Anti-fouling coating composition
The antifouling paint composition with a triorganosilyl group-containing copolymer and dicarboxylic acid ester addresses poor topcoat adhesion in silyl-based coatings by improving exposure adhesion, reducing peeling and propulsion resistance in ships.
Patent Information
- Application Number
- JP2024055144
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-15
AI Technical Summary
Silyl-based antifouling coatings exhibit poor adhesion of the topcoat to the undercoat after long-term exposure to outdoor environments, leading to partial peeling and increased propulsion resistance in ships, which affects fuel consumption and greenhouse gas emissions.
An antifouling paint composition containing a triorganosilyl group-containing copolymer and a dicarboxylic acid ester, which improves the adhesion of the topcoat to the undercoat even after prolonged exposure, maintaining antifouling performance and reducing peeling.
The composition enhances topcoat adhesion to undercoat antifouling films after long-term outdoor exposure, reducing peeling and propulsion resistance, thus minimizing fuel consumption and environmental impact.
Smart Images

Figure 2024146894000001 
Figure 2024146894000002 
Figure 2024146894000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an antifouling coating composition, an antifouling coating film, a substrate with an antifouling coating film, a method for producing a substrate with an antifouling coating film, etc. More specifically, the present invention relates to an antifouling coating composition containing a silyl resin (e.g., a triorganosilyl group-containing copolymer), etc. [Background technology]
[0002] In order to prevent fouling caused by marine organisms on substrates such as the bottom of a ship, a method of forming an antifouling coating film by coating the surface of the substrate with an antifouling paint is widely used. Currently, the main antifouling paint for the bottom of a ship is a silyl-based antifouling paint containing a resin such as an acrylic polymer containing a silyl ester group such as a triorganosilyl group.
[0003] In shipbuilding, the hull is generally constructed in blocks outside the dock, painted with antifouling paint (pre-painting), and then welded together (total assembly). After total assembly, antifouling paint is painted again on some or all of the joints (finish painting). Therefore, the silyl-based antifouling paint used in the finish painting is required to have "topcoat adhesion" to the undercoat paint.
[0004] As silyl-based antifouling paints, those described in Patent Documents 1 and 2, for example, are known.
[0005] Patent Document 1 describes an antifouling coating composition containing a resin component and an ester compound represented by a specific chemical formula (Claim 1, etc.). As the resin component, a silyl-based resin containing a triorganosilyl group is also exemplified (Claim 16, etc.). As the ester compound, Patent Document 1 describes a compound represented by formula (5) R-OOC-X-COO-R (wherein X and R are each a hydrocarbon group having 1 to 22 carbon atoms which may contain a heteroatom, the hydrocarbon group is aliphatic or aromatic, and has a linear, branched, or cyclic structure, and the two R are the same or different) (Claim 1, etc.). The invention described in Patent Document 1 has an objective of providing "an antifouling coating composition which can maintain a stable coating film dissolution rate over a long period of time in seawater, and can maintain stable antifouling performance without causing coating film abnormalities such as cracks, in order to alleviate the problem that "initial coating film dissolution can be excessive, or coating film abnormalities such as cracks can occur after a relatively short period of time." The patent document states that "the coating film formed by the antifouling coating composition of the present invention has a stable dissolution rate over the long term, making it possible to more precisely design the coating thickness, and to adjust the amount of paint used so that it is neither too much nor too little for the required antifouling performance (duration)" (paragraphs 0005, 0006, 0009).
[0006] Patent Document 2 describes an antifouling coating composition containing a triorganosilyl ester-containing copolymer, an ester compound, and cuprous oxide (Claim 1, etc.). As the ester compound, Patent Document 2 describes a compound represented by formula (4) R-OOC-X-COO-R (wherein X and R are hydrocarbon groups having 1 to 22 carbon atoms which may contain heteroatoms, and the hydrocarbon groups are aliphatic or aromatic and have a linear, branched, or cyclic structure. The two Rs are the same or different) (Claim 1, etc.). Like the invention described in Patent Document 1, the invention described in Patent Document 2 has an object to provide "an antifouling coating composition which can maintain a stable coating film dissolution rate over a long period of time in seawater, and can maintain stable antifouling performance without causing coating film abnormalities such as cracks, in order to solve the problem that "initial coating film dissolution may be excessively large, or coating film abnormalities such as cracks may occur after a relatively short period of time", and it is described that "according to the present invention, there is provided an antifouling coating composition which can form an antifouling coating film which maintains high antifouling performance over a long period of time" (paragraphs 0005, 0006, 0009).
[0007] The "ester compounds" in Patent Documents 1 and 2 are compounds having a specific structure in the present invention as described below, specifically, compounds having "at least one R 3 There is no disclosure of a dicarboxylic acid ester that satisfies the condition "having [Prior art documents] [Patent documents]
[0008] [Patent Document 1] WO2019 / 069777 [Patent Document 2] WO2019 / 069778 Summary of the Invention [Problem to be solved by the invention]
[0009] The silyl-based antifouling coating film formed from the silyl-based antifouling paint exhibits excellent antifouling properties against marine organisms, but it has been found recently that silyl-based antifouling coating films exposed to the outdoor environment for a long period of time tend to have poor topcoat adhesion. That is, the silyl-based antifouling coating film (undercoat coating film) formed by the pre-coating applied at the block stage is sometimes exposed to the outdoor environment for a fairly long period of time, but it has been found that when the block hull is assembled and the silyl-based antifouling paint is applied as a topcoat (overcoat), the topcoat adhesion is reduced and the coating film (topcoat coating film) formed by the topcoat may partially peel off. Even if the silyl-based antifouling coating film of the topcoat peels off partially, the antifouling properties of the bottom of the ship are exhibited to a certain extent because of the existence of the silyl-based antifouling coating film of the pre-coating, but the partial peeling creates a step in the coating film, which may have a negative effect on the ship's propulsion resistance. Considering the growing interest in reducing greenhouse gas emissions associated with ship navigation in recent years, there is a need to minimize the adverse effect on propulsion resistance that leads to increased fuel consumption, i.e., peeling of the topcoat silyl-based antifouling coating film.
[0010] The present invention aims to provide a silyl-based antifouling paint composition capable of forming a silyl-based antifouling paint film having excellent overcoat adhesion (referred to as "exposure adhesion" in the present invention) to an undercoat antifouling paint film after long-term exposure to an outdoor environment (referred to as "post-exposure antifouling paint film" in the present invention), which is necessary for a total assembly method, etc. Another objective of the present invention is to provide a silyl-based antifouling paint composition capable of forming a silyl-based bar-coat film having excellent overcoat adhesion without decreasing static antifouling property and / or storage stability (preferably both). [Means for solving the problem]
[0011] The present inventors have discovered that by using an antifouling coating film formed from an antifouling paint composition containing a dicarboxylate ester satisfying specific conditions together with a triorganosilyl group-containing copolymer, it is possible to improve exposure adhesion, i.e., adhesion of a topcoat antifouling coating film to an undercoat antifouling coating film after long-term exposure to an outdoor environment, and thereby to solve the above-mentioned problems.
[0012] That is, the present invention includes at least the following: [Section 1] The present invention comprises a triorganosilyl group-containing copolymer (A) and a dicarboxylic acid ester (B) represented by the following general formula (I), An antifouling coating composition, wherein the copolymer (A) has a structural unit derived from a triorganosilyl group-containing monomer (a1) and a structural unit derived from an alkoxyalkyl (meth)acrylate or an aryloxyalkyl (meth)acrylate (a2) and / or an alkyl (meth)acrylate or an aryl (meth)acrylate (a3). R 2 -OOC-R 1 -COO-R 2 …(I) Here, R 1 represents a divalent hydrocarbon group having 2 to 20 carbon atoms, R 2 are each independently a monovalent hydrocarbon group having 1 to 30 carbon atoms, 2 At least one R 3 having R 3 Is -(R 4 O) n - represents R 4 are each independently a divalent hydrocarbon group having 2 to 4 carbon atoms, and n is an integer of 2 or greater. [Section 2] Item 2. The antifouling coating composition according to Item 1, wherein the triorganosilyl group-containing monomer (a1) is triisopropyl methacrylate. [Section 3] 2. The antifouling coating composition according to Item 1, wherein the triorganosilyl group-containing copolymer (A) contains 40 to 80 mass % of structural units derived from the triorganosilyl group-containing monomer (a1). [Section 4] Item 2. The antifouling coating composition according to item 1, wherein the mass ratio [(a1):(a2)] of the structural units derived from the triorganosilyl group-containing monomer (a1) to the structural units derived from the alkoxyalkyl (meth)acrylate or aryloxyalkyl (meth)acrylate (a2) is 55:45 to 90:10. [Section 5] Item 2. The antifouling coating composition according to item 1, wherein the mass ratio [(a1):(a3)] of the structural units derived from the triorganosilyl group-containing monomer (a1) to the structural units derived from the alkyl(meth)acrylate or aryl(meth)acrylate (a3) is 60:40 to 90:10. [Section 6] R 1 Item 2. The antifouling coating composition according to item 1, wherein is a butylene group. [Section 7] R 4 Item 2. The antifouling coating composition according to item 1, wherein is an ethylene group. [Section 8] R 2 Item 2. The antifouling coating composition according to item 1, wherein the compound has a benzyl group. [Section 9] Item 9. An antifouling coating film formed from the antifouling coating composition according to any one of items 1 to 8. [Section 10] Item 10. A substrate with an antifouling coating film, comprising a substrate and the antifouling coating film according to item 9. [Section 11] A method for producing a substrate with an antifouling coating film, comprising the steps of: (1) applying or impregnating a substrate with the antifouling coating composition according to any one of items 1 to 8 to obtain a coated or impregnated body; and (2) drying the coated or impregnated body. Effect of the Invention
[0013] The antifouling coating composition of the present invention can improve the topcoat adhesion (exposure adhesion) to the undercoat antifouling coating film (exposed antifouling coating film) after long-term exposure in an outdoor environment facing the ground, and can also suppress peeling of the topcoat antifouling coating film after immersion in water. Such exposure adhesion is of course excellent when both the undercoat antifouling coating film and the topcoat antifouling coating film are the antifouling coating film of the present invention, but it is also preferable when one of the undercoat antifouling coating film and the topcoat antifouling coating film is the antifouling coating film of the present invention and the other is another antifouling coating film (an antifouling coating film formed from another antifouling paint, for example, another silyl-based antifouling paint), and the antifouling coating composition of the present invention can be adapted to various embodiments requiring exposure adhesion. By improving the exposure adhesion of the antifouling coating film (particularly the silyl-based antifouling coating film) according to the present invention, it is possible to suppress the waste of the antifouling coating composition due to partial peeling and the increase in the propulsion resistance of a moving body such as a ship. In addition, the "exposed adhesion" in the present invention is a performance that is distinguished from the conventional general "topcoat adhesion" that has been evaluated by adhesion to an undercoat antifouling coating film that has not been exposed to an outdoor environment for a long time. In addition, in the conventional general evaluation test of "topcoat adhesion", the test plate is placed facing the "sky side" rather than the "ground side", and under such test conditions, it was not possible to detect the problem of the decrease in topcoat adhesion that occurs when the formed coating film is exposed to an outdoor environment for a long time in a state where it faces the ground side, as in the total assembly method of ships, etc. From this perspective, the present invention can be said to be an invention that has an unexpected and remarkable effect that can solve the previously unsolved problem of the topcoat adhesion of the "exposed antifouling coating film" as described above. In addition, the antifouling coating composition of the present invention can also improve the above-mentioned exposed adhesion without decreasing the static antifouling property and / or storage stability (preferably both). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] As used herein, "(meth)acrylic acid" means "acrylic acid or methacrylic acid" or "acrylic acid and methacrylic acid", depending on the context, and "(meth)acrylate" means "acrylate or methacrylate" or "acrylate and methacrylate", depending on the context.
