka]

[0426] [ka]

[0427] [ka]

[0428] [ka]

[0429] [ka]

[0430] [ka]

[0431] [ka]

[0432] [ka]

[0433] [ka]

[0434] [ka]

[0435] [ka]

[0436] The above color-forming compounds may be used alone or in combination of two or more. The color-forming compound may be contained in any amount in the image recording layer. From the viewpoints of edge stain suppression, color development, color development over time, on-machine developability, and chemical resistance, the content of the color-forming compound is preferably 0.1% by mass to 95% by mass, more preferably 1% by mass to 75% by mass, and particularly preferably 1% by mass to 50% by mass, relative to the total mass of the image recording layer. The content of the color-forming compound in the image recording layer is preferably 1 mg / m from the viewpoints of edge stain suppression, color development, color development over time, on-machine developability, and chemical resistance. 2 ~100mg / m 2 is preferably 10 mg / m 2 ~80mg / m 2 More preferably, it is 20 mg / m 2 ~60mg / m 2 It is particularly preferred that:

[0437] The method for producing the color-forming compound is not particularly limited, and the compound can be produced by a known method. For example, the compound represented by the above formula (1) can be obtained according to the synthesis method shown below as a synthesis scheme. For example, a method for introducing a group represented by any one of the above formulas 1-1, 1-5, and 1-6 can be suitably exemplified by the synthetic schemes represented by the following formulas S1 to S3, and a method for introducing a group represented by any one of the above formulas 1-2 to 1-4 can be suitably exemplified by the synthetic scheme represented by the following formula S4. In addition, DMAP represents N,N-dimethylamino-4-pyridine, AcONa represents sodium acetate, NEt3 represents triethylamine, and catecol represents catechol, and R represents a group corresponding to each portion in Formulae 1-1 to 1-7.

[0438] [ka]

[0439] [ka]

[0440] [Other ingredients] The image recording layer may contain other components such as a surfactant, a polymerization inhibitor, a higher fatty acid derivative, a plasticizer, an inorganic layer compound, etc. For details, see paragraphs 0114 to 0159 of JP-A-2008-284817. As the polymerization inhibitor, for example, a known polymerization inhibitor such as phenothiazine can be used.

[0441] [Formation of Image Recording Layer] The image recording layer in the lithographic printing plate precursor of the present invention can be formed, for example, as described in paragraphs

[0142] to

[0143] of JP2008-195018A, by dispersing or dissolving each of the necessary components described above in a known solvent to prepare a coating liquid, applying the coating liquid onto a support by a known method such as bar coater coating, and drying. As the solvent, a known solvent can be used.Specific examples of the solvent include water, acetone, methyl ethyl ketone (2-butanone), cyclohexane, ethyl acetate, ethylene dichloride, tetrahydrofuran, toluene, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, acetylacetone, cyclohexanone, diacetone alcohol, ethylene glycol monomethyl ether acetate, ethylene glycol ethyl ether acetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether acetate, 1-methoxy-2-propanol, 3-methoxy-1-propanol, methoxymethoxyethanol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, 3-methoxypropyl acetate, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, methyl lactate, and ethyl lactate. The solvent may be used alone or in combination of two or more kinds. The solid content concentration in the coating liquid is preferably 1% by mass to 50% by mass. The coating amount (solid content) of the image recording layer after coating and drying varies depending on the application, but from the viewpoint of obtaining good sensitivity and good film properties of the image recording layer, it is 0.3 g / m 2 ~3.0g / m 2 is preferred. The thickness of the image recording layer is preferably from 0.1 μm to 3.0 μm, and more preferably from 0.3 μm to 2.0 μm. In the present invention, the layer thickness of each layer in the lithographic printing plate precursor is confirmed by preparing a slice by cutting the lithographic printing plate precursor in a direction perpendicular to its surface and observing the cross section of the slice with a scanning electron microscope (SEM).

[0442] From the viewpoint of imparting on-press developability, the image recording layer is preferably water-soluble or water-dispersible. Here, "water-soluble" means that 0.1 g or more of the image recording layer dissolves in 100 g of water at 20° C., and "water-dispersible" means that the image recording layer is uniformly dispersed in water at 20° C.

[0443] <Undercoat layer> The lithographic printing plate precursor of the present invention may have an undercoat layer (sometimes called an intermediate layer) between the image recording layer and the support. The undercoat layer strengthens the adhesion between the support and the image recording layer in the exposed area and makes it easier for the image recording layer to peel off from the support in the unexposed area, thereby contributing to improving developability while suppressing a decrease in printing durability. In addition, in the case of infrared laser exposure, the undercoat layer functions as a heat insulating layer, thereby preventing the heat generated by exposure from diffusing to the support and decreasing sensitivity.

[0444] The compound used in the undercoat layer may be a polymer having an adsorptive group and a hydrophilic group that can be adsorbed to the support surface. In order to improve adhesion with the image recording layer, a polymer having an adsorptive group and a hydrophilic group and further having a crosslinkable group is preferred. The compound used in the undercoat layer may be a low molecular weight compound or a polymer. The compound used in the undercoat layer may be a mixture of two or more kinds, if necessary.

[0445] When the compound used in the undercoat layer is a polymer, it is preferably a copolymer of a monomer having an adsorptive group, a monomer having a hydrophilic group, and a monomer having a crosslinkable group. The adsorptive group capable of being adsorbed to the surface of the support is preferably a phenolic hydroxy group, a carboxy group, -PO3H2, -OPO3H2, -CONHSO2-, -SO2NHSO2-, or -COCH2COCH3. The hydrophilic group is preferably a sulfo group or a salt thereof, or a salt of a carboxy group. The crosslinkable group is preferably an acryl group, a methacryl group, an acrylamide group, a methacrylamide group, or an allyl group. The polymer may have a crosslinkable group introduced by salt formation between a polar substituent of the polymer and a compound having an ethylenically unsaturated bond and a substituent having an opposite charge to the polar substituent, or may further be copolymerized with a monomer other than the above-mentioned monomers, preferably a hydrophilic monomer.

[0446] Specifically, preferred examples include a silane coupling agent having an addition-polymerizable ethylenic double bond reactive group described in JP-A-10-282679, and a phosphorus compound having an ethylenic double bond reactive group described in JP-A-2-304441. Also preferred are low-molecular or high-molecular compounds having a crosslinkable group (preferably an ethylenic unsaturated group), a functional group that interacts with the support surface, and a hydrophilic group described in JP-A-2005-238816, JP-A-2005-125749, JP-A-2006-239867, and JP-A-2006-215263. More preferred examples include polymers having an adsorptive group, a hydrophilic group and a crosslinkable group capable of being adsorbed onto the surface of a support, as described in JP-A Nos. 2005-125749 and 2006-188038.

[0447] The content of the ethylenically unsaturated group in the polymer used in the undercoat layer is preferably from 0.1 mmol to 10.0 mmol, and more preferably from 0.2 mmol to 5.5 mmol, per 1 g of the polymer. The weight average molecular weight (Mw) of the polymer used in the undercoat layer is preferably 5,000 or more, and more preferably from 10,000 to 300,000.

[0448] In addition to the above-mentioned compounds for the undercoat layer, the undercoat layer may contain a chelating agent, a secondary or tertiary amine, a polymerization inhibitor, a compound having an amino group or a functional group having polymerization inhibitory ability and a group that interacts with the support surface (e.g., 1,4-diazabicyclo[2.2.2]octane (DABCO), 2,3,5,6-tetrahydroxy-p-quinone, chloranil, sulfophthalic acid, hydroxyethylethylenediaminetriacetic acid, dihydroxyethylethylenediaminediacetic acid, hydroxyethyliminodiacetic acid, etc.) to prevent contamination over time.

[0449] The undercoat layer is applied by a known method. The coating amount (solid content) of the undercoat layer is 0.1 mg / m 2 ~150mg / m 2 is preferred, and 1 mg / m 2 ~100mg / m 2 is more preferred.

[0450] <Protective layer> The lithographic printing plate precursor of the present invention may have a protective layer (sometimes called an "overcoat layer") on the image recording layer. In one preferred embodiment, the lithographic printing plate precursor of the invention has a support, an image recording layer, and a protective layer in this order. In one preferred embodiment, the lithographic printing plate precursor of the invention has a support, an undercoat layer, an image recording layer, and a protective layer in this order.

[0451] The protective layer may have a function of preventing the image-forming inhibiting reaction by blocking oxygen, as well as a function of preventing the occurrence of scratches in the image-recording layer and ablation during exposure to high-intensity laser light.

