Glass top plate for cookers
The glass top plate with an infrared absorbing decorative layer and light shielding layer improves temperature measurement accuracy in cookers by reducing external infrared interference while maintaining decorativeness.
Patent Information
- Application Number
- JP2023060420
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
AI Technical Summary
Infrared sensors in cookers are affected by infrared rays emitted from lighting fixtures, leading to inaccurate temperature measurements due to multiple reflections within the glass top plate, and providing a light shielding layer on the surface limits decorativeness.
A glass top plate with an infrared absorbing decorative layer on the backside and a light shielding layer, combined with a window exposing the glass substrate at the infrared sensor position, maintains brightness and reduces infrared reflections.
The solution enhances temperature detection accuracy by attenuating external infrared interference while allowing for decorative designs, particularly in bright colors.
Smart Images

Figure 2024147415000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass top plate for a cooker. [Background technology]
[0002] Conventionally, there is known a technology for detecting the temperature of cooking equipment such as a pot by using an infrared sensor to detect the intensity of infrared rays emitted from the cooking equipment (see Patent Document 1). According to this technology, temperature detection with excellent thermal response can be performed by directly detecting infrared rays emitted from the bottom of the cooking equipment. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 3-184295 Summary of the Invention [Problem to be solved by the invention]
[0004] In the prior art, infrared rays emitted from a component other than the cooking utensil, such as a lighting fixture, may enter the infrared sensor. For example, infrared rays emitted from a lighting fixture may enter a glass top plate placed on the top surface of the cooking appliance, and may reach the infrared sensor due to multiple reflections within the glass top plate. This may result in the infrared rays emitted from the cooking utensil not being able to be measured accurately.
[0005] In order to solve the above problem, it is conceivable to provide a light-shielding layer on the surface of the glass top plate to block infrared rays from the lighting fixture. However, providing a light-shielding layer on the surface of the glass top plate makes the color tone of the glass top plate darker. This limits the decorativeness of the glass top plate, for example, making it impossible to apply decorations in bright white tones.
[0006] The present invention has been made in view of the above background, and aims to provide a glass top plate for a cooker that improves the temperature detection accuracy of an infrared sensor and also has a decorative feature. [Means for solving the problem]
[0007] One aspect of the present invention is A glass top plate for a cooker is placed on top of a cooker equipped with an infrared sensor, a glass substrate having a front surface and a back surface; an infrared absorbing decorative layer provided on the rear surface side of the glass substrate and containing an infrared absorbing agent and a pigment that absorb infrared rays; an infrared absorbing decorative layer window portion through which the glass substrate is exposed is formed in the infrared absorbing decorative layer at a position overlapping with the infrared sensor in a thickness direction of the glass substrate when the glass top plate is placed in the cooking appliance; The lightness L measured from the front side of the glass substrate in accordance with JIS 8781-4:2013 * is 50 or more, The glass top plate for a cooker has a reflectance of less than 25% for infrared rays having a wavelength of 940 nm as measured from the front surface side of the glass substrate.
[0008] Another aspect of the present invention is A glass top plate for a cooking appliance to be placed on top of a cooking appliance having an infrared sensor, a glass substrate having a front surface and a back surface; a decorative layer provided on the rear surface side of the glass substrate and containing a pigment; At least one infrared absorbing layer including an infrared absorbing agent that absorbs infrared rays; With the glass top plate placed in the cooker, a decorative layer window portion through which the glass substrate is exposed is formed in the decorative layer at a position overlapping with the infrared sensor in a thickness direction of the glass substrate, an infrared absorbing layer window portion through which the glass substrate is exposed is formed in the infrared absorbing layer at a position overlapping with the infrared sensor in a thickness direction of the glass substrate; The lightness L measured from the front side of the glass substrate in accordance with JIS 8781-4:2013 * is 50 or more, The glass top plate for a cooker has a reflectance of less than 25% for infrared rays having a wavelength of 940 nm as measured from the front surface side of the glass substrate. Effect of the Invention
[0009] According to one embodiment and another embodiment of the present invention, the lightness L measured from the front side of the glass substrate in accordance with JIS 8781-4:2013 * Since the value is 50 or more, the glass top plate can be decorated with bright colors such as white pigments or silver pigments, thereby improving the decorativeness of the glass top plate.
[0010] According to one and other aspects of the present invention, the reflectance of infrared rays with a wavelength of 940 nm measured from the front surface side of the glass substrate is less than 25%, so that infrared rays irradiated from the outside of the glass top plate can be attenuated while undergoing multiple reflections inside the glass top plate, thereby improving the detection accuracy of the infrared sensor. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an induction heating cooker according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing a conventional induction heating cooker. [Diagram 3] 1A and 1B are diagrams showing the glass top plate of Examples 1 and 2, where FIG. 1A is a schematic cross-sectional view of the glass top plate, and FIG. 1B is a schematic cross-sectional view showing the state in which visible light and infrared light are multiple-reflected within the glass top plate. [Figure 4]FIG. 4 is a schematic cross-sectional view of the glass top plate of Example 1 for explaining a disturbance strength test method. [Diagram 5] 1 is a graph showing the measurement results of the reflection spectrum of the glass top plates of Examples 1 and 2 and Comparative Examples 1 to 3. [Figure 6] 1 is a graph showing the measurement results of the reflection spectrum of an aluminum metal plate and a SUS430 metal plate. [Figure 7] 1 is a graph showing the results of a disturbance resistance test of the glass top plates of Examples 1 and 2 and Comparative Examples 1 to 3 when a metal plate made of SUS430 is used. [Figure 8] 1 is a graph showing the results of a disturbance strength test of the glass top plates of Examples 1 and 2 and Comparative Examples 1 to 3 when an aluminum metal plate is used. [Figure 9] 13A and 13B are diagrams showing a glass top plate of Example 3, in which FIG. 13A is a schematic cross-sectional view of the glass top plate, and FIG. 13B is a schematic cross-sectional view showing the state in which visible light and infrared light are multiple-reflected within the glass top plate. [Figure 10] 13A is a schematic cross-sectional view of the glass top plate of Example 4, and FIG. 13B is a schematic cross-sectional view showing the state in which visible light and infrared light are multiple-reflected within the glass top plate. [Figure 11] 1 is a graph showing the measurement results of the reflection spectrum of the glass top plates of Examples 3 to 4 and Comparative Example 4. [Figure 12] 13 is a graph showing the results of a disturbance strength test of the glass top plates of Examples 3 to 4 and Comparative Example 4 when an aluminum metal plate is used. [Figure 13] 13A and 13B are diagrams showing a glass top plate of Example 5, in which (a) is a schematic cross-sectional view of the glass top plate, and (b) is a schematic cross-sectional view showing the state in which visible light and infrared light are multiple-reflected within the glass top plate. [Figure 14] 1 is a graph showing the measurement results of the reflection spectrum of the glass top plates of Example 5 and Comparative Example 4. [Figure 15]13 is a graph showing the results of a disturbance strength test of the glass top plates of Example 5 and Comparative Example 4 when an aluminum metal plate is used. [Figure 16] FIG. 11 is a schematic cross-sectional view showing an induction heating cooker according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (Embodiment) 1. Overview of induction cooker 1 An embodiment in which a glass top plate 10 for a cooker of the present invention is applied to an induction heating cooker 1 will be described with reference to Fig. 1. As shown in Fig. 1, the induction heating cooker 1 includes a heating coil 2, a glass top plate 10, and an infrared sensor 3. The heating coil 2 heats a cooking utensil 4, such as a pot or frying pan, in which an object to be heated is placed and cooked.
[0013] The glass top plate 10 is placed on top of the heating coil 2. The cooking utensil 4 is placed on the glass top plate 10. The infrared sensor 3 is placed near the center position of the heating coil 2 in the radial direction and below the glass top plate 10, and detects infrared rays IR1 emitted from the cooking utensil 4. Specifically, it detects the infrared rays IR1 emitted from the cooking utensil 4 and transmitted through the glass top plate 10. The infrared sensor 3 outputs an output signal corresponding to the detected infrared rays to a control unit (not shown). The control unit calculates the temperature of the cooking utensil 4 based on the output signal obtained from the infrared sensor 3. However, a gas cooking utensil equipped with a gas burner (not shown) may be used as the cooking utensil.
