Polycrystalline silicon carbide substrate with density gradient and method of manufacturing the same
Polycrystalline SiC wafers with a density gradient address the limitations of uniform density SiC wafers by reducing costs and improving surface smoothness, enhancing device efficiency.
Patent Information
- Application Number
- JP2024054138
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-22
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-16
AI Technical Summary
The manufacturing of silicon carbide (SiC) wafers is limited by factors such as electrical and mechanical properties due to uniform density across the wafer, leading to increased costs and defects in electronic devices.
The development of polycrystalline SiC wafers with a density gradient, achieved through sintering processes and chemical vapor deposition, to create a smoother and more efficient surface for further layer formation.
The density gradient reduces manufacturing costs and improves surface smoothness, enhancing the bond strength between layers and reducing defects in electronic devices.
Smart Images

Figure 2024147517000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a polycrystalline silicon carbide (SiC) based substrate or wafer including a first density on a first side, a second density on a second side opposite the first side, and an increasing density gradient from the second side to the first side. [Background technology]
[0002] The semiconductor industry has shown considerable interest in silicon carbide (SiC), particularly for the manufacture of electronic devices or components (eg, diodes, transistors, or other similar power applications).
[0003] The development and manufacture of silicon carbide based electronic devices is limited by factors such as the electrical and mechanical properties of the silicon carbide wafers that are formed. Many silicon carbide wafers have a uniform (e.g., the same or substantially the same) density across the entire length, width, and thickness of the wafer.
[0004] The surface of the silicon carbide wafer may be planarized and polished to make the surface flat and smooth before bonding or forming additional layers on the silicon carbide wafer. For example, a silicon carbide wafer with a higher density will have smaller voids and potentially fewer voids, resulting in a smoother surface. However, a higher density wafer uses more material to increase density, which increases manufacturing costs. However, the higher density provides benefits to later manufacturing steps. Summary of the Invention
[0005] The present disclosure is directed to providing embodiments of a silicon carbide (SiC) wafer, which may be a polycrystalline SiC wafer, having a density gradient between a first side and a second side. The SiC wafer may be formed using a sintering process, followed by a temperature treatment to form the density gradient. Alternatively, the sintering process may be combined with chemical vapor deposition to form the density gradient.
[0006] At least one embodiment includes a polycrystalline SiC wafer or substrate having a first side and a second side opposite the first side. The first density is a density at the first side of the polycrystalline silicon carbide (SiC) material. The second density is a density at the second side of the polycrystalline silicon carbide (SiC) material, the second density being greater than the first density. A density gradient exists between the first side and the second side. The density of the density gradient can increase in a density gradient direction from the first side to the second side of the polycrystalline SiC wafer. [Brief description of the drawings]
[0007] For a better understanding of the embodiments, reference will now be made, by way of example, to the accompanying drawings, in which like reference numbers identify the same or similar elements or acts, unless the context dictates otherwise. The sizes and relative proportions of elements in the drawings are not necessarily drawn to scale. For example, some of these elements may be enlarged and positioned to improve the readability of the drawings. [Figure 1A] FIG. 1 illustrates a side perspective view of one embodiment of a polycrystalline silicon carbide (SiC) substrate having a density gradient. [Figure 1B] 1B is an enlarged view of cross section 1B-1B of the embodiment of the polycrystalline SiC substrate of FIG. 1A. [Figure 1C] 1C is an enlarged view of cross section 1C-1C of the embodiment of the polycrystalline SiC substrate of FIG. 1A. [Figure 1D] FIG. 1B is an enlarged view of cross section 1D-1D of the embodiment of the polycrystalline SiC substrate of FIG. 1A. [Figure 2A] FIG. 2 is a side perspective view of an embodiment of a polycrystalline SiC substrate shown in FIGS. 1A-1D, including a single crystal layer. [Figure 2B] 2B is an enlarged view of cross section 2B-2B shown in FIG. 2A at a location where a single crystal layer is to be bonded to a surface of the embodiment of the polycrystalline SiC substrate shown in FIGS. 1A-1D. [Diagram 3] FIG. 2 is a flow diagram of a method for manufacturing the embodiment of the polycrystalline SiC substrate shown in FIGS. 1A to 1D. [Figure 4A] 4A-4D are side views of respective steps of at least some of the embodiments of the manufacturing method shown in FIG. 3 for producing the device shown in FIGS. 1A-1D. [Figure 4B] 4A-4D are side views of respective steps of at least some of the embodiments of the manufacturing method shown in FIG. 3 for producing the device shown in FIGS. 1A-1D. [Diagram 5] FIG. 3 is a flow diagram of a method for producing a monocrystalline layer on the embodiment of the polycrystalline SiC substrate of FIGS. 2A and 2B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In the following description, specific details are set forth to provide a thorough understanding of various embodiments of devices, methods, and articles. However, one of ordinary skill in the art will understand that other embodiments may be practiced without these details. In other instances, well-known structures and methods related to, for example, silicon carbide substrates or layers (e.g., polycrystalline silicon carbide, single crystal silicon carbide, etc.), semiconductor manufacturing processes, etc., have not been shown or described in detail in some of the figures to avoid unnecessarily obscuring the description of the embodiments.
[0009] Unless the context requires otherwise, throughout the following specification and claims, the word "comprise" and variations thereof, such as "comprising" and "comprises," are to be interpreted in their open and inclusive sense, i.e., "including, but not limited to."
[0010] References throughout this specification to "one embodiment" or "one embodiment" mean that a particular feature, structure, or characteristic described in connection with an embodiment is included in at least one embodiment. Thus, the appearances of the phrases "in one embodiment" or "in one embodiment" in various places throughout this specification do not necessarily refer to the same embodiment or all embodiments. Furthermore, the particular features, structures, or characteristics may be combined in any suitable manner in one or more embodiments to yield further embodiments.
[0011] Headings are provided for convenience only and do not interpret the scope or meaning of the disclosure or claims.
[0012] The sizes and relative positions of elements in the figures are not necessarily drawn to scale, for example, the shapes and angles of various elements may not be drawn to scale, and some of these elements may be enlarged and positioned to improve the legibility of the figures.
