Herbaceous fibrous material and wet-pulverized material thereof, production method and usage thereof

A pretreatment process using hydrogen chloride gas or a mixed acid solution effectively improves fibrillation and enzymatic saccharification of herbaceous fibers, addressing high energy costs and solubilization issues, resulting in a material with enhanced industrial applicability.

JP2024147487AActive Publication Date: 2024-10-16NAT AGRI & FOOD RES ORG
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023219802
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-03
Filing Date
2023-12-26
Publication Date
2024-10-16
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

Existing methods for producing defibrated herbaceous fibers face challenges with high energy consumption and manufacturing costs due to repeated pulverization, and there is a lack of effective techniques to improve fibrillation properties while minimizing the solubilization of glucan and xylan.

Method used

A pretreatment process involving hydrogen chloride gas or a mixed aqueous solution containing hydrochloric acid and an electrolyte is used to treat herbaceous fibers, followed by a wet-pulverization step, which reduces glucan and xylan content and enhances enzymatic saccharification properties, resulting in a fluffy and bulky precipitate.

Benefits of technology

The process improves fibrillation properties, reduces solubilization of glucan and xylan, and enhances enzymatic saccharification rates, producing a material with unique structural properties suitable for various industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147487000016
    Figure 2024147487000016
  • Figure 2024147487000017
    Figure 2024147487000017
  • Figure 2024147487000018
    Figure 2024147487000018
Patent Text Reader

Abstract

To provide a new pretreatment technique to improve fibrillation properties of a herbaceous fibrous material, a new herbaceous fibrous material produced through the new pretreatment technique, and application products using the new herbaceous fibrous material.SOLUTION: A herbaceous fibrous material is provided, of which decrement of glucan percentage content (comparison to dried one, wt.%) is equal to or less than 30%, and of which decrement of xylan percentage content (comparison to dried one, wt.%) is from 5% or more to 50% or less. A production method for the herbaceous fibrous material is provided, including an acid treatment process for processing the herbaceous fibrous material under hydrogen gas atmosphere or processing it through contact with a mixed aqueous solution including hydrochloric acid and an electrolyte other than hydrochloric acid, which liberates chloride ions in water, at a temperature of substantially 10°C or more to 50°C or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a herbaceous fiber material and a wet-ground product thereof. More specifically, the present invention relates to a defibration pretreatment process that reduces the environmental load and production costs in order to provide a defibrated fiber material made from herbaceous fiber as a raw material, and to a herbaceous fiber material and a wet-ground product thereof that have novel structural characteristics and are obtained thereby. [Background technology]

[0002] Biomass, whose main component is cellulose, such as plant stems and leaves, has been mainly used in the paper and textile industries through the recovery of fibrous materials such as pulp and hemp. Plant-derived fibrous materials are expected to have superior value in terms of abundant resources, environmental impact compared to fibers derived from fossil resources, affinity with living organisms, biodegradability, etc.

[0003] In recent years, there has been active research into the application of such natural fibrous materials to new applications by defibrating and refining them to a high degree, thereby giving them new physical properties and functionality. One representative example of such research is the production and use of cellulose nanofibers (CNF). Highly defibrated and refined fibrous materials are being considered for use as functional additives (for applications in thickeners, ballpoint pen inks, water-based paints, adhesives, etc.), highly functional daily products (for applications in shoe rubber, air filters, etc.), reinforced resins (for applications in polypropylene, nylon 6, etc.), etc.

[0004] In addition, efforts are being made to use pulp, absorbent cotton, and other materials as raw materials, subject them to strong acid hydrolysis with sulfuric acid, hydrochloric acid, and other acids to break down the cellulose chains, recover only the crystalline cellulose portion with a degree of polymerization of several hundred, and use it as a functional additive as cellulose nanocrystals (CNC), a type of CNF. Expectations are growing for industrial use of such defibrated and finely divided fibrous materials, driven by the need to develop bioplastics for decarbonization and reducing the environmental burden.

[0005] However, the development and use of defibrated and finely divided fibrous materials has mainly been carried out using wood as a raw material, and with the exception of cotton, which can be purified into cellulose by degreasing, many herbaceous fibers have been left behind in cutting-edge research into their advanced uses.

[0006] In this situation, a method (grinder method) has been proposed and considered in which herbaceous fiber is powdered and then wet-pulverized to defibrate and refine the fiber. However, it has been pointed out that this method increases energy consumption and production costs due to repeated grinding. Thus, in order to provide a fiber material that is competitive in terms of production costs and reduces environmental impact, a pre-defibration process that improves the defibration properties of the raw material is considered to be necessary.

[0007] As an acid treatment technique for fibrous raw materials, a method of hydrolysis by heating in an aqueous solution of hydrochloric acid or sulfuric acid is known. To date, processes have been proposed in which glucan and xylan are hydrolyzed in one step (e.g., concentrated sulfuric acid saccharification) or two steps (e.g., dilute sulfuric acid saccharification) to recover as many monosaccharides as possible, but a method for hydrolysis while leaving most of the glucan and xylan intact has not been investigated.

[0008] The acid hydrolysis process, in which hydrogen chloride gas acts on fibrous raw materials, has long been considered as a core process for wood saccharification. Unlike the hydrolysis mechanism in liquids, which proceeds from the solid-liquid interface, hydrogen chloride gas treatment dissolves in the free water in the substrate, and is thought to hydrolyze locally and efficiently due to the heat generated by dissolution. However, conventional hydrogen chloride gas treatments were aimed at the complete decomposition of polysaccharides.

[0009] In recent years, it has been reported that an efficient CNC recovery process can be achieved by treating cellulosic raw materials such as filter paper powder with hydrogen chloride gas, which fragments the cellulose and allows CNC to be recovered (see Patent Document 1 and Non-Patent Document 1). However, there is no evidence that hydrogen chloride gas treatment promotes defibration of fibrous materials.

[0010] Furthermore, in Patent Document 2 by the present inventors, a technology is disclosed in which a material containing polysaccharides is treated with an acid, causing the polysaccharides to swell and become smaller in molecular weight, thereby producing a new material that is endowed with solubility and dispersibility. However, "solubilization" and "dispersion" refer to a state in which particles are apparently distributed uniformly in water, and are therefore clearly different from the material that gives a bulky precipitate provided by the present disclosure. Also, while Patent Document 2 swells "polysaccharides," the present disclosure differs in that the entire herbaceous stem and leaf tissue is fluffy to make it bulky. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Special Publication No. 2014-511907 [Patent Document 2] Patent No. 5190858 [Non-patent literature]

[0012] [Non-Patent Document 1] E. Kontturi, et al., Angew. Chem. Int. Ed., 55, 14455-14458 (2016) Summary of the Invention [Problem to be solved by the invention]

[0013] In view of the above circumstances, the present inventors have conducted extensive research into a pretreatment process for improving the defibration property of herbaceous fiber material. As a result, they have found that by treating herbaceous fiber material under a hydrogen chloride gas atmosphere or by subjecting it to an acid treatment in which the material is brought into contact with a solution that emits hydrogen chloride gas, not only is the defibration property of the fiber material improved, but the decrease in the glucan and xylan content is also significantly suppressed. In addition, the present inventors have found that by performing a wet grinding treatment after this acid treatment, a new material can be obtained that has excellent enzymatic saccharification properties and a "network structure" in which the entire tissue is fluffy. Based on these findings, the present inventors have completed the present disclosure.

[0014] The objective of the present invention is to provide a new pretreatment technology for improving the defibration ability of herbaceous fiber, to provide a new herbaceous fiber material obtained by said pretreatment technology, and to provide applied products using said new material. [Means for solving the problem]

[0015] In order to solve the above problems, the present disclosure provides a herbaceous fiber material characterized in that, compared to the composition of the raw herbaceous fiber material, the glucan content (based on the dry matter, by weight %) is reduced by 30% or less, and the xylan content (based on the dry matter, by weight %) is reduced by 5% to 50%.

[0016] The herbaceous fiber material may be produced by a method including the following steps: An acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10°C and 50°C. A process for washing and / or adjusting the pH of the treated product after the acid treatment process.

[0017] The present disclosure also provides an acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10°C and 50°C; a wet-grinding step in which the treated product that has been subjected to the acid treatment step is subjected to a wet-grinding step; A wet-ground herbaceous fibrous material produced by a method comprising: Compared with a wet-ground product obtained by the same method except that the acid treatment step was not performed on the raw herbaceous fiber material, The wet-ground product of herbaceous fibrous material is characterized in that when the wet-ground product is suspended in water and allowed to stand at room temperature for one hour or more, the apparent volume of the precipitate obtained is at least twice as large, and / or when the wet-ground product is treated with a fibrous decomposition enzyme, the saccharification rate of glucan is at least 1.5 times as large.

[0018] Furthermore, the present disclosure also provides a method for producing a herbaceous fiber material, comprising the steps of: An acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10°C and 50°C. A process for washing and / or adjusting the pH of the treated product after the acid treatment process.

[0019] The present disclosure also provides a method for producing a wet-ground herbaceous fibrous material, the method comprising the steps of: An acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10°C and 50°C. A wet-grinding step in which the treated product that has been subjected to the acid treatment step is subjected to a wet-grinding step.

[0020] Furthermore, the present disclosure also provides products such as resins, plastics, rubbers, inks or paints; paper, nonwoven fabrics, fibers, seedling pots or boards; saccharification raw materials or feed; which are characterized by containing the herbaceous fibrous material or a wet-ground product of the herbaceous fibrous material, or a fraction thereof, or a modified and / or altered product thereof. Effect of the Invention

[0021] According to the present disclosure, it is possible to provide a pretreatment technique for defibrating herbaceous fiber material, which can improve the defibration property of herbaceous fiber material while significantly suppressing the solubilization of glucan and xylan. Furthermore, the herbaceous fiber material obtained by this pretreatment technique is a material that has excellent enzymatic saccharification properties and a unique property in which the entire tissue becomes fluffy and gives rise to a bulky precipitate in water when further subjected to a wet grinding treatment.

