Mortal or concrete molding, and laminated structure body with the molding, and manufacturing method thereof

The embedded fiber reinforcing materials in mortar or concrete molded bodies address the challenge of producing thin, complex GRC shapes by ensuring strength and formability through a sequential deposition and curing method, allowing for thinner, reinforced structures.

JP2024146856APending Publication Date: 2024-10-15ASAHI BUILDING WALL
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024050991
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing methods for manufacturing glass fiber reinforced cement (GRC) molded bodies struggle to produce thin, complex shapes, particularly when using the direct spray method, and there is a need for thinner plate-shaped molded objects without compromising strength or design complexity.

Method used

A molded article made of mortar or concrete with embedded first and second fiber reinforcing materials in a sheet shape, separated by a spacer, allowing for a thickness of 5 mm to 20 mm, and a manufacturing method involving sequential deposition and curing steps to maintain reinforcement while achieving thin plate-like portions.

Benefits of technology

The solution enables the production of thin, reinforced mortar or concrete molded bodies with improved formability for complex shapes, maintaining strength and design integrity by embedding fiber reinforcing materials apart in the thickness direction, reducing thickness without increasing weight significantly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146856000001_ABST
    Figure 2024146856000001_ABST
Patent Text Reader

Abstract

To provide a mortar or a concrete molding which can be formed with a thin product thickness.SOLUTION: A molding 1 made of mortar or concrete includes a plate-shaped part 10. In the plate-shaped part 10, a first fiber reinforcement material 110, formed in a sheet shape, and a second fiber reinforcement material 120, formed in a sheet shape, are embedded with separation in the thickness direction, and the thickness t' of the plate-shaped part 10 is 5 mm or more and 20 mm or less. By providing the first fiber reinforcement material 110 and the second fiber reinforcement material 120 in the mortar or concrete with separation from each other in the thickness direction, the thickness t' of the plate-shaped part 10 can be made thin. The plate-shaped part 10 is made of, for example, fiber-reinforcement mortar or fiber-reinforcement concrete containing a reinforcement fiber. The reinforcement fiber is preferably made by bundling alkali-resistant glass fibers containing 16% or more of zirconia. Furthermore, by incorporating the fiber, the thickness t' can be made even thinner.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a mortar or concrete molded article, a laminated structure including the molded article, and methods for producing the same. [Background technology]

[0002] 2. Description of the Related Art Glass fiber reinforced cement molded bodies (hereinafter referred to as GRC molded bodies) have been used in the fields of construction and civil engineering. GRC consists of mortar or concrete reinforced with alkali-resistant glass fiber containing 16% or more zirconia. The direct spray (DS) method and the premix (PM) method are the two main methods known for forming GRC.

[0003] In the DS method, roving made of bundles of alkali-resistant glass fibers is cut into lengths of, for example, 20 mm to 40 mm using a chopper in a spray gun, and then sprayed onto a formwork together with mortar or ready-mixed concrete discharged from a pump to form a compact.

[0004] On the other hand, in the PM method, alkali-resistant glass fibers cut to a length of 5 mm to 20 mm in advance are mixed with mortar or ready-mixed concrete in a mixer and poured into a formwork for molding (Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-262713 A Summary of the Invention [Problem to be solved by the invention]

[0006] Meanwhile, GRC molded bodies produced by the PM method, in which alkali-resistant glass fibers are aligned in three dimensions, have a thickness of 50 mm or more and 100 mm or less, and are used to manufacture large, plate-shaped molded bodies. Compared to the PM method, the DS method allows for thinner thicknesses, for example 20mm to 50mm, because the alkali-resistant glass fibers are arranged two-dimensionally in random directions. However, when manufacturing molded bodies with complex shapes, it may not be possible to insert the spray gun used in the DS method into a mold and spray mortar containing glass fibers, so other molding methods are required.

[0007] It is desirable to form a molded body having a complex shape thinner, and even in the case of a plate-shaped molded body, it is desirable to make the thickness thin enough that there are no problems as a product. It is also desirable to make the thickness thin for a molded body made of mortar or concrete that does not contain reinforcing fibers such as glass fibers.

[0008] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a mortar or concrete molded body, a laminated structure including the molded body, and methods for manufacturing the same. [Means for solving the problem]

[0009] The present invention is a mortar or concrete molded body having a plate-shaped portion, wherein a first fiber reinforcing material formed in a sheet shape and a second fiber reinforcing material also formed in a sheet shape are embedded in the plate-shaped portion at a distance in the thickness direction, and further wherein the thickness of the plate-shaped portion is 5 mm or more and 20 mm or less.

[0010] In the present invention, the first fiber reinforcing material and the second fiber reinforcing material are embedded at a distance in the thickness direction to provide reinforcement, and the thickness of the plate-like portion can be reduced to 5 mm or more and 20 mm or less.

[0011] The mortar or concrete molded body of the present invention is preferably constructed such that at least a first surface side of the plate-shaped portion containing the first fiber reinforcement material, and / or a second surface side of the plate-shaped portion located opposite the first surface and further containing the second fiber reinforcement material, is made of fiber-mixed mortar or fiber-reinforced concrete having reinforcing fibers mixed in.

[0012] Mortar and concrete can be reinforced by mixing reinforcing fibers into them.

[0013] The mortar or concrete molded article of the present invention preferably contains chopped strands made by bundling alkali-resistant glass fibers as the reinforcing fibers.

[0014] By using the alkali-resistant chopped strands, high strength can be suitably maintained.

[0015] The mortar or concrete molded body of the present invention may include a plurality of the plate-shaped parts. In this case, it is preferable that the plate-shaped parts include a connection part connecting the plate-shaped parts, and the first fiber reinforcement of one plate-shaped part and the second fiber reinforcement of the other plate-shaped part are overlapped at the connection part.

[0016] At the connection portions connecting the plate-shaped portions, the first fiber reinforcement materials of one plate-shaped portion and the other plate-shaped portion, or the second fiber reinforcement materials of one plate-shaped portion and the other plate-shaped portion, are overlapped, thereby maintaining strength.

[0017] The present invention is a method for manufacturing a mortar or concrete molded body having a plate-shaped portion in which a first fiber reinforcing material formed in a sheet shape and a second fiber reinforcing material formed in a sheet shape are embedded at a distance in the thickness direction, the method comprising a plate forming step of forming the plate-shaped portion, a depositing step of depositing a first surface side material for forming a first surface side of the plate-shaped portion, an intermediate material for forming a middle portion, and a second surface side material for forming a second surface side located opposite to the first surface of the plate-shaped portion, in that order on a formwork or a skeleton, and a depositing step of depositing the first surface side material, the intermediate material, and the second surface side material deposited on the formwork or the skeleton. and a curing process for curing the material, wherein the first surface side material is made of the mortar or the ready-mixed concrete having the first fiber reinforcement material embedded therein, the intermediate material is made of the mortar or the ready-mixed concrete having a spacer embedded therein, and the second surface side material is made of the mortar or the ready-mixed concrete having the second fiber reinforcement material embedded therein, and during the curing process, the spacers keep the first fiber reinforcement material and the second fiber reinforcement material separated in the thickness direction within the mortar or the ready-mixed concrete of the formwork or main body.

