Lens manufacturing method

A two-step lens manufacturing process effectively blackens edge portions during press molding, ensuring consistent light-shielding performance by integrating a blackening treatment before the second molding step to prevent metal exposure.

JP2024147200APending Publication Date: 2024-10-16HOYA CORPORATION
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023060059
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-16

AI Technical Summary

Technical Problem

Existing lens manufacturing methods struggle to reliably blacken the edge portions of lenses with integrated optical function parts, especially when press molding, leading to potential exposure of the base metal and reduced light-shielding effectiveness due to deformation.

Method used

A two-step manufacturing process involving a first molding step to form the edge portion, followed by a blackening treatment, and a second molding step to integrate the optical function part, ensuring the edge portion maintains its blackened state despite deformation during press molding.

Benefits of technology

The method ensures reliable blackening of the edge portion, providing excellent light-shielding performance by preventing exposure of the base metal, even on non-flat surfaces, thus enhancing optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147200000001_ABST
    Figure 2024147200000001_ABST
Patent Text Reader

Abstract

To provide a lens manufacturing method that can achieve an excellent light shielding effect with an edge part surely subjected to blacking processing.SOLUTION: A lens manufacturing method is configured to implement: a first molding step of molding annular edge parts (20 and 50A) by a press-molding; a blacking processing step of conducting blacking processing to an outer surface of the edge part molded in the first molding step; and a second molding step of molding edge parts (20 and 50B) having the blacking processing conducted, and an optical function part (10) surrounded by the edge part to form optical surfaces (11 and 12) in the optical function part, and mutually fixing the optical function part and the edge parts (20 and 50A), in which a surface area increase rate of the edge part in the second molding step is configured to be within 5% in relation to the edge part molded in the first molding step.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a lens. [Background technology]

[0002] Patent Document 1 describes a technology for obtaining a high-performance lens with a multifunctional carrier by integrally bonding a carrier having a centering function between a molding die and a lens frame and a glass material during press molding in order to suppress accuracy errors such as decentering when manufacturing a lens by press molding. Patent Document 1 also describes a method for preventing ghosts and flares by applying a black paint to the inner peripheral surface of the multifunctional carrier before press molding. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 63-40733 Summary of the Invention [Problem to be solved by the invention]

[0004] In lenses with a structure in which the outside of an optical function part having an optical surface (lens surface) is surrounded by a edge part made of a different material from the optical function part, it is necessary to ensure optical performance by suppressing the reflection of harmful light at the edge part. For example, in the case of a metal edge part, if the lens is constructed while retaining its metallic luster, harmful reflected light is likely to occur, so measures are required to improve the light blocking properties by blackening the surface of the edge part.

[0005] In addition, in edge portions with a small thickness in the optical axis direction or edge portions with a large area of ​​the front and rear surfaces facing forward and backward in the optical axis direction, light reflected not only from the inner surface of the edge portion but also from the outer surface portions other than the inner surface is likely to cause stray light, so high light-blocking performance is also required in the outer surface portions other than the inner surface.

[0006] In the case of a lens manufacturing method in which the optical function part and the edge are integrated by press molding, it is assumed that the edge will be blackened before press molding, because it is difficult to blacken the inner peripheral surface of the edge after it has been integrated with the optical function part. However, if press molding is performed on a blackened edge, the bare metal of the edge will be exposed due to deformation during press molding, which may reduce the effect of the blackening treatment.

[0007] In the lens with multifunctional carrier described in Patent Document 1, the inner surface of the multifunctional carrier is blackened by applying black paint, but no special light-blocking measures are taken for areas other than the inner surface, and the above-mentioned problem is not solved.

[0008] The present invention has been made based on the above-mentioned problem awareness, and has as its object to provide a method for manufacturing a lens that can reliably blacken the edge portion to obtain an excellent light-shielding effect. [Means for solving the problem]

[0009] A manufacturing method of a lens according to one embodiment of the present invention includes a first molding step of molding an annular edge portion by press molding, a blackening treatment step of performing a blackening treatment on the outer surface of the edge portion molded in the first molding step, and a second molding step of press molding the edge portion that has been blackened and an optical functional portion surrounded by the edge portion to form an optical surface on the optical functional portion and to fix the optical functional portion and the edge portion to each other, and is characterized in that the surface area increase rate of the edge portion in the second molding step is within 5% based on the edge portion molded in the first molding step.

[0010] It is preferable that the edge portion is formed in the first molding step so that at least one of the outer surfaces on both sides facing the optical axis direction includes a non-flat portion.

[0011] It is preferable that the non-flat portion has a step shape connecting two flat portions at different positions in the optical axis direction, and the difference in the optical axis direction between the height of the step shape molded in the first molding step and the height of the step shape molded in the second molding step is 0.1 mm or less.

[0012] It is preferable that the press molding is performed using the same mold in the first molding step and the second molding step.

[0013] Alternatively, in the first molding step and the second molding step, press molding may be performed using different molding dies having edge-forming surfaces with similar shapes for molding the edge portions.

[0014] As an example, the edge portion is made of metal, and the blackening step blackens the outer surface of the edge portion by oxidizing the metal through heating.

[0015] As an example, the blackening step blackens the outer surface of the edge portion by chemical conversion treatment.

[0016] As an example, the blackening step blackens the outer surface of the edge portion by plating. Effect of the Invention

[0017] By applying the lens manufacturing method of the present invention, even in the case of performing press molding that involves deformation of the edge portion, the edge portion can be reliably blackened, and an excellent light blocking effect can be obtained. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a cross-sectional view showing a lens configuration. [Diagram 2] FIG. 2 is a diagram illustrating a first molding step. [Diagram 3] FIG. 2 is a diagram illustrating a first molding step. [Figure 4] FIG. 13 is a diagram illustrating a blackening process step. [Diagram 5]FIG. 11 is a diagram illustrating a second molding step. [Figure 6] FIG. 11 is a diagram illustrating a second molding step. [Figure 7] 5A to 5C are diagrams illustrating a second embodiment of a method for manufacturing a lens. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] A method for manufacturing a lens according to the present invention will be described below based on the illustrated embodiment. First, the configuration of a lens 1 manufactured by a manufacturing method to which the present invention is applied will be described with reference to Fig. 1. The direction along the optical axis X1 of the lens 1 is defined as the optical axis direction, and the direction perpendicular to the optical axis X1 is defined as the direction orthogonal to the optical axis. The direction orthogonal to the optical axis can also be called the radial direction of the lens 1. Fig. 1 is a cross-sectional view showing the lens 1 at a cross-sectional position including the optical axis X1.