[0452] A protective layer having such characteristics is described, for example, in U.S. Patent No. 3,458,311 and Japanese Patent Publication No. 55-49729. As the low oxygen permeability polymer that can be used in the protective layer, either a water-soluble polymer or a water-insoluble polymer can be appropriately selected and used, and two or more types can be mixed and used as necessary, but from the viewpoint of on-press developability, it is preferable that the protective layer contains a water-soluble polymer. In the present invention, the water-soluble polymer means a polymer having a solubility in water at 25° C. of more than 5% by mass. Examples of water-soluble polymers that can be used in the protective layer include polyvinyl alcohol, modified polyvinyl alcohol, polyvinylpyrrolidone, cellulose derivatives, polyethylene glycol, and poly(meth)acrylonitrile. The hydrophilic polymer preferably contains at least one selected from the group consisting of modified polyvinyl alcohol and cellulose derivatives. The modified polyvinyl alcohol is preferably an acid-modified polyvinyl alcohol having a carboxy group or a sulfo group, specifically, the modified polyvinyl alcohols described in JP-A-2005-250216 and JP-A-2006-259137. Examples of the cellulose derivatives include methyl cellulose, hydroxypropyl methyl cellulose, and carboxymethyl cellulose.

[0453] Among the above water-soluble polymers, it is preferable to contain polyvinyl alcohol, and it is more preferable to contain polyvinyl alcohol having a degree of saponification of 50% or more. The degree of saponification is preferably 60% or more, more preferably 70% or more, and even more preferably 85% or more. There is no particular upper limit to the degree of saponification, so long as it is 100% or less. The degree of saponification is measured according to the method described in JIS K 6726:1994. In addition, one preferred embodiment of the protective layer includes a layer containing polyvinyl alcohol and polyethylene glycol.

[0454] When the protective layer in the present invention contains a water-soluble polymer, the content of the water-soluble polymer relative to the total mass of the protective layer is preferably 1% by mass to 99% by mass, more preferably 3% by mass to 97% by mass, and even more preferably 5% by mass to 95% by mass.

[0455] The protective layer may contain an inorganic layered compound to improve the oxygen barrier properties. The inorganic layered compound is a thin, tabular particle, and examples thereof include mica groups such as natural mica and synthetic mica, talc represented by the formula: 3MgO·4SiO·H2O, taeniolite, montmorillonite, saponite, hectorite, zirconium phosphate, and the like. The inorganic layered compound preferably used is a mica compound. Examples of the mica compound include those represented by the formula: A(B,C)2-5 D4O 10 Examples of mica include natural mica and synthetic mica represented by the formula (OH,F,O)2 (wherein A is K, Na, or Ca, B and C are Fe(II), Fe(III), Mn, Al, Mg, or V, and D is Si or Al).

[0456] In the mica group, natural micas include muscovite, sodalite, phlogopite, biotite and lepidolite. Synthetic micas include fluorphlogopite KMg3(AlSi3O 10 )F2, potassium tetrasilicic mica KMg 2.5 SiO 10 )F2 and other non-swelling micas, and Na tetrasilicic mica NaMg 2.5 (SiO 10 )F2, Na or Li taeniolite (Na,Li)Mg2Li(SiO 10 ) F2, Na or Li hectorite of the montmorillonite series (Na, Li) 1 / 8 Mg 2 / 5 Li 1 / 8 (SiO 10 Examples of suitable micas include swellable micas such as )F2. Synthetic smectite is also useful.

[0457] Among the above mica compounds, fluorine-based swellable mica is particularly useful. That is, swellable synthetic mica has a layered structure consisting of unit crystal lattice layers with a thickness of about 10 Å to 15 Å (1 Å = 0.1 nm), and the metal atom substitution within the lattice is significantly larger than that of other clay minerals. As a result, the lattice layers have a positive charge deficiency, and to compensate for this, Li is inserted between the layers. + , Na + , Ca 2+ , Mg 2+ The cations present between these layers are called exchangeable cations and can be exchanged with various other cations. In particular, the cations present between the layers are Li + , Na + In the case of , the bond between the layered crystal lattices is weak due to the small ionic radius, and it swells greatly in water. When shear is applied in this state, it easily cleaves and forms a stable sol in water. Swellable synthetic mica has a strong tendency in this case, and is particularly preferred.

[0458] As for the shape of the mica compound, from the viewpoint of diffusion control, the thinner the thickness, the better, and the larger the planar size, the better, as long as it does not impede the smoothness of the coating surface or the transmittance of actinic rays. Therefore, the aspect ratio is preferably 20 or more, more preferably 100 or more, and particularly preferably 200 or more. The aspect ratio is the ratio of the major axis to the thickness of the particle, and can be measured, for example, from a projection of the particle in a microscopic photograph. The larger the aspect ratio, the greater the effect obtained.

[0459] The particle size of the mica compound is preferably 0.3 μm to 20 μm, more preferably 0.5 μm to 10 μm, and particularly preferably 1 μm to 5 μm in terms of average major axis. The average thickness of the particles is preferably 0.1 μm or less, more preferably 0.05 μm or less, and particularly preferably 0.01 μm or less. Specifically, for example, in the case of swellable synthetic mica, which is a representative compound, the preferred embodiment has a thickness of about 1 nm to 50 nm and a surface size (major axis) of about 1 μm to 20 μm.

[0460] The content of the inorganic layered compound is preferably 1% by mass to 60% by mass, more preferably 3% by mass to 50% by mass, based on the total solid content of the protective layer. Even when a plurality of inorganic layered compounds are used in combination, the total amount of the inorganic layered compounds is preferably within the above content. Within the above range, oxygen barrier properties are improved and good sensitivity is obtained. Also, deterioration of ink receptivity can be prevented.

[0461] The protective layer may contain known additives such as a plasticizer for imparting flexibility, a surfactant for improving coatability, inorganic particles for controlling surface slippage, etc. Furthermore, the protective layer may contain an oil sensitizer as described in the image recording layer.

[0462] The protective layer is applied by a known method. The coating amount (solid content) of the protective layer is 0.01 g / m 2 ~10g / m 2 is preferred, and 0.02 g / m 2 ~3g / m 2 More preferably, 0.02 g / m2 ~1g / m 2 is particularly preferred.

[0463] The lithographic printing plate precursor of the present invention may have layers other than those described above. The other layers are not particularly limited, and any known layers may be used. For example, a backcoat layer may be provided on the side of the support opposite to the image recording layer, if necessary.

[0464] The lithographic printing plate precursor of the present invention has a sagging region at the edge portion. The edge portion has a sagging region and represents an area of ​​3 mm (0.3 cm) inward from the edge face of the lithographic printing plate precursor. The above-mentioned end faces are specifically edges of at least two opposing sides of the lithographic printing plate precursor of the present invention. The sagging shape in the sagging shape region is preferably a sagging shape in which the sagging amount X is 25 to 150 μm and the sagging width Y is 70 to 300 μm.

[0465] FIG. 3 is a diagram showing a schematic cross-sectional shape of an edge portion of a lithographic printing plate precursor. 3, edge 1 of the lithographic printing plate precursor has a sagging region 2. The distance X between the upper end of edge surface 1c of edge 1 of the lithographic printing plate precursor (the boundary point between sagging region 2 and edge surface 1c) and an extension line of image recording layer surface 1a (protective layer surface if a protective layer is formed) is referred to as "sagging amount X," and the distance Y between the point where image recording layer surface 1a of edge 1 of the lithographic printing plate precursor begins to sag and the extension line of edge surface 1c is referred to as "sagging width Y."

[0466] In the sagging shape of the edge, the sagging amount X is preferably 25 μm or more, more preferably 35 μm or more, and even more preferably 40 μm or more. The upper limit of the sagging amount X is preferably 150 μm from the viewpoint of preventing deterioration of on-machine developability due to deterioration of the edge surface condition. When on-machine developability deteriorates, ink may adhere to the remaining image recording layer, which may cause edge staining. If the sagging amount X is too small, the ink adhered to the edge may be easily transferred to the blanket, which may cause edge staining. When the sagging amount X is in the range of 25 to 150 μm, if the sagging width Y is small, the occurrence of cracks at the edge increases, and printing ink may accumulate there, which may cause edge staining. From this viewpoint, the sagging width Y is preferably in the range of 70 to 300 μm, and more preferably in the range of 80 to 250 μm. The above sagging amount and sagging width ranges are not related to the edge shape of the support surface 1b of the edge 1 of the lithographic printing plate precursor. Usually, at the edge of the lithographic printing plate precursor 1, sagging occurs at the boundary B between the image recording layer and the support, and on the support surface 1b, similar to the image recording layer surface 1a.