[0013] The use of "lateral" means that a surface, sidewall, or similar or similar structure or feature is at an angle relative to another respective surface, sidewall, or similar or similar respective structure or feature. For example, if a first surface is transverse to a first sidewall, the first surface can be at an angle equal to 25 degrees, 35 degrees, 45 degrees, 75 degrees, 90 degrees, 120 degrees, etc.
[0014] Generally, polycrystalline silicon carbide (SiC) substrates, wafers, or layers have been utilized within various electronic devices and components (e.g., semiconductor dies, semiconductor packages, semiconductor transistors, etc.). These polycrystalline SiC substrates have a resistivity that results in a resistance that exists along the electrical path that passes through the polycrystalline SiC substrate. This resistance impedes an electrical signal as it passes through the electrical path and is referred to as on-resistance (R on ) for the polycrystalline SiC substrate. on) limits the efficiency or electrical characteristics of electronic devices fabricated from polycrystalline SiC substrates. For example, on-resistance (R on ) is high, electrical signals may be prevented from passing completely through the polycrystalline SiC substrate to reach their destination, resulting in functional errors within the electronic device or component.
[0015] As a polycrystalline SiC substrate is formed, density affects the formation of voids or otherwise affects the roughness of the surface on which subsequent layers or devices are formed. The present disclosure is directed to producing polycrystalline SiC substrates with flat surfaces that are less expensive and result in fewer voids. This is in contrast to conventional polycrystalline SiC substrates that are first formed using a sintering process, where larger voids exist between the grains. These voids may exist at or adjacent to the surface of a conventional polycrystalline SiC substrate that is planarized and polished (i.e., made flat). The surface of a conventional polycrystalline SiC substrate before being planarized and polished may be relatively rough and uneven, due in part to different grain sizes and crystal structures.
[0016] The surface of a conventional polycrystalline SiC substrate after being planarized and polished is flat (i.e., horizontal) and smooth (i.e., polished). However, during this planarization and polishing process, voids present at or adjacent to the surface of the conventional polycrystalline SiC substrate form depressions or recesses. After the surface is planarized and polished, another layer is generally formed on the surface of the conventional polycrystalline SiC substrate. When this layer is formed on the surface of the conventional polycrystalline SiC substrate, which has depressions and recesses, defect voids are formed between the layer and the surface. These defect voids, as described above, increase the on-resistance (R on ) and may cause a semiconductor package or device including this layer and a conventional polycrystalline SiC substrate to not operate within efficiency tolerances.
[0017] Manufacturing a conventional polycrystalline SiC substrate to have a low density can reduce costs. However, the low density creates a relatively rough surface due to a high number of defect voids. As a result, even after polishing and planarizing the surface of a low density polycrystalline SiC substrate, ridges and raised areas still remain.
[0018] The present disclosure is directed to one or more embodiments of a polycrystalline SiC substrate having a density gradient such that a first density at a first surface of the substrate is less than a second density at a second surface of the substrate opposite the first surface. The second density at the second surface may allow the second surface to be more effectively polished and planarized to increase the bond strength between layers of material (e.g., semiconductor material, silicon material, etc.) subsequently formed on the second surface. Meanwhile, at the same time, the manufacturing cost of the polycrystalline SiC substrate having a density gradient is reduced overall compared to manufacturing conventional high density polycrystalline SiC. In other words, the polycrystalline SiC substrate having a density gradient has the advantage of being manufactured to have a surface that is flatter and less rough than conventional low density polycrystalline SiC substrates, and less expensive than conventional high density polycrystalline SiC substrates.
[0019] At least one embodiment of the device of the present disclosure is summarized as follows: The device includes a polycrystalline silicon carbide (SiC) wafer including a first side and a second side opposite the first side. The first density is a density at the first side of the polycrystalline silicon carbide (SiC) wafer, and the second density is a density at the second side of the polycrystalline silicon carbide (SiC) wafer. The second density is greater than the first density. A density gradient exists between the first side and the second side, and the density of the density gradient increases in a density gradient direction from the first side to the second side of the polycrystalline silicon carbide (SiC) wafer.
[0020] At least one embodiment of the method of the present disclosure is summarized as follows: The method includes forming a polycrystalline silicon carbide (SiC) substrate, and after forming the polycrystalline silicon carbide (SiC) substrate, inducing mass transport oriented from a first side of the polycrystalline silicon carbide base substrate toward a second side opposite the first side, thereby generating a density gradient between a first side of the polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite the first side. Inducing material transport includes exposing a first side of the polycrystalline silicon carbide (SiC) substrate to a first temperature that transports material away from the first side of the polycrystalline silicon carbide (SiC) substrate and exposing a second side of the polycrystalline silicon carbide (SiC) substrate to a second temperature that transports material toward the second side of the polycrystalline silicon carbide (SiC) substrate, the second temperature being lower than the first temperature. Cooling the polycrystalline silicon carbide (SiC) substrate to produce a first density at the first side of the polycrystalline silicon carbide (SiC) substrate, a second density at the second side of the polycrystalline silicon carbide (SiC) substrate that is greater than the first density, and a density gradient between the first and second sides of the polycrystalline silicon carbide (SiC) substrate.
[0021] At least one embodiment of the method of the present disclosure is summarized as follows: The method includes creating a density gradient between a first side of a polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite the first side. Creating a density gradient between the first side and the second side includes exposing the second side of the polycrystalline silicon carbide (SiC) substrate to a chemical vapor deposition process to impregnate the second side of the polycrystalline silicon carbide (SiC) substrate with silicon (Si) and carbon (C).
[0022] 1A is directed to a side perspective view of a density gradient polycrystalline silicon carbide (SiC) substrate 100, which may be referred to herein as substrate 100. Substrate 100 may be a wafer and may be cylindrical as shown in FIG. 1A.
[0023] The substrate 100 includes a first surface 102 and a second surface 104 opposite the first surface 102. A first sidewall 106 is transverse to the first surface 102 and the second surface 104 and extends from the first surface 102 to the second surface 104. The second surface 104 has a roughness of 5 angstroms (Å) or less and is horizontal such that the second surface 104 is flat (i.e., polished, smooth, planarized, and level). The first surface 102 can be a rear surface, back surface, bottom surface, or lower surface based on the orientation of the substrate 100 shown in FIG. 1A, and the second surface 104 can be a front surface, top surface, or upper surface based on the orientation of the substrate 100 shown in FIG. 1A.
