Laminate and packaging material

A three-layer laminate structure with a specific resin layer containing a polar ethylene copolymer or its ionomer addresses adhesion issues in laminates with antistatic agents, maintaining strong adhesion even at high temperatures.

JP2024146905APending Publication Date: 2024-10-15JAPAN POLYETHYLENE CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024056855
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing laminates containing antistatic agents face issues with adhesion deterioration due to bleeding of the antistatic agent, especially at high temperatures, leading to reduced adhesive strength and the need for strict first-in, first-out management.

Method used

A laminate structure comprising three layers: a base layer, a resin layer containing a specific polar ethylene copolymer or its ionomer, and a base layer with an antistatic agent, where the resin layer includes a polyethylene resin composition with controlled properties to prevent adhesion deterioration.

Benefits of technology

The laminate maintains good adhesion even with base materials containing antistatic agents, particularly under high temperature conditions, ensuring stable adhesive strength and suitability for packaging applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146905000001
    Figure 2024146905000001
  • Figure 2024146905000002
    Figure 2024146905000002
Patent Text Reader

Abstract

To provide a laminate which is excellent in adhesiveness even if a base material containing an anti-static agent is used, and a packaging material using the same.SOLUTION: A laminate has at least three layers of a base material layer 1 (α), a resin layer (β) and a base material layer 2 (γ), and satisfies the following characteristics. The base material layer 1 (α) has an oxygen permeability at 20°C and 65% RH of 1,300 mL / m2 day MPa or less. The resin layer (β) contains a constitutional unit (m) derived from ethylene (a) composed of a polyethylene resin composition (B) containing 2 to 40 pts.wt. of a polar ethylenic copolymer (A) having the following characteristic (A) and / or an ionomer (A') of the polar ethylenic copolymer (A), and a constitutional unit (n) derived from a monomer having a carboxy group as essential constitutional units. The base material layer 2 (γ) is a base material containing an anti-static agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate having excellent adhesiveness even when a substrate containing an antistatic agent is used, and a packaging material using the same. [Background technology]

[0002] The glass transition points of PP, PE, and LLDPE are lower than room temperature, so when a low molecular weight antistatic agent (AS agent) is kneaded into the resin, it bleeds out over time through the amorphous parts onto the surface and between layers of the film at temperatures above the glass transition point. The bled-out AS agent is not bonded to the resin, but is attached to the surface or between layers. For this reason, OPP films containing AS agents have difficulty achieving laminate adhesive strength. Also, at high temperatures, the AS agent is more likely to bleed out, making it unusable. The OPP used in Japan is generally of the antistatic type (AS type). There is a difference in the amount of bleed-out between summer and winter. Therefore, the laminate adhesive strength decreases more quickly in summer, and it is necessary to manage it on a first-in, first-out basis so that it can be used quickly after processing. There are also cases where it is unavoidable to use the non-antistatic type. Summary of the Invention [Problem to be solved by the invention]

[0003] In view of the above problems, an object of the present invention is to provide a laminate which exhibits good adhesion even in the case of lamination adhesion to a substrate containing an antistatic agent, and which has good adhesion even under high temperature conditions. Another object of the present invention is to provide a packaging material using such a laminate. [Means for solving the problem]

[0004] The present inventors have conducted extensive research to solve the above problems and have found that by providing a resin layer (β) containing a resin composition (B) containing 2 to 40 parts by weight of a specific polar ethylene copolymer (A) and / or its ionomer (A') between a barrier substrate layer 1 (α) and a substrate layer 2 (γ) containing an antistatic agent, it is possible to obtain a laminate which is not susceptible to deterioration in adhesion due to bleeding of the antistatic agent, and which is particularly resistant to deterioration in adhesion at high temperatures, and have completed the present invention.

[0005] That is, the present invention is as follows. (Invention 1) A laminate having at least three layers, namely, a substrate layer 1 (α), a resin layer (β), and a substrate layer 2 (γ), each of which satisfies the following properties: Base layer 1 (α): Oxygen permeability is 1300 mL / m at 20°C and 65% RH 2 ·day·MPa or less. Resin layer (β): Contains a polyethylene resin composition (B) containing 2 to 40 parts by weight of a polar ethylene copolymer (A) having the following characteristic (a) and / or an ionomer (A′) of the polar ethylene copolymer (A). (a) Contains, as essential structural units, a structural unit (m) derived from ethylene and a structural unit (n) derived from a monomer having a carboxy group. Substrate layer 2(γ): A substrate containing an antistatic agent (Invention 2) 2. The laminate according to claim 1, wherein the polyethylene resin composition (B) further contains a polyethylene resin (C) having the following characteristics (c-1) to (c-7): (c-1) MFR (190℃, 21.18N load) is 0.1 to 100g / 10min (c-2) In DSC, the total heat of fusion ΔHm is 30 to 120 J / g (c-3) Crystallization temperature Tc is 25 to 90°C (c-4) Contains 80 to 98 mol% of structural units derived from ethylene as a main component, 2 to 20 mol% of structural units derived from propylene as an essential secondary component, and may contain 5 mol% or less of structural units derived from a third α-olefin other than ethylene and propylene as a secondary component. (However, when the structural units derived from the third α-olefin are contained, the total content of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol %). (c-5) Density is 0.88 to 0.94 g / cm 3 (c-6) The total amount of vinyl and vinylidene in polyethylene resin (C) is 0.35 (pieces / total 1000C) or more (Note that the number of vinyl and vinylidene units is the number per 1,000 carbon atoms in the main chain and side chains, measured by NMR.) (c-7) The number of branches (Y) due to comonomers in the polyethylene resin (C) and the density (X) satisfy the relationship of the following formula (1). Formula (1): (Y) ≧ -1157×(X)+1084 (where Y is the number per 1000 carbon atoms in total in the main chain and side chains as measured by NMR.) (Invention 3) The laminate according to Invention 1 or 2, wherein the ionomer (A') of the polar ethylene-based copolymer (A) is further characterized in that a phase angle δ at an absolute value of a complex elastic modulus G*=0.1 MPa measured with a rotational rheometer is 50 degrees to 75 degrees. (Invention 4) 3. The laminate according to claim 1 or 2, wherein the polyethylene resin composition (B) further contains a polyethylene resin (D) having the following properties (d-1) to (d-2): (d-1) MFR (190°C, 21.18N load) is 0.1 to 100g / 10min (d-2) Density is 0.91 to 0.97 g / cm 3 (Invention 5) The laminate according to Invention 1 or 2, wherein the ionomer (A') of the polar ethylene-based copolymer (A) is obtained by converting at least a part of the carboxy groups of the polar ethylene-based copolymer (A) into a metal-containing carboxylate salt containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table. (Invention 6) The laminate according to Invention 1 or 2, wherein the polar ethylene-based copolymer (A) contains 70 to 98 mol % of a structural unit (m) derived from ethylene as a main component and 2 to 30 mol % of a structural unit (n) derived from a monomer having a carboxy group as an essential subcomponent. (Invention 7) 3. The laminate according to claim 1 or 2, wherein the base layer 1(α) is a metal foil or a metal-deposited film. (Invention 8) 3. The laminate according to claim 1 or 2, characterized in that the laminate is formed by an extrusion coating method. (Invention 9) A packaging material comprising the laminate according to invention 1 or 2. Effect of the Invention