[0467] The formation of the end portion having the above-mentioned drooped shape can be achieved, for example, by adjusting the cutting conditions of the lithographic printing plate precursor. Specifically, this can be achieved by adjusting the gap between the upper and lower cutting blades, the amount of engagement, the blade angle, etc., of a slitter used when cutting the planographic printing plate precursor. FIG. 4 is a conceptual diagram showing an example of the cutting section of a slitter device. In the slitter device, a pair of upper and lower cutting blades 10 and 20 are arranged vertically. The cutting blades 10 and 20 are circular blades on a disk, and the upper cutting blades 10a and 10b are supported coaxially on a rotating shaft 11, and the lower cutting blades 20a and 20b are supported coaxially on a rotating shaft 21. The upper cutting blades 10a and 10b and the lower cutting blades 20a and 20b are rotated in opposite directions. The planographic printing plate precursor 30 is cut to a predetermined width by passing between the upper cutting blades 10a and 10b and the lower cutting blades 20a and 20b. An end portion having a drooped shape can be formed by adjusting the gap between the upper cutting blade 10a and the lower cutting blade 20a and the gap between the upper cutting blade 10b and the lower cutting blade 20b in the cutting section of the slitter device.

[0468] Specifically, the above-mentioned end portions are at least two opposing sides of the lithographic printing plate precursor of the present invention. In the planographic printing plate precursor according to the present invention, from the viewpoint of further suppressing edge staining, it is preferred that the area ratio of cracks present on the surface of the anodized film in the region corresponding to the sagging width Y is 10% or less. Here, the area corresponding to the sagging width Y means the area from the intersection of the extension line of the image recording layer surface (protective layer surface if a protective layer is formed) 1a in Figure 3 above and the extension line of the end surface 1c to the point where the extension line of 1a contacts the image recording layer surface (protective layer surface if a protective layer is formed).

[0469] The area ratio of cracks present on the surface of the anodized film is calculated by the following method. The constituent layers of the lithographic printing plate precursor (undercoat layer, image recording layer, protective layer) are removed using a PlasmaReactorPR300 manufactured by Yamato Scientific Co., Ltd. The surface of the exposed anodized film of the aluminum support is subjected to conductive treatment by vapor deposition of a 3 nm Pt-Pd film to prepare a sample. This sample is observed with a Hitachi High-Technologies Corporation S-4800 field emission scanning electron microscope (FE-SEM) at an acceleration voltage of 30 kV, and continuous photographs are taken from the edge to the center at an observation magnification of 1,500 times to obtain an image of 150 x 50 μm. The image is subjected to image processing software "ImageJ" to extract the crack shape using the brightness difference between the cracked part and the surface of the anodized film layer, binarize the image, and calculate the ratio of cracks in the 150 x 50 μm range, which is the crack area ratio.

[0470] From the viewpoint of preventing edge stains, the area ratio of cracks is more preferably 8% or less, and further preferably 7% or less.

[0471] In order to adjust the area ratio of cracks present on the surface of the anodized film in the region corresponding to the sagging width Y to 10% or less, the amount of the anodized film of the anodized film is, although not particularly limited, 0.5 to 3.0 g / m 2 It is preferable to control the temperature within the range of 100° C. to 150° C.

[0472] The on-press development type lithographic printing plate precursor of the present invention has an aluminum support having an anodized film, and one or more constituent layers including an image recording layer, and has a sagging region at an edge portion, the sagging region has a crack whose deepest portion reaches the aluminum support, Phosphate compounds are present in the cracks, The ratio of phosphorus to aluminum (P / Al) measured by FE-AES on the surface of a crack region formed in the aluminum support inside the crack is 0.04 or more.

[0473] The sagging region has a crack whose deepest portion reaches the aluminum support.

[0474] The ratio of phosphorus to aluminum (P / Al) measured by FE-AES on the surface of a crack region formed in the aluminum support inside the crack is 0.04 or more.

[0475] FE-AES is a "field emission Auger electron spectroscopy" that measures the type and amount of elements present by irradiating a sample with an electron beam and detecting the Auger electrons generated from the sample. The escape depth of Auger electrons is about 5 nm, so this method can obtain information on the extreme surface of the sample. The present inventors used FE-AES for the first time to measure the ratio of elements on the surface of the crack region formed in the aluminum support inside the crack. By using FE-AES, it became possible to obtain the ratio of phosphorus element to aluminum element (P / Al) on the surface of the crack region formed in the aluminum support.

[0476] (Method of measuring the ratio of phosphorus to aluminum (P / Al)) The sample was cut from the edge into 0.3 cm squares using a hand cutter, and 15 points per sample within the 0.3 cm square inside the crack were measured using Auger electron spectroscopy, and the average value was used. Auger electrons were detected by directly irradiating the aluminum support inside the crack with incident electrons from Auger electron spectroscopy, and the intensity (atom%) of P and Al inside the crack was measured. The P and Al from Auger electron spectroscopy defined here refer to the intensity of PLMM (123 eV) and AlKLL (1396 eV) in the Auger electron differential spectrum inside the crack. The measuring instruments used are as follows: Hand cutter: Sanhayato PC-205 hand cutter, Auger electron spectrometer: PHI4800 manufactured by ULVAC-PHI or JAMP-9510F manufactured by JEOL.

[0477] The ratio of phosphorus element to aluminum element (P / Al) is 0.04 or more. If the ratio is less than 0.04, the phosphorus compound cannot be present sufficiently on the surface of the aluminum support in the crack region, making it difficult to improve edge staining. The above ratio is preferably 0.06 or more, and more preferably 0.09 or more. The upper limit is preferably 1.2 or less, and more preferably 0.5 or less.

[0478] There is no particular limitation on the method for making the ratio of phosphorus element to aluminum element (P / Al) 0.04 or more, but examples thereof include the following.

[0479] (Method 1) Mist spray As a means for achieving the element ratio when measured by surface FE-AES of a crack region formed in the aluminum support inside the crack of the present invention, an on-press development type lithographic printing plate precursor has an aluminum support having an anodized film and one or more constituent layers including an image recording layer, has a sagging region at an end, and has a crack in the sagging region whose deepest part reaches the aluminum support, For example, a liquid containing a phosphoric acid compound can be misted to prepare an on-press development type lithographic printing plate precursor of the present invention.

[0480] (method) The mist spraying method may be any of an evaporative humidifier, an ultrasonic humidifier, a steam steamer, and a spray nozzle. The spray nozzle may be either a one-fluid nozzle (solution only) or a two-fluid nozzle (solution and air). A two-fluid nozzle is more preferable, and the mist particle size and flow rate can be controlled by controlling the air pressure and the flow rate of the solution (liquid containing a phosphoric acid compound). As a two-fluid nozzle, for example, Quigg Fogger (product name) manufactured by Spraying Systems can be used.

[0481] (Mist spray timing) Spraying the mist after sagging is effective against edge stains. When spraying the mist onto the edge, the form may be an assembly (also called a laminate) of lithographic printing plate precursors or individual lithographic printing plate precursors, with an assembly being preferred.

[0482] (mist particle size) The mist particle diameter is preferably 0.5 to 100 μm, and more preferably 1 to 20 μm. If the mist diameter is 0.5 μm or more, the mist is less likely to volatilize and the mist is more likely to land on the edge of the lithographic printing plate precursor. Therefore, an improvement effect on edge staining can be expected. If the mist diameter is 100 μm or less, the collision force is not too large, so the solution is less likely to enter between the plates of the stack of lithographic printing plate precursors, and multiple plate feeding is less likely to occur, which is preferable.

[0483] (Mist flow rate) The mist flow velocity is preferably 5 m / s or less, more preferably 3 m / s or less. By setting the flow velocity to 5 m / s or less, the solution enters between the plates of the stack of lithographic printing plate precursors, which is preferable because multiple plate feeding is less likely to occur.

[0484] (Mist distance) The distance between the mist nozzle and the edge is preferably 10 mm to 600 mm, more preferably 50 mm to 300 mm. If the distance between the nozzle and the edge is 10 mm or more, the spray area can be secured. If the distance is less than 600 mm, the mist can be prevented from evaporating or convecting, and the effect of improving edge stains can be expected.

