Lens manufacturing method
A two-step blackening process for lens manufacturing ensures comprehensive blackening of both inner and outer edge surfaces, addressing the issue of unwanted reflections and stray light in integrated optical and edge parts, resulting in improved light-shielding performance.
Patent Information
- Application Number
- JP2023060058
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2043-04-03
AI Technical Summary
Existing lens manufacturing methods fail to effectively blacken the edge portions of lenses, particularly the outer surfaces other than the inner circumferential surface, leading to unwanted reflections and stray light, especially in lenses with integrated optical and edge parts.
A two-step blackening process is employed, where the inner circumferential surface is treated before press molding, and the outer surfaces are treated post-molding, using methods like oxidation, chemical conversion, or plating to ensure comprehensive blackening of the edge portion.
The method reliably achieves excellent light-shielding effects by ensuring both inner and outer surfaces of the edge portion are blackened, reducing reflections and stray light, thereby enhancing optical performance.
Smart Images

Figure 2024147199000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a lens. [Background technology]
[0002] Patent Document 1 describes a technology for obtaining a high-performance lens with a multifunctional carrier by integrally bonding a carrier having a centering function between a molding die and a lens frame and a glass material during press molding in order to suppress accuracy errors such as decentering when manufacturing a lens by press molding. Patent Document 1 also describes a method for preventing ghosts and flares by applying a black paint to the inner peripheral surface of the multifunctional carrier before press molding. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 63-40733 Summary of the Invention [Problem to be solved by the invention]
[0004] In lenses with a structure in which the outside of an optical function part having an optical surface (lens surface) is surrounded by a edge part made of a different material from the optical function part, it is necessary to ensure optical performance by suppressing the reflection of harmful light at the edge part. For example, in the case of a metal edge part, if the lens is constructed while retaining its metallic luster, harmful reflected light is likely to occur, so measures are required to improve the light blocking properties by blackening the surface of the edge part.
[0005] In addition, in edge portions with a small thickness in the optical axis direction or edge portions with a large area of the front and rear surfaces facing forward and backward in the optical axis direction, light reflected not only from the inner surface of the edge portion but also from the outer surface portions other than the inner surface is likely to cause stray light, so high light-blocking performance is also required in the outer surface portions other than the inner surface.
[0006] In the case of a lens manufacturing method in which the optical function part and the edge are integrated by press molding, it is assumed that the edge will be blackened before press molding, because it is difficult to blacken the inner peripheral surface of the edge after it has been integrated with the optical function part. However, if press molding is performed on a blackened edge, there is a problem in that the bare metal of the edge will be exposed due to deformation during press molding, reducing the effect of the blackening treatment.
[0007] In the lens with multifunctional carrier described in Patent Document 1, the inner surface of the multifunctional carrier is blackened by applying black paint, but no special light-blocking measures are taken for areas other than the inner surface, and the above-mentioned problem is not solved.
[0008] The present invention has been made based on the above-mentioned problem awareness, and has as its object to provide a method for manufacturing a lens that can reliably blacken the edge portion to obtain an excellent light-shielding effect. [Means for solving the problem]
[0009] A lens manufacturing method of one aspect of the present invention is characterized by comprising: a first blackening step of performing blackening treatment on at least an inner surface of a ring-shaped edge portion before press molding; a molding step of press-molding an optical functional portion surrounded by the edge portion and the edge portion to form an optical surface on the optical functional portion and fix the outer surface of the optical functional portion and the inner surface of the edge portion to each other; and a second blackening step of blackening at least a portion of an outer surface other than the inner surface of the edge portion after press molding.
[0010] It is preferable that the edge portion is molded into a shape in which at least one of the outer surfaces on both sides facing the optical axis direction includes a non-flat portion by the molding step, and that the second blackening treatment step performs blackening treatment on an area that includes at least the non-flat portion.
[0011] It is preferable that the second blackening step is performed in a state where a masking portion is formed to cover the optical surface of the optical function portion, and that the masking portion is removed after the second blackening step.
[0012] As one example, the edge portion is made of metal, and at least one of the first blackening treatment step and the second blackening treatment step blackens the outer surface of the edge portion by oxidizing the metal through heating.
[0013] It is preferable that the optical function portion is made of glass, and the second blackening step involves heating the edge portion at a temperature lower than the glass transition temperature of the glass constituting the optical function portion to blacken it by oxidation.
[0014] As an example, at least one of the first blackening step and the second blackening step blackens the outer surface of the edge portion by chemical conversion treatment.
[0015] As an example, at least one of the first blackening step and the second blackening step blackens the outer surface of the edge portion by plating.
