Photosensitive resin composition, dry film, cured product, and printed wiring board
A photosensitive resin composition combining black and blue colorants with a near-infrared absorber addresses the challenge of achieving both excellent hiding properties and resolution in printed wiring boards, ensuring consistent color and light absorption across a wide wavelength range.
Patent Information
- Application Number
- JP2024052258
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional black photosensitive resin compositions used for printed wiring boards face challenges in achieving both excellent hiding properties across a wide range of wavelengths from visible light to near-infrared regions and maintaining high resolution, particularly due to issues with light transmittance and color consistency.
A photosensitive resin composition combining a black colorant with a blue colorant and a near-infrared absorber, optimized to maintain specific color differences and optical densities, ensuring excellent hiding properties and resolution across the desired wavelength range.
The composition achieves a black color with superior hiding properties and resolution, minimizing light penetration and maintaining consistent color tone across varying film thicknesses, thereby enhancing the effectiveness of printed wiring boards.
Smart Images

Figure 2024146873000001 
Figure 2024146873000002 
Figure 2024146873000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive resin composition, and more specifically to a photosensitive resin composition that can be suitably used for forming an insulating layer such as a solder resist, a dry film using the photosensitive resin composition, a cured product of the photosensitive resin composition or the dry film, and a printed wiring board using these cured products. [Background technology]
[0002] Solder resist, which is often used as the outermost layer of a printed wiring board, may be required to be black depending on its application. For example, in LED-related wiring boards, it may be required to have a black color with good light absorption to make the LED light stand out, or a black color with high concealing properties to make the conductor pattern of the wiring board less visible. In addition, printed wiring boards that mount electronic elements such as optical sensors require a material that covers the area around the sensor to prevent unnecessary light from entering from the outside, and therefore require high light blocking properties from the visible light range to the near infrared range.
[0003] As a photosensitive resin composition used for the above-mentioned applications, a black photosensitive resin composition using carbon black as a colorant is known (for example, Patent Document 1). However, a photosensitive resin composition with excellent hiding properties also has a low light transmittance, so the resolution of patterning during exposure tends to decrease. Therefore, the higher the resolution of parts becomes, the more difficult it is to meet the demands of conventional black photosensitive resin compositions.
[0004] In response to the above problems, a black curable resin composition has been proposed that uses a specific organic coloring pigment to ensure the transmittance of light (wavelengths in the ultraviolet light region) during exposure while having low light transmittance in the visible light region (Patent Document 2).
[0005] Furthermore, many of the colorants used in photosensitive resin compositions tend to have a sharp increase in transmittance above 750 nm in the near-infrared region, and in order to ensure light-blocking (concealing) properties over a wide wavelength region, a near-infrared absorber is sometimes added (Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2008-257045 A [Patent Document 2] JP 2014-63091 A [Patent Document 3] JP 2015-86357 A Summary of the Invention [Problem to be solved by the invention]
[0007] The black curable resin composition proposed in Patent Document 2 has high transmittance in the ultraviolet region and excellent resolution, but has a problem in that it exhibits a slightly reddish black color because its transmittance is relatively high up to a wavelength region of about 450 nm.
[0008] Therefore, an object of the present invention is to provide a photosensitive resin composition which has a black color with excellent hiding power over a wide range from the visible light region to the near infrared region, and which also has excellent resolution. [Means for solving the problem]
[0009] The present inventors have conducted research into the above-mentioned problems, and have found that by using a black colorant and a blue colorant in combination with a near-infrared absorber, a photosensitive resin composition can be obtained that has a black color with excellent hiding power in a wide range from the visible light region to the near-infrared region, and also has excellent resolution. The present invention is based on this finding. That is, the gist of the present invention is as follows.
[0010] [1] A photosensitive resin composition comprising: (A) an alkali-soluble resin; (B) a photopolymerization initiator; (C) a black colorant; (D) a blue colorant; and (E) a near-infrared absorbing agent, The photosensitive resin composition was applied to the copper foil surface of a full-surface copper foil substrate whose surface was chemically polished to produce a cured product with a film thickness of 10 μm. The a* and b* in the L*a*b* color system measured under the condition of including total reflection light in accordance with JIS Z 8729 on the surface of the cured product were defined as a*1 and b*1, respectively. When a cured product with a film thickness of 30 μm was produced under the same conditions and the a* and b* in the L*a*b* color system measured under the same conditions were defined as a*2 and b*2, respectively, the L*, a*, and b* in the L*a*b* color system measured under the condition of including total reflection light in accordance with JIS Z 8729 on the surface of the copper foil to which the photosensitive resin composition was applied were in the ranges of 58 < L* < 75, 16 < a* < 22, and 22 < b* < 27, respectively, the color difference Δa* calculated as |a*1 - a*2| and the color difference Δb* calculated as |b*1 - b*2| respectively satisfy the following formulas: Δa* < 0.2 Δb* < 0.2 A photosensitive resin composition, characterized by satisfying the above. [2] The photosensitive resin composition according to [1], wherein the (C) black colorant has a minimum absorption value in the visible light region of 380 to 780 nm at 380 to 500 nm and a maximum absorption value at 500 to 780 nm. [3] The photosensitive resin composition according to [1] or [2], wherein the (D) blue colorant has a minimum absorption value in the visible light region of 380 to 780 nm at 380 to 600 nm and a maximum absorption value at 600 to 780 nm. [4] The photosensitive resin composition according to [2], wherein the difference between the maximum absorption value and the minimum absorption value of the (C) black colorant is 20% or more. [5] The photosensitive resin composition according to any one of [1] to [4], wherein the (D) blue colorant is contained in a proportion of 15 to 25% by mass in terms of solid content with respect to the (C) black colorant. [6] The photosensitive resin composition according to any one of [1] to [5], wherein the (E) near-infrared absorber is contained in a proportion of 100 to 300% by mass in terms of solid content with respect to the (C) black colorant. [7] A dry film comprising: a first film; and a resin layer formed by applying the photosensitive resin composition according to any one of [1] to [6] on one surface of the first film and drying the composition. [8] A cured product obtained by curing the resin layer of the photosensitive resin composition according to any one of [1] to [6] or the dry film according to [7]. [9] The cured product according to [8], having an L* value of 15 or less as measured by the L*a*b* color system defined in JIS Z 8729.
[10] The cured product according to [8] or [9], which has a transmittance of 5% or less at a wavelength of 500 to 800 nm.
