Conductive paste, electronic component, and multilayered ceramic capacitor
A conductive paste with a specific solvent and dispersant composition addresses the viscosity and sheet attack issues in small particle conductive pastes, ensuring high smoothness and printability for multilayer ceramic capacitors.
Patent Information
- Application Number
- JP2024029798
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-02-29
- Publication Date
- 2024-10-15
AI Technical Summary
Conductive pastes with small particle sizes (100 nm or less) face issues with increased viscosity due to solvents like dihydroterpinyl acetate, leading to sheet attack and poor printability, making it difficult to achieve smooth printed films in multilayer ceramic capacitors.
A conductive paste composition using a conductive powder with an average particle diameter of 100 nm or less, incorporating a dispersant with a weight average molecular weight of 1000 or less, and a solvent system comprising glycol derivatives, dihydroterpineyl acetate, dihydroterpineol, and alkanediol, with specific mass ratios, maintains viscosity between 20-80 Pa·s, preventing sheet attack and ensuring high smoothness.
The solution provides a conductive paste with rheological properties suitable for screen printing, resulting in high smoothness and preventing sheet attack, thus enhancing the printability and quality of multilayer ceramic capacitors.
Smart Images

Figure 2024146781000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive paste, an electronic component, and a multilayer ceramic capacitor. [Background technology]
[0002] As electronic devices such as mobile phones and digital devices become lighter, thinner, and smaller, there is a demand for chip components such as multilayered ceramic capacitors (hereafter referred to as "MLCC") to be smaller, have higher capacitance, and perform better. The most effective way to achieve this is to make the internal electrode layers and dielectric layers thinner and create more layers.
[0003] MLCCs are generally manufactured as follows. First, to form a dielectric layer, a dielectric green sheet is formed using a dielectric ceramic powder such as barium titanate (BaTiO3) as the main component, and a binder resin made of a butyral resin such as polyvinyl butyral or an acrylic resin. A conductive paste composition in which a conductive powder is dispersed in an organic vehicle containing a binder resin and an organic solvent is printed in a predetermined pattern on the surface of the dielectric green sheet, and the conductive paste composition is dried to remove the organic solvent, forming a dry film that becomes an internal electrode layer. The dielectric green sheets on which the dry film is formed are stacked in multiple layers and integrated by heat and pressure bonding, and then cut to obtain chips, and the chips are subjected to a binder removal treatment at 500°C or less in an oxidizing atmosphere or an inert atmosphere. After that, the chips after the binder removal treatment are heated and fired at about 1300°C in a reducing atmosphere so as not to oxidize the internal electrode layers, and the internal electrode layers and the dielectric layers are integrated to obtain fired chips. Finally, a paste for external electrodes is applied to the fired chip and fired, and then the resulting external electrodes are plated with nickel or the like to complete the MLCC.
[0004] Conductive pastes for internal electrodes may be applied by various printing methods such as gravure printing, offset printing, inkjet printing, and screen printing. Therefore, the paste composition for internal electrodes is required to have rheological properties suitable for each printing method. For example, International Publication WO2014 / 073530 and JP2018-107089A discuss compositions of conductive paste compositions suitable for the rheological properties of gravure printing, JP2017-084588A discuss compositions suitable for the rheological properties of inkjet printing, and International Publication WO2014 / 104053A discuss compositions suitable for the rheological properties of screen printing.
[0005] A conductive paste composition for an internal electrode is generally obtained by dispersing a conductive powder, a ceramic powder, and a dispersant in an organic vehicle obtained by dissolving a binder resin in an organic solvent, and adjusting the viscosity with the organic solvent. Ethyl cellulose or the like is generally used as the binder resin constituting this organic vehicle, and terpineol has been used as the organic solvent (see JP 2018-168238 A).
[0006] However, because terpineol has high solubility in butyral resins and acrylic resins, when forming the internal electrode layer by coating the conductive paste, the dielectric green sheet may be corroded by the solvent in the conductive paste, causing the dielectric layer to become non-uniform, a phenomenon known as sheet attack.To prevent sheet attack, a solvent composition containing dihydroterpinyl acetate, which has low solubility in butyral resins and acrylic resins, has been investigated (see Japanese Patent Publication No. 2976268).
[0007] However, a solvent composition containing dihydroterpinyl acetate tends to increase the viscosity of the conductive paste, which can make printing on a dielectric green sheet difficult.
[0008] In addition, with the recent trend toward thinner electrode patterns, there is a demand for conductive pastes that use conductive powders with an average particle size of 100 nm or less, but pastes that contain conductive powders with such small particle sizes tend to have high viscosity. For this reason, when using conductive powders with an average particle size of 100 nm or less, if a solvent composition containing dihydroterpinyl acetate is used as a countermeasure against sheet attack, the viscosity of the conductive paste, which tends to be high, increases further, making it difficult to print the conductive paste and reducing the smoothness of the resulting printed film. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] International Publication No. WO2014 / 073530 [Patent Document 2] JP 2018-107089 A [Patent Document 3] JP 2017-084588 A [Patent Document 4] International Diet Publication No. WO2014 / 104053 [Patent Document 5] JP 2018-168238 A [Patent Document 6] Patent No. 2976268 Summary of the Invention [Problem to be solved by the invention]
[0010] In view of the above circumstances, the present invention aims to provide a conductive paste, an electronic component, and a multilayer ceramic capacitor that use a conductive powder with an average particle size of 100 nm or less that accompanies the thinning of electrode patterns, and that are less susceptible to sheet attack, have rheological properties suitable for screen printing, and produce a printed film with high smoothness after screen printing. [Means for solving the problem]
[0011] In order to solve the above problems, the conductive paste of the present invention is a conductive paste containing a conductive powder, a dispersant, a binder resin and an organic solvent, wherein the dispersant contains at least one of a polyalkylene glycol derivative having a weight-average molecular weight of 1000 or less and a polyalkylene glycol having a weight-average molecular weight of 1000 or less, the organic solvent contains dihydroterpineol acetate, dihydroterpineol and an alkanediol, and the content of the organic solvent is 40% by mass or more and 65% by mass or less.
