Curable organopolysiloxane composition

A curable organopolysiloxane composition with trivinylsiloxane and (meth)acrylic groups addresses the high cost and catalyst poisoning issues of platinum group metal catalysts, achieving effective curing and adhesion on various substrates with reduced platinum usage.

JP2024148039APending Publication Date: 2024-10-17SHIN ETSU CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023060920
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing organopolysiloxane compositions for release paper or release film require high amounts of platinum group metal catalysts, which are expensive and prone to catalyst poisoning, leading to inadequate curing and adhesion issues on substrates like plastic films and glassine paper.

Method used

Incorporating an organopolysiloxane with trivinylsiloxane units and (meth)acrylic groups, along with a reduced amount of platinum group metal catalyst, to facilitate curing while maintaining peeling force and adhesion, even on substrates with catalyst poisons.

Benefits of technology

The solution enables curing with a small amount of platinum group metal catalyst, forming a cured film with equivalent peeling force to conventional methods, and allows application on substrates where curing was previously difficult, reducing manufacturing costs and improving adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148039000001
    Figure 2024148039000001
  • Figure 2024148039000002
    Figure 2024148039000002
  • Figure 2024148039000003
    Figure 2024148039000003
Patent Text Reader

Abstract

To provide a curable organopolysiloxane composition which is capable of undergoing an addition reaction in the presence of a small amount of a platinum group metal based catalyst and has curability comparable to the prior art, the curable organopolysiloxane composition being also capable of forming a cured film having peel strength comparable to the prior art, especially as release paper and release films, where curing by the addition reaction proceeds even if a base material contains a catalyst poison component.SOLUTION: The curable organopolysiloxane composition contains: (A) an organopolysiloxane which has two or more silicon atom-bonded alkenyl groups in each molecule but does not have three or more (meth)acrylic groups in each molecule; (B) an organohydrogen polysiloxane which has two or more silicon atom-bonded hydrogen atoms on average but does not have three or more (meth)acrylic groups in each molecule; (C) a compound which is other than an organopolysiloxane among compounds having one or more (meth)acrylic groups in each molecule, and which has a molecular weight from 72 to 1,000, or the like; and (D) a platinum group metal based catalyst.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable organopolysiloxane composition that can be cured with a small amount of platinum, and in particular to an organopolysiloxane composition for use in release papers or release films. [Background technology]

[0002] Organopolysiloxane compositions that cure via an addition reaction in the presence of a platinum catalyst can be heated at relatively low temperatures and cure completely in a short period of time. As a result, they have been used in a wide range of applications, including various coating agents, base polymers for paints, binders for molded products, and pressure sensitive adhesives.

[0003] However, the platinum group metals used as catalysts are rare precious metals on Earth, so they are expensive, and platinum catalysts account for a large proportion of the manufacturing cost in any application. For this reason, reducing the amount of platinum group metal catalyst used is the most effective way to reduce the price.

[0004] In addition, some of the raw materials used in production contain components that act as poisons to platinum group metal catalysts, such as nitrogen compounds, sulfur compounds, and phosphorus compounds, and the catalyst poisoning components combine with the platinum group metals, preventing the curing process from proceeding through the addition reaction. Therefore, there is a demand for a curable organopolysiloxane composition that is less susceptible to the effects of catalyst poisons.

[0005] An example of an application that utilizes the characteristics of this addition reaction curing with a platinum catalyst is release paper or release film, and it is known that in order to prevent adhesion or sticking between a sheet-like substrate such as paper or plastic and an adhesive material, a cured coating of an organopolysiloxane composition is formed on the surface of the substrate to impart release properties.

[0006] Conventionally, platinum group metal catalysts are often used in organopolysiloxane compositions for release paper or release film at a platinum group metal concentration of 100 to 500 ppm by mass. This is because, when the platinum concentration is less than 100 ppm by mass, the curing reaction does not proceed sufficiently, the cured film becomes soft, and the amount of remaining Si-H groups is large, resulting in high peel strength, and the unreacted raw material organopolysiloxane remains as a migratory component, which causes the organopolysiloxane to migrate to the adhesive surface to be bonded to the release paper, resulting in a decrease in adhesive strength.