[11] A printed wiring board having a coating made of the cured product according to any one of [8] to
[10] . Effect of the Invention
[0011] According to the present invention, by adding a near-infrared absorber while using a black colorant and a blue colorant in combination, it is possible to realize a photosensitive resin composition that has a black color with excellent hiding power over a wide range from the visible light region to the near-infrared region, and also has excellent resolution. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] [Photosensitive resin composition] The photosensitive resin composition according to the present invention contains (A) an alkali-soluble resin, (B) a photopolymerization initiator, (C) a black colorant, (D) a blue colorant, and (E) a near-infrared absorbing agent as essential components. In the present invention, the photosensitive resin composition is applied to the copper foil surface of a full copper foil substrate whose surface has been chemically polished to prepare a cured product having a thickness of 10 μm, and the a* and b* of the L*a*b* color system measured on the surface of the cured product under conditions including total reflected light in accordance with JIS Z 8729 are respectively a*1 and b*1, and a cured product having a thickness of 30 μm is prepared under the same conditions and the a* and b* of the L*a*b* color system measured under the same conditions are respectively a*2 and b*2. The L*, a*, and b* in the L*a*b* color system measured under the condition of including total reflected light in accordance with JIS Z 8729 on the surface of the copper foil to which the photosensitive resin composition is applied are in the ranges of 58 < L* < 75, 16 < a* < 22, and 22 < b* < 27, respectively, The color difference Δa* calculated as |a*1 - a*2| and the color difference Δb* calculated as |b*1 - b*2| respectively satisfy the following formulas: Δa* < 0.2 Δb* < 0.2 It is characterized by satisfying the above.
[0013] That is, in the present invention, when a cured product (cured film) of a photosensitive resin composition having different film thicknesses is formed on the copper foil surface of a predetermined full-surface copper foil substrate, (C) a black colorant and (D) a blue colorant are used in combination, and (E) a near-infrared absorber is blended so that the changes (color differences) in a* and b* are within a predetermined range. Thus, a photosensitive resin composition having excellent concealing properties in a wide range from the visible light region to the near-infrared region and excellent resolution can be realized. The reason for this is not clear, but it can be speculated as follows. That is, although the hiding power of the cured product when a film made of the cured product is provided on the surface of a printed wiring board or the like depends on the optical density in the visible light and near-infrared regions in the photosensitive resin composition, by using a photosensitive resin composition having an optical density such that the color differences Δa* and Δb* are within a predetermined range for cured products having different film thicknesses, it is considered that light in that region hardly reaches the base of the film made of the cured product and the reflected light is absorbed, so the color tone hardly changes.
[0014] In the present invention, L*, a*, and b* in the L*a*b* color system can be measured in accordance with JIS Z 8729. Also, by measuring a* and b* of cured products having different film thicknesses respectively, the color difference Δa* and the color difference Δb* can be calculated. Specifically, it can be measured according to the following procedures (1) to (7). (1) First, prepare a printed wiring board obtained by chemically polishing (roughening) a copper foil surface of a full-surface copper foil substrate with a 35-μm-thick copper foil bonded to the entire surface at an etching rate of 1 μm using CZ-8101B manufactured by Meck Co., Ltd. The color tone of the surface of the full-surface copper foil substrate to which the photosensitive resin composition is applied may vary depending on the type of copper foil and the chemical polishing conditions. However, if the L*, a*, and b* in the L*a*b* color system of the copper foil surface after chemical polishing measured under the condition including total reflected light in accordance with JIS Z 8729 are in the ranges of 58 < L* < 75, 16 < a* < 22, and 22 < b* < 27, respectively, a conventionally known full-surface copper foil substrate and a conventionally known chemical polishing method can be used. For example, the copper foil surface can be chemically polished at an etching rate of 0.05 to 3 μm using CZ-8101B or CZ-8100M manufactured by Meck Co., Ltd. Also, for the measurement of L*, a*, and b*, a spectrophotometer CM-2600d manufactured by Konica Minolta Inc. can be used. (2) Next, apply the photosensitive resin composition to the copper foil surface of the printed wiring board whose surface has been chemically polished using an applicator, and dry it at 80°C for 10 minutes to form a resin layer. (3) Subsequently, expose the resin layer using an exposure apparatus equipped with a high-pressure mercury lamp (short arc lamp), and develop it for 60 seconds under the condition of a 1 mass% aqueous sodium carbonate solution at 30°C with a spray pressure of 0.2 MPa. (4) After irradiating the exposed and developed resin layer with ultraviolet rays under the condition of an integrated exposure amount of 1000 mJ / cm 2 using a UV conveyor furnace, heat it at 170°C for 60 minutes to cure the resin layer, and produce a substrate having a cured product with a thickness of 10 μm formed on the copper foil. (5) Measure a* and b* in the L*a*b* color system of the surface of the cured product of the substrate thus obtained under the condition including total reflected light in accordance with JIS Z 8729 using a spectrophotometer (manufactured by Konica Minolta Inc., CM-2600d). (6) Measure a* and b* in the L*a*b* color system in the same manner as the production of the substrate having a cured product with a thickness of 10 μm, except that a substrate having a cured product with a thickness of 30 μm is produced by changing the coating amount of the photosensitive resin composition on the copper foil. (7) Calculate the color differences Δa* and Δb* from the measured a* and b*.
[0015] As the chemical polishing treatment agent, a conventionally known treatment agent can be used, and examples thereof include copper chloride-based, persulfate-based, sulfuric acid / hydrogen peroxide-based, formic acid, and organic acid-based treatment agents. Specifically, copper chloride-based products include MultiPrep 200 manufactured by MacDermid Performance Solutions Japan Co., Ltd.; persulfate-based products include Microclean, ME-301, and PR-820 manufactured by MacDermid Performance Solutions Japan Co., Ltd.; sulfuric acid / hydrogen peroxide-based products include GB-1000F, GB-1400, GB-200, GB-3100, and GB-4300 manufactured by Shikoku Kasei Corporation; Multibond 100, Multibond 150, Multibond MP, Metex G-5, Metex G-6, ME-501, ME-602, ME-605, and ME-709 manufactured by MacDermid Performance Solutions Japan Co., Ltd.; CPE-900 and EMR-7000 manufactured by Mitsubishi Gas Chemical Trading Co., Ltd.; and organic acid-based products include CZ-8100, CZ-8101, and CZ-8201 manufactured by MEC Co., Ltd.
[0016] Each component constituting the photosensitive resin composition of the present invention will be described below. <(A) Alkali-soluble resin> The (A) alkali-soluble resin contained in the photosensitive resin composition according to the present invention may be any resin that is alkali-soluble, and known and commonly used resins are used. The alkali-soluble resin may be used alone or in combination of two or more. Examples include water-soluble resins such as carboxyl group-containing resins and phenolic hydroxyl group-containing resins. Among them, carboxyl group-containing resins and phenolic hydroxyl group-containing resins are preferred because of their excellent developability, and carboxyl group-containing resins are more preferred. The alkali-soluble resin can be made alkaline developable by containing a carboxyl group. In addition, from the viewpoint of photosensitivity, it is preferable to have an ethylenically unsaturated double bond in the molecule in addition to the carboxyl group, but only a carboxyl group-containing resin that does not have an ethylenically unsaturated double bond may be used. When the carboxyl group-containing resin does not have an ethylenically unsaturated double bond, it is necessary to use a photopolymerizable monomer in combination to make the composition photocurable. As the ethylenically unsaturated double bond, one derived from acrylic acid or methacrylic acid or a derivative thereof is preferred.