[0022] In other words, the present disclosure provides a new pretreatment technology for improving the defibration ability of herbaceous fiber, a new herbaceous fiber material obtained by the pretreatment technology, and application products using the new material. [Brief description of the drawings]

[0023] [Figure 1A] FIG. 2 is an image diagram of the formation of bulk precipitate according to the present disclosure. [Figure 1B] FIG. 2 is a photographic image comparing the sediment volume of the wet-milled product of the present disclosure (right) and a control sample (left). [Figure 1C] FIG. 1 is a micrograph of a wet-milled product according to the present disclosure (white bar: 50 μm). (Example 3) [Figure 2A] 2A is a graph showing the bulkiness of wet-ground products derived from various raw materials (Example 2). In Fig. 2A, the vertical axis shows the volume of the sediment of the sample (unit: mL), and the horizontal axis shows, from the left, rice straw, sugarcane bagasse, Miscanthus sinensis, and Erianthus, with the left bar showing data for the hydrochloric acid-calcium chloride aqueous solution treatment area and the right bar showing data for the control area (treated with calcium chloride aqueous solution). [Figure 2B] 2B is a graph showing the enzymatic saccharification rate of wet-milled materials derived from various raw materials (Example 2). In Fig. 2B, the vertical axis shows the enzymatic saccharification rate of glucan (unit: %), and the horizontal axis shows, from the left, rice straw, sugarcane bagasse, Miscanthus sinensis, and Erianthus, with the left bar showing data from the hydrochloric acid-calcium chloride aqueous solution treatment group and the right bar showing data from the control group (treated with calcium chloride aqueous solution). [Diagram 3] FIG. 11 is a schematic diagram showing a method of a gas phase treatment test in Example 3. [Figure 4]FIG. 1 is a photographic image showing a plate molded using the wet-milled product of the present disclosure (Example 8). [Diagram 5] FIG. 1 is a photographic image of a sheet (nonwoven fabric) formed using the wet-ground product of the present disclosure (Example 9). [Figure 6] FIG. 13 is a photographic image showing the method of the gas phase treatment test in Example 11. [Figure 7] FIG. 1 is a photographic image showing a rod-shaped product formed using the wet-ground product of the present disclosure (Example 12). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] This embodiment will be described in detail below.

[0025] (1) Herbaceous fibrous materials The herbaceous fiber material of this embodiment is characterized in that, compared to the composition of the raw herbaceous fiber material, the glucan content (by weight of dry matter) is reduced by 30% or less, and the xylan content (by weight of dry matter) is reduced by 5% or more and 50% or less.

[0026] "Herbaceous fiber raw material" refers to at least a part of the plant body of a herbaceous plant, and may be, for example, the stems and leaves of herbaceous plants that are by-produced during agricultural production (rice straw, wheat straw, corn stover, sugarcane trash, etc.) and / or underground parts, residues that are by-produced during the primary processing of agricultural products and / or during food production (sugarcane bagasse, rice husks, corn cobs, etc.), the stems and leaves of purpose-cultivated herbaceous resource crops (erianthus, miscanthus, silver grass, sorghum, switchgrass, napier grass, etc.), herbaceous plants and weeds (silver grass, etc.) cut down from the waterside of rivers and / or lakes, on slopes next to roads, etc., and aquatic plants. Preferably, the "herbaceous fiber raw material" may be one or more selected from the group consisting of rice straw, wheat straw, corn stover, sugarcane bagasse, sugarcane trash, Miscanthus sinensis, Miscanthus japonica, Erianthus, sorghum, Napier grass, Judea japonica, Danchiku, and hemp.

[0027] The herbaceous fiber raw material may be a shredded, finely crushed, pulverized, dried, defatted, bleached, mildly acid-treated, or mildly alkali-treated herbaceous fiber raw material. The herbaceous fiber raw material is preferably one from which cell wall components such as lignin have not been removed, but may be one from which cell wall components have been partially removed. This is because it is considered difficult to improve defibration properties if cell wall components other than cellulose are completely removed before acid treatment. For this reason, raw materials with a very high glucan (mainly containing cellulose) content such as highly refined pulp (specifically, raw materials with a glucan content of more than 80%) are not preferable as the herbaceous fiber raw material according to the present embodiment. Similarly, raw materials from which cell wall components other than cellulose have been completely removed are not preferable as the herbaceous fiber raw material according to the present embodiment.

[0028] The herbaceous fiber material is prepared by carrying out the above-mentioned acid treatment process on the herbaceous fiber raw material, followed by washing and / or pH adjustment. The herbaceous fiber raw material contains glucan and xylan as polysaccharides, but these are mostly decomposed and solubilized by conventional treatment in an acid aqueous solution. However, the herbaceous fiber material of the present embodiment is characterized in that the reduction rates of the glucan and xylan contents (based on the dry matter, weight %) are suppressed to 30% or less and 50% or less, respectively, compared with the composition of the raw herbaceous fiber raw material. Preferably, the reduction rate of the glucan content may be 30% or less, 25% or less, 20% or less, 15% or less, 14% or less, 13% or less, 12% or less, 11% or less, or 10% or less. Preferably, the reduction rate of the xylan content may be 50% or less, 45% or less, 40% or less, 39% or less, 38% or less, 37% or less, 36% or less, or 35% or less. The lower limit of the reduction rate of the xylan content may be 5% or more.

[0029] Here, the content of glucan or xylan is the weight ratio (%) of glucan or xylan to the dry weight of solid matter in the sample. The reduction rate of the content of glucan or xylan is the ratio (%) obtained by subtracting the content after acid treatment from the content before acid treatment, divided by the content before acid treatment. Here, the reduction rate of the content of glucan or xylan must be evaluated based on the sample remaining after washing the acid-treated product. Since monosaccharides, oligosaccharides, etc., which are hydrolysis products by acid treatment, remain in the sample after acid treatment, if the glucan or xylan content is measured without washing after acid treatment, theoretically, it will be almost the same as the sugar composition in the herbaceous fiber material before acid treatment. The amount of glucan and the amount of xylan are evaluated as the amount of homopolymers of glucose and xylose, respectively. The detailed calculation method of these values ​​is as described in Example 1.

[0030] The herbaceous fibrous material may contain lignin derived from the raw material. The lignin content in the herbaceous fibrous material (wt % based on the dry matter) is not particularly limited, but is usually 30% or less, and preferably 10% to 25%.

[0031] The herbaceous fibrous material of this embodiment also has improved defibrability due to the acid treatment process. Therefore, it is desirable that the herbaceous fibrous material is then subjected to a defibration process, but this use is not limited to this. Here, a method for confirming the improvement in defibrability includes a method of dispersing the herbaceous fibrous material obtained after defibration in water and measuring the apparent volume of the precipitate observed after leaving it to stand at room temperature for a certain period of time (for example, one hour or more). The apparent volume of the mass consisting of the precipitated herbaceous fibrous material can be measured visually using a graduated container (for example, a graduated cylinder). As the defibrability increases, the fibers become more likely to fluff and the precipitate becomes bulky. When the defibration process is continued for a long period of time, even if there is no difference in the final defibrability between a comparative control sample that has not been subjected to the acid treatment process and a treated sample, it is important to be able to reduce the time until the final defibrated state or the severity of the defibration process.

[0032] The herbaceous fiber material according to the present embodiment is an invention of a product, but its definition includes a manufacturing method. In the present embodiment, the inventors believe that the herbaceous fiber material has both seemingly contradictory structural characteristics of improved defibrability and retention of polysaccharides because limited modification of the herbaceous fiber raw material with hydrogen chloride gas has been performed. However, such a state of the herbaceous fiber material is transient, and it is impossible to clearly express the structure and characteristics of the actual material in words. Even if the morphology of the herbaceous fiber material is observed using a scanning electron microscope or the like, the defibrability of the tissue differs depending on the type of raw material, so in order to find an index that specifies the characteristics of the limited modification by hydrogen chloride gas by repeating measurements on a large number of samples and performing statistical processing, a significant amount of trial and error is required, which is not practical at all. The above-mentioned impossible or impractical circumstances also apply to wet-ground herbaceous fiber materials.

[0033] (2) Manufacturing method of herbaceous fiber material Next, a method for producing a herbaceous fiber material will be described. This production method includes an acid treatment step and a step of washing and / or adjusting the pH after the acid treatment as essential steps, and may include a pre-step of subjecting the herbaceous fiber raw material before the acid treatment to physical and / or chemical treatment (chopping, crushing, pulverization, drying, defatting, bleaching, mild acid treatment, mild alkali treatment, etc.) as needed.

[0034] That is, according to this embodiment, an acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10°C and 50°C; A step of washing and / or adjusting the pH of the treated product after the acid treatment step; A method for producing a herbaceous fibrous material comprising the steps of:

[0035] According to one embodiment, A pre-process of performing one or more treatments selected from chopping, crushing, pulverizing, drying, defatting, bleaching, mild acid treatment, and mild alkali treatment on the herbaceous fiber raw material; an acid treatment step in which the treated product from the previous step is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10° C. and 50° C.; A step of washing and / or adjusting the pH of the treated product after the acid treatment step; A method for producing a herbaceous fibrous material comprising the steps of:

[0036] The previous step in the present production method may be, for example, a step of drying the herbaceous fiber raw material. The herbaceous fiber raw material can be acid-treated in a dry or wet state, but in order to improve the efficiency of the acid treatment, it is desirable to reduce the moisture content. The moisture content of the herbaceous fiber raw material can usually be 40% or less, preferably 20% or less, and more preferably 10% or less. When acid treatment is performed under low moisture content conditions, components located near the free water or parts thereof are preferentially hydrolyzed, which is thought to reduce the physical strength of the tissue and improve defibration while minimizing excessive hydrolysis and loss of polysaccharides.

[0037] The previous step in the present production method may be, for example, a step of chopping, finely crushing, pulverizing, etc. the herbaceous fiber raw material. Since the acid is emitted from the gas phase or the solid-liquid interface toward the solid surface, it is desirable to chop, finely crush, pulverize, etc. the herbaceous fiber raw material before the acid treatment so that the herbaceous fiber raw material has a sufficient surface area and the gas can reach the inside of the raw material in a short time. These treatments can be carried out using known methods such as cutting with a sharp blade, cutting by impact force with a hammer mill or ball mill, or cutting by shear force with a grinder or extruder.

[0038] In addition, the pre-process in the present manufacturing method may be, for example, a process of degreasing, bleaching, or performing a mild acid treatment or a mild alkali treatment on the herbaceous fiber raw material, but it is preferable that the pre-process does not include a process of completely removing cell wall components other than cellulose. As described above, if cell wall components other than cellulose are completely removed before the acid treatment, it is considered difficult to improve the defibration property, but the effect of the present disclosure may be obtained even with a raw material whose cell wall has been mildly modified. Therefore, the pre-process in the present manufacturing method does not include a process of extremely increasing the glucan (mainly containing cellulose) content like highly refined pulp (specifically, the glucan content is made to exceed 80%) by removing cell wall components other than cellulose. The term "mild acid treatment" refers to, for example, an acid treatment in which a small amount of cell wall components are eluted (for example, the glucan content is 80% or less) by performing hydrolysis in a conventional acid solution for a short period of time. The term "mild alkali treatment" may be, for example, a conventional alkali treatment for the purpose of desalting, dexylania, delignification, etc., performed for a short period of time. The degreasing and bleaching treatments can be carried out by conventionally known techniques.