[0485] (Nozzle air pressure) The air supply pressure to the two-fluid nozzle is preferably 0.05 MPa to 0.7 MPa, and more preferably 0.1 MPa to 0.3 MPa. If the pressure is 0.05 MPa or more, the mist flow rate does not decrease and the mist particle size can be maintained at an appropriate level. If the pressure is 0.7 MPa or less, the mist flow rate does not increase, making it difficult to reduce the mist particle size.

[0486] (Nozzle angle) The mist nozzle may be disposed at a right angle to the axis or at an angle to the edge of the lithographic printing plate precursor. An oblique arrangement is more preferable. On the other hand, an oblique arrangement is preferable because it creates a mist flow in one direction, which is an efficient measure against edge staining. When the axis-right angle between the mist nozzle and the edge is taken as 0°, the nozzle inclination angle is preferably ±45° to ±85°.

[0487] (Solution supply method) The solution can be supplied to the nozzle by either the siphon type (a system that uses air pressure to supply the solution) or the pressurized type. If the nozzle moves up and down, the siphon type will cause fluctuations in the liquid flow rate due to the difference in height, so the pressurized type is more preferable. The pressurized type can be used in two ways: by putting the solution into a sealed tank and pressurizing the tank with air pressure to supply the solution, or by using a liquid delivery pump to supply the solution.

[0488] (Mist method) Methods for spraying mist uniformly across the edge in the width direction include a method in which the nozzle is fixed and the lithographic printing plate precursor itself is moved, and a method in which the lithographic printing plate precursor is fixed and the nozzle is moved. In the former method, one or more nozzles are placed across the width, and mist is sprayed onto the lithographic printing plate precursors accumulated on a skid while they are transported on a belt conveyor or roller conveyor. In the latter method, the accumulation of lithographic printing plate precursors is fixed, and a nozzle is attached to a multi-axis robot or linear motion robot to spray mist uniformly across the width.

[0489] (Method for detecting the size of aggregates) Since the stack of lithographic printing plate precursors comes in various sizes, the nozzle operating position is automatically adjusted according to the size. It is preferable to use an image recognition camera to detect the shape of the stack. It is more preferable to use a 3D camera to recognize the shapes in the XYZ directions all at once. It is also possible to arrange multiple contact and non-contact sensors and link them with the nozzle. 3D cameras made by Keyence or Mech-Mind can be used.

[0490] (Type of mist solution) The solution used for the mist is a liquid containing a phosphoric acid compound, and may be a liquid obtained by adding a phosphoric acid compound to water. The phosphoric acid compound is as described above. The water may be tap water or ion-exchanged water, and is preferably ion-exchanged water. By using ion-exchanged water, clogging of the nozzle can be suppressed and a stable mist can be supplied.

[0491] (Constant management of mist flow rate) It is preferable to incorporate feedback control that controls the mist flow rate based on the environmental humidity. When the environmental humidity is low, the amount of mist that evaporates increases, and the amount of humidification to the edge portion decreases. Therefore, a control that increases the nozzle discharge amount when the humidity is low is incorporated. The method of controlling the nozzle discharge amount is to adjust the air pressure or solution pressure using an electropneumatic regulator.

[0492] (Mist environment) In order to keep the mist environment constant, it is preferable to provide an area where the temperature and humidity are air-conditioned. Since the humidity of the environment tends to increase due to the mist spray, it is more preferable to provide an exhaust system to forcibly remove the mist.

[0493] (Mist quality assurance) The mist particle size has an effect on edge stain quality, and it is preferable to control the mist particle size to keep it constant. As a method for measuring the mist particle size, for example, a particle size distribution measuring device AEROTRAC manufactured by Microtrackbell can be used.

[0494] (others) It is preferable to provide a plate pressing mechanism so that the uppermost plate of the stack of lithographic printing plate precursors does not lift up when the mist is sprayed. The area to be pressed may be the entire plate or only the edge portion. When spraying the mist, it is preferable to provide protection to the top of the stack to prevent the mist from scattering. If protection is not provided, the mist will get on areas other than the edges, resulting in poor development.

[0495] The concentration of the solution containing the phosphoric acid compound is preferably 0.1 to 50% by mass, and more preferably 0.5 to 10% by mass. By misting a solution with a concentration of 0.1% by mass or more, it becomes easier to make the element ratio 0.04 or more, which is preferable because edge stains can be reduced. In addition, by making the concentration 50% by mass or less, the amount of coating on the edge droop is not too large, which makes it difficult for multiple plate feeding defects to occur.

[0496] The amount of mist sprayed was 0.1 g / m 2 ~50g / m 2 It is preferable that the thickness is 2 g / m 2 ~20g / m 2 It is more preferable that the spray amount is 0.1 g / m 2 By setting the ratio to be equal to or greater than this, it becomes easier to set the element ratio to be equal to or greater than 0.04, which is preferable since edge stains can be reduced. In addition, the spray amount is 50g / m 2By setting the amount of solution to be supplied to the edge portion to be not too large, the solution is less likely to get into spaces between the stacked planographic printing plate precursors, and adhesion between the planographic printing plate precursors is less likely to occur, which is preferable. According to "Method 1", the lithographic printing plate precursor of the present invention can be prepared.

[0497] When the above-mentioned "(Method 1) mist spray" is used, it is preferable that at least one of the one or more constituent layers including the image recording layer does not contain a phosphoric acid compound.

[0498] (Method 1-1) When at least one of the one or more constituent layers including the image recording layer contains a phosphoric acid compound, the element ratio measured by surface FE-AES of the crack region formed in the above-mentioned aluminum support inside the crack of the present invention can be achieved by misting water as described below. Specifically, an example of the method includes spraying a mist of water into the inside of the crack of an on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, a sagging region at an end, and a crack in the sagging region, the deepest part of which reaches the aluminum support, wherein at least one of the constituent layers includes a layer containing a phosphoric acid compound. The mist spraying is the same as that described in "Method 1." The phosphoric acid compound is as described above. This method is the same as "Method 1," except that water is used instead of the solution (liquid containing a phosphoric acid compound).

[0499] In addition, the following can also be mentioned as a method for making the ratio of phosphorus element to aluminum element (P / Al) 0.04 or more.

[0500] (Method 2) Exposing the lithographic printing plate precursor to a high humidity environment When at least one of the one or more constituent layers including the image recording layer contains a phosphoric acid compound, the element ratio as measured by surface FE-AES of the crack region formed in the above-mentioned aluminum support inside the crack of the present invention can be achieved by exposing the lithographic printing plate precursor to a high humidity environment as described below. Specifically, an on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, a sagging region at an edge, and a crack in the sagging region whose deepest part reaches the aluminum support, at least one of the one or more constituent layers including a layer containing a phosphoric acid compound, is exposed to an environment of 60 to 95% RH in a 25°C environment for one minute or more.

[0501] (Method of exposing a lithographic printing plate precursor to a high humidity environment) As a method of exposing a lithographic printing plate precursor to a high humidity environment, the lithographic printing plate precursor or a stack of lithographic printing plate precursors is exposed to a high humidity environment in a temperature and humidity controlled room or temperature and humidity chamber. The lithographic printing plate precursor may be laid flat or hung. The stack may be packed in aluminum craft or not, and no packaging is preferable. Edge stains are more effectively improved when the edges of the plate are exposed. As the temperature and humidity chamber, for example, a temperature and humidity chamber (FFM08-FR02 / 03) manufactured by Amefrec Co., Ltd. can be used, and the temperature and humidity can be automatically controlled to keep them constant.

[0502] (Construction of constant temperature and humidity chamber) The temperature and humidity chamber may have a planar or three-dimensional structure, and a three-dimensional structure is preferable when the site area is small. In that case, it is preferable to install an elevator or rack inside the temperature and humidity chamber so that a plurality of lithographic printing plates and their stacks can be installed.

[0503] In order to maintain a constant temperature and humidity environment in the temperature and humidity chamber, a double shutter and double door structure is preferable. Although a single shutter is effective, a double shutter and double door structure reduces the influence of outside air and improves edge stains in a short period of time.

[0504] The temperature and humidity chamber is preferably made of stainless steel or a material with an anti-rust coating.

[0505] It is preferable that the temperature and humidity in the constant temperature and humidity room is constant, and it does not matter whether there is air in the room or not. Air does not affect the edge stain quality.