[0018] In the manufacturing method of the present invention, by maintaining the distance between the first fiber reinforcement material and the second fiber reinforcement material with a spacer during curing, the first fiber reinforcement material and the second fiber reinforcement material can be embedded at a distance in the thickness direction, thereby making it possible to form the plate-shaped portion with a thin thickness. In the present invention, by embedding the first fiber reinforcement in mortar or ready-mix concrete on the first surface side, it is possible to prevent the first fiber reinforcement from being exposed in the molded state. Also, by embedding the second fiber reinforcement in mortar or ready-mix concrete on the second surface side, it is possible to prevent the second fiber reinforcement from being exposed in the molded state.

[0019] In the method for manufacturing a molded body of the present invention, the depositing step preferably comprises a first depositing step of placing the first surface side material into the formwork or main body, a second depositing step of depositing the intermediate material on the first surface side material, and a third depositing step of depositing the second surface side material on the intermediate material, and the first depositing step comprises a first manual laying step of manually laying the mortar or the ready-mixed concrete, which serves as a base for placing the first fiber reinforcement material, onto the formwork or main body, a second manual laying step of manually laying the first fiber reinforcement material onto the mortar or the ready-mixed concrete in the formwork or on the main body, and a third manual laying step of manually laying the mortar or the ready-mixed concrete on the first fiber reinforcement material after the second manual laying step to cover the first fiber reinforcement material with the mortar or the ready-mixed concrete. The second stacking process also includes a fourth manual loading process of manually stacking the spacer on the first surface side material, and a fifth manual loading process of manually stacking the mortar or the ready-mixed concrete on the spacer after the fourth manual loading process to cover the spacer with the mortar or the ready-mixed concrete. The third stacking process further includes a sixth manual laying process of manually laying the second fiber reinforcement material on the intermediate material, and a seventh manual laying process of manually laying the mortar or the ready-mixed concrete on the second fiber reinforcement material after the sixth manual laying process, thereby covering the second fiber reinforcement material with the mortar or the ready-mixed concrete. The plate-shaped parts are formed using the hand lay-up method, in which mortar or ready mixed concrete, the first fiber reinforcement, spacers, and the second fiber reinforcement are manually laid onto a formwork or framework, making it possible to form complex shapes, for example, those with multiple plate-shaped parts that cannot be reached by the spray gun of the DS method.

[0020] The manufacturing method of a mortar or concrete molded body of the present invention is preferably characterized in that the mortar or ready-mixed concrete of the first surface side material, and / or the mortar or ready-mixed concrete of the second surface side material, is a fiber-mixed mortar or fiber-mixed ready-mixed concrete containing reinforcing fibers.

[0021] By mixing reinforcing fibers, mortar or concrete can be reinforced, which can further prevent cracks from occurring on the first and second surfaces.

[0022] The laminated structure of the present invention comprises a base made of mortar or concrete, a foam laminated to the base, and a molded body made of mortar or concrete laminated to the foam and having a plate-shaped portion, wherein the plate-shaped portion has a first fiber reinforcing material formed in a sheet shape and a second fiber reinforcing material formed in a sheet shape embedded in the plate-shaped portion at a distance in the thickness direction, and has a thickness of 5 mm or more and 40 mm or less.

[0023] The foam may be, for example, a spray foam or a slab of polystyrene foam, polyurethane foam, polyethylene foam, or phenolic foam.

[0024] In the present invention, the first fiber reinforcing material and the second fiber reinforcing material are embedded at a distance in the thickness direction to provide reinforcement, and the thickness of the plate-like portion can be reduced to 5 mm or more and 40 mm or less.

[0025] The laminated structure of the present invention preferably has a plate-shaped portion made of fiber-mixed mortar or fiber-reinforced concrete mixed with the reinforcing fibers (short fibers), and it is desirable to use, as the reinforcing fibers (short fibers), chopped strands made by bundling alkali-resistant glass fibers, for example.

[0026] The laminated structure of the present invention is preferably such that the spray foam is a spray foam formed in an uneven shape with uneven thickness on the molded body side, and the plate-shaped portion comprises a main body in which the first fiber reinforcing material and the second fiber reinforcing material are embedded at a distance in the thickness direction and having a thickness of 5 mm to 40 mm, and a plurality of partial thickening portions formed on the spray foam side of the main body and increasing in thickness, and is formed in an uneven shape following the shape of the spray foam.

[0027] The spray foam may be polyurethane foam (e.g., spray rigid polyurethane foam for building insulation JISA9526:2017).

[0028] The molded body has a plurality of partially thickened portions that conform to the shape of the sprayed foam, so that the sprayed foam is hung on the molded body and stably positioned between the base and the molded body. Even if the molded body has a complex shape, the weight of the molded body increases only by the amount of the partially thickened portions that conform to the shape of the sprayed foam, so a significant increase in weight can be prevented.

[0029] The laminated structure of the present invention preferably comprises a finishing layer laminated on the plate-shaped portion of the molded body and made of a material different from the molded body, an anchor bolt is embedded in the thickness direction from the base into the plate-shaped portion or into the finishing layer, and a pressing member is attached to the end of the anchor bolt on the finishing layer side.

[0030] The pressing member is, for example, a nut. The formed body can be fixed to the base by the anchor bolt and the pressing member. This makes it possible to prevent the formed body from peeling off.

[0031] The finishing layer is made of a material different from that of the plate-shaped portion, such as mortar containing no reinforcing fibers, polymer cement mortar, or paint made of synthetic resin. The finishing layer may be a single layer of thickly applied mortar layer for repair finishing, or a single layer of synthetic resin paint, or may have a laminated structure of a mortar layer containing no reinforcing fibers as a base and a synthetic resin coating layer coating the mortar layer. The finishing layer can improve the appearance of the laminated structure.

[0032] The present invention is a method for manufacturing a laminated structure including a mortar or concrete molded body having a plate-shaped portion in which a first fiber reinforcement material formed in a sheet shape and a second fiber reinforcement material formed in a sheet shape are embedded at a distance in the thickness direction, the method comprising: a foam forming step of spraying a foam material onto a base made of mortar or concrete to form a sprayed foam having an uneven thickness and a plate forming step of molding the plate-shaped portion laminated onto the sprayed foam. The plate forming step comprises a depositing step of depositing, on the sprayed foam, a first surface side material for forming the sprayed foam side of the plate-shaped portion, an intermediate material for forming a middle portion, and a second surface side material for forming the side opposite to the sprayed foam side of the plate-shaped portion, in that order; and a curing step of curing the first surface side material, the intermediate material, and the second surface side material deposited on the sprayed foam, the first surface side material being made of the mortar or the ready mixed concrete in which the first fiber reinforcement material is embedded, and the intermediate material being made of a material having a spacer embedded therein. the first surface side material is made of the mortar or the ready-mixed concrete with the second fiber reinforcement material embedded therein, the depositing process is a process in which the mortar or the ready-mixed concrete of the first surface side material is applied to the spray foam to form a smooth surface, and in the curing process, the spacer keeps the first fiber reinforcement material and the second fiber reinforcement material separated in the thickness direction within the mortar or the ready-mixed concrete, and the base is a formwork or a structure.