[0039] In the acid treatment step of this production method, the herbaceous fiber material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution that emits hydrogen chloride gas. The action of hydrogen chloride gas partially decomposes the herbaceous fiber material, improving the efficiency of defibration, but at the same time, it is important to minimize the loss of polysaccharides in the herbaceous fiber material. Here, it is believed that reducing the loss of polysaccharides in the herbaceous fiber material will lead to maintaining its value as a fiber and also to its value as a saccharification raw material.

[0040] The acid treatment step in the present production method can be carried out by allowing the herbaceous fiber raw material (or its shredded, finely crushed, pulverized, dried, defatted, bleached, or mildly acid- or alkali-treated product) to coexist with hydrogen chloride gas. Hydrogen chloride gas can be supplied as commercially available hydrogen chloride gas, gas generated from a high-concentration hydrochloric acid aqueous solution, gas generated from a mixed aqueous solution that emits hydrogen chloride gas, or the like.

[0041] The "mixed aqueous solution that emits hydrogen chloride gas" may be a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water. The "electrolyte other than hydrochloric acid that liberates chloride ions in water" may be calcium chloride, magnesium chloride, ammonium chloride, or the like. Alternatively, the "mixed aqueous solution" may dissolve one or more electrolytes selected from calcium chloride, magnesium chloride, and ammonium chloride as the electrolyte other than hydrochloric acid that liberates chloride ions in water, or may contain a solute substantially equivalent to the aqueous solution in which the electrolyte is dissolved. Here, the "solute substantially equivalent to the aqueous solution in which the electrolyte is dissolved" may be, for example, lithium chloride, barium chloride, iron chloride, or the like, but is not particularly limited. The concentration of hydrochloric acid and the concentration of the electrolyte other than hydrochloric acid in the "mixed aqueous solution" may be, for example, 10:1 to 1:20, preferably 5:1 to 1:5, more preferably 2:1 to 1:5, and particularly preferably 1:1 to 1:5 in molar ratio, but is not limited thereto. Specifically, the "mixed aqueous solution" may contain 0.2 to 11 M hydrochloric acid and an electrolyte other than hydrochloric acid, such as calcium chloride, at 2 to 5 M, preferably 3 to 5 M, but is not limited thereto.

[0042] Methods for allowing the herbaceous fiber material (substrate) to coexist with hydrogen chloride gas include, in addition to a method of passing hydrogen chloride gas through a chamber filled with the substrate, a method of placing the substrate and a hydrogen chloride gas source (high-concentration hydrochloric acid solution, mixed aqueous solution that emits hydrogen chloride gas, etc.) in a closed container in a non-contact state, a method of contacting the substrate with a solution that serves as a hydrogen chloride gas source (high-concentration hydrochloric acid solution, mixed aqueous solution that emits hydrogen chloride gas, etc.), a method of contacting an electrolyte other than the above-mentioned hydrochloric acid in a solid state with hydrochloric acid to generate hydrogen chloride gas as the electrolyte dissolves, and the like, but are not limited to these methods. Note that in the "method of contacting the substrate with a solution that serves as a hydrogen chloride gas source" (hereinafter sometimes referred to as "liquid-phase treatment"), the entire substrate may be immersed in the solution, or at least a part of the substrate may be above the liquid surface. Specifically, the amount of solution per 1 g of substrate can be 0.5 mL or more, 0.75 mL or more, 1 mL or more, 1.25 mL or more, 1.5 mL or more, 1.75 mL or more, 2 mL or more, 2.25 mL or more, 2.5 mL or more, 2.75 mL or more, or 3 mL or more. In addition, the "method of passing hydrogen chloride gas through a chamber filled with a substrate" and the "method of placing a substrate and a hydrogen chloride gas source in a sealed container in a non-contact state" are sometimes referred to as "gas phase treatment" in this disclosure. After being used in a reaction under non-contact conditions (gas phase treatment), a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water can be heated to evaporate hydrogen chloride gas and water, and separated to increase the concentration of the electrolyte in the aqueous solution, thereby allowing the electrolyte to be reused or recycled.

[0043] The acid treatment step is carried out substantially within a temperature range of 10°C to 50°C. Here, "substantially" indicates that the total time of acid treatment at temperatures other than the above temperature range is 5% or less, preferably 3% or less, of the total acid treatment time. The preferred temperature conditions in the acid treatment step are 10°C to 40°C, 20°C to 35°C, and particularly room temperature (25±5°C). As for pressure conditions, the hydrolysis reaction proceeds faster by increasing the partial pressure of hydrogen chloride gas, but it can also be carried out under normal pressure or reduced pressure conditions. The treatment time is not particularly limited because it is affected by the structure of the raw material, the moisture content, the treatment temperature, the partial pressure and treatment method of hydrogen chloride gas, the size of the reaction chamber, etc. Conversely, the treatment conditions may be set so that the reduction rate of the glucan and xylan contents in the herbaceous fiber material falls within a predetermined range. For example, when 1 mL to 3 mL of a mixed aqueous solution that emits hydrogen chloride gas per 1 g of substrate (ground material) is contact treated at room temperature (25±5°C), the acid treatment time can usually be from a few minutes to 4 days, and can preferably be in the range of from 1 hour to 3 days, from 3 hours to 2 days, from 6 hours to 36 hours, from 8 hours to 30 hours, from 10 hours to 24 hours, or from 12 hours to 20 hours.

[0044] In the method for producing a herbaceous fiber material, the acid-treated product after the acid treatment step is washed and / or pH adjusted. Washing is performed to separate and remove hydrogen chloride gas and hydrochloric acid remaining in the acid-treated product after the acid treatment step, monosaccharides, oligosaccharides, and other hydrolyzates present as hydrolysis products, and deposits, water-extractable components, and acid-extractable components derived from the herbaceous fiber raw material, thereby improving the processing characteristics and usability of the herbaceous fiber material and suppressing quality deterioration when it is processed into boards, paper, etc.

[0045] The pH adjustment is performed to reduce or eliminate the corrosiveness, danger, and toxicity of hydrochloric acid to containers and grinding equipment, and to perform enzymatic reactions, biological culture, and other processes, and may include processes such as dilution with water, washing with water, and simple addition of water. The pH adjustment can also be performed by removing hydrogen chloride gas by heating, or by adjusting the pH in the gas phase with ammonia. The range of pH adjustment varies depending on the subsequent operation and is not particularly limited. The introduction of a pH adjustment process is effective in cases where water or a buffer solution is added to the acid-treated product without removing substances that can be removed by washing, and then a wet grinding process is performed to suppress the loss of free sugar and perform enzymatic saccharification as is. In particular, the pH adjustment process, which replaces the washing process, is industrially advantageous in terms of improving the sugar recovery rate and added value as a functional feed by minimizing the loss of functional components such as xylooligosaccharides, which are partial hydrolysates of xylan by acid.

[0046] However, as described above, even if washing is not performed while only adjusting the pH, when evaluating the rate of decrease in the glucan or xylan content, it is necessary to measure and evaluate the sample after washing.

[0047] In this manner, the herbaceous fiber material of the present embodiment can be produced. The herbaceous fiber material can be recovered as a water-insoluble matter after washing and / or pH adjustment. The glucan content and xylan content (evaluated as a homopolymer of glucan or xylose) of the recovered herbaceous fiber material are calculated to evaluate the component characteristics of the herbaceous fiber material. The glucan content and xylan content in the herbaceous fiber material can be modified by additionally performing a heat treatment in the presence of an acid or additionally performing an enzyme treatment after the acid treatment step. However, even if such additional treatment involving a change in the component characteristics of the material is performed, it is still included in the scope of the herbaceous fiber material of the present embodiment as long as the reduction rates of the glucan and xylan contents before and after the acid treatment step are within the above-mentioned predetermined ranges.

[0048] (3) Wet-ground herbaceous fibrous materials The wet-ground herbaceous fiber material according to the present embodiment is an acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10°C and 50°C; a wet-grinding step in which the treated product that has been subjected to the acid treatment step is subjected to a wet-grinding step; A wet-ground herbaceous fibrous material produced by a method comprising: Compared with a wet-ground product obtained by the same method except that the acid treatment step was not performed on the raw herbaceous fiber material, The wet-ground product is characterized in that the apparent volume of the precipitate obtained when the wet-ground product is suspended in water and allowed to stand at room temperature for one hour or more is more than doubled, and / or the saccharification rate of glucan when the wet-ground product is treated with a fibrous enzyme is more than 1.5 times higher.

[0049] The wet-ground herbaceous fiber material according to this embodiment (hereinafter, sometimes simply referred to as "wet-ground material") is produced by a method including the acid treatment step and the wet-ground step as essential steps. The "acid treatment step" and the "herbaceous fiber material" are as described above.

[0050] Since the defibrability of the herbaceous fibrous material is improved by the acid treatment step, the subsequent defibration step in the wet grinding step is more efficient. This effect can be evaluated, for example, by the apparent volume of the precipitate obtained when the wet-ground material obtained is suspended in water and allowed to stand at room temperature for one hour or more. When the herbaceous fibrous material is wet-ground, it is possible to obtain a bulky precipitate that is at least two times, preferably at least three times, larger than that of a wet-ground sample that has not been subjected to the acid treatment step (for example, a sample that has been contacted with a solution without hydrochloric acid, a sample that has been contacted with an aqueous solution of only hydrochloric acid, a sample before the acid treatment step, etc.) (see FIG. 1B). A detailed method for evaluating the bulky precipitate can be, for example, the method described later in the Examples.

[0051] The mechanism by which the wet-milled material becomes bulky in water will be explained with reference to Figures 1A and 1C. The tissue of the herbaceous fibrous material is defibrated by the wet-milling process so that it becomes fluffy (Figure 1C), forming a defibrated mechanical pulp-like structure that occupies a large space, and is thought to provide the bulky sediment (Figure 1A).