[0012] The conductive paste may further include a ceramic powder.
[0013] The conductive powder may be nickel powder.
[0014] The conductive paste is applied at a temperature of 25°C and a shear rate of 4 seconds. -1 The viscosity at may be 20 Pa·s or more and less than 80 Pa·s.
[0015] The content of the dispersant may be 0.5% by mass or more and 0.75% by mass or less.
[0016] The mass ratio of the dihydroterpinyl acetate, the dihydroterpineol, and the alkanediol may be 6 or more and 8 or less: 0.5 or more and 2 or less: 0.5 or more and 2 or less.
[0017] The alkanediol may be 2-ethyl-1,3-hexanediol.
[0018] The organic solvent may further include mineral spirits.
[0019] The mass ratio of the dihydroterpineol acetate, the dihydroterpineol, the mineral spirits and the alkanediol may be 3 or more and 4 or less: 0.5 or more and 2 or less: 4 or more and 6 or less: 0.5 or more and 1 or less.
[0020] The binder resin may include ethyl cellulose.
[0021] The binder resin may further contain, in addition to the ethyl cellulose, at least one resin selected from methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, nitrocellulose, and polyvinyl butyral.
[0022] The mass ratio of the sum of the polyalkylene glycol derivative and the polyalkylene glycol to the conductive powder may be 0.01 to 4:100, and the content of the conductive powder may be 35% by mass to 65% by mass.
[0023] The number average particle size of the conductive powder may be 30 nm or more and 100 nm or less.
[0024] In order to achieve the above object, an electronic component of the present invention is an electronic component formed by using the conductive paste of the present invention.
[0025] In order to solve the above problems, the multilayer ceramic capacitor of the present invention is a multilayer ceramic capacitor having at least a laminate in which dielectric layers and internal electrode layers are laminated, and the internal electrode layers are formed using the conductive paste of the present invention. Effect of the Invention
[0026] As described above, according to the present invention, it is possible to provide a conductive paste, an electronic component, and a multilayer ceramic capacitor that use a conductive powder having an average particle size of 100 nm or less that accompanies thinning of an electrode pattern, are less susceptible to sheet attack, have rheological properties suitable for screen printing, and further have a high degree of smoothness of the printed film after screen printing. [Brief description of the drawings]
[0027] [Figure 1] 1A and 1B are a perspective view and a side cross-sectional view of a multilayer ceramic capacitor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Hereinafter, an embodiment of the conductive paste, electronic component, and multilayer ceramic capacitor of the present invention will be described.
[0029] [Conductive paste] The conductive paste of this embodiment is a conductive paste containing a conductive powder, a dispersant, a binder resin and an organic solvent, the binder resin containing ethyl cellulose having a mass average molecular weight of 30,000 to 150,000 and an ethoxy group content of 45% to 52% by mass, the dispersant containing at least one of a polyalkylene glycol derivative and a polyalkylene glycol, and the organic solvent containing dihydroterpineol acetate, dihydroterpineol and an alkanediol. The conductive paste may further contain a ceramic powder in addition to the conductive powder, the dispersant, the binder resin and the organic solvent, but the ceramic powder is not an essential component. The conductive powder, ceramic powder, binder resin, organic solvent and dispersant contained in the conductive paste of this embodiment will be described in detail below.
[0030] (conductive powder) The conductive powder is not particularly limited, and a metal powder can be used, for example, one or more metal powders selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof. Among these, Ni or Ni alloy powder is preferred from the viewpoints of conductivity, corrosion resistance, and cost. As the Ni alloy, for example, an alloy of Ni and at least one element selected from the group consisting of Mn, Cr, Co, Al, Fe, Cu, Zn, Ag, Au, Pt, and Pd (Ni alloy) can be used. The Ni content in the Ni alloy is, for example, 50 mass% or more, preferably 80 mass% or more. In addition, the Ni powder may contain about several hundred ppm of S in order to suppress rapid gas generation due to partial thermal decomposition of the binder resin during the binder removal process.
[0031] The number average particle size of the conductive powder is preferably 30 nm or more and 100 nm or less, more preferably 40 nm or more and 90 nm or less. When the average particle size of the conductive powder is in the above range, it can be suitably used as a conductive paste for an internal electrode of a thin-film multilayer ceramic capacitor, and the smoothness of the dried film is improved. Here, the number average particle size is a value determined by observation with a scanning electron microscope (SEM), and is the average value obtained by measuring the particle size of each of a plurality of particles from an image observed with an SEM at a magnification of 10,000 times.
[0032] The content of the conductive powder in the total amount of the conductive paste is preferably 35% by mass or more and 65% by mass or less, and more preferably 35% by mass or more and 60% by mass or less. When the content of the conductive powder is in the above range, the conductive paste has excellent conductivity and dispersibility.
[0033] (ceramic powder) The ceramic powder is not particularly limited, and a known ceramic powder is appropriately selected depending on the type of the multilayer ceramic capacitor to be applied. Examples of the ceramic powder include perovskite oxides containing Ba and Ti, and preferably barium titanate (BaTiO3).
[0034] The ceramic powder may be a ceramic powder containing barium titanate as a main component and oxides as subcomponents. Examples of oxides include oxides of Mn, Cr, Si, Ca, Ba, Mg, V, W, Ta, Nb, and one or more rare earth elements. The ceramic powder may be a perovskite-type oxide ferroelectric ceramic powder in which the Ba and Ti atoms of barium titanate (BaTiO3) are replaced with other atoms, such as Sn, Pb, and Zr.