[0006] Even in the case of lamination adhesion with a substrate containing an antistatic agent, good adhesion is exhibited, and a laminate having good adhesion even under high temperature conditions can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The components used in the present invention and the laminate for extrusion lamination using these components will be described in detail below. The present invention relates to a laminate having at least three layers, namely, a substrate layer 1 (α), a resin layer (β) and a substrate layer 2 (γ), each of which satisfies the following properties.

[0008] 1. Base material layer 1 (α) The base layer 1(α) of the present invention has the following properties. Base layer 1 (α): Oxygen permeability is 1300 mL / m at 20°C and 65% RH2 ·day·MPa or less. This definition means that the material is made of a material with high barrier properties against oxygen and gases. For example, it can be a metal foil such as aluminum or a metal-deposited film. It can also be a barrier paper base material with a barrier coating applied to a paper base material. The oxygen permeability can be measured, for example, based on JIS K7126-2, using the following device. Device: OX-TRAN2 / 21 (made by MOCON) Temperature and humidity: 23℃, relative humidity 0% (dry) Transmission area: 50cm2

[0009] 2.Resin layer (β) The resin layer (β) of the present invention has the following properties. The polyethylene resin composition (B) contains 2 to 40 parts by weight of a polar ethylene copolymer (A) having the following characteristic (a) and / or an ionomer (A') of the polar ethylene copolymer (A). The blend amount is preferably 5 to 35 parts by weight. (a) Contains, as essential structural units, a structural unit (m) derived from ethylene and a structural unit (n) derived from a monomer having a carboxy group.

[0010] 2.1 Polar ethylene copolymer (A) The polar ethylene copolymer (A) is a copolymer that contains, as essential structural units, (a) a structural unit (m) derived from ethylene and (n) a structural unit derived from a monomer having a carboxy group. The structural unit (m) derived from ethylene and the structural unit (n) derived from a monomer having a carboxy group are essential structural units, and may further include a structural unit (p) which is a compound having one or more carbon-carbon double bonds in the molecular structure as a structural unit. There are two types of polar ethylene copolymers with different molecular structures due to the difference in polymerization method: a branched polar ethylene copolymer having a branched molecular structure polymerized by radical polymerization, and a linear polar ethylene copolymer polymerized by catalytic polymerization, which has been newly developed in recent years. Either of them can be used as the polar ethylene copolymer of the present invention, but the linear polar ethylene copolymer and its ionomer are preferred.

[0011] (1) Structural unit (m) The structural unit (m) essentially contains a structural unit derived from ethylene, and may further contain, as necessary, one or more structural units derived from an α-olefin having 3 to 20 carbon atoms. The structural unit derived from ethylene in the structural unit (m) may account for 65 to 100 mol % or 70 to 100 mol % based on the total moles of the structural unit (m).

[0012] (2) Structural unit (n) The structural unit (n) is a structural unit derived from a monomer having a carboxy group.

[0013] Specific examples of monomers having a carboxy group include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, norbornene dicarboxylic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid.

[0014] As the structural unit derived from a monomer having a carboxy group, from the viewpoint of industrial availability, preferably, a structural unit derived from acrylic acid, methacrylic acid, or 5-norbornene-2,3-dicarboxylic acid anhydride is mentioned, and in particular, a structural unit derived from acrylic acid may be used.

[0015] Furthermore, the structural unit derived from a monomer having a carboxy group may be of one type or of multiple types.

[0016] (3) Structural unit (p) The copolymer (A) used in the present invention may be a binary copolymer consisting of only the structural unit (m) and the structural unit (n), or a multi-component copolymer containing the structural unit (m), the structural unit (n), and a structural unit (p) other than these. The monomer that gives the structural unit (p) may be any monomer that is not included in the monomers that give the structural unit (m) and the structural unit (n), and is not limited as long as it is a compound having one or more carbon-carbon double bonds in the molecular structure.

[0017] A specific example of a non-cyclic monomer that provides the structural unit (p) is a (meth)acrylic acid ester having an ester group having 2 to 20 carbon atoms. Specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, and benzyl (meth)acrylate. Preferred is an acrylic acid ester, and a specific example of the compound is at least one selected from the group consisting of methyl acrylate, ethyl acrylate, n-butyl acrylate (nBA), isobutyl acrylate (iBA), t-butyl acrylate (tBA), and 2-ethylhexyl acrylate, and in particular may be at least one selected from the group consisting of n-butyl acrylate (nBA) and isobutyl acrylate (iBA). Other non-cyclic monomers include, for example, 5-hexen-1-ol, allyl methyl ether, ethyl-4-pentenoate, 4-chloro-1-butene, methyl vinyl ether, styrene, vinyltrimethylsilane, vinyl chloride, and (meth)acrylonitrile. The non-cyclic monomer may be of one type or of multiple types.

[0018] 2.2 Resin properties of polar ethylene copolymer (A) (1) Number of branches per 1,000 carbon atoms in a polymer In the copolymer according to the present invention, in order to increase the elastic modulus and obtain sufficient mechanical properties, 13 The number of methyl branches calculated by C-NMR may be 50 or less, 5.0 or less, 1.0 or less, or 0.5 or less per 1,000 carbons, with no particular limit on the lower limit, and the smaller the better. The number of ethyl branches may be 3.0 or less, 2.0 or less, 1.0 or less, or 0.5 or less per 1,000 carbons, with no particular limit on the lower limit, and the smaller the better. The number of butyl branches may be 7.0 or less, 5.0 or less, 3.0 or less, or 0.5 or less per 1,000 carbons, with no particular limit on the lower limit, and the smaller the better.