[0052] The wet-ground product according to the present embodiment may have high saccharification properties, such that the saccharification rate of glucan when treated with a fibrous enzyme is 1.5 times or more, preferably 2 times or more, compared to a wet-ground product obtained without carrying out the acid treatment step. Due to the high saccharification properties, nano-sized materials such as lignocellulose nanofibers (LCNF) and CNFs can be easily produced by further wet-grinding the wet-ground product. LCNFs are cellulose partially bonded to other cell wall components, and are expected to exhibit unique properties such as dispersibility, biodegradability, and derivatization properties. Furthermore, the cell walls of herbaceous fiber resources can be refined for cellulose under milder conditions than the cell walls of wood fiber resources. Due to this property, the nano-sized wet-ground product obtained by the present disclosure can be chemically modified under simple conditions such as alkali treatment and oxidation treatment, and it is expected to expand the demand for herbaceous fiber resources.

[0053] Examples of "fibrous decomposition enzymes" include cellulose decomposition enzymes such as cellobiohydrolase, endoglucanase, lytic polysaccharide monooxygenase, cellobiose dehydrogenase, cellooligosaccharide phosphorylase, cellobiose phosphorylase, and β-glucosidase; xylan decomposition enzymes such as xylanase, xylosidase, arabinofuranosidase, galactosidase, glucuronidase, and acetyl xylan esterase; pectin decomposition enzymes such as pectinase, pectolyase, arabinanase, galactanase, and pectin methyl esterase; xyloglucan decomposition enzymes such as xyloglucanase; (1-3),(1-4)-β-glucan decomposition enzymes such as lichenase; and lignin decomposition enzymes such as lignin peroxidase and laccase. Two or more of these fibrous decomposition enzymes can be used in combination. Preferably, cellulose decomposition enzymes can be used as the fibrous decomposition enzymes. A detailed method for evaluating the glycation property may be, for example, the method described below in the Examples.

[0054] The wet-ground product according to the present embodiment may be a fraction obtained by fractionating a fraction mainly composed of wet-ground products having a particle size of less than 1 μm after the wet-ground process, or may be a modified and / or altered product in which at least a part of the surface has been modified and / or altered. Here, "mainly composed of wet-ground products having a particle size of less than 1 μm" means that the concentration is sufficient to significantly express the characteristics of particles having a particle size of less than 1 μm, for example, 50% or more. Since the wet-ground product to be obtained by the present disclosure also contains particles having a large aspect ratio, there is a possibility that the major axis of the "wet-ground product having a particle size of less than 1 μm" may be greater than 1 μm. In addition, the "modified and / or altered product" may be, for example, a product in which polysaccharides such as chitosan, xyloglucan, carboxymethylcellulose sodium salt, alginate, galactomannan, gellan gum, carrageenan, and (1-3),(1-4)-β-glucan are physically adsorbed on the surface of the wet-ground product. Adding other substances during wet milling makes it possible to modify and / or alter the surface. This modification and / or alteration is expected to lead to functional changes when the resulting wet-milled product is used, as well as to suppress reassociation of particles during wet milling, thereby making milling more efficient.

[0055] One mode of use of the wet-ground material according to the present embodiment is fillers such as resins, plastics, rubbers, inks, and paints. By mixing the wet-ground material with various resins such as polypropylene and nylon 6 and other modifiers, it is possible to modify physical properties such as material strength while reducing the environmental impact of plastics that are burned or biodegraded. In addition, it can be used as a highly functional filler through conversion to lignocellulose nanoparticles that exhibit a dispersing effect. That is, according to the present embodiment, there are provided resins, plastics, rubbers, inks, or paints that contain the herbaceous fiber material, its wet-ground product, or fractions thereof, or modified and / or altered products thereof.

[0056] Other uses of the wet-ground material according to the present embodiment include mass-consumer materials such as paper, nonwoven fabric, fiber, filter, hardboard, plate, and three-dimensional molded product. Since the material exhibits high biodegradability, it can be used as a material for agricultural mulch, seedling pot, and the like that are assumed to deteriorate in the environment. The mass-consumer materials described above can be produced by mixing the herbaceous fiber material according to the present disclosure, its wet-ground product, or its fraction, modified product, etc., alone or with any auxiliary raw material, and molding it by a conventionally known method. That is, according to the present embodiment, paper, nonwoven fabric, fiber, filter, seedling pot, board, or three-dimensional molded product containing the herbaceous fiber material, its wet-ground product, or its fraction, or its modified and / or modified product, is provided. In addition, compared with a case where the wet-pulverized material is subjected to the acid treatment without the acid treatment, a compression molded product using the wet-pulverized material after the acid treatment has stronger binding properties and / or a higher density and / or has a lower expansion rate or water absorption rate after the water absorption, and therefore has high industrial usefulness.

[0057] Another aspect of the use of the wet-ground product according to the present embodiment is as a saccharification raw material. Linking enzyme saccharification, saccharification and fermentation by microorganisms with valuable product production can lead to the production of food, biofuel, and biomaterials. It can also be used as a highly digestible feed for ruminants. It is also possible to use the herbaceous fibrous material according to the present disclosure, its wet-ground product, or its fraction, modified product, etc., in stages. For example, the wet-ground product according to the present embodiment can be reused as a saccharification raw material after being used as a board. In this case, by subjecting the discarded molded product to a wet-ground process again, it is possible to obtain an enzyme saccharification rate equal to or higher than that of the original wet-ground product. In addition, for the purpose of storing the wet-ground product until its use or reuse, a three-dimensional molded product such as a rod, a bar, or a lump containing the wet-ground product can be manufactured. That is, according to the present embodiment, a saccharification raw material or a feed containing the herbaceous fibrous material, its wet-ground product, or a fraction thereof, or a modified and / or modified product thereof is provided.

[0058] (4) Method for producing wet-ground herbaceous fibrous material Next, a method for producing a wet-ground herbaceous fiber material will be described. This production method includes an acid treatment step and a wet-ground step as essential steps, and may include, as necessary, a pre-step of subjecting the herbaceous fiber raw material before the acid treatment to physical and / or chemical treatment (chopping, finely crushing, grinding, drying, degreasing, bleaching, mild acid treatment, mild alkali treatment, etc.); a step of washing and / or adjusting the pH after the acid treatment; a step of modifying and / or altering at least a part of the surface of the wet-ground product; and a step of separating and recovering a fraction mainly composed of wet-ground products having particle sizes of less than 1 μm from the wet-ground product obtained by the wet-ground product step. The "herbaceous fiber raw material" and "acid treatment step" are as described above.

[0059] According to this embodiment, an acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10°C and 50°C; a wet-grinding step in which the treated product that has been subjected to the acid treatment step is subjected to a wet-grinding step; The present invention provides a method for producing a wet-ground herbaceous fibrous material, comprising the steps of:

[0060] According to one embodiment, A pre-process of performing one or more treatments selected from chopping, crushing, pulverizing, drying, defatting, bleaching, mild acid treatment, and mild alkali treatment on the herbaceous fiber raw material; an acid treatment step in which the treated product from the previous step is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10° C. and 50° C.; a wet-grinding step in which the treated product that has been subjected to the acid treatment step is subjected to a wet-grinding step; The present invention provides a method for producing a wet-ground herbaceous fibrous material, comprising the steps of:

[0061] According to another embodiment, A pre-process of performing one or more treatments selected from chopping, crushing, pulverizing, drying, defatting, bleaching, mild acid treatment, and mild alkali treatment on the herbaceous fiber raw material; an acid treatment step in which the treated product from the previous step is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10° C. and 50° C.; A step of washing and / or adjusting the pH of the treated product after the acid treatment step; a wet-grinding step of performing a wet-grinding process on the treated product that has been subjected to the above steps; A step of recovering a fraction mainly composed of wet-milled material having a particle size of less than 1 μm from the wet-milled material obtained by the wet-milling step; The present invention provides a method for producing a wet-ground herbaceous fibrous material, comprising the steps of:

[0062] The "wet grinding process" can be carried out by known grinding devices such as an electric stone mill type defibrator, a bead mill, a ball mill, and other impact grinding devices, as well as an extruder, a high-pressure homogenizer, an ultrasonic crusher, a mortar and pestle, a blender, a polytron homogenizer, and other. When using these grinding devices, a grinding process can be introduced as a pretreatment as necessary to match the raw material receiving size of each grinding device. In addition, the wet-ground product according to the present embodiment can be molded by kneading it with a hydrophobic material while grinding it, either directly or after being subjected to a hydrophobic treatment such as acetylation.

[0063] In addition, various additives can be added during wet milling to promote defibration and micronization and to impart new functions. For example, by adding polysaccharides such as chitosan, xanthan gum (tamarind seed gum), guar gum, carboxymethylcellulose, xyloglucan, alginate, galactomannan, gellan gum, carrageenan, and salts of (1-3) and (1-4)-β-glucan, which exhibit interactivity with cellulose, the degree of exposure of which increases during milling, the surface of the wet milled product can be modified and / or altered, and new material properties can be imparted to the wet milled product. Examples of material properties that can be imparted to the wet milled product by surface modification and / or alteration include modification of the association and aggregation properties between wet milled products, imparting hydrophilic or hydrophobic properties, imparting positive or negative charges to the surface, imparting antibacterial properties, and modifying the structure and function by binding other molecules that recognize the characteristic structure of polysaccharides.

[0064] Since the defibrability of the herbaceous fibrous material is improved by the acid treatment process, defibration can be carried out efficiently in the subsequent wet grinding process. As a result, the herbaceous fibrous material exhibits a defibrated mechanical pulp-like structure, occupies a wide space, and can form a network structure, which gives rise to a bulky precipitate when suspended in water and allowed to stand.

[0065] In addition, since the enzymatic saccharification property of the polysaccharides of the herbaceous fiber material is significantly improved by the acid treatment process, by continuing the wet grinding process, it becomes possible to easily prepare nano-sized wet-ground material with particle sizes of less than 1 μm.

[0066] The "step of fractionating and recovering a fraction mainly composed of wet-ground material having a particle size of less than 1 μm from the wet-ground material obtained by the wet-ground process" is a step of recovering the wet-ground material that has been pulverized to nano size in the wet-ground process so that it can be used as a raw material for functional materials such as the above-mentioned plastics and boards. The fractionation means is not particularly limited, and for example, a method such as fractionation by particle size using a mesh or filter, or fractionation with a precipitate based on the dispersion characteristics in water or a dispersion medium can be applied. In addition, "mainly composed of wet-ground material having a particle size of less than 1 μm" means that the concentration is sufficient to significantly express the characteristics of particles having a particle size of less than 1 μm, for example, 50% or more.