[0024] The first density of the substrate 100 is the density at the first surface 102, and the second density of the substrate 100 is the density at the second surface 104. The first density of the substrate 100 is different from the second density of the substrate 100. For example, the first density is less than the second density. The substrate 100 having a density gradient includes a density gradient direction represented by an arrow 108 oriented in a direction away from the first surface 102 and toward the second surface 104. The density gradient of the substrate 100 increases in the density gradient direction 108 along the substrate 100 between the first surface 102 and the second surface 104. The density gradient increases in the density gradient direction 108 such that the first density at the first surface 102 is the lowest density of the density gradient and the second density at the second surface 104 is the highest density of the density gradient. In at least one embodiment, the first density is between 2.75 and 3.05 grams per cubic centimeter (i.e., between 2.75 and 3.05 g / cm 3 ) or equal to the upper and lower ends of this range (i.e., 2.75 g / cm 3 or equal to 3.05 g / cm 3In at least one embodiment, the second density is between 3.05 and 3.20 grams per cubic centimeter (i.e., between 3.05 and 3.20 g / cm 3 ) or equal to the upper and lower ends of this range (i.e., 3.05 g / cm 3 or 3.20 g / cm 3 In some embodiments, the second density is between 3.10 and 3.20 grams per cubic centimeter (i.e., between 3.10 and 3.20 g / cm 3 ) or may be equal to the upper and lower ends of this range (i.e., 3.10 g / cm 3 or 3.20 g / cm 3 In some embodiments, the second density is between 3.10 and 3.26 grams per cubic centimeter (i.e., 3.10 g / cm 3 ~3.26g / cm 3 ) or may be equal to the upper and lower ends of this range (i.e., 3.10 g / cm 3 or 3.26 g / cm 3 may be equal to.
[0025] In some embodiments, the first density at the first surface 102 of the substrate 100 is between 2.5 and 3.0 g / cm 3 and the second density at the second surface may be in the range of 3.0 to 3.3 g / cm 3 In some embodiments, the second density at the second surface 104 of the substrate 100 may be in the range of 3.2 to 3.3 g / cm 3 The percentage of voids present at or immediately adjacent to the first surface 102 of the substrate 100 may be in the range of 20% to 25%, or equal to the upper and lower limits of this range. The percentage of voids present at or immediately adjacent to the second surface 104 of the substrate 100 may be in the range of 2% to 0.5%, or equal to the upper and lower limits of this range.
[0026] In some embodiments, as the density increases from a first density at the first surface 102 to the second surface 104 of the substrate 100, the density increases linearly.
[0027] The substrate 100 includes a first thickness 110. The first thickness 110 may be in the range of 200 micrometers (μm) to 1.2 millimeters (mm), or may be equal to the upper and lower ends of this range (i.e., equal to 200 micrometers (μm) or equal to 1.2 millimeters (mm)). In some embodiments, the first thickness 110 may be greater than 1.2 millimeters (mm) or less than 200 micrometers (μm). In some embodiments, the first thickness 110 may be substantially equal to 1 millimeter (mm).
[0028] Each particle at or in close proximity to the first surface 102 of the substrate 102 (e.g., in a region having a first density) may have a size in the range of 1 micrometer (μm) to 20 micrometers (μm), or a size equal to the upper and lower ends of this range. Each particle at or in close proximity to the second surface 104 of the substrate 100 (e.g., in a region having a second density) may have a size in the range of 10 micrometers (μm) to 30 micrometers (μm), or a size equal to the upper and lower ends of this range. Each particle at a point midway between the first surface 102 and the second surface 104 may have a size in the range of 5 micrometers (μm) to 25 micrometers (μm), or a size equal to the upper and lower ends of this range. Each grain boundary at or immediately adjacent to the first surface 102 of the substrate 100 may have a size in the range of 1 micrometer (μm) to 20 micrometers (μm), or an upper and lower limit of this range. Each grain at or immediately adjacent to the second surface 104 of the substrate 100 may have a size in the range of 10 micrometers (μm) to 30 micrometers (μm), or an upper and lower limit of this range. Each void at or in close proximity to the first surface 102 of the substrate 100 (e.g., in the area having the first density) may be in the range of 5 micrometers (μm) to 50 micrometers (μm) or equal to the upper and lower ends of this range, and preferably each void at or in close proximity to the first surface 102 of the substrate 100 (e.g., in the area having the first density) may be in the range of 25 micrometers (μm) to 40 micrometers (μm) or equal to the upper and lower ends of this preferred range. Each void at or in close proximity to the second surface 104 of the substrate 100 may have a size of 5 micrometers (μm) or less. Each void at or in close proximity to the first surface 102 of the substrate 100 may have a size of 10 micrometers (μm) or less.
[0029] FIG. 1B is an enlarged view of the enclosed cross section 1B-1B in FIG. 1A. A first portion 112 of the substrate 100 is shown in FIG. 1B, which is in close proximity to the second surface 104 of the substrate 100. Thus, the first portion 112 of the substrate 100 has a respective density that is greater than the first density at the first surface 102 and less than the second density at the second surface 104. Since the first portion 112 of the substrate 100 shown in FIG. 1B is between the first surface 102 and the second surface 104, the respective density of the first portion 112 is less than the respective density of the respective portions of the substrate 100 that are closer to the second surface 104 than the first portion 112, and is greater than the respective density of the respective portions of the substrate 100 that are closer to the first surface 102 than the first portion 112. In other words, the first portion 112 is closer to the second surface 104 than the first surface 102.
[0030] The density is slightly lower than the second density of the substrate 100 at the second surface 104, so that in the first portion 112 of the substrate 100, there are very small or very few voids 114 between the grains 116 of the substrate 100. Because the voids 114 are very small or few in number, the first portion 112 of the substrate 100 has a relatively high density due to the first portion 112 being in close proximity to the second surface 104 of the substrate 100. The voids 114 may be present between adjacent ones of the grains 116, and at least some of the voids 114 may be present along grain boundaries 118 between the grains 116 of the substrate 100.