[0007] Methods for solving these problems have been studied for some time, and WO 2020 / 004254 and WO 2020 / 145151 propose a method of adding a (meth)acrylic group-containing compound to a platinum-catalyzed addition curing composition. This method makes it possible to form a cured film with good peel strength and residual adhesion rate even with a smaller amount of platinum catalyst added than before.

[0008] International Publication No. 2021 / 020247 reports that when this method is used as a platinum catalyst composition, it is also possible to form a good cured coating with a smaller amount of platinum catalyst added than conventional methods.

[0009] However, for applications to substrates where it is difficult to obtain adhesion with a silicone cured film, such as plastic film substrates, or substrates where the addition-cured silicone composition cures more slowly than other substrates, such as glassine paper, it cannot be said that the amount of platinum catalyst added has been reduced while still providing sufficient curability and adhesion. There is potential demand in the current market for applications to these substrates, and there is a need for technological development that can solve this problem. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] International Publication No. 2020 / 004254 [Patent Document 2] International Publication No. 2020 / 145151 [Patent Document 3] International Publication No. 2021 / 020247 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been made in view of the above circumstances, and has as its object the provision of a curable organopolysiloxane composition, particularly for release papers or release films, which is capable of undergoing an addition reaction with a small amount of platinum group metal catalyst, is capable of forming a cured coating having the same release strength as conventional compositions, and is similarly applicable to plastic film substrates on which adhesion to a silicone cured coating is difficult to obtain, and to substrates on which curing of the silicone composition by addition reaction is difficult to proceed due to, for example, the inclusion of a catalyst poison component. [Means for solving the problem]

[0012] As a result of intensive research into achieving the above-mentioned object, the present inventors discovered that the above-mentioned problems can be solved by blending, as component (A), an organopolysiloxane having trivinylsiloxane units at the molecular terminals, and, as component (C), a compound having one or more (meth)acrylic groups per molecule, in an addition reaction curing organopolysiloxane composition, which led to the completion of the present invention.