[0015] In this specification, when a numerical range is described as "N to M," it means "N or more and M or less," and N and M are included in the numerical range. The upper and lower limits (e.g., regarding the content of a component) described in this specification can be arbitrarily combined to set a numerical range.
[0016] In this specification (parts in particular in the examples), the unit "parts" added after a numerical value means "parts by mass" unless otherwise specified. Furthermore, parts by mass of a certain substance relative to 100 parts by mass of a reference substance is synonymous with % by mass of a certain substance relative to 100% by mass of the reference substance.
[0017] -Anti-fouling paint composition- The antifouling coating composition of the present invention contains a triorganosilyl group-containing copolymer (A) and a dicarboxylic acid ester (B) represented by the following general formula (II), wherein the copolymer (A) has a structural unit derived from a triorganosilyl group-containing monomer (a1) and a structural unit derived from an alkoxyalkyl (meth)acrylate or an aryloxyalkyl (meth)acrylate (a2) and / or an alkyl (meth)acrylate or an aryl (meth)acrylate (a3). R 2 -OOC-R 1 -COO-R 2 …(I) Here, R 1 represents a divalent hydrocarbon group having 2 to 20 carbon atoms, R 2 are each independently a monovalent hydrocarbon group having 1 to 30 carbon atoms, 2 R is at least 1 3 having R 3 Is -(R 4 O) n-, R 4 are each independently a divalent hydrocarbon group having 2 to 4 carbon atoms, and n is an integer of 2 or greater.
[0018] <(A) Triorganosilyl Group-Containing Copolymer> The term "triorganosilyl group-containing copolymer" generally refers to a copolymer having a triorganosilyl group in its chemical structure, but the triorganosilyl group-containing copolymer (A) in the present invention refers to a copolymer having (i) a constitutional unit derived from a triorganosilyl group-containing monomer (a1) (sometimes referred to as "monomer (a1)" in this specification) and (ii) a constitutional unit derived from an alkoxyalkyl (meth)acrylate or an aryloxyalkyl (meth)acrylate (a2) (sometimes referred to as "monomer (a2)" in this specification) and / or an alkyl (meth)acrylate or an aryl (meth)acrylate (a3) (sometimes referred to as "monomer (a3)" in this specification). The hydrolyzable polymer (A) may be any one of the above, or may be two or more of the constitutional units derived from the monomer (a1) and the monomer (a2) and / or the monomer (a3) that are different in structure, ratio, etc.
[0019] (a1) Triorganosilyl group-containing monomer The monomer (a1), that is, the triorganosilyl group-containing monomer (a1), is a monomer represented by the following formula (1).
[0020] [ka]
[0021] In formula (1), R 11 represents a hydrogen atom or a methyl group, and R 12 , R 13 and R 14 each independently represents a monovalent hydrocarbon group.
[0022] R 11 From the viewpoint of improving the long-term antifouling property and water resistance of the antifouling coating film, a methyl group is preferred.
[0023] R 12 , R 13 and R 14The "monovalent hydrocarbon group" in R includes linear, branched or cyclic alkyl groups and aryl groups. The alkyl group preferably has 1 to 12 carbon atoms, more preferably 1 to 8, and even more preferably 1 to 4 carbon atoms. The aryl group preferably has 6 to 14 carbon atoms, and more preferably 6 to 10 carbon atoms. From the viewpoint of imparting suitable hydrolysis to the antifouling coating film and improving the long-term antifouling property and water resistance, R 12 , R 13 and R 14 are each preferably independently a methyl group, an ethyl group, an isopropyl group, an n-propyl group, a sec-butyl group, an n-butyl group, or a phenyl group; R 12 , R 13 and R 14 More preferably, all of R are isopropyl, n-propyl, sec-butyl, or n-butyl. 12 , R 13 and R 14 It is more preferable that all of the groups are isopropyl groups.
[0024] That is, as the triorganosilyl group-containing copolymer (a1), trialkylsilyl (meth)acrylate, alkyldiarylsilyl (meth)acrylate, and aryldialkylsilyl (meth)acrylate are preferred, trialkylsilyl (meth)acrylate is more preferred, triisopropylsilyl (meth)acrylate is particularly preferred, and from the viewpoint of improving the water resistance inside the antifouling coating film to be formed, triisopropylsilyl methacrylate is the most preferred.
[0025] The monomer (a1) may be any one kind or may be two or more kinds. That is, the triorganosilyl group-containing copolymer (A) may contain a structural unit derived from any one kind of monomer (a1), or may contain a structural unit derived from two or more kinds of monomers (a1).
[0026] In addition, the structural unit derived from the monomer (a1) becomes the same structure as the structural unit derived from (meth)acrylic acid by hydrolysis. Therefore, in the triorganosilyl group-containing copolymer (A), a part of the structural unit derived from the monomer (a1) may become the same structure as the structural unit derived from (meth)acrylic acid by hydrolysis. In addition, the structural unit generated by hydrolysis may react with other components such as metal oxides contained in the antifouling coating composition to further form a metal ester.
[0027] The total amount of the constituent units derived from the triorganosilyl group-containing monomer (a1) relative to 100% by mass of all constituent units of the triorganosilyl group-containing copolymer (A) is preferably 10 to 90% by mass, more preferably 30 to 80% by mass, even more preferably 40 to 80% by mass, and even more preferably 45 to 75% by mass or less, from the viewpoint of improving the water resistance of the antifouling coating film and obtaining a coating film having an appropriate hydrolysis rate in water.
[0028] (a2) Alkoxyalkyl (meth)acrylate or aryloxyalkyl (meth)acrylate The alkoxyalkyl (meth)acrylate or aryloxyalkyl (meth)acrylate (a2), i.e., the monomer (a2), is a compound represented by the following formula (2): It is generally preferred that the triorganosilyl group-containing copolymer (A) of the present invention has a structural unit derived from the monomer (a2) from the viewpoint that the antifouling coating film formed has good antifouling properties.
[0029] [ka]
[0030] In formula (2), R 21 represents a hydrogen atom or a methyl group, and R 22 represents an alkyl group or an aryl group, and R 23 represents an alkylene group, and s represents an integer of 1 or more and 30 or less.
[0031] R 21From the viewpoint of ease of polymerization, a hydrogen atom is preferred, and from the viewpoint of water resistance of the formed coating film, a methyl group is preferred.
[0032] R 22 From the viewpoints of the stability of the antifouling coating composition and the physical properties of the coating film formed, the "alkyl group" and "aryl group" are preferably linear or branched alkyl groups and aryl groups having 1 to 6 carbon atoms, more preferably linear alkyl groups having 1 to 6 carbon atoms, more preferably alkyl groups having 1 to 4 carbon atoms (e.g., methyl, ethyl, propyl, butyl), and particularly preferably a methyl group.
[0033] R 23 The "alkylene group" is preferably an alkylene group having 2 to 6 carbon atoms, more preferably an alkylene group having 2 to 4 carbon atoms, still more preferably an ethylene group or propylene group, and particularly preferably an ethylene group.
[0034] s is preferably an integer of 1 or more and 15 or less, more preferably an integer of 1 to 6, and even more preferably 1. When s is in such a range, appropriate hydrophilicity is imparted to the coating film formed from the antifouling coating composition containing the triorganosilyl group-containing copolymer (A), and an antifouling coating film having excellent water resistance can be obtained, which is preferable.
[0035] Specific examples of the monomer (a2) include alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 3-methoxy-n-propyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, isobutoxybutyl diglycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, ethoxypolyethylene glycol (meth)acrylate, and butoxypolyethylene glycol (meth)acrylate; and aryloxyalkyl (meth)acrylates such as 2-phenoxyethyl (meth)acrylate and phenoxypolyethylene glycol (meth)acrylate. Among these, 2-methoxyethyl (meth)acrylate is preferred, and 2-methoxyethyl methacrylate is more preferred.
[0036] The monomer (a2) may be any one kind or may be two or more kinds, and may contain both an alkoxyalkyl (meth)acrylate and an aryloxyalkyl (meth)acrylate.
[0037] When the triorganosilyl group-containing copolymer (A) has a structural unit derived from the monomer (a2), the content of the structural unit is preferably 5 to 40 mass%, more preferably 10 to 35 mass%, and even more preferably 15 to 30 mass%, relative to 100 mass% of all structural units of the triorganosilyl group-containing copolymer (A), from the viewpoints of the antifouling performance, water resistance, and hardness of the antifouling coating film.
[0038] (a3) Alkyl (meth)acrylate or aryl (meth)acrylate The alkyl(meth)acrylate or aryl(meth)acrylate (a3), i.e., the monomer (a3), is a compound represented by the following formula (3): It is generally preferred that the triorganosilyl group-containing copolymer (A) of the present invention has a structural unit derived from the monomer (a3) from the viewpoint that the antifouling coating film formed has good coating strength and / or water resistance.
[0039] [ka]
[0040] In formula (3), R 31 represents a hydrogen atom or a methyl group, and R 32 represents an alkyl group or an aryl group.
[0041] R 32 The "alkyl group" and "aryl group" may be linear, branched, or cyclic. The number of carbon atoms in the alkyl group is preferably 1 to 18, more preferably 1 to 8, and even more preferably 1 to 4. The number of carbon atoms in the aryl group is preferably 6 to 14, and more preferably 6 to 10.
[0042] Specific examples of the monomer (a3) include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 3,5,5-trimethylhexyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, and stearyl (meth)acrylate; and aryl (meth)acrylates such as phenyl (meth)acrylate and benzyl (meth)acrylate. Among these, methyl methacrylate is preferred from the viewpoint of obtaining an antifouling coating film having excellent coating film strength and therefore excellent antifouling performance, and butyl acrylate is preferred from the viewpoint of obtaining an antifouling coating film having excellent water resistance and crack resistance. In the present invention, it is also preferred to use methyl methacrylate and butyl acrylate in combination as the monomer (a3).
[0043] The monomer (a3) may be any one kind or may be two or more kinds, and may contain both an alkyl (meth)acrylate and an aryl (meth)acrylate.
[0044] When the triorganosilyl group-containing copolymer (A) has a structural unit derived from the monomer (a3), the content of the structural unit is preferably 0.2 to 40 mass%, more preferably 1 to 35 mass%, and even more preferably 3 to 30 mass%, relative to 100 mass% of all structural units of the triorganosilyl group-containing copolymer (A).
[0045] When the triorganosilyl group-containing copolymer (A) has a structural unit derived from methyl methacrylate as a structural unit derived from the monomer (a3), the content of the structural unit is preferably 0.5 to 40 mass%, more preferably 1 to 35 mass%, and even more preferably 3 to 30 mass%, relative to 100 mass% of all structural units of the triorganosilyl group-containing copolymer (A).