[0017] Specific examples of carboxyl group-containing resins include the following compounds (which may be either oligomers or polymers): In this specification, (meth)acrylate is a general term for acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.
[0018] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc.
[0019] (2) Carboxylic acid-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0020] (3) Carboxylic acid-containing photosensitive urethane resins obtained by polyaddition reaction of diisocyanates with partially acid anhydride-modified products of reaction products of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins and biphenol type epoxy resins with monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, carboxyl group-containing dialcohol compounds and diol compounds.
[0021] (4) A photosensitive urethane resin containing a carboxyl group, which is terminated with (meth)acrylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3).
[0022] (5) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylation formed by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3).
[0023] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl groups present in the side chains.
[0024] (7) A carboxyl group-containing photosensitive resin obtained by reacting a multifunctional epoxy resin with the hydroxyl groups of a bifunctional (solid) epoxy resin further epoxidized with epichlorohydrin, with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.
[0025] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.
[0026] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, or the like.
[0027] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0028] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0029] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any one of the resins (1) to (11).
[0030] These carboxyl group-containing resins are not limited to those listed above, and may be used alone or in combination of two or more kinds.
[0031] The acid value of the carboxyl group-containing resin is preferably 40 to 150 mgKOH / g. By making the acid value of the carboxyl group-containing resin 40 mgKOH / g or more, alkaline development becomes good. Also, by making the acid value 150 mgKOH / g or less, it becomes easy to draw a good resist pattern. More preferably, it is 50 to 130 mgKOH / g.
[0032] The weight average molecular weight of the carboxyl group-containing resin varies depending on the resin skeleton, but is generally preferably 2,000 to 150,000. By making the weight average molecular weight 2,000 or more, it is possible to improve tack-free performance and resolution. Furthermore, by making the weight average molecular weight 150,000 or less, it is possible to improve developability and storage stability. It is more preferably 5,000 to 15,000. The weight average molecular weight can be measured by gel permeation chromatography (GPC).
[0033] The amount of the alkali-soluble resin (A) in the photosensitive resin composition is preferably 10 to 50% by mass, calculated as solid content. By making it 10% by mass or more, the coating strength can be improved. Also, by making it 50% by mass or less, the viscosity becomes appropriate and the printability is improved. More preferably, it is 10 to 40% by mass.
[0034] <(B) Photopolymerization initiator> The photosensitive resin composition according to the present invention contains a photopolymerization initiator (B) for photopolymerizing the above-mentioned (A) alkali-soluble resin and the later-described (D) photopolymerizable monomer. As the photopolymerization initiator, a known one can be used, for example, an α-aminoacetophenone-based photopolymerization initiator such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, or N,N-dimethylaminoacetophenone; 1-hydroxy-cyclohexylphenylketone; Hydroxyacetophenone photoinitiators such as 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, and 2-hydroxy-2-methyl-1-phenylpropan-1-one; bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethyl Phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,4,6-trimethylphenylphosphine oxide, acylphosphine oxide photopolymerization initiators such as methylbenzoyl)-phenylphosphine oxide, 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphine acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloylphenylphosphine acid isopropyl ester, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide;Benzoin-based photopolymerization initiators such as benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, and benzoin n-butyl ether; benzoin alkyl ether-based photopolymerization initiators; benzophenone-based photopolymerization initiators such as benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, and 4,4'-bisdiethylaminobenzophenone; acetophenone, 2,2-dimethoxy-2-phenylacetophenone acetophenone-based photopolymerization initiators such as 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone; thioxanthone-based photopolymerization initiators such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; anthraquinone, chlorothioxanthone, and chlorothioxanthone; Anthraquinone-based photopolymerization initiators such as chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; ketal-based photopolymerization initiators such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzoic acid ester-based photopolymerization initiators such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenyl)anthraquinone ... oxime ester photoinitiators such as ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium;These photopolymerization initiators may be used alone or in combination of two or more.
[0035] Commercially available α-aminoacetophenone-based photopolymerization initiators include Omnirad 907, 369, 369E, and 379 manufactured by IGM Resins. Commercially available acylphosphine oxide photopolymerization initiators include Omnirad 819 manufactured by IGM Resins. Commercially available titanocene photopolymerization initiators include JMT-784 manufactured by Yueyang Kimoutain Sci-Tech Co., Ltd. and GR-FMT manufactured by Hubei Kimoutain Sci-Tech Co., Ltd.
[0036] In addition, a photopolymerization initiator having two oxime ester groups in the molecule can also be suitably used, and specific examples thereof include oxime ester compounds having a carbazole structure represented by the following general formula (I). [ka]
[0037] In the above formula, X represents a hydrogen atom, an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a phenyl group, a phenyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an amino group, an alkylamino group having an alkyl group having 1 to 8 carbon atoms, or a dialkylamino group), a naphthyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an amino group, an alkylamino group having an alkyl group having 1 to 8 carbon atoms, or a dialkylamino group), and Y and Z each represent a hydrogen atom, an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a halogen group, a phenyl group, a phenyl group (substituted with an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, Ar represents an alkylene having 1 to 10 carbon atoms, vinylene, phenylene, biphenylene, pyridylene, naphthylene, thiophene, anthrylene, thienylene, furylene, 2,5-pyrrole-diyl, 4,4'-stilbene-diyl, or 4,2'-styrene-diyl, and n is an integer of 0 or 1.
[0038] In particular, in the above formula, X 1 , Y 1 are each a methyl group or an ethyl group, Z is methyl or phenyl, n is 0, and Ar is phenylene, naphthylene, thiophene, or thienylene.
[0039] In addition to the above-mentioned photopolymerization initiators, benzoin compounds, acetophenone compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, and xanthone compounds can be used as photopolymerization initiators. Among the above, from the viewpoint of deep curing, thioxanthone compounds and tertiary amine compounds are preferred, and thioxanthone compounds are more preferred. In addition, two or more of the above compounds may be used in combination. It is preferable to use the photopolymerization initiators exemplified here as photopolymerization initiator assistants or sensitizers in combination with the above-mentioned photopolymerization initiators rather than using them alone as photopolymerization initiators.
[0040] The amount of the photopolymerization initiator (B) in the photosensitive resin composition is preferably 1 to 50 parts by mass, more preferably 1 to 20 parts by mass, based on 100 parts by mass of the alkali-soluble resin (A) in terms of solid content, which can improve the curability in deep areas.