[0035] Also, a powder having the same composition as the dielectric ceramic powder constituting the green sheet of the multilayer ceramic capacitor may be used as the ceramic powder. This suppresses the occurrence of cracks due to the mismatch of shrinkage at the interface between the dielectric layer and the internal electrode layer during the sintering process. In addition to the above, such ceramic powders include oxides such as ZnO, ferrite, PZT, BaO, Al2O3, Bi2O3, R (rare earth element)2O3, and TiO2. Note that one type of ceramic powder may be used, or two or more types may be used.
[0036] The number average particle diameter of the ceramic powder is, for example, 10 nm to 100 nm, preferably 10 nm to 70 nm. When the number average particle diameter of the ceramic powder is in the above range, it is possible to form a sufficiently thin and uniform internal electrode when used as a conductive paste for an internal electrode. The number average particle diameter is a value determined by observation with a scanning electron microscope (SEM), and is the average value obtained by measuring the particle diameter of each of a plurality of particles from an image observed with an SEM at a magnification of 50,000 times.
[0037] The content of the ceramic powder is preferably 1 part by mass or more and 30 parts by mass or less, more preferably 3 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the conductive powder is within the above range, the conductivity and dispersibility are excellent.
[0038] The content of the ceramic powder is preferably 1% by mass or more and 20% by mass or less, more preferably 3% by mass or more and 20% by mass or less, based on the total amount of the conductive paste. When the content of the conductive powder is within the above range, the conductive paste has excellent conductivity and dispersibility.
[0039] (binder resin) The binder resin essentially contains ethyl cellulose having a mass average molecular weight of 30,000 to 150,000 and an ethoxy group content of 45% to 52% by mass. By containing such ethyl cellulose, a conductive paste having high smoothness as a conductive film after drying can be obtained. In addition, there is a firing step in the process of processing the conductive paste into an internal electrode, and the residual carbon content after this firing does not increase excessively, so printability can be sufficiently ensured.
[0040] If the mass average molecular weight of the ethyl cellulose is less than 30,000, it may be difficult to obtain a sufficient viscosity for printing, and if the molecular weight is more than 150,000, the viscosity of the resulting conductive paste may be high, resulting in poor printability.
[0041] Furthermore, if the ethoxy group content of ethyl cellulose is 45% by mass or more and 52% by mass or less, the compatibility with organic solvents is excellent and the solubility is good, so that a conductive paste having a high smoothness as a conductive film after drying can be obtained. The ethoxy group content of ethyl cellulose is more preferably 47% by mass or more and 52% by mass or less.
[0042] The binder resin may be the above-mentioned ethyl cellulose alone or may further contain a resin other than ethyl cellulose. For example, the binder resin may further contain, in addition to ethyl cellulose, at least one resin selected from methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, nitrocellulose, and polyvinyl butyral.
[0043] From the viewpoint of improving the adhesive strength with the dielectric green sheet, the binder resin may contain polyvinyl butyral.
[0044] When a resin other than ethyl cellulose is contained as the binder resin, the mass ratio of ethyl cellulose:resin other than ethyl cellulose is preferably 10 or more and 90 or less:90 or more and 10 or less.
[0045] The content of the binder resin is preferably 1 part by mass or more and 10 parts by mass or less, more preferably 1 part by mass or more and 8 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the binder resin is within the above range, the conductive powder has excellent conductivity and dispersibility.
[0046] The content of the binder resin is preferably 0.5% by mass to 10% by mass, more preferably 1% by mass to 6% by mass, based on the entire conductive paste. When the content of the binder resin is within the above range, the conductive paste has excellent conductivity and dispersibility.
[0047] (Organic solvent) The organic solvent includes a solvent of dihydroterpinyl acetate, dihydroterpineol, and alkanediol. When the mass ratio of dihydroterpinyl acetate, dihydroterpineol, and alkanediol is 6 to 8: 0.5 to 2: 0.5 to 2, a conductive paste without sheet attack and with high smoothness after screen printing can be obtained. If this mass ratio is not met, the conductive paste may have a high viscosity that is not suitable for use in screen printing, and the smoothness of the conductive film after drying may be insufficient.
[0048] Furthermore, mineral spirits may be contained as an organic solvent. When mineral spirits is contained, if the mass ratio of dihydroterpineol acetate, dihydroterpineol, mineral spirits and alkanediol is 3 to 4: 0.5 to 2: 4 to 6: 0.5 to 1, a conductive paste without sheet attack and with high smoothness after screen printing can be obtained.
[0049] The alkanediol is not particularly limited, but examples of the alkanediol that can be used include 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 2-ethyl-1,3-hexanediol, 2-methyl-2,4-pentanediol, and 3-methyl-1,5-pentanediol.
[0050] The total content of the organic solvent is preferably 80 parts by mass or more and 160 parts by mass or less, more preferably 100 parts by mass or more and 140 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the organic solvent is within the above range, the conductive powder has excellent conductivity and dispersibility.
[0051] The total content of the organic solvent is preferably 40% by mass or more and 65% by mass or less, more preferably 50% by mass or more and 60% by mass or less, based on the entire conductive paste. When the content of the organic solvent is within the above range, the conductive paste has excellent conductivity and dispersibility.
[0052] (Dispersant) The dispersant contained in the conductive paste of the present invention is a polyalkylene glycol derivative or polyalkylene glycol. By containing such a dispersant, the conductive paste can have a viscosity suitable for use in screen printing, and a conductive paste having high smoothness as a conductive film after drying can be obtained.