[0033] The applied first surface material is leveled, and the intermediate material and second surface material are piled up in order, and the thickness is increased only in the areas corresponding to the uneven sprayed foam, so that the molded body can be prevented from increasing significantly in weight. Also, the hand layup method allows molded bodies of complex shapes to be molded on the sprayed foam. Effect of the Invention

[0034] According to the molded article of the present invention, the plate-shaped portion can be molded thin. Furthermore, by embedding the first fiber reinforcing material and the second fiber reinforcing material on the first surface side and the second surface side, the designed shape and strength of the first surface and the second surface can be favorably maintained. According to the method for producing a molded body of the present invention, the first fiber reinforcement and the second fiber reinforcement are fixed with a spacer and cured, so that the first fiber reinforcement and the second fiber reinforcement can be embedded apart in the thickness direction. This allows a thin plate-like part to be formed with suitable strength against bending, etc. In addition, in the DS method, a molded body having a complex shape with multiple plate-like parts may not be produced because the spray gun cannot enter the mold frame, but in the production method of the present invention, each plate-like part is molded in a plate molding process, so that a molded body having a complex shape can be easily produced. This allows the moldability of the molded body to be emphasized. [Brief description of the drawings]

[0035] [Figure 1] FIG. 2 is a partial cross-sectional view of a molded article according to an embodiment of the present invention. [Diagram 2] 2A to 2C are diagrams for explaining a method for manufacturing the plate-shaped portion in FIG. [Diagram 3] 3(a) to 3(g) are diagrams for explaining each step of the manufacturing method shown in FIG. 2. [Figure 4] FIG. 3 is a diagram for explaining the steps of the manufacturing method shown in FIG. 2. [Diagram 5] 1 is a cross-sectional view of a laminated structure according to an embodiment of the present invention. [Figure 6] 6(a) to 6(f) are diagrams illustrating a method for manufacturing the laminated structure of FIG. [Figure 7] FIG. 2A is a perspective view showing another example of the configuration of the molded body according to the embodiment of the present invention, and FIG. 2B is a cross-sectional view of a connection part of the molded body of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] Hereinafter, a molded article according to an embodiment of the present invention will be described with reference to the drawings. As shown in FIG. 1, the molded body 1 is formed in a flat plate shape, and furthermore, the molded body 1 is composed of one plate-shaped portion 10. The plate-shaped portion 10 is composed of mortar or concrete, and is preferably composed of fiber-mixed mortar or fiber-reinforced concrete mixed with reinforcing fibers. The reinforcing fibers are, for example, glass fibers, carbon fibers, or steel fibers, and preferably chopped strands in which multiple fibers are bundled together are used. The chopped strands are, for example, rovings cut to a predetermined length such as 6 mm, 13 mm, or 19 mm, and are preferably composed of fibers (JISR3410) made of alkali-resistant AR glass containing 16% or more zirconia. The following explanation will be given on the assumption that the plate-shaped portion 10 is made of mortar mixed with chopped strands of glass fibers, which are fiber bundles made of alkali-resistant AR glass containing 16% or more zirconia and cut to a specified length, i.e., glass fiber reinforced cement (hereinafter referred to as GRC); however, the same applies to mortar in the case of concrete.

[0037] Furthermore, as shown in Figure 1, the plate-like portion 10 is formed in a plate shape having a first surface 11 and a second surface 12 located opposite the first surface 11, and the plate-like portion 10 further includes first fiber reinforcing material 110 and second fiber reinforcing material 120 formed in a lattice pattern and embedded therein at a distance from each other in the thickness direction.

[0038] (First fiber reinforcement 110 and second fiber reinforcement 120) The first fiber reinforcement 110 and the second fiber reinforcement 120 are formed as continuous fiber reinforcement by weaving or knitting fibers. The fibers are made of yarns or rovings of glass fibers, carbon fibers, aramid fibers, etc., and preferably, a lattice-shaped sheet made of woven yarns or rovings of alkaline-resistant AR glass fibers containing 16% or more of zirconia is used. The yarns are made by bundling monofilaments with a binder, and the rovings are made by bundling yarns, and the chopped strands are usually made by chopping rovings to a predetermined length. The first fiber reinforcement 110 and the second fiber reinforcement 120 are formed as a sheet having a plurality of openings 111, 121 by plain weaving or the like, as shown in Figure 4 described below. The size of the openings 111, 121 is not limited, but they are formed, for example, to a size of 5 mm square or 10 mm square, so that at least a portion of the mortar aggregate, coarse aggregate for ready-mixed concrete, and reinforcing fibers can penetrate and partially penetrate the first fiber reinforcement 110 and the second fiber reinforcement 120 during the production of the plate-shaped portion 10, and preferably the entire openings can pass through. Mortar fills the openings 111, 121 of the first fiber reinforcement 110 and the second fiber reinforcement 120. Chopped strands in the mortar also fill the openings 111, 121. The first fiber reinforcement material 110 may be configured by stacking a plurality of sheets. In this case, the first fiber reinforcement material 110 arranged on the first surface 11 side and the first fiber reinforcement material 110 arranged on the second surface 12 side may be stacked with those having the same size of opening 111 or those having different sizes of opening 111. The second fiber reinforcement material 120 may be configured by stacking multiple sheets, similar to the first fiber reinforcement material 110. When stacking multiple second fiber reinforcement materials 120, sheets with the same size of opening 121 may be stacked together, or sheets with different sizes may be stacked together, and mortar or chopped strands may be inserted into each opening 121 of the second fiber reinforcement material 120. The following description will be given on the assumption that the plate-shaped portion 10 has one first fiber reinforcement material 110 embedded on the first surface 11 side and one second fiber reinforcement material 120 embedded on the second surface 12 side. Examples of the first fiber reinforcement material 110 and the second fiber reinforcement material 120 that can be used include an alkali-resistant glass fiber net (ARG fiber net) manufactured by Nippon Electric Glass Co., Ltd., with openings formed to a size of 5 mm square or 10 mm square, and a carbon fiber mesh roll manufactured by Yoshino Co., Ltd., with openings formed to a size of 5 mm square. In addition, although its alkali resistance is not particularly high, it can be considered to be used as the first fiber reinforcement 110 and the second fiber reinforcement 120 formed in a lattice pattern with 5 mm square openings made of basalt fiber (basalt fiber) developed for civil engineering use. Furthermore, the first fiber reinforcement 110 and the second fiber reinforcement 120 may be a so-called continuous strand mat or chopped strand mat having a thin thickness. The fibers constituting the chopped strand mat and the continuous strand mat are, for example, yarns, rovings, or chopped strands made by bundling glass fibers (JISK7010:E glass) containing 0.8% or less alkali (Na2O, K2O) or alkali-resistant AR glass fibers containing 16% or more zirconia. The chopped strand mat may be made of a plurality of chopped strands oriented two-dimensionally and held in a sheet shape by a binder, and the continuous strand mat may be made of continuous yarns or rovings stacked in the thickness direction and held in a sheet shape by a binder. The first fiber reinforcement 110 and the second fiber reinforcement 120 are both formed to allow mortar aggregate, coarse aggregate for ready-mixed concrete, and reinforcing fibers to pass through when the plate-shaped portion 10 is manufactured.

[0039] The plate-shaped portion 10 has a thickness t1 (first covering portion) from the first surface 11 to the first fiber reinforcement 110 of, for example, 1 mm or more and 3 mm or less. The plate-like portion 10 has a thickness t2 (second covering portion) from the second surface 12 to the second fiber reinforcement 120 of, for example, 1 mm or more and 3 mm or less. Furthermore, the plate-shaped portion 10 has a thickness t3 from the first fiber reinforcement 110 to the second fiber reinforcement 120 of, for example, 3 mm or more and 18 mm or less. The thickness t3 does not include the thicknesses of the first fiber reinforcement 110 and the second fiber reinforcement 120. Hereinafter, the portion disposed between the first fiber reinforcement 110 and the second fiber reinforcement 120 in the thickness direction from the first surface 11 to the second surface 12 of the plate-shaped portion 10 will be referred to as the intermediate portion 130. The plate-like portion 10 has a thickness t' from the first surface 11 to the second surface 12 of, for example, 5 mm to 20 mm. If it is thinner than 5 mm, the strength of the product will be weak, and if it is thicker than 20 mm, the weight will increase, which is not preferable. Further, when the plate-like portion 10 is viewed from the first surface 11 side, its contour shape is not limited, but is formed, for example, in a long and narrow rectangular shape.