[0031] FIG. 1C is an enlarged view of the enclosed cross section 1C-1C in FIG. 1A. A second portion 120 of the substrate 100 is shown in FIG. 1C, which is in close proximity to the first surface 102 of the substrate 100. Thus, the second portion 112 of the substrate has a respective density that is greater than the first density at the first surface and less than the second density at the second surface 104. Since the second portion of the substrate 100 shown in FIG. 1C is between the first surface 102 and the second surface 104, the respective density of the second portion 120 is less than the respective density of the respective portion of the substrate 100 that is closer to the second surface 104 than the second portion, and is greater than the respective density of the respective portion of the substrate 100 that is closer to the first portion 102 of the substrate 100. In other words, the second portion 120 is closer to the first surface 102 than the second surface 104.
[0032] 1B and 1C , the respective voids 114 that exist along the grain boundaries 118 between the grains 116 in the second portion 120 shown in FIG. 1B are larger than the respective voids 114 that exist along the grain boundaries 118 between the grains 116 in the first portion 112. The respective voids 114 in the second portion 120 being larger than the respective voids in the first portion 112 means that the second portion 120 has a respective density that is less than the respective density of the first portion 112.
[0033] In some embodiments of the substrate 100, a first number of respective voids 114 present in the first portion 112 may be less than a second number of respective voids 114 in the second portion 120. Because the respective voids 114 are generally larger and more numerous in the second portion 120 compared to those respective voids 114 present in the first portion 112, the first portion 112 of the substrate 100 has a respective density that is greater than the respective density of the second portion 120 of the substrate 100.
[0034] FIG. 1D is an enlarged view of cross section 1D-1D of the embodiment of polycrystalline SiC substrate 100 shown in FIG. 1A. As shown in FIG. 1D, second surface 104 includes slight depressions 122 present along second surface 104. Voids 114 may cause slight depressions 122 in second surface 104 after second surface 104 is planarized and polished. Details of planarizing and polishing second surface 104 will be described in detail later in this specification. However, these slight depressions 122 are much smaller compared to depressions when a similar or similar surface of a conventional low-density polycrystalline SiC substrate is planarized and polished. For example, when a similar or similar surface of a conventional low-density polycrystalline SiC substrate is planarized and polished, each depression will be much larger and therefore larger ridges and protuberances will be present on a similar or similar surface of a conventional low-density polycrystalline SiC substrate. In other words, the depressions 122 in the planarized and polished second surface 104 of substrate 100 are more similar or similar to depressions that were present in a similar or similar planarized and polished surface of a conventional high density polycrystalline SiC substrate, while at the same time, substrate 100 is less expensive to manufacture than a conventional high density polycrystalline SiC substrate. In other words, substrate 100 is less expensive to manufacture than a conventional low density polycrystalline SiC substrate, and has a better surface finish than a conventional high density polycrystalline SiC substrate.
[0035] 2A is a perspective side view of a monocrystalline layer 124 bonded to and overlying an embodiment of the second surface 104 of the substrate 100. The monocrystalline layer 124 may be silicon carbide (SiC). The monocrystalline layer 124 is bonded or bonded to the second surface 104 of the substrate 100 at a bond or bonding region 128 that is between the monocrystalline layer 124 and the substrate 100. The monocrystalline layer 124 has a surface 128 that faces away from the second surface 104 of the substrate 100 and faces away from the substrate 100. The monocrystalline layer 124 has a second thickness 130 that extends from the second surface 104 of the substrate 100 to the surface 128 of the monocrystalline layer 124. The second surface 104 of the substrate 100 is covered with a monocrystalline layer 124 that includes a second sidewall 132 that is transverse to the surface 128 and the second surface 104, extends from the second surface 104 to the surface 128, and is coplanar with the first sidewall 106 of the substrate 100.
[0036] The second thickness 130 can be less than or equal to 1 micrometer (μm). In some embodiments, the second thickness 130 can be greater than 1 micrometer (μm).
[0037] 2B is an enlarged view of the enclosed cross section 2B-2B in FIG. 2A. As shown in FIG. 2B, in the bonding region, one or more cavities 134 exist between the single crystal layer 124 and the substrate 100. The one or more cavities 134 exist between the second surface 104 and the single crystal layer 124 due to the presence of the depressions 122 at the second surface 104 of the substrate 100 when the single crystal layer 124 is formed, bonded, or bonded to the second surface 104 of the substrate 100. In some embodiments, the one or more cavities 134 may not exist at all. This is because the depressions 122 may not exist at all or the depressions 122 are small enough to fill the small depressions 122 at the second surface 104 of the substrate 100 when the single crystal layer 124 is formed, bonded, or bonded to the second surface 104 of the substrate 100.
[0038] Even if one or more cavities 134 are present due to small depressions 122 in the second surface 104 of the substrate 100 after planarization and polishing, the one or more cavities 134 are small enough that the one or more cavities have a negligible effect on the impedance of the respective electrical signals passing through the substrate 100 and the single crystal layer 124. Even if one or more cavities 134 are present due to small depressions 122 in the second surface 104 of the substrate 100 after planarization and polishing, there may be only a small number of the one or more cavities present such that the one or more cavities have a negligible effect on the impedance of the respective electrical signals passing through the substrate 100 and the single crystal layer 124.
[0039] 5 is a flow diagram 200 of a method for manufacturing the embodiment of the substrate 100 shown in Figures 1A-1D. The flow diagram 200 includes a first step 202, a second step 204, and a third step 206.
[0040] In a first step 202, a polycrystalline silicon carbide (SiC) base substrate 208 is formed, which may be referred to as a base substrate 208. For example, the base substrate 208 may be formed by utilizing a furnace to sinter together a mixture of powdered silicon (Si) and powdered carbon (C) to form the base substrate 208, or by utilizing a furnace to sinter together powdered silicon carbide (SiC) to form the base substrate 208. In other words, the base substrate 208 may be formed utilizing a sintering process known within the silicon carbide (SiC) substrate forming industry. After formation, the base substrate 208 includes a first surface 210 corresponding to the first surface 102 and a second surface 212 corresponding to the second surface 104 opposite the first surface 210. The base substrate 208 extends from the first surface 210 to the second surface 212 and includes a sidewall 214 lateral to the first surface 210 and the second surface 212.