[0067] The "step of modifying and / or altering at least a part of the surface of the wet-ground product" is a step that can be added when a step of modifying and / or altering at least a part of the surface of the wet-ground product is provided separately from the wet-ground product step, such as the wet-ground product treatment performed by adding the polysaccharide described above. This step can be performed at any stage in the present production method. For example, this step can be performed during wet-ground product, after the wet-ground product step, or between the acid treatment step and the wet-ground product step. This step can be, for example, a step of physically adsorbing the polysaccharide described above onto the surface of the wet-ground product.

[0068] As described above, the "acid treatment step" in this embodiment is positioned as a pre-defibration treatment step for improving the defibration property of the herbaceous fiber raw material to be subsequently defibrated. Therefore, this embodiment also provides a pre-defibration method characterized in that the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water. EXAMPLES

[0069] The present embodiment will now be described in detail with reference to examples.

[0070] Example 1: Liquid-phase treatment of 1 g of coarsely ground rice straw, bagasse, Miscanthus sinensis, and Erianthus As herbaceous fiber raw materials, rice straw powder (grinding degree 4mm or less, moisture content 9.7%), sugarcane bagasse powder (grinding degree 2mm or less, moisture content 1.1%), Miscanthus sinensis powder (grinding degree 2mm or less, moisture content 3.3%) and Erianthus powder (grinding degree 2mm or less, moisture content 7.3%) were used and subjected to acid treatment (liquid phase treatment), and the reduction rate of glucan and xylan content was investigated.

[0071] (1) Acid treatment (liquid phase treatment) test 1.00 g of each of the above raw materials was weighed out and placed in a plastic tube. 10 mL of hydrochloric acid-calcium chloride aqueous solution (hydrochloric acid concentration 1 mol / L, calcium chloride concentration 4 mol / L) was added to each raw material, and the raw materials were immersed at room temperature (25±5°C, the same applies below), and the tubes were closed and left to stand for 18 hours to carry out acid treatment. At this point, each raw material was completely immersed in the aqueous solution.

[0072] (2) Measurement of glucan and xylan content The acid-treated sample was placed on a Buchner funnel with filter paper, washed with 200 mL of ion-exchanged water, and the solid on the filter paper was collected. The solid was dried in an oven at 105°C until it reached a constant weight, and then returned to room temperature and the dry weight was measured. The sample (above solid) was then finely ground using a ball mill crusher (MM301, Verder Scientific Co., Ltd.), and the glucan and xylan amounts in the sample were measured according to the method of the National Renewable Energy Laboratory (Sluiter, A., Hames, B., Ruiz, R., Scarlata, C., Sluiter, J., Templeton, D., Crocker, D., Determination of structural carbohydrates and lignin in biomass, laboratory analytical procedure. National Renewable Energy Laboratory, Golden, CO,USA. (2008)). The glucan and xylan amounts in the raw material before acid treatment were also measured in the same manner.

[0073] That is, according to the method of the National Renewable Energy Laboratory, 20 mg of the sample was thoroughly mixed with 1 mL of 72% (w / w) sulfuric acid and left to stand at 30 ° C. for 1 hour. Then, 0.15 mL of this mixture was mixed with 1.05 mL of ion-exchanged water and treated at 100 ° C. for 2 hours to perform acid hydrolysis. This acid hydrolyzate was centrifuged at 10,000 × g for 10 minutes, 1 mL of the supernatant was taken out, and 1 mL of calcium carbonate suspension (a suspension of 1 g of calcium carbonate in 3 mL of ion-exchanged water) was added to it to neutralize it. Using a part of this neutralized product, the amount of glucose was measured using Glucose CII-Test Wako (FUJIFILM Wako Pure Chemical Industries, Ltd.) and the amount of xylose was measured using D-Xylose Assay Kit (Megazyme Co., Ltd.), and the amount of linear glucan and the amount of linear xylan were calculated, respectively. The moisture content was calculated as a percentage by subtracting the bone-dry weight (weight of the sample dried at 105°C until it reached a constant weight and then returned to room temperature) from the air-dry weight of the sample.

[0074] (3) Results As a result, as shown in Table 1, in the herbaceous fiber material obtained after acid treatment, the reduction rate of the glucan content was within 4% and the reduction rate of the xylan content was within 30% compared to the composition of the herbaceous fiber raw material (before acid treatment). In addition, the sample recovery rate after acid treatment was 77% or more.

[0075] The reason why some treatments have a higher glucan content after acid treatment than before is that glucan is relatively stable to acid treatment, whereas components other than glucan are dissolved by acid treatment, resulting in an increase in the ratio of glucan to the total amount of the sample. On the other hand, xylan has low crystallinity and is easily solubilized by acid treatment, so that conventional acid treatment involving heating easily hydrolyzes xylan down to monosaccharides. Thus, by carrying out the acid treatment of the present disclosure on herbaceous fiber raw materials, it was possible to obtain herbaceous fiber materials in which the solubilization of xylan was suppressed.

[0076] [Table 1] *Dry weight of sample before and after acid treatment, respectively **Calculated as {(Content before acid treatment - Content after acid treatment) / Content before treatment} x 100 (%). *** Calculated as (dry weight of sample after acid treatment / dry weight of sample before acid treatment) x 100 (%). ****Calculated as (amount of linear glucan or linear xylan in sample / dry weight of sample) x 100 (%).

[0077] Example 2: Liquid-phase treatment and wet-grinding treatment of 0.05 g of coarsely ground rice straw, bagasse, Miscanthus sinensis, and Erianthus As herbaceous fiber raw materials, rice straw powder (grinding degree 4mm or less, moisture content 9.7%), sugarcane bagasse powder (grinding degree 2mm or less, moisture content 1.1%), Miscanthus sinensis powder (grinding degree 2mm or less, moisture content 3.3%) and Erianthus powder (grinding degree 2mm or less, moisture content 7.3%) were used, and acid treatment (liquid phase treatment) and wet grinding treatment were performed.

[0078] (1) Acid treatment (liquid phase treatment) test 50 mg of each of the above raw materials was weighed out and placed in a 2 mL plastic tube. Two types of zirconia beads (Nikkato, 500 mg of 0.6 mm diameter and one 5 mm diameter) were added to this, and 400 μL of hydrochloric acid-calcium chloride aqueous solution (hydrochloric acid concentration 1 mol / L, calcium chloride concentration 4 mol / L) was added and mixed, and the tube was sealed and left to stand at room temperature for 18 hours to perform acid treatment. At this time, each raw material was completely immersed in the aqueous solution. As a control, the same amount of the above raw materials was treated in the same way by adding calcium chloride aqueous solution (4 mol / L) instead of hydrochloric acid-calcium chloride aqueous solution.

[0079] (2) Wet grinding test The tube after the above treatment was centrifuged at room temperature (12,000×g for 5 minutes) to remove the supernatant, and then 2 mL of ion-exchanged water was added and the tube was inverted upside down to wash the solid matter (herbaceous fiber material), and centrifuged again (12,000×g for 5 minutes) to remove the supernatant. This washing procedure was repeated three more times. After that, ion-exchanged water was added to the tube to adjust the total weight with the sample (total weight of the tube contents) to 1 g, and the tube was placed in a bead grinding device (Micro Smash MS-100R, TOMY Co., Ltd.) and ground at room temperature at 4000 rpm for 20 seconds x 6 times to perform wet grinding treatment.

[0080] (3) Measurement of sediment volume The volume of the precipitate was measured for the sample (wet-milled product) obtained after the above treatment. That is, the contents of the tube after the wet-milling treatment were suspended in a small amount of ion-exchanged water together with the zirconia beads, transferred to a 15 mL plastic tube, and further ion-exchanged water was added to the tube to increase the apparent liquid volume to 5 mL. The tube was stirred for 30 seconds with a vortex mixer to suspend the sample, and then left to stand at room temperature for 1 hour, resulting in the formation of a precipitate. The apparent volume occupied by the precipitate was measured using the scale on the plastic tube. The apparent volume occupied by the sample (wet-milled product) in the above precipitate was calculated by subtracting (0.25 mL) from the measured value.

[0081] (4) Measurement of enzymatic saccharification rate In addition, the enzymatic saccharification rate of glucan by fibrous enzymes was measured for the sample (wet-milled product) obtained after the above treatment. That is, a cellulase preparation (Cellic CTec2, Novozymes) and a β-glucosidase preparation (Novozyme 188, Novozymes) were used as fibrous enzymes. 100 mM (final concentration) of sodium acetate buffer (pH 5.0), 0.6 FPU (final amount) of cellulase preparation, and 0.6 CbU (final amount) of β-glucosidase preparation were added to the sample in a 2 mL plastic tube after the wet-milling treatment. In addition, sodium azide (Nacalai Tesque) 0.05% (w / v) (final concentration), chloramphenicol (Nacalai Tesque) 50 μg / ml (final concentration), and tetracycline (Nacalai Tesque) 50 μg / ml (final concentration) were added to prevent microbial growth during saccharification. Ion-exchanged water was further added to the tube to adjust the total volume to 1 mL, and the tube was sealed, and the saccharification reaction was carried out at 50°C for 48 hours while inverting the tube. After the reaction, the sample temperature was returned to room temperature, and a portion of the sample was used to perform acid hydrolysis of the saccharification solution according to the method described in paragraph 0071, and the amount of free glucose was measured using a Glucose CII-Test Wako (FUJIFILM Wako Pure Chemical Industries, Ltd.). In addition, the total glucan amount of each herbaceous fiber raw material was measured by the method described in Example 1 (2). The glucose release rate (enzymatic saccharification rate) was calculated by dividing the value obtained by converting the amount of free glucose measured above into the amount of glucan by the total amount of glucan in the raw material.

[0082] (5) Results The results are shown in Tables 2, 3 and 2. As shown in Table 2 and FIG. 2A, the volumes of the precipitates of the wet-ground products of rice straw, sugarcane bagasse, Miscanthus sinensis and Erianthus increased by 5, 3, 5.7 and 3.6 times, respectively, compared to the control. In addition, as shown in Table 3 and FIG. 2B, the enzymatic saccharification rates of the wet-ground products increased by 1.9, 2.7, 2.1 and 3.4 times, respectively, compared to the control. Thus, it was shown that the pulverized products obtained by subjecting herbaceous fiber raw materials to the acid treatment of the present disclosure and then wet-pulverizing them gave bulky precipitates when suspended in water and allowed to stand, and that the enzymatic saccharification rate of glucan by fibrous enzymes was improved.

[0083] [Table 2]

[0084] [Table 3] *Calculated as [amount of glucan converted from the amount of free glucose / total amount of glucan in raw material] x 100 (%).

