Ethylene vinyl alcohol copolymer for melt electrowriting molding, laminated product composed of the copolymer, and method for producing the laminated product

The use of ethylene vinyl alcohol copolymer with defined properties addresses thermal decomposition issues in MEW molding, resulting in laminates with enhanced mechanical strength and biocompatibility for cell scaffolding materials.

JP2024147138AInactive Publication Date: 2024-10-16MITSUBISHI CHEM CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023059956
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-16
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Laminates manufactured using thermoplastic resins like PCL and PLLA for cell scaffolding materials via MEW molding suffer from thermal decomposition during processing, leading to decreased molecular weight and mechanical strength.

Method used

Employing an ethylene vinyl alcohol copolymer with specific properties such as a melt index of 60 g/10 minutes or more, melt viscosity of 2000 Pa·s or less, apparent viscosity of 500 Pa·s or less, and a half-crystallization time of 4 minutes or more, for MEW molding to produce fibers and laminates with high mechanical strength and biocompatibility.

Benefits of technology

The ethylene vinyl alcohol copolymer enables the formation of laminates with excellent biocompatibility and high mechanical strength, suitable for cell scaffolding materials and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147138000004
    Figure 2024147138000004
  • Figure 2024147138000005
    Figure 2024147138000005
  • Figure 2024147138000006
    Figure 2024147138000006
Patent Text Reader

Abstract

To provide a material for melt electrowriting (MEW) molding that yields a laminated product with superior biocompatibility and high mechanical strength.SOLUTION: An ethylene vinyl alcohol copolymer with a melt index of at least 60 g / 10 min, measured at 220°C and 2.16 kg, is suitable for MEW molding applications. The copolymer is utilized as a material to form fibers with a melt electrowriting (MEW) device, and the fibers are laminated to form a laminated product.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ethylene-vinyl alcohol copolymer (EVOH) for melt electrolighting molding, which can be suitably used for molding cell scaffold materials and the like, and a laminate made of said copolymer. [Background technology]

[0002] In regenerative medicine, scaffolds are used to allow cells to adhere and grow. For example, nonwoven fabrics with a high specific surface area for cell adhesion are produced by electrospinning as scaffolds. In recent years, a technology has been established that can form regular structures on the microscale with fiber diameters of 1 to 50 μm by melt electrowriting, which is one of the electrospinning techniques.

[0003] Melt Electrowriting (MEW) is a method that combines electrospinning and AM (Additive Manufacturing) technologies, in which a jet of molten polymer is controlled and rapidly solidified to form fibers. It is said to be able to stably layer micron-sized fibers and directly draw complex structures, overcoming the resolution problems that many other additive manufacturing technologies have.

[0004] As an example of a scaffold formed using such MEW, Patent Document 1 discloses a cell scaffold having a specific arrangement structure using a thermoplastic resin such as PCL (polycaprolactone). Non-Patent Document 1 discloses a cell scaffold using PLLA (poly-L-lactic acid). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2020 / 210877 [Non-patent literature]

[0006] [Non-Patent Document 1] Huaizhong Xu etc., “Design and manufacturing of 3D high-precision micro-fibrous poly(L-lactic acid) scaffold using melt electrowriting technique for bone tissue engineering”, Materials & Design, Vol.210(2021), 110063 Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, attempts have been made to use MEW molding to mold laminates using thermoplastic resins such as PCL and PLLA to serve as cell scaffolds and the like. However, laminates produced by MEW molding using PCL, PLLA, etc., tend to decompose when heated during molding, resulting in a decrease in molecular weight and a decrease in mechanical strength.

[0008] Therefore, in order to solve the above problems, the object of the present invention is to provide a MEW molding material that can give a laminate having excellent biocompatibility and high mechanical strength, a laminate using the same, and a method for manufacturing the laminate. [Means for solving the problem]

[0009] The present invention relates to the following [1] to

[12] .

[0010] [1] Ethylene-vinyl alcohol copolymer for melt electrolighting (MEW) molding, with a melt index of 60 g / 10 min or greater measured at 220°C and 2.16 kg.

[0011] [2] The ethylene-vinyl alcohol copolymer according to [1], having a melt viscosity of 2000 Pa s or less after heating at 240°C for 3 hours at 0.5 Hz as measured with a rheometer.