[0046] When the triorganosilyl group-containing copolymer (A) has a structural unit derived from butyl acrylate as a structural unit derived from the monomer (a3), the content of the structural unit is preferably 0.2 to 20 mass%, more preferably 1 to 15 mass%, and even more preferably 3 to 10 mass%, relative to 100 mass% of all structural units of the triorganosilyl group-containing copolymer (A).
[0047] (a4) Other monomers The triorganosilyl group-containing copolymer (A) of the present invention may further contain, as necessary, a constituent unit derived from a monomer other than the triorganosilyl group-containing monomer (a1), the alkoxyalkyl (meth)acrylate or aryloxyalkyl (meth)acrylate (a2), and the alkyl (meth)acrylate or aryl (meth)acrylate (a3) that is copolymerizable with the triorganosilyl group-containing monomer (a1) (sometimes referred to as "other monomer (a4)" in this specification).
[0048] Examples of the other monomers (a4) include organosiloxane-containing monomers (a41) (sometimes referred to as "monomer (a41)" in this specification); hydroxyalkyl (meth)acrylates (a42) (sometimes referred to as "monomer (a42)" in this specification); glycidyl (meth)acrylates (a43) (sometimes referred to as "monomer (a43)" in this specification); unsaturated carboxylic acids (a44) (sometimes referred to as "monomer (a44)" in this specification); metal ester group-containing unsaturated monomers (a45) (sometimes referred to as "monomer (a45)" in this specification); and other vinyl compounds (a46) (sometimes referred to as "monomer (a46)" in this specification).
[0049] Among these, from the viewpoint of providing an antifouling coating film having good antifouling properties, organosiloxane-containing monomers (a41) are preferred, and from the viewpoint of improving the retention of aesthetic appearance over time when applied to an old coating film and the crack resistance of the antifouling coating film after immersion in seawater, unsaturated carboxylic acids (a44) are preferred.
[0050] The other monomer (a4) may be any one kind or may be two or more kinds. That is, the triorganosilyl group-containing copolymer (A) may have a structural unit derived from any one kind of other monomer (a4), or may contain structural units derived from two or more kinds of other monomers (a4). The triorganosilyl group-containing copolymer (A) preferably has a structural unit derived from at least one kind selected from the group consisting of monomers (a41), (a42), (a43), (a44), (a45) and (a46), and more preferably has structural units derived from at least monomers (a2) and (a3).
[0051] (a41) Organosiloxane-containing monomer The monomer (a41), that is, the organosiloxane-containing monomer (a41), is a monomer represented by the following formula (41): The monomer (a41) may be any one type or two or more types.
[0052] [ka]
[0053] In formula (41), R 411 , R 412 and R 413 each independently represents a monovalent hydrocarbon group, each X independently represents a (meth)acryloyloxyalkyl group or a mercaptoalkyl group, m is 1 or greater, n is 0 or greater, p and q are each independently 0 or 1, and n+p+q is 1 or greater.
[0054] R 411 , R 412 and R 413 Examples of the hydrocarbon group in R include a linear, branched or cyclic alkyl group and an aryl group. The number of carbon atoms in the alkyl group is preferably 1 to 12, more preferably 1 to 8, and further preferably 1 to 4. The number of carbon atoms in the aryl group is preferably 6 to 14, and more preferably 6 to 10. From the viewpoint of ease of polymerization, R 411 , R 412 and R 413 are each independently preferably an alkyl group such as a methyl group or a butyl group.
[0055] Examples of X include (meth)acryloyloxyalkyl groups such as (meth)acryloyloxyethyl group, (meth)acryloyloxypropyl group, and (meth)acryloyloxybutyl group; and mercaptoalkyl groups such as mercaptomethyl group, mercaptoethyl group, mercaptopropyl group, and mercaptobutyl group. From the viewpoint of uniform polymerization progress, X is preferably a (meth)acryloyloxyalkyl group, and from the viewpoint of reducing the viscosity of the hydrolyzable polymer (A) and making it easy to handle, it is preferably a mercaptoalkyl group. The "alkyl" in the "(meth)acryloyloxyalkyl group" and the "alkyl" in the "mercaptoalkyl group" may each be linear or branched, and from the viewpoint of reactivity, the number of carbon atoms is preferably 1 to 12, more preferably 2 to 6, and even more preferably 2 to 4.
[0056] m and n are (SiR 412 2O), (SiXR 413 O). m+n is preferably 2 or more. In other words, the organosiloxane-containing monomer (a41) is preferably a polyorganosiloxane block-containing monomer.
[0057] In this specification, when two or more different repeating units are listed in parallel between brackets [ ] as in formula (41), it means that the repeating units may be repeated in any order, such as random, alternating, or block. That is, for example, in the formula -[Y3-Z3]- (where Y and Z each represent a repeating unit), the repeating units may be random, such as -YYZYZZ-, alternating, such as -YZYZYZ-, or block, such as -YYYZZZ- or -ZZZYYY-.
[0058] A first embodiment of the monomer (a41) is a monomer (a411) in which n is 0, p is 1, and q is 0. It is preferable that the triorganosilyl group-containing copolymer (A) contains a structural unit derived from such a monomer (a411), for example, because the antifouling coating composition is likely to form an antifouling coating film having excellent antifouling properties. From the viewpoint of ease of polymerization, etc., m in the monomer (a41) is preferably 3 or more, more preferably 5 or more, and is preferably 200 or less, more preferably 70 or less.
[0059] Examples of the monomer (a411) include commercially available products "FM-0711" (single-terminated methacryloyloxyalkyl-modified organopolysiloxane, number average molecular weight: 1,000), "FM-0721" (single-terminated methacryloyloxyalkyl-modified organopolysiloxane, number average molecular weight: 5,000), and "FM-0725" (single-terminated methacryloyloxyalkyl-modified organopolysiloxane, number average molecular weight: 10,000) manufactured by JNC Corporation; Examples of commercially available products that can be used include "X-22-174ASX" (single-terminated methacryloyloxyalkyl-modified organopolysiloxane, functional group equivalent: 900 g / mol), "KF-2012" (single-terminated methacryloyloxyalkyl-modified organopolysiloxane, functional group equivalent: 4,600 g / mol), and X-22-2426 (single-terminated methacryloyloxyalkyl-modified organopolysiloxane, functional group equivalent: 12,000 g / mol) manufactured by Polysiloxane Corporation.
[0060] A second embodiment of the monomer (a41) is a monomer (a412) in which n is 0 and p and q are 1. It is preferable that the triorganosilyl group-containing copolymer (A) contains a structural unit derived from such a monomer (a412), for example, because the antifouling coating composition has excellent repairability, that is, excellent adhesion to the old antifouling coating film after use (after immersion in seawater) and is easy to form an antifouling coating film. From the viewpoint of ease of polymerization, etc., m in the monomer (a412) is preferably 3 or more, more preferably 5 or more, and preferably 200 or less, more preferably 70 or less.
[0061] Examples of the monomer (a412) include commercially available products "FM-7711" (both terminally methacryloyloxyalkyl-modified organopolysiloxane, number average molecular weight: 1,000), "FM-7721" (both terminally methacryloyloxyalkyl-modified organopolysiloxane, number average molecular weight: 5,000), and "FM-7725" (both terminally methacryloyloxyalkyl-modified organopolysiloxane, number average molecular weight: 10,000) manufactured by JNC Corporation; and commercially available products "X-22-164" (both terminally methacryloyloxyalkyl-modified organopolysiloxane, functional group equivalent: 190 g / mol) and "X-22-164AS" (both terminally methacryloyloxyalkyl-modified organopolysiloxane, functional group equivalent: 4 50g / mol), "X-22-164A" (both terminal methacryloyloxyalkyl modified organopolysiloxane, functional group equivalent: 860g / mol), "X-22-164B" (both terminal methacryloyloxyalkyl modified organopolysiloxane, functional group equivalent: 1630g / mol), "X-22-164C" (both terminal methacryloyloxyalkyl modified organopolysiloxane, functional group equivalent: 2,370g / mol), "X-22-164E" (both terminal methacryloyloxyalkyl modified organopolysiloxane, functional group equivalent: 3,900g / mol), "X-22-167B" (both terminal mercaptoalkyl modified organopolysiloxane, functional group equivalent: 1,670g / mol), etc. can be used.
[0062] A third embodiment of the monomer (a41) is a monomer (a413) in which n is 1 or more. It is preferable that the triorganosilyl group-containing copolymer (A) contains a structural unit derived from such a monomer (a413), for example, because the viscosity of the antifouling coating composition tends to decrease and the handling tends to become easier. In the monomer (a413), m is preferably 50 to 1,000, and n is preferably 1 to 30.
[0063] As the monomer (a413), for example, commercially available products "KF-2001" (side chain mercaptoalkyl-modified organopolysiloxane, functional group equivalent: 1,900 g / mol) and "KF-2004" (side chain mercaptoalkyl-modified organopolysiloxane, functional group equivalent: 30,000 g / mol) manufactured by Shin-Etsu Chemical Co., Ltd. can be used.
[0064] When the triorganosilyl group-containing copolymer (A) has a structural unit derived from an organosiloxane-containing monomer (a41), the content of the structural unit is preferably 0.5 to 50 mass%, more preferably 1 to 30 mass%, and even more preferably 1.5 to 15 mass%, relative to 100 mass% of all structural units of the triorganosilyl group-containing copolymer (A), from the viewpoints of the antifouling performance, water resistance, and adhesion to substrates under alternating dry and wet conditions of the antifouling coating film.
[0065] (a42) Hydroxyalkyl (meth)acrylate Specific examples of the monomer (a42), that is, the hydroxyalkyl (meth)acrylate, include hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate.
[0066] The monomer (a42) may be any one kind or may be two or more kinds.
[0067] When the triorganosilyl group-containing copolymer (A) has a structural unit derived from a monomer (a42), the content of the structural unit is preferably 0.5 to 30 mass%, more preferably 1 to 20 mass%, and even more preferably 2 to 15 mass%, relative to 100 mass% of all structural units of the triorganosilyl group-containing copolymer (A).
[0068] (a43) Glycidyl (meth)acrylate The monomer (a43), that is, glycidyl (meth)acrylate, may be any one kind or may be two or more kinds.
[0069] When the triorganosilyl group-containing copolymer (A) has a structural unit derived from the monomer (a43), the content of the structural unit is preferably 0.5 to 30 mass%, more preferably 1 to 20 mass%, and even more preferably 2 to 15 mass%, relative to 100 mass% of all structural units of the triorganosilyl group-containing copolymer (A).
[0070] (a44) Unsaturated carboxylic acids Specific examples of the monomer (a44), that is, the unsaturated carboxylic acid, include (meth)acrylic acid, (meth)acryloyloxyalkylsuccinic acid, (meth)acryloyloxyalkylphthalic acid, (meth)acryloyloxyalkylhexahydrophthalic acid, itaconic acid, maleic acid, maleic anhydride, itaconic acid, crotonic acid, and 6-acrylamide hexanoic acid. From the viewpoints of ease of handling and availability of the compound, and the viscosity of the polymer obtained by polymerization, (meth)acrylic acid is preferred.
[0071] The monomer (a44) may be any one kind or may be two or more kinds.