[0016] As an example, the second blackening step blackens the outer surface of the edge portion by applying a synthetic resin. Effect of the Invention
[0017] By applying the manufacturing method of the lens of the present invention, the inner peripheral surface of the edge portion and the outer surface other than the inner peripheral surface can be reliably blackened, thereby obtaining an excellent light blocking effect. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a cross-sectional view showing a lens configuration. [Diagram 2] FIG. 11 is a diagram illustrating a first blackening processing step. [Diagram 3] FIG. 2 is a diagram illustrating a molding step. [Figure 4] FIG. 2 is a diagram illustrating a molding step. [Diagram 5] FIG. 2 is a cross-sectional view showing the lens after the molding step is completed. [Figure 6]FIG. 11 is a diagram illustrating a second blackening processing step. [Figure 7] 11A and 11B are diagrams illustrating a masking process for an optical function portion. [Figure 8] FIG. 13 is a diagram showing the state after a second blackening step is performed on a lens that has been subjected to a masking process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] A method for manufacturing a lens according to the present invention will be described below based on the illustrated embodiment. First, the configuration of a lens 1 manufactured by a manufacturing method to which the present invention is applied will be described with reference to Fig. 1. The direction along the optical axis X1 of the lens 1 is defined as the optical axis direction, and the direction perpendicular to the optical axis X1 is defined as the direction orthogonal to the optical axis. The direction orthogonal to the optical axis can also be called the radial direction of the lens 1. Fig. 1 is a cross-sectional view showing the lens 1 at a cross-sectional position including the optical axis X1.
[0020] The lens 1 is composed of an optical function part 10 made of glass and an annular edge part 20 that surrounds the outside of the optical function part 10. The edge part 20 is made of a material different from the glass that constitutes the optical function part 10, and in this embodiment, the edge part 20 is made of metal. For the metal that constitutes the edge part 20, a material that can be deformed together with the glass material that constitutes the optical function part 10 near the forming temperature of the glass material is selected.
[0021] The optical function section 10 has optical surfaces (lens surfaces) on both sides in the optical axis direction. The lens 1 of this embodiment is a biconvex lens in which the optical surfaces 11 and 12 on both sides of the optical function section 10 are both convex. The side in the optical axis direction to which the optical surface 11 faces is defined as a first direction Xa, and the side to which the optical surface 12 faces is defined as a second direction Xb. Note that the optical surface of the lens formed by applying the manufacturing method of the present invention is not limited to this embodiment, and the optical surface may be any of a convex surface, a concave surface, and a flat surface. In addition, the optical surface may be a spherical surface or an aspherical surface.
[0022] The optical function portion 10 has an outer peripheral surface 13 that connects the outer edge portions of the optical surface 11 and the optical surface 12. The outer peripheral surface 13 is a cylindrical surface centered on the optical axis X1.
[0023] The edge portion 20 has a front surface portion 21 as an outer surface facing a first direction Xa, which is one side of the optical axis direction. The front surface portion 21 has, in order from the inner diameter side closest to the optical surface 11, an inner flat surface 21a, a tapered surface 21b, and an outer flat surface 21c.
[0024] The edge portion 20 has a rear surface portion 22 as an outer surface facing the second direction Xb, which is the other side of the optical axis direction. The rear surface portion 22 has, in order from the inner diameter side closest to the optical surface 12, an inner flat surface 22a, a tapered surface 22b, and an outer flat surface 22c.
[0025] The front and rear of the front surface portion 21 and the rear surface portion 22 are designated for convenience. This does not limit the front surface portion 21 (first direction Xa) to face forward in the optical axis direction of the optical system and the rear surface portion 22 (second direction Xb) to face backward in the optical axis direction of the optical system when the lens 1 is incorporated into an optical device.
[0026] The inner flat surface 21a and the outer flat surface 21c of the front surface portion 21, and the inner flat surface 22a and the outer flat surface 22c of the rear surface portion 22 are each a plane substantially perpendicular to the optical axis X1, and are provided in an annular range centered on the optical axis X1. The tapered surface 21b and the tapered surface 22b are each a truncated cone-shaped surface whose diameter increases as it progresses in the second direction Xb in the optical axis direction (whose diameter decreases as it progresses in the first direction Xa). The tapered surface 21b of the front surface portion 21 is stepped, and the tapered surface 22b of the rear surface portion 22 is stepped, and the tapered surface 21b and the tapered surface 22b form non-flat portions of the front surface portion 21 and the rear surface portion 22, respectively.
[0027] In the edge portion 20, the region including the inner flat surface 21a and the inner flat surface 22a is defined as the inner flat portion 20a, the region including the tapered surface 21b and the tapered surface 22b is defined as the intermediate tapered portion 20b, and the region including the outer flat surface 21c and the outer flat surface 22c is defined as the outer flat portion 20c. The edge portion 20 is configured such that the inner flat portion 20a and the outer flat portion 20c are partially shifted in the optical axis direction with the intermediate tapered portion 20b in between.
[0028] The edge portion 20 has an inner peripheral surface 23 that connects the inner edge portions of the inner flat surface 21a and the inner flat surface 22a, and an outer peripheral surface 24 that connects the outer edge portions of the outer flat surface 21c and the outer flat surface 22c. The inner peripheral surface 23 and the outer peripheral surface 24 are each a cylindrical surface centered on the optical axis X1. The inner peripheral surface 23 of the edge portion 20 is fixed to the outer peripheral surface 13 of the optical function portion 10. The outer peripheral surface 24 of the edge portion 20 is a surface that constitutes the outermost edge of the lens 1.