[0012] [3] The ethylene-vinyl alcohol copolymer according to [1] or [2], having an apparent viscosity of 500 Pa s or less at a shear rate of 100 to 10,000 [1 / s] after heat treatment at 240°C for 9 hours.

[0013] [4] The ethylene-vinyl alcohol copolymer according to any one of [1] to [3], wherein the semi-crystallization time at a cooling crystallization temperature (Tc) + 10°C is 4 minutes or longer.

[0014] [5] A fiber made of the ethylene-vinyl alcohol copolymer according to any one of [1] to [4] or a laminate made of such fibers.

[0015] [6] The fiber or laminate according to [5], wherein the fiber diameter of the fibers is 0.1 μm to 500 μm.

[0016] [7] The fiber or laminate according to [5] or [6], wherein the number of layers in the laminate is 1 to 500.

[0017] [8] A method for producing a laminate by forming fibers using an ethylene-vinyl alcohol copolymer described in any one of [1] to [4] by MEW molding and stacking the fibers.

[0018] [9] The method for producing a laminate according to [8], wherein the table temperature when producing the laminate is 70°C or higher.

[0019]

[10] The method for producing a laminate according to [8] or [9], wherein the syringe temperature during production of the laminate is 230°C or higher.

[11] The method for producing a laminate described in any one of [8] to

[10] , wherein the table / nozzle distance when producing the laminate is 2 mm or less.

[0020]

[12] The method for producing a laminate described in any one of [8] to

[11] , wherein the nozzle diameter when producing the laminate is 0.6 mm or less. Effect of the Invention

[0021] The present invention makes it possible to form a laminate having excellent biocompatibility and high mechanical strength by performing MEW molding using an ethylene-vinyl alcohol copolymer (EVOH) having specific physical properties. [Brief description of the drawings]

[0022] [Figure 1] FIG. 2 is a diagram for explaining MEW molding in one example of a method for producing a laminate of the present invention. [Diagram 2] FIG. 2 is a diagram for explaining a MEW apparatus in an example of a method for producing a laminate of the present invention. [Diagram 3] 1 is a micrograph showing a first structural example of a laminate of the present invention. [Figure 4] 4 is a micrograph showing a second structural example of the laminate of the present invention. [Diagram 5] 4 is a micrograph showing a third structural example of the laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, the present invention will be described based on one embodiment, however, the present invention is not limited to the embodiment described below.

[0024] (Book EVOH) An ethylene-vinyl alcohol copolymer (hereinafter, also referred to as the present EVOH) for molten electrolighting (hereinafter, also referred to as MEW) molding according to one embodiment of the present invention is characterized in that it has a melt index (MI) measured at 220°C and 2.16 kg of 60 g / 10 min or more.

[0025] This EVOH is suitable for MEW molding. MEW molding is, for example, a method in which a polymer is heated and melted in a syringe with a nozzle, the polymer is charged by applying a voltage, and the molten polymer in the syringe is continuously extruded from the nozzle by pressurizing with nitrogen or the like to form micron-sized fibers on a table. By controlling the movement of the nozzle or table or the voltage between the table and the nozzle, a three-dimensional object of any shape can be formed. Conventional solution electrospinning is a method in which a polymer is dissolved in a solvent, whereas MEW differs in that the polymer is melted. For details about MEW, please refer to the paper by Huaizhong Xu et al., “Design and manufacturing of 3D high-precision micro-fibrous poly(L-lactic acid) scaffold using melt electrowriting technique for bone tissue engineering”, Materials & Design, Vol.210(2021), 110063, especially “2.1.2.Melt electrowritten device”.

[0026] MEW molding can be performed, for example, as shown in FIG. 1, using a MEW device 1 equipped with a syringe 2 having a nozzle 3, a table 4, and the like. A material is put into the syringe 2 and heated to 60 to 300°C to melt it, and the molten material is charged with a voltage of 1 to 5 kV (charged positively (+) in FIG. 1). Air such as nitrogen is filled from above to pressurize the syringe 2 to 0.02 to 0.20 MPa, and the molten material in the syringe 2 is continuously extruded from the nozzle 3 and cooled and solidified on the table 4 to form a thread-like fiber. Note that the table 4 is negatively charged (-) in FIG. 1. The table 4 is movable on a horizontal plane according to a preset pattern, and the extruded material can be arranged at a desired position on the table 4. By repeatedly moving the table 4 along the same or different paths, the fibers are layered and a laminate with a preset three-dimensional structure can be formed.