[0019] (2) Method for measuring the amount of structural units derived from monomers having a carboxy group and non-cyclic monomers in the copolymer, and the number of branches The amount of structural units derived from monomers having a carboxy group and non-cyclic monomers in the copolymer of the present invention, and the number of branches per 1,000 carbon atoms are 13 It can be determined using C-NMR spectroscopy. 13 C-NMR is measured by the following method. 200-300 mg of sample is placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of a mixed solvent of o-dichlorobenzene (C6H4Cl2) and deuterated bromide benzene (C6D5Br) (C6H4Cl2 / C6D5Br = 2 / 1 (volume ratio)) and hexamethyldisiloxane, a chemical shift standard substance, and the tube is sealed after replacing with nitrogen. The tube is heated and dissolved to prepare a homogeneous solution, which is used as the NMR measurement sample. NMR measurements are performed at 120°C using an AV400M NMR instrument from Bruker Japan Ltd. equipped with a 10 mmφ cryoprobe. 13 C-NMR was measured using the inverse gate decoupling method with a sample temperature of 120°C, a pulse angle of 90°, a pulse interval of 51.5 seconds, and an accumulation count of 512 or more. The chemical shifts are those of hexamethyldisiloxane. 13 The C signal was set to 1.98 ppm, and the other 13 The chemical shifts of the C signals are based on this. Obtained 13 In C-NMR, the signals specific to the monomers or branches of the multicomponent copolymer are identified and their intensities are compared, so that the amount of structural units of each monomer in the multicomponent copolymer and the number of branches can be analyzed. The positions of the signals specific to the monomers or branches can be referred to publicly known materials, or can be independently identified depending on the sample. Such an analysis method is commonly known to those skilled in the art.

[0020] (4) Molecular structure of copolymer The molecular chain terminal of the copolymer according to the present invention may be a structural unit (m) derived from ethylene, a structural unit (n) derived from a monomer having a carboxy group, or a structural unit (p) derived from a non-cyclic monomer.

[0021] Further, examples of the copolymer according to the present invention include random copolymers, block copolymers, and graft copolymers of a structural unit (m) derived from ethylene, a structural unit (n) derived from a monomer having a carboxy group, and a structural unit (p) derived from a non-cyclic monomer.

[0022] (5) Linear structure The linear polar ethylene copolymer or linear ionomer preferably used in the present invention is characterized in that these structural units are copolymerized substantially linearly, preferably randomly. "Substantially linear" refers to a state in which the copolymer has no branching or the frequency of branching structures is low, and the copolymer can be considered to be linear. Specifically, this refers to a state in which the phase angle δ of the copolymer is 50 degrees or more under the conditions described below. Furthermore, the linear polar ethylene copolymer and its linear ionomer preferably used in the present invention are preferably produced in the presence of a transition metal catalyst, from the viewpoint of making the molecular structure linear. It is known that the molecular structure of the copolymer varies depending on the production method, such as polymerization by a high-pressure radical polymerization process or polymerization using a metal catalyst. The difference in molecular structure can be controlled by selecting the production method, but the molecular structure can also be estimated from the complex modulus measured with a rotational rheometer, as described in JP 2010-150532 A, for example.

[0023] (6) Absolute value of complex elastic modulus G * Phase angle δ at =0.1MPa In the linear polar ethylene copolymer preferably used in the present invention, the phase angle δ at the absolute value of the complex elastic modulus G*=0.1 MPa measured by a rotational rheometer must be 50 to 75 degrees. The lower limit of the phase angle δ may be 51 degrees or more, and the upper limit of the phase angle δ may be 64 degrees or less. More specifically, when the phase angle δ (G*=0.1 MPa) at the absolute value of the complex modulus G*=0.1 MPa measured using a rotational rheometer is 50 degrees or more, this indicates that the molecular structure of the copolymer is a linear structure that does not contain any long chain branches or a substantially linear structure that contains a small amount of long chain branches that does not affect the mechanical strength. Furthermore, when the phase angle δ (G*=0.1 MPa) at the absolute value of the complex modulus G*=0.1 MPa measured using a rotational rheometer is lower than 50 degrees, the molecular structure of the copolymer contains excessive long chain branches, resulting in poor mechanical strength. The phase angle δ at the absolute value of the complex modulus G*=0.1 MPa measured by a rotational rheometer is affected by both the molecular weight distribution and long chain branching. However, for copolymers with Mw / Mn≦4, more preferably Mw / Mn≦3, it is an index of the amount of long chain branching, and the more long chain branches contained in the molecular structure, the smaller the δ(G*=0.1 MPa) value. If the Mw / Mn of a copolymer is 1.5 or more, the δ(G*=0.1 MPa) value will not exceed 75 degrees even if the molecular structure does not contain long chain branches.

[0024] In the present invention, the method for measuring the complex elastic modulus is as follows. The sample is placed in a 1.0 mm thick mold for hot pressing, preheated for 5 minutes in a hot press machine with a surface temperature of 180°C, and then the residual gas in the sample is degassed by repeatedly applying and depressurizing pressure, and then pressurized to 4.9 MPa and held for 5 minutes. The sample is then transferred to a press machine with a surface temperature of 25°C and cooled by holding at a pressure of 4.9 MPa for 3 minutes to create a pressed plate made of a sample with a thickness of approximately 1.0 mm. The pressed plate made of the sample is processed into a circle with a diameter of 25 mm to serve as a measurement sample, and a Rheometrics ARES type rotational rheometer is used as a measurement device for dynamic viscoelastic properties, and dynamic viscoelasticity is measured under the following conditions in a nitrogen atmosphere. Plate: φ25mm parallel plate ·Temperature: 160℃ Distortion: 10% Measurement angular frequency range: 1.0×10 -2 ~1.0×10 2 rad / s Measurement interval: 5 points / decade Absolute value of complex elastic modulus G * Common logarithm logG of (Pa) * Plot the phase angle δ against logG * = 5.0, the value of δ (degrees) at the point * = 0.1MPa). * If there is no point corresponding to =5.0, logG * Using two points around =5.0, logG *The δ value at logG = 5.0 is calculated by linear interpolation. * <5, logG * Using the three largest values, we plot logG on a quadratic curve. * = 5.0.

[0025] 2.3 Ionomer of polar ethylene copolymer (A') The ionomer of the polar ethylene copolymer means that at least a part of the carboxy groups of the polar ethylene copolymer (A) is converted to a metal-containing carboxylate containing a metal ion, preferably a metal-containing carboxylate containing at least one metal ion selected from Groups 1, 2, or 12 of the periodic table. 2.3.1 Method for producing ionomeric bodies The method for producing an ionomer according to the present invention includes a step of converting at least a portion of the carboxy groups of the structural unit (n) of the copolymer (A) into a metal-containing carboxylate by reacting the carboxy groups with a compound containing at least one metal ion selected from Groups 1, 2, or 12 of the periodic table.

