Thermosetting resin composition, sheet, and metal-based substrate
A resin composition combining polyhedral alumina and agglomerated boron nitride addresses thermal conductivity and adhesion issues in printed wiring boards, enhancing both properties for improved performance.
Patent Information
- Application Number
- JP2023060673
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2043-04-04
AI Technical Summary
Existing resin compositions for printed wiring boards focus primarily on single types of fillers for thermal conductivity, neglecting the potential benefits of combining different filler types, and fail to address the adhesion issues in forming fine wiring circuits.
A resin composition comprising epoxy resin, polyhedral alumina, and agglomerated boron nitride, which enhances thermal conductivity, insulation reliability, and peel strength by utilizing specific shapes and combinations of fillers.
The composition achieves superior thermal conductivity and insulation reliability, suitable for highly conductive printed wiring boards with improved adhesion.
Smart Images

Figure 2024147925000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin composition, a sheet, and a metal base substrate. [Background technology]
[0002] In recent years, with the demand for smaller electronic devices, higher frequencies, and higher power output, the manufacture of printed wiring boards using the build-up method has become common in order to achieve higher integration of semiconductors and smaller printed wiring boards, etc. These printed wiring boards are required to have high heat dissipation performance, and development is underway to use materials with excellent thermal conductivity.
[0003] For example, Patent Document 1 discloses an epoxy resin composition comprising an epoxy resin monomer, a curing agent, and a filler, the filler comprising a first filler containing boron nitride particles having a D50 of 20 μm or more and an average aspect ratio of primary particles of 30 or less, or an aggregate of the boron nitride particles, and a second filler containing boron nitride particles having a D50 of less than 10 μm and an average aspect ratio of 5 or less, or an aggregate of the boron nitride particles.
[0004] Patent Document 2 discloses a resin composition containing molybdenum-containing aluminum oxide (A) and a resin (B), in which the average particle size of the aluminum oxide (A) is 1000 μm or less. Furthermore, it discloses that the shape of the aluminum oxide (A) is not limited and is a spherical or polyhedral particle.
[0005] Patent Document 3 discloses an epoxy resin composition containing an epoxy resin monomer, a curing agent containing a novolak resin obtained by novolakizing a divalent phenol compound, and a mixed filler of α-alumina and boron nitride. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2021-165401 [Patent Document 2] International Publication No. 2015-060125 [Patent Document 3] JP 2016-155985 A Summary of the Invention [Problem to be solved by the invention]
[0007] As shown in Patent Documents 1 and 2, resin compositions to which boron nitride or alumina is added as a filler have been widely studied for the purpose of imparting high thermal conductivity. However, all of these documents mainly focus on the addition of the same type of filler, and there are not many studies that focus on the effects obtained by using different types of fillers in combination.
[0008] Patent Document 3 discloses a resin composition using two types of fillers, α-alumina and boron nitride, in combination, but it focuses on the structure of the epoxy resin monomer in particular, and by using an epoxy resin monomer with a characteristic structure, a cured product with a high order structure centered on alumina can be obtained, which shows excellent thermal conductivity. There are no particular restrictions on the α-alumina used, except for the particle size, and the research is insufficient as a study focusing on the filler.
[0009] Furthermore, with the trend toward higher integration of semiconductors and smaller printed wiring boards, there is a demand for forming fine wiring circuits. However, when a fine roughened shape is formed, there is a problem that adhesion, i.e., peel strength, decreases. However, this is not mentioned in any of the above documents, and further improvement is necessary.
[0010] In view of the above, an object of the present invention is to provide a resin composition, a varnish, an inorganic composite sheet thereof, and a metal base substrate, which all have thermal conductivity, insulating reliability, and peel strength. [Means for solving the problem]
[0011] The present inventors have conducted extensive research to solve the above problems, and have found that a resin composition that contains an epoxy resin, alumina, and aggregated boron nitride, and in which the alumina is polyhedral and has 14 or more faces, can provide a resin composition that has good thermal conductivity, insulating reliability, and peel strength.