[0040] The molded body 1 consisting of the plate-like portion 10 thus configured is provided in a structure and used as an interior or exterior fitting, etc. When the molded body 1 is in use, the first surface 11 side of the plate-like portion 10 is disposed so as to face the interior of the room, and the second surface 12 side is disposed so as to face a structural part. The first surface 11, which is disposed on the exposed side when the molded body 1 is in use, has a shape designed for aesthetic purposes, for example. In the illustrated example, the first surface 11 of the plate-like portion 10 is shown flat, but this is not limited thereto, and for example, recessed or protruding portions may be provided. The first surface 11 may also be formed as a surface that is curved outwardly in a concave or convex manner as a whole. Even when the first surface 11 is a curved surface in this way, the second surface 12 is also formed as a curved surface that is curved in the same manner as the first surface 11 as a whole. In these cases, the first fiber reinforcement 110 on the first surface 11 side and the second fiber reinforcement 120 on the second surface 12 side are both embedded in the mortar and are not exposed to the outside. Although not shown in the drawings, the first surface 11 and the second surface 12 may be painted or the like.

[0041] (Manufacturing method) The manufacturing method of the molded body 1 includes a plate forming step of forming the plate-like portion 10. As shown in Figure 2, the plate molding process includes a depositing process in which a first surface side material M1 for molding the first surface 11 side of the plate-shaped portion 10, an intermediate material M2 for molding the middle portion 130 arranged between the first fiber reinforcement material 110 and the second fiber reinforcement material 120 of the plate-shaped portion 10, and a second surface side material M3 for molding the second surface 12 side located opposite the first surface 11 of the plate-shaped portion 10 are deposited in sequence onto a formwork 20, and a curing process in which the first surface side material M1, intermediate material M2, and second surface side material M3 deposited onto the formwork 20 are cured. The depositing process includes a first depositing process in which a first surface side material M1 for forming the first surface 11 side of the plate-shaped portion 10, which contains unhardened mortar mixed with cement, water, aggregate, etc. (hereinafter, the unhardened mortar will be referred to as mortar material 30) and a first fiber reinforcement material 110, is placed in a formwork; a second depositing process in which an intermediate material M2 for forming the intermediate portion 130 disposed between the first fiber reinforcement material 110 and the second fiber reinforcement material 120 of the plate-shaped portion 10, which contains a spacer 140 and the mortar material 30, is deposited on the first surface side material M1; and a third depositing process in which a second surface side material M3 for forming the second surface 12 side located opposite the first surface 11 of the plate-shaped portion 10, which contains the second fiber reinforcement material 120 and the mortar material 30, is deposited on the intermediate material M2.

[0042] A. First deposition process The first depositing process includes a first manual laying process of manually laying mortar material 30, which serves as a base for placing the first fiber reinforcement material 110, on the bottom 21 of the formwork 20 before the first fiber reinforcement material 110 is placed into the formwork 20, a second manual laying process of manually laying the first fiber reinforcement material 110 on top of the mortar material 30 in the formwork 20, and a third manual laying process of manually laying the mortar material 30 on the first fiber reinforcement material 110 after the second manual laying process, to cover the first fiber reinforcement material 110 with the mortar material 30.

[0043] (First manual loading process) In the first manual loading step, as shown in Fig. 3(a), mortar material 30 is poured from a bucket or the like into formwork 20. Mortar material 30 is made by mixing cement, water, aggregate, and alkali-resistant chopped strands. If it is for concrete, coarse aggregate is also mixed to make ready-mix concrete. The cement that can be used includes ordinary Portland cement, early strength Portland cement, extra early strength Portland cement, moderate heat Portland cement, low heat Portland cement, sulfate resistant Portland cement, ordinary Portland cement (low alkali type), early strength Portland cement (low alkali type), extra early strength Portland cement (low alkali type) as specified in JIS R 5210. Low alkali type cements other than JIS R 5210 may also be used. In addition to silica sand, the aggregate may include slag, fly ash, dolomite, etc. The aggregate for mortar and the coarse aggregate for ready-mix concrete are preferably of a size that allows them to pass through the openings 111, 121 of the first fiber reinforcement 110 and the openings 121 of the second fiber reinforcement 120 so as to suitably fill the openings 111, 121. The mortar material 30 may also contain silica fume as an additive, a naphthalene sulfonate-formaldehyde high condensate salt-based or polycarboxylic acid ether-based compound-based water reducing agent, and an alkylene oxide compound of a lower alcohol as a shrinkage reducing agent. The following description will be given on the assumption that the mortar material 30 is made by mixing ordinary Portland cement, silica sand, additives, a water reducing agent, a shrinkage reducing agent, chopped strands (AR glass), and water. After the mortar material 30 is poured into the formwork 20, the surface of the mortar material 30 is smoothed and further spread with, for example, a trowel to cover the bottom 21. The thickness of the mortar material 30 serving as the base is, for example, 1 mm to 3 mm. By pouring the mortar material 30 into the formwork 20 before placing the first fiber reinforcement 110 in the formwork 20, the first fiber reinforcement 110 is prevented from coming close to the formwork surface, and further, in a process described later, the mortar material 30 can be permeated into the openings 111 of the first fiber reinforcement 110 while the entire first fiber reinforcement 110 is buried in the mortar material 30. The formwork 20 has a bottom 21 for forming the first surface 11 of the plate-like portion 10, and although not shown, the bottom 21 is configured to have a shape that resembles the first surface 11 of the plate-like portion 10, and has, for example, recessed portions, portions that protrude into the formwork, etc. This bottom 21 forms the first surface 11 of the plate-like portion 10 into an aesthetically designed shape.

[0044] (Second manual laying process) 3(b), in the second manual laying step, a first fiber reinforcement material 110 is placed on the mortar material 30 in the formwork 20. The second manual laying step is performed before the mortar material 30 placed in the formwork 20 in the first manual laying step exhibits the strength and durability of mortar.

[0045] (Third manual loading process) 3(c), the third manual laying step involves applying the mortar material 30 to the first fiber reinforcement 110 and embedding the first fiber reinforcement 110 in the mortar material 30. The third manual laying step is performed before the mortar material 30 placed in the formwork 20 in the first manual laying step develops the strength and durability of mortar. In this manner, the first surface side material M1 (the mortar material 30 and the first fiber reinforcing material 110) for forming the first surface 11 side of the plate-like portion 10 is piled up on the bottom 21 of the formwork 20.

[0046] B.Second deposition process The second depositing process includes a fourth manual laying process of manually laying a spacer 140 on the first fiber reinforcement material 120 to which the mortar material 30 has been applied in the third manual laying process, and a fifth manual laying process of manually laying the mortar material 30 on the spacer 140 after the fourth manual laying process to cover the spacer 140 with the mortar material 30.

[0047] (Fourth manual laying process) 3(d), in the fourth manual laying step, a spacer 140 is placed on the first fiber reinforcement material 110 to which the mortar material 30 has been applied. The fourth manual laying step is performed before the mortar material 30 placed in the formwork 20 in the first manual laying step and the third manual laying step develops the strength and durability of mortar.