[0026] The metal ion-containing compound may be an oxide, hydroxide, carbonate, bicarbonate, acetate, formate, etc., of a metal from Groups 1, 2, or 12 of the Periodic Table. The compound containing metal ions may be supplied to the reaction system in the form of particles or fine powder, or may be dissolved or dispersed in water or an organic solvent and then supplied to the reaction system, or a master batch may be prepared using an ethylene / unsaturated carboxylic acid copolymer or an olefin copolymer as a base polymer and then supplied to the reaction system. In order to ensure smooth reaction, it is preferable to prepare a master batch and then supply the compound containing metal ions to the reaction system.

[0027] The reaction with the compound containing metal ions may be carried out by melt kneading using various types of equipment such as a vent extruder, a Banbury mixer, a roll mill, etc., and the reaction may be a batch or continuous method. Since the reaction can be carried out smoothly by discharging water and carbon dioxide gas by-produced by the reaction using a degassing device, it is preferable to carry out the reaction continuously using an extruder equipped with a degassing device such as a vent extruder. In the reaction with the compound containing metal ions, a small amount of water may be injected to promote the reaction.

[0028] 2.4 Polyethylene resin (C) Furthermore, as a preferred embodiment of the present invention, the polyethylene resin composition (B) contains a polyethylene resin (C) having the following characteristics (c-1) to (c-7). (c-1) MFR (190℃, 21.18N load) is 0.1 to 100g / 10min (c-2) In DSC, the total heat of fusion ΔHm is 30 to 120 J / g (c-3) Crystallization temperature Tc is 25 to 90°C (c-4) Contains 80 to 98 mol% of structural units derived from ethylene as a main component, 2 to 20 mol% of structural units derived from propylene as an essential secondary component, and may contain 5 mol% or less of structural units derived from a third α-olefin other than ethylene and propylene as a secondary component. (However, when the structural units derived from the third α-olefin are contained, the total content of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol %). (c-5) Density is 0.88 to 0.94 g / cm 3 (c-6) The total amount of vinyl and vinylidene in polyethylene resin (C) is 0.35 (pieces / total 1000C) or more (Note that the number of vinyl and vinylidene units is the number per 1,000 carbon atoms in the main chain and side chains, measured by NMR.) (c-7) The number of branches (Y) due to comonomers in the polyethylene resin (C) and the density (X) satisfy the relationship of the following formula (1). Formula (1): (Y) ≧ -1157×(X)+1084 (where Y is the number per 1000 carbon atoms in total in the main chain and side chains as measured by NMR.)

[0029] (i) Characteristics of polyethylene resin (C) (c-1)MFR The polyethylene resin (C) used in the present invention has a melt flow rate (MFR: 190°C, 21.18N load) of 0.1 to 100g / 10min, preferably 1 to 80g / 10min, more preferably 3 to 70g / 10min. If the MFR is less than 1g / 10min, the extensibility during molding is poor and the motor load in the extruder is high, which is not preferred. On the other hand, if the MFR exceeds 100g / 10min, the state of the molten film during molding becomes unstable, which is not preferred.

[0030] The MFR of the polymer can be adjusted, for example, by appropriately adjusting the polymerization temperature, the amount of comonomer, etc. The MFR of the polyethylene resin (C) is measured in accordance with JIS-K6922-2:1997 Appendix (190°C, 21.18N load).

[0031] (c-2) In DSC, the total heat of fusion ΔHm is 30 to 120 J / g The total heat of fusion ΔHm of the polyethylene resin (C) used in the present invention is 30 to 120 J / g, preferably 32 to 118 J / g, and more preferably 35 to 115 J / g. If ΔHm is less than 30 J / g, blocking becomes poor, which is not preferable. On the other hand, if ΔHm exceeds 120 J / g, the adhesiveness becomes poor, which is undesirable. In order to adjust ΔHm of the polyethylene resin (C), for example, a method of appropriately adjusting the comonomer content, polymerization temperature, catalyst amount, etc. can be used. Here, ΔHm indicates the heat of fusion in the melting curve measured by a differential scanning calorimeter (DSC). In general, ethylene resins with low crystallinity tend to have a broader melting peak and a smaller ΔHm than ethylene resins with high crystallinity.

[0032] (c-3) Crystallization temperature Tc is 25 to 90°C The crystallization temperature Tc of the polyethylene resin (C) used in the present invention is 25 to 90° C., preferably 27 to 88° C., and more preferably 30 to 85° C. If Tc is less than 25° C., the crystallinity is too low, which is undesirable as blocking is poor. On the other hand, if Tc is more than 90° C., the adhesiveness is undesirable as a result of the presence of highly crystalline components. Here, Tc indicates the maximum peak temperature among the crystallization peaks in the crystallization curve measured by a differential scanning calorimeter (DSC). (c-4) Monomer structure The polyethylene resin (C) used in the present invention is a polyethylene resin (C) characterized by containing 80 to 98 mol% of structural units derived from ethylene as a main component and 2 to 20 mol% of structural units derived from propylene as a secondary component, and a specific example is a copolymer polymerized by catalytic polymerization method, which is a copolymer polymerized substantially randomly in a linear chain. Specifically, it is a random copolymer of ethylene and propylene. Preferably, the structural units derived from ethylene are 80 to 98 mol%, the structural units derived from propylene are 2 to 20 mol%, and more preferably, the structural units derived from ethylene are 85 to 95 mol%, and the structural units derived from propylene are 5 to 15 mol%. Here, the monomer amount such as the ethylene content is 13 The values ​​were measured and calculated by C-NMR under the conditions described in the Examples below.

[0033] In addition, it is preferable that the composition does not contain any structural units derived from other α-olefins, particularly α-olefins having 4 to 20 carbon atoms, and other monomer components, but such structures may be contained in a substantially small amount. In this specification, an α-olefin other than ethylene and propylene is referred to as a third α-olefin. The polyethylene resin (C) of the present invention may contain a structural unit derived from a third α-olefin other than ethylene and propylene as a minor component, for example, 5 mol% or less, preferably 2 mol% or less, more preferably 1.5 mol% or less, even more preferably 1 mol% or less, and most preferably 0.5 mol% or less. Here, when the polyethylene resin (C) of the present invention contains a structural unit derived from a third α-olefin, the total of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol%. In this case, the content of the structural units derived from propylene is preferably higher than the content of the structural units derived from the third α-olefin. Furthermore, when the polyethylene resin (C) of the present invention contains structural units derived from a third α-olefin, one or more kinds of the third α-olefin can be used. The polyethylene resin (C) may be one type or a combination of two or more types, so long as it satisfies (c-1) to (c-7). When propylene is used as a secondary component and is an essential comonomer, and in particular when high-pressure ionic polymerization using a metallocene catalyst (described later) is used, it is possible to obtain ethylene-α-olefin copolymers with a specifically high total number of vinyl and vinylidene units. This effect is difficult to obtain when α-olefins such as 1-hexene and 1-octene are polymerized as the main comonomer components.