[0085] Example 3: Gas-phase treatment of 0.05 g of coarsely ground rice straw, sugarcane bagasse, Miscanthus sinensis, and Erianthus As herbaceous fiber raw materials, rice straw powder (grinding degree 4mm or less, moisture content 9.7%), sugarcane bagasse powder (grinding degree 2mm or less, moisture content 1.1%), Miscanthus sinensis powder (grinding degree 2mm or less, moisture content 3.3%) and Erianthus powder (grinding degree 2mm or less, moisture content 7.3%) were used, and acid treatment (vapor phase treatment) and wet grinding treatment were performed.

[0086] (1) Acid treatment (vapor phase treatment) test 50 mg of each of the above raw materials was weighed out and placed in a 2 mL plastic tube. As shown in Figure 3, 100 μL of hydrochloric acid-calcium chloride aqueous solution (hydrochloric acid concentration 1 mol / L, calcium chloride concentration 4 mol / L) was placed as a droplet in the same tube so as not to come into contact with the raw materials. The tube was then capped and left to stand at room temperature for 96 hours, thereby carrying out acid treatment. As a control, the same amount of raw material was left to stand for 96 hours without adding the hydrochloric acid-calcium chloride aqueous solution.

[0087] (2) Wet grinding test After removing the droplets from the tube after the above treatment, 950 μL of ion-exchanged water was added. Zirconia beads (Nikkato, 500 mg of 0.6 mm diameter and one 5 mm diameter) were added to the tube, and the tube was placed in a bead grinding device (Micro Smash MS-100R, TOMY) and crushed at room temperature and 4000 rpm for 20 seconds x 6 times to perform wet crushing treatment. A portion of the resulting wet crushed material was collected and observed at 200x magnification using a microscope (BX51, Olympus) (Figure 1C, white bar: 0.05 mm). Figure 1C shows that the tissue became fluffy due to the crushing treatment.

[0088] (3) Measurement of sediment volume and its results The sediment volumes of the samples (wet-ground products) obtained after the above treatment were measured by the method described in (3) of Example 2. As a result, as shown in Table 4, the apparent volumes of the sediments of the wet-ground products of rice straw, sugarcane bagasse, Miscanthus sinensis, and Erianthus increased by 3.7 times, 2.8 times, 6.3 times, and 2.2 times, respectively, compared to the control.

[0089] [Table 4]

[0090] Example 4: Liquid-phase treatment and wet-grinding treatment of 10 g of coarsely ground rice straw Rice straw powder (fineness of crushing: 4mm or less, moisture content: 9.7%) was used as a herbaceous fiber material and was subjected to acid treatment (liquid phase treatment) and wet grinding treatment.

[0091] (1) Acid treatment (liquid phase treatment) test 10 g of the above raw material was weighed into a plastic tube, and 40 mL of hydrochloric acid-calcium chloride aqueous solution (hydrochloric acid concentration 1 mol / L, calcium chloride concentration 4 mol / L) was added to immerse the raw material in the aqueous solution. The tube was sealed and left to stand at room temperature for 18 hours to carry out acid treatment (liquid phase treatment). At this time, the raw material was completely immersed in the aqueous solution. As a control, the same treatment was carried out using 40 mL of water instead of the hydrochloric acid-calcium chloride aqueous solution.

[0092] (2) Wet grinding test The acid-treated sample was filtered through a Buchner funnel with filter paper placed therein, and the solid matter collected as the non-passed matter was washed with 200 ml of ion-exchanged water and then collected. Of the collected sample, 300 mg of the dried matter was suspended in 50 ml of ion-exchanged water and crushed with a Polytron (PT1200E, KINEMATICA) at room temperature for 60 seconds, thereby carrying out wet grinding treatment.

[0093] (3) Measurement of sediment volume and its results From the sample after the wet grinding treatment, the water-insoluble fraction was collected and dispersed in 30 mL of ion-exchanged water. While vigorously stirring this dispersion, 5 mL was collected using a glass pipette with a large tip hole and transferred to a 15 mL plastic tube. The volume of the precipitate was then measured using the method described in (3) of Example 2. As a result, as shown in Table 5, the apparent volume of the precipitate in the wet-ground sample was 3.5 times higher than that in the control group.

[0094] [Table 5]

[0095] (Example 5) Effect of composition of mixed aqueous solution used in liquid phase treatment Rice straw powder (fineness of grinding: 4 mm or less, moisture content: 9.7%) was used as a herbaceous fiber material, and acid treatment (liquid-phase treatment) was performed using mixed aqueous solutions of different compositions to investigate the effect on the enzymatic saccharification rate of the wet-ground material.

[0096] (1) Acid treatment (liquid phase treatment) test and wet grinding test The raw material was subjected to acid treatment in the same manner as in Example 2(1) except that an aqueous solution of hydrochloric acid-magnesium chloride (hydrochloric acid concentration: 1 mol / L, magnesium chloride concentration: 4 mol / L) or an aqueous solution of hydrochloric acid-ammonium chloride (hydrochloric acid concentration: 1 mol / L, ammonium chloride concentration: 5.56 mol / L) was used instead of an aqueous solution of hydrochloric acid-calcium chloride. However, in the aqueous solution of hydrochloric acid-ammonium chloride, the immersion time was extended from 18 hours (Example 2) to 66 hours. The sample (herbaceous fibrous material) after the acid treatment was then washed and wet-pulverized in the same manner as in Example 2(2).

[0097] (2) Measurement of enzymatic saccharification rate The sample (wet-pulverized product) prepared as above was subjected to an enzymatic saccharification reaction in the same manner as in (4) of Example 2, and the enzymatic saccharification rate of glucan was measured. As a control, the same treatment was carried out using 1 mol / L hydrochloric acid instead of the hydrochloric acid-magnesium chloride aqueous solution and the hydrochloric acid-ammonium chloride aqueous solution.

[0098] (3) Results As a result, as shown in Table 6, in the treatment areas with the hydrochloric acid-magnesium chloride aqueous solution and the hydrochloric acid-ammonium chloride aqueous solution, the saccharification rate of total glucan increased by 1.9 times and 1.6 times, respectively, compared to the control. This suggests that changing the type of "electrolyte other than hydrochloric acid that liberates chloride ions in water" contained in the mixed aqueous solution used for acid treatment also has the effect of improving the enzymatic saccharification rate of glucan.

[0099] [Table 6] *Calculated as [amount of glucan converted from the amount of free glucose / total amount of glucan in raw material] x 100 (%).

[0100] (Example 6) Wet grinding test with added polysaccharide Rice straw powder (fineness of grinding: 4 mm or less, moisture content: 9.7%) was used as the herbaceous fiber material, and liquid-phase processing and wet-grinding processing with the addition of different polysaccharides were performed, and the apparent volume of the precipitate of the wet-grinding product was examined. The polysaccharides used were chitosan (Chitosan 100, Fujifilm Wako Pure Chemical Industries), tamarind seed gum (Tamarind gum (derived from tamarind seed), Tokyo Chemical Industry Co., Ltd.), and gellan gum (Gellan gum, Fujifilm Wako Pure Chemical Industries).

[0101] (1) Acid treatment (liquid phase treatment) test and wet grinding test The above raw materials were subjected to acid treatment and water washing in the same manner as in (1) and (2) of Example 2. Next, ion-exchanged water (polysaccharide-free group), or chitosan, tamarind seed gum, or gellan gum was added to the sample (herbaceous fiber material) to a final concentration of 0.2% (w / v), and then wet-grinding was performed in the same manner as in (2) of Example 2. The control group was treated in the same manner, except that the acid treatment was performed using a calcium chloride aqueous solution (4 mol / L) instead of the hydrochloric acid-calcium chloride aqueous solution.

[0102] (2) Measurement of sediment volume and its results The volumes of the precipitates of the samples (wet-pulverized products) prepared as described above were measured and compared using the method of Example 2(3). As a result, as shown in Table 7, the apparent volumes of the precipitates in the polysaccharide-free group and the groups with chitosan, tamarind seed gum, and gellan gum added were 4.3 times, 2.7 times, 4.3 times, and 4.1 times, respectively, compared to the control group. Thus, it was shown that when wet-pulverization was performed with the addition of polysaccharides, bulky precipitates were obtained, similar to the case of no polysaccharide addition.

[0103] By adding polysaccharides to a sample and carrying out wet grinding, the polysaccharides are chemically or physically bound to at least a part of the surface of the wet-ground product, making it possible to modify and / or alter the surface. When surface modification or alteration is carried out with chitosan, it is possible to impart properties such as antibacterial properties and anionic coagulation properties to the wet-ground product. In the case of tamarind seed gum and gellan gum, it is possible to impart properties such as modification of the dispersion properties and modification of the cellulose decomposition properties of the wet-ground product. In the case of other polysaccharides, it is expected to contribute to the modification of physical properties, modification of biorecognition properties, imparting a charge, and stabilization of material properties during freezing and drying.

[0104] [Table 7]

[0105] (Example 7) Wet grinding process using a ball mill Rice straw powder (fineness of crushing: 4mm or less, moisture content: 9.7%) was used as a herbaceous fiber material, and liquid-phase treatment and wet-milling treatment using a ball mill were carried out, and the apparent volume of the precipitate of the wet-milled material was investigated.

[0106] (1) Acid treatment (liquid phase treatment) test 1 g of the above raw material was weighed into a plastic tube, and 8 mL of hydrochloric acid-calcium chloride aqueous solution (hydrochloric acid concentration 1 mol / L, calcium chloride concentration 4 mol / L) was added to bring the raw material into contact with the aqueous solution. At this time, the raw material was completely immersed in the aqueous solution. The tube was sealed and left to stand at room temperature for 18 hours to carry out acid treatment (liquid phase treatment). As a control, the same treatment was carried out using hydrochloric acid aqueous solution (1 mol / L) instead of the hydrochloric acid-calcium chloride aqueous solution.

[0107] (2) Wet grinding test The sample (herbaceous fiber material) after the above treatment was placed on a Buchner funnel with filter paper set in it, and washed with a sufficient amount of ion-exchanged water. The washed solid was divided into two equal parts, each of which was suspended in 10 mL of ion-exchanged water, and sealed in a 50 mL stainless steel jar together with a stainless steel ball with a diameter of 2 cm. This was then ground in a ball mill (Mixer Mill MM400, Verder Scientific, 15 strokes / second, 4 minutes) to perform wet grinding treatment.