[0020] The lens 1 is composed of an optical function part 10 made of glass and an annular edge part 20 that surrounds the outside of the optical function part 10. The edge part 20 is made of a material different from the glass that constitutes the optical function part 10, and in this embodiment, the edge part 20 is made of metal. The metal that constitutes the edge part 20 may be selected from a material that can be deformed together with the glass material that constitutes the optical function part 10 near the forming temperature of the glass material.

[0021] The optical function section 10 has optical surfaces (lens surfaces) on both sides in the optical axis direction. The lens 1 of this embodiment is a biconvex lens in which the optical surfaces 11 and 12 on both sides of the optical function section 10 are both convex. The side in the optical axis direction to which the optical surface 11 faces is defined as a first direction Xa, and the side to which the optical surface 12 faces is defined as a second direction Xb. Note that the optical surface of the lens formed by applying the manufacturing method of the present invention is not limited to this embodiment, and the optical surface may be any of a convex surface, a concave surface, and a flat surface. In addition, the optical surface may be a spherical surface or an aspherical surface.

[0022] The optical function portion 10 has an outer peripheral surface 13 that connects the outer edge portions of the optical surface 11 and the optical surface 12. The outer peripheral surface 13 is a cylindrical surface centered on the optical axis X1.

[0023] The edge portion 20 has a front surface portion 21 as an outer surface facing a first direction Xa, which is one side of the optical axis direction. The front surface portion 21 has, in order from the inner diameter side closest to the optical surface 11, an inner flat surface 21a, a tapered surface 21b, and an outer flat surface 21c.

[0024] The edge portion 20 has a rear surface portion 22 as an outer surface facing the second direction Xb, which is the other side of the optical axis direction. The rear surface portion 22 has, in order from the inner diameter side closest to the optical surface 12, an inner flat surface 22a, a tapered surface 22b, and an outer flat surface 22c.

[0025] The front and rear of the front surface portion 21 and the rear surface portion 22 are designated for convenience. This does not limit the front surface portion 21 (first direction Xa) to face forward in the optical axis direction of the optical system and the rear surface portion 22 (second direction Xb) to face backward in the optical axis direction of the optical system when the lens 1 is incorporated into an optical device.

[0026] The inner flat surface 21a and the outer flat surface 21c in the front surface portion 21, and the inner flat surface 22a and the outer flat surface 22c in the rear surface portion 22 are each a plane substantially perpendicular to the optical axis X1, and are provided in an annular range centered on the optical axis X1. The tapered surface 21b and the tapered surface 22b are each a truncated cone-shaped surface whose diameter increases as it advances in the second direction Xb in the optical axis direction (and whose diameter decreases as it advances in the first direction Xa). The front surface portion 21 has a structure in which the inner flat surface 21a and the outer flat surface 21c, which are two flat portions located at different positions in the optical axis direction, are connected by the tapered surface 21b which is a step shape, and the tapered surface 21b forms a non-flat portion in the front surface portion 21. The rear surface portion 22 has a structure in which two flat portions, an inner flat surface 22a and an outer flat surface 22c, which are located at different positions in the optical axis direction, are connected by a tapered surface 22b having a step shape, and the tapered surface 22b forms a non-flat portion of the rear surface portion 22.

[0027] In the edge portion 20, the region including the inner flat surface 21a and the inner flat surface 22a is defined as the inner flat portion 20a, the region including the tapered surface 21b and the tapered surface 22b is defined as the intermediate tapered portion 20b, and the region including the outer flat surface 21c and the outer flat surface 22c is defined as the outer flat portion 20c. The edge portion 20 is configured such that the inner flat portion 20a and the outer flat portion 20c are partially shifted in the optical axis direction with the intermediate tapered portion 20b in between.

[0028] The edge portion 20 has an inner peripheral surface 23 that connects the inner edge portions of the inner flat surface 21a and the inner flat surface 22a, and an outer peripheral surface 24 that connects the outer edge portions of the outer flat surface 21c and the outer flat surface 22c. The inner peripheral surface 23 and the outer peripheral surface 24 are each a cylindrical surface centered on the optical axis X1. The inner peripheral surface 23 of the edge portion 20 is fixed to the outer peripheral surface 13 of the optical function portion 10. The outer peripheral surface 24 of the edge portion 20 is a surface that constitutes the outermost edge of the lens 1.

[0029] The outer surface of the edge portion 20 is blackened to suppress light reflection, as will be described in detail later. The blackening of the edge portion 20 suppresses internal reflection at the inner circumferential surface 23 and the generation of stray light that does not pass through the optical function portion 10 in a proper path when the lens 1 is incorporated into an optical device, thereby improving the optical performance (light blocking effect). The outer surface of the edge portion 20 refers to the portion that appears on the outside when the edge portion 20 and the annular member 31 that is its base material are in a single state (before being combined with the optical function portion 10), and the inner circumferential surface 23 that is fixed to the outer circumferential surface 13 of the optical function portion 10 when the lens 1 is completed, and the inner circumferential surface 34 of the annular member 31 are also included in the outer surface of the edge portion 20. The blackening of the outer surface is a process for reducing light reflection by preventing the color and luster of the metal (base metal) that is the material of the edge portion 20 from being exposed to the outer surface as it is. The blackening process is not limited to making the outer surface of the edge 20 completely black, but may be any process that provides a predetermined level of reflection reduction effect compared to when the bare metal of the edge 20 is exposed.