[0072] When the triorganosilyl group-containing copolymer (A) has a structural unit derived from a monomer (a44), the content of the structural unit is preferably 0.01 to 20 mass%, more preferably 0.1 to 10 mass%, relative to 100 mass% of all structural units of the triorganosilyl group-containing copolymer (A).
[0073] (a45) Metal ester group-containing unsaturated monomer The metal ester group-containing unsaturated monomer is generally a collective term for monomers having a metal ester group in the chemical structure formed by bonding a metal with a carboxylic acid, but the metal ester group-containing unsaturated monomer (a45) in the present invention refers to a monomer represented by the following formula (45).
[0074] [ka]
[0075] In formula (45), M represents a divalent metal atom, R 451 represents a monovalent organic group containing a terminal ethylenically unsaturated group (CH2=C<) (referred to as a "terminally ethylenically unsaturated organic group" in this specification), and R 452 represents a monovalent group containing a terminal ethylenically unsaturated group (CH2=C<) (terminally ethylenically unsaturated organic group), or a monovalent organic group having 1 to 30 carbon atoms that does not contain a terminal ethylenically unsaturated group (referred to as a "non-terminal ethylenically unsaturated organic group" in this specification).
[0076] Specific examples of the divalent metal atom of M include copper, zinc, magnesium, calcium, neodymium, titanium, zirconium, iron, ruthenium, cobalt, nickel, and aluminum. Among these divalent metal atoms, copper, zinc, and nickel are preferred, and copper and zinc are more preferred.
[0077] R 451 and R 452 The terminal ethylenically unsaturated organic group preferably has 2 to 50 carbon atoms, more preferably 2 to 30 carbon atoms, even more preferably 2 to 10 carbon atoms, still more preferably 2 to 6 carbon atoms, and particularly preferably 2 to 3 carbon atoms.
[0078] The terminal ethylenically unsaturated group may further contain an ethylenically unsaturated group in addition to the terminal, but preferably contains an ethylenically unsaturated group only at the terminal.
[0079] R 452 In the above, examples of the non-terminal ethylenically unsaturated organic group include an aliphatic hydrocarbon group having 1 to 30 carbon atoms, which may be linear or branched; an alicyclic hydrocarbon group having 3 to 30 carbon atoms, which may be saturated or unsaturated alicyclic; and an aromatic hydrocarbon group having 6 to 30 carbon atoms. The non-terminal ethylenically unsaturated organic group may further contain a substituent (for example, a hydrogen group).
[0080] R 452is preferably an organic acid residue derived from a monobasic acid, and specific examples thereof include groups obtained by removing a carboxy group from organic acids such as versatic acid, palmitic acid, stearic acid, isostearic acid, oleic acid, linoleic acid, linolenic acid, abietic acid, neoabietic acid, pimaric acid, dehydroabietic acid, 12-hydroxystearic acid, and naphthenic acid, and among these, groups obtained by removing a carboxy group from abietic acid, versatic acid, or naphthenic acid are preferred, and groups obtained by removing a carboxy group from abietic acid or versatic acid are more preferred. Versatic acid is a general term for a mixture of highly branched carboxylic acids having 9 to 11 carbon atoms, mainly 10 carbon atoms.
[0081] In the monomer (a45), M represents a divalent metal atom, and R 451 and R 452 and R 1 and R 2 each represent a terminal ethylenically unsaturated organic group, specific examples of which include zinc diacrylate, zinc dimethacrylate, zinc acrylate methacrylate, zinc di(3-acryloyloxypropionate), zinc di(3-methacryloyloxypropionate), zinc di(3-(meth)acryloyloxy-2-methylpropionate), copper diacrylate, copper dimethacrylate, copper acrylate methacrylate, copper di(3-acryloyloxypropionate), copper di(3-methacryloyloxypropionate), and copper di(3-(meth)acryloyloxy-2-methylpropionate).
[0082] In the monomer (a45), M represents a divalent metal atom, and R 451 represents a terminal ethylenically unsaturated organic group, and R 452Specific examples of those in which represents a non-terminal ethylenically unsaturated organic group include rosin zinc 3-(meth)acryloyloxypropionate, zinc versatate 3-(meth)acryloyloxypropionate, zinc (meth)acrylic acid rosin, zinc (meth)acrylic acid versatate, zinc (meth)acrylic acid naphthenate, rosin copper 3-(meth)acryloyloxypropionate, copper versatate 3-(meth)acryloyloxypropionate, rosin copper (meth)acrylate, copper (meth)acrylic acid versatate, and copper (meth)acrylic acid naphthenate.
[0083] The monomer (a45) may be any one kind or may be two or more kinds.
[0084] When the triorganosilyl group-containing copolymer (A) has a structural unit derived from the monomer (a45), the content of the structural unit is preferably 0.5 to 30 mass%, more preferably 1 to 20 mass%, and even more preferably 2 to 15 mass%, relative to 100 mass% of all structural units of the triorganosilyl group-containing copolymer (A).
[0085] (a46) Other vinyl compounds Specific examples of the monomer (a46), that is, the other vinyl compounds (a46), include styrene, α-methylstyrene, vinyl acetate, vinyl benzoate, vinyltoluene, acrylonitrile, vinylpyridine, vinylpyrrolidone, and vinyl chloride.
[0086] The monomer (a46) may be any one kind or may be two or more kinds.
[0087] Ratio of constituent units The ratio of the constituent units derived from monomer (a1), i.e., the triorganosilyl group-containing monomer (a1), contained in the triorganosilyl group-containing copolymer (A), to the constituent units derived from monomer (a2), i.e., the alkoxyalkyl (meth)acrylate or aryloxyalkyl (meth)acrylate (a2), and / or the ratio of the constituent units derived from monomer (a3), i.e., the alkyl (meth)acrylate or aryl (meth)acrylate (a3), can be appropriately adjusted taking into consideration the type of each monomer, the effects of the present invention, other technical matters, etc.
[0088] The mass ratio of the structural units derived from monomer (a1) to the structural units derived from monomer (a2) [(a1):(a2)] is preferably 55:45 to 90:10, and more preferably 60:40 to 80:20. In other words, when the total of the structural units derived from monomer (a1) and the structural units derived from monomer (a2) is taken as 100% by mass, the structural units derived from monomer (a1) are preferably 55 to 90% by mass, and more preferably 60 to 80% by mass, and the structural units derived from monomer (a2) are the remainder of each.
[0089] The mass ratio of the structural units derived from monomer (a1) to the structural units derived from monomer (a3) [(a1):(a3)] is preferably 60:40 to 90:10, and more preferably 65:35 to 88:12. In other words, when the total of the structural units derived from monomer (a1) and the structural units derived from monomer (a3) is taken as 100% by mass, the structural units derived from monomer (a1) are preferably 60 to 90% by mass, and more preferably 65 to 88% by mass, and the structural units derived from monomer (a3) are the remainder of each.
[0090] The content (mass) ratio of the constituent units derived from each monomer in the triorganosilyl group-containing copolymer (A) can be regarded as the same as the charge amount (mass) ratio of each monomer (reaction raw material) used in the polymerization reaction when the hydrolysis of the triorganosilyl group-containing copolymer (A) is sufficiently suppressed, for example, immediately after the polymerization of the triorganosilyl group-containing copolymer (A) or when the storage period of the coating composition using it is short. Note that the total constituent units in the triorganosilyl group-containing copolymer (A) do not include the constituent units derived from the polymerization initiator and the chain transfer agent.
[0091] The content of each monomer can also be determined by analyzing the obtained triorganosilyl group-containing copolymer (A) or the triorganosilyl group-containing copolymer (A) isolated from the coating composition. Specific analytical methods include gas chromatography mass spectrometry (GC-MS), infrared spectroscopy (IR), magnetic resonance spectroscopy (NMR), inductively coupled plasma mass spectrometry (ICP-MS), and inductively coupled plasma atomic emission spectrometry (ICP-AES) using the triorganosilyl group-containing copolymer (A) or its decomposition products as samples.
[0092] Number average molecular weight (Mn) and weight average molecular weight (Mw) The number average molecular weight (Mn) and weight average molecular weight (Mw) of the triorganosilyl group-containing copolymer (A) can be appropriately adjusted so that the degree of the effect of the present invention is desired, and taking into consideration the viscosity and storage stability of the obtained antifouling coating composition, the coating wear rate (dissolution rate, renewal ability) of the obtained antifouling coating film, etc. The Mn of the triorganosilyl group-containing copolymer (A) is preferably 1,000 or more, more preferably 1,500 or more, and also preferably 50,000 or less, more preferably 30,000 or less, particularly preferably 15,000 or less. The Mw of the hydrolyzable polymer (A) is preferably 2,000 or more, more preferably 3,000 or more, and also preferably 50,000 or less, more preferably 40,000 or less.
[0093] Mn and Mw can be measured by gel permeation chromatography according to a conventional method and converted into standard polystyrene. For example, more specific measurement methods and conditions for Mw can be found in the Examples described below, and measurement methods and conditions similar thereto can be applied to Mw.
[0094] Content of component (A) The content of the triorganosilyl group-containing copolymer (A) can be appropriately adjusted depending on the type and characteristics of the component, so that the effects of the present invention, particularly the adhesion upon exposure, are at a desired level, and also taking into consideration other technical matters of the obtained antifouling coating composition (e.g., coating workability). The content of the triorganosilyl group-containing copolymer (A) is, for example, preferably 10% by mass or more, more preferably 12% by mass or more, and preferably 40% by mass or less, more preferably 30% by mass or less, based on 100% by mass of the solid content of the antifouling coating composition.
[0095] In this specification, the "solid content" of the antifouling coating composition of the present invention or each component contained therein (for example, a solution containing component (A), an oxidized polyethylene wax as an anti-sagging agent / anti-settling agent (F), a fatty acid amide wax, etc.) refers to the components excluding the volatile components contained as a solvent in the antifouling coating composition of the present invention or each component. Such a solid content can be calculated according to a conventional method as the ratio of the mass of the substance obtained by drying the antifouling coating composition of the present invention or each component in a hot air dryer at 125°C for 3 hours to the mass of the antifouling coating composition of the present invention or each component. More specifically, according to JIS K 5601-1-2:2008, 1±0.1 g of the measurement target is weighed out on a flat-bottomed dish, spread evenly on the bottom surface using a wire of known mass, dried at 125°C for 1 hour at 1 atmospheric pressure, and the mass of the wire is subtracted from the obtained heating residue to obtain a mass percentage value.
[0096] When the solid content of each component is indicated on a label, catalog, etc., that value can be regarded as the solid content of that component. When the composition of the antifouling coating composition of the present invention (the type and amount of each component, and the solid content of each component) is known by the above-mentioned measurement method, a value calculated based on that composition can be regarded as the solid content of the antifouling coating composition of the present invention.
[0097] <(B) Dicarboxylic acid ester> Dicarboxylate is generally a general term for a compound in which two carboxy groups in the chemical structure are both esterified. In the present invention, the dicarboxylate (B) is represented by the general formula (I): R 2 -OOC-R 1 -COO-R 2 (I) (wherein, R 1 represents a divalent hydrocarbon group having 2 to 20 carbon atoms, R 2 are each independently a monovalent hydrocarbon group having 1 to 30 carbon atoms, 2 At least one R 3 R 3 Is -(R 4 O) n - represents R 4 are each independently a divalent hydrocarbon group having 2 to 4 carbon atoms, and n is an integer of 2 or more. 2 The carbon number of R 2 R in the structure of 3 (Furthermore, R in the structure 4 ) is also included. 2 As is clear from the above, the "hydrocarbon group" of R 3 :-(R 4 O) n It may contain an oxygen atom derived from the - structure in its skeleton (main chain).