[0014] 2. Configuration of the glass top plate 10 The glass top plate 10 has a front surface 10A and a back surface 10B. The front surface 10A is the surface on which a cooking utensil 4 such as a pot is placed and which is visible to the user, and the back surface 10B is the surface opposite the front surface 10A. The back surface 10B is the surface that faces the heating coil 2 and the infrared sensor 3 when the glass top plate 10 is placed on the induction heating cooker 1.
[0015] As shown in Fig. 1, the glass top plate 10 for a cooker in this embodiment includes a glass substrate 11, an infrared absorbing decorative layer 12, and a light-shielding layer 13. However, for the convenience of explanation, the thicknesses of the glass substrate 11, the infrared absorbing decorative layer 12, and the light-shielding layer 13 are exaggerated. Although not mentioned in detail, the thicknesses of the members constituting the glass top plate 10 may be exaggerated in other drawings as well.
[0016] The glass substrate 11 has a front surface 11A and a back surface 11B. An infrared absorbing decorative layer 12 is laminated on the back surface 11B of the glass substrate 11. A light-shielding layer 13 is laminated on the surface of the infrared absorbing decorative layer 12 opposite to the glass substrate 11. However, the glass substrate 11 may also have a configuration including an infrared absorbing layer 22 laminated on the back surface 11B, a decorative layer 32 laminated on the infrared absorbing layer 22, and a light-shielding layer 13 laminated on the decorative layer 32 (see FIG. 9). The glass substrate 11 may also have a configuration including an infrared absorbing layer 22 laminated on the front surface 11A, a decorative layer 32 laminated on the back surface 11B, and a light-shielding layer 13 laminated on the decorative layer 32 (see FIG. 13).
[0017] Although not shown in detail, a coating layer for protecting the glass substrate 11 may be formed on the surface 11A of the glass substrate 11. Also, when the infrared absorbing layer 22 is laminated on the surface 11A of the glass substrate 11, a coating layer may be formed on the surface of the infrared absorbing layer 22. However, the coating layer may not be formed in positions in the thickness direction of the glass substrate 11 that overlap the rear window portion 14 and the front window portion 15 described below.
[0018] The glass substrate 11 is preferably made of a transparent low-expansion glass ceramic. The transparent low-expansion glass ceramic is preferably one that is translucent and has a low expansion coefficient. For example, there is one in which β-quartz solid solution is precipitated in the main crystal phase. The volume crystallinity of the low-expansion glass ceramic in which β-quartz solid solution is precipitated is about 70%, and the size of the crystal is 0.1 μm or less. The β-quartz solid solution exhibits negative expansion characteristics, which cancel out the positive expansion characteristics of the remaining glass phase, resulting in a thermal expansion coefficient of almost zero. The refractive index (nD) is 1.541, the size of the precipitated crystal of the β-quartz solid solution is 0.1 μm or less, which is smaller than the wavelength of visible light, and the refractive index of the crystal phase and the remaining glass phase are almost the same, so there is no light scattering, it is transparent in appearance, and it transmits light from the visible light range to the infrared range well.
[0019] The thickness of the glass substrate 11 is preferably 0.5 mm to 8 mm, and more preferably 3 mm to 5 mm.
[0020] The infrared absorbing decorative layer 12 is formed by kneading a pigment, a silicone resin, a thickening resin, an organic solvent, and an infrared absorbing agent, applying the mixture to an object, and then baking the mixture. Since the infrared absorbing decorative layer 12 contains a pigment, it is colored and has opacity. The thickness of the infrared absorbing decorative layer 12 is preferably 0.1 μm to 20 μm, and more preferably 5 μm to 15 μm.
[0021] The decorative layer 32 is formed by kneading a pigment, a silicone resin, a thickening resin, and an organic solvent, applying the mixture to an object, and then baking the mixture. The decorative layer 32 is colored and opaque because it contains a pigment. The thickness of the decorative layer 32 is preferably 0.1 μm to 20 μm, and more preferably 5 μm to 15 μm.
[0022] The pigment contained in the infrared absorbing decorative layer 12 or the decorative layer 32 is not particularly limited, and a white pigment, a silver pigment, or a gold pigment can be suitably used. In this case, the glass top plate 10 for a cooker can show a high-class design of white, silver, or gold. However, the pigment may be a dark color such as a black pigment or a gray pigment.
[0023] In addition, a pearlescent pigment can be suitably used as the pigment. In this case, the glass top plate 10 for cooking utensils shows a lustrous pearlescent color tone, and can exhibit a more excellent design. As the pearlescent pigment, for example, an inorganic pigment coated with at least one selected from titanium oxide, zirconium oxide, and iron oxide can be used. That is, as the pearlescent pigment, for example, a pigment composed of an inorganic pigment and a pearlescent coating coating the inorganic pigment can be used. Examples of the inorganic pigment to be coated include kaolin, talc, sericite, pyroferrite, natural mica, synthetic mica, and aluminum oxide. As the pearlescent pigment, a commercially available product can be used.
[0024] Silicone resin refers to a polymer of an organic silicon compound with a siloxane bond as the main skeleton. As the silicone resin, for example, commercially available products such as Straight Silicone Varnish KR282 (manufactured by Shin-Etsu Chemical Co., Ltd.), Straight Silicone Varnish KR271 (manufactured by Shin-Etsu Chemical Co., Ltd.), Straight Silicone Varnish KR311 (manufactured by Shin-Etsu Chemical Co., Ltd.), Modified Silicone Varnish KR211 (manufactured by Shin-Etsu Chemical Co., Ltd.), Silicone Alkyd Varnish (manufactured by Shin-Etsu Chemical Co., Ltd.), Silicone Epoxy Varnish ES100N (manufactured by Shin-Etsu Chemical Co., Ltd.), etc. can be used.
[0025] The thickening resin is more easily combusted than the silica-forming material, and a resin compatible with the silica-forming material can be suitably used. The thickening resin makes it possible to adjust the viscosity of the paint for forming the infrared absorbing decorative layer 12, making it easier to apply the paint to the glass substrate 11 during baking.
[0026] The paint can further contain an organic solvent. As the organic solvent, a solvent in which the silica-forming material can be dissolved can be used. The amount of the organic binder and the organic solvent added can be appropriately adjusted in consideration of the viscosity of the paint. The organic components contained in the paint, such as the organic binder and the organic solvent, can be eliminated when the paint is baked.
[0027] The paint may contain an infrared absorbing agent, which may be one or more of metal hexaborides such as calcium hexaboride, strontium hexaboride, barium hexaboride, lanthanum hexaboride, etc., with lanthanum hexaboride being preferred.
[0028] As the infrared absorbing agent, one or more tungstates such as calcium tungstate, sodium tungstate, magnesium tungstate, lithium tungstate, and cesium tungstate can be used, with cesium tungstate being preferred.
[0029] As the infrared absorbing agent, one or more of a cyanine compound, a phthalocyanine compound, a naphthalocyanine compound, a dithiolate metal complex, a squarium compound, a quinone compound, and a diimmonium compound can be used.
[0030] The lightness L measured from the front side of the glass top plate 10 on which the infrared absorbing decorative layer 12 or the decorative layer 32 is formed. * is preferably 50 or more, and more preferably 55 or more. * is the lightness L measured in accordance with the Japanese Industrial Standards (formerly the Japanese Industrial Standards; hereafter referred to as JIS) Z8781-4:2013. * It is.
[0031] The light-shielding layer 13 can be made of a black film that does not transmit light. The light-shielding layer 13 can be made of various black heat-resistant films, and may be a laminate of two or more layers. The thickness of the light-shielding layer 13 is preferably 1 μm to 20 μm, and more preferably 5 μm to 15 μm.
[0032] As the light-shielding layer 13, for example, a black metallic gloss film can be formed. The metallic gloss film can be composed of a precious metal and / or a metal oxide. Examples of the precious metal and the metal components of the metal oxide include Au, Pt, Pd, Rh, Ru, Bi, Sn, Ni, Fe, Cr, Ti, Ca, Si, Ba, Sr, Mg, Ag, Zr, In, and Mn. The metallic gloss film can be composed of any of these precious metals, metals, and metal oxides, or a combination of these. When forming a metallic gloss film, the thickness is preferably 2 μm or less to prevent an increase in cost. In addition, if light-shielding properties can be obtained, it is preferable to make the thickness of the metallic gloss film as small as possible.