[0034] (c-5) Density The polyethylene resin (C) used in the present invention has a density of 0.88 to 0.94 g / cm 3 and preferably 0.88 to 0.93 g / cm 3 and more preferably 0.88 to 0.92 g / cm 3 The density is 0.88g / cm 3If the density is less than 0.94 g / cm3, blocking will be poor, which is not preferred. 3 If it exceeds this value, the adhesiveness becomes poor, which is not preferable.

[0035] The density of the polymer can be adjusted by appropriately adjusting, for example, the comonomer content, polymerization temperature, catalyst amount, etc. The density of the polyethylene resin (C) is measured in accordance with JIS-K6922-2:1997 Appendix (for low-density polyethylene) (measurement temperature 23°C).

[0036] (c-6) Total number of vinyls and vinylidenes In copolymers obtained by copolymerizing ethylene with one or more α-olefins, even if diene monomers are not actively added, various double bonds (vinyl, vinylidene, cis-vinylene, trans-vinylene, tri-substituted olefins) may be produced due to differences in the mechanisms of the manufacturing process, and the amounts and types of double bonds vary. In the present invention, it has been found that, among various double bonds contained in polyethylene resin (C), vinyl and vinylidene are particularly important in terms of adhesive strength, and it has also been found that a resin composition containing polyethylene resin (C) in which the total number of vinyl and vinylidene is greater than that of a normal ethylene-α-olefin copolymer is particularly suitable as a resin composition for low-temperature lamination and achieves the effects of the present invention, and has been completed based on this discovery.

[0037] The polyethylene resin (C) used in the present invention has a total number of vinyl and vinylidene double bonds per 1000 carbon atoms in total in the main chain and side chains, as measured by NMR, of 0.35 (units / total 1000 C) or more, preferably 0.40 to 5.0 (units / total 1000 C), more preferably 0.45 to 4.5 (units / total 1000 C), and even more preferably 0.50 to 4.0 (units / total 1000 C). When the total number of vinyl and vinylidene is within the above range, the resin composition has excellent adhesive strength, and when it is less than 0.35, the adhesive strength is not sufficient. The total number of vinyl and vinylidene can be controlled within the above range by appropriately selecting a suitable metallocene catalyst, adjusting the polymerization temperature, the type of comonomer, and the amount of comonomer. The number of double bonds is per 1,000 carbon atoms in the main chain and side chains combined. 1 The value was calculated using the integrated intensity of a characteristic peak in the H-NMR spectrum, and was measured and calculated under the conditions described in the Examples below. Furthermore, in the present invention, the number of vinyl groups in the polyethylene resin (C) preferably satisfies the range of 0.2 (groups / total 1000C) or more. In the present invention, the number of vinylidene units in the polyethylene resin (C) preferably satisfies the range of 0.12 (units / total 1000C) or more.

[0038] (c-7) Relationship between branch number (Y) and density (X) due to comonomer The polyethylene resin (C) used in the present invention preferably has a branch number (Y) due to a comonomer and a density (X) that satisfy the following formula (1). Formula (1): (Y) ≧ -1157×(X)+1084 When the density and the number of branches satisfy the relationship of the above formula (1), the number of branches due to the comonomer is sufficiently ensured, resulting in a resin composition with excellent adhesive strength. Here, the number of branches (Y) due to comonomers is the number per 1000 total carbon atoms in the main chain and side chains (number / total 1000C) measured by NMR for the polyethylene resin (C). Moreover, the density (X) is the density of the polyethylene resin (C) and is measured as described above. The number of branches (Y) due to comonomers indicates the amount of tertiary carbons contained in the polymer, and is the number per 1000 carbons in total in the main chain and side chains, as measured by NMR. For example, see EW Hansen, R. Blom, and OM Bade, Polymer, Vol. 36, p. 4295 (1997). 13It can be calculated from the C-NMR spectrum. The relationship between the density and the number of branches can be adjusted by the polymerization conditions such as the type and ratio of the comonomers to be copolymerized and the polymerization temperature.

[0039] (ii) Polymerization catalyst and polymerization method for polyethylene resin (C) The catalyst used in the production of the polyethylene resin (C) used in the present invention is not particularly limited, but a metallocene catalyst is more preferably used. The metallocene catalyst is not particularly limited, but may be a catalyst containing a metallocene compound such as a zirconium compound coordinated with a group having a cyclopentadienyl skeleton and a cocatalyst as a catalytic component. In particular, it is preferable to use a metallocene compound such as a zirconium compound coordinated with a group having a cyclopentadienyl skeleton. The production method is not particularly limited, and a high-pressure ionic polymerization method, a gas phase method, a solution method, a slurry method, or the like can be used. In order to obtain the polyethylene resin (C) according to the present invention having adjusted double bonds, it is desirable to carry out the polymerization at a high temperature of 150 to 330° C., and therefore it is preferable to use a high-pressure ionic polymerization method (Chapter 4 of "Polyethylene Technology Reader," edited by Kazuo Matsuura and Naotaka Mikami, 2001).

[0040] (iii) Amount of polyethylene resin (C) The content of the polyethylene resin (C) in the resin composition (B) is preferably 1 to 90% by weight, more preferably 5 to 50% by weight, or even more preferably 10 to 40% by weight.

[0041] 2.5 Polyethylene resin (D) It is preferable that the polyethylene resin composition (B) further contains a polyethylene resin (D) having the following characteristics (d-1) to (d-2). (d-1) MFR (190°C, 21.18N load) is 0.1 to 100g / 10min (d-2) Density is 0.91 to 0.97 g / cm 3 Low density polyethylene is preferred.