[0030] Next, the configuration of the mold 40 used in manufacturing the lens 1 will be described with reference to Figs. 2, 3, 5, and 6. The mold 40 is composed of a body mold 41, a lower mold 42, and an upper mold 43. The body mold 41 is cylindrical and has an internal space surrounded by an inner peripheral surface 41a, which is a cylindrical surface. The central axis X2 of the mold 40 is an axis line extending in the vertical direction through the center of the inner peripheral surface 41a. The body mold 41 has a body mold lower end surface 41b at its lower end and a body mold upper end surface 41c at its upper end. The body mold lower end surface 41b and the body mold upper end surface 41c are each surfaces approximately perpendicular to the central axis X2. The internal space of the body mold 41 penetrates in the vertical direction and opens at the inner regions of the body mold lower end surface 41b and the body mold upper end surface 41c.

[0031] The lower mold 42 has an insertion part 42a inserted from below into the internal space of the body mold 41, and a large-diameter part 42b provided at the bottom of the insertion part 42a and having a larger diameter than the insertion part 42a. The upper mold 43 has an insertion part 43a inserted from above into the internal space of the body mold 41, and a large-diameter part 43b provided at the top of the insertion part 43a and having a larger diameter than the insertion part 43a. The outer peripheral surfaces of the insertion part 42a and the insertion part 43a can slide in the vertical direction relative to the inner peripheral surface 41a of the body mold 41, and movement in a direction perpendicular to the central axis X2 is restricted. In other words, the lower mold 42 and the upper mold 43 can move in the vertical direction relative to the body mold 41 in a state where the central axes of the lower mold 42 and the upper mold 43 are aligned to coincide with the central axis X2.

[0032] The lower die 42 has an optical forming surface 44 at the upper end of the insertion portion 42a. The optical forming surface 44 is a concave surface that is deepest at the center on the central axis X2 and becomes shallower toward the outer diameter side. At the upper end of the insertion portion 42a, a flange forming surface 45 is further formed around the optical forming surface 44. The flange forming surface 45 has an inner flat surface 45a, a tapered surface 45b, and an outer flat surface 45c, in that order from the inner side toward the outer side in the radial direction close to the optical forming surface 44. The inner flat surface 45a and the outer flat surface 45c are surfaces that are approximately perpendicular to the central axis X2 and are provided in an annular range centered on the central axis X2. The outer flat surface 45c is located above the inner flat surface 45a. The tapered surface 45b is a truncated cone-shaped surface centered on the central axis X2, and one end (the end on the small diameter side) of the tapered surface 45b is connected to the inner flat surface 45a, and the other end (the end on the large diameter side) of the tapered surface 45b is connected to the outer flat surface 45c.

[0033] The upper mold 43 has an optical forming surface 46 at the lower end of the insertion portion 43a. The optical forming surface 46 is a concave surface that is deepest at the center on the central axis X2 and becomes shallower toward the outer diameter side. At the lower end of the insertion portion 43a, a flange forming surface 47 is further formed around the optical forming surface 46. The flange forming surface 47 has an inner flat surface 47a, a tapered surface 47b, and an outer flat surface 47c, in that order from the inner side toward the outer side in the radial direction close to the optical forming surface 46. The inner flat surface 47a and the outer flat surface 47c are surfaces that are approximately perpendicular to the central axis X2, and are provided in an annular range centered on the central axis X2. The outer flat surface 45c is located above the inner flat surface 45a. The tapered surface 47b is a truncated cone-shaped surface centered on the central axis X2, and one end (the end on the small diameter side) of the tapered surface 47b is connected to the inner flat surface 47a, and the other end (the end on the large diameter side) of the tapered surface 47b is connected to the outer flat surface 47c.

[0034] When forming lens 1 by press molding using mold 40, the positions at which insertion portion 42a of lower mold 42 and insertion portion 43a of upper mold 43 are each most inserted into barrel mold 41 are called the press movement ends of lower mold 42 and upper mold 43. As shown in Figures 3 and 6, when lower mold 42 and upper mold 43 reach their respective press movement ends, optical forming surfaces 44 and optical forming surfaces 46, and edge forming surfaces 45 and edge forming surfaces 47 face each other with a predetermined gap between them in the vertical direction.

[0035] As an example, the position where the large diameter portion 42b abuts against the barrel mold lower end surface 41b can be set as the press movement end of the lower mold 42. Also, the position where the large diameter portion 43b abuts against the barrel mold upper end surface 41c can be set as the press movement end of the upper mold 43. Alternatively, the press movement end of the upper mold 43 may be determined by a configuration other than the large diameter portion 43b abutting against the barrel mold upper end surface 41c.

[0036] In manufacturing the lens 1, a glass preform 30, which is the base material of the optical function part 10, and the edge part 20 are placed inside a molding die 40 (see FIG. 5), and a lower die 42 and an upper die 43 are brought close to each other to perform press molding to integrate the optical function part 10 and the edge part 20 (see FIG. 6). The glass preform 30 is made of spherical glass.

[0037] When blackening the outer surface of edge portion 20, when lens 1 is completed as shown in Figure 1, it is difficult to subsequently blacken inner surface 23 of edge portion 20 (especially the portion that is fixed to outer surface 13 of optical function portion 10).

[0038] On the other hand, if blackening treatment is performed on the outer surface of the base material of edge portion 20 (annular member 31 shown in FIG. 2) before press forming with forming die 40, the effect of the blackening treatment may be lost when the base material is transformed into edge portion 20 by press forming, as the metal bare metal is partially exposed on the outer surface of edge portion 20. In particular, in the front surface portion 21 and rear surface portion 22 which are extended in the radial direction and have non-flat portions (step shapes) such as tapered surface 21b and tapered surface 22b, the metal bare metal is likely to be exposed due to the effects of press forming.

[0039] The lens manufacturing method of the present embodiment uses press molding to obtain a lens 1 in which the outer surface of the edge portion 20 is reliably blackened, and the details of this method will be described below.

[0040] The manufacturing method of the lens of this embodiment includes a first molding step, a blackening step, and a second molding step. Figures 1, 4(B), 5, and 6 show the edge portion 20 after the blackening step, and the blackened outer surface of the edge portion 20 is highlighted by a thick line.