[0048] (Spacer 140) The spacer 140 is intended to hold the first fiber reinforcement material 110 and the second fiber reinforcement material 120 at a predetermined distance in the thickness direction of the plate-like portion 10 to be molded during the process of molding the plate-like portion 10. The spacer 140 is configured to include at least a plurality of straight holes that extend linearly through the thickness direction, continuous holes that are not linear but are connected while bending from one surface to the opposite surface, non-through holes that are connected linearly or while bending from one surface or the other surface to the middle of the thickness direction, and holes that extend to the opposite surface, and these holes (straight holes, continuous holes, non-through holes) form voids that are impregnated with the mortar material. In addition, the spacer 140 is preferably one that allows the mortar material 30, especially the aggregate, to pass from one surface to the other surface so that the voids are suitably filled. For example, a sheet of glass fiber or hollow fiber can be used as the spacer 140. The sheet is, for example, a continuous strand mat or a chopped strand mat, and the fibers constituting these are, for example, glass fibers (JISK7010: E glass) containing 0.8% or less of alkali (Na2O, K2O) or alkali-resistant AR glass fibers containing 16% or more of zirconia, bundled yarns, rovings, or chopped strands. The continuous strand mat is composed of continuous yarns or rovings stacked in the thickness direction and held in a sheet shape by a binder, and the chopped strand mat is composed of multiple chopped strands oriented two-dimensionally and held in a sheet shape by a binder. These spacers 140 are impregnated with the mortar material 30 when the plate-shaped part 10 is formed, and are configured so that the mortar material 30 can pass from one side to the other side. Any material through which the mortar material 30 can pass, and nonwoven fabric may be used. Additionally, the spacer 140 may be a thermoplastic three-dimensional network fiber structure (JISL4500) that is impregnated with the mortar material 30 and through which the mortar material 30 can pass from one side to the other. The following description will be given taking as an example a case where a continuous strand mat made of E-glass yarn or roving is used for the spacer 140. Although the thickness t4 of the spacer 140 is not limited, it is preferable to use one having a dimension in the thickness direction larger than that of the first fiber reinforcement 110 and the second fiber reinforcement 120, for example, 3 mm or more and 18 mm or less, which corresponds to the thickness t3 of the intermediate layer. If the sheet is thin, multiple sheets may be stacked to achieve a thickness equivalent to t3.

[0049] (Fifth manual loading process) In the fifth manual laying step, the mortar material 30 is applied to the spacer 140, and the spacer 140 is embedded in the mortar material 30, as shown in Fig. 3(e). In the fifth manual laying step, the mortar material 30 is impregnated into the continuous strand mat (spacer 140) to fill the voids. The fifth manual laying step is performed before the mortar material 30 placed in the formwork 20 in the first and third manual laying steps develops the strength and durability of mortar. In this manner, the intermediate material M2 (the mortar material 30 and the spacers 140) for forming the intermediate portion 130 of the plate-shaped portion 10 is deposited on the first surface side material M1.

[0050] C. Third deposition process The third stacking process includes a sixth manual laying process in which the second fiber reinforcement material 120 is manually laid on top of the spacer 140 (intermediate material) to which the mortar material 30 has been applied in the fifth manual laying process, and a seventh manual laying process in which, after the sixth manual laying process, the mortar material 30 is manually laid on the second fiber reinforcement material 120 to cover the second fiber reinforcement material 120 with the mortar material 30.

[0051] (Sixth manual construction process) 3(f), the sixth manual laying step involves placing the second fiber reinforcement material 120 on the spacer 140 to which the mortar material 30 has been applied. The sixth manual laying step is performed before the mortar material 30 placed in the formwork 20 in the first manual laying step, the third manual laying step, and the fifth manual laying step exhibits the strength and durability of mortar.

[0052] (Seventh manual loading process) In the seventh manual laying step, the mortar material 30 is applied to the second fiber reinforcement 120, and the second fiber reinforcement 120 is embedded in the mortar material 30 as shown in Fig. 3(g). The surface of the mortar material 30 may be finished by smoothing it with a trowel or the like. The seventh manual laying step is performed before the mortar material 30 placed in the formwork 20 in the first manual laying step, the third manual laying step, and the fifth manual laying step exhibits the strength and durability of mortar. In this manner, the second surface side material M3 (the mortar material 30 and the second fiber reinforcing material 120) for forming the second surface side 12 of the plate-shaped portion 10 is deposited on the intermediate material M2.

[0053] D.Curing process In the curing step, the mortar material 30 is solidified in a state where the first fiber reinforcement 110, the spacer 140, and the second fiber reinforcement 120 are embedded in the mortar material 30 of the formwork 20 to form the plate-like portion 10 (molded body 1) having strength and durability as mortar. As shown in the exploded perspective view of the molding material in Fig. 4, the spacer 140 is disposed between the first fiber reinforcement 110 and the second fiber reinforcement 120, so that the second fiber reinforcement 120 is supported by the spacer 140 and held at a position separated from the first fiber reinforcement 110 in the thickness direction, and curing is performed in that state. After the curing process, the plate-like portion 10 is formed, and in the solidified mortar, the first fiber reinforcement 110 and the second fiber reinforcement 120 are arranged apart from each other in the thickness direction. In the mortar that has developed strength and durability, a spacer 140 is arranged between the first fiber reinforcement 110 and the second fiber reinforcement 120.

[0054] The plate-like portion 10 thus formed is attached to a structural part so that the first surface 11 faces the interior of the room, and thus provides an attractive appearance.

[0055] In the plate-like portion 10 of the molded product 1 according to the embodiment of the present invention, the first fiber reinforcing material 110 and the second fiber reinforcing material 120 are provided in the mortar at a distance from each other in the thickness direction, thereby suitably reinforcing the plate-like portion 10 and reducing the thickness t' of the plate-like portion 10. This allows the weight to be reduced and the handling to be easier than when the plate-like portion 10 is manufactured by the conventional DS method.

[0056] By mixing the chopped strands in the mortar, cracks on the first surface 11 side can be further prevented. In addition, the second surface 12 side is also made of chopped strands, which can prevent cracks.

[0057] (Laminated structure) The molded body according to the embodiment of the present invention may be provided as a part of a structure in which a plurality of materials are laminated. The laminated structure 2 shown in Fig. 5 includes a base 40 made of mortar or concrete, a spray foam 50 laminated on the base 40, a molded body 3 laminated on the spray foam 50, and a finishing layer 60 laminated on a plate-shaped portion 100 of the molded body 3. The same components as those in the above embodiment are given the same reference numerals and their description will be omitted.

[0058] The base 40 is a formwork or a framework. The formwork is used when molding the materials constituting the spray foam 50 and the molded body 3, and further, even after molding is completed, the formwork remains integrated with the molded body 3 and the spray foam 50, and functions as a part that provides strength to the laminated structure 2. The base 40 may include reinforcing materials such as reinforcing fibers and reinforcing bars.

[0059] The spray foam 50 is, for example, polyurethane foam (for example, spray rigid polyurethane foam for thermal insulation of buildings JISA9526:2017), and the surface opposite the base 40 is unevenly formed due to uneven thickness. Instead of the spray foam 50, a plate-shaped material such as polystyrene foam, polyurethane foam, polyethylene foam, or phenol foam can be used as the foam, but the spray foam 50 is more suitable than a plate-shaped material when forming the molded body 3 into a complex shape by the hand lay-up method, such as forming the molded body 3 into a curved surface.