[0012] That is, the present invention includes the following aspects. (1) An epoxy resin composition comprising an epoxy resin (A), an alumina (B), and an aggregated boron nitride (C), Epoxy resin composition, characterized in that the alumina (B) is polyhedral and has 14 or more sides. (2) A varnish containing the epoxy resin composition described in 1 above. (3) An inorganic composite sheet, which is obtained by applying the varnish according to item 2 above to a carrier material, and forming the varnish layer in an uncured state to a thickness of 100 to 200 μm. (4) A metal base substrate obtained by laminating the inorganic composite sheet according to item 3 above. Effect of the Invention
[0013] The resin composition of the present invention uses alumina of a specific shape and aggregated boron nitride, and thus has excellent thermal conductivity and insulating reliability, and can be suitably used as a material for highly thermally conductive printed wiring boards, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] An embodiment of the present invention will be described in detail below. The present invention is not limited to the following embodiment, and can be carried out by making appropriate modifications within the scope that does not impair the effects of the present invention.
[0015] <Epoxy resin composition> The epoxy resin composition of the present embodiment contains an epoxy resin (A), an alumina (B), and an aggregated boron nitride (C), and the alumina (B) is polyhedral and has 14 or more faces. [Epoxy resin (A)] In this embodiment, the epoxy resin (A) is not particularly limited, but preferably includes those that are suitably used as semiconductor encapsulants. For example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AD type epoxy resin, phenol novolac type epoxy resin, orthocresol novolac type epoxy resin, naphthalene skeleton-containing epoxy resin, biphenyl skeleton-containing epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, heterocyclic epoxy resin, etc. are suitable. From the viewpoint of melt viscosity, orthocresol novolac type epoxy resin, bisphenol type epoxy resin, biphenyl skeleton-containing epoxy resin are preferred, and from the viewpoint of moisture resistance and solder reflow resistance, orthocresol novolac type epoxy resin is preferred. In addition, from the viewpoint of handling of the B stage sheet, phenol biphenyl aralkyl epoxy resin having a softening temperature of 80°C or less is preferred. These epoxy resins may be used alone or in combination of two or more.
[0016] In the present embodiment, the amount of the epoxy resin in the resin composition is preferably 3% by mass to 15% by mass, and more preferably 4% by mass to 12% by mass, based on the total mass of the resin composition. By setting the amount to 4% by mass to 12% by mass, the resulting epoxy resin composition has excellent moldability and, when cured, has high thermal conductivity, which is preferable.
[0017] In the present embodiment, a curing agent may be further included. The curing agent may be any agent capable of undergoing a curing reaction with the epoxy resin, and examples of the curing agent include phenolic resins, amine compounds, amide compounds, acid anhydride compounds, cyanate ester compounds, compounds having an unsaturated double bond-containing substituent, and diene polymers.
[0018] Examples of the hardener for the phenol resin include phenol novolac resin, cresol novolac resin, aromatic hydrocarbon formaldehyde resin modified phenol resin, dicyclopentadiene phenol addition type resin, phenol aralkyl resin (Zylok resin), polyhydric phenol novolac resin synthesized from a polyhydric hydroxy compound such as resorcin novolac resin and formaldehyde, naphthol aralkyl resin, tetraphenylolethane resin, naphthol novolac resin, naphthol-phenol co-condensed novolac resin, naphthol-cresol Examples of polyhydric phenol compounds include aryl-co-condensed novolac resins, biphenyl-modified phenol resins (polyhydric phenol compounds in which phenol nuclei are linked via bismethylene groups), biphenyl-modified naphthol resins (polyhydric naphthol compounds in which phenol nuclei are linked via bismethylene groups), aminotriazine-modified phenol resins (polyhydric phenol compounds in which phenol nuclei are linked via melamine, benzoguanamine, or the like), and alkoxy group-containing aromatic ring-modified novolac resins (polyhydric phenol compounds in which phenol nuclei and alkoxy group-containing aromatic rings are linked via formaldehyde).
[0019] Examples of the amine compounds include diaminodiphenylmethane, diethylenetriamine, triethylenetetramine, diaminodiphenylsulfone, isophoronediamine, imidazole, BF3-amine complexes, and guanidine derivatives.
[0020] Examples of the amide-based compound include dicyandiamide, and polyamide resins synthesized from a dimer of linoleic acid and ethylenediamine.
[0021] Examples of the acid anhydride compounds include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride.