[0041] [First molding step] 2 and 3 show the first molding step. In the first molding step, the edge portion 20 is formed from the annular member 31 (base material of the edge portion 20) by press molding using a molding die 40. The annular member 31 has annular flat surfaces 32 and 33 that are approximately perpendicular to the central axis X2 when placed in the molding die 40, a cylindrical inner circumferential surface 34 that connects the inner edge portions of the flat surfaces 32 and 33, and a cylindrical outer circumferential surface 35 that connects the outer edge portions of the flat surfaces 32 and 33.

[0042] In the first molding step, as shown in FIG. 2, the annular member 31 is held between the lower die 42 and the upper die 43 of the molding die 40. The flat surface 32 of the annular member 31 is placed on the outer flat surface 45c of the edge forming surface 45, and is held in a state in which a part of the flat surface 32 protrudes toward the inner diameter side (at a position closer to the central axis X2) than the outer flat surface 45c. The lower die 42 is held at the press moving end with the large diameter portion 42b abutting against the lower end surface 41b of the body die, and the lower die 42 is supported from below so that the insertion portion 42a does not come off the body die 41. The inside of the molding die 40 is set to a temperature suitable for press molding the annular member 31. This temperature varies depending on the material of the annular member 31, and may be set to room temperature or may be heated to a predetermined temperature.

[0043] Next, the upper die 43 with the insertion portion 43a inserted into the body die 41 is pressed downward using a press device (not shown). The edge forming surface 47 of the descending upper die 43 presses the flat surface 33 of the annular member 31 from above. The thickness of the annular member 31 from the flat surface 32 to the flat surface 33 before pressing is set to be larger than the distance between the edge forming surface 45 and the edge forming surface 47 when the lower die 42 and the upper die 43 are at their respective press movement ends. Therefore, when the lower die 42 and the upper die 43 are moved toward each other to their respective press movement ends, the annular member 31 is deformed and extended in the radial direction by the pressing force of the edge forming surface 45 and the edge forming surface 47.

[0044] More specifically, the annular member 31 extends toward the inner diameter side and the outer diameter side while decreasing the thickness in the direction along the central axis X2. When the upper die 43 is lowered to the pressing movement end shown in FIG. 3, the shape of the flat surface 32 side changes to a shape along the edge forming surface 45 to become the front surface 21. That is, the inner flat surface 21a having a shape transferred from the inner flat surface 45a, the tapered surface 21b having a shape transferred from the tapered surface 45b, and the outer flat surface 21c having a shape transferred from the outer flat surface 45c are formed. Also, the shape of the flat surface 33 side changes to a shape along the edge forming surface 47 to become the rear surface 22. That is, the inner flat surface 22a having a shape transferred from the inner flat surface 47a, the tapered surface 22b having a shape transferred from the tapered surface 47b, and the outer flat surface 22c having a shape transferred from the outer flat surface 47c are formed.

[0045] The inner peripheral surface 23 of the flange 20 is formed from the inner peripheral surface 34 of the annular member 31 extending inwardly, and has a generally cylindrical shape centered on the optical axis X1. The outer peripheral surface 24 of the flange 20 is formed from the outer peripheral surface 35 of the annular member 31 extending outwardly, and has a generally cylindrical shape centered on the optical axis X1.

[0046] [Blackening process step] When the first molding step is completed, the mold 40 is disassembled to remove the molded edge portion 20. Next, a blackening step is performed to blacken the outer surface of the edge portion 20. Fig. 4(A) shows the edge portion 20 before the blackening step, and Fig. 4(B) shows the edge portion 20 after the blackening step.

[0047] As a method of blackening treatment in the blackening treatment step, for example, oxidation by heating metal, chemical conversion treatment, plating treatment, etc. can be applied. In oxidation by heating metal, the outer surface of the annular member 31, which is the workpiece, is oxidized by heating in an atmosphere containing oxygen, and the metallic luster is removed and blackened. Examples of metal materials that are easily oxidized by heating include copper and iron. As an example of chemical conversion treatment, the annular member 31, which is the workpiece made of iron, is immersed in an alkaline aqueous solution to form a black oxide film (iron tetroxide film) on the outer surface of the annular member 31. As an example of plating treatment, plating such as black nickel plating or black chrome plating is performed on the outer surface of the annular member 31, which is the workpiece.

[0048] The second molding step, which follows the blackening step, is carried out in a state where the glass preform 30 is heated to a temperature above the glass transition temperature at which the glass preform 30 softens. Therefore, the area blackened in the blackening step is required to have heat resistance that does not deteriorate or damage even when heated to the glass transition temperature range. Each of the above methods satisfies this heat resistance condition.

[0049] By subjecting the edge portion 20 in a separate state before being fixed to the optical function portion 10 to blackening treatment, the entire edge portion 20 including the inner peripheral surface 23, which is difficult to blacken after being fixed to the optical function portion 10, can be reliably blackened.

[0050] In the blackening step, the entire outer surface of the edge portion 20 may be blackened according to a uniform standard. Alternatively, the degree of blackening may be varied for each portion of the edge portion 20 to set a light blocking effect suitable for each portion of the edge portion 20. When the degree of blackening is varied for each portion, it is also possible to use a different blackening method for each portion of the edge portion 20.

[0051] For example, the inner circumferential surface 23 of the edge portion 20 constitutes the inner surface of the optical path surrounding the optical function portion 10, and is a portion where suppression of internal reflection is particularly important. Therefore, in the blackening treatment step, the effect of preventing stray light on the inner circumferential surface 23 may be improved by making a selection such as increasing the thickness of the blackening layer or using a blackening material with high blackness.

[0052] The front surface 21, rear surface 22 and outer circumferential surface 24 of the edge portion 20 are used to position the lens 1 relative to the lens barrel, other lenses, etc. Therefore, in the blackening step, the thickness of the blackening layer may be reduced, or a type of blackening treatment with excellent surface accuracy may be selected, thereby minimizing the effect on the shape accuracy of the outer surface of the edge portion 20 as much as possible and achieving excellent positioning accuracy.