[0027] A specific example of the MEW device will be described with reference to FIG. 2. The device includes a MEW needle equipped with a nozzle 3 and a syringe 2, and a table 4. The syringe 2 is made of stainless steel or the like, and can be filled with material. The syringe 2 can be heated with a heater to melt the material inside, and nitrogen (N2) can be injected into the syringe 2 to apply pressure, and the molten material can be continuously pushed out from the syringe 2. It is preferable to inject nitrogen into the syringe 2 and apply pressure in the range of 0.02 to 0.20 MPa. It is preferable that the nozzle 3 and table 4 are connected to a positive and negative power source, or a combination of either a positive or negative power source and a ground, and a voltage of 1 to 5 kV is applied. It is also preferable that the syringe 2 is covered with a ceramic cover to insulate it from high voltage, and the nozzle 3 is covered with a copper plate or the like to prevent heat loss at the tip. The table is movable, and the movement speed is preferably a maximum of 250 mm / s and the movement accuracy is preferably 0.1 μm to 10 μm. Also, the table can be heated by a heater.

[0028] This EVOH has a melt index (MI) of 60 g / 10 min or more, measured at 220°C and 2.16 kg. A melt index within this range allows for favorable use in terms of fluidity during MEW molding, and enables the production of three-dimensional structures with high mechanical strength. From this viewpoint, the melt index is preferably 62 g / 10 min or more, more preferably 64 g / 10 min or more, and even more preferably 68 g / 10 min or more. The upper limit is not particularly limited, but is preferably 150 g / 10 min or less, more preferably 100 g / 10 min or less, from the viewpoint of avoiding a decrease in the mechanical strength of the laminate due to an excessively low molecular weight of the resin. The melt index can be measured, for example, in accordance with JIS K7210 (2014).

[0029] The present EVOH is a copolymer of vinyl alcohol and ethylene represented by the following formula 1, and the ethylene content is preferably 30 mol % to 43 mol %, and more preferably 35 mol % to 40 mol %.

[0030] [ka]

[0031] The EVOH preferably has a melt viscosity of 2000 Pa·s or less after heating at 240°C for 3 hours at 0.5 Hz as measured with a rheometer. This range is preferable in that it enables the material to be efficiently discharged from the nozzle during MEW molding. From this viewpoint, the viscosity is more preferably 1000 Pa·s or less, and even more preferably 300 Pa·s or less. Although there is no particular lower limit, the viscosity is preferably 10 Pa·s or more, and more preferably 100 Pa·s or more. The melt viscosity can be measured, for example, using a commercially available rheometer in accordance with JIS K7244-10 (2005).

[0032] The present EVOH preferably has an apparent viscosity of 500 Pa·s or less at a shear rate in the range of 100 to 10,000 [1 / s] after heat treatment at 240° C. for 9 hours. This range is preferable in that the material can be efficiently discharged from the nozzle during MEW molding. From this viewpoint, the viscosity is more preferably 200 Pa·s or less, and even more preferably 160 Pa·s or less. Although there is no particular lower limit, the viscosity is preferably 10 Pa·s or more, and more preferably 40 Pa·s or more. The term "heat treatment at 240°C for 9 hours" means that a material processed into a sheet having a thickness of 0.5 mm is sandwiched between 25 μm thick polyimide films, which are then sandwiched between 1 mm thick stainless steel plates, and then heat-treated for 9 hours in an oven heated to 240°C. The apparent viscosity can be measured, for example, in accordance with JIS K7117-1 (1999), at a measurement temperature of 240°C.

[0033] The present EVOH preferably has a crystallization half time of 4 minutes or more at a crystallization temperature (Tc) + 10°C upon cooling. This range is preferable in that fiber formation during MEW molding is good. From this viewpoint, 6 minutes or more is more preferable, and 8 minutes or more is even more preferable. The upper limit is not particularly limited, but 20 minutes or less is preferable. The crystallization half time can be calculated, for example, based on a crystallization peak that appears when the material is held under isothermal conditions for a certain period of time in differential scanning calorimetry.