[0098] R 1 The "divalent hydrocarbon group having 2 to 20 carbon atoms" may have any of a linear, branched, or cyclic structure, or may be a combination of these structures. 1The "divalent hydrocarbon group having 2 to 20 carbon atoms" (each of the above structures) of R may be a saturated or unsaturated aliphatic hydrocarbon group, or may be an aromatic hydrocarbon group. The number of carbon atoms in the linear hydrocarbon group is preferably 2 to 12, more preferably 2 to 8, and even more preferably 2 to 4. The number of carbon atoms in the branched hydrocarbon group is preferably 3 to 12, more preferably 3 to 8, and even more preferably 3 to 4. The number of carbon atoms in the cyclic hydrocarbon group is preferably 6 to 14, and more preferably 6 to 10. From the viewpoint of imparting excellent exposure adhesion and other good performance to the antifouling coating film, R 1 The "divalent hydrocarbon group having 2 to 20 carbon atoms" is preferably a linear or branched alkylene group (divalent saturated aliphatic hydrocarbon group) having 1 to 12 carbon atoms, more preferably a linear alkylene group having 1 to 8 carbon atoms. For example, an n-butylene group (having 4 carbon atoms) can be represented by R 1 is one of the particularly preferred "divalent hydrocarbon groups having 2 to 20 carbon atoms".
[0099] R 2 The "monovalent hydrocarbon group having 1 to 30 carbon atoms" may have any of a linear, branched, or cyclic structure, or may be a combination of these structures. 2 The "monovalent hydrocarbon group having 1 to 30 carbon atoms" (each of the above structures) of R may be a saturated or unsaturated aliphatic hydrocarbon group, or may be an aromatic hydrocarbon group. The number of carbon atoms in the linear or branched hydrocarbon group is preferably 3 to 20, more preferably 4 to 15, and even more preferably 5 to 10. The number of carbon atoms in the cyclic hydrocarbon group is preferably 6 to 14, and more preferably 6 to 10. From the viewpoint of imparting excellent exposure adhesion and other good performance to the antifouling coating film, R 2 The "monovalent hydrocarbon group having 1 to 30 carbon atoms" is preferably R 3 and preferably a linear or branched monovalent hydrocarbon group having 3 to 20 carbon atoms, which may contain an oxygen atom derived from 3 For example, a benzyl group (7 carbon atoms) is a linear monovalent hydrocarbon group having 5 to 10 carbon atoms, which may contain an oxygen atom derived from R 2is one of the particularly preferred "monovalent hydrocarbon groups having 1 to 30 carbon atoms".
[0100] R 2 "At least one R 3 " may be present at the terminal on the ester bond (carboxy group) side in the "monovalent hydrocarbon group having 1 to 30 carbon atoms", or at the terminal opposite thereto, or in the region between those terminals. "At least one" refers to two R 2 R in 3 The total number of R is at least one. 2 One (or more) R 3 and the other R 2 R 3 Even in an embodiment not having the above formula (I), the dicarboxylic acid ester (B) of the present invention satisfies the conditions of formula (I).
[0101] R 3 , i.e. -(R 4 O) n - In R 4 The divalent hydrocarbon groups having 2, 3, and 4 carbon atoms are ethylene, propylene, and butylene groups, respectively, and (R 4 O) are divalent groups derived from ethylene glycol, propylene glycol, and butylene glycol, respectively. For example, R 4 is an ethylene group (carbon number 2), that is, R 3 As -(CH2CH2O) n -, a divalent group derived from ethylene glycol (the number of repeating units is n), 2 is one of the particularly preferred ones.
[0102] Specific examples of the dicarboxylate ester (B) include diesters derived from adipic acid (HOOC-(CH2)4-COOH). Specific examples of the diesters derived from adipic acid include benzyl-diethylene glycol monomethyl adipate represented by the following formula (I-1) and bis[2-(2-butoxyethoxy)ethyl] adipate represented by the following formula (I-2).
[0103] [ka]
[0104] The content of the dicarboxylate (B) can be appropriately adjusted depending on the type and characteristics of the component so that the effects of the present invention, particularly the adhesion upon exposure, are at a desired level, and also taking into consideration other technical matters of the obtained antifouling coating composition (e.g., coating workability). The content of the dicarboxylate (B) is, for example, preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, and preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, relative to 100% by mass of the solid content of the antifouling coating composition.
[0105] <Optional ingredients> The antifouling coating composition of the present invention may further contain components other than the triorganosilyl group-containing copolymer (A) and the dicarboxylate (B) as necessary. Examples of such optional components include antifouling agents (C), pigments (D), monocarboxylic acid compounds (E) and / or their metal esters, antisagging agents / antisettling agents (F), dehydrating agents (G), solvents (H), plasticizers (I), defoamers (J), and binder components (K) (also referred to as components (C) to (K) in this specification). These optional components are not essential for achieving the effects of the present invention, but may be components that are naturally required or commonly used for implementing (producing, using, etc.) the antifouling coating composition, components that can facilitate or enhance the effects of the present invention, or components that can achieve effects other than those of the present invention. Furthermore, if desired, other components used in general antifouling coating compositions may be included as components of the antifouling coating composition of the present invention.
[0106] <(C) Antifouling agent> The antifouling coating composition of the present invention can exhibit a certain level of excellent antifouling performance even without containing the antifouling agent (C), but may contain the antifouling agent (C) as necessary. Examples of the antifouling agent (C) include cuprous oxide, metal pyrithiones (e.g., copper pyrithione, zinc pyrithione), (+ / -) 4-[1-(2,3-dimethylphenyl)ethyl]-1H-imidazole (also known as medetomidine), 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitrile (also known as tralopyril), 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one (also known as DCOIT), pyridinetriphenylborane, 4-isopropylpyridinediphenylmethylborane, N,N-dimethyl-N'-(3,4-dichlorophenyl)urea (also known as diuron), N-(2,4,6-trichlorophenyl)maleimide, and 2,4,5,6-tetrachloroisophthalnitrile. , 2-methylthio-4-tert-butylamino-6-cyclopropylamino-1,3,5-triazine (also known as Sibutrin), bisdimethyldithiocarbamoyl zinc ethylene bisdithiocarbamate (also known as polycarbamate), chloromethyl-n-octyl disulfide, N,N'-dimethyl-N'-phenyl-(N-fluorodichloromethylthio)sulfamide (also known as dichlofluanid), tetraalkyl thiuram disulfide (also known as TMTD), zinc dimethyl dithiocarbamate (also known as ziram), zinc ethylene bisdithiocarbamate, 2,3-dichloro-N-(2',6'-diethylphenyl)maleimide, 2,3-dichloro-N-(2'-ethyl-6'-methylphenyl)maleimide, etc. Antifouling agent (C) may be used alone or in combination of two or more. For example, cuprous oxide, metal pyrithione, medetomidine, tralopyril, and DCOIT are preferred as antifouling agents (C).
[0107] When the antifouling coating composition of the present invention contains an antifouling agent (C), its content can be appropriately adjusted depending on the purpose (antifouling performance) and the type of the component, and the like. For example, the content is preferably 10 to 80 mass% and more preferably 20 to 70% for cuprous oxide, 0.1 to 15 mass% and more preferably 0.5 to 8 mass% for metal pyrithiones, preferably 0.01 to 1 mass% and more preferably 0.03 to 0.5 mass% for medetomidine, preferably 0.5 to 10 mass% and more preferably 3 to 7 mass% for tralopyril, and preferably 0.1 to 8 mass% and more preferably 0.5 to 5 mass% for DCOIT, relative to 100 mass% solids of the composition.
[0108] <(D) Pigment> The antifouling coating composition of the present invention may contain a pigment (D) for the purposes of coloring the coating film and concealing the base, and / or for the purpose of adjusting the coating film strength to an appropriate level.
[0109] Examples of the pigment (D) include extender pigments such as zinc oxide, zinc phosphate, talc, mica, clay, potassium feldspar, calcium carbonate, kaolin, alumina white, white carbon, aluminum hydroxide, magnesium carbonate, barium carbonate, barium sulfate (e.g., precipitated barium sulfate), calcium sulfate (e.g., gypsum), and zinc sulfide; and color pigments such as red iron oxide (red iron oxide), titanium white (titanium oxide), yellow iron oxide, carbon black, naphthol red, and phthalocyanine blue. The pigment (D) may be used alone or in combination of two or more kinds.
[0110] When the antifouling coating composition of the present invention contains a pigment (D), the content thereof can be appropriately adjusted depending on the purpose and the type of the component, and is, for example, preferably 0.5 to 40 mass % relative to 100 mass % of the solid content of the composition.
[0111] <(E) Monocarboxylic acid compound> The antifouling coating composition of the present invention can contain a monocarboxylic acid compound (E) and / or a metal ester thereof for the purpose of improving the renewal property of the antifouling coating film formed from the surface in water, promoting the release of an antifouling agent (C) into water to improve the antifouling property when the antifouling coating film contains the agent, and further imparting appropriate water resistance to the antifouling coating film. The monocarboxylic acid compound (E) and / or a metal ester thereof may be used alone or in combination of two or more.
[0112] Examples of the monocarboxylic acid compound (E) include versatic acid, palmitic acid, stearic acid, isostearic acid, rosin, naphthenic acid, and salicylic acid. The monocarboxylic acid compound (E) may be used alone or in combination of two or more. For example, versatic acid and rosin are preferred as the monocarboxylic acid compound (E).
[0113] The monocarboxylic acid compound (E) may form a metal ester (e.g., copper ester). The metal ester may be formed in advance before the production of the antifouling coating composition, or may be formed by reaction with other coating components during the production of the antifouling coating composition.
[0114] Versatic acid is a mixture containing branched alkyl carboxylic acids with 5 to 15 carbon atoms, mainly 9 to 11, and especially 10 carbon atoms. Rosin (rosins such as gum rosin, wood rosin, tall oil rosin, and rosin derivatives such as hydrogenated rosin and disproportionated rosin) is a mixture of abietic acid and its isomers, which have three ring structures containing conjugated double bonds and a carboxyl group. Naphthenic acid, salicylic acid, and the like are also compounds with a ring structure and a carboxyl group.
[0115] When the antifouling coating composition of the present invention contains a monocarboxylic acid compound (E) and / or a metal ester thereof, the content thereof can be appropriately adjusted in consideration of the effects of the present invention, depending on the type and properties of the component, etc. The content of the monocarboxylic acid compound (E) and / or a metal ester thereof is preferably 0.1 mass% or more, more preferably 0.2 mass% or more, and is preferably 15 mass% or less, more preferably 10 mass% or less, based on 100 mass% of the solid content of the antifouling coating composition.
[0116] <(F) Anti-sagging and anti-settling agents> The antifouling coating composition of the present invention may contain an anti-sagging agent / anti-settling agent (F) for the purpose of adjusting the viscosity of the composition, etc. The anti-sagging agent / anti-settling agent (F) may be used alone or in combination of two or more kinds.