[0053] [Second molding step] After the blackening step is completed, the second molding step is performed. As shown in Fig. 5, in the second molding step, the edge portion 20 (whose outer surface has already been blackened) and the glass preform 30 are held between the lower mold 42 and the upper mold 43 of the molding die 40. The lower mold 42 is held at the press moving end with the large diameter portion 42b abutting against the lower end surface 41b of the body mold. In addition, the lower mold 42 is supported from below so that the insertion portion 42a does not come off the body mold 41.

[0054] The glass preform 30 is placed on the optical forming surface 44 of the lower mold 42. The glass preform 30 is held at a position on the central axis X2 by the recessed shape of the optical forming surface 44. The glass preform 30 may be supplied onto the optical forming surface 44 with the insertion portion 42a removed downward from the body mold 41, or may be supplied from the upper end side of the body mold 41 with the insertion portion 42a inserted into the body mold 41.

[0055] The front surface 21 of the edge portion 20 is placed on the edge portion forming surface 45 of the lower die 42. Since the front surface 21 has been molded into a shape that is a transfer of the edge portion forming surface 45 in the previous first molding step, the edge portion 20 can be held on the edge portion forming surface 45 with high precision and stability.

[0056] As shown in Fig. 5, after the glass preform 30 and the edge portion 20 are placed inside the molding die 40, the glass preform 30 is softened by heating it until it exceeds the glass transition temperature of the glass preform 30. Then, using a pressing device (not shown), the upper die 43 with the insertion portion 43a inserted into the body die 41 is pressed downward. The glass preform 30 is pressed and deformed between the optical forming surface 46 of the descending upper die 43 and the optical forming surface 44 of the lower die 42 whose descending is restricted. The glass preform 30 extends toward the outer diameter side while decreasing its thickness in the direction along the central axis X2.

[0057] The second molding step is performed in a nitrogen gas atmosphere that does not contain enough oxygen to oxidize the edge portion 20, so that the edge portion 20 does not become blackened due to oxidation when it is heated together with the glass preform 30. Therefore, it is necessary to blacken the edge portion 20 (particularly the inner peripheral surface 23) in a blackening step prior to the second molding step.

[0058] When the upper die 43 is lowered to the pressing movement end shown in Fig. 6, the glass preform 30 is pressed by the lower die 42 and the upper die 43 in the inner region of the annular member 31, and as a result, the optical functional part 10 having the optical surfaces 11 and 12 to which the shapes of the optical forming surfaces 44 and the optical forming surfaces 46 are transferred on both sides in the optical axis direction is formed. In addition, when the glass preform 30 is extended toward the outer diameter side to become the optical functional part 10, the outer peripheral surface 13 of the optical functional part 10 is in close contact with the inner peripheral surface 23 of the edge part 20 and fixed to each other, and the optical functional part 10 and the edge part 20 are integrated to form the lens 1. The outer peripheral surface 13 of the optical functional part 10 has a substantially cylindrical shape corresponding to the inner peripheral surface 23 of the edge part 20.

[0059] In the previous first molding step, the rear surface 22 of the edge 20 is molded into a shape that is a transfer of the edge forming surface 47 of the upper die 43, so when the upper die 43 moves to the press movement end in Fig. 6 in the second molding step, the rear surface 22 does not receive a strong pressing force from the edge forming surface 47, and the edge 20 maintains its original shape. Therefore, the shape of the edge 20 does not change before and after the second molding step.

[0060] By making the edge portion 20 at the stage where the first molding step has been performed and the edge portion 20 at the stage where the second molding step has been performed identical in shape and preventing local deformation or increase in surface area of ​​the edge portion 20 in the second molding step, exposure of the metal base metal on the outer surface of the edge portion 20 can be prevented, and the effect of blackening performed in the blackening treatment step can be maintained even after press molding in the second molding step.

[0061] After the second molding step is completed, the lens 1 is cooled to a predetermined temperature and then disassembled to remove the mold 40. In this manner, the lens 1 (FIG. 1) is formed, which has a hybrid structure consisting of an optical function part 10, which is a press-molded glass product, and a metal edge part 20.

[0062] 1, in the completed lens 1, the entire outer surface of the edge portion 20, including the front portion 21, the rear portion 22, the inner peripheral surface 23, and the outer peripheral surface 24, is blackened. After the shape of the edge portion 20 is changed from the annular member 31 in the first molding step, the edge portion 20 after the shape change is subjected to a blackening treatment in a blackening treatment step, and deformation of the edge portion 20 is suppressed in the second molding step after the blackening treatment, so that it is possible to obtain lens 1 with edge portion 20 reliably blackened without being affected by the deformation of the edge portion 20 from the annular member 31 in the first molding step.

[0063] In particular, non-flat portions such as tapered surface 21b and tapered surface 22b are areas where the metal base is likely to be exposed when press-molded after blackening treatment, but such non-flat portions can also be reliably blackened.

[0064] In the blackening step, the edge portion 20 is blackened while it is in a separate state, so that the work can be performed efficiently. For example, when blackening the edge portion 20, there is no need to mask the optical surfaces 11 and 12 of the optical function portion 10 to protect them from dirt or clouding.

[0065] In the blackening step, the entire edge portion 20 may be subjected to the blackening treatment, or only a specific portion of the edge portion 20 may be subjected to the blackening treatment.

[0066] For example, as described above, in locations including non-flat portions such as tapered surface 21b and tapered surface 22b of edge portion 20, the base metal is likely to be exposed due to changes in shape caused by press molding. Therefore, it is preferable that at least tapered surface 21b and its periphery, and tapered surface 22b and its periphery of edge portion 20 are included in the target region of the blackening treatment in the blackening treatment step.

[0067] Furthermore, the inner flat surface 21a and the outer flat surface 21c of the front surface 21, and the inner flat surface 22a and the outer flat surface 22c of the rear surface 22 are parts that receive a force that causes the edge portion 20 to extend in the radial direction during press molding by the molding die 40. Even if there is no significant change in shape such as a step, bend, or unevenness, such extended parts may be expanded relative to the original blackened area, resulting in the exposure of the base metal. Therefore, by including the inner flat surface 21a, the outer flat surface 21c, the inner flat surface 22a, and the outer flat surface 22c in the blackening treatment step, a more reliable light-shielding effect can be obtained.