[0041] When the photosensitive resin composition contains the benzoin compound or the like as a photopolymerization initiator, the amount of the benzoin compound or the like is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the alkali-soluble resin (A) in terms of solid content, which can improve the curability of the deeper portion.
[0042] <(C) Black colorant> The black colorant (C) constituting the photosensitive resin composition according to the present invention is not particularly limited, and a conventionally known black colorant can be used, but preferably, a black colorant having a minimum absorption value at 380 to 500 nm and a maximum absorption value at 500 to 780 nm in the visible light region of 380 to 780 nm can be mentioned. By using such a specific black colorant, even if the content of the black colorant is increased, excellent resolution can be maintained even in a black concentration with a high OD value because the transmittance is high in the ultraviolet region. From the viewpoint of resolution, a black colorant in which the difference between the maximum absorption value and the minimum absorption value is 20% or more can be preferably used.
[0043] In the visible light region of 380-780 nm, examples of black colorants that have a minimum absorption value at 380-500 nm and a maximum absorption value at 500-780 nm include black perylene-based black pigments, zirconium nitride powder, and a mixture of zirconium nitride powder and titanium nitride powder or titanium oxynitride powder. Among these, black perylene-based black pigments and zirconium nitride powder can be used more preferably. In addition, as black perylene-based black pigments, Pigment Black 31, Pigment Black 32, and BASF's Lumogen Black FK4280 and FK 4281, which are known as black perylene-based black pigments that also have an absorption band in the near infrared, can be used preferably.
[0044] The blending amount of the (C) black colorant is preferably 1.0 to 2.5 mass %, and more preferably 1.6 to 1.8 mass %, based on the total solid content of the photosensitive resin composition, from the viewpoint of obtaining a desired high OD value in the visible light region.
[0045] <(D) Blue colorant> The (D) blue colorant constituting the photosensitive resin composition according to the present invention is not particularly limited, and a conventionally known blue colorant can be used, but preferably, a blue colorant having a minimum absorption value at 380 to 600 nm and a maximum absorption value at 600 to 780 nm in the visible light region of 380 to 780 nm can be used. By using such a blue colorant in combination with the above-mentioned black colorant, it is possible to suppress the appearance of reddish color while increasing the blending ratio of the black colorant (i.e., while improving the hiding power in the visible light region).
[0046] Any blue colorant having the above-described absorption wavelength characteristics may be used without particular limitation, and may be either an organic colorant or an inorganic colorant, although the use of an organic colorant is preferred.
[0047] Among organic colorants, phthalocyanine, dioxazine, and perylene are preferred because they have excellent photocurability, coloring properties, and visible light shielding properties.Specific examples of phthalocyanine colorants include Pigment Blue 15:3, 15:4, and 15:6, perylene colorants include Lumogen Black FK4280 and Lumogen Black FK4281, and oxazine colorants include Pigment Violet 23 and 37.One of these colorants can be used alone, or two or more can be used in combination.
[0048] The blending amount of the (D) blue colorant is preferably 15 to 25 mass % and more preferably 23 to 27 mass % in terms of solid content relative to the (C) black colorant from the viewpoint of setting the a* value in the desired range, and more preferably 0.2 to 0.9 mass % and more preferably 0.2 to 0.5 mass % relative to the total solid content of the photosensitive resin composition from the viewpoint of obtaining a desired high OD value in the visible light region.
[0049] <(E) Near infrared absorbing agent> As the near infrared absorbing agent (E) constituting the photosensitive resin composition according to the present invention, known and commonly used ones can be used, but it is preferable to use a dye having an absorption maximum at 500 to 1000 nm, and it is more preferable to use one having a maximum absorption wavelength of 800 to 1000 nm. As such dyes, metal complex dyes and condensed polycyclic dyes can be used, and specifically, for example, phthalocyanine dyes, porphyrin dyes, cyanine dyes, quaterylene dyes, squarylium dyes, azo dyes, aminium dyes, anthraquinone dyes, diimonium dyes, naphthalocyanine dyes, nickel complex dyes, copper ion dyes, dithiol metal complexes, heterocyclic compounds, etc. Among these, heterocyclic compounds, quaterine dyes, phthalocyanine dyes, naphthalocyanine dyes, etc. that also have absorption in the visible light region are preferred. Examples of the products include FDN-003, FDN-004, FDN-005, FDN-006, FDN-007, FDN-008, FDN-009, and FDN-010 (all manufactured by Yamada Chemical Industry Co., Ltd.). In addition, dyes having a maximum absorption within the above wavelength range and a metal complex that efficiently absorbs light and has a sensitizing effect are preferred. One or more of these can be used.
[0050] From the viewpoint of improving the hiding power in a wide range from the visible light region to the near infrared region while also achieving good resolution, the near infrared absorber (E) is preferably contained in a proportion of 100 to 300 mass %, more preferably 200 to 280 mass %, and even more preferably 235 to 255 mass %, calculated as the solid content, relative to the black colorant (C).
[0051] From the viewpoint of obtaining a black color having excellent hiding power over a wide range from the visible light region to the near infrared region, the blending amount of the (E) near infrared absorber is preferably 1 to 6 mass %, and more preferably 3 to 5 mass %, based on the total solid content of the photosensitive resin composition.
[0052] <Photopolymerizable monomer> The photosensitive resin composition of the present invention may contain a photopolymerizable monomer. The photopolymerizable monomer is a monomer having an ethylenically unsaturated double bond. Examples of such photopolymerizable monomers include known and commonly used polyester (meth)acrylates, polyether (meth)acrylates, urethane (meth)acrylates, carbonate (meth)acrylates, and epoxy (meth)acrylates. Specifically, alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; mono- or diacrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-methylolacrylamide, and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; and various other compounds such as hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, and trishydroxyethyl isocyanurate. Polyhydric acrylates derived from hydric alcohols or their alkylene oxide adducts or ε-caprolactone adducts; phenols such as phenoxy acrylate and bisphenol A diacrylate or their alkylene oxide adducts; acrylates derived from glycidyl ethers such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and acrylates and melamine acrylates obtained by directly acridating polyols such as polyether polyols, polycarbonate diols, hydroxyl group-terminated polybutadienes, and polyester polyols, or by urethane acridating polyols via diisocyanates, and the methacrylates corresponding to the acrylates can be appropriately selected and used. Such photopolymerizable monomers can also be used as reactive diluents.
[0053] The photopolymerizable monomer may be used alone or in combination of two or more. The amount of the photopolymerizable monomer is preferably 0.5 to 30 parts by mass, calculated as solid content, per 100 parts by mass of (A) alkali-soluble resin. When the amount is 0.5 parts by mass or more, the photocurability is good, and pattern formation is easy in alkali development after irradiation with active energy rays. When the amount is 30 parts by mass or less, halation is unlikely to occur and good resolution can be obtained.