[0506] Once the sagging shape is formed after slitting, edge staining can be easily improved by exposing either the planographic printing plate precursor alone or the stack to a high humidity environment. The effect of improving edge stains can be sustained by exposing the film to a high humidity environment once.

[0507] The humidity in a high humidity environment is preferably 60% RH or more, more preferably 70% RH or more, and even more preferably 80% RH or less, as a relative humidity in a 25° C. environment. By setting the relative humidity in a 25°C environment to 60% RH or higher, the above element ratio becomes easier to achieve, and the effect of reducing edge stains can be expected. The humidity in the high humidity environment is preferably 95% RH or less as the relative humidity in a 25° C. environment. By setting the relative humidity in a 25° C. environment to 95% RH or less, condensation is unlikely to occur, the coating film is unlikely to soften, and adhesion between the planographic printing plate precursors is unlikely to occur, which is preferable.

[0508] The on-press development type lithographic printing plate precursor or the stack is preferably exposed for 1 minute or more. A time of 1 minute or more is preferable because edge stains are easily reduced. In a preferred embodiment, the on-press development type lithographic printing plate precursor or the stack is exposed to an environment of 60 to 95% RH as a relative humidity in a 25° C. environment for 1 minute or more. Moreover, the on-press development type lithographic printing plate precursor or the stack is more preferably exposed to an environment of 70 to 95% RH, and even more preferably 80 to 95% RH, as a relative humidity in a 25° C. environment.

[0509] According to Method 2, the lithographic printing plate precursor of the present invention can be prepared.

[0510] As described above, in the planographic printing plate precursor of the present invention, the sagging region has cracks whose deepest parts reach the aluminum support, and a phosphoric acid compound is present in the cracks. The phosphoric acid compound is as described above. According to the mist spraying by the above-mentioned method 1, it is believed that the phosphoric acid compound is present in the cracks by spraying a liquid containing the phosphoric acid compound. Furthermore, according to the above-mentioned methods 1-1 and 2, at least one of the one or more layers having an image recording layer in the lithographic printing plate precursor contains a phosphoric acid compound, and according to method 1-1, it is believed that the phosphoric acid compound migrates into the cracks by spraying a mist of water, and according to method 2, it is believed that the phosphoric acid compound migrates into the cracks by exposing the lithographic printing plate precursor to a high humidity environment.

[0511] In the lithographic printing plate precursor of the present invention, when the solid content of one or more constituent layers in the sagging region of the on-press development type lithographic printing plate precursor is A and the solid content of one or more constituent layers in the region other than the sagging region of the on-press development type lithographic printing plate precursor is B, A≧B, and the difference between A and B, AB, is 0.8 g / m 2 is less than.

[0512] The "sagging-shaped region" (sagging-shaped region 2 in Figure 3) in the "on-press development type lithographic printing plate precursor having a sagging-shaped region at its end" of the present invention, as explained above using drawings etc., is a "sagging-shaped region having the end face of the lithographic printing plate precursor as its tip", and in the present invention, it is provided at the end (end face 1 in Figure 3), which is a region 0.3 cm from the end face (end face 1c in Figure 3) toward the inside of the lithographic printing plate precursor.

[0513] The solid content (A) of the one or more constituent layers at the end portion is measured as follows. A region of 0.3 cm from an edge of the lithographic printing plate precursor is cut using a cutter, and the mass of the edge is measured (mass A1). The film components formed on the end are removed using a mixed solvent of solvent and water, and the mass of the end after removing the film components is measured (mass B1). The value obtained by "mass A1 - mass B1" represents the solid content (solid content 1: A) of one or more constituent layers at the end. Taking into account the area of ​​the cut part, the unit is "g / m 2 "

[0514] The solid content (B) of one or more constituent layers in the region other than the end portion is measured as follows. In addition, in the planographic printing plate precursor of the present invention, a 0.3 cm region (defined as a region other than the edge) is cut out at a position 3 cm from the edge using a cutter, and the mass of the region other than the edge is measured (mass A2). The film components formed in the area other than the end are removed using a mixed solvent of solvent and water, and the mass of the area other than the end after the film components are removed is measured (mass B2). The value obtained by "mass A2 - mass B2" represents the solid content (solid content 2: B) of one or more constituent layers in the region other than the end. Taking into account the area of ​​the cut portion, the unit is "g / m 2 " Solid content 1 - solid content 2 value (g / m 2 ) is AB, which is the difference between A and B, where A is the solid content of one or more constituent layers at the end of the lithographic printing plate precursor and B is the solid content of one or more constituent layers in the region other than the end of the lithographic printing plate precursor, and is 0.8 g / m 2 is less than. As a mixed solvent of a solvent and water, for example, MFG (propylene glycol monomethyl ether):MEK (methyl ethyl ketone):MA (methanol):water=43:34:8:15 (weight ratio) can be used.

[0515] The difference in the solid content (AB) is 0.8 g / m 2 If this is the case, in the stack of lithographic printing plate precursors, the lithographic printing plate precursors tend to adhere to each other, which tends to cause multiple plate feeding defects.

[0516] The difference in solid content is 0.6 g / m 2 It is preferable that the content is 0.3 g / m or less. 2 It is more preferable that: The difference in the solid content is preferably small, and is preferably 0 or more.

[0517] The difference in solid content is 0.8 g / m 2 The method for achieving this is not particularly limited, but examples thereof include the above-mentioned method 1, method 1-1, method 2, etc.

[0518] [Backcoat layer] The lithographic printing plate precursor according to the present invention may have a backcoat layer (hereinafter also referred to as a "back surface layer") on the non-printing side (hereinafter also simply referred to as the "non-printing side") opposite the image recording layer across the support. By containing tabular particles in the backcoat layer of the lithographic printing plate precursor of the present invention, the surface of the backcoat layer becomes hard, which is thought to prevent damage and peeling of the back layer during the manufacturing and processing steps of the lithographic printing plate precursor, transportation in the setter, bender, and stocker platemaking process, and the process of transporting and mounting the made printing plate to the printing press. The present invention includes, as preferred embodiments, an embodiment in which the backcoat layer contains tabular grains, and an embodiment in which the backcoat layer contains tabular grains and grains other than the above-mentioned tabular grains. In either embodiment, the surface of the backcoat layer becomes hard, and it is believed that, as described above, damage and peeling of the back layer can be prevented.

[0519] (tabular grain) The tabular particles may be any particles having an aspect ratio of 5 or more. The aspect ratio is preferably 10 or more, more preferably 50 or more, and particularly preferably 100 or more. Here, the aspect ratio is defined as the ratio of the major axis to the thickness of the particle. The larger the aspect ratio, the greater the effect obtained. Specifically, the aspect ratio (Z) is expressed by the relationship Z=L / a. L is the major axis of the particle. L refers to the number average particle size of the particles obtained by dynamic light scattering using a dynamic light scattering particle size distribution measuring device (LB-500, manufactured by Horiba, Ltd.) while dispersing the particles in a solvent. a is the unit thickness of the particle. The unit thickness a is a value that can be calculated by measuring the diffraction peak of the particles by powder X-ray diffraction. It can be measured using a powder X-ray diffraction device (SmartLabSE, manufactured by Rigaku Corporation).

[0520] (Thickness of Tabular Grain) The thickness of the tabular grains satisfying an aspect ratio of 5 or more is preferably smaller than the thickness of the backcoat layer. When the thickness of the tabular grains is smaller than the thickness of the backcoat layer, the tabular grains are less likely to fall off, and the process is not contaminated, which is preferable. The thickness of the tabular grains is not particularly limited, but is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 10 nm or less. The thickness of the tabular grains is expressed by the unit thickness (a) of the tabular grains.

[0521] (Composition of Tabular Grains) Examples of the tabular particles include, but are not limited to, tabular particles that do not contain silicon atoms and oxygen atoms, such as graphite, and tabular particles that contain silicon atoms and oxygen atoms, such as mica, bentonite containing montmorillonite as the main component, montmorillonite classified as smectite, beidellite, nontronite, saponite, hectorite, sauconite, stevenite, and vermiculite group, illite group, etc. As the tabular particles, tabular particles that contain silicon atoms and oxygen atoms are preferred, and smectite, bentonite, or mica are more preferred.

[0522] Mica is, for example, a compound represented by the general formula: A(B,C) 2-5 D4O 10 Examples of mica include natural mica and synthetic mica represented by the formula (OH,F,O)2 (wherein A is K, Na, or Ca, B and C are Fe(II), Fe(III), Mn, Al, Mg, or V, and D is Si or Al).