[0042] 2.6 Additives The resin composition (B) of the present invention may be used as an ionomer resin material by blending with additives such as conventionally known antioxidants, ultraviolet absorbers, lubricants, antistatic agents, colorants, pigments, crosslinking agents, foaming agents, nucleating agents, flame retardants, conductive materials, and fillers, within the scope of the gist of the present invention. 3. Base material layer 2 (γ) The base layer 2 is a base material containing an antistatic agent, and examples thereof include a polypropylene (PP) film, a polyester (PET) film, a polyethylene (PE) film, and a linear low-density polyethylene (LLDPE) film. The resin constituting the base layer 2 is often low in crystallinity. As the antistatic agent, a known antistatic agent that has been conventionally used for preventing static electricity in OPP films and the like can be used. Examples of the antistatic agent include anionic antistatic agents such as adipic acid, glutamic acid, sulfonates, sulfate salts, phosphate salts, and phosphonate salts; cationic antistatic agents such as amines, imidazolines, amine ethylene oxide adducts, quaternary ammonium salts, and pyridinium salts; amphoteric antistatic agents having both a cationic group and an anionic group, such as guanidine salts obtained by reacting alkylamines with maleic anhydride and sulfonic acids derived from polyethyleneimine; and nonionic antistatic agents such as polyols, ester compounds of polyols and aliphatic carboxylic acids, ether compounds, higher alcohol ethylene oxide adducts, alkylphenol ethylene oxide adducts, fatty acid amides, and ethylene oxide adducts thereof.

[0043] 4.Laminate The laminate of the present invention has at least three layers: a substrate layer 1 (α), a resin layer (β), and a substrate layer 2 (γ), and is characterized in that the resin layer (β) is present between the substrate layer 1 (α) and the substrate layer 2 (γ). The substrate layer 1(α), the resin layer (β), and the substrate layer 2(γ) may be adjacent to each other or may be separated from each other, but are laminated as a whole to form a laminate. For example, an adhesive layer may be provided between the substrate layer 1(α) and the resin layer (β), or between the resin layer (β) and the substrate layer 2(γ). As long as the laminate of the present invention has the above-mentioned configuration, it may have further layers. For example, a different resin layer and / or a different substrate layer may be present on the outside of the substrate layer 1 (α) and / or the substrate layer 2 (γ).

[0044] The method for producing the laminate is not particularly limited, but for example, the so-called extrusion coating method in which a polyethylene resin composition is melt-extruded and laminated on a substrate layer is preferred. The extrusion coating is preferably performed by laminating one or more layers by a method such as a single layer, sandwich lamination, coextrusion lamination, or tandem lamination. According to the present invention, high-speed molding is possible because of good adhesion to the substrate.

[0045] The method for ensuring the adhesion between the base layer 1 (α) and the resin layer (β) is not particularly limited, but for example, the surface of the base layer 1 (α) can be subjected to a surface treatment, and if necessary, an anchor coat treatment can be performed. Examples of the surface treatment method include various treatment methods such as corona discharge treatment, ozone treatment, flame treatment, and low-temperature plasma treatment. Another example is a method of spraying ozone onto a molten resin.

[0046] One embodiment of the method for producing the laminate of the present invention is to use an extrusion lamination molding machine, feed the base layer 2 (γ) from the feeder, extrude the polyethylene resin composition (A) to form a resin layer (β) to a predetermined thickness, feed the base layer 1 (α) from the sand side, and form preferably an adhesive layer (C) on the surface of the base layer 2 (γ) on the resin layer (β) side, and perform extrusion sand lamination to produce a laminate having at least three or four layers, that is, the base layer 1 (α), the resin layer (β), the adhesive layer (C), and the base layer 2 (γ). A known adhesive can be used as the adhesive layer (C).

[0047] The laminate of the present invention exhibits good adhesion even when laminated to a substrate containing an antistatic agent, and is a laminate having good adhesion even under high temperature conditions, and therefore can be suitably used particularly as films for packaging bags, films for packaging food, paper containers for liquids, packaging containers for frozen desserts such as yokan and jelly, dried foods, oils and fats, confectioneries, etc., paper bundling, paper cups, paper trays, etc. EXAMPLES

[0048] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. The measurement methods, resins, and adhesives used in the examples and comparative examples are as follows.

[0049] 1. Evaluation method for resin properties (1) Melt flow rate (MFR) The MFR was measured in accordance with JIS-K6922-2:1997 Appendix (190°C, 21.18N load). (2) Density The density was measured in accordance with JIS-K6922-2:1997 Appendix (23°C, in the case of low-density polyethylene).

[0050] (3) Total heat of fusion ΔHm, crystallization temperature Tc The total heat of fusion ΔHm and the crystallization temperature Tc were measured according to the method of JIS K7121-1987. The pellets were hot pressed into a sheet, which was then punched out as a measurement sample. The measurement was carried out under the following conditions, with the first heating, the temperature drop, and the second heating in sequence. The temperature of the maximum peak height during the temperature drop was taken as Tc, and the heat of fusion in the melting curve during the second heating was taken as ΔHm. Equipment: SII NanoTechnology Inc. DSC7020 <Temperature rise and fall conditions> First temperature rise: 30℃ to 200℃ at 10℃ / min -Temperature drop: 200℃ to -30℃ at 10℃ / min Second temperature rise: -30℃ to 200℃ at 10℃ / min Temperature retention time: 5 minutes after first temperature rise, 5 minutes after temperature fall Sample size: 5mg Temperature Calibration: Indium Reference: Aluminum

[0051] (4) Amount of comonomer, number of branches and number of double bonds due to comonomer The amount of comonomer and the number of branches due to the comonomer (Y) were measured by 13C-NMR, and the number of double bonds (vinyl, vinylidene) was measured by 1H-NMR under the following conditions, and were calculated as the number per 1000 carbons in total in the main chain and side chains. Equipment: Bruker Biospin AVANCE III cryo-400MHz Solvent: o-dichlorobenzene / bromobenzene = 8 / 2 mixed solution <Sample amount> Sample 460mg / solvent 2.3ml <13C-NMR> 1H decoupled, NOE available Number of scans: 256 Flip angle: 90° · Pulse interval 20 seconds · AQ (acquisition time) = 5.45s D1 (waiting time) = 14.55s <1H-NMR> - Number of scans: 1400 Flip angle: 1.03° AQ (acquisition time) = 1.8s D1 (waiting time) = 0.01s

[0052] (4) Adhesive strength The obtained laminate was cut into strips 15 mm wide in the machine direction, and peeled at the interface between the base layer 1 (α) and the resin layer (β). The adhesive strength was determined by the peel strength in a T-peel test using 5 specimens at a peel speed of 300 mm / min.

[0053] (5) Heat seal strength Two of the obtained laminates were stacked, the temperature of the lower sealing bar was set to 30 °C, the temperature of the upper sealing bar was 140 °C, the sealing pressure was 0.2 MPa, and heat sealing was performed for a sealing time of 1.0 second. The 180° peel strength with a width of 15 mm was measured. Based on the obtained heat seal strength values, the heat sealability was evaluated according to the following criteria. ○: The heat seal strength is 10 N / 15 mm width or more. ×: The heat seal strength is less than 10 N / 15 mm width.