[0022] Examples of the cyanate ester compound include bisphenol A type cyanate ester resins, bisphenol F type cyanate ester resins, bisphenol E type cyanate ester resins, bisphenol S type cyanate ester resins, bisphenol sulfide type cyanate ester resins, phenylene ether type cyanate ester resins, naphthylene ether type cyanate ester resins, biphenyl type cyanate ester resins, tetramethylbiphenyl type cyanate ester resins, polyhydroxynaphthalene type cyanate ester resins, phenol novolac type cyanate ester resins, cresol novolac type cyanate ester resins, triphenyl Examples of the cyanate ester resin include phenylmethane type cyanate ester resins, tetraphenylethane type cyanate ester resins, dicyclopentadiene-phenol addition reaction type cyanate ester resins, phenol aralkyl type cyanate ester resins, naphthol novolac type cyanate ester resins, naphthol aralkyl type cyanate ester resins, naphthol-phenol co-condensed novolac type cyanate ester resins, naphthol-cresol co-condensed novolac type cyanate ester resins, aromatic hydrocarbon formaldehyde resin modified phenol resin type cyanate ester resins, biphenyl modified novolac type cyanate ester resins, and anthracene type cyanate ester resins.
[0023] The compound having an unsaturated double bond-containing substituent is not particularly limited as long as it has two or more unsaturated bond-containing substituents in the molecule. Examples of the unsaturated bond-containing substituent include compounds having an allyl group, an isopropenyl group, a 1-propenyl group, an acryloyl group, a methacryloyl group, a styryl group, a styrylmethyl group, and the like.
[0024] The diene polymer may be, for example, a non-modified diene polymer that is not modified by a polar group. Here, the polar group is a functional group that affects the dielectric properties, and may be, for example, a phenol group, an amino group, an epoxy group, etc. The diene polymer is not particularly limited, and may be, for example, 1,2-polybutadiene or 1,4-polybutadiene.
[0025] As the diene-based polymer, a butadiene homopolymer in which 50% or more of the butadiene units in the polymer chain are 1,2-bonds, and a derivative thereof can also be used.
[0026] The amount of the curing agent used relative to the amount of the epoxy resin used is preferably 0.7 to 1.3, more preferably 0.8 to 1.2, in terms of the ratio of the epoxy equivalent of the epoxy resin to the active hydrogen equivalent of the curing agent (epoxy equivalent / active hydrogen equivalent). If the (epoxy equivalent / active hydrogen equivalent) is outside the above range, the obtained cured product may be insufficiently cured.
[0027] In this embodiment, a curing accelerator may further be included. The curing accelerator may be included for the purpose of accelerating the curing reaction between the epoxy resin and the curing agent, and examples thereof include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, and urea-based curing accelerators. The curing accelerators may be used alone or in combination of two or more.
[0028] Examples of the phosphorus-based curing accelerator include organic phosphine compounds such as triphenylphosphine, tributylphosphine, tri-para-tolylphosphine, diphenylcyclohexylphosphine, and tricyclohexylphosphine; organic phosphite compounds such as trimethyl phosphite and triethyl phosphite; and phosphonium salts such as ethyltriphenylphosphonium bromide, benzyltriphenylphosphonium chloride, butylphosphonium tetraphenylborate, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylphosphine triphenylborane, tetraphenylphosphonium thiocyanate, tetraphenylphosphonium dicyanamide, butylphenylphosphonium dicyanamide, and tetrabutylphosphonium decanoate.
[0029] Examples of the amine curing accelerator include triethylamine, tributylamine, N,N-dimethyl-4-aminopyridine (4-dimethylaminopyridine, DMAP), 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo[5.4.0]-undecene-7 (DBU), and 1,5-diazabicyclo[4.3.0]-nonene-5 (DBN).
[0030] Examples of the imidazole-based hardening accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4 ... Examples of the compound include ethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5 hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, and 2-methylimidazoline.
[0031] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-butylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, and 1-phenylbiguanide.
[0032] Examples of the urea-based curing accelerator include 3-phenyl-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, chlorophenylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, and 3-(3,4-dichlorophenyl)-1,1-dimethylurea.
[0033] Among the above-mentioned curing accelerators, it is preferable to use phosphorus-based curing accelerators and imidazole-based curing accelerators from the viewpoint of curability, and from the viewpoint of insulation reliability, phosphorus-based curing accelerators are particularly preferable.