[0033] The metallic gloss film can be formed by baking a diluted solution of an organometallic compound of the above-mentioned metals, such as Au, Pt, Pd, Rh, Ru, Bi, Sn, Ni, Fe, Cr, Ti, Ca, Si, Ba, Sr, Mg, Ag, Zr, In, and Mn. The diluted solution of these organometallic compounds may be used alone or in any ratio. The baking temperature of the diluted solution of the organometallic compound may be, for example, 600 to 900°C.
[0034] In addition, from the viewpoints of being able to be produced at low cost and having excellent heat resistance and light shielding properties, the light shielding layer 13 is preferably made of a silica film or a heat-resistant resin film in which a black inorganic pigment is dispersed. When forming a silica film in which a black inorganic pigment is dispersed, a paint for the light shielding layer 13 containing the above-mentioned silica forming material and the black inorganic pigment can be baked. As the silica forming material, silicone resin and / or silica sol can be used, as in the above-mentioned decorative layer 32. In addition, as the black inorganic pigment, for example, Cr-Fe oxide, Cu-Cr-Mn oxide, Co-Mn-Cr-Fe oxide, Co-Ni-Cr-Fe oxide, Co-Ni-Cr-Fe-Mn oxide, etc. can be used. Specifically, as the black inorganic pigment, a commercially available product can be used, and the blending ratio thereof can be appropriately adjusted according to the light shielding properties of the light shielding layer 13. In addition, since these black inorganic pigments are generally made of particles having a spherical or nearly spherical shape, the light shielding layer 13 containing the black inorganic pigment may have low adhesion to the decorative layer 32. Therefore, an additive consisting of scaly particles such as mica can be added to the light-shielding layer 13 together with the black pigment. As such an additive, in addition to minerals such as mica, the above-mentioned pearl pigment can also be used. In addition, organic solvents, organic binders, etc. can be added to the paint for the light-shielding layer 13.
[0035] When forming a heat-resistant resin film with a black inorganic pigment dispersed therein as the light-shielding layer 13, a light-shielding coating material containing at least a heat-resistant resin raw material that hardens by heating during baking to produce a heat-resistant resin and a black inorganic pigment can be baked. As the heat-resistant resin, a silicone resin, a polyimide resin, a polyamide resin, a fluororesin, or a composite of these can be used. As the black inorganic pigment, the above-mentioned pigments can be used, and the blending ratio can be appropriately adjusted depending on the light-shielding properties of the light-shielding layer 13.
[0036] As shown in FIG. 1, when the glass top plate 10 is placed on the upper part of the induction cooking appliance 1, the rear surface 10B of the glass top plate 10 is provided with a rear window 14 that exposes the rear surface 11B of the glass substrate 11 at a position overlapping with the infrared sensor 3 in the thickness direction of the glass substrate 11 without applying the infrared absorbing decorative layer 12 and the light blocking layer 13. The infrared sensor 3 faces the rear surface 11B of the glass substrate 11 through the rear window 14. The infrared ray IR1 emitted from the cooking appliance 4 is transmitted through the glass substrate 11 and detected by the infrared sensor 3. The inner shape of the rear window 14 may be a polygonal shape such as a triangular shape or a rectangular shape, or may be a circular shape or an oval shape, and any shape can be appropriately selected. In this embodiment, the inner shape of the rear window 14 is formed into a circular shape. The inner diameter dimension of the rear window 14 is preferably 1 mm to 30 mm, more preferably 5 mm to 20 mm. In this embodiment, the inner diameter of the rear window portion 14 is set to 10 mm.
[0037] 1, when the infrared absorbing decorative layer 12 and the light-shielding layer 13 are formed on the rear surface 10B of the glass top plate 10, the rear window portion 14 is composed of an infrared absorbing decorative layer window portion 14A formed in the infrared absorbing decorative layer 12 and a light-shielding layer window portion 14B formed in the light-shielding layer 13. In this case, the rear window portion 14 is formed by forming the infrared absorbing decorative layer 12 and the light-shielding layer 13 on the rear surface 11B of the glass substrate 11, except for the portion corresponding to the rear window portion 14.
[0038] The infrared absorbing decorative layer window portion 14A and the light-shielding layer window portion 14B are formed in a position of the infrared absorbing decorative layer 12 that overlaps with the infrared sensor 3 in the thickness direction of the glass substrate 11 when the glass top plate 10 is placed on the induction heating cooker 1.
[0039] 9(a) and 9(b), when the infrared absorbing layer 22, the decorative layer 32, and the light-shielding layer 13 are formed on the rear surface 10B of the glass top plate 10, the rear window portion 14 is composed of the infrared absorbing layer window portion 14C formed in the infrared absorbing layer 22, the decorative layer window portion 14D formed in the decorative layer 32, and the light-shielding layer window portion 14B formed in the light-shielding layer 13. In this case, the rear window portion 14 is formed by forming the infrared absorbing layer 22, the decorative layer 32, and the light-shielding layer 13 on the rear surface 11B of the glass substrate 11, except for the portion corresponding to the rear window portion 14.
[0040] The infrared absorbing layer window portion 14C, the decorative layer window portion 14D and the light-shielding layer window portion 14B are formed in a position of the infrared absorbing decorative layer 12 that overlaps with the infrared sensor 3 in the thickness direction of the glass substrate 11 when the glass top plate 10 is placed on the induction heating cooker 1.
[0041] The thickness of the infrared absorbing layer 22 formed on the rear surface 11B of the glass substrate 11 is preferably 0.1 μm to 20 μm, and more preferably 5 μm to 15 μm.
[0042] As shown in FIG. 13(a) and FIG. 13(b), when the infrared absorbing layer 22 is formed on the surface 10A of the glass top plate 10, the infrared absorbing layer 22 formed on the surface 10A of the glass top plate 10 has a front window 15 where the surface 11A of the glass substrate 11 is exposed. The front window 15 is composed of an infrared absorbing layer window 15A formed on the infrared absorbing layer 22. In this case, the front window 15 (infrared absorbing layer window 15A) is formed by forming the infrared absorbing layer 22 on the surface 11A of the glass substrate 11 except for a portion corresponding to the front window 15. The front window 15 and the back window 14 are formed at a position where they overlap in the thickness direction of the glass substrate 11. The inner diameter dimension of the front window 15 and the inner diameter dimension of the back window 14 are formed to be approximately the same. "Approximately the same" includes the case where they are the same, and also includes the case where they can be recognized as substantially the same even if they are not the same.
[0043] The thickness of the infrared absorbing layer 22 formed on the surface 11A of the glass substrate 11 is preferably 0.1 μm to 20 μm, and more preferably 5 μm to 15 μm.
[0044] The glass top plate 10 of this embodiment preferably has a reflectance of less than 25%, more preferably less than 20%, of infrared rays having a wavelength of 940 nm measured from the surface 11A side of the glass substrate 11. Since infrared rays having a wavelength of 940 nm are within the range of wavelengths used in the invention described in JP-A-2007-115420 and are close to the wavelengths used in the reflective photointerrupter described in JP-A-2022-32748, the infrared reflectance of the glass top plate 10 can be suitably used for measuring the reflectance of the infrared rays.
[0045] 3. Issues with conventional technology Problems of the conventional technology will be described with reference to Fig. 2. As shown in Fig. 2, an induction heating cooker 51 according to the conventional technology includes a heating coil 2, a glass top plate 50, and an infrared sensor 3. The glass top plate 50 for a cooker of the conventional technology includes a glass substrate 11, a decorative layer 32 laminated on the back surface 11B side of the glass substrate 11, and a light-shielding layer 13 laminated on the decorative layer 32. The glass top plate 50 of the conventional technology differs from this embodiment in that it does not have the infrared absorbing decorative layer 12. The same components as those of this embodiment are denoted by the same reference numerals, and duplicated explanations will be omitted.
[0046] As shown in FIG. 2, infrared rays IR2 emitted from the lighting fixture 5 outside the induction cooking device 51 are incident on the front surface 10A of the glass top plate 10. The infrared rays IR2 incident on the glass top plate 10 are reflected by the decorative layer 32 on the rear surface 11B of the glass substrate 11. The reflected infrared rays IR2 are further reflected on the front surface 11A of the glass substrate 11. In this way, the infrared rays IR2 incident on the glass top plate 10 are multiple-reflected between the front surface 11A and the rear surface 11B of the glass substrate 11 and reach the rear window portion 14. The infrared rays IR2 that reach the rear window portion 14 are detected by the infrared sensor 3. Then, the infrared sensor 3 detects the infrared rays IR1 emitted from the heated cooking device 4 and transmitted through the glass substrate 11, and the infrared rays IR2 emitted from the external lighting fixture 5 and then multiple-reflected within the glass substrate 11. As a result, there is a risk that the temperature of the cooking device 4 cannot be measured accurately.