[0013] Accordingly, the present invention provides the following curable organopolysiloxane composition, in particular a curable organopolysiloxane composition for release paper or release film (hereinafter sometimes simply referred to as organopolysiloxane composition). 1. A curable organopolysiloxane composition comprising the following components (A) to (D): (A) An organopolysiloxane having two or more silicon-bonded alkenyl groups per molecule, with an alkenyl group content of 0.001 to 0.7 mol / 100 g, and not having three or more (meth)acrylic groups per molecule, wherein 50% by mass or more of component (A) is a siloxane unit having at least one molecular terminal represented by the following formula (1): (CH2=CH-)3SiO1 / 2 (1) It is blocked off by The viscosity at 25°C measured using a rotational viscometer is 7 mPa s or more, and the viscosity when dissolved in 30% toluene (the viscosity of a solution in which 30% organopolysiloxane is dissolved in toluene) is 70,000 mPa s or less. Organopolysiloxane: 100 parts by mass, (B) an organohydrogenpolysiloxane having an average of two or more silicon-bonded hydrogen atoms (Si-H groups) per molecule and no more than three (meth)acrylic groups per molecule: an amount in which the number of moles of Si-H groups in component (B) corresponds to 1 to 10 times the number of moles of alkenyl groups in component (A); (C) one or more selected from the following (C-1) and (C-2): 0.01 to 5.0 parts by mass per 100 parts by mass of the (A) component, (C-1) A compound having one or more (meth)acrylic groups in one molecule, and having a molecular weight of 72 to 1,000 that is not an organopolysiloxane. (C-2) An organopolysiloxane having three or more (meth)acrylic groups in one molecule, the organopolysiloxane having a weight average molecular weight of 500 or more and 20,000 or less in terms of polystyrene, as determined by gel permeation chromatography (GPC) analysis (solvent: toluene). (D) Platinum group metal catalyst: an amount such that the platinum concentration in the total mass of the components (A), (B), (C), and (D) is 1 to 100 ppm by mass 2. The curable organopolysiloxane composition of 1, further comprising (E) a dilution solvent in an amount of 0 to 100,000 parts by mass per 100 parts by mass of component (A). 3. The curable organopolysiloxane composition of 1 or 2, further comprising 0.01 to 5.0 parts by mass of (F) a reaction inhibitor per 100 parts by mass of component (A). 4. The curable organopolysiloxane composition of any of 1 to 3, wherein component (B) contains 5 to 30 mol % of phenyl groups as a total number of substituents on Si atoms. 5. The curable organopolysiloxane composition according to any one of 1 to 4, wherein component (A) contains 1 to 20 mol % of the total number of substituents on Si atoms being phenyl groups. 6. Furthermore, (G) at least two alkenyl groups, R 10 (3-g1) R 9 g1 SiO 1 / 2 Siloxane unit (M R9R10 Units), R 10 SiO 3 / 2 Siloxane unit (T R10 Units) (wherein R 9 are each independently an alkenyl group; R 10 are each independently an unsubstituted or halogen- or cyano-substituted monovalent hydrocarbon group that does not contain an aliphatic unsaturated bond, and g1 is an integer of 1 to 3. R9R10 Unit / T R10 The molar ratio of units is 2 / 8 to 8 / 2, the viscosity at 25°C is in the range of 1 to 1,000 mPa s, and the molecular terminal is M R9R10 Unit or M R9R10 6. The curable organopolysiloxane composition according to any one of 1 to 5, comprising 0.1 to 20.0 parts by mass of an organopolysiloxane having units and a portion of which is a silanol group or an alkoxy group per 100 parts by mass of the component (A). 7. The curable organopolysiloxane composition according to any one of claims 1 to 6, wherein component (C) is an organopolysiloxane having one or more difunctional and / or trifunctional siloxane units having a (meth)acrylic group in one molecule. 8. The curable organopolysiloxane composition of any one of 1 to 7, further comprising (H) 0.01 to 5.0 parts by mass of an organic peroxide per 100 parts by mass of component (A). 9. The curable organopolysiloxane composition of claim 8, wherein component (H) is a polyfunctional organic peroxide having two or more peroxide bonds in the molecule. 10. Any of the curable organopolysiloxane compositions of 1 to 9, containing (D) a platinum group metal catalyst in an amount such that the platinum concentration in the combined mass of components (A) to (D) is 1 to 40 ppm by mass. 11. The curable organopolysiloxane composition according to any one of 1 to 10, which is used for a release paper or release film. 12. A method for producing a release paper or release film using the organopolysiloxane composition for release paper or release film described in 11. Effect of the Invention

[0014] According to the present invention, it is possible to provide a curable organopolysiloxane composition which is capable of undergoing an addition reaction with a small amount of a platinum group metal catalyst and has the same curability as conventional compositions, in particular an organopolysiloxane composition for release paper or release film which is capable of forming a cured coating having the same release strength as conventional compositions.

[0015] This makes it possible to form cured silicone films even under conditions where curing was previously difficult, significantly reducing manufacturing costs and making it possible to form cured films by addition reaction even on substrates containing catalyst poisons. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described in detail below. [Component (A)] The component (A) of the present invention is an organopolysiloxane having two or more silicon-bonded alkenyl groups per molecule, with an alkenyl group content of 0.001 to 0.7 mol / 100 g and not having three or more (meth)acrylic groups per molecule, wherein at least 50 mass % of component (A) is a siloxane unit represented by the following formula (1) at least one of the molecular terminals (CH2=CH-)3SiO 1 / 2 (1) and has a viscosity of 7 mPa s or more at 25°C as measured by a rotational viscometer, and a 30% by mass toluene solution viscosity (the viscosity of a solution in which 30% by mass of organopolysiloxane is dissolved in toluene) of 70,000 mPa s or less. The above organopolysiloxanes can be used alone or in appropriate combination of two or more.