[0034] The amount of the curing accelerator used can be appropriately adjusted to obtain the desired curability, but is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the total amount of the mixture of the epoxy resin and the curing agent. When the amount of the curing accelerator used is within the above range, the curability and insulation reliability are excellent, which is preferable.
[0035] [Alumina (B)] In this embodiment, "alumina" refers to aluminum oxide, which may be transition alumina of various crystal forms such as gamma, delta, theta, and kappa, or may contain alumina hydrate in transition alumina, but is preferably essentially of the alpha crystal form because of its superior stability.
[0036] The alumina is preferably in the form of a polyhedron, particularly a polyhedron having 14 or more sides, which is preferable because it greatly improves the opportunity for surface contact and provides excellent thermal conductivity compared to a polyhedron having less than 14 sides.
[0037] The shape of alumina can be confirmed by a scanning electron microscope (SEM). Using a JEOL JCM7000, images obtained by multiple SEM images from any field of view of the sample are observed. Then, from the observation results of 50 randomly selected alumina particles, the shape of 60% or more of the particles on a number basis can be judged to be the shape that the sample has.
[0038] In this embodiment, the average particle size of the alumina (B) is preferably 25 μm or more and 45 μm or less. When the average particle size is 25 μm or more, it is preferable because the increase in viscosity when made into a varnish is suppressed. When the average particle size is 45 μm or less, it is preferable because the processability of the sheet is excellent.
[0039] The "average particle size" in the present invention is a value calculated as the volume-based median size D50 from the volume-based cumulative particle size distribution measured by a laser diffraction / scattering particle size distribution analyzer.
[0040] The content of alumina (B) in the epoxy resin composition of the present embodiment may be 30 to 80 parts by mass, or may be 40 to 70 parts by mass, based on 100 parts by mass of the total solid content of the epoxy resin composition. The suitable content of alumina (B) can be set depending on the content of aggregated boron nitride (C) described below.
[0041] The alumina (B) of this embodiment may be commercially available alumina particles, or alumina particles produced by the methods described in JP 2016-028993 A and WO 2021 / 070729 A may be used.
[0042] Commercially available alumina particles include DAW45 (manufactured by Denka), CB-A20S, CB-AS30S, CB-P15 (manufactured by Showa Denko KK), AZ series (manufactured by Nippon Steel Material & Chemical Co., Ltd.), AH40-S (manufactured by DIC Corporation), and AO-502 (manufactured by Admatechs). From the viewpoint of fluidity, CB-A20S, CB-A30S, CB-P15 (manufactured by Showa Denko KK), and AO-502 (manufactured by Admatechs) are preferred, and from the viewpoint of thermal conductivity, AH40-S (manufactured by DIC Corporation) is preferred, but the present invention is not limited to these.
[0043] These alumina particles may be used alone or in combination, but it is preferable to use a combination of a plurality of them. When using a combination of a plurality of them, it is preferable that the polyhedral alumina particles are contained in the total alumina (B) at 50 mass% or more, and more preferably at 60 mass% or more. By being within the above range, the thermal conductivity of the inorganic composite sheet and metal base substrate obtained is particularly excellent, which is preferable.
[0044] [Agglomerated boron nitride (C)] The aggregated boron nitride (C) of this embodiment is an aggregated boron nitride in which scale-like boron nitride is randomly oriented. By using the aggregated boron nitride (C), the orientation of boron nitride in the planar direction is suppressed, and when the inorganic composite sheet described below is formed, the thermal conductivity in the thickness direction is improved, which is preferable.
[0045] The average particle size of the aggregated boron nitride (C) is preferably 5 μm or more and 50 μm or less, more preferably 10 μm or more and 40 μm or less. When it is 5 μm or more, an increase in viscosity is suppressed, and when it is 50 μm or less, excellent moldability is obtained.
[0046] The specific surface area of the aggregated boron nitride (C) is 1 to 4 cm 2 / g, and 1.5 to 3.5 cm 2 When the specific surface area is within the above range, an increase in viscosity is suppressed, which is preferable. The specific surface area is determined by the BET method.