[0523] Natural mica includes muscovite, sodalite, phlogopite, biotite, and lepidolite. Synthetic mica includes fluorphlogopite KMg3(AlSi3O 10 )F2, potassium tetrasilicic mica KMg 2.5 (SiO 10 )F2 and other non-swelling micas, and Na tetrasilicic mica NaMg 2.5 (SiO 10 )F2, Na or Li taeniolite (Na,Li)Mg2Li(SiO 10 ) Swelling mica such as F2.

[0524] In the present invention, among micas, fluorine-based swellable mica is particularly useful. That is, this swellable synthetic mica has a layered structure consisting of unit crystal lattice layers with a thickness of about 100 to 150 nm (10 to 15 Å), and the metal atom substitution within the lattice is significantly larger than that of other clay minerals. As a result, the lattice layers have a positive charge deficiency, and to compensate for this, Na + , Ca 2+ , Mg 2+ The cations present between these layers are called exchangeable cations, and they exchange with various cations. In particular, the cations between the layers are Li + , Na + In the case of , the bond between the layered crystal lattices is weak due to the small ionic radius, and it swells greatly in water. When shear is applied in this state, it is easily cleaved and forms a stable sol in water. Swellable synthetic mica has a strong tendency in this respect, and is useful in the present invention. In particular, swellable synthetic mica is preferably used from the viewpoint that particles of uniform quality are easily available.

[0525] Montmorillonite contained in bentonite and smectite: Si8(Al3.34Mg 0.66 )O 20 (OH)4 is a layered structure of thin, flat crystals with a thickness of about 1 nm and a width of about 50 to 1000 nm. + , Ca 2+ , K + , Mg 2+ The interlayer ions are Na. + Montmorillonite, which contains a lot of ions, is rich in Na + Since the electrical attraction between the unit layers due to ions is weak, when dispersed in water, Na + The ions and water molecules hydrate and swell, eventually separating into unit layers. When shear is applied in this state, the layers easily cleave, forming a stable sol in water.

[0526] The interlayer cations of mica, bentonite, and smectite can be easily exchanged with other cations. By exchanging the cations with quaternary ammonium ions or other cations, the material becomes less dispersible in water, but has an affinity for organic solvents and disperses.

[0527] Specific examples of mica, bentonite, and smectite include Somasif MEB-3 mica manufactured by Katakura Coop Agri Co., Ltd., Kunipia-F, Kunipia-G, Kunipia-G4, and Kunipia-G10 bentonites manufactured by Kunimine Kogyo Co., Ltd., Smectites Sumecton-SA, Sumecton-ST, Sumecton-SW, Sumecton-SWN, and Sumecton-SWF, and bentonites Moistnite-U, Moistnite-S, and Moistnite-HC.

[0528] As mentioned above, the interlayer cations of mica, bentonite, and smectite can be easily exchanged with other cations. By exchanging the cations with quaternary ammonium ions or other cations, they become less likely to disperse in water, but they become more compatible with organic solvents and can be dispersed. Specifically, organically modified mica products such as Somasif MAE, Somasif MTE, and Somasif MEE manufactured by Katakura Co-op Chemical Co., Ltd., organically modified bentonite products such as Kunivis-110, Kunivis-127, and Moistnite-WO manufactured by Kunimine Kogyo Co., Ltd., and organically modified smectite products such as Sumecton-SAN, Sumecton-SAN-P, Sumecton-STN, and Sumecton-SEN are examples of such products, and each product has a different type of organic solvent suitable for dispersion.

[0529] The tabular grain content in the backcoat layer is 1 to 1000 mg / m 2 is preferable, and 5 to 800 mg / m 2 More preferably, 10 to 600 mg / m 2 The above tabular grains may be used alone or in combination of two or more kinds.

[0530] The backcoat layer preferably contains a polymer or a metal oxide obtained by hydrolysis and polycondensation of an organometallic compound or an inorganic metal compound.

[0531] (polymer) The backcoat layer preferably contains a polymer. The backcoat layer preferably contains an organic polymer as a base polymer for forming the layer. It is preferable that the backcoat layer forms a uniform film and has high adhesion to the support. Polymers preferably used as the base polymer are listed below, but are not limited thereto. Suitable examples of the resin include polybutene, polybutadiene, polyamide, polyester resin, polyurethane, polyurea, polyimide, polysiloxane, polycarbonate, epoxy resin, chlorinated polyethylene, aldehyde condensation resin of alkylphenol, polyvinyl chloride, polyvinylidene chloride, polystyrene, acrylic resin and copolymer resin thereof, hydroxycellulose, polyvinyl alcohol, polyvinyl acetal resin, vinylidene chloride copolymer resin, phenoxy resin, cellulose acetate, carboxymethyl cellulose, novolac resin, pyrogallol acetone resin, etc.

[0532] The content of the polymer relative to the total solid content of the backcoat layer is preferably from 99.99 to 50 mass %, more preferably from 99.9 to 60 mass %, and particularly preferably from 99.5 to 70 mass %.

[0533] (Metal oxides obtained by hydrolysis and polycondensation of organometallic compounds or inorganic metal compounds) The backcoat layer preferably contains a metal oxide obtained by hydrolysis and polycondensation of an organometallic compound or an inorganic metal compound.

[0534] The metal oxide obtained by hydrolysis and polycondensation of the above-mentioned organometallic compound or inorganic metal compound (hereinafter, also simply referred to as metal oxide) is preferably a so-called sol-gel reaction liquid obtained by hydrolysis and polycondensation of the organometallic compound or inorganic metal compound in water and an organic solvent with a catalyst such as an acid or an alkali. Examples of the organometallic compound or inorganic metal compound include metal alkoxides, metal acetylacetonates, metal acetates, metal oxalates, metal nitrates, metal sulfates, metal carbonates, metal oxychlorides, metal chlorides, and condensates obtained by partially hydrolyzing and oligomerizing these compounds.

[0535] Metal alkoxides are compounds represented by the formula M(OR)n (wherein M represents a metal element, R represents an alkyl group, and n represents the oxidation number of the metal element). Specific examples include Si(OCH3)4, Si(OC2H5)4, Si(OC3H7)4, Si(OC4H9)4, Al(OCH3)3, Al(OC2H5)3, Al(OC3H7)3, Al(OC4H9)3, B(OCH3)3, B(OC2H5)3, B(OC3H7)3, B(OC4H9)3, Ti(OCH3)4, Ti(OC2H5)4, Ti(OC3H7)4, Ti(OC4H9)4, Zr(OCH3)4, Zr(OC2H5)4, Zr(OC3H7)4, Zr(OC4H9)4, and other alkoxides of atoms such as Ge, Li, Na, Fe, Ga, Mg, P, Sb, Sn, Ta, and V. In addition, mono-substituted silicon alkoxides such as CH3Si(OCH3)3, C2H5Si(OCH3)3, CH3Si(OC2H5)3, and C2H5Si(OC2H5)3 are also used.

[0536] Among the organometallic compounds or inorganic metal compounds, metal alkoxides are preferred because they are highly reactive and easily produce polymers made of metal-oxygen bonds. Among them, silicon alkoxide compounds such as Si(OCH3)4, Si(OC2H5)4, Si(OC3H7)4, and Si(OC4H9)4 are particularly preferred because they are inexpensive and easily available, and the metal oxides obtained from them have excellent coating properties. Oligomers obtained by partially hydrolyzing and condensing these silicon alkoxide compounds are also preferred. For example, an ethyl silicate oligomer with an average pentamer containing about 40% by mass of SiO2 can be mentioned. The organometallic compounds or inorganic metal compounds can be used alone or in combination of two or more kinds.

[0537] Furthermore, it is also preferable to use a so-called silane coupling agent in which one or two alkoxy groups of the above silicon tetraalkoxy compound are substituted with an alkyl group or a reactive group in combination with the metal alkoxide. Examples of the silane coupling agent include silane coupling agents in which one or two alkoxy groups of the above silicon tetraalkoxy compound are substituted with a hydrophobic substituent such as a long-chain alkyl group having 4 to 20 carbon atoms or a fluorine-substituted alkyl group, and in particular, silane coupling agents having a fluorine-substituted alkyl group are preferred. Specific examples of the silane coupling agent include CF3CH2CH2Si(OCH3)3, CF3CF2CH2CH2Si(OCH3)3, and CF3CH2CH2Si(OC2H5)3, and examples of commercially available products include LS-1090 manufactured by Shin-Etsu Chemical Co., Ltd. The content of the silane coupling agent is preferably 5 to 90 mass % of the total solid content of the backcoat layer, more preferably 10 to 80 mass %.