[0054] <Thermosetting component> The photosensitive resin composition of the present invention may contain a thermosetting component in addition to the above-mentioned components. Examples of the thermosetting component include known and commonly used components such as isocyanate compounds, blocked isocyanate compounds, amino resins, maleimide compounds, benzoxazine resins, carbodiimide resins, cyclocarbonate compounds, epoxy compounds, oxetane compounds, and episulfide resins. Among these, the preferred thermosetting component is an epoxy resin.
[0055] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, biphenyl type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, triphenylmethane type epoxy resins, and the like. These may be used alone or in combination of two or more.
[0056] Examples of commercially available epoxy resins include jER 828, 806, 807, YX8000, YX8034, and 834 manufactured by Mitsubishi Chemical Corporation; YD-128, YDF-170, ZX-1059, and ST-3000 manufactured by Nippon Steel Chemical & Material Co., Ltd.; EPICLON 830, 835, 840, 850, N-730A, and N-695 manufactured by DIC Corporation; and RE-306 manufactured by Nippon Kayaku Co., Ltd.
[0057] The equivalent weight of the epoxy group of the epoxy resin in the photosensitive resin composition is preferably 0.5 to 2.5 in terms of solid content relative to the equivalent weight of the carboxyl group of the carboxyl group-containing resin (1). By making it 0.5 equivalent weight or more, it is possible to prevent the carboxyl group from remaining in the cured product, and to obtain good heat resistance, alkali resistance, electrical insulation, etc. Also, by making the blending amount 2.5 equivalent weight or less, it is possible to prevent the low molecular weight cyclic (thio)ether group from remaining in the dried coating film, and to ensure good strength of the cured product, etc.
[0058] When the photosensitive resin composition of the present invention contains a thermosetting component, it may contain a thermosetting catalyst for promoting the curing of the thermosetting component. Examples of the thermosetting catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. Other commercially available compounds include, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all trade names of imidazole-based compounds) manufactured by Shikoku Chemical Industry Co., Ltd., and U-CAT 3513N (trade name of dimethylamine-based compound), DBU, DBN, and U-CAT SA 102 (all bicyclic amidine compounds and salts thereof) manufactured by San-Apro Co., Ltd.
[0059] The compounds are not limited to the above, and may be used alone or in combination of two or more as long as they are heat curing catalysts for epoxy resins or oxetane compounds, or catalysts that promote the reaction of at least one of epoxy groups and oxetanyl groups with carboxyl groups. In addition, S-triazine derivatives such as guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine·isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-S-triazine·isocyanuric acid adduct may also be used, and preferably, these compounds that also function as adhesion promoters are used in combination with the heat curing catalyst.
[0060] The thermosetting catalyst may be used alone or in combination of two or more. From the viewpoint of the storage stability of the resin composition and the heat resistance of the cured coating, the amount of the thermosetting catalyst is preferably 0.01 to 30 parts by mass, and more preferably 0.1 to 20 parts by mass, calculated as solid content per 100 parts by mass of the alkali-soluble resin (A).
[0061] <Other ingredients> The photosensitive resin composition according to the present invention may contain a filler as required in order to improve the physical strength of the cured product and adjust the matte surface. As the filler, known inorganic or organic fillers may be used, and barium sulfate, spherical silica, hydrotalcite, and talc are particularly preferred. In order to obtain flame retardancy, metal oxides and metal hydroxides such as aluminum hydroxide may be used as extender pigment fillers.
[0062] The amount of the filler to be blended is not particularly limited, but from the viewpoints of viscosity, coatability, moldability, etc., the amount is preferably 300 parts by mass or less, more preferably 50 to 200 parts by mass, per 100 parts by mass of the alkali-soluble resin, calculated as solid content.
[0063] The above-mentioned filler may be surface-treated to enhance dispersibility in the photosensitive resin composition. By using a surface-treated filler, aggregation can be suppressed. The surface treatment method is not particularly limited, and a known and commonly used method may be used, but it is preferable to treat the surface of the inorganic filler with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group.
[0064] As the coupling agent, silane-based, titanate-based, aluminate-based, zircoaluminate-based, and other coupling agents can be used. Among them, silane-based coupling agents are preferred. Examples of such silane-based coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane, which can be used alone or in combination. It is preferable that these silane-based coupling agents are immobilized on the surface of the filler in advance by adsorption or reaction. Here, the amount of the coupling agent to be treated with respect to 100 parts by mass of the spherical silica is preferably 0.5 to 10 parts by mass.
[0065] In addition to the above-mentioned colorants, the photosensitive resin composition according to the present invention may contain other colorants as necessary. As the colorant, a known colorant such as red, green, or yellow can be used, and any of a pigment, dye, and coloring matter can be used, but from the viewpoint of reducing the environmental load and having little effect on the human body, a colorant that does not contain halogen is preferable.
[0066] The photosensitive resin composition may contain an organic solvent from the viewpoint of ease of preparation and coatability when forming a resin layer. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. Known and commonly used organic solvents can be used. These organic solvents can be used alone or in combination of two or more.
[0067] The amount of the organic solvent in the photosensitive resin composition can be appropriately changed depending on the materials constituting the photosensitive resin composition, and can be, for example, 30 to 300 parts by mass per 100 parts by mass of the solid content of the alkali-soluble resin.
[0068] The photosensitive resin composition may further contain, as necessary, components such as elastomers, mercapto compounds, urethanization catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper inhibitors, antioxidants, rust inhibitors, thickeners such as organic bentonite and montmorillonite, at least one of silicone-based, fluorine-based, and polymer-based defoamers and leveling agents, and flame retardants such as phosphorus compounds such as phosphinates, phosphate ester derivatives, and phosphazene compounds. These may be known in the field of electronic materials.
[0069] <Dry film> The photosensitive resin composition of the present invention can also be in the form of a dry film comprising a first film and a resin layer made of the photosensitive resin composition formed on the first film. The first film in the dry film according to the present invention refers to a film that is at least adhered to the resin layer when the film is laminated by heating or the like onto a substrate such as a board so that the resin layer made of the photosensitive resin composition formed on the dry film is in contact with the substrate and integrally molded. The first film may be peeled off from the resin layer in a step after lamination. In particular, in the present invention, it is preferable to peel off from the resin layer in a step after exposure.
[0070] To prepare a dry film, the photosensitive resin composition of the present invention is diluted with an organic solvent to adjust the viscosity to an appropriate level, and then coated onto a first film in a uniform thickness using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like, and typically dried for 1 to 30 minutes at a temperature of 50 to 130° C. to obtain a film. There are no particular limitations on the coating film thickness, but it is generally appropriately selected within the range of 1 to 150 μm, preferably 10 to 60 μm, in terms of the film thickness after drying.