[0047] 4. Effects of this Form As shown in FIG. 1, the glass top plate 10 of this embodiment has an infrared absorbing decorative layer 12 on the back surface 11B of the glass substrate 11. The infrared ray IR2 incident from the front surface 10A of the glass top plate 10 is reflected multiple times inside the glass top plate 10. At this time, a part of the infrared ray IR2 is absorbed by the infrared absorbing decorative layer 12 at the back surface 11B of the glass substrate 11, and the other part is reflected. As a result, the intensity of the infrared ray IR2 incident on the glass top plate 10 is reduced. When the infrared ray IR2 reaches the infrared absorbing decorative layer 12 in the process of repeating multiple reflections inside the glass top plate 10, a part of the infrared ray IR2 is absorbed by the infrared absorbing decorative layer 12. In this way, each time the infrared ray IR2 repeats multiple reflections inside the glass substrate 11, the infrared ray IR2 is absorbed by the infrared absorbing decorative layer 12, and the intensity of the infrared ray IR2 is reduced. As a result, the infrared ray IR2 incident on the front surface 10A of the glass top plate 10 from the outside is prevented from reaching the infrared sensor 3. This reduces the influence of external lighting fixtures 5, making it easier to detect infrared rays IR1 emitted from cooking utensils 4, and improving the accuracy of temperature measurement of cooking utensils 4.
[0048] The configuration in which the glass substrate 11 has an infrared absorbing layer 22 laminated on the back side, a decorative layer 32 laminated on the infrared absorbing layer 22, and a light-shielding layer 13 laminated on the decorative layer 32, and the configuration in which the glass substrate 11 has an infrared absorbing layer 22 laminated on the front side, a decorative layer 32 laminated on the back side, and a light-shielding layer 13 laminated on the decorative layer 32, will be described in detail later.
[0049] 5. Examples and Comparative Examples 5-1. Configuration in which infrared absorbing decorative layer 12 is provided on rear surface 11B of glass substrate 11 Example 1 A glass top plate 10 of Example 1 will be described with reference to Fig. 3(a). The glass top plate 10 of Example 1 includes a glass substrate 11, an infrared absorbing decorative layer 12 formed on the rear surface 11B of the glass substrate 11, and a light-shielding layer 13 formed on the surface of the infrared absorbing decorative layer 12 opposite to the glass substrate 11. For ease of explanation, the heating coil 2, cooking utensils 4, and lighting fixtures 5 are omitted in Fig. 3(a). In the following figures, the heating coil 2, cooking utensils 4, and lighting fixtures 5 may be omitted.
[0050] A paste-like paint 1 was prepared by kneading 40 parts by mass of pearl pigment, 30 parts by mass of silicone resin, 10 parts by mass of thickening resin, 10 parts by mass of organic solvent, and 10 parts by mass of lanthanum hexaboride. The silicone resin contained 50% by mass of organic solvent. The lanthanum hexaboride was a lanthanum hexaboride dispersion (containing approximately 4% by mass of lanthanum hexaboride) manufactured by Sumitomo Metal Mining Co., Ltd. The composition of the paint 1 is shown in Table 1.
[0051] A paste-like paint 1 was applied to the entire back surface 11B of a 4 mm-thick glass substrate 11 made of translucent low-expansion glass ceramics (N-0) by screen printing using a 300-mesh screen, excluding the back window portion 14. The paint was then heated and cured at a temperature of 300°C to form an infrared absorbing decorative layer 12. The thickness of the infrared absorbing decorative layer 12 was measured with a film thickness meter to be 7 μm. The content of lanthanum hexaboride per unit area in the infrared absorbing decorative layer 12 was 0.08 g / m 2 It was.
[0052] Next, 40 parts by mass of commercially available black inorganic pigment, 50 parts by mass of silicone resin raw material, and 10 parts by mass of organic solvent were kneaded to prepare a paste-like light-shielding paint. The light-shielding paint was applied to the entire surface of the infrared absorbing decorative layer 12 formed on the back surface 11B of the glass substrate 11, except for the back window portion 14, by screen printing. Then, the light-shielding paint was laminated on the infrared absorbing decorative layer 12 by heating and curing at a temperature of 300°C to form a light-shielding layer 13. The thickness of the light-shielding layer 13 was measured with a film thickness meter and was 10 μm. The inner diameter dimension of the back window portion 14 of Example 1 was 10 mm. In this way, the glass top plate 10 of Example 1 was produced.
[0053] Example 2 Paint paint 2 was prepared in the same manner as in Example 1, except that 10 parts by mass of cesium tungstate dispersion (containing approximately 25% by mass of cesium tungstate) was used instead of 10 parts by mass of lanthanum hexaboride dispersion in Example 1. Also, a glass top plate 10 of Example 2 was produced in the same manner as in Example 1, except that paint paint 2 was used. The blending composition of paint paint 2 is shown in Table 1. The content of cesium tungstate per unit area in the infrared absorbing decorative layer 12 of Example 2 was 0.7 g / m 2 It was.
[0054] [Table 1]
[0055] Comparative Example 1 As Comparative Example 1, a glass top plate 10, KZ-YP76S, manufactured by Panasonic Corporation, was used. The glass top plate 10 of Comparative Example 1 includes a glass substrate 11, a decorative layer 32 laminated on the rear surface 11B of the glass substrate 11, and a light-shielding layer 13 laminated on the surface of the decorative layer 32 opposite to the glass substrate 11. A rear window portion 14 is formed on the rear surface 11B of the glass substrate 11. The composition of the pigment forming the decorative layer 32 and the composition of the pigment forming the light-shielding layer 13 are unknown.
[0056] Comparative Example 2 As Comparative Example 2, a glass top plate 10, KZ-K32EST, manufactured by Panasonic Corporation, was used. The glass top plate 10 of Comparative Example 2 includes a glass substrate 11, a decorative layer 32 laminated on the rear surface 11B of the glass substrate 11, and a light-shielding layer 13 laminated on the surface of the decorative layer 32 opposite to the glass substrate 11. A rear window portion 14 is formed on the rear surface 11B of the glass substrate 11. The composition of the pigment forming the decorative layer 32 and the composition of the pigment forming the light-shielding layer 13 are unknown.
[0057] Comparative Example 3 As Comparative Example 3, a glass top plate 10, KZ-YP77K, manufactured by Panasonic Corporation, was used. The glass top plate 10 of Comparative Example 3 includes a glass substrate 11, a decorative layer 32 laminated on the rear surface 11B of the glass substrate 11, and a light-shielding layer 13 laminated on the surface of the decorative layer 32 opposite to the glass substrate 11. A rear window portion 14 is formed on the rear surface 11B of the glass substrate 11. The composition of the pigment forming the decorative layer 32 and the composition of the pigment forming the light-shielding layer 13 are unknown.
[0058] (Brightness measurement) The glass top plates 10 of Examples 1 and 2 and Comparative Examples 1 to 3 were measured using an integrating sphere spectrophotometer (SP-60 manufactured by X-rite) to measure the L *The values were measured. The integrating sphere corresponds to the geometric condition c of JIS Z8722. The measurement conditions were illuminant D65 (JIS Z8781-2), 10° field of view (CIE1964 standard observer of JIS Z87891-1), and regular reflection included (including the specular reflection component described in JIS8722). The measurement results are summarized in Table 2.
[0059] (Infrared reflectance spectroscopy measurement) The infrared IR reflection spectrum of the glass top plates 10 of Examples 1 and 2 and Comparative Examples 1 to 3 was measured at wavelengths of 340 nm to 2500 nm using a spectrometer manufactured by JASCO Corporation. An integrating sphere unit was used as the measurement condition. The measurement results are shown in FIG. 5 and summarized in Table 2.
[0060] (Disturbance strength test) When infrared rays IR2 incident on the glass top plate 10 from the external lighting fixture 5 are multiple-reflected, the intensity of the infrared rays IR2 detected by the infrared sensor 3 was measured as follows. That is, when the infrared rays IR2 from the external lighting fixture 5 are treated as disturbances, the disturbance intensity was measured.