[0538] As a catalyst useful for forming the sol-gel reaction liquid, organic and inorganic acids and alkalis are used. Examples of such acids include inorganic acids such as hydrochloric acid, sulfuric acid, sulfurous acid, nitric acid, nitrous acid, hydrofluoric acid, phosphoric acid, and phosphorous acid; organic acids such as formic acid, acetic acid, propionic acid, butyric acid, glycolic acid, chloroacetic acid, dichloroacetic acid, trichloroacetic acid, fluoroacetic acid, bromoacetic acid, methoxyacetic acid, oxaloacetic acid, citric acid, oxalic acid, succinic acid, malic acid, tartaric acid, fumaric acid, maleic acid, malonic acid, ascorbic acid, benzoic acid, and substituted benzoic acids such as 3,4-dimethoxybenzoic acid; phenoxyacetic acid, phthalic acid, picric acid, nicotinic acid, picolinic acid, pyrazine, pyrazole, dipicolinic acid, adipic acid, p-toluic acid, terephthalic acid, 1,4-cyclohexene-2,2-dicarboxylic acid, erucic acid, lauric acid, and n-undecanoic acid; and alkalis such as hydroxides of alkali metals and alkaline earth metals, and ammonia, ethanolamine, diethanolamine, and triethanolamine.

[0539] Other preferred catalysts that can be used include organic acids such as sulfonic acids, sulfinic acids, alkylsulfuric acids, phosphonic acids, and phosphoric esters, specifically, p-toluenesulfonic acid, dodecylbenzenesulfonic acid, p-toluenesulfinic acid, ethyl acid, phenylphosphonic acid, phenylphosphinic acid, phenyl phosphate, and diphenyl phosphate.

[0540] The catalyst may be used alone or in combination of two or more kinds. The amount of the catalyst is preferably 0.001 to 10 mass% and more preferably 0.05 to 5 mass% based on the raw material metal compound. When the amount of the catalyst is within this range, the sol-gel reaction is smoothly initiated, and abrupt reaction is suppressed, preventing the generation of non-uniform sol-gel particles.

[0541] To initiate the sol-gel reaction, an appropriate amount of water is required. The amount of water added is preferably 0.05 to 50 times, more preferably 0.5 to 30 times, the amount required to completely hydrolyze the raw metal compound. When the amount of water is within this range, the hydrolysis proceeds well.

[0542] A solvent is added to the sol-gel reaction liquid. The solvent may be any solvent that dissolves the raw metal compound and dissolves or disperses the sol-gel particles generated by the reaction. Examples of the solvent include lower alcohols such as methanol, ethanol, propanol, and butanol, and ketones such as acetone, methyl ethyl ketone, and diethyl ketone. For the purpose of improving the quality of the coated surface of the backcoat layer, mono- or di-alkyl ethers or acetates of glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, and dipropylene glycol can be used. As the solvent, lower alcohols that are miscible with water are preferred. The sol-gel reaction liquid is adjusted to a concentration suitable for coating with a solvent, but if the entire amount of the solvent is added to the reaction liquid from the beginning, the raw material is diluted, making it difficult for the hydrolysis reaction to proceed. Therefore, a method in which a part of the solvent is added to the sol-gel reaction liquid and the remaining solvent is added when the reaction has progressed is preferred.

[0543] (Other ingredients) For the purpose of imparting flexibility, adjusting slipperiness, and improving the coating surface condition, plasticizers, surfactants, and other additives may be added to the backcoat layer as necessary within the range that does not impair the effects of the present invention.

[0544] Examples of the plasticizer that may be used effectively include phthalates such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, diisobutyl phthalate, dioctyl phthalate, octyl capryl phthalate, dicyclohexyl phthalate, ditridecyl phthalate, butyl benzyl phthalate, diisodecyl phthalate, and diallyl phthalate; glycol esters such as dimethyl glycol phthalate, ethyl phthalyl ethyl glycolate, methyl phthalyl ethyl glycolate, butyl phthalyl butyl glycolate, and triethylene glycol dicaprylate; phosphate esters such as tricresyl phosphate and triphenyl phosphate; aliphatic dibasic acid esters such as diisobutyl adipate, dioctyl adipate, dimethyl sebacate, dibutyl sebacate, dioctyl azelate, and dibutyl maleate; polyglycidyl methacrylate, triethyl citrate, glycerin triacetyl ester, and butyl laurate.

[0545] The amount of plasticizer added to the backcoat layer varies depending on the type of polymer used in the layer containing tabular grains, but it is preferably added in an amount that does not cause the glass transition temperature to fall below 60°C.

[0546] The surfactant may be anionic, cationic, nonionic or amphoteric surfactant. Specific examples include polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene polystyryl phenyl ethers, polyoxyethylene polyoxypropylene alkyl ethers, glycerin fatty acid partial esters, sorbitan fatty acid partial esters, pentaerythritol fatty acid partial esters, propylene glycol mono fatty acid esters, sucrose fatty acid partial esters, polyoxyethylene sorbitan fatty acid partial esters, polyoxyethylene sorbitol fatty acid partial esters, polyethylene glycol fatty acid esters, polyglycerin fatty acid partial esters, poly nonionic surfactants such as oxyethylated castor oils, polyoxyethylene glycerin fatty acid partial esters, fatty acid diethanolamides, N,N-bis-2-hydroxyalkylamines, polyoxyethylene alkylamines, triethanolamine fatty acid esters, and trialkylamine oxides, fatty acid salts, abietic acid salts, hydroxyalkanesulfonates, alkanesulfonates, dialkylsulfosuccinate salts, linear alkylbenzenesulfonates, branched alkylbenzenesulfonates, alkylnaphthalenesulfonates, and alkylphenoxypolyoxyethylenepropylsulfonates;

[0547] Examples of anionic surfactants include polyoxyethylene alkyl sulfophenyl ether salts, N-methyl-N-oleyl taurine sodium salt, N-alkyl sulfosuccinic acid monoamide disodium salt, petroleum sulfonates, sulfated beef tallow oil, sulfate ester salts of fatty acid alkyl esters, alkyl sulfate ester salts, polyoxyethylene alkyl ether sulfate ester salts, fatty acid monoglyceride sulfate ester salts, polyoxyethylene alkyl phenyl ether sulfate ester salts, polyoxyethylene styryl phenyl ether sulfate ester salts, alkyl phosphate ester salts, polyoxyethylene alkyl ether phosphate ester salts, polyoxyethylene alkyl phenyl ether phosphate ester salts, partially saponified products of styrene / maleic anhydride copolymers, partially saponified products of olefin / maleic anhydride copolymers, and naphthalene sulfonate formalin condensates; cationic surfactants include alkylamine salts, quaternary ammonium salts, polyoxyethylene alkylamine salts, and polyethylene polyamine derivatives; and amphoteric surfactants such as carboxybetaines, aminocarboxylic acids, sulfobetaines, aminosulfates, and imitazolines. Among the surfactants listed above, polyoxyethylene can be read as polyoxyalkylene such as polyoxymethylene, polyoxypropylene, polyoxybutylene, etc., and these surfactants are also included.

[0548] More preferred surfactant is the fluorine-based surfactant that contains perfluoroalkyl group in molecule.The example of fluorine-based surfactant can include anion type such as perfluoroalkyl carboxylate, perfluoroalkyl sulfonate, perfluoroalkyl phosphate, amphoteric type such as perfluoroalkyl betaine, cationic type such as perfluoroalkyl trimethyl ammonium salt, and non-ionic type such as perfluoroalkyl amine oxide, perfluoroalkyl ethylene oxide adduct, perfluoroalkyl group and hydrophilic group-containing oligomer, perfluoroalkyl group and lipophilic group-containing oligomer, perfluoroalkyl group, hydrophilic group and lipophilic group-containing oligomer, perfluoroalkyl group and lipophilic group-containing urethane.

[0549] The surfactants can be used alone or in combination of two or more kinds. The content of the surfactant relative to the total solid content of the layer containing tabular grains is preferably in the range of 0.001 to 10 mass %, more preferably 0.01 to 5 mass %.