[0029] The outer surface of the edge portion 20 is blackened to suppress light reflection, as will be described in detail later. The blackening of the edge portion 20 suppresses internal reflection at the inner circumferential surface 23 and the generation of stray light that does not pass through the optical function portion 10 in a proper path when the lens 1 is incorporated into an optical device, thereby improving the optical performance (light blocking effect). The outer surface of the edge portion 20 refers to the portion that appears on the outside when the edge portion 20 and the annular member 31 that is its base material are in a single state (before being combined with the optical function portion 10), and the inner circumferential surface 23 that is fixed to the outer circumferential surface 13 of the optical function portion 10 when the lens 1 is completed, and the inner circumferential surface 34 of the annular member 31 are also included in the outer surface of the edge portion 20. The blackening of the outer surface is a process for reducing light reflection by preventing the color and luster of the metal (base metal) that is the material of the edge portion 20 from being exposed to the outer surface as it is. The blackening process is not limited to making the outer surface of the edge 20 completely black, but may be any process that provides a predetermined level of reflection reduction effect compared to when the bare metal of the edge 20 is exposed.
[0030] Next, the configuration of the mold 40 used in manufacturing the lens 1 will be described with reference to FIG. 3 and FIG. 4. The mold 40 is composed of a body mold 41, a lower mold 42, and an upper mold 43. The body mold 41 is cylindrical and has an internal space surrounded by an inner peripheral surface 41a, which is a cylindrical surface. The central axis X2 of the mold 40 is an axis line extending in the vertical direction through the center of the inner peripheral surface 41a. The body mold 41 has a body mold lower end surface 41b at its lower end and a body mold upper end surface 41c at its upper end. The body mold lower end surface 41b and the body mold upper end surface 41c are each surfaces approximately perpendicular to the central axis X2. The internal space of the body mold 41 penetrates in the vertical direction and opens at the inner regions of the body mold lower end surface 41b and the body mold upper end surface 41c.
[0031] The lower mold 42 has an insertion part 42a inserted from below into the internal space of the body mold 41, and a large-diameter part 42b provided at the bottom of the insertion part 42a and having a larger diameter than the insertion part 42a. The upper mold 43 has an insertion part 43a inserted from above into the internal space of the body mold 41, and a large-diameter part 43b provided at the top of the insertion part 43a and having a larger diameter than the insertion part 43a. The outer peripheral surfaces of the insertion part 42a and the insertion part 43a can slide in the vertical direction relative to the inner peripheral surface 41a of the body mold 41, and movement in a direction perpendicular to the central axis X2 is restricted. In other words, the lower mold 42 and the upper mold 43 can move in the vertical direction relative to the body mold 41 in a state where the central axes of the lower mold 42 and the upper mold 43 are aligned to coincide with the central axis X2.
[0032] The lower die 42 has an optical forming surface 44 at the upper end of the insertion portion 42a. The optical forming surface 44 is a concave surface that is deepest at the center on the central axis X2 and becomes shallower toward the outer diameter side. At the upper end of the insertion portion 42a, a flange forming surface 45 is further formed around the optical forming surface 44. The flange forming surface 45 has an inner flat surface 45a, a tapered surface 45b, and an outer flat surface 45c, in that order from the inner side toward the outer side in the radial direction close to the optical forming surface 44. The inner flat surface 45a and the outer flat surface 45c are surfaces that are approximately perpendicular to the central axis X2 and are provided in an annular range centered on the central axis X2. The outer flat surface 45c is located above the inner flat surface 45a. The tapered surface 45b is a truncated cone-shaped surface centered on the central axis X2, and one end (the end on the small diameter side) of the tapered surface 45b is connected to the inner flat surface 45a, and the other end (the end on the large diameter side) of the tapered surface 45b is connected to the outer flat surface 45c.
[0033] The upper mold 43 has an optical forming surface 46 at the lower end of the insertion portion 43a. The optical forming surface 46 is a concave surface that is deepest at the center on the central axis X2 and becomes shallower toward the outer diameter side. At the lower end of the insertion portion 43a, a flange forming surface 47 is further formed around the optical forming surface 46. The flange forming surface 47 has an inner flat surface 47a, a tapered surface 47b, and an outer flat surface 47c, in that order from the inner side toward the outer side in the radial direction close to the optical forming surface 46. The inner flat surface 47a and the outer flat surface 47c are surfaces that are approximately perpendicular to the central axis X2, and are provided in an annular range centered on the central axis X2. The outer flat surface 45c is located above the inner flat surface 45a. The tapered surface 47b is a truncated cone-shaped surface centered on the central axis X2, and one end (the end on the small diameter side) of the tapered surface 47b is connected to the inner flat surface 47a, and the other end (the end on the large diameter side) of the tapered surface 47b is connected to the outer flat surface 47c.
[0034] When forming lens 1 by press molding using mold 40, the positions at which insertion portion 42a of lower mold 42 and insertion portion 43a of upper mold 43 are each most inserted into barrel mold 41 are called the press movement ends of lower mold 42 and upper mold 43. As shown in Fig. 4, when lower mold 42 and upper mold 43 reach their respective press movement ends, optical forming surfaces 44 and optical forming surfaces 46, and edge forming surfaces 45 and edge forming surfaces 47 face each other with a predetermined gap between them in the vertical direction.