[0068] In addition, in the blackening step, it is also possible to intentionally exclude a predetermined portion of the edge portion 20 from the blackening treatment. For example, when the lens 1 is incorporated into the lens barrel of an optical device, the outer peripheral surface 24 of the edge portion 20 may be surrounded and held by the inner surface of the lens barrel, resulting in a structure in which light in the optical path does not reach the outer peripheral surface 24. In such a case, omitting the blackening treatment of the outer peripheral surface 24 does not affect the optical performance, so it is possible to choose not to blacken the outer peripheral surface 24 in the blackening treatment step.

[0069] In the blackening step, when only a portion of the edge portion 20 is blackened, the blackening process may be performed while masking the other portions.

[0070] Next, a second embodiment of the manufacturing method of the lens to which the present invention is applied will be described with reference to FIG. 7. The second embodiment is common to the above embodiment in that the processing is performed in the order of a first molding step, a blackening treatment step, and a second molding step. FIG. 7(A) shows an edge portion 50A at the stage where the first molding step is completed. FIG. 7(B) shows an edge portion 50B at the stage where the blackening treatment step is completed. FIG. 7(C) shows a lens 1 in a state where the optical function portion 10 and the edge portion 50C are integrated after the second molding step is completed. The optical function portion 10 shown in FIG. 7(C) has the same configuration and manufacturing method as the above embodiment, and therefore will not be described.

[0071] As a difference from the edge portion 20 manufactured by the manufacturing method of the above embodiment, in the second embodiment, the edge portion 50A at the stage of being molded in the first molding step and the edge portion 50B after the blackening treatment have different shapes from the edge portion 50C molded in the second molding step.

[0072] That is, the configuration of the first mold for forming the edge portion 50A in the first molding step and the configuration of the second mold for forming the edge portion 50C in the second molding step are different from each other. Although the first mold and the second mold are not illustrated, the shape of the edge portion forming surface of the lower mold and the upper mold of the first mold corresponds to the shape of the front portion 51 and the rear portion 52 of the edge portion 50A (50B), and the shape of the edge portion forming surface of the lower mold and the upper mold of the second mold corresponds to the shape of the front portion 51 and the rear portion 52 of the edge portion 50C. Since the optical function portion 10 is not molded in the first molding step, the lower mold and the upper mold of the first mold may be configured to omit the optical forming surface corresponding to the optical forming surface 44 and the optical forming surface 46 of the above embodiment.

[0073] 7(C), the edge portion 50C after the completion of the second molding step has a front portion 51 as an outer surface facing the first direction Xa, and a rear portion 52 as an outer surface facing the second direction Xb. The edge portion 50C also has a cylindrical inner circumferential surface 53 fixed to the outer circumferential surface 13 of the optical function portion 10, and a cylindrical outer circumferential surface 54 that constitutes the outermost edge of the lens 1.

[0074] The front surface 51 has an inner flat surface 51a, a tapered surface 51b, and an outer flat surface 51c, in that order from the inner diameter side close to the optical surface 11. The rear surface 52 has an inner flat surface 52a, a tapered surface 52b, and an outer flat surface 52c, in that order from the inner diameter side close to the optical surface 11. The inner flat surface 51a, the outer flat surface 51c, the inner flat surface 52a, and the outer flat surface 52c are each flat surfaces approximately perpendicular to the optical axis X1. The tapered surface 51b and the tapered surface 52b are each a truncated cone-shaped surface whose diameter increases as it advances in the second direction Xb in the optical axis direction (the diameter decreases as it advances in the first direction Xa). Therefore, although there are some differences in the dimensions of each surface, the edge portion 50C basically has the same configuration as the edge portion 20 of the above embodiment, and has the tapered surface 51b and the tapered surface 52b, which are non-flat portions (step shapes).

[0075] Of the edge portion 50, the region including the inner flat surface 51a and the inner flat surface 52a is referred to as the inner flat portion 50a, the region including the tapered surface 51b and the tapered surface 52b is referred to as the intermediate tapered portion 50b, and the region including the outer flat surface 51c and the outer flat surface 52c is referred to as the outer flat portion 50c.

[0076] In the first molding step, a simple circular metal annular member (not shown) like the annular member 31 of the above embodiment is press molded using a first mold to form the edge portion 50A shown in Fig. 7(A). The edge portion 50A after the first molding step has step surfaces 51d and 52d as portions corresponding to the tapered surfaces 51b and 52b of the edge portion 50C. The step surfaces 51d and 52d are cylindrical surfaces that are approximately perpendicular (parallel to the optical axis X1) to the inner flat surface 51a, the outer flat surface 51c, the inner flat surface 52a, and the outer flat surface 52c, respectively. In consideration of ease of release of the lower and upper dies in the first molding die, the step surfaces 51 d and 52 d may be truncated cone-shaped surfaces having a predetermined inclination (draft gradient) with a smaller angle of inclination with respect to the optical axis X1 than the tapered surfaces 51 b and 52 b, rather than being cylindrical surfaces completely parallel to the optical axis X1.

[0077] In the blackening step, the outer surface of the edge portion 50A formed in the first molding step is blackened to form the edge portion 50B having a blackened outer surface. The blackening method in the blackening step can be the same as that in the above embodiment.

[0078] In the second molding step, the glass preform is pressed by the optical forming surfaces of the lower and upper dies of the second mold to form the optical function portion 10. The edge portion 50B is pressed by the edge forming surfaces of the lower and upper dies of the second mold to form the edge portion 50C. The outer peripheral surface 13 of the optical function portion 10 and the inner peripheral surface 53 of the edge portion 50C are then closely fixed to each other to form the lens 1.

[0079] The edge forming surfaces of the lower and upper dies of the second mold have a tapered surface corresponding to the shape of the tapered surface 51b and a tapered surface corresponding to the shape of the tapered surface 52b. In the second molding step, these tapered surfaces of the second mold come into contact with and press the step surface 51d and the step surface 52d of the edge 50B, deforming the step surface 51d into the tapered surface 51b and deforming the step surface 52d into the tapered surface 52b. During this deformation, the edge 50B is slightly extended in the radial direction to become the edge 50C. In other words, the surface area increases with the deformation from the edge 50B to the edge 50C.