[0053] In the conductive paste, the mass ratio of the total of the polyalkylene glycol derivative and the polyalkylene glycol to the conductive powder is preferably 0.01 to 4:100, and more preferably 0.02 to 3:100. When the polyalkylene glycol derivative and the polyalkylene glycol are contained within the above range, the viscosity change over time of the conductive paste is suppressed, the viscosity stability can be improved, and the obtained electrode layer has high smoothness. In addition, sheet attack and peeling failure of the green sheet can be suppressed. Note that, when the mass ratio of the total of the polyalkylene glycol derivative and the polyalkylene glycol to the conductive powder is more than 4:100, when the conductive paste is printed on the green sheet, mesh marks may be generated on the printed surface or the viscosity of the paste may be significantly reduced. Here, "the total of polyalkylene glycol derivatives and polyalkylene glycol" includes three cases: "the total of only polyalkylene glycol derivatives when the conductive paste does not contain polyalkylene glycol but contains only polyalkylene glycol derivatives", "the total of only polyalkylene glycols when the conductive paste does not contain polyalkylene glycol derivatives but contains only polyalkylene glycol", and "the total of polyalkylene glycols and polyalkylene glycol derivatives when the conductive paste contains both polyalkylene glycol and polyalkylene glycol derivatives".
[0054] The polyalkylene glycol derivative is an acid-based compound and may contain functional groups such as a carboxyl group, a phenol group, a sulfo group, and a phosphoric acid group. The weight-average molecular weight of the polyalkylene glycol derivative and the polyalkylene glycol, measured by GPC (Gel Permeation Chromatography), in terms of polystyrene is 1000 or less. If the weight-average molecular weight of the polyalkylene glycol derivative and the polyalkylene glycol exceeds 1000, a viscosity appropriate for a conductive paste cannot be obtained. Examples of such dispersants include the Newpol series of Sanyo Chemical Industry Co., Ltd. and the Unilube series of NOF Corporation, but are not limited thereto. In addition, the polyalkylene glycol and the polyalkylene glycol derivative may be used in combination. In addition, the type of the polyalkylene glycol and the polyalkylene glycol derivative used in the dispersant may be only one type, or two or more types.
[0055] The conductive paste may contain a dispersant other than the polyalkylene glycol derivative as long as the effect of the present invention is not impaired. Examples of the dispersant other than the above include higher fatty acids, amine-based dispersants, amino acid-based dispersants, cationic dispersants other than acid-based dispersants, nonionic dispersants, amphoteric surfactants, and polymer-based dispersants. These dispersants may be used alone or in combination of two or more.
[0056] (Method of manufacturing conductive paste) The method for producing the conductive paste of the present embodiment is not particularly limited, and a conventionally known method can be used. The conductive paste can be produced, for example, by preparing the above-mentioned components and stirring and kneading them with a three-roll mill, a ball mill, a mixer, or the like. In this case, if a dispersant is applied to the surface of the conductive powder in advance, the conductive powder is sufficiently loosened without agglomeration, and the dispersant is distributed over the surface, making it easy to obtain a uniform conductive paste. Alternatively, the binder resin may be dissolved in an organic solvent for a vehicle to produce an organic vehicle, and the conductive powder, ceramic powder, organic vehicle, and dispersant may be added to the organic solvent for the paste, and the mixture may be stirred and kneaded with a mixer to produce the conductive paste.
[0057] The conductive paste can be suitably used in electronic components such as multilayer ceramic capacitors, varistors, etc. A multilayer ceramic capacitor has dielectric layers formed using dielectric green sheets and internal electrode layers formed using the conductive paste.
[0058] In the multilayer ceramic capacitor, the dielectric ceramic powder contained in the dielectric green sheet and the ceramic powder contained in the conductive paste are preferably powders of the same composition. In the multilayer ceramic capacitor manufactured using the conductive paste of this embodiment, even if the thickness of the dielectric green sheet is, for example, 2 μm or less, sheet attack and peeling failure of the green sheet are suppressed.
[0059] [Electronic components] Hereinafter, embodiments of electronic components and the like that can be manufactured using the conductive paste of the present invention will be described with reference to the drawings. In the drawings, the components may be shown in schematic form or at a different scale as appropriate. The positions and directions of components will be described with reference to the XYZ orthogonal coordinate system shown in FIG. 1 as appropriate. In this XYZ orthogonal coordinate system, the X and Y directions are horizontal directions, and the Z direction is vertical (up-down direction).
[0060] 1A and 1B are a perspective view and a side cross-sectional view showing a multilayer ceramic capacitor 1, which is an example of an electronic component according to an embodiment. The multilayer ceramic capacitor 1 includes a ceramic laminate 10 in which dielectric layers 12 and internal electrode layers 11 are alternately laminated, and an external electrode 20.
[0061] A method for manufacturing the multilayer ceramic capacitor 1 using the conductive paste will be described below. First, the conductive paste is printed on a dielectric layer made of a ceramic green sheet, and dried to form a dry film. A plurality of dielectric layers having this dry film on the upper surface are laminated by pressure bonding to obtain a laminate, and the laminate is then fired and integrated to produce a ceramic laminate 10 in which internal electrode layers 11 and dielectric layers 12 are alternately laminated. Then, a pair of external electrodes 20 is formed on both ends of the ceramic laminate 10 to manufacture the multilayer ceramic capacitor 1. A more detailed description will be given below.
[0062] First, a ceramic green sheet, which is an unfired ceramic sheet, is prepared. For example, the ceramic green sheet is prepared by adding an organic binder such as polyvinyl butyral and a solvent such as terpineol to a raw powder of a specific ceramic such as barium titanate, applying the dielectric layer paste to a support film such as a PET film in a sheet form, and drying to remove the solvent. The thickness of the dielectric layer made of the ceramic green sheet is not particularly limited, but is preferably 0.05 μm or more and 3 μm or less from the viewpoint of the demand for miniaturization of the multilayer ceramic capacitor.