[0034] The EVOH may contain other ingredients. Other components include additives such as heat resistance agents, ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, lubricants, slip agents, crystal nucleating agents, tackifiers, sealability improvers, antifogging agents, release agents, plasticizers, pigments, dyes, fragrances, flame retardants, biodegradation promoters, ester exchange promoters, and ester exchange inhibitors, as well as inorganic fillers such as calcium carbonate, zinc carbonate, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, sodium aluminosilicate, magnesium silicate, potassium titanate, glass balloons, glass flakes, glass powder, silicon carbide, silicon nitride, boron nitride, gypsum, calcined kaolin, zinc oxide, antimony trioxide, zeolite, hydrotalcite, wollastonite, silica, talc, metal powder, alumina, graphite, carbon black, carbon nanotubes, glass cut fibers, glass milled fibers, glass fibers, gypsum whiskers, metal fibers, metal whiskers, ceramic whiskers, carbon fibers, and cellulose nanofibers. When other components are contained, their content in the present EVOH is preferably 30% by mass or less, and more preferably 5% by mass or less.

[0035] (This laminate) By using MEW molding, the present EVOH can be made into filamentous fibers or a laminate in which the fibers are laminated (hereinafter, also referred to as the present laminate). The laminate can have a three-dimensional structure, for example, a lattice structure in which square or rectangular spaces are regularly arranged in a plan view (see FIG. 3), a diagonal lattice structure in which diamond-shaped spaces are regularly arranged in a plan view, a honeycomb structure in which hexagons are regularly arranged in a plan view (see FIG. 4), a structure in which each row in the vertical and horizontal directions is sinusoidally curved and equally spaced in the vertical and horizontal directions (see FIG. 5), etc. The length of one side of the repeating structural unit in these spaces is not particularly limited, but is preferably 20 μm to 1000 μm, more preferably 100 μm to 500 μm.

[0036] The above fibers preferably have a fiber diameter of 0.1 μm to 500 μm. This range is preferable in terms of achieving both strength and the possibility of achieving the effect of increasing the specific surface area. From this viewpoint, 1 μm to 100 μm is more preferable, and 5 μm to 30 μm is even more preferable. The fiber diameter can be measured, for example, by observation under an electron microscope, and can also be adjusted by the nozzle diameter and voltage of the MEW device.

[0037] The present laminate preferably has a laminated structure of 1 to 500 layers with the above-mentioned fibers stacked on top of each other. This range is preferable in terms of the degree of freedom in designing the laminate. From this viewpoint, 2 to 100 layers are more preferable, and 5 to 50 layers are further preferable. In the present invention, the laminate is formed by stacking the above-mentioned fibers in a regular pattern, and does not include irregular arrangements such as nonwoven fabrics.

[0038] The laminate preferably has a tensile strength of 8 cN / dtex or more. When the content is within this range, the mechanical strength of the laminate becomes good, which is preferable in terms of the applicability to various applications. From this viewpoint, 10 cN / dtex or more is more preferable, and 12 cN / dtex or more is even more preferable. Although there is no particular upper limit, 30 cN / dtex or less is preferable. The tensile strength of the laminate can be measured, for example, by the method shown in the Examples below, and can be adjusted to fall within the above range by forming an appropriate number of layers using the present EVOH in MEW molding.

[0039] The present laminate preferably has a breaking elongation of 10% or more. When the content is within this range, the mechanical strength of the laminate becomes good, which is preferable in terms of the applicability to various applications. From this viewpoint, 50% or more is more preferable, and 100% or more is even more preferable. Although there is no particular upper limit, 500% or less is preferable. The breaking elongation of the laminate can be measured, for example, by the method shown in the Examples below, and can be adjusted to fall within the above range by using the present EVOH and forming an appropriate number of layers in MEW molding.

[0040] The present laminate preferably has a tensile strength per fiber of 50 MPa or more. This range is preferable in that the mechanical strength of the laminate is maintained. From this viewpoint, the pressure is more preferably 55 MPa or more, and even more preferably 60 MPa or more. There is no particular upper limit, but the pressure is preferably 100 MPa or less. The tensile strength per fiber of the laminate can be measured, for example, by the method shown in the Examples below, and can be adjusted to fall within the above range by MEW molding using the present EVOH.