[0041] After the first step 202 of forming the base substrate 208, a second step 204 of forming or creating a density gradient in the base substrate 208 is performed. The density gradient is formed or created in the base substrate 208 by applying a first temperature 214 to the first surface 210 and a second temperature 216 to the second surface 212. The first temperature 214 is different from the second temperature 216. For example, the first temperature 214 is higher than the second temperature 216. The first temperature 214 can be equal to or higher than 2000 degrees Celsius and the second temperature 216 can be equal to or lower than 2000 degrees Celsius. In some embodiments, the first temperature 214 can be equal to or higher than 2200 degrees Celsius and the second temperature 216 can be equal to or lower than 2000 degrees Celsius. The application of a first temperature 214 to the first surface 210 and the application of a second temperature 216 to the second surface 212 occur simultaneously, causing atoms and particles of the base substrate to move or be transported in a mass transport direction represented by arrow 218. The mass transport direction 218 is directed away from the first surface and toward the second surface 212. As the atoms and particles move in the mass transport direction 218, the first density at the first surface 210 decreases and the second density at the second surface 212 increases. In other words, the second density at the second surface 212 becomes greater than the first density at the first surface 210. After the first temperature 214 is applied to the first surface 210 and the second temperature 216 is applied to the second surface 212 for a period of time, the base substrate 208 is cooled. As the base substrate 208 cools from previous heating at the first temperature 214 and the second temperature 216, the first density at the first surface 210, the second density at the second surface 212, and the density gradient between the first surface 210 and the second surface 212 of the base substrate 208 become fixed. After cooling the base substrate 208 for a period of time, the base substrate 208 has a gradient density that increases along the substrate in the mass transport direction 218, with the second density at the second surface 212 being the maximum density of the base substrate 208 and the first density at the first surface 210 being the minimum density of the base substrate 208. The density of the substrate between the first surface 210 and the second surface 212 is an intermediate density that is greater than the first density at the first surface 210 and less than the second density at the second surface 212.
[0042] In an alternative embodiment, the density gradient in the base substrate 208 between the first surface 210 and the second surface 212 may be formed utilizing a chemical vapor deposition (CVD) process instead of applying a first temperature 214 to the first surface 210 and a second temperature 216 to the second surface 212. When a CVD process is utilized instead of applying a first temperature 214 and a second temperature 216 to the base substrate 208, additional silicon carbide (SiC) or silicon (Si) and carbon (C) particles or atoms are introduced to the second surface 212 of the base substrate, and the additional SiC or Si and C particles and atoms impregnate the base substrate 208 at the second surface 212 to form a density gradient in the base substrate 208, where the second density at the second surface 212 is greater than the first density at the first surface 210, and the intermediate density between the first surface 210 and the second surface 212 is greater than the first density and less than the second density. If a CVD process is utilized, additional SiC or Si and C particles and atoms may infiltrate the base substrate 208 and fill the voids 114 at the second surface or at a depth within the base substrate that is less than a third thickness 220 of the base substrate that extends from the first surface 210 to the second surface 212, respectively. The third thickness 220 of the base substrate 208 may be greater than the first thickness 110 of the substrate 100.
[0043] In view of the above, in at least one embodiment, when performing a CVD process, a porous polycrystalline SiC substrate is placed in a furnace. A hydrogen gas flow is introduced into the furnace. In the hydrogen gas flow, silane and ethene are introduced into the hydrogen gas flow. Alternatively, propane can be introduced into the hydrogen gas flow as a carbon source. In other words, some carbon source and some silicon source are introduced into the hydrogen gas flow so that carbon and silicon are present in the hydrogen gas flow. By introducing silane and ethene into the hydrogen gas flow, free silicon and free carbon are formed. These free silicon and free carbon are then deposited on the porous substrate as silicon carbide. During the time that the free silicon and free carbon are deposited on the porous substrate, the furnace is at a temperature substantially equal to 1600 degrees Celsius. This causes the free silicon and free carbon to be deposited on the porous substrate as silicon carbide (SiC). Furthermore, because the substrate is porous (i.e., having a porosity in the range of 7%-23%, or equal to the upper and lower ends of this range), the silicon carbide (SiC) that is deposited on the porous substrate actually infiltrates the porous substrate and fills voids within the porous substrate at or in close proximity to the second surface 212 of the base substrate 208. This results in the silicon carbide infiltrating the base substrate 208 and forming a density gradient between the first surface 210 and the second surface 212 of the base substrate 208.
[0044] After the second step 204 of forming and creating a density gradient across the base substrate 208, a third step 206 is performed, in which the second surface 212 of the base substrate 208 is planarized (i.e., leveled) and polished (i.e., smoothed) by a planarization polishing tool 222, which may be a chemical mechanical planarization tool that rotates to planarize and polish the second surface 212 of the base substrate 208. After the second surface 212 is planarized and polished by the planarization polishing tool 222, the polycrystalline SiC substrate 100 is produced. The second surface 212 may be polished to have a roughness of 5 angstroms (Å) or less, so that the second surface 212 is the same or similar to the second surface 104 described hereinabove.
[0045] During the third step 206 shown in FIG. 4A, the second surface 212 can be more easily planarized and effectively polished by the planarizing polishing tool 222. This is because there are fewer voids 114 at, adjacent to, or in close proximity to the second surface 212 due to the densification process in the second step 204, in which a density gradient is formed in the base substrate, and therefore the second density (e.g., high density) at the second surface 212 is greater than the first density (e.g., low density) at the first surface 210. In other words, if there are any depressions 122 present in the second surface 212 after planarization and polishing by the planarizing polishing tool 222, the depressions 122 are small such that the second surface 212 has a roughness of 20 angstroms (Å) or less. In some embodiments, the depressions are small such that the second surface 212 has a roughness of 5 angstroms (Å) or less.
[0046] After the third step 206 shown in Figure 4B, the base substrate 208 is transformed into the substrate 100 shown in Figures 1A-1C. In other words, after the manufacturing method of the flow diagram 200 is completed, the substrate 100 is manufactured.
[0047] Utilizing the manufacturing method of flow diagram 200 is less expensive than manufacturing a conventional polycrystalline SiC substrate that is dense throughout the conventional polycrystalline SiC substrate. This is because a greater amount of material is required to manufacture a conventional polycrystalline SiC substrate that is dense throughout the conventional polycrystalline SiC substrate compared to manufacturing substrate 100. Utilizing the manufacturing method of flow diagram 200 is also less expensive than manufacturing a conventional dense polycrystalline SiC substrate. This is because less energy may be required to sinter together base substrate 208 than to form a conventional base substrate that is dense throughout the conventional base substrate, which is then utilized to form a conventional dense polycrystalline SiC substrate.