[0080] The amount of deformation from edge portion 50B to edge portion 50C in the second molding step is small, and the shape of edge portion 50A molded in the first molding step is maintained except that the inclination of step surface 51d and step surface 52d is slightly changed to form tapered surface 51b and tapered surface 52b. In other words, edge portion 50A molded in the first molding step has a shape similar to edge portion 50C molded in the second molding step. In other words, the edge portion forming surface of the first molding die that molds edge portion 50A and the edge portion forming surface of the second molding die that molds edge portion 50C have similar shapes.

[0081] In the first molding step, in which edge portion 50A including non-flat portions (step surface 51d and step surface 52d) is molded using a simple flat-shaped annular member as a base material, the deformation amount (increase in surface area) of edge portion 50A due to molding is large, so blackening treatment is not performed before the first molding step. Then, in the second molding step, in which edge portion 50C, which has an approximate shape of edge portion 50A (50B), is finished, the deformation amount (increase in surface area) from blackened edge portion 50B to edge portion 50C is small, and exposure of the base metal in edge portion 50C is unlikely to occur. Therefore, even if press molding is performed in the second molding step, the blackening of the outer surface of edge portion 50C is maintained.

[0082] In this way, even with the manufacturing method of the second embodiment, it is possible to obtain a lens 1 in which the edge portion 50C is reliably blackened after the second molding step, without being affected by the deformation of the annular member to the edge portion 50A in the first molding step.

[0083] In each of the above embodiments, the edge portion (20, 50A) having the same shape or a similar shape to the final edge portion (20, 50C) press-molded together with the optical function portion 10 is formed in the first molding step, the edge portion is subjected to a blackening treatment step, and then the optical function portion (10) is molded in the second molding step to be integrated with the edge portion (20, 50C). By manufacturing the lens 1 in this manner, the blackening treatment of the edge portion is not affected by the press molding, and each portion of the edge portion is reliably blackened to obtain a lens with excellent light-blocking performance.

[0084] As a result of research by the applicant, it was found that if the increase rate of the surface area of ​​the edge in the second molding step is within 5% based on the edge in the state molded in the first molding step, the effect of the blackening treatment of the edge performed between the first and second molding steps can be maintained without being impaired by the press molding in the second molding step. Therefore, in the present invention, the condition is that the increase rate of the surface area of ​​the edge in the second molding step is within 5%.

[0085] For example, as in the second embodiment, when the shape of the edge portion formed in the first molding step is different from the shape of the edge portion formed in the second molding step, the increase rate of the designed surface area of ​​the edge portion in the second molding step is set to within 5%. Alternatively, the increase rate of the designed surface area of ​​the edge portion in the second molding step may be set to a predetermined value smaller than 5%, taking into account a margin of error in molding accuracy in the first and second molding steps.

[0086] As in the first embodiment, when the same mold is used in the first and second molding steps and the edge portions molded in each molding step have the same shape by design, the increase rate of the edge portion surface area in the second molding step is 0%, so the above condition is met. However, based on differences in the implementation conditions (e.g., temperature) of each molding step and tolerances in accuracy during molding, the shapes of the edges actually molded in the first and second molding steps may be very slightly different. Even in such a case, the above condition can be met by performing management to select those in which the increase rate of the edge portion surface area in the second molding step is within 5% as acceptable and those in which the increase rate of the edge portion surface area in the second molding step is more than 5% as unacceptable.

[0087] Alternatively, as in the first embodiment, it is possible to use the same mold in the first and second molding steps, but to make the shape of the edge formed in the first molding step and the shape of the edge formed in the second molding step similar (not identical) to each other by making the pressing force (the amount of movement of the press by the mold) different in the first and second molding steps. For example, in the first molding step, the relative movement of the lower and upper molds is stopped just before the end of the press movement, and preliminary processing is performed with a slightly weaker pressing force, and in the second molding step, the lower and upper molds are moved to the end of the press movement, respectively, to form the edge pressed with the original pressing force. In this case, management should be performed so as to satisfy the above-mentioned condition that the increase rate of the surface area of ​​the edge in the second molding step is within 5%.

[0088] In addition, when there is a step shape connecting two flat parts at different positions in the optical axis direction, such as tapered surface 21b and tapered surface 22b of edge portion 20, and tapered surface 51b (step surface 51d) and tapered surface 52b (step surface 52d) of edge portion 50C, it is preferable that the difference in the optical axis direction height of the step shape formed in the first molding step and the optical axis direction height of the step shape formed in the second molding step is 0.1 mm or less. By satisfying this condition, it is possible to suppress the amount of deformation at the step shape in the second molding step to a small amount, and to obtain the effect of preventing bare metal from being exposed on the outer surface of the blackened edge portion.

[0089] For example, in an application example to the second embodiment (Figure 7), the difference between the optical axis direction height t1 of tapered surface 51b and the optical axis direction height t2 of step surface 51d is set to 0.1 mm or less, and the difference between the optical axis direction height t3 of tapered surface 52b and the optical axis direction height t4 of step surface 52d is set to 0.1 mm or less.

[0090] The manufacturing method of the present invention is suitable for lenses having non-flat parts at locations other than the inner peripheral surface of the edge portion, such as the intermediate tapered portion 20b of the edge portion 20 and the intermediate tapered portion 50b of the edge portion 50C, but is not limited to this type of lens, and is also useful for lenses having an edge portion whose entire outer surfaces on both sides in the optical axis direction are flat. When a lens is press-molded using a device such as the mold 40, if a load in the optical axis direction is applied to the edge portion during press molding, the edge portion is stretched in the radial direction. Even if the outer surfaces on both sides in the optical axis direction of the edge portion are flat, the base metal is likely to be exposed on the outer surface as the edge portion is stretched in the radial direction. Therefore, by performing a blackening treatment step in which the flat-shaped front portion and the flat-shaped rear portion of the edge portion are blackened after the press molding in the first molding step, the front portion and the rear portion after the extension can be reliably blackened.