[0071] As the first film, any known film can be used without any particular limitation, and for example, a film made of a thermoplastic resin such as a polyester film such as polyethylene terephthalate or polyethylene naphthalate, a polyimide film, a polyamideimide film, a polypropylene film, or a polystyrene film can be suitably used. Among these, a polyester film is preferred from the viewpoints of heat resistance, mechanical strength, handling, etc. A laminate of these films can also be used as the first film.
[0072] From the viewpoint of improving mechanical strength, the above-mentioned thermoplastic resin film is preferably a film stretched in a uniaxial or biaxial direction.
[0073] The thickness of the first film is not particularly limited, but can be, for example, 10 μm to 150 μm.
[0074] After forming a resin layer of the photosensitive resin composition of the present invention on the first film, it is preferable to further laminate a peelable second film on the surface of the resin layer for the purpose of preventing dust from adhering to the surface of the resin layer, etc. The second film in the dry film of the present invention refers to a film that is peeled off from the resin layer before lamination when the dry film is laminated by heating or the like so that the resin layer side of the dry film is in contact with a base material such as a substrate to be integrally molded.
[0075] The second film that can be peeled off from the resin layer may be, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, surface-treated paper, etc., as long as the adhesive strength between the resin layer and the second film is smaller than the adhesive strength between the resin layer and the first film when the second film is peeled off.
[0076] The thickness of the second film is not particularly limited, but can be, for example, 10 μm to 150 μm.
[0077] <Cured product> The cured product of the present invention is obtained by curing the above-mentioned photosensitive resin composition or the resin layer of the above-mentioned dry film.
[0078] The cured product of the present invention preferably has an L* of 15 or less as measured in the L*a*b* color system defined in JIS Z 8729. Specifically, the L*, a*, and b* of the L*a*b* color system can be measured in the same manner as described above, except that a substrate having a 20 μm-thick cured product formed on copper foil is prepared by changing the amount of photosensitive resin composition applied.
[0079] The cured product of the present invention preferably has a transmittance of 5% or less at a wavelength of 500 to 800 nm. Specifically, it can be measured as follows. The photosensitive resin composition is applied to a 1 mm thick F-1 glass substrate (light transmittance 90%) using an applicator so that the film thickness after drying is 25 μm, and dried at 80° C. for 10 minutes to form a resin layer on the glass substrate. Next, the resin layer is exposed to light using an exposure device equipped with a high-pressure mercury lamp (short arc lamp), and developed with a 1% by mass aqueous sodium carbonate solution at 30° C. for 60 seconds under conditions of a spray pressure of 0.2 MPa. The obtained substrate is then exposed to light in a UV conveyor furnace with an integrated exposure dose of 1000 mJ / cm. 2 After irradiating with ultraviolet light under the above conditions, the resin layer is cured by heating at 150° C. for 60 minutes to prepare an evaluation substrate. The transmittance of the obtained evaluation substrate at wavelengths of 500 to 800 nm is measured using a UV-VIS measurement device (V-670 EX, manufactured by JASCO Corporation).
[0080] <Printed wiring board> The printed wiring board of the present invention has a cured product obtained from the resin layer of the photosensitive resin composition or dry film of the present invention. As a method for producing the printed wiring board of the present invention, for example, the photosensitive resin composition of the present invention is adjusted to a viscosity suitable for the coating method using the organic solvent, and applied to a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating, and then the organic solvent contained in the composition is evaporated and dried (temporarily dried) at a temperature of 60 to 100 ° C. to form a tack-free resin layer. In addition, in the case of a dry film, the resin layer is attached to the substrate by a laminator or the like so that the resin layer contacts the substrate, and then the first film is peeled off to form a resin layer on the substrate.
[0081] The above-mentioned substrates include printed wiring boards and flexible printed wiring boards with circuits formed in advance using copper or the like, as well as materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, copper-clad laminates for high-frequency circuits using materials such as fluororesin-polyethylene-polyphenylene ether, polyphenylene oxide-cyanate, etc., including copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates, etc.
[0082] In the case of a dry film form, the lamination onto the substrate is preferably performed under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, when a circuit-formed substrate is used, even if the surface of the circuit substrate is uneven, the dry film adheres to the circuit substrate, so that no air bubbles are mixed in, and the filling of the recesses on the substrate surface is improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.
[0083] When the photosensitive resin composition of the present invention contains an organic solvent, it is preferable to apply the photosensitive resin composition to the surface of a substrate and then perform volatilization drying. The volatilization drying can be performed using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, etc. (a method of countercurrent contact of hot air in a dryer using a heat source of an air heating method using steam, or a method of spraying the hot air from a nozzle onto the substrate).
[0084] After forming a resin layer on a substrate, the resin layer is selectively exposed to active energy rays through a photomask having a predetermined pattern formed thereon, and the unexposed portion is developed with a dilute alkaline aqueous solution (e.g., 0.3 to 3 mass% aqueous sodium carbonate solution) to form a pattern of the cured product. In the case of a dry film, after exposure, the first film is peeled off from the dry film and development is performed to form a patterned cured product on the substrate. In addition, in the case of a dry film form, the first film may be peeled off from the dry film before exposure, and the exposed resin layer may be exposed and developed, as long as the characteristics are not impaired. Furthermore, a cured coating excellent in various properties such as adhesion and hardness can be formed by irradiating the cured product with active energy rays and then heat curing (e.g., 100 to 220°C), or irradiating active energy rays after heat curing, or by heat curing only to perform final finish curing (main curing).
[0085] The exposure machine used for the above-mentioned active energy ray irradiation may be a machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm. Furthermore, a direct imaging machine (for example, a laser direct imaging machine that directly draws an image with a laser based on CAD data from a computer) may also be used. The lamp light source or laser light source of the direct imaging machine may have a maximum wavelength in the range of 350 to 450 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 10 to 1000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 The range may be:
[0086] The developing method can be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution can be an aqueous alkali solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.
[0087] After the cured coating is formed on the substrate as described above, components such as electronic elements are mounted on the substrate by solder reflow treatment. The solder reflow treatment can be performed by a conventionally known method. In general, the solder reflow treatment is performed under treatment conditions of, for example, 245 to 260°C for 5 to 10 seconds.
[0088] The photosensitive resin composition or dry film of the present invention is preferably used for manufacturing electronic parts such as printed wiring boards, and more preferably used to form a permanent coating. In this case, the photosensitive resin composition or dry film of the present invention is used to form a cured product by the above-mentioned method or the like. When the resin layer of the photosensitive resin composition or dry film of the present invention is insulating, it is preferably used to form a solder resist, a coverlay, or an interlayer insulating layer. EXAMPLES
[0089] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.