[0048] While manufacturing substrate 100 using the manufacturing method of flow diagram 200 is less expensive than manufacturing conventional high density polycrystalline SiC substrates, the high second density at second surface 212 of base substrate 208, similar to the high density of conventional high density polycrystalline SiC substrates, allows second surface 212 of base substrate 208 to be effectively and consistently planarized and polished to reduce the size of dimples 122, reduce the number of dimples 122 present after planarization and polishing, or to eliminate dimples 122 altogether.
[0049] In view of the above, the method of manufacturing substrate 100 is less expensive than producing a conventional high density polycrystalline SiC substrate that is dense throughout, yet still allows second surface 212 to be effectively and consistently planarized and polished in the same manner that each surface of a conventional high density polycrystalline SiC substrate is planarized and polished.
[0050] After the substrate 100 is manufactured using the processes described herein, the substrate 100 may be utilized in forming an electronic component, such as a semiconductor package, a semiconductor die, or any other similar electronic or semiconductor component. For example, after the substrate 100 is manufactured, the substrate 100 may be further refined or processed (e.g., singulated, back-ground, etc.) to form an electronic component. Alternatively, for example, one or more additional layers may be formed, or semiconductor structures may be formed, or semiconductor structures may be bonded, on the second surface 104 of the substrate 100 (e.g., on the monocrystalline layer 124). For example, in at least one embodiment, the monocrystalline layer 124 is formed on the second surface 104 (as described in more detail with respect to FIG. 5 herein below).
[0051] FIG. 5 is a flow diagram 300 of a method for fabricating a monocrystalline layer 124 on the second surface 104 of the substrate 100. As shown in FIG. 5, the first step 202, the second step 204, and the third step 206 of the flow diagram 200 of the method for fabricating the substrate 100 are performed as previously described herein. After the formation of the substrate 100, a fourth step 302 is performed in which the monocrystalline layer 124 is formed, bonded, or attached to the second surface 104 of the substrate 100. For example, the monocrystalline layer 124 can be a wafer thinner than the substrate 100 that is bonded, bonded, or adhered to the second surface 104 of the substrate 100. Alternatively, the monocrystalline layer 124 can be formed, bonded, or attached to the second surface 104 of the substrate 100 by depositing the monocrystalline layer 124 on the second surface 104 of the substrate by a deposition method. For example, the deposition method can be a sputtering method, an evaporation method, a crystal growth method, or any other technique for forming, bonding, or joining the single crystal layer 124 to the second surface 104 of the substrate 100 .
[0052] In at least one embodiment, in the fourth step 302, the monocrystalline layer 124 is directly and physically bonded to the second surface 212. For example, the monocrystalline layer 124 may be formed by first bonding a monocrystalline substrate (not shown) to the second surface 104 using a surface activated bonding (SAB) method by exposing the second surface 212 to argon (Ar) ion or neutral atom bombardment (e.g., a beam of particles, which may be argon (Ar), neutral atoms, or any other similar or similar type of particles or atoms, which may be suitable) in an ultra-high vacuum to clean and activate the second surface 212 of the substrate 100. Once the second surface 104 is cleaned and activated by the SAB method, the monocrystalline substrate 124 is applied to the second surface 104, such that the monocrystalline substrate is directly and physically bonded to the second surface 104. Once the single crystal substrate is directly and physically bonded to the second surface 104, a portion of the single crystal substrate is removed such that a single crystal layer 124 remains on a second surface 212 that corresponds to the second surface 104 of the substrate 100. Before the second surface 212 is exposed to the irradiation of argon (Ar) ions or neutral atoms, the second surface 212 may be planarized or polished.
[0053] In at least one alternative embodiment, a first conductive layer (not shown) is formed on the second surface 212 and a second conductive layer (not shown) is formed on a surface of the single crystal substrate that is bonded to the second surface 212. The first conductive layer and the second conductive layer may be formed using a sputtering method. Once the first conductive layer and the second conductive layer are formed, the first layer and the second layer may be cleaned and activated using the SAB method as described above, and then the respective surfaces of the single crystal substrate may be applied to the second surface 212. After the single crystal substrate is directly and physically bonded to the second surface 212, a portion of the single crystal substrate is removed such that the single crystal layer 124 remains on the second surface 104 of the substrate. The first conductive layer and the second conductive layer may be planarized and polished before the first conductive layer and the second conductive layer are exposed to irradiation with argon (Ar) ions or neutral atoms.
[0054] If at least a portion of the recess 122 is present on the second surface 104 of the substrate 100 when the single crystal layer 124 is formed, bonded, or joined to the second surface 104 of the substrate 100, which corresponds to the second surface 212, one or more cavities 134 may be formed and present between the single crystal layer 124 and the substrate 100. However, these one or more cavities 134 may be small such that the one or more cavities have little or no impedance to an electrical signal as the electrical signal passes through the substrate 100 and the single crystal layer 124. Alternatively, the recess 122 may not be present such that there is no one or more cavities between the single crystal layer 124 and the substrate 100. Alternatively, the recess 122 may be completely filled when the single crystal layer 124 is formed, bonded, or joined to the second surface of the substrate 100. By keeping the one or more cavities 134 small, or by avoiding them altogether, there is little or no impedance to the electrical signal as it passes through the substrate 100 and the single crystal layer 124, resulting in more efficient and precise devices incorporating the substrate 100 and the single crystal layer 124.
[0055] When one or more cavities are present between the substrate 100 and the monocrystalline layer 124, the one or more cavities have a size of 10 micrometers (μm) or less.
[0056] In view of the above discussion, substrate 100 is cheaper to manufacture in a manner similar to that of manufacturing a conventional low-density polycrystalline SiC substrate, which is generally low-density, and which, when planarized and polished in a manner similar to that of planarizing or polishing each surface of a conventional high-density polycrystalline SiC substrate, has less roughness on the second surface.