[0061] An infrared sensor 3 is disposed below the rear window 14 of the glass top plate 10 at a position overlapping the glass top plate 10 in the thickness direction. An InGaAs photodiode sensor module is used as the infrared sensor 3. The infrared sensor 3 converts the amount of infrared light IR2 that enters the rear window 14 into a voltage value.
[0062] As shown in FIG. 4, a rectangular metal plate 6 is placed on the top surface of a glass top plate 10. Either an aluminum metal plate 6 or a SUS430 metal plate 6 is used as the metal plate 6. The aluminum metal plate 6 is a model of a cookware 4 such as an aluminum pot, and the SUS430 metal plate 6 is a model of a cookware 4 such as a stainless steel pot. The metal plate 6 is placed in a position overlapping the rear window portion 14 of the glass top plate 10 in the thickness direction of the glass top plate 10. A light source that emits infrared rays with a wavelength of 940 nm is placed on the edge of the metal plate 6. The light source is a floodlight kit (modified) manufactured by Akizuki Electronics Co., Ltd., and consumes 2 W of power. This light source is a model of a lighting fixture 5 that corresponds to external disturbance.
[0063] The distance X from the axis P of the infrared sensor 3 to the edge of the metal plate 6 was changed by moving the metal plate 6 relative to the light source, and the voltage detected by the infrared sensor 3 was measured for each distance X. The detected voltage results are shown in Figures 7 and 8. Table 2 summarizes the detected voltage when the distance X from the axis P of the infrared sensor 3 is 5 cm.
[0064] 6 shows the reflection spectra of the aluminum metal plate 6 and the SUS430 metal plate 6 used in the experiment. The measurement conditions were the same as those for the glass top plate 10, so a detailed description will be omitted.
[0065] [Table 2]
[0066] (Measurement results) As shown in Table 2, the lightness L of the glass top plate 10 of Example 1 * The lightness L of the glass top plate 10 of Example 2 is 60.4. * The value was 60.3. In this way, the glass top plate 10 of Example 1 and Example 2 can be decorated with bright colors such as white, and the degree of freedom in decoration is high.
[0067] Lightness L of the glass top plate 10 of Comparative Example 1 * The lightness L of the glass top plate 10 of Comparative Example 2 was 69.3. * The lightness L of the glass top plate 10 of Comparative Example 1 and Comparative Example 2 was 62.6. The glass top plate 10 of Comparative Example 3 was also capable of being decorated with a bright white color tone. * The value was 28.3. For this reason, for the glass top plate 10 of Comparative Example 3, decoration with bright white tones was impossible, and decoration with dark tones was limited, so that decorativeness was restricted.
[0068] 5 shows the reflection spectrum of the glass top plate 10 of Examples 1 and 2 and Comparative Examples 1 to 3. As shown in Table 2, the reflectance of infrared IR2 at a wavelength of 940 nm was 18.2% for Example 1 and 18.8% for Example 2. In contrast, the reflectance of Comparative Example 1 was 31.1%, and the reflectance of Comparative Example 2 was 27.2%, which were high reflectances. This is because the lightness L of Comparative Examples 1 and 2 was 18.2%. * This is believed to be due to the fact that Comparative Examples 1 and 2 do not contain an infrared absorbing agent, and that the reflectance of Comparative Example 3 was as low as 7.9%. This is because the glass top plate 10 of Comparative Example 3 has a low lightness L * This is thought to be due to the absorption of infrared IR2, as the value is low at 28.3.
[0069] 7 shows a graph of the output voltage of the infrared sensor 3 versus the distance X from the axis P of the infrared sensor 3 to the edge of the metal plate 6 made of SUS430 in a disturbance strength test. The smaller the output voltage of the infrared sensor 3 shown on the vertical axis, the smaller the influence of the external lighting fixture 5, which is preferable.
[0070] The output voltages of Examples 1 and 2 are smaller than those of Comparative Examples 1 and 2 when the distance X from the axis P of the infrared sensor 3 is 3 cm to 7 cm. In other words, the glass top plates 10 of Examples 1 and 2 are less susceptible to the influence of the external lighting fixtures 5 than those of Comparative Examples 1 and 2. This makes it possible to improve the accuracy of the infrared sensor 3.
[0071] The output voltages of Examples 1 and 2 are smaller than that of Comparative Example 3 when the distance X from the axis P of the infrared sensor 3 is 3 cm to 4 cm. That is, Examples 1 and 2 are less susceptible to the influence of the external lighting fixture 5 than Comparative Example 3 when the distance X from the axis P of the infrared sensor 3 is 3 cm to 4 cm.
[0072] The output voltages of Examples 1 and 2 are the same as those of Comparative Example 3 when the distance X from the axis P of the infrared sensor 3 is 5 cm to 7 cm. In other words, when the distance X from the axis P of the infrared sensor 3 is 5 cm to 7 cm, the influence of the external lighting fixture 5 is about the same in Examples 1 and 2 as in Comparative Example 3. However, as described above, the brightness L of Example 1 * is 60.4, and the lightness L * The lightness L of Comparative Example 3 is 60.3. * Since the degree of freedom in decoration in Comparative Example 3 is 28.3, it is lower than that in Examples 1 and 2.
[0073] Fig. 8 shows a graph of the output voltage of the infrared sensor 3 versus the distance X from the axis P of the infrared sensor 3 to the edge of the aluminum metal plate 6 in a disturbance strength test. As shown in Fig. 6, the reflectance of infrared rays IR with a wavelength of 940 nm is higher for the aluminum metal plate 6 than for the SUS430 metal plate 6.
[0074] Returning to Fig. 8, the output voltages of Examples 1 and 2 are smaller than those of Comparative Examples 1 and 2 when the distance X from the axis P of the infrared sensor 3 is 3 cm to 7 cm. In other words, Examples 1 and 2 are less susceptible to the influence of the external lighting fixture 5 than Comparative Examples 1 and 2. This makes it possible to improve the accuracy of the infrared sensor 3.
[0075] The output voltages of Examples 1 and 2 are smaller than that of Comparative Example 3 when the distance X from the axis P of the infrared sensor 3 is 3 cm to 6 cm. That is, Examples 1 and 2 are less susceptible to the influence of the external lighting fixture 5 than Comparative Example 3 when the distance X from the axis P of the infrared sensor 3 is 3 cm to 6 cm.
[0076] The output voltage of Example 1 is the same as that of Comparative Example 3 when the distance X from the axis P of the infrared sensor 3 is 7 cm. In other words, when the distance X from the axis P of the infrared sensor 3 is 7 cm, the influence of the external lighting fixture 5 in Example 1 is about the same as that in Comparative Example 3. However, as described above, the brightness L * The lightness L of Comparative Example 3 is 60.4. * Since the value is 28.3, the degree of freedom in decoration in Comparative Example 3 is inferior to that in Example 1.
[0077] Moreover, the output voltage of Example 2 is smaller than that of Comparative Example 3 even when the distance X from the axis P of the infrared sensor 3 is 7 cm. In other words, the influence of the external lighting device 5 in Example 2 is smaller than that in Comparative Example 3 even when the distance X from the axis P of the infrared sensor 3 is 7 cm.
[0078] The effects of Examples 1 and 2 will be considered with reference to Fig. 3(b). When visible light V is irradiated onto the glass top plate 10 and passes through the glass substrate 11 to reach the infrared absorbing decorative layer 12, part of the visible light V is reflected by the infrared absorbing decorative layer 12, while the remaining majority enters the infrared absorbing decorative layer 12. The visible light V is reflected by the pigment contained in the infrared absorbing decorative layer 12, enters the glass substrate 11, and is transmitted through the glass substrate 11. As a result, in the glass top plate 10 of Examples 1 and 2, the lightness L * is relatively large, which contributes to the decorativeness of the glass top plate 10.
[0079] On the other hand, when infrared rays IR2 are irradiated to the glass top plate 10 and pass through the glass substrate 11 to reach the infrared absorbing decorative layer 12, a part of the infrared rays IR2 is reflected by the infrared absorbing decorative layer 12, and the remaining majority enters the infrared absorbing decorative layer 12. The infrared rays IR2 are absorbed by the infrared absorbing agent contained in the infrared absorbing decorative layer 12 and attenuated. A part of the infrared rays IR2 that enter the infrared absorbing decorative layer 12 is reflected by the pigment. The infrared rays IR2 reflected by the pigment are further absorbed by the infrared absorbing agent and attenuated as they travel through the infrared absorbing decorative layer 12. The infrared rays IR2 that reach the glass substrate 11 are weak. Furthermore, when the infrared rays IR2 are multiple-reflected within the glass top plate 10, the infrared rays IR2 are attenuated when they reach the infrared absorbing decorative layer 12. This allows the intensity of the infrared rays IR2 that reach the infrared sensor 3 to be sufficiently reduced. In this way, in the glass top plate 10 of Example 1 and Example 2, the infrared rays IR2 irradiated to the glass top plate 10 can be attenuated.