[0060] The molded body 3 comprises a plate-shaped portion 100, which comprises a main body 100A formed with a basic thickness t5 described below, in which a first fiber reinforcement material 110 and a second fiber reinforcement material 120 are arranged in mortar at a distance in the thickness direction, and a plurality of partially thickened portions 100B formed on the spray foam 50 side of the main body 100A and which are thickened.

[0061] In the main body 100A, the thickness of the intermediate portion 130 from the first fiber reinforcement 110 to the second fiber reinforcement 120 is, for example, 3 mm or more and 38 mm or less in order to embed the pressing member 80 described later. In addition, in the main body 100A, the minimum thickness of the first covering portion 150 covering the first fiber reinforcement 110 from the dashed line in Fig. 5 to the first fiber reinforcement 110 is, for example, 1 mm or more and 3 mm or less, and the minimum thickness of the second covering portion 160 covering the second fiber reinforcement 120 from the second surface 102 located opposite to the first covering portion 150 to the second fiber reinforcement 120 is, for example, 1 mm or more and 3 mm or less. Therefore, the thickness t5 of the main body 100A from the dashed line on the spray foam side shown in Fig. 5 to the second surface 102 is formed to be, for example, 5 mm or more and 40 mm or less. Furthermore, when the embedding position of the pressing member 80 is changed to between the first fiber reinforcement 110 and the second fiber reinforcement 120 and is the second covering portion 160, the thickness from the first fiber reinforcement 110 to the second fiber reinforcement 120 is, for example, 3 mm to 18 mm, the thickness of the second covering portion 160 is, for example, 3 mm to 38 mm, and the thickness t5 of the main body 100A is, for example, 5 mm to 40 mm. Note that, when the pressing member 80 is not embedded in the main body 100A, the thickness from the first fiber reinforcement 110 to the second fiber reinforcement 120 may be, for example, 3 mm to 18 mm, the thickness of the second covering portion 160 may be, for example, 1 mm to 3 mm, and the thickness t5 of the main body 100A may be, for example, 5 mm to 20 mm.

[0062] The partial thickening portions 100B are areas where the thickness increases from the first covering portion 150 of the plate-shaped portion 100A toward the base portion 40 and the sprayed foam 50, and the partial thickening portions 100B are formed to come into contact with concave and convex portions of the sprayed foam 50. By providing these partial thickening portions 100B, the first surface 101 of the plate-shaped portion 100 is formed in an uneven shape that follows the shape of the sprayed foam 50.

[0063] The partially thickened portion 100B penetrates deep into the depression of the spray foam 50. For example, the depression 511 below the overhang portion 510 formed in the spray foam 50 shown in Fig. 5 is filled to the very back with fiber-mixed mortar (the partially thickened portion 100B) containing chopped strands (reinforcing fibers).

[0064] The finishing layer 60 is made of a material different from that of the plate-shaped portion 100, such as mortar containing no reinforcing fibers, polymer cement mortar, or paint made of synthetic resin such as urethane. The finishing layer 60 may be a single layer, or may have a laminated structure of a base layer such as mortar and a coating layer of synthetic resin. The thickness of the finishing layer 60 is, for example, 1 mm or more and 10 mm or less. The finishing layer can improve the appearance of the laminated structure 2.

[0065] Furthermore, the laminated structure 2 includes a plurality of anchor bolts 70 standing upright from the base 40 , and pressing members 80 attached to the tips of the anchor bolts 70 for pressing the molded body 3 .

[0066] The anchor bolt 70 is embedded in the thickness direction into the plate-shaped portion 100. The tip of the anchor bolt 70 protrudes further toward the finishing layer 60 than the second fiber reinforcing material 120 of the plate-shaped portion 100, and is covered by the second covering portion 160 of the plate-shaped portion 100.

[0067] The pressing member 80 is provided in the intermediate portion 130 of the plate-like portion 100, and specifically, is disposed between the first fiber reinforcement 110 and the second fiber reinforcement 120 in the thickness direction. The pressing member 80 is composed of, for example, a nut 81 and a washer 82 welded to the nut 81. The pressing member 80 may be configured without the washer 82, or may be configured to use another plate-shaped member welded to the nut 81 instead of the washer 82. The pressing member 80 may also be turned upside down to press the plate-like portion 100 with the washer 82 spreading out like a brim from the nut 81 facing down.

[0068] Although not shown in the drawings, the position of the pressing member 80 may be the second covering portion 160 or the finishing layer 60 instead of the intermediate portion 130. When a part of the pressing member 80 or the tip of the anchor bolt 70 protrudes from the plate-shaped portion 100, the finishing layer 60 is composed of, for example, a thick layer of mortar having a thickness of 10 mm or more that does not contain reinforcing fibers.

[0069] (Method of manufacturing laminated structure 2) The manufacturing method for the laminated structure 2 includes a foam formation process in which a foam material is sprayed onto the base 40 to form a sprayed foam 50 having an uneven thickness and an uneven surface, a plate forming process in which a plate-like portion 100 is formed laminated onto the sprayed foam 50, and a finishing process in which a finishing layer 60 is formed laminated onto the plate-like portion 100.

[0070] 6(a), the foam forming step involves spraying a foaming material such as urethane foam onto the base 40 to form the sprayed foam 50. Also, in the foam forming step, a plurality of anchor bolts 70 are erected from the base 40 and penetrate the sprayed foam 50.

[0071] The plate forming process includes a depositing process in which a first surface side material M1 for forming the first surface 101 side of the plate-shaped portion 100, an intermediate material M2 for forming the intermediate portion 130, and a second surface side material M3 for forming the second coating portion 160 on the second surface 102 side of the plate-shaped portion 100 are deposited in sequence onto the spray foam 50, and a curing process in which the first surface side material M1, intermediate material M2, and second surface side material M3 deposited on the spray foam 50 are cured.

[0072] The first surface side material M1 is the same as the first surface side material M1 used in manufacturing the plate-shaped portion 10, and is made of mortar or ready-mixed concrete with a first fiber reinforcement 110 embedded therein. The intermediate material M2 is the same as the intermediate material M2 used in manufacturing the plate-shaped portion 10, and is made of mortar or ready-mixed concrete with a spacer embedded therein. The second surface side material M3 is the same as the second surface side material M3 used in manufacturing the plate-shaped portion 10, and is made of mortar or ready-mixed concrete with a second fiber reinforcement 120 embedded therein. The following description will be given taking as an example a case where the mortar material 30 used in manufacturing the plate-shaped portion 10 is used as the mortar.

[0073] In the stacking step, first, the first surface side material M1 is stacked on the spray foam 50. As shown in Fig. 6(b), the mortar material 30 is applied to the uneven parts of the spray foam 50 to form a smooth surface. Then, the first fiber reinforcement material 110 is placed on the mortar material 30, and the mortar material 30 is further applied to bury the first fiber reinforcement material 110 in the mortar material 30. The application of the mortar material 30 to the spray foam 50 and the first fiber reinforcement material 110 is performed by hand.

[0074] Next, in the stacking step, the intermediate material M2 is stacked on the smoothed surface of the first surface side material M1. As shown in Fig. 6(c), the pressing member 80 is attached to the anchor bolt 70, and the intermediate material M2 is placed on the mortar material 30 (first surface side material M1) of the spacer 140. Then, as shown in Fig. 6(d), the mortar material 30 is impregnated into the gaps of the spacer 140. The mortar material 30 is also applied to the spacer 140 by hand.