[0090] <Synthesis example: Synthesis of alkali-soluble resin> To 650 parts by mass of diethylene glycol monoethyl ether acetate, 1,070 g of orthocresol novolac epoxy resin (EPICLON N-695, manufactured by DIC Corporation, softening point 95°C, epoxy equivalent 214, average functionality 7.6), 360 g of acrylic acid, and 1.5 g of hydroquinone were charged, and the mixture was heated to 100°C with stirring to dissolve uniformly. Next, 4.3 parts by mass of triphenylphosphine was added, heated to 110° C. and reacted for 2 hours, after which 1.6 parts by mass of triphenylphosphine was further added, the temperature was raised to 120° C. and the reaction was further carried out for 12 hours. To the resulting reaction solution, 525 g of aromatic hydrocarbon (T-Sol 150, manufactured by Standard Oil Co., Ltd. Osaka Sales Office) and 608 g (4.0 mol) of tetrahydrophthalic anhydride were added, and the reaction was carried out for 4 hours at 110° C. Furthermore, 142.0 g of glycidyl methacrylate was added to the resulting reaction solution, and the reaction was carried out for 4 hours at 115° C. In this way, a solution of an alkali-soluble resin having a solid content of 65% and an acid value of the solid content of 77 mgKOH / g was obtained.
[0091] <Preparation of Photosensitive Resin Composition> The components shown in Table 1 below were mixed at room temperature using a three-roll mill to obtain the photosensitive resin compositions shown in the table. Each value in the table indicates parts by mass, and values other than the solvent are expressed in terms of solid content.
[0092] In addition, each component *1 to *7 in Table 1 below is as follows. *1: Alkali-soluble resin synthesized in the synthesis example *2: α-aminoacetophenone photopolymerization initiator (manufactured by IGM Resins) *3: Oxime ester photopolymerization initiator represented by the following formula [ka] *4: α-aminoacetophenone photopolymerization initiator (IGM Resins) *5: Perylene black (minimum absorption wavelength 400 nm, maximum absorption wavelength 600 nm, difference between maximum and minimum absorption values 50%) *6: Carbon black (minimum absorption wavelength 780 nm, maximum absorption wavelength 380 nm, difference between maximum and minimum absorption values less than 20%) *7: NITRBLACK UB-2 (manufactured by Mitsubishi Materials Corporation, minimum absorption wavelength 350 nm, maximum absorption wavelength 500 nm, difference between maximum and minimum absorption values 20%) *8: FASTOGEN BLUE FA5380 (DIC Corporation, minimum absorption wavelength 510 nm, maximum absorption wavelength 660 nm) *9: Cromophtal Violet D 5700 (manufactured by BASF Japan Ltd., minimum absorption wavelength 420 nm, maximum absorption wavelength 560 nm) *10: Naphthalocyanine-based dye (manufactured by Yamada Chemical Industry Co., Ltd., maximum absorption wavelength 853 nm) *11: Naphthalocyanine-based dye (manufactured by Yamada Chemical Industry Co., Ltd., maximum absorption wavelength 992 nm) *12: Lumogen IR 765 (manufactured by BASF Japan Ltd., maximum absorption wavelength 765 nm) *13: N-770 (phenol novolac type epoxy resin, manufactured by DIC Corporation) *14: jER 828 (bisphenol type epoxy resin, manufactured by Mitsubishi Chemical Corporation) *15: NC-3000-H (epoxy resin, manufactured by Nippon Kayaku Co., Ltd.) *16: Talc (manufactured by Nippon Talc Co., Ltd., average particle diameter 0.85 μm) *17: Barium sulfate (average particle diameter 0.8 μm) *18: Propylene glycol monomethyl ether acetate
[0093] <Measurement of a* and b* A printed wiring board was prepared by chemically polishing (roughening treatment) a copper foil surface of a full copper foil substrate with a 35-μm-thick copper foil bonded to the entire surface at an etching rate of 1 μm using CZ-8101B manufactured by Meck Co., Ltd. Each photosensitive resin composition obtained as described above was applied to the copper foil surface of the printed wiring board with a chemically polished surface using an applicator and dried at 80°C for 10 minutes to form a resin layer. Next, the resin layer was exposed using an exposure apparatus equipped with a high-pressure mercury lamp (short arc lamp), and developed for 60 seconds under the condition of spraying a 1% by mass aqueous sodium carbonate solution at 30°C with a spray pressure of 0.2 MPa. The obtained substrate was irradiated with ultraviolet rays in a UV conveyor furnace under the condition of an integrated exposure amount of 1000 mJ / cm 2 and then heated at 170°C for 60 minutes to cure the resin layer, thereby producing a substrate having a 10-μm-thick cured product formed on the copper foil. Next, the surface of the cured product of the substrate obtained as described above was measured for a* and b* in the L*a*b* color system under the condition including total reflected light in accordance with JIS Z 8729 using a spectrophotometer (CM-2600d, manufactured by Konica Minolta, Inc.). In addition, when the surface of a full-surface copper foil substrate with a copper thickness of 35 μm whose copper foil surface was chemically polished was measured for L*, a*, and b* in the L*a*b* color system under the condition including total reflected light in accordance with JIS Z 8729 using a spectrophotometer (CM-2600d, manufactured by Konica Minolta, Inc.), the results were L* = 62, a* = 20.8, and b* = 25.4.
[0094] In addition, a* and b* in the L*a*b* color system were measured in the same manner as above, except that a substrate having a cured product with a thickness of 30 μm formed on a copper foil was prepared by changing the coating amount of the photosensitive resin composition.
[0095] Color differences Δa* and Δb* were calculated from the obtained a* and b*. The results were as shown in Table 1.
[0096] <Measurement of L*> L* in the L*a*b* color system was measured in the same manner as <Measurement of a* and b*> above, except that a substrate having a cured product with a thickness of 20 μm formed on a copper foil was prepared by changing the coating amount of the photosensitive resin composition. The measurement results were as shown in Table 1.
[0097] <Evaluation of Light Transmittance> Each photosensitive resin composition was applied to an F-1 glass substrate with a thickness of 1 mm (light transmittance 90%) using an applicator so that the film thickness after drying was 25 μm, and dried at 80°C for 10 minutes to form a resin layer on the glass substrate. Next, the resin layer was exposed using an exposure apparatus equipped with a high-pressure mercury lamp (short arc lamp), and developed for 60 seconds under the condition of a spray pressure of 0.2 MPa with a 1 mass% aqueous sodium carbonate solution at 30°C. The obtained substrate was irradiated with ultraviolet rays in a UV conveyor furnace under the condition of an integrated exposure amount of 1000 mJ / cm 2 and then heated at 150°C for 60 minutes to cure the resin layer to obtain an evaluation substrate.