[0063] Next, the above-mentioned conductive paste is printed (applied) on one side of the ceramic green sheet by a known method such as screen printing, and then dried to form a dry film, to prepare a plurality of sheets. Note that, from the viewpoint of the requirement for thinning of the internal electrode layer 11, it is preferable that the thickness of the printed conductive paste (dried film) is 1 μm or less after drying.
[0064] Next, the ceramic green sheet is peeled off from the support film, and the dielectric layer made of the ceramic green sheet and the dry film formed on one side thereof are alternately laminated, and then a laminate is obtained by a heat and pressure treatment. Note that a configuration in which protective ceramic green sheets not coated with the conductive paste are further arranged on both sides of the laminate may be adopted.
[0065] Next, the laminate is cut to a predetermined size to form green chips, and the green chips are subjected to a binder removal treatment and fired under a reducing atmosphere to produce the ceramic laminate 10. The binder removal treatment is preferably performed in air or N2 gas. The temperature during the binder removal treatment is, for example, 200°C or higher and 400°C or lower. The temperature is preferably held for 0.5 hours or higher and 24 hours or lower during the binder removal treatment. The firing is performed in a reducing atmosphere to suppress oxidation of the metal used in the internal electrode layers, and the temperature during firing of the laminate is, for example, 1000°C or higher and 1350°C or lower, and the temperature is held for, for example, 0.5 hours or higher and 8 hours or lower.
[0066] By firing the green chip, the organic binder in the green sheet is completely removed, and the ceramic raw material powder is fired to form the ceramic dielectric layer 12. The organic vehicle in the dried film is also removed, and the nickel powder or the alloy powder mainly composed of nickel is sintered or melted and integrated to form the internal electrodes, forming a multilayer ceramic sintered body in which the dielectric layers 12 and the internal electrode layers 11 are alternately stacked. Note that, from the viewpoint of taking oxygen into the dielectric layers to increase reliability and suppressing reoxidation of the internal electrodes, the multilayer ceramic sintered body after firing may be subjected to an annealing treatment.
[0067] A pair of external electrodes 20 is then provided on the produced fired laminated ceramic body to manufacture the laminated ceramic capacitor 1. For example, the external electrode 20 includes an external electrode layer 21 and a plating layer 22. The external electrode layer 21 is electrically connected to the internal electrode layer 11. The external electrode 20 is preferably made of, for example, copper, nickel, or an alloy thereof. The electronic component is not limited to a laminated ceramic capacitor, and may be an electronic component other than a laminated ceramic capacitor, such as a varistor. EXAMPLES
[0068] The present invention will be described in detail below based on examples and comparative examples, but the present invention is not limited to these examples.
[0069] [Materials used] (conductive powder) As the conductive powder, Ni powder (number average particle size 60 nm) was prepared by the following method and used.
[0070] <Wet nickel powder production> [Preparation of solutions of nickel salts and metal salts of metals more noble than nickel] An aqueous solution of nickel chloride hexahydrate (NiCl2·6H2O, molecular weight: 237.69) was dissolved in 1 L of pure water so that 100 g of Ni metal was present (referred to as the "100 g-Ni / L aqueous solution"). Another aqueous solution of ammonium palladium (II) chloride (also known as ammonium tetrachloropalladate (II)) ((NH4)2PdCl4, molecular weight: 284.31), a metal salt of a metal more noble than nickel, was dissolved in 1 L of pure water so that 1.2 g of Pd metal was present (referred to as the "1.2 g-Pd / L aqueous solution"). Then, 1000mL of 100g-Ni / L aqueous solution, 8.5mL of 1.2g-Pd / L aqueous solution, and 1.27g of L-methionine (CH3SC2H4CH(NH2)COOH, molecular weight: 149.21) containing one sulfide group (-S-) in the molecule as a sulfur-containing compound as an autolysis suppression auxiliary were dissolved in 881mL of pure water to prepare a nickel salt nucleating agent-containing solution, which is an aqueous solution containing nickel salt as the main component, a sulfur-containing compound, and a nucleating agent that is a metal salt of a metal more noble than nickel. Here, in the nickel salt nucleating agent-containing solution, the sulfide compound L-methionine is a trace amount of 0.005 (0.5 mol%) in molar ratio to nickel, and palladium (Pd) is 100 mass ppm (55.16 mol ppm) to nickel (Ni).
[0071] [Preparation of reducing agent solution] As a reducing agent, hydrazine hydrate (N2H4·H2O, molecular weight: 50.06) was diluted 1.67 times with pure water to prepare 207 g of commercially available industrial grade 60% hydrazine hydrate (Otsuka-MGC Chemical Co., Ltd.) to prepare a reducing agent solution, which is an aqueous solution containing hydrazine as the main component and does not contain alkali hydroxide.
[0072] [Alkaline hydroxide solution] As the alkali hydroxide, sodium hydroxide (NaOH, molecular weight: 40.0) was dissolved in pure water to prepare 757 mL of an alkali hydroxide solution containing sodium hydroxide at a concentration of 382 g / L.
[0073] [Amine compound solution] As an amine compound, 1.02 g of ethylenediamine (abbreviation: EDA) (H2NC2H4NH2, molecular weight: 60.1), an alkyleneamine containing two primary amino groups (-NH2) in the molecule, was dissolved in 18 mL of pure water to prepare an amine compound solution, which is an aqueous solution containing ethylenediamine. Note that, with the exception of 60% hydrazine hydrate, all of the materials used in the nickel salt nucleating agent-containing solution, reducing agent solution, alkali hydroxide solution, and amine compound solution were reagents manufactured by Wako Pure Chemical Industries, Ltd.