[0091] In addition, in the lens 1 of the above embodiment, the edge portion 20 (50C) has a tapered surface 21b (51b) and a tapered surface 22b (52b) on both sides in the optical axis direction. However, the manufacturing method of the present invention is also useful for a type of lens in which only one of the outer surfaces of the edge portion on both sides facing the optical axis direction has a non-flat portion, and the other outer surface in the optical axis direction is composed only of a flat surface.

[0092] The lens 1 of the above embodiment has tapered surface 21b (51b) and tapered surface 22b (52b) as the non-flat portion of edge portion 20 (50C), but the shape of the non-flat portion of the edge portion of the lens is not limited to this. For example, even if the outer surface of the edge portion has a recess (groove), protrusion, or notch, the location of such recess, protrusion, or notch is suitable for blackening treatment in the blackening treatment step performed between the first molding step and the second molding step.

[0093] The edge portion 20 (50C) in the above embodiment has a configuration in which a uniform shape continues in the circumferential direction centered on the optical axis X1, but the shape of the edge portion may be different in a part of the circumferential direction. For example, a tapered surface, a recess, a protrusion, a notch, etc. may be present only in a part of the circumferential direction of the edge portion.

[0094] In the above embodiment, the spherical glass preform 30 is placed inside the molding die 40 and press-molded, but the glass preform that is the base material for the optically functional portion is not limited to a spherical shape.

[0095] In the lens 1 of the above embodiment, the material of the edge portion 20 (50C) is metal, but the material of the edge portion of the lens manufactured by applying the present invention can be selected to be other than metal. For example, the edge portion may be made of a glass different from the glass that constitutes the optical function portion. Alternatively, the edge portion may be made of ceramics.

[0096] The embodiments of the present invention are not limited to the above-mentioned embodiments or their modifications, and may be modified, substituted, or altered in various ways without departing from the spirit of the technical idea of ​​the present invention. Furthermore, if the technical idea of ​​the present invention can be realized in a different way due to technological progress or other derived technology, it may be implemented using that method. Therefore, the claims cover all embodiments that may be included within the scope of the technical idea of ​​the present invention. [Explanation of symbols]

[0097] 1: Lens 10:Optical function section 11:Optical surface 12:Optical surface 13: Outer surface 20: Edge section 20a:Inner flat part 20b: Intermediate tapered section 20c: Outer flat part 21: Front part (outer surface facing the optical axis direction) 21a: Inner flat surface (flat part) 21b: Tapered surface (non-flat part, step shape) 21c: Outer flat surface (flat part) 22: Rear surface (outer surface facing the optical axis direction) 22a: Inner flat surface (flat part) 22b: Tapered surface (non-flat part, step shape) 22c: Outer flat surface (flat part) 23: Inner surface 24: Outer surface 30: Glass preform 31: Annular member 32:Flat surface 33:Flat surface 34: Inner peripheral surface 35: Outer surface 40: Molding mold 41: Body type 41a: Inner peripheral surface 41b:Bottom end surface 41c: Upper end surface of body mold 42: Lower mold 43: Upper mold 44:Optical forming surface 45: Edge forming surface 45a: Inner flat surface 45b: Tapered surface 45c: Outer flat surface 46:Optical forming surface 47: Edge forming surface 47a: Inner flat surface 47b: Tapered surface 47c: Outer flat surface 50A: Edge (after the first molding step) 50B: Edge (after blackening step) 50C: Edge (after the second molding step) 50a: Inner flat part 50b: Intermediate tapered section 50c: Outer flat part 51: Front part (outer surface facing the optical axis direction) 51a: Inner flat surface (flat part) 51b: Tapered surface (non-flat portion, step shape formed in the second forming step) 51c: Outer flat surface (flat part) 51d: Step surface (non-flat part, step shape formed in the first forming step) 52: Rear surface (outer surface facing the optical axis direction) 52a: Inner flat surface (flat part) 52b: Tapered surface (non-flat portion, step shape formed in the second forming step) 52c: Outer flat surface (flat part) 52d: Step surface (non-flat part, step shape formed in the first forming step) 53: Inner surface 54: Outer surface X1: Optical axis X2: Central axis of the mold

Claims

1. A first molding step of forming an annular edge portion by press molding; a blackening step of performing blackening on the outer surface of the edge portion formed in the first forming step; a second molding step of press-molding the edge portion that has been subjected to the blackening treatment and an optical function portion surrounded by the edge portion to form an optical surface on the optical function portion and to fix the optical function portion and the edge portion to each other; having A method for manufacturing a lens, characterized in that the surface area increase rate of the edge portion in the second molding step is within 5% based on the edge portion molded in the first molding step.

2. The method for manufacturing a lens according to claim 1 , wherein the edge portion is formed in the first molding step so that at least one of the outer surfaces on both sides facing the optical axis direction includes a non-flat portion.

3. 3. The method for manufacturing a lens according to claim 2, characterized in that the non-flat portion has a step shape connecting two flat portions at different positions in the optical axis direction, and a difference in the optical axis direction between a height of the step shape molded in the first molding step and a height of the step shape molded in the second molding step is 0.1 mm or less.

4. The method for manufacturing a lens according to claim 1 , wherein the press molding is performed using the same mold in the first molding step and the second molding step.

5. 4. The method for manufacturing a lens according to claim 1, wherein in the first molding step and the second molding step, press molding is performed using different molding dies having edge-forming surfaces for molding the edge portions with similar shapes.

6. 4. The method for manufacturing a lens according to claim 1, wherein the edge portion is made of metal, and the blackening step blackens an outer surface of the edge portion by oxidizing the metal through heating.

7. The method for manufacturing a lens according to claim 1 , wherein the blackening step blackens the outer surface of the edge portion by chemical conversion treatment.

8. The method for manufacturing a lens according to claim 1 , wherein the blackening step blackens the outer surface of the edge portion by plating.

Citation Information

Patent Citations

  • Infrared lens integrally formed by hot pressing, forming die and preparation method thereof

    CN112612097A

  • Blackening of surface of steel metal product

    JP1979056949A

  • Lens holding member and thin film formation method

    JP1993341167A

  • Optical component and its manufacture method

    JP2007133197A

  • Optical part and method of manufacturing it

    JP2009222781A