[0047] The particle strength of the aggregated boron nitride (C) is preferably 20 MPa or less, more preferably 18 MPa or less, and particularly preferably 15 MPa or less. If it is 20 MPa or less, the air content in the heat dissipation sheet can be suppressed and the thermal conductivity can be improved. In addition, if the particle strength is 5 MPa or more, damage to the aggregated boron nitride is suppressed during the manufacturing process, which is preferable.
[0048] Particle strength can be measured in accordance with JIS R1639-5:2007. After scattering the agglomerated boron nitride particles on the sample stage of a microcompression tester ("MCT-W500" manufactured by Shimadzu Corporation), five agglomerated boron nitride particles are selected and a crushing test is carried out one by one to calculate the particle strength. The particle strength (σ: MPa) is calculated using the equation σ = α × P / (π × d2) from the dimensionless number (α = 2.48) that changes depending on the position within the particle, the crushing test force (P: N), and the particle size (d: μm). In accordance with JIS R1625:2010, the crushing strength of five inorganic filler components is plotted in a Weibull plot, and the crushing strength at which the cumulative destruction rate is 63.2% is taken as the particle strength of the agglomerated boron nitride particles.
[0049] The agglomerated boron nitride (C) of this embodiment may be a commercially available product, such as HP-40MF, HP40-J2 (manufactured by Mizushima Ferroalloy Co., Ltd.), PTX60 (manufactured by Momentive Corp.), Agglomerates 50 (manufactured by 3M Co., Ltd.), etc. Preferred are HP-40MF and HP40-J2 (manufactured by Mizushima Ferroalloy Co., Ltd.) which are sintered to produce agglomerates without internal voids.
[0050] The content of the aggregated boron nitride (C) in the epoxy resin composition of the present embodiment may be 10 to 75 parts by mass, and preferably 40 to 70 parts by mass, per 100 parts by mass of the total solid content of the epoxy resin composition.
[0051] The total content of alumina (B) and aggregated boron nitride (C) in the epoxy resin composition of the present embodiment may be 70 to 95 parts by mass, and preferably 75 to 90 parts by mass, per 100 parts by mass of the total solid content of the epoxy resin composition. By being within the above range, an increase in the viscosity of the epoxy resin composition or its varnish can be suppressed, and a uniform coating film can be formed.
[0052] As long as it is within the above range, the content of alumina (B) and aggregated boron nitride (C) may be any combination, but the mass ratio of alumina (B) and aggregated boron nitride (C) is preferably 50:50 to 95:5, more preferably 55:45 to 90:10, and particularly preferably 60:40 to 85:15. If it is within the above range, it is preferable because both thermal conductivity and insulation reliability can be provided at excellent levels.
[0053] By combining alumina (B) and aggregated boron nitride (C), it is possible to obtain a thermal conductivity superior to that of conventional materials, and therefore to reduce the amount of filler in the epoxy resin composition. Furthermore, by reducing the amount of filler, the dielectric breakdown voltage of the epoxy resin composition is increased, and the variation in the dielectric breakdown voltage is suppressed, thereby stabilizing the electrical properties.
[0054] <Varnish> The present invention relates to a varnish containing the epoxy resin composition. The varnish can be prepared by a known method, and the epoxy resin composition can be dissolved (diluted) in an organic solvent to form a varnish.
[0055] As the solvent, for example, a polar solvent such as methyl ethyl ketone, methoxypropanol, N,N-dimethylformamide, or dimethylsulfoxide can be used, and the solvent may be used alone or in combination of two or more kinds.
[0056] The amount of the solvent used is not particularly limited, and can be appropriately determined, for example, taking into consideration the sheet processability. Specifically, it is preferable to adjust the viscosity of the resulting varnish to 3000 mPa·s to 15000 mPa·s. If the viscosity is 3000 mPa·s or more, poor appearance due to repellency during coating is suppressed, which is preferable. If the viscosity is 15000 mPa·s or less, poor appearance due to streaking during coating is suppressed, which is preferable.
[0057] [Other ingredients] The varnish of the present embodiment may contain other components, such as a silane coupling agent and a dispersant, as long as the other components do not impair the object of the present invention.
[0058] Examples of the silane coupling agent include epoxy silane, etc.