[0075] In the stacking step, the second surface side material M3 is stacked on the intermediate material M2. As shown in Fig. 6(e), the second fiber reinforcement material 120 is placed on the spacer 140, and as shown in Fig. 6(f), the mortar material 30 is applied to bury the second fiber reinforcement material 120 in the mortar material 30. The application of the mortar material 30 to the second fiber reinforcement material 120 is also performed by hand.

[0076] The finishing process can be performed before or after the curing process when the first surface side material M1, the intermediate material M2, and the second surface side material M3 have not yet developed the strength of mortar. When the finishing process is performed before the curing process, a material such as finishing mortar is piled on the second surface side material M3, and curing is performed together with the first surface side material M1, the intermediate material M2, and the second surface side material M3 so that they develop strength. When the finishing process is performed after the curing process, a material such as finishing mortar is applied to the molded body 3, and curing is performed.

[0077] The laminated structure 2 manufactured in this manner can be used as a heat insulating member. If the base is a formwork, the laminated structure 2 can be attached to the structural part of a building with the formwork integrated therein. If the base is the framework of a structural part, the laminated structure 2 can be integrated with the framework and used as an exterior wall for heat insulation.

[0078] In the plate-like portion 100 of the molded body 3, the first fiber reinforcement 110 and the second fiber reinforcement 120 are provided in the mortar at a distance in the thickness direction, thereby suitably reinforcing the plate-like portion 100 and reducing the thickness t5 of the main body 100A of the plate-like portion 100. Furthermore, since the weight of the molded body 3 increases only by the amount of the partially thickened portion 100B that follows the shape of the spray foam 50, a significant increase in the weight of the molded body 3 can be suppressed.

[0079] Furthermore, since the molded body 3 is provided with multiple partially thickened portions 100B that follow the shape of the spray foam 50, the spray foam 50 hangs over the molded body 3 and is stably positioned between the base 40 and the molded body 3. Furthermore, since the partially thickened portions 100B hang over the overhang portions 510, the bonding strength between the spray foam 50 and the molded body 3 can be further increased, and for example, peeling of the molded body 3 from the spray foam 50 can be prevented.

[0080] The molded article of the present invention can be practiced without being limited to the above explanation and illustrated examples.

[0081] The present invention may be configured as a molded body made of mortar or concrete having a plurality of the plate-like portions 10. For example, the molded body 1A shown in Fig. 7(a) has two plate-like portions 10 (one of which is designated by reference numeral 10A and the other by reference numeral 10B in Fig. 7(a)), It is configured in an L-shape. After molding one plate-shaped portion 10A, the other plate-shaped portion 10B is molded so as to be connected to the end portion of one plate-shaped portion 10A while the one plate-shaped portion 10A is held upright, whereby the molded body 1 can be manufactured.

[0082] As shown in Fig. 7(b), the connecting portion 10C connecting the plate-shaped portion 10A and the plate-shaped portion 10B includes a first fiber reinforcement 110 and a second fiber reinforcement 120 arranged in mortar at a distance from the first fiber reinforcement 110 in the thickness direction, similar to the plate-shaped portion 10A and the plate-shaped portion 10B, and the first fiber reinforcement 110 of the adjacent plate-shaped portions 10A and 10B are arranged so as to overlap each other, and the second fiber reinforcement 110 of the adjacent plate-shaped portions 10A and 10B are overlapped each other. In Fig. 7(b), the cross sections of the first fiber reinforcement 110 and the second fiber reinforcement 120 are represented by circles, the cross sections of the first fiber reinforcement 110 and the second fiber reinforcement 120 of the plate-shaped portion 10A are represented by a dashed line, and the cross sections of the first fiber reinforcement 110 and the second fiber reinforcement 120 of the plate-shaped portion 10B are represented by a dashed line. In the connection portion 10C, the overall thickness tc1 may exceed 20 mm, but is preferably set to, for example, 24 mm or less.

[0083] The number of plate-like parts 10 provided on the molded body is not limited to two, and the shape of the molded body is not limited to the above description and illustrated example, and may be a molded body with a complex shape having multiple plate-like parts. When manufacturing such a molded body with a complex shape by the DS method, a situation may occur in which it is not possible to insert a spray gun into a mold frame, but according to the present invention, each plate-like part is molded by the above manufacturing method, so that a molded body with a complex shape can be easily manufactured. The manufacturing method of the present invention can handle complex shapes and can bring out the shaping properties of the molded body. The part where the plate-like parts 10 are connected to each other may be configured as a connection part 10C.

[0084] The molded body may be formed in a single plate shape as shown in FIG. 1 or may be formed by connecting a plurality of plate-shaped parts 10, but may also be formed with a plate-shaped part 10 at least in a part. For example, in the molded body 1A shown in FIG. 7(a), when the length L of the other plate-shaped part 10B is short, the plate-shaped part 10B may be formed as a protruding part. The protruding part is different from the cross-sectional structure of the plate-shaped part 10 shown in FIG. 1, and is formed by embedding the first fiber reinforcement 110 and / or the second fiber reinforcement 120 extending from the end of one plate-shaped part 10A in a folded state, and is reinforced by these first fiber reinforcement 110 and / or the second fiber reinforcement 120. In this protruding part, mortar also enters the openings 111, 121 of the first fiber reinforcement 110 and / or the second fiber reinforcement 120.

[0085] The molded article may have a second surface, instead of the first surface, that is aesthetically designed. The applications of the molded articles are not limited to interior and exterior applications. In manufacturing the molded body, the forming of each plate-like portion is not limited to being performed by hand laying as in the hand lay-up method described above, but may be performed by stacking the plates using a machine and then pouring in mortar or ready-mixed concrete.

[0086] In the illustrated example, the spacer 140 is laid so as to cover the entire first fiber reinforcement 110, but a plurality of spacers 140 may be arranged spaced apart on the first fiber reinforcement 110 as long as they can maintain the distance between the first fiber reinforcement 110 and the second fiber reinforcement 120. Also, as the spacer 140, a plurality of blocks made of resin or the like may be arranged spaced apart on the first continuous sheet. The blocks may have voids into which the mortar material can enter, or may not have voids.

[0087] In addition, the spacer 140 in the above embodiment has a smaller wire diameter than the first fiber reinforcing material and does not contribute to the strength of mortar or concrete, but the spacer may also be used to reinforce mortar or concrete. In this case, the spacer 140 may be a lattice-shaped sheet made of a fiber-reinforced composite material such as fiber reinforced plastics.

[0088] Spacers can also be used in laminated structures to improve the strength of the plate-shaped portions. Furthermore, if the spacer is entangled with a retaining member such as a nut embedded in the middle portion, the molded body can be fixed even more firmly to the anchor bolt.

[0089] Although the case where the molding is performed using the mortar material 30 mixed with fibers such as chopped strands has been described, the molded body may be formed by omitting reinforcing fibers from mortar or concrete as the mortar material 30. In this case as well, the molded body can be suitably reinforced and the thickness t1 can be set to 20 mm or less by embedding the sheet-like first fiber reinforcing material on the first surface side and the second fiber reinforcing material on the second surface side. In addition, in the above embodiment, a form was described in which the reinforcing fibers also penetrate into the gaps in the holes of the spacer in the middle part, but the inclusion of reinforcing fibers in the middle part may be omitted, and at least the first surface side of the plate-like part containing the first fiber reinforcement material, and / or the second surface side of the plate-like part located opposite the first surface and further containing the second fiber reinforcement material, may be made of fiber-mixed mortar or fiber-reinforced concrete containing reinforcing fibers mixed in. In the case of concrete, in the present invention, small coarse aggregate is used and the concrete is formed to a thickness t' of 5 mm to 20 mm.