[0074] [Crystallization process] The nickel salt nucleating agent-containing solution was placed in a Teflon (registered trademark)-coated stainless steel container equipped with a stirring blade, and heated while stirring until the liquid temperature reached 85°C. After that, a reducing agent solution with a liquid temperature of 27°C was added and mixed for 10 seconds so that the molar ratio of Ni metal to hydrazine hydrate became 1:1.46 to prepare a nickel salt-reducing agent-containing solution. An alkali hydroxide solution with a liquid temperature of 27°C was added and mixed for 120 seconds to this nickel salt-reducing agent-containing solution so that the molar ratio of Ni metal to sodium hydroxide became 1:3.54 to prepare a reaction solution (nickel chloride + palladium salt + hydrazine + sodium hydroxide) with a liquid temperature of 70°C, and the reduction reaction (crystallization reaction) was initiated (reaction start temperature 70°C). The amine compound solution was added dropwise to the reaction solution over a period of 20 minutes from 8 to 28 minutes after the start of the reaction so that the molar ratio of Ni metal to ethylenediamine was 1:0.01 (1.0 mol%), and the reduction reaction was carried out while suppressing the self-decomposition of hydrazine, causing nickel crystallization powder to precipitate in the reaction solution. The reduction reaction was completed within 60 minutes from the start of the reaction, and the supernatant of the reaction solution was transparent, confirming that all the nickel components in the reaction solution were reduced to metallic nickel and became nickel crystallization powder. The reaction solution containing the nickel crystallization powder was in the form of a slurry, and an aqueous solution of mercaptoacetic acid (thioglycolic acid) (HSCH2COOH, molecular weight: 92.12) was added to this nickel crystallization powder-containing slurry to perform surface treatment (sulfur coating treatment) of the nickel crystallization powder.
[0075] [Wet crushing process] After the surface treatment, the nickel crystallized powder-containing slurry was washed by repeatedly decanting and adding pure water (electrical conductivity 1 μS / cm) until the electrical conductivity of the slurry became 15 μS / cm or less, and the nickel crystallized powder-containing slurry with a nickel concentration of 25 mass% was obtained, and then subjected to wet crushing.
[0076] [Acid washing process] The nickel crystallized powder-containing slurry after the wet disintegration process was neutralized by dropping 1% by mass of sulfuric acid aqueous solution (H2SO4, molecular weight: 98.08) and maintaining the pH of the nickel crystallized powder-containing slurry at 4 to 5 for 20 minutes. The nickel concentration of the nickel crystallized powder-containing slurry at this time was 5% by mass. The neutralization reaction formula is Ni(OH)2+H2SO4→NiSO4+2H2O.
[0077] [Solvent replacement process, solid-liquid separation process] After the acid washing step, a filter paper was placed on the Nutsche, and the nickel crystallized powder-containing slurry was added thereto for filtration. Then, pure water with a conductivity of 1 μS / cm was added to the nickel crystallized powder on the filter paper, and the filtrate was filtered and washed until the conductivity of the filtrate after filtration was 30 μS / cm or less. Then, ethanol (boiling point: 78.3 ° C) with a purity of 99.9% or more was added to the Nutsche and passed through, and the solvent in the nickel slurry was replaced from water to ethanol. The ethanol concentration contained in the solvent of the nickel slurry after the solvent replacement was 92.4 mass%, and the remaining 7.6 mass% was water. Here, the ethanol concentration was determined by collecting the final filtrate (last 50 mL) of the solid-liquid separation step, measuring the Karl Fischer moisture content (150 ° C), and calculating "100-moisture content (%) = solvent concentration in the filtrate (%)", and the ethanol concentration was determined as the solvent concentration in the filtrate. It was calculated in the same manner in other examples. After the solvent replacement, filtration was continued until the solid content concentration reached 40 mass % or more to perform solid-liquid separation, and a nickel powder cake was obtained.
[0078] [Drying process] The nickel powder cake was dried in a vacuum dryer set at a temperature of 120° C. for 6 hours to obtain wet nickel powder.
[0079] <Evaluation of conductive powder and its results> (number average particle size) The obtained wet nickel powder was observed with a scanning electron microscope (SEM, JEOL Ltd., JSM-7100F), and the area of 100 to 200 particles whose overall shape could be confirmed by image processing of the SEM images was measured, and the diameter of each particle was calculated by converting the measured area into a perfect circle, and the average of the calculated diameters was calculated, which was taken as the number average particle size. The number average particle size of the obtained nickel powder was 60 nm.
[0080] (binder resin) The binder resin used was prepared by dissolving 10.5% by mass of ethyl cellulose resin (weight average molecular weight 100,000, ethoxy group content of 48.0% by mass to 49.5% by mass) in dihydroterpinyl acetate as a vehicle.
[0081] (Dispersant) The dispersants used were a polyalkylene glycol derivative having a weight-average molecular weight of 1,000 or less and an acidic functional group, a polyalkylene glycol derivative having a weight-average molecular weight of 10,000 or more and an acidic functional group, and an amine derivative (N,N-di(hydroxyethyl)laurylamine).
[0082] [Examples 1, 2, and 3] Ni powder 44% by mass, ethyl cellulose resin (weight average molecular weight 100x10 3A binder resin in a vehicle consisting of a polyalkylene glycol derivative (a polyalkylene glycol derivative having a weight-average molecular weight of 1000 or less and an acidic functional group and an ethoxy group content of 48.0% by mass or more and 49.5% by mass or less) as a dispersant, and an organic solvent listed in the solvent composition column in Table 1 below were prepared. Then, the binder resin was mixed to a total of 3% by mass, the polyalkylene glycol derivative was mixed to a total of 0.5% by mass or 0.75% by mass (0.50% by mass in Example 1, 0.75% by mass in Example 2, and 0.80% by mass in Example 3), and the organic solvent was mixed to a total of 100% by mass as a whole, and these materials were mixed in a three-roll mill to prepare a conductive paste, and the viscosity, printed film smoothness, and sheet attack property were evaluated.