[0117] Examples of the sagging and settling prevention agent (F) include organic clay waxes (e.g., stearate salts, lecithin salts, and alkylsulfonates of Al, Ca, and Zn), organic waxes (e.g., polyethylene wax, oxidized polyethylene wax, fatty acid amide wax, and hydrogenated castor oil wax), mixtures of organic clay waxes and organic waxes, and synthetic fine silica. Examples of such sagging and settling prevention agents (F) that can be used include commercially available products such as "Disparlon 305," "Disparlon 4200-20," "Disparlon A630-20X," and "Disparlon 6900-20X" manufactured by Kusumoto Chemicals Co., Ltd.; and "ASA D-120" manufactured by Ito Oil Mills Co., Ltd.
[0118] When the antifouling coating composition of the present invention contains an anti-sagging agent / anti-settling agent (F), the content thereof can be appropriately adjusted depending on the purpose, the type of the component, etc., and is, for example, preferably 0.01 mass % or more, more preferably 0.1 mass % or more, and preferably 10 mass % or less, more preferably 3 mass % or less, based on 100 mass % of the solid content of the composition.
[0119] <(G) Dehydrating Agent> The antifouling coating composition of the present invention may contain a dehydrating agent (G) for the purpose of improving the storage stability of the composition, etc. The dehydrating agent (G) may be used alone or in combination of two or more kinds.
[0120] Examples of the dehydrating agent (G) include alkoxysilanes such as ethyl silicate and propyl silicate; zeolites commonly known as "molecular sieves; porous alumina; orthoesters such as orthoformic acid alkyl esters; orthoboric acid; and isocyanates. Among these, alkoxysilanes are preferred from the viewpoints of availability and improved storage stability.
[0121] When the antifouling coating composition of the present invention contains a dehydrating agent (G), the content thereof can be appropriately adjusted depending on the purpose, the type of the component, and the like. For example, the content is preferably 0.1 mass % or more, more preferably 0.2 mass % or more, and is preferably 10 mass % or less, more preferably 2.5 mass % or less, relative to 100 mass % of the solid content of the composition.
[0122] <(H) Solvent> The antifouling coating composition of the present invention may contain a solvent (H) such as water or an organic solvent for the purpose of adjusting the viscosity of the composition. The antifouling coating composition of the present invention can be prepared using a liquid containing the triorganosilyl group-containing copolymer (A) obtained when synthesizing the triorganosilyl group-containing copolymer (A). In this case, the solvent contained in the liquid, or a solvent added separately when mixing the triorganosilyl group-containing copolymer (A) with the dicarboxylic acid ester (B) and optional components as necessary, corresponds to the solvent (H). The solvent (H) may be any one type or two or more types. As the solvent (H), an organic solvent is preferable.
[0123] Examples of the organic solvent include aromatic organic solvents such as xylene, toluene, and ethylbenzene; ketones such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; aliphatic monohydric alcohols (having 1 to 10 carbon atoms, preferably about 2 to 5 carbon atoms) such as ethanol, isopropyl alcohol, n-butanol, isobutanol, and propylene glycol monomethyl ether; and ester solvents such as ethyl acetate and butyl acetate.
[0124] When the antifouling coating composition of the present invention contains a solvent (H), the content thereof can be appropriately adjusted depending on the purpose and the type of the component, and is, for example, preferably 0 to 50 mass %, more preferably 0 to 30 mass %, relative to 100 mass % of the composition.
[0125] <(I) Plasticizer> The antifouling coating composition of the present invention may contain a plasticizer (I) for the purpose of imparting plasticity to the antifouling coating film to be formed, etc. The plasticizer (I) may be used alone or in combination of two or more kinds.
[0126] The plasticizer (I) may be in a liquid state or a solid state (e.g., powder state) under room temperature (e.g., 25°C) conditions, and examples thereof include chlorinated paraffin, n-paraffin, tricresyl phosphate (TCP), dioctyl phthalate (DOP, also known as bis(2-ethylhexyl) phthalate), dioctyl adipate (DOA, also known as bis(2-ethylhexyl) adipate), diisodecyl phthalate (DIDP), diisononyl adipate, and tris(2-ethylhexyl) trimellitate, and preferred are chlorinated paraffin and TCP.
[0127] When the antifouling coating composition of the present invention contains a plasticizer (I), the content thereof is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, and is preferably 5 mass % or less, more preferably 3 mass % or less, relative to 100 mass % of the solid content of the antifouling coating composition of the present invention, from the viewpoint of maintaining good plasticity of the antifouling coating film, etc.
[0128] <(J) Defoaming agent> The antifouling coating composition of the present invention may contain an antifoaming agent (surface conditioner, leveling agent) (J) for the purpose of smoothing the coating film to be formed, etc. The antifoaming agent (J) may be used alone or in combination of two or more kinds.
[0129] As the defoaming agent (J), commercially available defoaming agents such as silicone-based defoaming agents, fluorine-based defoaming agents, and polymer-based defoaming agents can be used without limitation, and examples thereof include "BYK-066N" (manufactured by BYK Japan K.K., silicone-based defoaming agent), "BYK-350" (manufactured by BYK Japan K.K., surface conditioner, acrylic copolymer), and "BYK-354" (manufactured by BYK Japan K.K., defoaming agent, acrylic polymer).
[0130] When the antifouling coating composition of the present invention contains an antifoaming agent (J), the content thereof can be appropriately adjusted depending on the purpose, the type of the component, etc., and is, for example, preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and preferably 3% by mass or less, more preferably 1% by mass or less, relative to 100% by mass of the solid content of the composition.
[0131] <(K) Binder Component> The antifouling coating composition of the present invention may contain a binder component (K) for the purpose of imparting water resistance, crack resistance, and strength to the antifouling coating film formed. The binder component (K) refers to any binder component other than the triorganosilyl group-containing copolymer (A). The binder component (K) may be used alone or in combination of two or more.
[0132] Examples of the binder component (K) include polyester polymers, (meth)acrylic (co)polymers, vinyl (co)polymers, terpene phenol resins, petroleum resins, and ketone resins. Among these, polyester polymers, (meth)acrylic (co)polymers, vinyl (co)polymers, and petroleum resins are preferred, and polyester polymers and petroleum resins are more preferred.
[0133] When the antifouling coating composition of the present invention contains a binder component (K), the content thereof can be appropriately adjusted depending on the purpose and the type of the component, and is, for example, preferably 0.1 to 40 mass % relative to 100 mass % of the solid content of the composition.
[0134] <Method of manufacturing antifouling coating composition> The antifouling coating composition of the present invention can be produced by the same means (apparatus, method, conditions, etc.) as those for general antifouling coating compositions using components (A) and (B) and, if necessary, components (C) to (K) and other optional components. Specifically, after synthesizing the triorganosilyl group-containing copolymer (A), the obtained triorganosilyl group-containing copolymer (A) (a solution thereof), the dicarboxylate ester (B), and, if necessary, components (C) to (K) and other optional components are added to a container all at once or successively, and stirred and mixed to produce the composition.
[0135] -Anti-fouling coating film- The antifouling coating film of the present invention is formed from the antifouling coating composition of the present invention. The antifouling coating film of the present invention is formed by drying the antifouling coating composition of the present invention in the same manner as in the case of forming a conventional antifouling coating film from a conventional antifouling coating composition. However, the antifouling coating film of the present invention is not limited to the one immediately after being formed from the antifouling coating composition of the present invention in this way, and also includes those that have been exposed to an outdoor environment for a long period of time, or those that have been used as an antifouling coating film by immersing in water, etc., and have deteriorated due to exerting a predetermined function. The antifouling coating film of the present invention immediately after being formed or exposed to an outdoor environment for a long period of time basically contains the same substances (particularly components (A) and (B)) as the antifouling coating composition of the present invention, except that volatile components such as solvents are lost due to drying, etc., and the one after use, such as immersed in water, contains (remains) the same substances as the antifouling coating composition of the present invention, except that in addition to the volatile components, some components are lost (released) due to the exertion of antifouling performance.
[0136] The thickness of the antifouling coating film of the present invention is not particularly limited and can be set to an appropriate range depending on the properties (e.g., coating wear rate) and applications (type of substrate, period of use, etc.) of the antifouling coating film of the present invention. For example, the thickness immediately after formation is preferably 30 to 1,000 μm.
[0137] In one embodiment of the present invention, the antifouling coating film of the present invention is an antifouling coating film formed as a prior coating in a total assembly method, before or after exposure to an outdoor environment for a long period of time. In one embodiment of the present invention, the antifouling coating film of the present invention is an antifouling coating film formed as a top coating in a total assembly method.
[0138] -Substrate with antifouling coating- The substrate with an antifouling coating film of the present invention comprises a substrate and the antifouling coating film of the present invention. The antifouling coating film of the present invention is usually formed on a substrate and used as a substrate with an antifouling coating film.
[0139] The substrate is not particularly limited as long as it is capable of forming the antifouling coating film of the present invention and exhibiting its function, and examples thereof include substrates that are entirely or at least partially submerged in water, preferably in seawater, all or at least partly, permanently or temporarily, such as ships (e.g., large steel ships such as container ships, tankers, and bulk carriers, and hull panels for fishing boats, FRP boats, wooden boats, yachts, and the like, including both newly built and repaired ships), fishing and other marine materials (e.g., ropes, fishing nets, fishing gear, floats, buoys, diver suits, underwater goggles, oxygen cylinders, swimsuits, torpedoes), underwater structures (e.g., structures such as oil pipelines, water conveyance piping, circulating water pipes, water supply and drainage outlets of thermal and nuclear power plants, undersea cables, seawater utilization equipment (seawater pumps, etc.), megafloats, coastal roads, undersea tunnels, port facilities, various underwater civil engineering structures in canals, waterways, etc.). In consideration of the effects of the present invention (adhesion under exposure), the substrate is preferably a ship (a new ship or a ship already in service) or an underwater structure, and particularly preferably a large steel ship such as a container ship, a tanker, or a bulk carrier which is manufactured by an assembly method, i.e., constructed in blocks, pre-painted, exposed to the outdoor environment for a long period of time, welded, and then finished with a coating to form an antifouling coating film.
[0140] The substrate may be a substrate treated with an anti-rust agent or other treatment agent, or a substrate having a surface on which a coating film other than an anti-fouling coating film, such as an anti-rust coating film (e.g., zinc-rich paint), an anti-corrosion coating film (e.g., epoxy-based heavy-duty anti-corrosion coating), a binder coating film, etc. (non-anti-fouling coating film), an anti-fouling coating film formed from the present invention or other anti-fouling coating composition that has been exposed to an outdoor environment for a long period of time (post-exposure anti-fouling coating film), or an anti-fouling coating film formed from the present invention or other anti-fouling coating composition that has deteriorated, changed, or worn out (old anti-fouling coating film) is formed. In the substrate with the anti-fouling coating film of the present invention, the anti-fouling coating film of the present invention does not need to be formed in direct contact with the surface of the substrate, and may be formed on the substrate via the above-mentioned treatment agent, coating film, etc. Thus, the substrate with the anti-fouling coating film of the present invention may further contain other treatment agents, coating films, etc. in addition to the substrate and the anti-fouling coating film of the present invention. The anti-fouling coating film of the present invention can be formed on various non-anti-fouling coating films, post-exposure anti-fouling coating films, old anti-fouling coating films, etc.