[0098] For the evaluation substrate obtained as described above, the transmittance at wavelengths of 500 to 800 nm was measured using a UV-VIS measurement device (V-670 EX, manufactured by JASCO Corporation), and the light transmittance was evaluated according to the following evaluation criteria. ○: Transmittance is 5% or less ×: Transmittance is more than 5% The evaluation results are shown in Table 1 below.
[0099] <Evaluation of resolution> Each photosensitive resin composition obtained as described above was applied to the surface of a polyethylene terephthalate film (T-60, manufactured by Toray Industries, Inc., thickness 38 μm) as a first film using an applicator so that the film thickness after drying would be 25 μm, and the film was dried at 80° C. for 10 minutes to form a resin layer. A polypropylene film (OPP-FOA, manufactured by Futamura Corporation, thickness 18 μm) was laminated onto the resin layer as a second film to produce a dry film.
[0100] Next, the copper foil surface of an FR-4 copper-clad laminate (100 mm x 150 mm x 0.8 mmt, double-sided copper foil, copper foil thickness on both sides is 18 μm) was chemically polished at an etching rate of 1 μm using CZ-8101B manufactured by MEC Co., Ltd., and the exposed surface of the resin layer of each dry film obtained by peeling off the second film from each dry film obtained as described above was bonded to the chemically polished copper foil surface. Next, using a vacuum laminator (MVLP-500 manufactured by Meiki Seisakusho Co., Ltd.), heat lamination was performed under conditions of pressure: 0.8 MPa, 70°C, 1 minute, and vacuum: 133.3 Pa, to adhere the substrate and resin layer to obtain a test substrate. Next, using a parallel light exposure device equipped with a short-arc type high-pressure mercury lamp, each film was exposed through an exposure mask from the polyethylene terephthalate film side, which was the first film, using a negative pattern designed to have an SRO (solder resist opening) of 200 μm, and then the first film was peeled off by hand in about 1 second to expose the resin layer. The exposure amount was set to an amount that would result in 7 steps when exposed using a Stouffer 41 step from the first film in contact with the photosensitive film. Thereafter, 1 wt % Na was applied to the exposed surface of the exposed photosensitive film. 2 CO 3 Using an aqueous solution, 30℃, spray pressure 2kg / cm 2 The pattern was then developed for 90 seconds under the conditions of 1000 mJ / cm. 2 The patterned photosensitive film was irradiated with an exposure dose of 100 μm, and then heated at 150°C for 60 minutes for additional curing to form a cured film, producing a test substrate with a cured film formed on the substrate. The openings of 100 μm in diameter in each test substrate were observed by SEM to evaluate the difference in size between the top and bottom openings. The resolution was evaluated according to the following criteria. ○: The difference between the top and bottom is 30 μm or less ×: The difference between the top and bottom is more than 30 μm. The evaluation results are shown in Table 1 below.
[0101] [Table 1]
[0102] As is clear from Table 1, the photosensitive compositions (Examples 1 to 5) that use a specific black colorant in combination with a specific blue colorant and further contain a near-infrared absorber have a black color that is excellent in hiding power over a wide range from the visible light region to the near-infrared region, while also having excellent resolution. On the other hand, the photosensitive resin composition not containing any of the specific black colorant, the specific blue colorant, and the near-infrared absorbing agent (Comparative Examples 1 to 3, 5) is excellent in resolution but insufficient in terms of excellent hiding power. Also, even the photosensitive resin composition (Comparative Example 4) containing both the black colorant and the blue colorant and further the near-infrared absorbing agent cannot achieve both resolution and hiding power due to the absorption characteristics of the black colorant and the blue colorant.
Claims
1. A photosensitive resin composition comprising: (A) an alkali-soluble resin; (B) a photopolymerization initiator; (C) a black colorant; (D) a blue colorant; and (E) a near-infrared absorbing agent, The photosensitive resin composition was applied to the copper foil surface of a full copper foil substrate whose surface had been chemically polished to prepare a cured product having a thickness of 10 μm. The a* and b* of the L*a*b* color system measured on the surface of the cured product under conditions including total reflected light in accordance with JIS Z 8729 were designated a*1 and b*1, respectively. A cured product having a thickness of 30 μm was prepared under the same conditions, and the a* and b* of the L*a*b* color system measured under the same conditions were designated a*2 and b*2, respectively. the L*, a* and b* of the L*a*b* color system, measured on the surface of the copper foil to which the photosensitive resin composition is applied under conditions including total reflected light in accordance with JIS Z 8729, are within the ranges of 58<L*<75, 16<a*<22 and 22<b*<27, respectively; The color difference Δa* calculated as |a*1-a*2| and the color difference Δb* calculated as |b*1-b*2| are expressed by the following formulas, respectively: Δa*<0.2 Δb*<0.2 A photosensitive resin composition, characterized in that:
2. 2. The photosensitive resin composition according to claim 1, wherein the black colorant (C) has a minimum absorption value at 380 to 500 nm and a maximum absorption value at 500 to 780 nm in the visible light region of 380 to 780 nm.
3. 2. The photosensitive resin composition according to claim 1, wherein the (D) blue colorant has a minimum absorption value in the range of 380 to 600 nm and a maximum absorption value in the range of 600 to 780 nm in the visible light region of 380 to 780 nm.
4. The photosensitive resin composition according to claim 3 , wherein the black colorant (C) has a difference between the maximum absorption value and the minimum absorption value of 20% or more.
5. 2. The photosensitive resin composition according to claim 1, wherein the blue colorant (D) is contained in an amount of 15 to 25 mass % in terms of solid content relative to the black colorant (C).
6. 2. The photosensitive resin composition according to claim 1, wherein the near infrared absorbing agent (E) is contained in an amount of 100 to 300 mass% in terms of solid content relative to the black colorant (C).
7. A dry film comprising: a first film; and a resin layer formed by applying the photosensitive resin composition according to claim 1 to one surface of the first film and drying the composition.
8. A cured product obtained by curing the photosensitive resin composition according to claim 1 or the resin layer of the dry film according to claim 7.
9. 9. The cured product according to claim 8, which has an L* value of 15 or less as measured in the L*a*b* color system defined in JIS Z 8729.
10. The cured product according to claim 8, having a transmittance of 5% or less at a wavelength of 500 to 800 nm.
11. A printed wiring board provided with a coating comprising the cured product according to claim 8.
Citation Information
Patent Citations
Black solder resist composition and cured product thereof
JP2008257045A
Black curable resin composition
JP2014063091A
Curable resin composition, dry film, cured product, and display member
JP2015086357A
Cited By
Wafer supporting apparatus and SiC epitaxial growth apparatus
CN121653828A
Photosensitive resin composition, dry film, cured product, and printed wiring board
WO2026204479A1
Photosensitive resin composition, dry film, cured product, and printed wiring board
WO2026204480A1