[0017] An example of the component (A) is an organopolysiloxane having a structure represented by the following formula (2). M α M Vi β D γ D Vi δ T ε T Vi ζ Q η (2)

[0018] In the formula, M is RSiO 1 / 2 , M Vi is R a P (3-a) SiO 1 / 2 , D is RSiO 2 / 2 , D Vi is RPSiO 2 / 2 , T is RSiO 3 / 2 , T Vi is PSiO 3 / 2 , Q is SiO 4 / 2 where a is an integer of 0 to 3. In the formula, the letters α, δ, ε, ζ, and η each independently represent 0 or a positive number, and β and γ each represent a positive number.

[0019] The organopolysiloxane that accounts for 50 mass % or more of the component (A) is an organopolysiloxane having at least one molecular end blocked with a monofunctional siloxane unit of the above formula (1), and at least one M Vi corresponds to the above formula (1) where a is 0 (CH2=CH-)3SiO 1 / 2 It is a unit. This organopolysiloxane preferably accounts for 60 mass % or more of the component (A), and more preferably 70 mass % or more. If this organopolysiloxane accounts for less than 50 mass % of the component (A), the curability decreases.

[0020] The remaining 50% or less of component (A) may be an organopolysiloxane represented by formula (2) above, whose molecular ends are not blocked with the monofunctional siloxane unit of formula (1) above, but if more than 50% is used, the curability decreases.

[0021] In the above formula (2), each R is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms and no aliphatic unsaturated bonds, preferably having 1 to 10 carbon atoms, and more preferably having 1 to 8 carbon atoms.

[0022] Specific examples of R include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, and dodecyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, naphthyl, and tolyl; aralkyl groups such as benzyl and phenethyl; and groups in which a portion of the hydrogen atoms bonded to carbon atoms of these groups have been substituted with halogen atoms, epoxy groups, amino groups, polyether groups, cyano groups, hydroxyl groups, or the like.

[0023] Among these, in order to reduce the curability and the peel strength of the obtained cured product, it is preferable that 80 mol % or more of the total number of R are methyl groups. In order to further increase the adhesion to the film substrate, it is preferable that 1 to 20 mol % of the total number of R are aryl groups, more preferably 1 to 15 mol %, even more preferably 1 to 10 mol %, and even more preferably 1 to 5 mol %. For industrial purposes, a phenyl group is preferably used as the aryl group.

[0024] Furthermore, a part of R may be a (meth)acrylic group-containing group represented by the following formula (3). CH2=CR 1 COR 2 - (3)

[0025] However, one molecule should not contain more than three (meth)acrylic groups; if there are more than three, the peelability of the cured film decreases. 1 R is a hydrogen atom or a methyl group, and preferably a hydrogen atom. 2 OR 3 Or R 3 R is a divalent group represented by the formula: 3R is a divalent organic group having 1 to 20 carbon atoms, which may have a branched or cyclic structure, and may contain an epoxy group, an ester bond, a urethane bond, an ether bond, an isocyanate bond, or a hydroxyl group. 3 Examples of the divalent hydrocarbon groups include linear alkylene groups such as methylene, ethylene, propylene, butylene, hexamethylene, octamethylene, and decylene, branched alkylene groups such as methylethylene and methylpropylene, cyclic alkylene groups such as cyclohexylene, alkenylene groups such as propenylene, arylene groups such as phenylene, and aralkylene groups such as methylenephenylene and methylenephenylenemethylene. The divalent hydrocarbon groups may have ester bonds, urethane bonds, ether bonds, and isocyanate bonds between the carbon atoms. In addition, the divalent hydrocarbon groups having these bonds may include a plurality of types. Furthermore, some or all of the hydrogen atoms of these divalent hydrocarbon groups may be substituted with epoxy groups or hydroxyl groups. Among these, R 3 As the alkyl group, a propylene group is preferable.