[0035] As an example, the position where the large diameter portion 42b abuts against the barrel mold lower end surface 41b can be set as the press movement end of the lower mold 42. Also, the position where the large diameter portion 43b abuts against the barrel mold upper end surface 41c can be set as the press movement end of the upper mold 43. Alternatively, the press movement end of the upper mold 43 may be determined by a configuration other than the large diameter portion 43b abutting against the barrel mold upper end surface 41c.
[0036] In manufacturing the lens 1, a glass preform 30, which is the base material for the optical function portion 10, and an annular member 31, which is the base material for the edge portion 20, are placed inside a molding die 40 (see FIG. 3), and press molding is performed by bringing a lower die 42 and an upper die 43 close to each other (see FIG. 4). The glass preform 30 is made of spherical glass, and the annular member 31 is made of a ring-shaped metal. The annular member 31 is defined as the edge portion before press molding, and the edge portion 20 is defined as the edge portion after press molding.
[0037] When blackening the outer surface of the edge portion 20, it is difficult to later blacken the inner peripheral surface 23 of the edge portion 20 (particularly the portion fixed to the outer peripheral surface 13 of the optical function portion 10) when the lens 1 is completed as shown in Fig. 1. On the other hand, if blackening is performed on the outer surface of the annular member 31, which is the edge portion before press molding using the molding die 40, the metal base metal may be partially exposed on the outer surface of the edge portion 20 when the annular member 31 is deformed into the edge portion 20 by press molding, and the effect of the blackening treatment may be lost. In particular, the metal base metal is likely to be exposed due to the influence of press molding at the front portion 21 and the rear portion 22, which are extended in the radial direction and have non-flat portions (step shapes) such as the tapered surface 21b and the tapered surface 22b.
[0038] The lens manufacturing method of the present embodiment uses press molding to obtain a lens 1 in which the outer surface of the edge portion 20 is reliably blackened, and the details of this method will be described below.
[0039] The manufacturing method of the lens of this embodiment includes a first blackening step, a molding step, and a second blackening step. In Figures 2 to 8, the portions of the edge portion 20 and the annular member 31 that have been subjected to the blackening steps are highlighted with thick lines.
[0040] [First blackening step] 2 shows an annular member 31, which is an edge portion, before being subjected to press molding by a molding die 40. The annular member 31 has annular flat surfaces 32 and 33 that are approximately perpendicular to the central axis X2 when placed in the molding die 40, a cylindrical inner circumferential surface 34 that connects the inner edge portions of the flat surfaces 32 and 33, and a cylindrical outer circumferential surface 35 that connects the outer edge portions of the flat surfaces 32 and 33.
[0041] In the first blackening step, at least the inner circumferential surface 34 of the annular member 31 is blackened. As a method of blackening in the first blackening step, for example, oxidation by heating metal, chemical conversion treatment, plating treatment, etc. can be applied. In the oxidation by heating metal, the outer surface of the annular member 31, which is the workpiece, is oxidized by heating in an atmosphere containing oxygen, and the metallic luster is removed and blackened. Examples of metal materials that are easily oxidized by heating include copper and iron. As an example of chemical conversion treatment, the annular member 31, which is the workpiece made of iron, is immersed in an alkaline aqueous solution to form a black oxide film (iron tetroxide film) on the outer surface of the annular member 31. As an example of plating treatment, plating such as black nickel plating or black chrome plating is performed on the outer surface of the annular member 31, which is the workpiece.
[0042] The molding step following the first blackening step is carried out in a state where the glass preform 30 is heated to a temperature above the glass transition temperature at which the glass preform 30 softens. Therefore, the area blackened in the first blackening step is required to have heat resistance so that it will not deteriorate or be damaged even when heated to the glass transition temperature range. Each of the above methods satisfies this heat resistance condition.
[0043] By subjecting the inner surface 34 to the blackening treatment in the first blackening treatment step, the inner surface 23 of the edge portion 20, which is difficult to blacken after the press molding process using the molding die 40, can be reliably blackened.
[0044] In the first blackening treatment step, it is sufficient that the target of the blackening treatment includes at least the inner circumferential surface 34, and the blackening treatment may also include the flat surface 32, the flat surface 33, the outer circumferential surface 35, etc., which are the outer surface parts other than the inner circumferential surface 34. In particular, when a method is adopted in which it is difficult to treat only the area of the inner circumferential surface 34, such as dipping, in which the entire object to be treated is submerged in the treatment liquid, the entire outer surface of the annular member 31 may be the target of the blackening treatment in the first blackening treatment step.
[0045] [Molding step] After the first blackening step is completed, a molding step is performed. In the molding step, first, as shown in Fig. 3, the glass preform 30 and the annular member 31 (whose inner peripheral surface 34 has been blackened) are held between a lower die 42 and an upper die 43 of a molding die 40. The annular member 31 is held with the flat surface 32 placed on the outer flat surface 45c of the edge forming surface 45, with a portion of the annular member 31 protruding toward the inner diameter side (at a position closer to the central axis X2) than the outer flat surface 45c.