[0041] The present laminate preferably has a breaking elongation per fiber of 10% or more. This range is preferable in that the mechanical strength of the laminate is maintained. From this viewpoint, 50% or more is more preferable, and 100% or more is even more preferable. Although there is no particular upper limit, 500% or less is preferable. The breaking elongation per fiber of the laminate can be measured, for example, by the method shown in the Examples below, and can be adjusted to fall within the above range by MEW molding using the present EVOH.

[0042] (Manufacturing method) The present EVOH can be produced, for example, by copolymerizing ethylene and vinyl alcohol. The melt index of the present EVOH can be adjusted to an appropriate range by adjusting, for example, the copolymerization ratio or molecular weight. In addition, the melt viscosity can be adjusted to an appropriate range by, for example, adjusting the copolymerization ratio or the molecular weight, the apparent viscosity can be adjusted to an appropriate range by, for example, adjusting the copolymerization ratio or the molecular weight, and the crystallization half time can be adjusted to an appropriate range by, for example, adjusting the stereoregularity, copolymerization ratio, or molecular weight.

[0043] The present laminate can be produced by forming the present EVOH into thread-like, string-like or elongated fibers by MEW molding, and laminating the fibers.

[0044] The table temperature during production of the present laminate is preferably 70° C. or higher. This range is preferable in terms of adhesion of the laminate to the table. From this viewpoint, the temperature is more preferably 100° C. or higher, and even more preferably 115° C. or higher. There is no particular upper limit to the temperature, but the temperature is preferably 150° C. or lower in order to prevent thermal deterioration of the resin.

[0045] The syringe temperature during production of the present laminate is preferably 230° C. or higher. This range is preferable in that the present EVOH can be efficiently melted in a syringe. From this viewpoint, the temperature is more preferably 235° C. or higher, and even more preferably 240° C. or higher. There is no particular upper limit to the temperature, but the temperature is preferably 300° C. or lower in order to prevent a decrease in molecular weight due to thermal decomposition of the resin.

[0046] The nozzle diameter when producing the present laminate is preferably 0.6 mm or less. This range is preferable in terms of the stability of fiber formation. From this viewpoint, it is more preferably 0.4 mm or less, and even more preferably 0.2 mm or less. There is no particular lower limit, but it is preferably 0.05 mm or more in order to avoid clogging of the nozzle.

[0047] When producing the present laminate, the distance from the top surface of the table to the tip of the nozzle (hereinafter also referred to as the table / nozzle distance) is preferably 2 mm or less. This range is preferable in terms of lamination stability during MEW molding. From this viewpoint, it is more preferable that the distance is 1.8 mm or less, and even more preferable that the distance is 1.75 mm or less. Although there is no particular lower limit, it is preferable that the distance is 0.5 mm or more in order to avoid electrical conduction caused by the table / nozzle being too close to each other.

[0048] (Application) This laminate can be formed into a three-dimensional lattice structure as shown in Figures 3 to 5 and used as a cell scaffold, etc. In addition, it can also be used as a wearable device member, for example.

[0049] The present EVOH can be suitably used for MEW molding and can be molded into any micron-sized three-dimensional structure. This EVOH can be used to form thread-like fibers by MEW molding, and laminates formed by stacking these fibers have high mechanical strength and are biocompatible, making them suitable for use as cell scaffolding materials, etc.

[0050] <Explanation of terms> In the present invention, when it is described as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as the meaning of "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified. EXAMPLES

[0051] An embodiment of the present invention will be described below, however, the present invention is not limited to the following embodiment.

[0052] The materials shown below were used to mold Examples 1 to 4 and Comparative Examples 1 and 2 shown below.