[0057] After the single crystal layer 124 is formed or bonded to the second surface 104 of the substrate 100, the single crystal layer 124 may be further refined or processed (e.g., polished, thinned, etc.) to form an electronic component, or, for example, one or more additional layers may be formed or a semiconductor structure may be formed or bonded to the single crystal layer 124 (e.g., a dielectric layer, a conductive layer, a non-conductive layer, etc.).
[0058] After the single crystal layer 124 is formed or bonded to the second surface 104 of the substrate 100, the substrate 100 and the single crystal layer 124, one or more additional layers (e.g., a dielectric layer, a conductive layer, a non-conductive layer, etc.) may be formed on the substrate 100 and the single crystal layer 124. Once these one or more additional layers are formed, the substrate 100, the single crystal layer 124, and the one or more additional layers may be singulated into individual dies or into individual stacked assemblies that may be further processed to form various semiconductor dice, semiconductor packages, semiconductor components, or other similar electronic components. The semiconductor dice, semiconductor packages, semiconductor components, or other similar electronic components may be positioned within a phone, tablet, computer, or some other similar electronic device.
[0059] The individual dies singulated from the substrate 100, the single crystal layer 124, and one or more additional layers may then be encapsulated in a molding compound, epoxy, resin, or similar material to form a respective semiconductor package, semiconductor component, or other similar electronic component. The semiconductor package may be positioned within a phone, tablet, computer, or other similar electronic device.
[0060] The first density at the first surface 102 of the substrate 100 may have a low density compared to the density of a single crystal silicon carbide (SiC) substrate, and the second density at the second surface 102 of the substrate 100 may have a density similar to the density of a single crystal silicon carbide (SiC) substrate. However, the manufacture of the substrate 100 may be inexpensive compared to the manufacture of a high density polycrystalline SiC substrate and compared to the manufacture of a single crystal SiC substrate.
[0061] The substrate 100 may have a resistivity of 20 milliohm-centimeters (mohm-cm) or less at the second surface 104 of the substrate 100. In some embodiments, the substrate 100 may have a resistivity of 5 milliohm-centimeters (mohm-cm) or less at the second surface 104 of the substrate 100.
[0062] When single crystal layer 124 is present on substrate 100 having a density gradient, single crystal layer 124 may have a resistivity less than 25 mohm-cm, or preferably equal to 18 mohm-cm, or in the range of 15 to 20 mohm-cm, or the upper and lower ends of this range.
[0063] At least one embodiment of a device of the present disclosure is summarized as including a polycrystalline silicon carbide (SiC) wafer including a first side and a second side opposite the first side; a first density at the first side of the polycrystalline silicon carbide (SiC) wafer and a second density at the second side of the polycrystalline silicon carbide (SiC) wafer, the second density being greater than the first density; and a density gradient between the first side and the second side, the density of the density gradient increasing in a density gradient direction from the first side to the second side of the polycrystalline silicon carbide (SiC) wafer.
[0064] The polycrystalline silicon carbide (SiC) wafer may further include a surface on the second side having a roughness of less than 5 angstroms (Å).
[0065] The resistivity on the second side of the polycrystalline silicon carbide (SiC) wafer may be less than or equal to 20 milliohm-centimeters (mohm-cm).
[0066] The resistivity on the second side of the polycrystalline silicon carbide (SiC) wafer may be less than 5 milliohm-centimeter (mohm-cm).
[0067] The polycrystalline silicon carbide (SiC) wafer may have a thickness extending from the first side to the second side of 800 micrometers (μm) or less.
[0068] The device may further include a monocrystalline silicon carbide (SiC) layer that may be bonded to a second side of the polycrystalline silicon carbide (SiC) wafer.
[0069] The polycrystalline silicon carbide (SiC) wafer may have a first thickness extending from the first side to the second side, and the monocrystalline silicon carbide (SiC) layer may include a surface facing an opposite side of the polycrystalline silicon carbide (SiC) wafer and a second thickness extending from the second side to a surface of the monocrystalline silicon carbide (SiC) layer, and the second thickness may be less than the first thickness.
[0070] The second thickness can be less than or equal to 1 micrometer (μm).
[0071] The first thickness can be less than or equal to 800 micrometers (μm).
[0072] At least one embodiment of the method of the present disclosure includes forming a polycrystalline silicon carbide (SiC) substrate; and after forming the polycrystalline silicon carbide (SiC) substrate, generating a density gradient between a first side of the polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite the first side by inducing mass transport oriented in a mass transport direction from a first side of the polycrystalline silicon carbide base substrate toward a second side opposite the first side, wherein inducing mass transport includes: heating the polycrystalline silicon carbide base substrate to a first temperature that transports mass away from the first side of the polycrystalline silicon carbide (SiC) substrate; and exposing a first side of a polycrystalline silicon carbide (SiC) substrate to a second temperature that transports material toward the second side of the polycrystalline silicon carbide (SiC) substrate, the second temperature being lower than the first temperature; and cooling the polycrystalline silicon carbide (SiC) substrate to produce a first density at the first side of the polycrystalline silicon carbide (SiC) substrate, a second density at the second side of the polycrystalline silicon carbide (SiC) substrate that is greater than the first density, and a density gradient between the first and second sides of the polycrystalline silicon carbide (SiC) substrate.
[0073] Forming a polycrystalline silicon carbide (SiC) substrate can include sintering at least one of silicon carbide (SiC) powder and a powder mixture of silicon (Si) and carbon (C).
[0074] The second temperature can be greater than or equal to 2000 degrees Celsius.
[0075] The first temperature may be less than or equal to 2000 degrees Celsius.
[0076] The first temperature may be equal to 2000 degrees Celsius and the second temperature may be equal to or greater than 2100 degrees Celsius.
[0077] The method may further include bonding a monocrystalline silicon carbide (SiC) substrate to the second side of the polycrystalline silicon carbide (SiC) base substrate.
[0078] The density gradient can increase in a direction of mass transport from a first side to a second side of a polycrystalline silicon carbide (SiC) substrate.
[0079] At least one embodiment of the method of the present disclosure may be summarized as including creating a density gradient between a first side of a polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite the first side, where creating a density gradient between the first side and the second side includes exposing the second side of the polycrystalline silicon carbide (SiC) substrate to a chemical vapor deposition process to impregnate the second side of the polycrystalline silicon carbide (SiC) substrate with silicon (Si) and carbon (C).