[0059] The dispersant is not particularly limited as long as it is a dispersant used for paints, and examples thereof include Disperbyk-110, 111, 180, 161, BYK-W996, W9010, W903, etc. By using a dispersant, not only can the dispersibility of alumina (B) be improved, but also the viscosity of the varnish can be adjusted within the above-mentioned range.
[0060] <Inorganic composite sheet> The varnish of the present invention is suitably used for an inorganic composite sheet. The inorganic composite sheet is produced by applying the above-mentioned varnish to a carrier material and drying the applied varnish by heating. The inorganic composite sheet is formed in a semi-cured state on the surface of the carrier material. That is, the heat drying is a process for bringing the varnish applied to the carrier material into a B-stage, and the epoxy resin in the varnish is partially reacted by heating the varnish applied to the carrier material. Therefore, the inorganic composite sheet of this embodiment has a property of being melted once and then cured by the heating and pressurization of the lamination molding.
[0061] The method of applying the varnish is not particularly limited, and can be carried out by a known method. For example, methods such as comma coating, die coating, lip coating, and gravure coating can be mentioned. As a method for forming an inorganic composite sheet of a predetermined thickness, a comma coating method in which a coated object is passed through a gap, and a die coating method in which varnish is applied from a nozzle with an adjusted flow rate are preferred.
[0062] The thickness of the inorganic composite sheet formed on the carrier material is preferably 100 to 200 μm. When the thickness is 100 μm or more, the thermal resistance is preferably small. As the thickness approaches 200 μm, the dielectric breakdown voltage is preferably large.
[0063] As the carrier material, it is preferable to use a polymer film or a metal sheet. Examples of the polymer film include polyolefins such as polyethylene, polypropylene, and polyvinyl chloride, polyesters such as polyethylene terephthalate, polycarbonate, acetyl cellulose, and tetrafluoroethylene. Examples of the metal sheet include metal foils such as copper foil, aluminum foil, and nickel foil. Furthermore, examples of the carrier material include release paper.
[0064] <Metal-based substrate> The inorganic composite sheet of the present invention can be suitably used as a metal base substrate by laminating. Specifically, two or more inorganic composite sheets obtained as described above are laminated to a desired thickness, and then a metal foil is placed on one or both outermost layers to form a laminate, and the laminate is laminated and integrated by heating and pressing such as press molding. Here, as the metal foil, a single metal foil, an alloy metal foil, or a composite metal foil such as copper, aluminum, brass, or nickel can be used. The conditions for heating and pressing the laminate may be appropriately adjusted under the conditions under which the varnish of the present invention is cured, but if the pressure is too low, air bubbles may remain inside the obtained metal base substrate, and the electrical properties may be reduced, so it is preferable to pressurize under conditions that satisfy the moldability. For example, a metal base substrate can be integrally molded by heating and pressing under conditions of a heating temperature of 100 to 200°C and a pressure of 0.98 to 4.9 MPa for 10 minutes to 2 hours.
[0065] The epoxy resin composition of the present invention has both insulating reliability and thermal conductivity, and an inorganic composite sheet containing it can be suitably used for printed wiring boards such as heat dissipation substrates on which semiconductor wafers, high brightness LEDs, power semiconductor devices, etc. are mounted. EXAMPLES
[0066] The present invention will now be described in more detail with reference to examples and comparative examples, but is not limited thereto.
[0067] (Viscosity evaluation) The viscosity (25° C.) of the varnishes obtained in the examples and comparative examples described below was measured using an E-type viscometer TVE-20H (manufactured by Toki Sangyo Co., Ltd.).
[0068] (Thermal conductivity evaluation) The metal base substrates obtained in the examples and comparative examples described below were cut into 1 cm squares, and then carbon black was sprayed on both sides to prepare measurement samples. The thermal conductivity of the obtained measurement samples was calculated by the laser flash method.
[0069] (90 degree peel strength evaluation) The metal base substrates obtained in the examples and comparative examples described later were cut into a size of 50 mm x 120 mm to obtain test samples. The copper foil was peeled off so that a central 10 mm-wide copper foil was left, and the peel strength of the copper foil was measured for the central 10 mm-wide copper foil in accordance with JIS C 6481. Shimadzu Corporation's "Autograph" was used as the peel strength measuring device. The copper foil peel strength was measured for 20 test samples. The average of the measured copper foil peel strengths for the 20 test samples was taken as the 90-degree peel strength.