[0083] In the solvent composition column in Table 1 below, DHTA is dihydroterpineol acetate, DHT is dihydroterpineol, MSA is mineral spirits A, and EtHexdiol is 2-ethyl-1,3-hexanediol (alkanediol). In addition, the numerical values such as 70 / 15 / 15 indicate mass ratios. According to this, for example, in Example 1 in which the solvent composition column states DHTA / DHT / EtHexdiol=70 / 15 / 15, dihydroterpineol acetate, dihydroterpineol, and 2-ethyl-1,3-hexanediol are blended as organic solvents in a mass ratio of 70:15:15.
[0084] [Comparative Examples 1 to 6] In comparison with the examples, the composition and blending of the organic solvent were changed to give Comparative Examples 1 to 6. In each Comparative Example, the dispersant used was a polyalkylene glycol derivative or an amine derivative (N,N-di(hydroxyethyl)laurylamine) similar to that in Example 1. In Comparative Example 6, a polyalkylene glycol derivative dispersant having a weight average molecular weight of 10,000 or more and an acidic functional group was used. In each Comparative Example, the mass % concentration of the dispersant when the entire conductive paste is taken as 100 mass % was set to one of 0.25 mass %, 0.75 mass %, and 1.00 mass %. The conductive pastes thus composed were evaluated for viscosity, print film smoothness, and sheet attack resistance.
[0085] [Table 1]
[0086] [Evaluation method] (viscosity) The viscosity of the conductive paste composition was measured at 25°C using a rheometer (Anton Paar MCR501 Rheometer) after leaving the conductive paste composition at room temperature (25°C) for one day from the time of production. -1 If the viscosity was between 20 Pa·s and 60 Pa·s, it was evaluated as ○ (excellent), if it was between 60 Pa·s and 80 Pa·s, it was evaluated as △ (good), and if it was 80 Pa·s or more, it was evaluated as × (unacceptable). If it was rated as ○ (excellent) or △ (good), it had a viscosity that was particularly suitable for screen printing, i.e., it had rheological properties.
[0087] (Printed film smoothness evaluation) The conductive paste composition was applied by screen printing onto a 4 μm thick dielectric green sheet, and dried in a thermal convection oven at 80°C for 5 minutes. Confocal images were then taken with a laser microscope (Keyence, VK-X1000) with a 20x objective lens to evaluate the waviness Wc value (cutoff λc = 0.08 mm). A Wc value of less than 0.45 μm was evaluated as ◯ (good), and a value of 0.45 μm or more was evaluated as × (not good).
[0088] (Seat attack evaluation) The conductive paste composition was applied to a 4 μm-thick dielectric green sheet in a thickness of 0.1 mm and a diameter of 5 mm, and then dried in a thermal convection oven at 80°C for 20 minutes. The back surface of the dielectric green sheet where the conductive paste composition was dropped was visually checked for erosion. Those without erosion were rated as ◎ (best quality), those with slight erosion were rated as ○ (good quality), those with partial erosion were rated as △ (good quality), and those with severe erosion that exposed the paste were rated × (unacceptable). When the back surface of the dielectric green sheet where the conductive paste composition was dropped was observed with an optical microscope, those where slight erosion was confirmed were rated as ○ (excellent quality).
[0089] From Examples 1 and 2 in Table 1, by using a polyalkylene glycol derivative with a weight average molecular weight of 1000 or less and an acidic functional group as a dispersant, using dihydroterpineol acetate, dihydroterpineol and 2-ethyl-1,3-hexanediol as an organic solvent in a solvent ratio of 70:15:15 by mass, and setting the mass % concentration of the dispersant to 0.5 mass % or 0.75 mass %, the viscosity of the conductive paste can be stabilized within a viscosity range of 20 Pa·s to 55 Pa·s, which is easy to apply the paste, and the average roughness of the dried film surface obtained from the conductive paste can be set to 0.03 μm or less, resulting in a higher smoothness of the dried film surface. In addition, the erosion of the dielectric green sheet by the conductive paste was slight, resulting in excellent results. In addition, in terms of viscosity, the viscosity of Example 1 is Δ (good) whereas the viscosity of Example 2 is ◯ (excellent), so it is more preferable that the mass % concentration of the dispersant is 0.75%.
[0090] From Example 3 in Table 1, by using a polyalkylene glycol derivative with a weight average molecular weight of 1000 or less and an acidic functional group as a dispersant, using dihydroterpineol acetate, dihydroterpineol, mineral spirit A, and 2-ethyl-1,3-hexanediol as organic solvents in a solvent ratio of 32:10:50:8 by mass, and setting the mass % concentration of the dispersant to 0.8 mass %, the viscosity of the conductive paste can be stabilized within a viscosity range of 20 Pa·s or more and less than 60 Pa·s, which is easy to apply the paste, and the average roughness of the dried film surface obtained from the conductive paste can be made 0.03 μm or less, resulting in further improving the smoothness of the dried film surface. In addition, it was possible to prevent the erosion of the dielectric green sheet by the conductive paste from occurring.
[0091] On the other hand, from Comparative Example 1 in Table 1, when only an amine-based dispersant (N,N-di(hydroxyethyl)laurylamine) was used as the dispersant, the viscosity was △ (good), which was slightly higher than that of Example 2. In addition, the smoothness of the printed film was × (not good). And the sheet attack property was ◯ (excellent). In other words, when only an amine-based dispersant was used, excellent sheet attack property could be obtained, but the viscosity of the conductive paste became slightly higher, making it difficult to obtain a smooth printed film.