[0054] 2. Materials (1) Polar ethylene copolymer (A) or ionomer (A’) (PE-1), (PE-4) (PE-1) and (PE-4) were obtained by the production methods of ionomer 1 and ionomer 2 described in JP-A-2022-150804. The physical properties of the obtained resins are shown in Tables 1 and 2. Commercially available (PE-2, PE-3, PE-5) were used as the ethylene copolymer or ionomer of component (A or A’), respectively. The physical property values are shown in Tables 1 and 2. (PE-2): Himilan 1652 manufactured by Mitsui Dow Polychemical Co., Ltd. (PE-3): Lexparl EB240H manufactured by Japan Polyethylene Corporation (PE-5): Nuclel N1108C manufactured by Mitsui Dow Polychemical Co., Ltd. (2) Polyethylene resin (C) (PE-6) obtained by the following production method was used as the polyethylene resin (C). The physical property values are shown in Tables 1 and 2.

[0055] <Production method of PE-6> (i) Preparation of catalyst To 0.05 mol of the complex “rac-dimethylsilylenebisindenylhafnium dimethyl” prepared by the method described in JP-A-10-218921, an equimolar amount of “N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate” was added and diluted to 50 liters with toluene to prepare a catalyst solution.

[0056] (ii) Polymerization method A stirring autoclave type continuous reactor with an internal volume of 5.0 liters was used, the pressure inside the reactor was kept at 80 MPa, and the raw material gas was continuously supplied at a rate of 40 kg / hour while appropriately adjusting the ethylene and propylene. In addition, the catalyst solution described in the above section "(i) Adjustment of catalyst" was continuously supplied, and the polymerization temperature was appropriately adjusted within the range of 150 to 250°C to obtain a polyethylene resin (C).

[0057] (3) Polyethylene resin (D) A polyethylene resin (PE-7) having the physical properties shown in Tables 1 and 2 was used.

[0058] (4) Adhesive layer As the adhesive layer, (AC-1) described below was used. (AC-1) Toyo Morton Olivine EL420 and methanol mixed in a ratio of 1:6.

[0059] (5) Base material layer 1 (α) Aluminum foil manufactured by Toyo Aluminum Co., Ltd. (thickness: 7 μm, oxygen permeability is approximately 0 mL / m at 20°C and 65% RH) 2 ·day·MPa) was used. Hereinafter, this will be referred to as (Group-1).

[0060] (6) Base material layer 2 (γ) An OPP film FOR (thickness 20 μm) containing an antistatic agent manufactured by Futamura Chemical Co., Ltd. was used. Hereinafter, this is referred to as (Group-2).

[0061] Example 1 15% by weight of ionomer (A') (PE-1), 17% by weight of polyethylene resin (C) (PE-6), and 68% by weight of polyethylene resin (D) (PE-7) were blended together and thoroughly mixed, followed by using a 40 mmφ single-screw extruder to obtain pellets of polyethylene resin composition (B). Using an extrusion lamination molding machine, a 500 mm wide (base-2) was fed from the feeder as the base layer 2 (γ), and the pellets obtained above were adjusted to a take-up speed of 100 m / min and a coating thickness of 15 μm, and (base-1) was fed from the sand side as the base layer 1 (α), and extrusion sand lamination was performed. Next, anchor coating treatment was performed using (AC-1) on the opposite side of the resin layer (β) side of the base layer 1 (α), and LDPE (Novatec LC600A manufactured by Japan Polyethylene Co., Ltd.) was extrusion laminated at a take-up speed of 100 m / min and a coating thickness of 20 μm to obtain a laminate of the base layer 2 (γ), the resin layer (β), the base layer 1 (α), and the LC600A layer. The extrusion lamination molding machine was set so that the temperature of the resin extruded from the T-die attached to the extruder with a diameter of 90 mm was 310°C, and the extrusion rate was adjusted so that the coating thickness would be the specified value when the cooling roll surface temperature was 20°C, the die width was 560 mm, and the take-up speed was 100 m / min. Next, the adhesive strength and heat seal strength were evaluated using the obtained laminate. The evaluation results are shown in Table 1.

[0062] Example 2 A laminate was produced in the same manner as in Example 1, except that 7% by weight of the ionomer (A') (PE-1), 18.6% by weight of the polyethylene resin (C) (PE-6), and 74.4% by weight of the polyethylene resin (D) (PE-7) were used. The evaluation results are shown in Table 1.

[0063] Example 3 A laminate was produced in the same manner as in Example 1, except that PE-2 was used instead of the ionomer body (A') in Example 1. The evaluation results are shown in Table 1.

[0064] Example 4 15% by weight of the ionomer (A') (PE-4) and 85% by weight of the polyethylene resin (D) (PE-7) were blended together and thoroughly mixed, followed by using a 40 mmφ single screw extruder to obtain pellets of the polyethylene resin composition (B). Using an extrusion lamination molding machine, a 500 mm wide (base-2) was fed from the feeder as the base layer 2 (γ), and the pellets obtained above were adjusted to a take-up speed of 100 m / min and a coating thickness of 15 μm. The (base-1) was fed from the sand side as the base layer 1 (α), and extrusion sand lamination was performed. At this time, anchor coating treatment was performed using (AC-1) as an adhesive layer on the base layer 2 (γ) surface on the resin layer (β) side. Next, anchor coating treatment was performed using (AC-1) on the opposite surface of the resin layer (β) side of the base layer 1 (α), and LDPE (Novatec LC600A manufactured by Japan Polyethylene Co., Ltd.) was extrusion laminated at a take-up speed of 100 m / min and a coating thickness of 20 μm to obtain a laminate of the base layer 2 (γ), the resin layer (β), the base layer 1 (α), and the LC600A layer. The extrusion lamination molding machine was set so that the temperature of the resin extruded from the T-die attached to the extruder with a diameter of 90 mm was 310°C, and the extrusion rate was adjusted so that the coating thickness would be the specified value when the cooling roll surface temperature was 20°C, the die width was 560 mm, and the take-up speed was 100 m / min. Next, the adhesive strength and heat seal strength were evaluated using the obtained laminate. The evaluation results are shown in Table 2.

[0065] Example 5 A laminate was produced in the same manner as in Example 4, except that 15% by weight of the ionomer (A') (PE-4), 17% by weight of the polyethylene resin (C) (PE-6), and 68% by weight of the polyethylene resin (D) (PE-7) were used. The evaluation results are shown in Table 2.

[0066] Example 6 A laminate was produced in the same manner as in Example 4, except that 15% by weight of polar polyethylene resin (A) (PE-5), 17% by weight of polyethylene resin (C) (PE-6), and 68% by weight of polyethylene resin (D) (PE-7) were used. The evaluation results are shown in Table 2.