[0108] (3) Measurement of sediment volume and its results The sample (wet-milled product) after the above treatment was added to a 50 mL measuring cylinder, and the total volume was adjusted to 50 mL using ion-exchanged water, and then thoroughly suspended. After standing for 1 hour, the apparent volume of the precipitate of the wet-milled product was measured. As a result, as shown in Table 8, the apparent volume of the precipitate in the hydrochloric acid-calcium chloride aqueous solution treatment group (average value of two samples) was 3.4 times that of the control group.

[0109] [Table 8]

[0110] (Example 8) Plate made from wet-ground material For the rice straw treatment samples (2 samples) after ball milling prepared in Example 7, the sediment volume was measured, and 10 mL of the supernatant was removed to make 40 mL. The resulting solution was centrifuged at 6,320×g for 1 minute, after which the supernatant was discarded and the sediment was collected. The collected wet-pulverized product was dried at 60°C to reduce the moisture content to about 80%, and then molded into a plate. That is, a part of the dried wet-pulverized product was added to a disk-shaped heat press mold φ14 (1-6002-18, AS ONE Corporation) with an inner diameter of 14 mm, and heated from room temperature to 160°C at 20 MPa (equivalent value of diameter 5.5 cm), and then maintained at 160°C for 20 minutes to perform drying and compression treatment, and then air-cooled to return to room temperature. As a result, a plate-shaped molded product as shown in FIG. 4 was obtained. This molded product had a diameter of 14 mm, a thickness of 3 mm, and a density of 1.24 g / cm 3 It became.

[0111] (Example 9) Sheet (nonwoven fabric) made from wet-ground material The rice straw sample after polytron crushing prepared in Example 4 was adjusted to a concentration of 1% (w / v) in terms of raw material, and 40 mL of the sample was taken and centrifuged at 6,320 x g for 1 minute, after which the supernatant was discarded and the precipitate was collected. The collected wet crushed material was made up to 20 mL with ion-exchanged water, and then stirred to make a suspension. 10 mL of the suspension was poured into a plastic petri dish with a diameter of 10 cm and left to dry at 50 ° C for 12 hours or more to obtain a sheet-like molded product (nonwoven fabric) (Figure 5). As shown in Figure 5, it was found that the defibrated herbaceous fibrous material was bonded to each other and molded into a sheet.

[0112] (Example 10) Forming of plate using wet-ground material and evaluation of properties Rice straw powder (fineness of grinding: 4 mm or less, moisture content: 9.7%) was used as the herbaceous fiber raw material, and liquid-phase processing and wet-grinding processing were performed using a single-axis wet grinder. The resulting wet-grinding material was compressed into a plate shape and dried to obtain a sample, whose properties were evaluated.

[0113] 1 kg of the rice straw powder was mixed with 2 L of hydrochloric acid-calcium chloride aqueous solution (hydrochloric acid concentration 1 mol / L, calcium chloride concentration 4 mol / L) in a plastic bag and left to stand at room temperature for 16 hours to obtain a herbaceous fiber material. As a control, the same amount of calcium chloride aqueous solution (calcium chloride concentration 4 mol / L) was used instead of the hydrochloric acid-calcium chloride aqueous solution and treated under the same conditions.

[0114] The treated sample (herbaceous fibrous material) was neutralized by adding 25% (w / w) aqueous ammonia solution, and then washed with tap water. The excess water was then squeezed out to produce a wet solid, which was then wet-pulverized using a single-shaft wet grinder (Shokusenki: Kobe Steel Engineering Co., Ltd.) to obtain 17.3 g (moisture content 71.1%) of "acid-treated pulverized sample." The control was treated in the same way as above without adding the aqueous ammonia solution, and 19.7 g (moisture content 69.1%) of "control pulverized sample" was obtained.

[0115] The acid-treated crushed sample and the control crushed sample obtained above were each laid out in a 70mm x 70mm plate-making mold with a 69mm x 69mm cooking sheet (manufactured by ZHI JIN HOME Co., Ltd.) placed underneath. The mold was then pressurized at 10MPa for 5 minutes, the seeped liquid was wiped off, and the mold was dried at 105°C for 12 hours. The mold was then pressurized at 20MPa for 10 minutes, and the obtained plate-shaped sample was removed from the mold.

[0116] The density of the obtained plate-shaped sample was measured by measuring the mass and volume, and then a small piece of 20 mm x 20 mm was prepared and the weight and thickness were measured. The small piece was then immersed in 20 mL of distilled water at room temperature, and after 12 hours, it was taken out and drained on a paper towel for 5 seconds, and the weight and thickness were measured again. The water absorption thickness swelling rate (TS) and water absorption rate (WA) were calculated using the following formulas (I) and (II).

[0117]

number

[0118]

number

[0119] The results are shown in Table 9. The density of the acid-treated plate sample was 0.70 g / cm 3 The value of the control plate sample (0.58 g / cm 3 ) and it was confirmed that the samples were more consolidated than the samples in the control group. The TS and WA values ​​were 10.1% and 85.2%, respectively, for the acid-treated plate samples, and 23.3% and 121%, respectively, for the control plate samples. These results confirmed that the hydrochloric acid treatment produced a stable molded product that was less likely to swell in water. [Table 9]

[0120] The plate-shaped sample prepared in the mold was torn by hand and then dry-pulverized in a blender (Force Mill, manufactured by Osaka Chemical Industry Co., Ltd.) for 10 seconds x 4 times. This dry-pulverized material (50 mg) was directly or further wet-pulverized in the presence of zirconia beads according to the method of Example 2, and then subjected to enzymatic saccharification according to the method of Example 2 to evaluate the release rates of glucose and xylose. The amounts of glucose residues and xylose residues contained in the acid-treated pulverized sample and the control pulverized sample in this example were used as denominators when measuring the release rates.

[0121] The results are shown in Table 10. The glucose release rates of the acid-treated pulverized sample, the sample obtained by processing the same sample into a plate and then dry-pulverizing it (acid-treated dry-pulverized sample), and the sample obtained by wet-pulverizing it with zirconia beads (acid-treated wet-pulverized sample) were 79.0%, 45.4%, and 76.6%, respectively, and the xylose release rates were 66.4%, 42.2%, and 76.8%, respectively. The glucose release rates of the control pulverized sample, the sample obtained by processing the same sample into a plate and then dry-pulverizing it (control dry-pulverized sample), and the sample obtained by wet-pulverizing it with zirconia beads (control wet-pulverized sample) were 29.7%, 25.0%, and 30.9%, respectively, and the xylose release rates were 11.5%, 16.7%, and 24.5%, respectively. Thus, the acid-treated crushed sample before processing into plates showed high glucose and xylose release rates during enzymatic saccharification, whereas the values ​​decreased in the dry-crushed sample after processing into plates. Furthermore, the glucose and xylose release rates were largely restored by wet-crushing. This increase in the sugar release rate was limited in the control crushed sample. It became clear that the material could be reused as a saccharification raw material by applying an appropriate crushing process after processing into plates.

[0122] [Table 10]

[0123] (Example 11) Production and saccharification of herbaceous fiber material 2.22 g of rice straw powder (fineness of crushing 4 mm or less, moisture content 9.7%) was taken and placed in the bottom of a 200 ml glass bottle (mouth inner diameter × body diameter × height: φ47 × φ62 × 109 mm, Figure 6) together with a magnetic stirrer (length 30 mm, φ5 mm). Four pieces of sponge 10 mm thick and 30 mm long were attached to the inside of the glass bottle with double-sided tape, and a polypropylene dish φ42 mm and depth 15 mm was placed on top of them and held at a height of 70 mm from the bottom. 10 mL of hydrochloric acid-calcium chloride aqueous solution (hydrochloric acid concentration 1 mol / L, calcium chloride concentration 4 mol / L) was added on top of the dish, and the glass bottle was sealed with the lid. The bottle was placed on a magnetic stirrer and stirred at room temperature at 20 revolutions per minute for 3 days. The lid of the glass bottle was then opened, the dish was removed, and the rice straw powder sample after gas-phase treatment was collected. Approximately 1 g of the sample was weighed onto a weighed aluminum dish and dried at 105°C for 18 hours, after which the moisture content was measured, which was found to be 10.4%.

[0124] 55 mg of rice straw powder after gas phase treatment was weighed into four 2 mL plastic tubes, and 1.5 mL of ion-exchanged water was added to two tubes, and the tubes were washed three times as in Example 2 to prepare washed samples. The remaining two tubes were not washed and prepared as non-washed samples. For the washed samples, zirconia beads (equivalent to 500 mg of 0.6 mm diameter beads and one 5 mm diameter bead) from Example 2 were added to each tube, and then ion-exchanged water was added to adjust the total weight of the samples to 1 g as in Example 2, and the samples were wet-pulverized using a bead crusher (acid-treated and washed samples). For the non-washed samples, 950 μL of ion-exchanged water was added to each tube (pH adjustment), and zirconia beads were added, and the samples were wet-pulverized using a bead crusher as in Example 3 (acid-treated and non-washed samples). For the control, rice straw powder before acid treatment was used, and the same wet-pulverization procedure as for the acid-treated and non-washed samples was performed (untreated and non-washed samples).

[0125] These wet-ground samples were transferred to 15 mL plastic tubes and the precipitate volume was measured after adding water according to the method of Example 2. The results are shown in Table 11. The values ​​in the table are the average values ​​of the results for two samples under each condition. The volume was 2.85 mL for the acid-treated and washed sample, 2.5 mL for the acid-treated and unwashed sample, and 0.75 mL for the untreated and unwashed sample. Thus, it was confirmed that the gas-phase acid-treated sample using a glass bottle also became a bulky suspension after wet-ground. The hydrochloric acid-calcium chloride aqueous solution used in the reaction under non-contact conditions can be heated to evaporate hydrogen chloride gas and water, and separated, thereby increasing the calcium chloride concentration in the aqueous solution and allowing calcium chloride to be reused or recycled.

[0126] [Table 11] *Values ​​are the average of two samples

[0127] The samples after the bead-crushing treatment obtained above (acid-treated / washed sample, acid-treated / unwashed sample, and untreated / unwashed sample) were subjected to enzymatic saccharification and the amounts of liberated glucose and liberated xylose were measured by the method of Example 2. Using these values, the glucose liberation rate and xylose liberation rate relative to the total glucan amount and total xylan amount in the rice straw powder before acid treatment were calculated as the average value of the results for two samples under each condition.