[0141] The "non-antifouling coating film" that may be present on the substrate refers to a coating film other than the antifouling coating film, such as an undercoat coating film or an intermediate coating film, which is formed on the substrate before forming the antifouling coating film of the present invention, depending on the type and use of the substrate. The type of the non-antifouling coating film is not particularly limited, and examples thereof include an anti-rust coating film formed from an anti-rust paint, an anti-corrosion coating film formed from an anti-corrosion paint, and a binder coating film formed from a binder paint. Examples of the anti-corrosion coating film include those formed from an anti-corrosion paint containing an epoxy resin. Examples of the binder coating film include those formed from a binder paint containing one or more types of resin such as an epoxy resin, a vinyl resin, or a (meth)acrylic resin. When coating a substrate such as a ship, there is no clear distinction between the anti-corrosion coating film (undercoat coating film) and the binder coating film (intermediate coating film), and a coating film that serves both purposes may be used, but the "non-antifouling coating film" may be a binder coating film that also has the function of an anti-corrosion coating film.
[0142] The "post-exposure antifouling coating film" that may be present on the substrate refers to an antifouling coating film that has been exposed to an outdoor environment for a long period of time (e.g., 3 to 6 months) with the coating film facing the ground, and is in a deteriorated or altered state, particularly in relation to topcoat adhesion, compared to a healthy antifouling coating film before exposure. The "old antifouling coating film" that may be present on the substrate refers to an antifouling coating film that has been used in contact with water (seawater) for a certain period of time (e.g., the service life of the antifouling coating film), and is in a deteriorated, altered, or worn state compared to a healthy antifouling coating film before use (before immersion in seawater). The degree of deterioration, alteration, or wear of the post-exposure antifouling coating film or the old antifouling coating film is not particularly limited, and may be to a degree that is deemed necessary or preferable to form the antifouling coating film of the present invention. The type of antifouling coating film is not particularly limited, and may be the antifouling coating film of the present invention or another antifouling coating film. Other examples of antifouling coating films include hydrolysis type (e.g., coating films formed from silyl ester resin-based antifouling paints) and hydration decomposition type (e.g., coating films formed from vinyl chloride-isobutyl vinyl ether resin-based antifouling paints).
[0143] In the substrate, the portion on which the antifouling coating film of the present invention is formed is not particularly limited, and can be appropriately selected depending on the application. For example, when the substrate is a ship, the bottom of the ship (part always submerged) or the waterline (alternate wet and dry part) exposed to a biological fouling environment can be the portion on which the antifouling coating film of the present invention is formed (part of the substrate). In addition, when the antifouling coating film of the present invention is an antifouling coating film for a top coat applied to a substrate after assembly, it may be formed on a part of the substrate, such as the periphery of a joint, or may be formed on the entire substrate including the joint.
[0144] In one embodiment of the present invention, the substrate with the antifouling coating film of the present invention has a substrate to which an all-in-one coating method or other coating method requiring topcoat adhesion is applied, and the antifouling coating film of the present invention formed thereon as a pre-coating before exposure to an outdoor environment for a long period of time.
[0145] In one embodiment of the present invention, the substrate with the antifouling coating film of the present invention comprises a substrate to which an assembly technique or other coating technique requiring topcoat adhesion is applied, the antifouling coating film of the present invention formed thereon as a pre-coat and after exposure to an outdoor environment for a long period of time, and the antifouling coating film of the present invention formed as a topcoat, and the substrate has excellent adhesion (exposure adhesion) between the former antifouling coating film and the latter antifouling coating film.
[0146] In one embodiment of the present invention, the substrate with the antifouling coating film of the present invention comprises a substrate to which an assembly technique or other coating technique requiring topcoat adhesion is applied, a silyl-based antifouling coating film other than that of the present invention formed thereon as a pre-coat and after exposure to an outdoor environment for a long period of time, and the antifouling coating film of the present invention formed as a top-coat, and the adhesion (exposure adhesion) between the former antifouling coating film and the latter antifouling coating film is preferable.
[0147] In one embodiment of the present invention, the substrate with the antifouling coating film of the present invention comprises a substrate to which an assembly technique or other coating technique requiring topcoat adhesion is applied, an antifouling coating film according to the present invention formed thereon as a pre-coat after exposure to an outdoor environment for a long period of time, and a silyl-based antifouling coating film other than that of the present invention formed thereon as a topcoat, and the adhesion (exposure adhesion) of the former antifouling coating film and the latter antifouling coating film are preferable.
[0148] -Method of manufacturing substrate with antifouling coating film- The method for producing a substrate having an antifouling coating film of the present invention includes the following steps (1) and (2): (1) a step of coating or impregnating a substrate with the antifouling coating composition of the present invention to obtain a coated or impregnated body; (2) A step of drying the coated or impregnated body.
[0149] The application in step (1) can be carried out according to a general method, for example, a method of applying the antifouling coating composition to a substrate using an airless spray, an air spray, a brush, a roller, etc. The impregnation in step (1) can also be carried out according to a general method, for example, a method of immersing a substrate in the antifouling coating composition.
[0150] The conditions for coating or impregnation can be adjusted so as to form an antifouling coating film having a desired thickness, taking into consideration the drying conditions in step (2). For example, an appropriate amount of the antifouling coating composition per unit area of the substrate can be coated or impregnated so that the thickness of the dried coating film after step (2) is 10 to 300 μm, preferably 30 to 200 μm.
[0151] The drying in step (2) may be carried out according to a general method at an appropriate temperature and other conditions for an appropriate time. For example, the coated or impregnated body obtained in step (1) may be left at room temperature (e.g., 25°C) for preferably 0.5 to 14 days, more preferably 1 to 7 days. The drying in this step may be carried out under heating or while blowing air.
[0152] Steps (1) and (2) can be repeated as necessary. For example, if an antifouling coating film of a desired thickness cannot be formed by performing steps (1) and (2) only once, steps (1) and (2) can be performed a second time after the first time of steps (1) and (2), and steps (1) and (2) can be further performed as many times as necessary.
[0153] In one embodiment of the present invention, the method for producing a substrate with an antifouling coating film of the present invention includes step (1) which is performed as a pre-coat coating in an assembly technique or other coating technique requiring topcoat adhesion, and step (2).
[0154] In one embodiment of the present invention, the method for producing a substrate with an antifouling coating film of the present invention includes a step (1) and a step (2) performed as a preliminary coating in a total assembly method or other coating method requiring topcoat adhesion. In this embodiment, after the antifouling coating film formed in the step (2) is exposed to an outdoor environment for a long period of time to become a post-exposure antifouling coating film, the method may further include a step of removing dirt on the surface of the post-exposure antifouling coating film by washing with water or the like as necessary and drying, followed by a step of coating or impregnating a substrate with the antifouling coating composition of the present invention to obtain a coated or impregnated body as a finish coating; and a step of drying the coated or impregnated body.
[0155] In one embodiment of the present invention, the method for producing a substrate with an antifouling coating film of the present invention includes step (1) performed as a finish coating in a total assembly method or other coating method requiring topcoat adhesion, and step (2). In this embodiment, the substrate having an antifouling coating film (post-exposure antifouling coating film) formed from the antifouling coating composition of the present invention or other antifouling coating compositions (e.g., silyl-based antifouling coating compositions) by a separate pre-coating is the subject of step (1). In addition, in this embodiment, a necessary step, for example, a step of removing dirt on the surface of the post-exposure antifouling coating film by washing with water or the like and drying the antifouling coating film may be further included before step (1).
[0156] -Other aspects of the present invention- The antifouling coating composition, the antifouling coating film, the substrate with an antifouling coating film, and the method for producing a substrate with an antifouling coating film described in this specification can be converted into other inventions based on patent practice and common general technical knowledge.
[0157] For example, the "method for producing a substrate with an antifouling coating film" of the present invention can be converted into an "antifouling method for a substrate" including a step of forming the antifouling coating film of the present invention on at least a part of the substrate. The "step of forming an antifouling coating film" in the "antifouling method for a substrate" is basically the same as the steps (1) and (2) in the "method for producing a substrate with an antifouling coating film". That is, the antifouling method for a substrate of the present invention can be rephrased as including: (1') a step of coating or impregnating at least a part of the substrate with the antifouling paint composition of the present invention to obtain a coated or impregnated body; and (2') a step of drying the coated or impregnated body. In addition, the part of the substrate on which the antifouling coating film of the present invention is formed is not particularly limited, and can be appropriately selected according to the application. For example, when the substrate is a ship, the bottom of the ship (part always submerged) or the waterline part (alternate wet and dry part) exposed to a biological fouling environment can be the part (part of the substrate) on which the antifouling coating film of the present invention is formed.
[0158] In addition, the technical matters described in this specification with respect to the "manufacturing method of a substrate having an antifouling coating film" can be appropriately read as technical matters with respect to the "antifouling method of a substrate". For example, in the embodiment in which the substrate has an antifouling coating film after exposure, the "antifouling method of a substrate" of the present invention can be read as the "coating method of a substrate having an antifouling coating film after exposure". EXAMPLES
[0159] (1) Synthesis of triorganosilyl group-containing copolymer solution (A-1) [Synthesis Example 1] A reaction vessel equipped with a stirrer, reflux condenser, thermometer, nitrogen inlet tube and dropping funnel was charged with 43 parts of xylene and 10 parts of triisopropylsilyl methacrylate (TIPSMA), and heated and stirred under a nitrogen atmosphere until the liquid temperature reached 80°C. While maintaining the same conditions, monomers (50 parts of triisopropylsilyl methacrylate (TIPSMA), 25 parts of 2-methoxyethyl methacrylate (MEMA), 10 parts of methyl methacrylate (MMA), 5 parts of butyl acrylate (BA)) and a polymerization initiator (1.35 parts of 2,2'-azobis (2-methylbutyronitrile) (AMBN) were added to the reaction vessel from the dropping device at 30 minute intervals for a total of four times, and then the liquid temperature was raised to 105°C. After continuing heating and stirring at the same temperature for 30 minutes, 23.7 parts of xylene was added to the reaction vessel to obtain a solution (A-1) of a triorganosilyl group-containing copolymer.
[0160] [Synthesis Example 2] and [Synthesis Example 3] Solutions of triorganosilyl group-containing copolymers (A-2) and (A-3) were obtained in the same manner as in Synthesis Example 1, except that the composition of the monomers (TIPSMA, MEMA, MMA and BA) was changed as shown in Table 1.
[0161] <Solid content of copolymer solution (heating residue)> The solid content of the triorganosilyl group-containing copolymer solutions (A-1) to (A-3) was calculated based on JIS K 5601-1-2:2008 by measuring the mass of the solution obtained by drying each solution for 1 hour in a hot air dryer at 125°C, and calculating the ratio to the mass of the original solution.
[0162] <Viscosity of copolymer solution> The Gardner viscosities of the triorganosilyl group-containing copolymer solutions (A-1) to (A-3) were measured at 25° C. using a Gardner bubble viscometer.
[0163] <Weight average molecular weight (Mw) of copolymer> The weight average molecular weight (Mw) of the copolymer contained in the triorganosilyl group-containing copolymer solutions (A-1) to (A-3) was measured by gel permeation chromatography (GPC) under the following conditions.