[0067] Comparative Example 1 A laminate was produced in the same manner as in Example 1, except that 100% by weight of the polyethylene resin (D) (PE-7) was used. The evaluation results are shown in Table 1.

[0068] Comparative Example 2 A laminate was produced in the same manner as in Example 1, except that 20% by weight of the polyethylene resin (C) (PE-6) and 80% by weight of the polyethylene resin (D) (PE-7) were used in Example 1. The evaluation results are shown in Table 1.

[0069] Comparative Example 3 A laminate was produced in the same manner as in Example 1, except that 15% by weight of polar polyethylene resin (A) (PE-3), 17% by weight of polyethylene resin (C) (PE-6), and 68% by weight of polyethylene resin (D) (PE-7) were used in Example 1. The evaluation results are shown in Table 1.

[0070] Comparative Example 4 A laminate was produced in the same manner as in Example 4, except that 100% by weight of the polyethylene resin (D) (PE-7) was used. The evaluation results are shown in Table 2.

[0071] Comparative Example 5 A laminate was produced in the same manner as in Comparative Example 4, except that the resin temperature was changed to 325° C. The evaluation results are shown in Table 2.

[0072] Comparative Example 6 A laminate was produced in the same manner as in Example 4, except that 20% by weight of the polyethylene resin (C) (PE-6) and 80% by weight of the polyethylene resin (D) (PE-7) were used. The evaluation results are shown in Table 2.

[0073] [Table 1]

[0074] [Table 2]

[0075] (Results of Examples and Comparative Examples) Comparing the above Examples 1 to 3 with Comparative Examples 1 to 3, it is found that the laminate using the ionomer (A') of the polar ethylene copolymer of the present invention is excellent in adhesive strength between the base layer 1 (α) and the resin layer (β) and is also excellent in heat seal strength. In particular, the adhesive strength does not decrease even after storage at high temperatures. Furthermore, by comparing the results of Example 1 with Example 3, it is found that Example 1, which is a laminate using a polar ethylene copolymer or ionomer having a linear molecular structure (phase angle δ is 50 degrees to 75 degrees at absolute value of complex elastic modulus G*=0.1 MPa measured with a rotational rheometer), is a laminate having superior adhesive strength and heat seal strength to Example 3, which uses a polar ethylene copolymer or ionomer having a branched structure. Comparison of the results of Examples 4 to 6 with Comparative Examples 4 to 6 shows that the laminate using the polar ethylene copolymer (A) and / or its ionomer (A') of the present invention is excellent in adhesive strength between the base layer 1 (α) and the resin layer (β) and is also excellent in heat seal strength. Comparison of the results of Example 5 with Example 4 shows that the laminate containing the polyethylene resin (C) is superior in adhesive strength and heat seal strength. On the other hand, by comparing the results of Comparative Example 5 with those of Comparative Example 4, it can be seen that the adhesive strength and heat seal strength of the 325°C processed product of Comparative Example 5 stored at 23°C and 50% for one week were good, but that the adhesive strength and heat seal strength of the product stored at 40°C and 90% for one week decreased.

Claims

1. A laminate having at least three layers, namely, a substrate layer 1 (α), a resin layer (β), and a substrate layer 2 (γ), each of which satisfies the following properties. Substrate layer 1 (α): Oxygen permeability is 1300 mL / m at 20° C. and 65% RH 2 ·day·MPa or less. Resin layer (β): comprises a polyethylene resin composition (B) containing 2 to 40 parts by weight of a polar ethylene copolymer (A) having the following characteristic (a) and / or an ionomer (A') of the polar ethylene copolymer (A). (a) Contains, as essential structural units, a structural unit (m) derived from ethylene and a structural unit (n) derived from a monomer having a carboxy group. Substrate layer 2 (γ): Substrate containing an antistatic agent

2. The laminate according to claim 1, wherein the polyethylene resin composition (B) further contains a polyethylene resin (C) having the following characteristics (c-1) to (c-7): (c-1) MFR (190°C, 21.18N load) of 0.1 to 100g / 10min (c-2) In DSC, the total heat of fusion ΔHm is 30 to 120 J / g. (c-3) Crystallization temperature Tc is 25 to 90° C. (c-4) Contains 80 to 98 mol % of structural units derived from ethylene as a main component, 2 to 20 mol % of structural units derived from propylene as an essential minor component, and may contain 5 mol % or less of structural units derived from a third α-olefin other than ethylene and propylene as a minor component. (However, when the structural units derived from the third α-olefin are contained, the total amount of the structural units derived from ethylene, the structural units derived from propylene, and the structural units derived from the third α-olefin does not exceed 100 mol %). (c-5) density is 0.88 to 0.94 g / cm 3 (c-6) The total amount of vinyl and vinylidene in the polyethylene resin (C) is 0.35 (pieces / total 1000C) or more (Note that the number of vinyl and vinylidene groups is the number per 1,000 carbon atoms in total in the main chain and side chains as measured by NMR.) (c-7) The number of branches (Y) due to comonomers in the polyethylene resin (C) and the density (X) satisfy the relationship of the following formula (1). Formula (1): (Y)≧−1157×(X)+1084 (where Y is the number per 1000 total carbon atoms in the main chain and side chains as measured by NMR.)

3. The ionomer (A') of the polar ethylene copolymer (A) is further characterized in that the phase angle δ at an absolute value of the complex elastic modulus G*=0.1 MPa measured by a rotational rheometer is 50 degrees to 75 degrees.

4. The laminate according to claim 1 or 2, wherein the polyethylene resin composition (B) further contains a polyethylene resin (D) having the following characteristics (d-1) to (d-2): (d-1) MFR (190°C, 21.18N load) is 0.1 to 100g / 10min (d-2) Density is 0.91 to 0.97 g / cm 3

5. The ionomer (A') of the polar ethylene-based copolymer (A) is characterized in that at least a part of the carboxy groups of the polar ethylene-based copolymer (A) is converted into a metal-containing carboxylate salt containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table.

6. The laminate according to claim 1 or 2, characterized in that the polar ethylene-based copolymer (A) contains 70 to 98 mol % of a structural unit (m) derived from ethylene as a main component and 2 to 30 mol % of a structural unit (n) derived from a monomer having a carboxy group as an essential subcomponent.

7. 3. The laminate according to claim 1, wherein the substrate layer 1 (α) is a metal foil or a metal-deposited film.

8. 3. The laminate according to claim 1, wherein the laminate is formed by an extrusion coating method.

9. A packaging material comprising the laminate according to claim 1 or 2.