[0090] The molded bodies 1, 1A, and 3 may also be laminated on a body. [Explanation of symbols]

[0091] 1,1A,3 Molded body 2. Laminated structure 10, 10A, 10B, 100 Plate-shaped part 11,101 Front page 12,102 Front page 10C Connection 100A Main Unit 100B Partially thickened part 110 First Fiber Reinforcement Material 111 Aperture 120 Second fiber reinforcement material 121 Aperture 130 Middle Section 140 Spacer 20 Formwork 21 Bottom 40 base 50 Spray foam 60 Finishing layer 70 Anchor Bolt 80 Holding member 81 Nut 82 Washer M1 First side material M2 intermediate material M3 Second side material

Claims

1. A molded body made of mortar or concrete having a plate-shaped portion, The plate-shaped portion has a first fiber reinforcing material formed in a sheet shape and a second fiber reinforcing material formed in a sheet shape embedded therein at a distance in a thickness direction, The molded body is further characterized in that the thickness of the plate-like portion is 5 mm or more and 20 mm or less.

2. The molded body described in claim 1, characterized in that at least a first surface side of the plate-shaped portion containing the first fiber reinforcement material, and / or a second surface side of the plate-shaped portion located opposite the first surface and further containing the second fiber reinforcement material, is made of fiber-mixed mortar or fiber-reinforced concrete containing reinforcing fibers.

3. 3. The molded article according to claim 2, wherein the reinforcing fibers are chopped strands formed by bundling alkali-resistant glass fibers.

4. The plate-shaped portion includes a plurality of plate-shaped portions and a connecting portion connecting the plate-shaped portions to each other. A molded body as described in any one of claims 1 to 3, characterized in that, at the connection portion, the first fiber reinforcement materials of one of the plate-shaped portions and the other of the plate-shaped portions are overlapped, and / or the second fiber reinforcement materials of one of the plate-shaped portions and the other of the plate-shaped portions are overlapped.

5. A method for manufacturing a mortar or concrete molded body having a plate-like portion in which a first fiber reinforcing material formed in a sheet shape and a second fiber reinforcing material formed in a sheet shape are embedded at a distance in a thickness direction, the method comprising the steps of: A plate forming step of forming the plate-shaped portion is provided, The plate forming process includes: a depositing step of depositing a first surface side material for forming a first surface side of the plate-like portion, an intermediate material for forming an intermediate portion, and a second surface side material for forming a second surface side located opposite to the first surface of the plate-like portion, in that order, on a formwork or a framework; a curing process for curing the first surface side material, the intermediate material, and the second surface side material deposited on the formwork or the skeleton, the first surface side material is made of the mortar or the ready-mixed concrete having the first fiber reinforcing material embedded therein; the intermediate material is made of the mortar or the ready-mixed concrete in which a spacer is embedded, the second surface side material is made of the mortar or the ready-mixed concrete having the second fiber reinforcing material embedded therein; A method for manufacturing a molded body, characterized in that in the curing process, the first fiber reinforcement and the second fiber reinforcement are maintained separated in the thickness direction within the formwork or the mortar or fresh concrete of the main body by the spacer.

6. the depositing step includes a first depositing step of putting the first surface side material into the formwork or the skeleton, a second depositing step of depositing the intermediate material on the first surface side material, and a third depositing step of depositing the second surface side material on the intermediate material, The method for manufacturing a molded body described in claim 5, characterized in that the first deposition process includes a first manual laying process of manually laying the mortar or the ready-mixed concrete onto the formwork or the main body, which serves as a base for placing the first fiber reinforcement material, a second manual laying process of manually laying the first fiber reinforcement material on the base, and a third manual laying process of manually laying the mortar or the ready-mixed concrete onto the first fiber reinforcement material after the second manual laying process, to cover the first fiber reinforcement material with the mortar or the ready-mixed concrete.

7. The second stacking step includes a fourth manual stacking step of manually stacking a spacer on the first surface side material, and a fifth manual stacking step of manually stacking the mortar or the ready-mixed concrete on the spacer after the fourth manual stacking step to cover the spacer with the mortar or the ready-mixed concrete, The method for manufacturing a molded body described in claim 6, characterized in that the third deposition process includes a sixth manual laying process of manually laying the second fiber reinforcement material on the intermediate material, and a seventh manual laying process of manually laying the mortar or the ready-mixed concrete on the second fiber reinforcement material after the sixth manual laying process to cover the second fiber reinforcement material with the mortar or the ready-mixed concrete.

8. 8. The method for producing a molded body according to claim 5, wherein at least the mortar or the ready-mixed concrete of the first surface side material, and / or the mortar or the ready-mixed concrete of the second surface side material is a fiber-mixed mortar or a fiber-mixed ready-mixed concrete containing reinforcing fibers.

9. a base made of mortar or concrete; A foam laminated to the base; a mortar or concrete molded body laminated to the foamed body and having a plate-shaped portion; A laminated structure characterized in that the plate-shaped portion has a first fiber reinforcing material formed in a sheet shape and a second fiber reinforcing material formed in a sheet shape embedded at a distance in the thickness direction, and has a thickness of 5 mm or more and 40 mm or less.

10. The spray foam is a spray foam formed into an uneven shape with an uneven thickness on the molded body side, The laminated structure described in claim 9, characterized in that the plate-shaped portion comprises a main body in which the first fiber reinforcement material and the second fiber reinforcement material are embedded at a distance in the thickness direction and have a thickness of 5 mm to 40 mm, and a plurality of partial thickening portions formed on the spray foam side of the main body and increasing in thickness, and is formed in an uneven shape following the shape of the spray foam.

11. A finishing layer is provided on the plate-shaped portion of the molded body, An anchor bolt is embedded in the thickness direction from the base portion to the plate-shaped portion or the finishing layer, 11. The laminated structure according to claim 9, wherein a pressing member is attached to an end of the anchor bolt on a finishing layer side.

12. A method for manufacturing a laminated structure including a mortar or concrete molded body having a plate-like portion in which a first fiber reinforcing material formed in a sheet shape and a second fiber reinforcing material formed in a sheet shape are embedded at a distance in a thickness direction, the method comprising the steps of: a foam forming step of spraying a foam material onto a base made of mortar or concrete to form a sprayed foam having a non-uniform thickness and an uneven shape; and a plate forming step of forming the plate-shaped portion laminated to the spray foam, The plate forming process includes: a depositing step of depositing, in order, a first surface material for forming the spray foam side of the plate-shaped portion, an intermediate material for forming an intermediate portion, and a second surface material for forming the opposite side of the plate-shaped portion to the spray foam side, on the spray foam; a curing process for curing the first surface side material, the intermediate material, and the second surface side material deposited on the sprayed foam, the first surface side material is made of the mortar or the ready-mixed concrete having the first fiber reinforcing material embedded therein; the intermediate material is made of the mortar or the ready-mixed concrete in which a spacer is embedded, the second surface side material is made of the mortar or the ready-mixed concrete having the second fiber reinforcing material embedded therein; The depositing step is to apply the mortar or the ready-mixed concrete of the first surface side material to the spray foam to form a smooth surface, In the curing step, the first fiber reinforcement material and the second fiber reinforcement material are maintained apart from each other in a thickness direction in the mortar or the fresh concrete by the spacer, A method for manufacturing a laminated structure, characterized in that the base is a formwork or a framework.

Citation Information

Patent Citations

  • Concrete molded body and method for manufacturing it

    JP2005262713A