[0080] The method may further include bonding a monocrystalline silicon carbide (SiC) substrate to the second side of the polycrystalline silicon carbide (SiC) substrate.
[0081] The method may further include forming a polycrystalline silicon carbide (SiC) substrate by sintering at least one of silicon carbide (SiC) powder and a powder mixture of silicon (Si) and carbon (C) prior to creating a density gradient between a first side of the polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate.
[0082] The density gradient can increase in a density gradient direction away from a first side of the polycrystalline silicon carbide (SiC) substrate toward a second side of the polycrystalline silicon carbide (SiC) substrate.
[0083] The various embodiments described above can be combined to provide further embodiments. Aspects of the embodiments can be modified, if necessary, to employ concepts from various patents, applications, and publications to provide further embodiments.
[0084] These modifications can be made to the embodiments in light of the above detailed description. In general, in the following claims, the terms used should not be construed to limit the scope of the claims to the specific embodiments disclosed in the specification and claims, but should be construed to include all possible embodiments along with the full scope of equivalents to which such claims are entitled. Accordingly, the claims are not limited by this disclosure.
Claims
1. a polycrystalline silicon carbide (SiC) wafer including a first side and a second side opposite the first side; a first density on the first side of the polycrystalline silicon carbide (SiC) wafer; a second density on the second side of the polycrystalline silicon carbide (SiC) wafer, the second density being greater than the first density; and a density gradient between the first side and the second side, the density of the density gradient increasing in a density gradient direction from the first side to the second side of the polycrystalline silicon carbide (SiC) wafer; Including, the device.
2. 10. The device of claim 1, wherein the polycrystalline silicon carbide (SiC) wafer further comprises a surface on the second side having a roughness of less than 5 angstroms (Å).
3. 10. The device of claim 1, wherein the resistivity of the polycrystalline silicon carbide (SiC) wafer on the second side is less than or equal to 20 milliohm-centimeters (mohm-cm).
4. 10. The device of claim 1, wherein the resistivity of the polycrystalline silicon carbide (SiC) wafer on the second side is less than 20 milliohm-centimeters (mohm-cm).
5. 10. The device of claim 1, further comprising a thickness extending from the first side to the second side of the polycrystalline silicon carbide (SiC) wafer, the thickness being less than or equal to 800 micrometers (μm).
6. 10. The device of claim 1, further comprising a monocrystalline silicon carbide (SiC) layer bonded to the second side of the polycrystalline silicon carbide (SiC) wafer.
7. the polycrystalline silicon carbide (SiC) wafer has a first thickness extending from the first side to the second side; The single crystal silicon carbide (SiC) layer is an opposing surface of the polycrystalline silicon carbide (SiC) wafer; and a second thickness extending from the second side to a surface of the single crystal silicon carbide (SiC) layer, the second thickness being less than the first thickness.
8. The device of claim 7 , wherein the second thickness is less than or equal to 1 micrometer (μm).
9. The device of claim 8 , wherein the first thickness is less than or equal to 800 micrometers (μm).
10. forming a polycrystalline silicon carbide (SiC) substrate; after forming the polycrystalline silicon carbide (SiC) substrate, inducing mass transport oriented in a mass transport direction from a first side of the polycrystalline silicon carbide base substrate toward a second side opposite the first side, thereby creating a density gradient between the first side of the polycrystalline silicon carbide (SiC) substrate and the second side of the polycrystalline silicon carbide (SiC) substrate opposite the first side, wherein the inducing of mass transport comprises: exposing the first side of the polycrystalline silicon carbide (SiC) substrate to a first temperature that transports material away from the first side of the polycrystalline silicon carbide (SiC) substrate; exposing the second side of the polycrystalline silicon carbide (SiC) substrate to a second temperature that transports material toward the second side of the polycrystalline silicon carbide (SiC) substrate, the second temperature being less than the first temperature; and creating a density gradient. cooling the polycrystalline silicon carbide (SiC) substrate to produce a first density on the first side of the polycrystalline silicon carbide (SiC) substrate, a second density on the second side of the polycrystalline silicon carbide (SiC) substrate that is greater than the first density, and the density gradient between the first side and the second side of the polycrystalline silicon carbide (SiC) substrate; A method comprising:
11. forming the polycrystalline silicon carbide (SiC) substrate; Silicon carbide (SiC) powder, Silicon (Si) and carbon (C) powder mixture The method of claim 10 , comprising sintering at least one of:
12. The method of claim 10, wherein the second temperature is greater than or equal to 2000 degrees Celsius.
13. The method of claim 12 , wherein the first temperature is less than or equal to 2000 degrees Celsius.
14. 11. The method of claim 10, wherein the first temperature is equal to 2000 degrees Celsius and the second temperature is greater than or equal to 2100 degrees Celsius.
15. 11. The method of claim 10, further comprising bonding a single crystal silicon carbide (SiC) substrate to the second side of the polycrystalline silicon carbide (SiC) base substrate.
16. 11. The method of claim 10, wherein the density gradient increases in the direction of mass transport from the first side to the second side of the polycrystalline silicon carbide (SiC) substrate.
17. generating a density gradient between a first side of a polycrystalline silicon carbide (SiC) substrate and a second side of the polycrystalline silicon carbide (SiC) substrate opposite the first side, wherein generating the density gradient between the first side and the second side comprises: exposing the second side of the polycrystalline silicon carbide (SiC) substrate to a chemical vapor deposition process to impregnate the second side of the polycrystalline silicon carbide (SiC) substrate with silicon (Si) and carbon (C).
18. 20. The method of claim 17, further comprising bonding a single crystal silicon carbide (SiC) substrate to the second side of the polycrystalline silicon carbide (SiC) substrate.
19. Prior to creating the density gradient between the first side of the polycrystalline silicon carbide (SiC) substrate and the second side of the polycrystalline silicon carbide (SiC) substrate, Silicon carbide (SiC) powder, Silicon (Si) and carbon (C) powder mixture 20. The method of claim 17, further comprising forming the polycrystalline silicon carbide (SiC) substrate by sintering at least one of:
20. 20. The method of claim 17, wherein the density gradient increases in a density gradient direction away from the first side of the polycrystalline silicon carbide (SiC) substrate toward the second side of the polycrystalline silicon carbide (SiC) substrate.