[0026] Also, P is -(CH2) n It is an alkenyl group represented by -CH=CH2 (n is an integer of 0 to 8). n is preferably 0 to 8, 0 to 6, and more preferably 0 to 4. Specific examples include a vinyl group, an allyl group, a butenyl group, a propenyl group, a 5-hexenyl group, an octenyl group, and a decenyl group, and among these, a vinyl group is preferable.

[0027] In formula (2), the letters α, δ, ε, ζ, and η are each independently 0 or a positive number, β and γ are positive numbers, 2≦β+δ+ζ≦4,000, and preferably 2≦β+δ+ζ≦1,000. α is preferably 0 or 1 to 100, more preferably 1 to 80, and even more preferably 1 to 60, β is preferably 1 to 100, more preferably 1 to 80, and even more preferably 1 to 60, and α+β is preferably 2 to 200, more preferably 2 to 100, and even more preferably 2 to 50. δ is preferably 0 or 1 to 3,000, more preferably 1 to 2,000, and even more preferably 1 to 1,500. ζ is preferably 0 or 1 to 100, more preferably 0 or 1 to 40, and even more preferably 0 or 1 to 20.

[0028] Furthermore, γ is 5 to 27,000, preferably 10 to 20,000, more preferably 40 to 20,000, even more preferably 100 to 20,000, still more preferably 500 to 15,000, and even more preferably 1,000 to 15,000. When γ is less than 10, the kinetic viscosity of the organopolysiloxane composition is too low, and the coated surface may become rough. On the other hand, when γ exceeds 27,000, the kinetic viscosity of the organopolysiloxane composition becomes too high, and the coatability decreases, resulting in poor smoothness and a large difference in the amount of coating depending on the location.

[0029] In addition, ε is a positive number from 0 to 200, preferably a positive number from 0 to 20, and more preferably a positive number from 0 to 10. η is a positive number from 0 to 1,000, preferably a positive number from 0 to 10, and more preferably a positive number from 0 to 5.

[0030] The alkenyl group content of the (A) component is 0.001 to 0.7 mol / 100 g, more preferably 0.002 to 0.5 mol / 100 g, even more preferably 0.003 to 0.1 mol / 100 g, and even more preferably 0.005 to 0.07 mol / 100 g. If the alkenyl group content is less than 0.001 mol / 100 g, there may be too few reaction sites, resulting in poor curing, whereas if the alkenyl group content exceeds 0.7 mol / 100 g, the crosslink density may be too high, resulting in too high low-speed peel strength or difficulty in peeling.

[0031] The number average molecular weight of component (A) is preferably 800 or more and 2 million or less, more preferably 3,000 or more and 1 million or less. When a composition is prepared using a dilution solvent for component (E), more preferable results can be obtained by increasing the number average molecular weight of component (A) to 10,000 or more. If the number average molecular weight of component (A) is lower than 800, the amount of coating on the substrate may be insufficient. If it exceeds 2 million, the workability may be reduced. In the present invention, the number average molecular weight can be measured by the number average molecular weight converted into polystyrene by gel permeation chromatography (GPC) analysis (solvent: toluene) (hereinafter the same).

[0032] In the present invention, the number average molecular weight by GPC analysis is a value measured under the following measurement conditions. Equipment: Tosoh Corporation high-speed GPC system HLC-8320 Analytical column: TSKgel SuperHZ manufactured by Tosoh Corporation Developing solvent: toluene Flow rate: 0.35mL / min Column temperature: 40℃ Sample input volume: 2,500 μL Detector: RI Molecular weight calculation: Polystyrene-equivalent molecular weight calculated using a calibration curve created from the analysis values ​​of polystyrene molecular weight standard samples