[0053] <Material> The material used for MEW molding had the following physical properties: (1) EVOH1 Melt index (MI): 71g / 10min (220℃, 2.16kg) Glass transition temperature (Tg): 59℃ Melting temperature (Tm): 175℃ Cooling crystallization temperature (Tc): 150℃ Crystallization half time at Tc+10℃: 10 min Ethylene content: 38mol% Melt viscosity after heating for 3 hours: 210 Pa s (0.5 Hz, 240°C) Apparent viscosity after 9 hours of heat treatment in the shear rate range of 100 to 10,000 [1 / s]: 150 Pa·s (240°C)

[0054] (2) EVOH2 Melt index (MI): 18g / 10min (220℃, 2.16kg) Glass transition temperature (Tg): 57℃ Melting temperature (Tm): 165℃ Cooling crystallization temperature (Tc): 140℃ Crystallization half-time at Tc+10℃: No data Ethylene content: 44mol% Melt viscosity after heating for 3 hours: 2100 Pa s (0.5 Hz, 240°C) Apparent viscosity in the shear rate range of 100 to 10,000 [1 / s] after 9 hours of heat treatment: No data

[0055] (3) PLA Melt index (MI): 11g / 10min (170℃, 2.16kg) Glass transition temperature (Tg): 64℃ Melting temperature (Tm): 174℃ Cooling crystallization temperature (Tc): 94℃ Crystallization half time at Tc+10℃: 5 min Melt viscosity after heating for 3 hours: Below measurement limit Apparent viscosity in the shear rate range of 100 to 10,000 [1 / s] after 9 hours of heat treatment: No data

[0056] (MEW device and laminate production) The MEW device used was the one shown in Figure 2. For details, please refer to the paper by Huaizhong Xu et al., shown in paragraph

[0024] , especially "2.1.2. Melt electrowritten device." The nitrogen pressure was set to 0.1 MPa, and the voltage between the nozzle and the table was set to 2.1 kV. The laminate was formed into a lattice shape with each side of the lattice being 230 μm. The number of layers in the laminate was set as shown in Table 1 below. For details on the method of forming the laminate, the above-mentioned paper, especially "2.1.3 Scaffold design and fabrication," can be referred to.

[0057] (Examples 1 to 4) The laminates of Examples 1 to 4 were molded using the above-mentioned EVOH1 as the material in the MEW device with the "table temperature," "syringe temperature," "table / nozzle distance," and "nozzle diameter" set as shown in Table 1 below. Note that the nozzle diameters in Table 1 are expressed in G (gauge), and the respective inner diameters are 23 G ≒ 0.35 mm, 27 G ≒ 0.22 mm, and 30 G ≒ 0.12 mm. Note that in Examples 3 and 4, thread-like fibers could be molded but laminates could not be molded, so there is no data on the laminates.

[0058] Comparative Example 1 The laminate of Comparative Example 1 was molded using the above-mentioned EVOH2 as the material, and the "table temperature," "syringe temperature," "table / nozzle distance," and "nozzle diameter" were set in the MEW device as shown in Table 1 below. Note that, as shown in Table 1, Comparative Example 1 was not molded because the material could not be discharged from the nozzle.

[0059] The laminate of Comparative Example 2 was produced using the above-mentioned PLA as the material and setting the "table temperature," "syringe temperature," "table / nozzle distance," and "nozzle diameter" in the MEW apparatus as shown in Table 1 below.

[0060] [Table 1] [Table 2]

[0061] (Laminate properties) The fiber diameter of each of the laminates of Examples 1 to 4 and Comparative Examples 1 and 2 was measured, and the results are shown in the above Table 1. The fiber diameter of the laminate can be measured by observation with an electron microscope.

[0062] (Evaluation of manufacturing method of laminate) When each of the laminates of Examples 1 to 4 and Comparative Examples 1 and 2 was formed using the MEW apparatus, the following evaluations were carried out.

[0063] (Evaluation of extrusion and stretchability) We visually confirmed whether the material was being discharged without any problems from the nozzle of the MEW device, stretched, and formed into a thread-like shape. If the fibers were discharged without clogging and the fibers were continuously stretched, the result was judged as "passable." If the fibers were clogged or the fibers were discontinuously stretched, the result was judged as "unacceptable."

[0064] (Table Adhesion) Whether the bottom layer of the laminate was adhered to the table of the MEW device was visually observed and evaluated according to the following criteria. A: The bottom layer of the laminate is bonded in all areas. B: Peeling off from the table in some areas C: Peeled off from the table in all areas

[0065] (Evaluation of the laminate) The laminates of Examples 1 to 4 and Comparative Examples 1 and 2 were used to carry out the following evaluations.