[0080] 5-2. Configuration in which infrared absorbing layer 22 is provided on rear surface 11B of glass substrate 11 Example 3 9(a), a glass top plate 10 of Example 3 will be described. The glass top plate 10 of this example includes a glass substrate 11, an infrared absorbing layer 22 formed on the rear surface 11B of the glass substrate 11, a decorative layer 32 laminated on the infrared absorbing layer 22, and a light-shielding layer 13 laminated on the decorative layer 32.
[0081] A translucent paint having translucency and in a paste form was prepared by kneading 100 parts by mass of a vehicle (GLS-001, manufactured by Teikoku Ink Mfg. Co., Ltd.), 5 parts by mass of an organic solvent (Z-705, manufactured by Teikoku Ink Mfg. Co., Ltd.), 0.5 parts by mass of a curing agent (GLS reinforcing agent, manufactured by Teikoku Ink Mfg. Co., Ltd.), and 10 parts by mass of cesium tungstate (cesium tungstate dispersion (approximately 25% by mass as cesium tungstate), manufactured by Sumitomo Metal Mining Co., Ltd.). The composition of the translucent paint is shown in Table 3.
[0082] A paste-like translucent paint was applied to the entire back surface 11B of a 4 mm-thick glass substrate 11 made of translucent low-expansion glass ceramics (N-0) by screen printing using a 400-mesh screen, except for the back window portion 14. The paint was then heated and cured at a temperature of 160°C to form an infrared absorbing layer 22. The thickness of the infrared absorbing layer 22 was measured with a film thickness meter to be 4 μm. The content of cesium tungstate per unit area in the infrared absorbing layer 22 was 0.5 g / m 2 It was.
[0083] Next, 98.3 parts by mass of white ink for glass containing a white pigment (Teikoku Ink Mfg. Co., Ltd., GLS-619), 1.7 parts by mass of black ink for glass containing a black pigment (Teikoku Ink Mfg. Co., Ltd., GLS-919), 5 parts by mass of organic solvent (Teikoku Ink Mfg. Co., Ltd., Z-705), and 0.5 parts by mass of hardener (Teikoku Ink Mfg. Co., Ltd., GLS reinforcer) were kneaded together to prepare a paste-like paint 3. The composition of paint 3 is shown in Table 3.
[0084] A paste-like paint 3 was applied to the entire surface of the infrared absorbing layer 22 formed on the rear surface 11B of the glass substrate 11, except for the rear window portion 14, by screen printing using a 300 mesh screen. The paint was then heated and cured at a temperature of 160°C to form a decorative layer 32. The thickness of the decorative layer 32 was measured with a thickness gauge and found to be 7 μm.
[0085] Next, 100 parts by mass of black ink for glass containing a black pigment (Teikoku Ink Mfg. Co., Ltd., GLS-919), 5 parts by mass of an organic solvent (Teikoku Ink Mfg. Co., Ltd., Z-705), and 0.5 parts by mass of a curing agent (Teikoku Ink Mfg. Co., Ltd., GLS reinforcement agent) were kneaded to prepare a paste-like light-shielding paint 2. The light-shielding paint 2 was applied to the entire surface of the decorative layer 32 formed on the rear surface 11B of the glass substrate 11, except for the rear window portion 14, by screen printing using a 300-mesh screen. Thereafter, the light-shielding paint 2 was laminated on the decorative layer 32 by heating at a temperature of 160°C and curing, thereby forming the light-shielding layer 13. The thicknesses of the infrared absorbing layer 22, the decorative layer 32, and the light-shielding layer 13 were measured with a film thickness meter and found to be 18 μm. The inner diameter dimension of the rear window portion 14 of Example 3 was 10 mm. In this manner, the glass top plate 10 of Example 3 was produced.
[0086] Example 4 10(a), a glass top plate 10 of Example 4 will be described. The glass top plate 10 of this example includes a glass substrate 11, an infrared absorbing layer 22 formed on the rear surface 11B of the glass substrate 11, an infrared absorbing decorative layer 12 laminated on the infrared absorbing layer 22, and a light blocking layer 13 laminated on the infrared absorbing decorative layer 12.
[0087] For the glass top plate 10 of Example 4, first, an infrared absorbing layer 22 was formed on the rear surface 11B of the glass substrate 11 in the same manner as in Example 3.
[0088] 98.3 parts by mass of white ink for glass containing a white pigment (Teikoku Ink Mfg. Co., Ltd., GLS-619), 1.7 parts by mass of black ink for glass containing a black pigment (Teikoku Ink Mfg. Co., Ltd., GLS-919), 5 parts by mass of organic solvent (Teikoku Ink Mfg. Co., Ltd., Z-705), 0.5 parts by mass of hardener (Teikoku Ink Mfg. Co., Ltd., GLS reinforcing agent), and 10 parts by mass of cesium tungstate (cesium tungstate dispersion (approximately 25% by mass as cesium tungstate) manufactured by Sumitomo Metal Mining Co., Ltd.) were kneaded together to prepare a paste-like paint 4. The formulation of paint 4 is shown in Table 3.
[0089] A paste-like paint 4 was applied to the entire surface of the infrared absorbing layer 22 formed on the rear surface 11B of the glass substrate 11, excluding the rear window portion 14, by screen printing using a 300 mesh screen. The infrared absorbing decorative layer 12 was then formed by heating and curing at a temperature of 160°C. The thickness of the infrared absorbing decorative layer 12 was measured with a thickness gauge and found to be 7 μm.
[0090] Thereafter, a light-shielding layer 13 was formed in the same manner as in the third embodiment, thereby producing a glass top plate 10 of the fourth embodiment.
[0091] [Table 3]
[0092] Comparative Example 4 As Comparative Example 4, a glass top plate 10, KZ-L32AST, manufactured by Panasonic Corporation, was used. The glass top plate 10 of Comparative Example 4 includes a glass substrate 11, a decorative layer 32 laminated on the rear surface 11B of the glass substrate 11, and a light-shielding layer 13 laminated on the surface of the decorative layer 32 opposite to the glass substrate 11. A rear window portion 14 is formed on the rear surface 11B of the glass substrate 11. The composition of the pigment forming the decorative layer 32 and the composition of the pigment forming the light-shielding layer 13 are unknown.
[0093] (Various measurements) For Example 3, Example 4, and Comparative Example 4, brightness measurement, infrared reflection spectrum measurement, and disturbance strength test were performed in the same manner as in Examples 1 and 2 and Comparative Examples 1 to 3. However, in the disturbance strength test, only the metal plate 6 made of aluminum was used, and no test was performed using the metal plate 6 made of SUS430. The results are summarized in Table 4 and Figs. 11 and 12. Table 4 lists the detection voltage of the infrared sensor 3 when the distance X from the axis P of the infrared sensor 3 to the edge of the metal plate 6 is 5 cm.
[0094] [Table 4]
[0095] (Measurement results) As shown in Table 4, the lightness L of the glass top plate 10 of Example 3 * The lightness L of the glass top plate 10 of Example 4 is 55.1. * The value was 54.2. In this way, the glass top plate 10 of Example 1 and Example 2 can be decorated with bright colors such as white, and has a high degree of freedom in terms of decoration.
[0096] Lightness L of Comparative Example 4 * The value was 62.6. The glass top plate 10 of Comparative Example 4 also allows decoration in bright white tones.
[0097] 11 shows the reflection spectrum of the glass top plate 10 of Examples 3 and 4 and Comparative Example 4. As shown in Table 4, the reflectance of infrared rays with a wavelength of 940 nm was 13.0% for Example 3 and 10.5% for Example 4. This is thought to be because Example 3 has an infrared absorbing decorative layer 12 in addition to the infrared absorbing layer 22, and therefore has excellent infrared absorbing ability.