[0128] The results are shown in Table 12. The glucose release rates of the acid-treated / washed sample, the acid-treated / unwashed sample, and the untreated / unwashed sample were 69.5%, 76.0%, and 35.0%, respectively, and the xylose release rates were 46.9%, 110%, and 11.6%, respectively. Thus, it was confirmed that the samples obtained by gas-phase acid treatment showed a high saccharification rate. In addition, the sugar recovery rate was improved by using the unwashed sample compared to the washed sample. The unwashed sample contained functional components such as xylooligosaccharides, which are partial hydrolysates of xylan by acid, because it was not washed and pH was adjusted by adding water. Therefore, it is considered possible to produce industrially useful materials with high sugar recovery rates and value as functional feed by minimizing runoff due to washing and controlling the effects of acid by removing hydrogen chloride by heating, adjusting pH from the gas phase with ammonia, etc., and adjusting pH so as to leave washing water.

[0129] [Table 12] *Values ​​are the average of two samples

[0130] 1 g of the rice straw powder after the gas phase treatment obtained above was ball milled at 15 reciprocations / second for 4 minutes using the method described in Example 1. After drying the obtained fine powder at 105 ° C, 500 mg was transferred to a 15 mL plastic tube, 12 mL of ion-exchanged water was added, and the mixture was stirred by vortex for 5 minutes. The mixture was then centrifuged at 10,000 × g for 5 minutes, and the supernatant was removed by suction, for a washing treatment. The entire amount of the residue was transferred to a weighed aluminum dish with a diameter of 5 cm, dried at 105 ° C, and weighed to obtain 415 mg of washed residue. 20 mg of each of the sample before washing (rice straw powder after gas phase treatment) and the sample after washing (washed residue) were weighed, and the amount of glucan and xylan in the sample was measured using the method described in Example 1.

[0131] The results are shown in Table 13. The glucan and xylan amounts of the sample before washing were 164 mg and 53 mg, respectively, and the glucan and xylan amounts of the sample after washing were 151 mg and 37 mg, respectively. Thus, the glucan content relative to the total glucan and total xylan amounts in the rice straw powder before acid treatment increased from 32.8% to 36.3% by gas-phase treatment, and the xylan content decreased from 10.6% to 8.92% (a decrease rate of 15.8%). These results show that the acid treatment in the gas-phase treatment can obtain a herbaceous fiber material in which the solubilization of xylan is significantly suppressed. The herbaceous fiber material according to the present disclosure is a material with unprecedented functionality that combines seemingly contradictory structural characteristics of improved defibration and retention of polysaccharides, and has high industrial usefulness even before wet grinding.

[0132] [Table 13]

[0133] (Example 12) Molding of rod-shaped objects using wet-ground material 1.00 kg of the acid-treated crushed sample (moisture content 74.3%) prepared by the method described in Example 10 was weighed and packed into a mold for a bar. The mold is divided into three parts: a bottom part, a middle part, and an upper part. First, a cooking sheet (manufactured by ZHI JIN HOME) was laid on the bottom and sides of the tapered part of the bottom mold, and the sample was placed on it and filled while pressing by hand. When the bottom mold was filled, a middle mold was installed and the sample was similarly packed up in the middle part. When the middle part was filled to the top position, a silicon sheet was placed on the top and an upper mold was set on top of it. Next, the entire mold was pressurized at 10 MPa for 10 minutes, and then dried together with the mold at 105 ° C for 72 hours. Finally, the mold was returned to room temperature and further pressurized at 20 MPa for 5 minutes, and then the sample was removed from the mold to obtain a rod-shaped molded product.

[0134] A photograph of the molded product is shown in Figure 7. The size of the molded product is 5 mm in height at the bottom + 29 mm in the taper part, 66 mm x 180 mm in length x width at the bottom, 52 mm x 165 mm in length x width at the top, 289 g in weight, and 0.64 g / cm in density.3 By molding into a rod shape, it was possible to create a structure suitable for storing the wet-ground material. In this way, it was confirmed that rod-shaped moldings could be produced using the acid-treated ground sample.

[0135] Although the embodiment and examples of the present disclosure have been described in detail above, the specific configurations are not limited to these, and design changes that do not depart from the gist of the present disclosure are included in the present disclosure.

Claims

1. A herbaceous fiber material characterized in that, compared to the composition of the raw herbaceous fiber material, the glucan content (based on the dry matter, by weight %) is reduced by 30% or less, and the xylan content (based on the dry matter, by weight %) is reduced by 5% or more and 50% or less.

2. an acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10° C. and 50° C.; a step of washing and / or adjusting the pH of the treated product after the acid treatment step; The herbaceous fiber material according to claim 1, which is produced by a method comprising the steps of:

3. The herbaceous fiber material according to claim 2, characterized in that the mixed aqueous solution contains one or more electrolytes selected from calcium chloride, magnesium chloride, and ammonium chloride dissolved therein as an electrolyte other than hydrochloric acid that liberates chloride ions in water, or contains a solute substantially equivalent to that of an aqueous solution in which the electrolytes are dissolved.

4. The herbaceous fiber material according to claim 1, characterized in that the herbaceous fiber raw material is one or more selected from the group consisting of rice straw, wheat straw, corn stover, sugarcane bagasse, sugarcane trash, Miscanthus sinensis, Miscanthus japonica, Erianthus, sorghum, Napier grass, Judea japonica, Danchiku, and hemp.

5. an acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10° C. and 50° C.; a wet-grinding step in which the treated product that has been subjected to the acid treatment step is subjected to a wet-grinding step; A wet-ground herbaceous fibrous material produced by a method comprising: Compared with a wet-ground product obtained by the same method except that the acid treatment step was not performed on the raw herbaceous fiber material, The wet-ground product of herbaceous fibrous material is characterized in that the apparent volume of the precipitate obtained when the wet-ground product is suspended in water and allowed to stand at room temperature for one hour or more is at least twice as large, and / or the saccharification rate of glucan when the wet-ground product is treated with a fibrous decomposition enzyme is at least 1.5 times as large.

6. The wet-ground herbaceous fiber material described in claim 5 is characterized in that, compared to the composition of the raw herbaceous fiber material, the reduction rate of the glucan content (based on the dry matter, weight %) is 30% or less, and the reduction rate of the xylan content (based on the dry matter, weight %) is 5% or more and 50% or less.

7. The wet-ground herbaceous fiber material described in claim 5, characterized in that the mixed aqueous solution contains one or more electrolytes selected from calcium chloride, magnesium chloride, and ammonium chloride dissolved therein as an electrolyte other than hydrochloric acid that liberates the chloride ions in water, or contains a solute substantially equivalent to that of an aqueous solution in which the electrolytes are dissolved.

8. The wet-ground herbaceous fiber material according to claim 5, characterized in that the herbaceous fiber raw material is one or more selected from the group consisting of rice straw, wheat straw, corn stover, sugarcane bagasse, sugarcane trash, Miscanthus sinensis, Miscanthus japonica, Erianthus, sorghum, Napier grass, Judea japonica, Danchiku, and hemp.

9. 6. The wet-pulverized herbaceous fiber material according to claim 5, characterized in that in the wet-pulverization step, one or more polysaccharides selected from the group consisting of chitosan, xyloglucan, sodium carboxymethylcellulose, alginate, galactomannan, gellan gum, carrageenan, and (1-3),(1-4)-β-glucan are added to the treated product that has been subjected to the acid treatment step.

10. 6. The wet-ground herbaceous fibrous material according to claim 5, wherein at least a portion of the surface of the wet-ground material has been modified and / or altered.

11. 6. The wet-ground herbaceous fibrous material according to claim 5, comprising a wet-ground material having a particle size of less than 1 μm.

12. an acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10° C. and 50° C.; a step of washing and / or adjusting the pH of the treated product after the acid treatment step; A method for producing a herbaceous fiber material, comprising:

13. an acid treatment step in which the herbaceous fiber raw material is treated in a hydrogen chloride gas atmosphere or contacted with a mixed aqueous solution containing hydrochloric acid and an electrolyte other than hydrochloric acid that liberates chloride ions in water at a temperature substantially between 10° C. and 50° C.; a wet-grinding step in which the treated product that has been subjected to the acid treatment step is subjected to a wet-grinding step; A method for producing a wet-ground herbaceous fibrous material, comprising:

14. 14. The method according to claim 12 or 13, wherein the mixed aqueous solution dissolves one or more electrolytes selected from calcium chloride, magnesium chloride, and ammonium chloride as an electrolyte other than hydrochloric acid that liberates chloride ions in water, or contains a solute substantially equivalent to that of an aqueous solution in which the electrolyte is dissolved.

15. 14. The method according to claim 12 or 13, wherein the herbaceous fiber raw material is at least one selected from the group consisting of rice straw, wheat straw, corn stover, sugarcane bagasse, sugarcane trash, Miscanthus sinensis, Miscanthus versicolor, Erianthus, sorghum, Napier grass, Judea japonica, Danchiku, and hemp.

16. The method according to claim 13, characterized in that in the wet grinding step, one or more polysaccharides selected from the group consisting of chitosan, xyloglucan, sodium carboxymethylcellulose, alginate, galactomannan, gellan gum, carrageenan, and (1-3),(1-4)-β-glucan are added to the treated product that has been subjected to the acid treatment step.

17. The method according to claim 13, further comprising the step of modifying and / or altering at least a portion of the surface of the wet-ground material.

18. The method according to claim 13, further comprising a step of recovering a fraction mainly composed of wet-ground material having a particle size of less than 1 μm from the wet-ground material obtained in the wet-ground step.

19. A resin, plastic, rubber, ink or paint, characterized by containing a herbaceous fiber material according to any one of claims 1 to 4, or a wet-ground product of the herbaceous fiber material according to any one of claims 5 to 11, or a fraction thereof, or a modified and / or altered product thereof.

20. A paper, nonwoven fabric, fiber, seedling pot, board or three-dimensional molded product, characterized in that it contains the herbaceous fiber material according to any one of claims 1 to 4 or the herbaceous fiber material according to any one of claims 5 to 11, or a fraction thereof, or a modified and / or altered product thereof.

21. A saccharified raw material or feed, comprising a herbaceous fiber material according to any one of claims 1 to 4, or a wet-ground product of the herbaceous fiber material according to any one of claims 5 to 11, or a fraction thereof, or a modified and / or altered product thereof.

Citation Information

Patent Citations

  • Methods for producing microcrystalline cellulose

    JP2014511907A

  • Manufacturing method of glucan-containing composition

    JP2018104504A

  • Method for production of microcrystalline cellulose

    RU2281993C1

  • Jidomakiudedokei

    JP1976090858A