[0550] In the case where the backcoat layer contains a polymer, dyes for coloring, silane coupling agents for improving adhesion to the aluminum support, diazo resins consisting of diazonium salts, organic phosphonic acids, organic phosphoric acids, cationic polymers, and the like, as well as waxes commonly used as slipping agents, higher fatty acids, higher fatty acid amides, silicone compounds consisting of dimethylsiloxane, modified dimethylsiloxanes, polyethylene powders, and the like can be appropriately added.

[0551] The coating amount of the backcoat layer is preferably 0.01 to 30 g / m 2 , more preferably 0.1 to 10 g / m 2 , and particularly preferably 0.2 to 5 g / m 2 It is.

[0552] (Grains other than tabular grains) The backcoat layer preferably further contains particles other than the above-mentioned tabular particles (hereinafter also referred to as "non-tabular particles"). By containing non-tabular particles, the back layer is more unlikely to be scratched or peeled off, which is preferable. Here, the non-tabular particles can be any particles that do not belong to the above-mentioned range of tabular particles. That is, the aspect ratio of the particles other than ...

Claims

1. An on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, the on-press development type lithographic printing plate precursor having a sagging region at an edge portion, The sagging region has a crack whose deepest portion reaches the aluminum support, A phosphoric acid compound is present in the cracks, a ratio of phosphorus to aluminum (P / Al) measured by FE-AES on a surface of a crack region formed in the aluminum support inside the crack is 0.04 or more; When the solid content of one or more constituent layers at the end of the on-press development type lithographic printing plate precursor is A and the solid content of one or more constituent layers in the region other than the end of the on-press development type lithographic printing plate precursor is B, A≧B, and the difference between A and B, A−B, is 0.8 g / m 2 is less than On-press development type lithographic printing plate precursor.

2. The on-press development type lithographic printing plate precursor according to claim 1 , wherein the phosphoric acid compound is at least one compound selected from the group consisting of phosphoric acid, phosphonic acid, phosphinic acid, phosphoric acid salts, phosphonic acid salts, and phosphinic acid salts.

3. The on-press development type lithographic printing plate precursor according to claim 1 , wherein a ratio of phosphorus element to aluminum element (P / Al) is 0.06 or more.

4. A-B is 0.6g / m 2 2. The on-press development type lithographic printing plate precursor according to claim 1, wherein:

5. an on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, a sagging region at an end portion, a crack in the sagging region whose deepest portion reaches the aluminum support, A method for producing an on-press development type lithographic printing plate precursor, comprising the step of producing the on-press development type lithographic printing plate precursor according to claim 1 by mist-spraying a liquid containing a phosphoric acid compound.

6. The method for preparing an on-press development type lithographic printing plate precursor according to claim 5, wherein the concentration of the liquid containing the phosphoric acid compound is from 0.1 to 50% by mass.

7. A method for producing an on-press development type lithographic printing plate precursor according to claim 1, comprising spraying a mist of water into the inside of the crack of an on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, the on-press development type lithographic printing plate precursor having a sagging region at an end and a crack in the sagging region whose deepest portion reaches the aluminum support, at least one of the constituent layers including a layer containing a phosphoric acid compound.

8. The amount of mist sprayed is 0.1 g / m 2 ~50g / m 2 The method for preparing an on-press development type lithographic printing plate precursor according to claim 5 or 7,

9. 2. A method for producing an on-press development type lithographic printing plate precursor comprising: exposing an on-press development type lithographic printing plate precursor having an aluminum support having an anodized film and one or more constituent layers including an image recording layer, the on-press development type lithographic printing plate precursor having a sagging region at an edge and a crack in the sagging region whose deepest part reaches the aluminum support, the one or more constituent layers including a layer containing a phosphoric acid compound, to an environment of 60 to 95% RH at a relative humidity of 25° C. for 1 minute or more to produce the on-press development type lithographic printing plate precursor according to claim 1.

10. The method for preparing an on-press development type lithographic printing plate precursor according to claim 9, wherein the on-press development type lithographic printing plate precursor is exposed to an environment of 70 to 95% RH as a relative humidity in a 25° C. environment for 1 minute or more.

11. The method for preparing an on-press development type lithographic printing plate precursor according to claim 9, wherein the on-press development type lithographic printing plate precursor is exposed to an environment of 80 to 95% RH as a relative humidity in a 25° C. environment for 1 minute or more.

12. The method for preparing an on-press development type lithographic printing plate precursor according to any one of claims 5, 7 and 9, wherein the phosphoric acid compound is at least one compound selected from the group consisting of phosphoric acid, phosphonic acid, phosphinic acid, phosphoric acid salts, phosphonic acid salts and phosphinic acid salts.

13. A dummy lithographic printing plate having an aluminum support having an anodized film and one or more constituent layers including a polymer layer, the dummy plate having a sagging region at an edge portion, the sagging region has a crack whose deepest portion reaches the aluminum support, A phosphoric acid compound is present in the cracks, a ratio of phosphorus element to aluminum element (P / Al) measured by FE-AES on the surface of a crack region formed in the aluminum support inside the crack is 0.04 or more, and when a solid content of one or more constituent layers at the end portion of the dummy lithographic printing plate is A and a solid content of one or more constituent layers in a region other than the end portion of the dummy lithographic printing plate is B, A≧B, and the difference between A and B, A−B, is 0.8 g / m 2 A lithographic printing plate dummy plate that is less than 100 mm.

14. The dummy lithographic printing plate according to claim 13, wherein the phosphoric acid compound is at least one compound selected from the group consisting of phosphoric acid, phosphonic acid, phosphinic acid, phosphoric acid salts, phosphonic acid salts, and phosphinic acid salts.

15. The dummy lithographic printing plate according to claim 13, wherein a ratio of phosphorus element to aluminum element (P / Al) is 0.06 or more.

16. A-B is 0.6g / m 2 The dummy lithographic printing plate according to claim 13, wherein:

17. A dummy lithographic printing plate has an aluminum support having an anodized film and one or more constituent layers including a polymer layer, and has a sagging region at an end, and the sagging region has a crack whose deepest part reaches the aluminum support, and A method for producing a dummy lithographic printing plate, comprising the steps of: producing the dummy lithographic printing plate according to claim 13 by mist-spraying a liquid containing a phosphoric acid compound.

18. The method for producing a dummy lithographic printing plate according to claim 17, wherein the concentration of the liquid containing the phosphoric acid compound is 0.1 to 50% by mass.

19. A method for producing a dummy lithographic printing plate, comprising: spraying water into the inside of the crack of a dummy lithographic printing plate having an aluminum support having an anodized film and one or more constituent layers including a polymer layer, a sagging region at an end, and a crack in the sagging region whose deepest part reaches the aluminum support, wherein at least one of the one or more constituent layers includes a layer containing a phosphoric acid compound, thereby producing the dummy lithographic printing plate described in claim 13.

20. The amount of mist sprayed is 0.1 g / m 2 ~50g / m 2 The method for producing a dummy lithographic printing plate according to claim 17 or 19,

21. A method for producing a dummy lithographic printing plate, comprising exposing a dummy lithographic printing plate having an aluminum support having an anodized film and one or more constituent layers including a polymer layer, a sagging region at an edge, and a crack in the sagging region whose deepest part reaches the aluminum support, wherein at least one of the one or more constituent layers includes a layer containing a phosphoric acid compound, to an environment of 60 to 95% RH at a relative humidity of 25° C. for one minute or more to produce the dummy lithographic printing plate according to claim 13.

22. The method for preparing a dummy lithographic printing plate according to claim 21, wherein the dummy lithographic printing plate is exposed to an environment of 70 to 95% RH as a relative humidity in a 25° C. environment for one minute or more.

23. The method for preparing a dummy lithographic printing plate according to claim 21, wherein the dummy lithographic printing plate is exposed to an environment of 80 to 95% RH as a relative humidity in a 25° C. environment for 1 minute or more.

24. The method for preparing a dummy lithographic printing plate according to any one of claims 17, 19 and 21, wherein the phosphoric acid compound is at least one compound selected from the group consisting of phosphoric acid, phosphonic acid, phosphinic acid, phosphoric acid salts, phosphonic acid salts, and phosphinic acid salts.

Citation Information

Patent Citations

  • Original lithographic printing plate and its use

    JP2020501936A

  • Systems and methods for pitch axis envelope limiting of aircraft

    JP2021075268A

  • On-machine development type lithographic printing plate precursor processing method and printing method

    WO2015129504A1

  • On-press development type lithographic printing plate precursor, method for fabricating lithographic printing plate, on-press development type lithographic printing plate dummy plate, and printing method

    WO2019151447A1