[0092] In addition, in Comparative Examples 2 and 3 in Table 1, when EtHexdiol was not used as an organic solvent, the viscosity was × (not good) or ◯ (excellent). Furthermore, the print smoothness was × (not good). And the sheet attack property was ◯ (good) or △ (good). In other words, when EtHexdiol was not used as an organic solvent, excellent or good sheet attack property could be obtained, but it was difficult to obtain a smooth printed film.
[0093] Furthermore, from Comparative Example 4 in Table 1, when a polyalkylene glycol derivative having a weight average molecular weight of 1000 or less and an acidic functional group was used as a dispersant and the mass % concentration of the dispersant was set to 0.25%, the viscosity and print smoothness were × (not good), and the sheet attack property was ◯ (excellent). In other words, when the mass % concentration of the polyalkylene glycol derivative having a weight average molecular weight of 1000 or less and an acidic functional group was set to 0.25%, excellent sheet attack property could be obtained, but it was difficult to obtain a smooth printed film.
[0094] In addition, in Comparative Example 5 of Table 1, when a polyalkylene glycol derivative having a weight average molecular weight of 1000 or less and an acidic functional group was used as a dispersant and the mass % concentration of the dispersant was 1.00%, the viscosity was ◯ (excellent). In addition, the smoothness of the printed film was × (not good). And the sheet attack property was ◯ (excellent). In other words, when the mass % concentration of the polyalkylene glycol derivative having a weight average molecular weight of 1000 or less and an acidic functional group was 1.00%, it was possible to obtain excellent sheet attack property and viscosity, but it was difficult to obtain a smooth printed film.
[0095] In addition, from Comparative Example 6 in Table 1, when a polyalkylene glycol derivative having a weight average molecular weight of 10,000 or more and an acidic functional group is used as a dispersion, and the mass % concentration of the dispersant is 0.75%, the viscosity and the smoothness of the printed film are × (not good), and the sheet attack property is ◯ (excellent). In other words, when a polyalkylene glycol derivative having a weight average molecular weight of 10,000 or more and an acidic functional group is used as a dispersion, it is possible to provide excellent sheet attack property, but it is difficult to obtain a smooth printed film. From the results of this Comparative Example 6 and the results of Example 2 described above, it is preferable to set the upper limit of the weight average molecular weight of the dispersant to 1000. On the other hand, the lower limit of the weight average molecular weight of the dispersant is not particularly limited, but it may be set to about 200 as a polymer.
[0096] As described above, the present invention can provide a conductive paste which, as a conductive film after drying, is less susceptible to sheet attack, has rheological properties suitable for screen printing, and further produces a printed film with high smoothness after screen printing, and is therefore industrially useful. [Explanation of symbols]
[0097] 1...Multilayer ceramic capacitor 10...Ceramic laminate 11...Internal electrode layer 12...Dielectric layer 20...External electrode 21...External electrode layer 22…Plating layer
Claims
1. A conductive paste comprising a conductive powder, a dispersant, a binder resin and an organic solvent, the dispersant contains at least one of a polyalkylene glycol derivative having a weight-average molecular weight of 1000 or less and a polyalkylene glycol having a weight-average molecular weight of 1000 or less, The organic solvent comprises dihydroterpineol acetate, dihydroterpineol and an alkanediol; The conductive paste has an organic solvent content of 40% by mass or more and 65% by mass or less.
2. The conductive paste of claim 1 further comprising a ceramic powder.
3. The conductive paste according to claim 1 , wherein the conductive powder is nickel powder.
4. Temperature: 25°C and shear rate: 4 sec -1 2. The conductive paste according to claim 1, wherein the viscosity at 20 Pa·s or more and less than 80 Pa·s is 20 Pa·s or more and less than 80 Pa·s.
5. The conductive paste according to claim 1 , wherein the content of the dispersant is 0.5% by mass or more and 0.75% by mass or less.
6. The conductive paste according to claim 1 , wherein a mass ratio of the dihydroterpineol acetate, the dihydroterpineol, and the alkanediol is 6 or more and 8 or less: 0.5 or more and 2 or less: 0.5 or more and 2 or less.
7. The conductive paste of claim 1, wherein the alkanediol is 2-ethyl-1,3-hexanediol.
8. The conductive paste of claim 1 , wherein the organic solvent further comprises mineral spirits.
9. 9. The conductive paste according to claim 8, wherein the mass ratio of the dihydroterpineol acetate, the dihydroterpineol, the mineral spirits and the alkanediol is 3 or more and 4 or less: 0.5 or more and 2 or less: 4 or more and 6 or less: 0.5 or more and 1 or less.
10. The conductive paste according to claim 1 , wherein the binder resin comprises ethyl cellulose.
11. The conductive paste according to claim 10, wherein the binder resin further contains, in addition to the ethyl cellulose, at least one resin selected from the group consisting of methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, nitrocellulose, and polyvinyl butyral.
12. a mass ratio of the sum of the polyalkylene glycol derivative and the polyalkylene glycol to the conductive powder is 0.01 to 4:100, The conductive paste according to claim 1 , wherein the conductive powder content is 35% by mass or more and 65% by mass or less.
13. The conductive paste according to claim 1 , wherein the number average particle size of the conductive powder is 30 nm or more and 100 nm or less.
14. An electronic component formed by using the conductive paste according to claim 1.
15. The laminate has at least a dielectric layer and an internal electrode layer stacked thereon, A multilayer ceramic capacitor, wherein the internal electrode layers are formed using the conductive paste according to claim 1 .
Citation Information
Patent Citations
Silver oxide slurry, and conductive paste and method for producing the same
JP2017084588A
Conductive paste and method for manufacturing substrate having conductive pattern
JP2018107089A
Conductive paste
JP2018168238A
Conductive paste and method for manufacturing multilayer ceramic electronic components using the same
JP2976268B2
Conductive paste composition
WO2014073530A1