[0098] In contrast, the reflectance of Comparative Example 4 was 26.3%, which was a high reflectance. * This is believed to be due to the fact that Comparative Example 4 does not contain an infrared absorbing agent and that
[0099] 12, the output voltages of Examples 3 and 4 are smaller than that of Comparative Example 4 when the distance X from the axis P of the infrared sensor 3 is 3 cm to 7 cm. In other words, Examples 3 and 4 are less susceptible to the influence of the external lighting fixture 5 than Comparative Example 4. This makes it possible to improve the accuracy of the infrared sensor 3.
[0100] In Examples 3 and 4, the lightness L *When the reflectance of infrared light IR with a wavelength of 940 nm is 50 or more, the reflectance of infrared light IR is less than half that of Comparative Example 4. As shown in Table 4, even in the disturbance strength test, the detected voltage when the distance X from the axis P of the infrared sensor 3 is 5 cm, the detected voltage of Example 3 (2 mV) and the detected voltage of Example 4 (1 mV) were less than 30% of the detected voltage of Comparative Example 4 (7 mV).
[0101] The effect of Example 3 will be considered with reference to FIG. 9(b). Visible light V is irradiated onto the glass top plate 10, passes through the glass substrate 11 and reaches the infrared absorbing layer 22. A portion of the visible light V is reflected by the infrared absorbing layer 22 and is emitted from the glass substrate 11 to the outside. Since the infrared absorbing layer 22 of Example 3 is translucent, most of the visible light V passes through the infrared absorbing layer 22 and reaches the decorative layer 32. When the visible light V reaches the decorative layer 32, it is reflected by the decorative layer 32, and then passes through the infrared absorbing layer 22 and the glass substrate 11 to be emitted to the outside. As a result, in the glass top plate 10 of Example 3, the lightness L * is relatively large, which contributes to the decorativeness of the glass top plate 10.
[0102] On the other hand, when the infrared ray IR2 is irradiated to the glass top plate 10 and passes through the glass substrate 11 to reach the infrared absorbing layer 22, a part of the infrared ray IR is reflected by the infrared absorbing layer 22, and the remaining majority of the infrared ray IR enters the infrared absorbing layer 22. The infrared ray IR2 is absorbed by the infrared absorbing agent contained in the infrared absorbing layer 22 and attenuates. When the infrared ray IR2 reaches the decorative layer 32, the infrared ray IR2 is reflected by the decorative layer 32 and passes through the infrared absorbing layer 22. At this time, the infrared ray IR2 is absorbed by the infrared absorbing agent contained in the infrared absorbing layer 22, so that the infrared ray IR2 is further attenuated. By the time the infrared ray IR2 reaches the glass substrate 11, the infrared ray IR2 is attenuated and becomes weak. While the infrared ray IR2 is multiple-reflected in the glass top plate 10, the infrared ray IR2 is attenuated every time the infrared ray IR2 reaches the infrared absorbing layer 22. This makes it possible to reduce the infrared ray IR2 detected by the infrared sensor 3. In this way, in the glass top plate 10 of the third embodiment, the infrared ray IR2 irradiated to the glass top plate 10 can be attenuated.
[0103] 10(b), the effects of Example 4 will be considered. Visible light V is the same as in Example 3, so duplicated descriptions will be omitted.
[0104] On the other hand, when infrared rays IR2 are irradiated onto the glass top plate 10 and pass through the glass substrate 11 to reach the infrared absorbing layer 22, a part of the infrared rays IR2 is reflected by the infrared absorbing decorative layer 12, and the remaining majority of the infrared rays IR2 enter the infrared absorbing layer 22. The infrared rays IR2 are absorbed by the infrared absorbing agent contained in the infrared absorbing layer 22 and attenuated. When the infrared rays IR2 reach the infrared absorbing decorative layer 12, a part of the infrared rays IR2 is reflected by the infrared absorbing decorative layer 12 and passes through the infrared absorbing layer 22. At this time, the infrared rays IR2 are absorbed by the infrared absorbing agent, so that the infrared rays IR2 are further attenuated. On the other hand, the infrared rays IR2 that enter the infrared absorbing decorative layer 12 are absorbed by the infrared absorbing agent contained in the infrared absorbing decorative layer 12. When the infrared rays IR2 reach the light-shielding layer 13, they are reflected by the light-shielding layer 13 and pass through the infrared absorbing decorative layer 12, and are further absorbed by the infrared absorbing agent. While the infrared rays IR2 are multiple-reflected within the glass top plate 10, when the infrared rays IR reach the infrared absorbing layer 22 and the infrared absorbing decorative layer 12, the infrared rays IR2 are attenuated, and the infrared rays IR2 detected by the infrared sensor 3 can be reduced. Thus, it is considered that the glass top plate 10 of Example 4 can effectively attenuate the infrared rays IR2 irradiated to the glass top plate 10.
[0105] 5-3. Configuration in which infrared absorbing layer 22 is provided on surface 11A of glass substrate 11 Example 5 13(a), a glass top plate 10 of Example 5 will be described. The glass top plate 10 of this example includes a glass substrate 11, an infrared absorbing layer 22 formed on a front surface 11A of the glass substrate 11, a decorative layer 32 formed on a rear surface 11B of the glass substrate 11, and a light-shielding layer 13 formed on the decorative layer 32.
[0106] A light-transmitting coating material shown in Table 3 was applied to the entire surface 10A of the glass top plate 10 used in Comparative Example 4, except for the front window portion 15, by screen printing using a 300-mesh screen. The coating was then heated at 160°C for curing to form an infrared absorbing layer 22. The thickness of the infrared absorbing layer 22 was measured with a film thickness meter and found to be 7.5 μm. The inner diameter of the front window portion 15 of Example 5 was 10 mm. In this manner, the glass top plate 10 of Example 5 was produced.
[0107] (Various measurements) For Example 5 and Comparative Example 4, brightness measurement, infrared reflection spectrum measurement, and disturbance strength test were performed in the same manner as for Examples 1-2 and Comparative Examples 1-3. However, in the disturbance strength test, only the metal plate 6 made of aluminum was used, and no test was performed using the metal plate 6 made of SUS430. The results are shown in Figs. 14 and 15 and are summarized in Table 5. Table 5 lists the detection voltage of the infrared sensor 3 when the distance X from the axis P of the infrared sensor 3 to the edge of the metal plate 6 is 5 cm.
[0108] [Table 5]
[0109] (Measurement results) As shown in Table 5, the lightness L of the glass top plate 10 of Example 5 * The lightness L of the glass top plate 10 of Comparative Example 4 was 58.7. Thus, the glass top plate 10 of Example 5 can be decorated with a bright white color tone. * The lightness L of Example 5 is 62.6 because the infrared absorbing layer 22 is formed. * is thought to have decreased by 3.9.
[0110] 14 shows the reflection spectrum of the glass top plate 10 of Example 5 and Comparative Example 4. As shown in Table 5, the reflectance of infrared light with a wavelength of 940 nm was 15.1% in Example 5. This is considered to be due to the fact that Example 5 is provided with the infrared absorbing layer 22.
[0111] In contrast, the reflectance of Comparative Example 4 was 26.3%, which was a high reflectance. * This is thought to be due to the fact that Comparative Example 4 does not contain an infrared absorbing agent.
[0112] 15, the output voltage of Example 5 is smaller than that of Comparative Example 4 when the distance X from the axis P of the infrared sensor 3 is 3 cm to 7 cm. In other words, Example 5 is less susceptible to the influence of the external lighting fixture 5 than Comparative Example 4. This makes it possible to improve the accuracy of the infrared sensor 3.
[0113] Furthermore, as shown in Table 5, when the distance X from the axis P of the infrared sensor 3 is 5 cm, the output voltage of the infrared sensor 3 is 1 mV in Example 5, whereas it is 7 mV in Comparative Example 4. That is, the output voltage in Example 5 is reduced to 14% compared to Comparative Example 4. In this way, Example 5 is less susceptible to the influence of the external lighting fixture 5 compared to Comparative Example 4, and therefore the accuracy of the infrared sensor 3 can be improved.