[0046] The thickness of the annular member 31 from the flat surface 32 to the flat surface 33 before press working is set to be larger than the distance between the edge forming surface 45 and the edge forming surface 47 when the lower die 42 and the upper die 43 are at their respective press movement ends. Therefore, when the lower die 42 and the upper die 43 are moved toward each other to their respective press movement ends, the annular member 31 is deformed and extends in the radial direction due to the pressing force from the edge forming surface 45 and the edge forming surface 47.
[0047] The glass preform 30 is placed on the optical forming surface 44 of the lower die 42. The concave shape of the optical forming surface 44 holds the glass preform 30 at a position on the central axis X2. The lower die 42 is held at the press moving end with the large diameter portion 42b abutting against the barrel mold lower end surface 41b, and the lower die 42 is supported from below so that the insertion portion 42a does not come off the barrel mold 41. The glass preform 30 may be supplied onto the optical forming surface 44 with the insertion portion 42a removed downward from the barrel mold 41, or may be supplied from the upper end side of the barrel mold 41 with the insertion portion 42a inserted into the barrel mold 41.
[0048] 3, the glass preform 30 and the annular member 31 are placed inside the mold 40, and then the glass preform 30 is softened by heating it until the temperature exceeds the glass transition temperature of the glass preform 30. Then, using a pressing device (not shown), the upper mold 43 with the insertion portion 43a inserted into the body mold 41 is pressed downward. The glass preform 30 is pressed and deformed between the optical forming surface 46 of the descending upper mold 43 and the optical forming surface 44 of the lower mold 42 whose descending is restricted. The glass preform 30 extends toward the outer diameter while decreasing in thickness in the direction along the central axis X2.
[0049] In addition, since the molding step is performed in a nitrogen gas atmosphere that does not contain sufficient oxygen to oxidize the annular member 31, the annular member 31 does not become blackened due to oxidation when the annular member 31 is heated together with the glass preform 30. Therefore, prior to the molding step, it is necessary to perform a first blackening treatment step to blacken the inner peripheral surface 34 of the annular member 31.
[0050] When the upper mold 43 descends and the glass preform 30 is deformed to a certain extent, the descending edge forming surface 47 comes into contact with the flat surface 33 of the annular member 31 from above, and the annular member 31 is pressed and deformed between the edge forming surface 45 and the edge forming surface 47. At this time, the annular member 31 extends toward the inner diameter side while reducing its thickness in the direction along the central axis X2. At that time, the shape of the flat surface 32 side changes to a shape along the edge forming surface 45 to become the front surface 21. That is, the inner flat surface 21a having a shape transferred from the inner flat surface 45a, the tapered surface 21b having a shape transferred from the tapered surface 45b, and the outer flat surface 21c having a shape transferred from the outer flat surface 45c are formed. Also, the shape of the flat surface 33 side changes to a shape along the edge forming surface 47 to become the rear surface 22. That is, an inner flat surface 22a having a shape transferred from the inner flat surface 47a, a tapered surface 22b having a shape transferred from the tapered surface 47b, and an outer flat surface 22c having a shape transferred from the outer flat surface 47c are formed.
[0051] When the upper die 43 is lowered to the pressing movement end shown in Fig. 4, the glass preform 30 is pressed by the lower die 42 and the upper die 43 in the inner region of the annular member 31, resulting in the optical functional part 10 having the optical surfaces 11 and 12 to which the shapes of the optical forming surfaces 44 and the optical forming surfaces 46 are transferred on both sides in the optical axis direction. In addition, as a result of the annular member 31 being pressed by the lower die 42 and the upper die 43, the edge part 20 is formed having the front surface 21 and the rear surface 22 to which the shapes of the edge part forming surfaces 45 and the edge part forming surfaces 47 are transferred on both sides in the optical axis direction. Furthermore, as a result of the glass preform 30 extended toward the outer diameter side and the annular member 31 extended toward the inner diameter side being in close contact with each other, the outer peripheral surface 13 of the optical functional part 10 and the inner peripheral surface 23 of the edge part 20 are in close contact and fixed. The inner circumferential surface 23 of the flange portion 20 is formed based on the inner circumferential surface 34 of the annular member 31 extending toward the inner diameter side, and has a substantially cylindrical shape centered on the optical axis X1. The outer circumferential surface 13 of the optical function part 10 has a substantially cylindrical shape corresponding to the inner circumferential surface 23 of the flange portion 20. The outer circumferential surface 24 of the flange portion 20 is formed based on the outer circumferential surface 35 of the annular member 31, and has a substantially cylindrical shape centered on the optical axis X1.
[0052] The inner peripheral surface 34 of the annular member 31 is a portion that receives a load in the compressive direction during press molding in the molding die 40. Therefore, the inner peripheral surface 23 of the edge portion 20 formed based on the inner peripheral surface 34 of the annular member 31 does not undergo surface elongation that would cause the bare metal to be exposed, and the effect of the blackening treatment performed in the first blackening treatment step can be maintained even after press molding.