[0033] The viscosity of component (A) measured at 25°C using a rotational viscometer is preferably 7 mPa·s or more and 70,000 mPa·s or less when dissolved in 30% by mass toluene (viscosity of a solution in which 30% by mass of organopolysiloxane is dissolved in toluene), more preferably 10 mPa·s or more and 60,000 mPa·s or less when dissolved in 30% by mass toluene, even more preferably 30 mPa·s or more and 50,000 mPa·s or less when dissolved in 30% by mass toluene, and even more preferably 50 mPa·s or more and 40,000 mPa·s or less when dissolved in 30% by mass toluene. When a composition is prepared using a dilution solvent for component (E), more preferable results can be obtained by increasing the viscosity of component (A) measured at 25°C using a rotational viscometer to 30,000 mPa·s or more, or to 100 mPa·s or more when dissolved in 30% by mass toluene. If the viscosity is less than 7 mPa·s, the amount of coating may be insufficient. Furthermore, if the viscosity of the 30% by mass toluene solution exceeds 70,000 mPa·s, workability may decrease.

[0034] In the present invention, the viscosity of the component (A) is a value measured using a BM type viscometer (for example, manufactured by Tokyo Keiki Co., Ltd.) The rotor, rotation speed, and rotation time are appropriately selected according to the viscosity based on conventional methods.

[0035] The viscosity of a 30% by mass solution of organopolysiloxane in toluene was measured by adding 150 g of organopolysiloxane to 350 g of toluene, mixing and stirring until the organopolysiloxane was dissolved, and then measuring the viscosity using the above-mentioned viscosity measurement method.

[0036] Specific examples of such component (A) include siloxanes containing alkenyl groups at both ends, siloxanes containing alkenyl groups at the side chain, siloxanes containing alkenyl groups at one end and at the side chain, siloxanes containing alkenyl groups at both ends and at the side chain, branched siloxanes containing alkenyl groups at both ends, and branched siloxanes containing alkenyl groups at both ends and in the side chain.

[0037] The organopolysiloxane may be one represented by the following structural formula: M Vi 2Dγ , M.M. Vi D γ , M2D γ D Vi δ , M.M. Vi D γ D Vi δ , M Vi 3D γ T1, MM Vi 2D γ T1,M Vi 4D γ T2, M Vi 2D γ D Vi δ , M Vi 2D γ Q1, M.M. Vi D γ Q1, M α D γ D Vi δ T Vi ζ , M α M Vi α D γ D Vi δ T Vi ζ (M, M vi , D, D Vi , T, T vi , Q, γ, δ, and ζ are the same as in formula (2) above. The same applies below.)

[0038] Further specific structural examples include the following: M Vi 2D 100 , M2D 97 D Vi 3. M.M. Vi D 97 D Vi 3. M2D 26 D Vi 4. M2D 96 D Vi 4. M2D 95 D Vi 5. M.M. Vi D 95 D Vi 5. M Vi 3D 100T1, M Vi 4D 100 T2, MM Vi D 100 T2, M Vi 2D 97 D Vi 1. M.M. Vi D 97 D Vi 1. M Vi 2D 95 D Vi 3. M.M. Vi D 95 D Vi 3. M3D 93 D Vi 3T Vi 1. M2M Vi D 93 D Vi 3T Vi 1. M Vi 2D 20000 , M.M. Vi D 20000 , M2D 10000 D Vi 20、 MM Vi D 10000 D Vi 20 , M Vi 2D 100γ Q1, M.M. Vi D 200 Q1.

[0039] [(B) Component] The (B) component is an organohydrogenpolysiloxane having an average of two or more silicon-bonded hydrogen atoms (Si-H groups) per molecule and not having three or more (meth)acrylic groups per molecule (i.e., not including the (C) component described below), and may be used alone or in suitable combination of two or more. An organopolysiloxane crosslinked product is formed by addition reaction of the Si-H groups of this organohydrogenpolysiloxane with the alkenyl groups of the (A) component.

[0040] The organohydrogenpolysiloxane of component (B) preferably has 3 to 100, and more preferably 10 to 80, silicon-bonded hydrogen atoms (Si—H groups) per molecule.