[0164] Equipment: "HLC-8320GPC" (Tosoh Corporation) Column: "TSKgel guardcolumn SuperMP(HZ)-M" + "TSKgel SuperMultiporeHZ-M" + "TSKgel SuperMultiporeHZ-M" (all manufactured by Tosoh Corporation) Eluent: tetrahydrofuran (THF) Flow rate: 0.35ml / min Detector: RI Column thermostat temperature: 40℃ Standard material: polystyrene Sample preparation method: The polymer solution prepared in each production example was diluted with THF, and then filtered through a membrane filter to obtain a filtrate, which was used as a GPC measurement sample.
[0165] Table 1 shows information (monomer mixture and properties) regarding the triorganosilyl group-containing copolymer solutions (A-1) to (A-3).
[0166] [Table 1]
[0167] (2) Preparation of antifouling coating compositions of Examples 1 to 11 and Comparative Examples 1 to 6 [Example 1] 1.0 parts of xylene, 0.5 parts of Solvesso #100, and 12.0 parts of rosin solution (WW rosin made in China) were added to a plastic container and mixed using a paint shaker. Then, 20.0 parts of triorganosilyl group-containing copolymer solution (A-1) and 2.0 parts of dicarboxylate ester (Daifatty-101) were added to the resulting solution and stirred until they were uniformly mixed. Next, 5 parts of zinc oxide (zinc oxide type 2), 0.5 parts of organic red pigment (Noveperm Red F5RK), 50 parts of cuprous oxide (NC-301), 0.5 parts of titanium oxide (Typake R-930), 0.5 parts of red oxide (TODA COLOR NM-50), 4.0 parts of talc (FC-1), 2.0 parts of copper pyrithione (Copper Omadine Powder), 0.5 parts of oxidized polyethylene wax (ASA D-120), and 0.5 parts of tetraethoxysilane (ethyl silicate 28) were added to the obtained solution, and 200 parts of glass beads were added and dispersed by stirring for 1 hour using a paint shaker. 1.0 part of fatty acid amide wax (Disparlon A6900-20X) was added to the obtained dispersion, and these were stirred and dispersed for 20 minutes, and then the glass beads were removed from the mixture using an 80-mesh filter to produce an antifouling paint composition.
[0168] [Example 2] to [Example 11] and [Comparative Example 1] to [Comparative Example 6] The antifouling coating compositions of Examples 2 to 11 and Comparative Examples 1 to 6 were produced in the same manner as in Example 1, except that the types and amounts of each raw material component were changed as shown in Table 2. In the Comparative Examples, instead of the dicarboxylic acid ester (Daifatty-101) corresponding to component (B), a dicarboxylic acid ester (DOA or DOP) or other compound (TCP, etc.) corresponding to plasticizer (I) that does not satisfy the conditions of component (B) was added at the same stage.
[0169] The amount of each component shown in Table 2 indicates the amount in the form. For example, the amount of fatty acid amide wax in the form (as a whole) in Example 1 is 0.5 parts as shown in Table 2, but since the solid content is 20 mass% as shown in Table 3, the amount of fatty acid amide wax itself is 0.1 parts.
[0170] (3) Performance evaluation test of antifouling coating film [Test Example 1] Exposure adhesion test An epoxy-based anticorrosive paint (product name "Banno 1500", manufactured by Chugoku Paint Co., Ltd.) was applied to a sandblasted steel plate (150 mm x 70 mm x 2.3 mm) using an applicator to a dry film thickness of 150 μm, and dried at 23° C. for 24 hours to form a cured coating film. Next, an epoxy-based binder paint (product name "CMP AC-EP", manufactured by Chugoku Paint Co., Ltd.) was applied to the cured coating film to a dry film thickness of 100 μm, and dried at 23° C. for 24 hours.
[0171] Next, each of the antifouling coating compositions of the Examples and Comparative Examples listed in Table 2 was applied to the test plate (on the surface of the dried coating film of the epoxy-based binder paint) using an applicator to a dry film thickness of 150 μm, and then dried at 23° C. for 7 days to form an antifouling coating film (first layer of antifouling coating film).
[0172] The test plate on which the antifouling coating film was formed was placed on an outdoor exposure stand (within the grounds of the Ohtake Research Institute of Chugoku Paint Co., Ltd.) and exposed outdoors for 120 days. When the test plate obtained was placed on the outdoor exposure stand, it was fixed so that the coating film faced the ground at an angle of 45° to the horizontal (ground). Hereinafter, outdoor exposure means that the test was carried out under these conditions.
[0173] The test plate exposed to the outdoors was lightly rinsed with water and dried, and then each of the antifouling paint compositions of the Examples and Comparative Examples listed in Table 2 (the same as those used to form the first layer of the antifouling coating film) was applied onto the antifouling coating film using an applicator to a dry film thickness of 150 μm, and the plate was dried at 23° C. for 7 days to form an antifouling coating film (second layer of the antifouling coating film), thereby producing Test Plate 1.
[0174] The obtained test plate 1 was immersed in artificial seawater at 23°C for one month, and then dried at 23°C for one day. An adhesion test was then carried out based on the 4mm x 4mm 25-grid grid peel test (cross-cut method) specified in JIS K5600 5-6:1999, and the interlayer adhesion between the first and second antifouling coating films was evaluated according to the following evaluation criteria. When making a cut, a cut was made from the second coating film side of the test plate to reach the first coating film. (Evaluation Criteria) 5: Peeled area is less than 5%. 4: The peeled area is 5% or more and less than 20%. 3: The peeled area is 20% or more and less than 40%. 2: The peeled area is 40% or more and less than 60%. 1: Peeled area is 60% or more.
[0175] [Test Example 2] Static stain resistance test Test plate 2 was prepared in the same manner as Test plate 1 above, except that a sandblasted steel plate of a different size (300 mm×100 mm×2.3 mm) was used.
[0176] The obtained test panel 2 was suspended and immersed in the Seto Inland Sea off the coast of Hatsukaichi City, Hiroshima Prefecture, at a water level of 400 mm or less, and left to stand, and every month from the start of immersion, the area of the part of the antifouling coating film where aquatic organisms were attached (hereinafter also referred to as the "attached area") (%) was investigated, assuming that the total area of the antifouling coating film on the test panel that was constantly submerged in seawater is 100%, and this was continued for 4 months. The static antifouling property was evaluated based on the following evaluation criteria. (Evaluation Criteria) 5: The adhesion area is less than 5%. 4: The adhesion area is 5% or more and less than 20%. 3: The adhesion area is 20% or more and less than 40%. 2: The adhesion area is 40% or more and less than 60%. 1: The adhesion area is 60% or more.
[0177] [Test Example 3] Storage stability test Each of the antifouling coating compositions of the Examples and Comparative Examples was stored at 50°C for 2 months, and the viscosity was measured immediately before storage and every 2 weeks after storage. The viscosity of each composition was measured using a Stormer viscometer (manufacturer: Taiyu Kizai Co., Ltd., product name: Stormer viscometer, model: 691) at a temperature of 23°C. The viscosity measured at each time point after storage was divided by the viscosity measured immediately before storage to obtain the "viscosity increase rate (%)", and the storage stability was evaluated based on the following evaluation criteria. In Table 2, "-" indicates that the measurement was not performed because the viscosity life was close to its limit. (Storage stability evaluation criteria) 5: Viscosity after 8 weeks of storage is less than 120% of the viscosity before storage 4: Viscosity after 6 weeks of storage is less than 120% of the viscosity before storage 3: Viscosity after 4 weeks of storage is less than 120% of the viscosity before storage 2: Viscosity after 2 weeks of storage is less than 120% of the viscosity before storage 1: Viscosity after 2 weeks of storage is 120% or more of the viscosity before storage
[0178] Information regarding the antifouling coating compositions of Examples 1 to 11 and Comparative Examples 1 to 6 (compositions and evaluation test results of the antifouling coating films formed) is shown in Table 2. In addition, details of the components (products) used in the production of those antifouling coating compositions and shown in Table 2 are shown in Table 3.
[0179] As can be seen from the results in Table 2, in various embodiments, the antifouling coating composition of the present invention is capable of forming an antifouling coating film that is excellent in exposure adhesion and also has a well-balanced static antifouling property and storage stability. On the other hand, as is clear from a comparison between Example 2 and Comparative Example 1, an antifouling coating composition that does not contain a dicarboxylate ester (B) (or a plasticizer (I)) has significantly poor exposure adhesion. Furthermore, as is clear from Comparative Examples 2 to 6, when a predetermined amount of plasticizer (I) (relatively more than conventional amounts) is used, the decrease in exposure adhesion can be prevented, but instead, the static antifouling property and storage stability decrease.
[0180] [Table 2-1]
Table 2-2
[0181]
Table 3
Claims
1. The present invention comprises a triorganosilyl group-containing copolymer (A) and a dicarboxylic acid ester (B) represented by the following general formula (I), An antifouling coating composition, wherein the copolymer (A) has a structural unit derived from a triorganosilyl group-containing monomer (a1) and a structural unit derived from an alkoxyalkyl (meth)acrylate or an aryloxyalkyl (meth)acrylate (a2) and / or an alkyl (meth)acrylate or an aryl (meth)acrylate (a3). R 2 -OOC-R 1 -COO-R 2 …(I) Here, R 1 represents a divalent hydrocarbon group having 2 to 20 carbon atoms, R 2 are each independently a monovalent hydrocarbon group having 1 to 30 carbon atoms, 2 At least one R 3 having R 3 Ha-(R 4 O) n - represents R 4 are each independently a divalent hydrocarbon group having 2 to 4 carbon atoms, and n is an integer of 2 or greater.
2. 2. The antifouling coating composition according to claim 1, wherein the triorganosilyl group-containing monomer (a1) is triisoprosilyl methacrylate.
3. 2. The antifouling coating composition according to claim 1, wherein the triorganosilyl group-containing copolymer (A) contains 40 to 80 mass % of structural units derived from the triorganosilyl group-containing monomer (a1).
4. The antifouling coating composition according to claim 1, wherein the mass ratio [(a1):(a2)] of the structural units derived from the triorganosilyl group-containing monomer (a1) to the structural units derived from the alkoxyalkyl (meth)acrylate or aryloxyalkyl (meth)acrylate (a2) is 55:45 to 90:
10.
5. The antifouling coating composition according to claim 1, wherein the mass ratio [(a1):(a3)] of the structural units derived from the triorganosilyl group-containing monomer (a1) to the structural units derived from the alkyl(meth)acrylate or aryl(meth)acrylate (a3) is 60:40 to 90:
10.
6. The R 1 The antifouling coating composition according to claim 1 , wherein is a butylene group.
7. The R 4 The antifouling coating composition according to claim 1 , wherein is an ethylene group.
8. The R 2 The antifouling coating composition according to claim 1 , wherein has a benzyl group.
9. An antifouling coating film formed from the antifouling coating composition according to any one of claims 1 to 8.
10. A substrate with an antifouling coating film, comprising a substrate and the antifouling coating film according to claim 9.
11. A method for producing a substrate with an antifouling coating film, comprising the steps of: (1) applying or impregnating a substrate with the antifouling coating composition according to any one of claims 1 to 8 to obtain a coated or impregnated body; and (2) drying the coated or impregnated body.
Citation Information
Patent Citations
Antifouling paint composition and coated article having antifouling coating formed using said composition on surface
WO2019069777A1
Antifouling paint composition and coated article having antifouling coating formed using said composition on surface
WO2019069778A1