[0053] After the press molding is completed, the lens 1 is cooled to a predetermined temperature and then disassembled to remove the mold 40. In this manner, the lens 1 is formed with a hybrid structure consisting of an optical function part 10, which is a press-molded glass product, and a metal edge part 20. Figure 5 shows the lens 1 at the stage where the molding step has been completed, with at least the inner peripheral surface 23 of the edge part 20 being blackened.
[0054] [Second blackening step] After the molding step is completed, a second blackening step is performed. In the second blackening step, the outer surface of the edge portion 20 other than the inner peripheral surface 23 is blackened. The blackening step in the second blackening step is performed using a method that does not affect the optical performance of the optical function portion 10, whose molding has been completed. For example, the oxidation by heating metal, chemical conversion treatment, plating treatment, etc., which are described in the first blackening step, can also be applied to the second blackening step.
[0055] When the edge portion 20 is oxidized by heating in the second blackening step, the edge portion 20 is heated at a temperature lower than the glass transition temperature of the glass material constituting the optical function portion 10 by a predetermined temperature or more, thereby making it possible to perform the blackening treatment on the outer surface of the edge portion 20 without causing effects such as deformation of the optical function portion 10. For example, the heating temperature of the edge portion 20 is set to 300°C or higher and lower than the above glass transition temperature. The glass transition temperature of glass materials generally used for glass lenses is often 400°C or higher, and this setting makes it possible to effectively blacken the outer surface of the edge portion 20 made of copper, iron, etc., while ensuring a sufficient margin that does not affect the optical performance of the optical function portion 10.
[0056] Since the second blackening step is not subjected to a heat treatment in a high temperature range that softens the glass material constituting the optical function section 10, the second blackening step differs from the first blackening step in that the heat resistance requirements for the blackened areas in the second blackening step are relaxed. Therefore, in addition to the above-mentioned methods, it is also possible to use a blackening material with a relatively low heat resistance, such as applying a black paint made of synthetic resin, as the method of blackening in the second blackening step.
[0057] 6 shows lens 1 at the stage where the second blackening step has been completed, with front surface 21, rear surface 22, and outer surface 24 being blackened in addition to inner peripheral surface 23 of edge portion 20. Because the blackening process is performed after press molding using mold 40, it is possible to achieve blackening that corresponds to the outer surface shape of edge portion 20 after press molding, without being affected by deformation of edge portion 20 from annular member 31 before press molding. In particular, blackening can be reliably performed even on front surface 21 and rear surface 22 that have non-flat portions such as tapered surface 21b and tapered surface 22b.
[0058] If the flat surfaces 32 and 33 of the annular member 31 have not been blackened in the previous first blackening treatment step, the flat surfaces 32 and 33 are newly blackened by carrying out the second blackening treatment step.
[0059] Even if the flat surfaces 32 and 33 of the annular member 31 are blackened in the first blackening step and the base metal is exposed at the front surface 21 and the rear surface 22 of the edge portion 20 due to the effects of press molding in the molding die 40, the exposed portions can be removed and the material can be reliably blackened by performing the second blackening step.
[0060] In the second blackening step, the entire edge portion 20 other than the inner peripheral surface 23 may be subjected to the blackening treatment, or a specific part of the outer surface other than the inner peripheral surface 23 may be subjected to the blackening treatment. In particular, it is preferable to perform the second blackening step so that the target area of the blackening treatment includes areas where, when blackening is performed in the first blackening step, the effect of blackening is likely to be reduced (the base metal of the metal will be exposed) due to deformation or extension in the subsequent molding step.
[0061] For example, as described above, in locations including non-flat portions such as tapered surface 21b and tapered surface 22b of edge portion 20, the base metal is likely to be exposed due to changes in shape caused by press molding. Therefore, it is preferable that at least tapered surface 21b and its periphery, and tapered surface 22b and its periphery of edge portion 20 are included in the target region of the blackening treatment in the second blackening treatment step.
[0062] Furthermore, the inner flat surface 21a and the outer flat surface 21c of the front surface 21, and the inner flat surface 22a and the outer flat surface 22c of the rear surface 22 are parts that receive a force that causes the edge portion 20 to extend in the radial direction during press molding by the molding die 40. Even if there is no significant change in shape such as a step, bend, or unevenness, such extended parts may be expanded relative to the original blackened area, resulting in the bare metal being exposed. Therefore, by including the inner flat surface 21a, the outer flat surface 21c, the inner flat surface 22a, and the outer flat surface 22c in the blackening treatment in the second blackening treatment step, a more reliable light-shielding effect can be obtained.
[0063] In addition, in the second blackening step, it is also possible to intentionally exclude a predetermined portion of the edge portion 20 from the target of the blackening treatment. For example, when the lens 1 is incorporated into the lens barrel of an optical device, the outer peripheral surface 24 of the edge portion 20 may be surrounded and held by the inner surface of the lens barrel, resulting in a structure in which light in the optical path does not reach the outer peripheral surface 24. In such a case, omitting the blackening treatment of the outer peripheral surface 24 does not affect the optical performance, so it is possible to choose not to blacken the outer peripheral surface 24 in the second blackening step.