[0041] The Si-H group content is preferably 0.001 to 3.5 mol / 100 g, more preferably 0.01 to 2.5 mol / 100 g, even more preferably 0.02 to 2.0 mol / 100 g, and even more preferably 0.1 to 1.7 mol / 100 g. If the Si-H group content is too low, the curing property and adhesion may deteriorate, and if it is too high, the peeling force may become heavy.

[0042] The organohydrogenpolysiloxane of the component (B) preferably has a structure represented by the following formula (4). M ο M H π D ρ D H σ T τ T H φ Q χ (4)

[0043] In the formula, M is R'SiO 1 / 2 , M H is R'2HSiO 1 / 2 , D is R'2SiO 2 / 2 , D H R'HSiO 2 / 2 , T is R'SiO 3 / 2 , T H HSiO 3 / 2 , Q is SiO 4 / 2 and R' is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 12 carbon atoms and no aliphatic unsaturated bonds. ο, π, ρ, and τ are independently 0 or a positive number, π is 0 or a positive number from 1 to 40, σ is a positive number from 0 to 100, φ is a positive number from 0 to 10, and χ is a positive number from 0 to 10, where π, σ, and φ are not 0 at the same time, and 2≦π+σ+φ≦100.)

[0044] In the above formula (4), R' can be exemplified as the same as R in the above formula (2), and among these, a monovalent hydrocarbon group having 1 to 8 carbon atoms is preferable.

[0045] Specific examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, and dodecyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, naphthyl, and tolyl; aralkyl groups such as benzyl and phenethyl; and groups in which some of the hydrogen atoms bonded to carbon atoms in these groups have been substituted with halogen atoms, epoxy groups, or polyether groups.

[0046] When it is necessary to further improve the adhesion to the film substrate, aryl groups preferably account for 5 to 30 mol %, more preferably 6 to 25 mol %, of the total number of R' and H. Industrially, phenyl groups are preferably used as the aryl groups.

[0047] In the above formula (4), o, π, ρ, and τ are each independently 0 or a positive number, o is preferably 0 or 1 to 10, more preferably 0 or 1 to 8, and even more preferably 0 or 1 to 5. π is preferably 0 or 1 to 10, more preferably 0 or 1 to 8, and even more preferably 0 or 1 to 5, and o+π is preferably 2 to 12, and even more preferably 2 to 10. ρ is preferably 0 or 1 to 100, more preferably 0 or 1 to 8, and even more preferably 0 or 1 to 5, and τ is preferably 0 or 1 to 10, more preferably 1 to 8, and even more preferably 1 to 5. σ is a positive number of 0 to 100, preferably 2 to 100, and more preferably 10 to 80. φ is a positive number of 0 to 10, preferably 0 to 5, and χ is a positive number of 0 to 10, preferably 0 to 5. In addition, π, σ, and φ are not 0 at the same time, and π+σ+φ is 3-100, and preferably 10-80.

[0048] Specific examples of the organohydrogenpolysiloxane of component (B) include siloxanes containing hydrogensilyl groups at both ends, siloxanes containing hydrogensilyl groups in the side chain, siloxanes containing hydrogensilyl groups at one end and in the side chain, siloxanes containing hydrogensilyl groups at both ends and in the side chain, siloxanes containing branched hydrogensilyl terminal groups, and branched siloxanes containing hydrogensilyl groups at the end and in the side chain.

[0049] The organohydrogenpolysiloxane may be one represented by the following structural formula: M H 2D ρ , M2D H σ , M2D ρ D H σ , M H 2D ρ D H σ , M H 3D ρ T1, M H 4D ρ T2, M ο D ρ D H σ T H φ M ο D ρ D H σ T H φ Q χ (M, M H , D, D H , T, T H , Q, ο, ρ, σ, φ, and χ are the same as in formula (4) above. The same applies below.)