[0114] The effect of the fifth embodiment will be considered with reference to FIG. 13(b). When visible light V is irradiated onto the glass top plate 10 and reaches the infrared absorbing layer 22 formed on the surface 11A of the glass substrate 11, a part of the visible light V is reflected by the infrared absorbing layer 22. Most of the visible light V proceeds to the infrared absorbing layer 22. Since the infrared absorbing layer 22 is transparent, the visible light V passes through the infrared absorbing layer 22 and reaches the glass substrate 11. A part of the visible light V that reaches the glass substrate 11 is reflected by the surface 11A of the glass substrate 11, passes through the infrared absorbing layer 22, and is emitted to the outside. Most of the visible light V enters the glass substrate 11. The visible light V that enters the glass substrate 11 reaches the decorative layer 32. The visible light V that reaches the decorative layer 32 is reflected by the decorative layer 32, passes through the glass substrate 11 and the infrared absorbing layer 22, and is emitted to the outside. As a result, in the glass top plate 10 of the fifth embodiment, the brightness L * is relatively large, which contributes to the decorativeness of the glass top plate 10.
[0115] On the other hand, when the glass top plate 10 is irradiated with infrared rays IR2, a part of the infrared rays IR is reflected by the infrared absorbing layer 22 formed on the surface 11A of the glass substrate 11. The infrared rays IR2 that are not reflected by the infrared absorbing layer 22 enter the infrared absorbing layer 22. The infrared rays IR2 that enter the infrared absorbing layer 22 are absorbed by the infrared absorbing agent contained in the infrared absorbing layer 22 and attenuated. When the infrared rays IR reach the surface 11A of the glass substrate 11, the infrared rays IR2 are reflected by the surface 11A of the glass substrate 11 and proceed inside the infrared absorbing layer 22. Then, the infrared rays IR2 are absorbed by the infrared absorbing agent of the infrared absorbing layer 22, are further attenuated, and are emitted to the outside. The infrared rays IR that are not reflected by the surface 11A of the glass substrate 11 enter the inside of the glass substrate 11. The infrared rays IR2 reach the decoration layer 32 and are reflected by the decoration layer 32. The infrared rays IR2 reflected by the decoration layer 32 pass through the glass substrate 11 and reach the infrared absorbing layer 22. The infrared rays IR that reach the infrared absorbing layer 22 are almost entirely absorbed by the infrared absorbing agent of the infrared absorbing layer 22. When the infrared rays IR2 reach the infrared absorbing layer 22 after being multiple-reflected within the glass top plate 10, the infrared rays IR2 are attenuated, and the infrared rays IR2 detected by the infrared sensor 3 can be reduced. In this way, in the glass top plate 10 of the fifth embodiment, the infrared rays IR2 irradiated to the glass top plate 10 can be effectively attenuated.
[0116] The present invention is not limited to the above-described embodiments, and can be applied to various embodiments without departing from the gist of the present invention.
[0117] In this embodiment, the lighting device 5 is illustrated as an example of a member different from the cooking device 4, but the present invention is not limited thereto. FIG. 16 shows another embodiment. In another embodiment, the induction heating cooker 1 includes a second heating means 7, exemplified by a radiant heater, in addition to the heating coil 2. A second back window 16 is formed on the back surface 10B of the glass top plate 10 at a position overlapping the second heating means 7 in the thickness direction of the glass substrate 11. The back surface 11B of the glass substrate 11 is exposed from the second back window 16. The second back window 16 is composed of a second infrared absorbing decorative layer window 16A formed in the infrared absorbing decorative layer 12 and a second light-shielding layer window 16B formed in the light-shielding layer 13.
[0118] The second heating means 7 is a member different from the cooking utensil 4, and emits infrared rays IR3. In this case, it is considered that the infrared rays IR3 emitted from the second heating means 7 are incident on the glass top plate 10. Even in this case, the infrared rays IR3 incident on the glass top plate 10 are absorbed by the infrared absorbing decorative layer 12, and are therefore prevented from reaching the infrared sensor 3. This allows the accuracy of the infrared sensor 3 to be improved. [Explanation of symbols]
[0119] 1: induction heating cooker, 3: infrared sensor, 10: glass top plate, 10A: front surface of glass top plate, 10B: rear surface of glass top plate, 11: glass substrate, 11A: front surface of glass substrate, 11B: rear surface of glass substrate, 12: infrared absorbing decorative layer, 13: light shielding layer, 22: infrared absorbing layer, 32: decorative layer
Claims
1. A glass top plate for a cooker is placed on top of a cooker equipped with an infrared sensor, a glass substrate having a front surface and a back surface; an infrared absorbing decorative layer provided on the rear surface side of the glass substrate and containing an infrared absorbing agent and a pigment that absorb infrared rays; an infrared absorbing decorative layer window portion through which the glass substrate is exposed is formed in the infrared absorbing decorative layer at a position overlapping with the infrared sensor in a thickness direction of the glass substrate when the glass top plate is placed in the cooking appliance; The lightness L measured from the front surface side of the glass substrate in accordance with JIS 8781-4:2013 * is 50 or more, A glass top plate for a cooking appliance, the reflectance of which is less than 25% for infrared rays having a wavelength of 940 nm as measured from the front surface side of the glass substrate.
2. Further, an infrared absorbing layer containing an infrared absorbing agent that absorbs infrared rays is provided, 2. The glass top plate for a cooking appliance according to claim 1, wherein the infrared absorbing layer has an infrared absorbing layer window portion through which the glass substrate is exposed, the infrared absorbing layer being formed at a position overlapping the infrared sensor in a thickness direction of the glass substrate.
3. A glass top plate for a cooking appliance to be placed on top of a cooking appliance having an infrared sensor, a glass substrate having a front surface and a back surface; a decorative layer provided on the rear surface side of the glass substrate and containing a pigment; At least one infrared absorbing layer including an infrared absorbing agent that absorbs infrared rays; With the glass top plate placed in the cooker, a decorative layer window portion through which the glass substrate is exposed is formed in the decorative layer at a position overlapping with the infrared sensor in a thickness direction of the glass substrate, an infrared absorbing layer window portion through which the glass substrate is exposed is formed in the infrared absorbing layer at a position overlapping with the infrared sensor in a thickness direction of the glass substrate; The lightness L measured from the front surface side of the glass substrate in accordance with JIS 8781-4:2013 * is 50 or more, A glass top plate for a cooking appliance, the reflectance of which is less than 25% for infrared rays having a wavelength of 940 nm as measured from the front surface side of the glass substrate.
4. 4. The glass top plate for a cooker according to claim 2, wherein the infrared absorbing layer is provided on the front surface or the back surface of the glass substrate.
5. Further, a light-shielding layer having light-shielding properties is provided on the back side of the infrared absorbing decorative layer, 2. The glass top plate for a cooking appliance according to claim 1, wherein the light-shielding layer has a light-shielding layer window portion through which the glass substrate is exposed, the light-shielding layer being formed at a position overlapping the infrared sensor in a thickness direction of the glass substrate.
6. Further, a light-shielding layer having a light-shielding property is provided on a back surface side of the decorative layer, 4. The glass top plate for a cooking appliance according to claim 3, wherein the light-shielding layer has a light-shielding layer window portion through which the glass substrate is exposed, the light-shielding layer being formed at a position overlapping the infrared sensor in a thickness direction of the glass substrate when the glass top plate is placed on the cooking appliance.
7. The glass top plate for a cooker according to any one of claims 1 to 3, wherein the infrared absorbing agent is capable of absorbing infrared rays having a wavelength of 780 nm to 2 µm.
8. 4. The glass top plate for a cooker according to claim 1, wherein the infrared absorbing agent is one or more compounds selected from the group consisting of metal hexaborides and tungstates.
9. 9. The glass top plate for cookware according to claim 8, wherein the infrared absorbing agent is lanthanum hexaboride.
10. The content of the lanthanum hexaboride is 0.005 [g / m 2 10. The glass top plate for a cooker according to claim 9, wherein the thickness of the glass top plate is equal to or greater than 100 μm.
11. 9. The glass top plate for cookware according to claim 8, wherein the infrared absorbing agent is cesium tungstate.
12. The content of the cesium tungstate is 0.08 [g / m 2 12. The glass top plate for a cooker according to claim 11, wherein
13. The lightness L * The glass top plate for a cooker according to any one of claims 1 to 3, wherein the hardness is 55 or more.
14. 4. The glass top plate for a cooker according to claim 1, wherein the reflectance of infrared light having a wavelength of 940 nm measured from the front surface side of the glass substrate is less than 20%.
15. The glass top plate for a cooker according to claim 1 , wherein the cooker is an induction heating cooker.
Citation Information
Patent Citations
Induction heating cooker
JP1991184295A
Cited By
Tableware heater and heating method
WO2026230069A1