[0064] In order to protect the optical surfaces 11 and 12 of the optical function part 10 and perform efficient blackening of the edge part 20, the second blackening step may be performed in a state in which the optical function part 10 has been masked. If the optical function part 10 is not masked, the second blackening step directly transitions from the state shown in FIG. 5 to the state shown in FIG. 6.
[0065] When the masking process is performed on the optical functional part 10, a masking part 36 that covers the optical functional part 10 is formed after the molding step, as shown in Fig. 7. The masking part 36 is formed so as to cover the entire optical surface 11 and the optical surface 12 of the optical functional part 10, and further to cover the boundary part between the outer peripheral surface 13 of the optical functional part 10 and the inner peripheral surface 23 of the edge part 20. Note that in Figs. 7 and 8, the masking part 36 is represented by a dashed line to easily distinguish the difference from the blackened part of the edge part 20, but this does not mean that there is a hole in the masking part 36, and the masking part 36 completely covers the optical surface 11 and the optical surface 12 without any gaps.
[0066] The masking portion 36 can be formed by applying a masking paint, adhering a masking tape having an adhesive surface, pressing other masking materials, or the like.
[0067] After the masking portion 36 is formed, a second blackening step is performed. As a result, the edge portion 20 is blackened outside the masked optical function portion 10, as shown in Fig. 8. By performing the second blackening step while the optical function portion 10 is protected by the masking portion 36, it is possible to prevent the optical surfaces 11 and 12 from becoming dirty or cloudy.
[0068] After the second blackening step is completed, the masking portion 36 is removed. If the masking portion 36 is formed from masking paint, the paint is washed away and removed using a cleaning agent having a composition suitable for removing the paint. If the masking portion 36 is formed from masking tape, the tape is peeled off and removed. By removing the masking portion 36, the lens 1 is completed, in which the entire outer surface of the edge portion 20 has been blackened, as shown in FIG. 6.
[0069] It is also possible to use the masking treatment for purposes other than protection of the optical function portion 10. For example, when a predetermined portion of the edge portion 20 is to be excluded from the blackening treatment in the second blackening treatment step, the masking treatment may be used for the purpose of not subjecting the predetermined portion to the blackening treatment.
[0070] As described above, by performing the second blackening treatment step after the molding step, the outer surface area of edge portion 20 other than inner surface 23 can be reliably blackened, thereby ensuring the overall light-blocking effect of edge portion 20.
[0071] According to the lens manufacturing method described above, the inner surface 23 of the edge portion 20, which is difficult to blacken after being fixed to the optical function portion 10, is blackened in a first blackening step prior to the press processing (molding step) using the molding die 40, and the parts other than the inner surface 23 of the edge portion 20 are blackened in a second blackening step after the press processing (molding step) using the molding die 40. This ensures that each part of the edge portion 20 can be blackened reliably, and a lens 1 with excellent light-blocking performance of the edge portion 20 can be obtained.
[0072] In addition, by varying the blackening method and the degree of blackening between the first blackening step and the second blackening step, it is possible to obtain a blackening form suitable for each step, and it is possible to set a finely tuned light blocking effect for each part of the edge portion 20.
[0073] For example, the inner circumferential surface 23 of the edge portion 20 constitutes the inner surface of the optical path surrounding the optical function portion 10, and is a portion where suppression of internal reflection is particularly important. Therefore, in the first blackening treatment step, it is preferable to improve the stray light prevention effect on the inner circumferential surface 23 by making selections such as increasing the thickness of the blackening layer or using a blackening material with high blackness.
[0074] The front surface 21, rear surface 22 and outer circumferential surface 24 of the edge portion 20 are used to position the lens 1 relative to the lens barrel, other lenses, etc. Therefore, in the second blackening step, it is preferable to minimize the effect on the shape accuracy of the outer surface of the edge portion 20 and obtain excellent positioning accuracy by making selections such as reducing the thickness of the blackening layer and selecting a type of blackening treatment with excellent surface accuracy.
[0075] The manufacturing method of the present invention is suitable for a type of lens having a non-flat portion at a location other than the inner peripheral surface of the edge portion, such as the intermediate tapered portion 20b of the edge portion 20 in the above embodiment, but is not limited to this type of lens, and is also useful for a lens having an edge portion whose entire outer surfaces on both sides in the optical axis direction are flat. When a lens is press-molded using a device such as the mold 40, if a load in the optical axis direction is applied to the edge portion during press molding, the edge portion is stretched in the radial direction. Even if the outer surfaces on both sides in the optical axis direction of the edge portion are flat, the base metal is likely to be exposed on the outer surface as the edge portion is stretched in the radial direction. Therefore, by performing a second blackening treatment step in which the flat-shaped front portion and the flat-shaped rear portion of the edge portion are blackened after press molding, the front portion and the rear portion after stretching can be reliably blackened.
[0076] In addition, in the lens 1 of the above embodiment, the edge portion 20 has tapered surfaces 21b and 22b on both sides in the optical axis direction, but the manufacturing method of the present invention is also useful for a type of lens in which only one of the outer surfaces of the edge portion on both sides facing the optical axis direction has a non-flat portion, and the other outer surface in the optical axis direction is composed only of a flat surface.