[0070] (Long-term insulation reliability) The copper foil in the metal base substrate obtained in the Examples and Comparative Examples described below was etched to pattern the copper foil into a circle with a diameter of 2.5 cm to obtain a test sample. Using 20 of the obtained test samples, an AC voltage of 3 kV was applied between the test samples for 1000 hours in an environment of a temperature of 85°C and a humidity of 85%, and it was evaluated whether or not dielectric breakdown occurred. The long-term insulation reliability was evaluated according to the following criteria. [Criteria for long-term insulation reliability] ○: No test samples experienced dielectric breakdown △: Dielectric breakdown occurred in 1 or more but less than 10 test samples ×: Dielectric breakdown occurred in 10 or more test samples.
[0071] (Examples 1 to 3, Comparative Examples 1 to 3) A resin composition was prepared using the epoxy resin, alumina, and aggregated boron nitride shown below as raw materials according to the formulation shown in Table 1, and used as a varnish as is. [Epoxy resin (A)] Epicron 850 (DIC, bisphenol A type epoxy resin) NC-3000 (Phenol biphenyl aralkyl epoxy resin, manufactured by Nippon Kayaku Co., Ltd.) VG-3101 (Printec, trifunctional epoxy resin) [Alumina (B)] AH40-S (DIC, average particle size 32 μm, 14-sided) DAW45FC (manufactured by Denka, average particle size 36 μm) [Agglomerated boron nitride (C)] HP-40MF (manufactured by Mizushima Ferroalloy Co., Ltd., average particle size 36 μm) HP40-J2 (manufactured by Mizushima Ferroalloy Co., Ltd., average particle size 16 μm) [Other ingredients] YP50 (Phenoxy resin, manufactured by Nippon Steel Materials & Chemicals Co., Ltd.) Dicyandiamide (Nippon Carbide, hardener) 2E4MZ (Shikoku Kasei Co., Ltd., hardening accelerator) BYK-W903 (Big Chemie Japan, dispersant) KBE-403 (Shin-Etsu Chemical Co., Ltd., coupling agent, γ-glycidoxypropyltriethoxysilane)
[0072] (Preparation of metal base substrate) The obtained varnish was kneaded in a planetary mixer and mixed with a specified amount of solvent (a mixture of methyl ethyl ketone and dimethylformamide) to obtain a varnish with a viscosity adjusted to 3000 mPa s. Next, this varnish was applied to a polyethylene terephthalate (PET) film with a thickness of 75 μm and dried by heating at 130°C for 8 minutes, forming a 150 μm thick inorganic composite sheet in a B-stage state on one side of the carrier material.
[0073] Ten of the obtained inorganic composite sheets were stacked, copper foil of 18 μm was placed on both sides, and the stack was heated and pressed in a vacuum at a heating temperature of 175° C. and a pressure of 2.94 MPa for 90 minutes to produce a metal base substrate.
[0074] The evaluation results of the varnish and metal base substrate obtained above are shown in Table 1.
[0075] [Table 1]
Claims
1. An epoxy resin composition comprising an epoxy resin (A), an alumina (B), and an aggregated boron nitride (C), Epoxy resin composition, characterized in that the alumina (B) is polyhedral and has 14 or more sides.
2. A varnish comprising the epoxy resin composition according to claim 1.
3. 3. An inorganic composite sheet, comprising: a carrier material coated with the varnish according to claim 2; and a layer of the varnish in an uncured state having a thickness of 100 to 200 μm.
4. A metal base substrate obtained by laminating and molding the inorganic composite sheet according to claim 3.
Citation Information
Patent Citations
Thermally conductive silicone composition and thermally conductive silicone material
JP2021075630A
Epoxy resin composition, resin sheet, prepreg, metallic foil with resin, metal substrate, and power semiconductor device
JP2021165401A
Thermally conductive composition, thermally conductive grease, and thermally conductive sheet
JP7289023B1
Epoxy resin composition, semi-cured epoxy resin composition and cured epoxy resin composition, and resin sheet, prepreg, laminate sheet, metal substrate, wiring board and power semiconductor device, using these
JP2016155985A
Resin composition, heat-dissipating material, and heat-dissipating member
WO2015060125A1