[0066] (Laminated body state) The laminates of Examples 1 to 4 and Comparative Examples 1 and 2 were used and evaluated according to the following criteria. A: The laminate is formed according to the set pattern. B: The laminate is formed slightly tilted from the set pattern, but this does not pose a problem in practical use. C: The laminate cannot be formed according to the set pattern, but thread-like fibers can be formed by stretching the material.

[0067] (Mechanical strength) The tensile strength and breaking elongation of each of the laminates of Examples 1 to 4 and Comparative Examples 1 and 2 were measured and evaluated according to the following criteria. The results are shown in Table 2. Note that measurements were not possible for examples other than Example 1 and Comparative Example 2. The tensile strength and breaking elongation of the laminate were measured using a tension and compression testing device (manufactured by Orientec Co., Ltd.) at a tension speed of 10 mm / min. ○: Tensile strength 8cN / dtex or more and breaking elongation 10% or more ×: Tensile strength less than 8cN / dtex or elongation at break less than 10%

[0068] In addition, the tensile strength and breaking elongation per fiber of each of the laminates of Examples 1 to 4 and Comparative Examples 1 and 2 were measured and evaluated according to the following criteria. The results are shown in Table 2. Note that measurements were not possible for examples other than Example 1 and Comparative Example 2. The tensile strength and breaking elongation per fiber of the laminate were measured using a tension and compression tester (manufactured by Orientec Co., Ltd.) at a tension speed of 10 mm / min. ○: Tensile strength 50 MPa or more and breaking elongation 10% or more ×: Tensile strength less than 50 MPa or breaking elongation less than 10%

[0069] <Result> In Example 1, a laminate could be formed, and as shown in Table 2, the mechanical strength was also good. In Example 2, the state of the laminate was inferior to that of Example 1, but was still at a level that did not pose any practical problems. In Examples 3 and 4, a laminate could not be formed, but thread-like fibers could be formed. In Comparative Example 1, the material could not be stretched, and even thread-like fibers could not be formed. In Comparative Example 2, a laminate could be formed, but as shown in Table 2, the mechanical strength was poor.

[0070] From these results, it was confirmed that ethylene-vinyl alcohol copolymers with a melt index of 60 g / 10 min or more measured at 220°C and 2.16 kg can at least be molded into thread-like fibers and are suitable for MEW molding. [Explanation of symbols]

[0071] 1 MEW Equipment 2 Syringes 3 Nozzles 4 Tables

Claims

1. An ethylene vinyl alcohol copolymer for melt electrolighting (MEW) molding having a melt index of 60 g / 10 min or more measured at 220° C. and 2.16 kg.

2. 2. The ethylene-vinyl alcohol copolymer according to claim 1, having a melt viscosity of 2000 Pa·s or less after heating at 240° C. for 3 hours at 0.5 Hz as measured with a rheometer.

3. The ethylene-vinyl alcohol copolymer according to claim 1, having an apparent viscosity of 500 Pa·s or less at a shear rate of 100 to 10,000 [1 / s] after heat treatment at 240° C. for 9 hours.

4. 2. The ethylene-vinyl alcohol copolymer according to claim 1, wherein the half-crystallization time at a crystallization temperature (Tc) + 10°C is 4 minutes or more.

5. A fiber comprising the ethylene-vinyl alcohol copolymer according to any one of claims 1 to 4, or a laminate comprising such fibers.

6. The fiber or laminate according to claim 5, wherein the fiber diameter of the fiber is from 0.1 μm to 500 μm.

7. The fiber or laminate according to claim 5, wherein the number of layers of the laminate is 1 to 500.

8. A method for producing a laminate, comprising forming fibers by MEW molding using the ethylene-vinyl alcohol copolymer according to any one of claims 1 to 4, and stacking the fibers.

9. The method for producing a laminate according to claim 8 , wherein a table temperature during production of the laminate is 70° C. or higher.

10. The method for producing a laminate according to claim 8 , wherein a syringe temperature during production of the laminate is 230° C. or higher.

11. The method for producing a laminate according to claim 8 , wherein the distance between the table and the nozzle when producing the laminate is 2 mm or less.

12. The method for producing a laminate according to claim 8, wherein a nozzle diameter when producing the laminate is 0.6 mm or less.