[0077] Although the lens 1 of the above embodiment has tapered surface 21b and tapered surface 22b as non-flat parts, the shape of the non-flat part of the edge of the lens is not limited to this. For example, even if the outer surface of the edge has a recess (groove), protrusion, or notch, the location of such a recess, protrusion, or notch is suitable for blackening treatment in the second blackening treatment step after press molding.
[0078] In the above embodiment, the edge portion 20 has a uniform shape that continues in the circumferential direction around the optical axis X1, but the shape of the edge portion may be different in a part of the circumferential direction. For example, the edge portion may have a tapered surface, a recess, a protrusion, a notch, etc. only in a part of the circumferential direction.
[0079] In the above embodiment, the spherical glass preform 30 is placed inside the molding die 40 and press-molded, but the glass preform that is the base material for the optically functional portion is not limited to a spherical shape.
[0080] In the lens 1 of the above embodiment, the material of the edge portion 20 is metal, but the material of the edge portion of the lens manufactured by applying the present invention can be selected to be other than metal. For example, the edge portion may be made of a glass different from the glass that constitutes the optical function portion. Alternatively, the edge portion may be made of ceramics.
[0081] The embodiments of the present invention are not limited to the above-mentioned embodiments or their modifications, and may be modified, substituted, or altered in various ways without departing from the spirit of the technical idea of the present invention. Furthermore, if the technical idea of the present invention can be realized in a different way due to technological progress or other derived technology, it may be implemented using that method. Therefore, the claims cover all embodiments that may be included within the scope of the technical idea of the present invention. [Explanation of symbols]
[0082] 1: Lens 10:Optical function section 11:Optical surface 12:Optical surface 13: Outer surface 20: Edge (edge after press molding) 20a:Inner flat part 20b: Intermediate tapered section 20c: Outer flat part 21: Front part (outer surface facing the optical axis direction) 21a: Inner flat surface 21b: Tapered surface (non-flat part) 21c: Outer flat surface 22: Rear surface (outer surface facing the optical axis direction) 22a: Inner flat surface 22b: Tapered surface (non-flat part) 22c: Outer flat surface 23: Inner surface 24: Outer surface 30: Glass preform 31: Annular part (edge before press forming) 32:Flat surface 33:Flat surface 34: Inner peripheral surface 35: Outer surface 36: Masking section 40: Molding mold 41: Body type 42: Lower mold 43: Upper mold 44:Optical forming surface 45: Edge forming surface 45a: Inner flat surface 45b: Tapered surface 45c: Outer flat surface 46:Optical forming surface 47: Edge forming surface 47a: Inner flat surface 47b: Tapered surface 47c: Outer flat surface X1: Optical axis X2: Central axis of the mold
Claims
1. a first blackening step of performing blackening treatment on at least an inner peripheral surface of an annular edge portion before press forming; a molding step of press-molding an optical function portion surrounded by the edge portion and the edge portion to form an optical surface on the optical function portion and fix an outer peripheral surface of the optical function portion and an inner peripheral surface of the edge portion to each other; a second blackening step of blackening at least a part of an outer surface other than the inner circumferential surface of the edge portion after press molding; A method for manufacturing a lens, comprising the steps of:
2. The edge portion is formed in such a shape that at least one of the outer surfaces on both sides facing the optical axis direction includes a non-flat portion by the molding step, The method for manufacturing a lens according to claim 1 , wherein the second blackening step performs blackening on an area including at least the non-flat portion.
3. 3. The method for manufacturing a lens according to claim 1, wherein the second blackening step is performed in a state where a masking portion is formed to cover the optical surface of the optical function portion, and the masking portion is removed after the second blackening step.
4. 3. The method for manufacturing a lens according to claim 1, wherein the edge portion is made of metal, and at least one of the first blackening treatment step and the second blackening treatment step blackens an outer surface of the edge portion by oxidation through heating of the metal.
5. 5. The method for manufacturing a lens according to claim 4, wherein the optical function portion is made of glass, and the second blackening step heats the edge portion at a temperature lower than the glass transition temperature of the glass constituting the optical function portion.
6. 3. The method for manufacturing a lens according to claim 1, wherein at least one of the first blackening step and the second blackening step blackens the outer surface of the edge portion by a chemical conversion treatment.
7. 3. The method for manufacturing a lens according to claim 1, wherein at least one of the first blackening step and the second blackening step blackens the outer surface of the edge portion by plating.
8. 3. The method for manufacturing a lens according to claim 1, wherein the second blackening step blackens the outer surface of the edge portion by applying a synthetic resin.
Citation Information
Patent Citations
Infrared lens integrally formed by hot pressing, forming die and preparation method thereof
CN112612097A
Blackening of surface of steel metal product
JP1979056949A
Lens holding member and thin film formation method
JP1993341167A
Lens array, lens array assembly equipped with plurality of the same, intermediate product of lens array and production of lens array
JP2000227505A
Lens holding frame and camera
JP2002072347A