[0050] Further specific structural examples include the following: M H 2D 10 , M H 2D 100 , M2D H 80 , M2D 27 D H 3. M2D 97 DH 3. M2D 26 D H 4. M2D 25 D H 5. M2D 24 D H 6. M2D 96 D H 4. M2D 95 D H 5. M H 3D 100 T1, M H 4D 100 T2, M H 2D 97 D H 1、 M H 2D 95 D H 3. M3D 93 D H 3T H 1、 M5D 10 D H 40 T1Q1, M5D 10 D H 40 T H 1Q1, M H 5D 10 D H 40 T1Q1, M2D H 30、 M2D H 60

[0051] The number average molecular weight of component (B) is preferably 194 to 10,000, and more preferably 874 to 5,000. If the number average molecular weight of component (B) is too small, adhesion may be significantly reduced, whereas if it is too large, reactivity may be poor and curing properties may decrease, resulting in a decrease in residual adhesion rate and an increase in peel strength due to insufficient curing.

[0052] The kinetic viscosity of component (B) at 25°C measured using an Ostwald viscometer is 2 to 500 mm 2 / s is preferable, and 2 to 300 mm 2 / s is more preferable, and 5 to 200 mm 2 / s is more preferable. 2If the molecular weight is less than 500 mm / s, the reactivity is good due to the small molecular weight, but the adhesion to the substrate may deteriorate. 2 If it exceeds this limit, the reactivity will deteriorate and the curing property will decrease, resulting in a decrease in the residual adhesion rate and an increase in the peel force due to insufficient curing.

[0053] The amount of component (B) is an amount corresponding to 1.0 to 10.0 times the number of moles of Si-H groups in component (B) relative to the number of moles of alkenyl groups in component (A), preferably 1.2 to 6.0 times, more preferably 1.5 to 6.0, and even more preferably 2.0 to 6.0. If the amount of component (B) is too small, the curing property and adhesion become insufficient, while if the amount of component (B) is too large, the amount of remaining Si-H groups increases, resulting in a high peel force, and the number of Si-H groups decreases over time, resulting in a fluctuation in peel force over time.

[0054] [(C) component] The component (C) of the present invention is (C-1) a compound having one or more (meth)acrylic groups in one molecule, which is not an organopolysiloxane, and has a molecular weight of 72 to 1,000, and / or (C-2) an organopolysiloxane having three or more (meth)acrylic groups in one molecule, the organopolysiloxane having a weight average molecular weight of 500 to 20,000 in terms of polystyrene as determined by gel permeation chromatography (GPC) analysis (solvent: toluene). The component (C) may be used alone or in appropriate combination of two or more. The upper limit of the weight average molecular weight of the component (C-2) is preferably 10,000 or less, more preferably 5,000 or less. In addition, the molecular weight of the component (C) is, in the case of a siloxane, 29 The measurement can be performed by Si-NMR. For the Si-NMR, for example, Win Lambda manufactured by JEOL Ltd. can be used. The measurement method is to put 1.5 g of sample and 3.5 g of d-chloroform into a Teflon (registered trademark) sample tube with a diameter of 10 mm, stir well, set it in the Si-NMR, and perform measurement with an accumulation number of 600 times.

[0055] The compound other than the organopolysiloxane (C-1) is, for example, a compound having one (meth)acrylic group represented by the following formula (5). CH2=CR 4 COOR 5 (5) (In the formula, R 4 is a hydrogen atom or a methyl group, R 5 is a hydrogen atom, or an alkyl group, aryl group, or aralkyl group having 1 to 20 carbon atoms, which may have a branched or cyclic structure, and which may contain an epoxy group, a urethane bond, an ether bond, an isocyanate bond, or a hydroxyl group.

[0056] R 5 Specific examples of R include a methyl group, an ethyl group, a propyl group, a butyl group, a hexyl group, a cyclohexyl group, a phenyl group, a dicyclopentanyl group, a dicyclopentenyl group, a furfuryl group, a tetrahydrofuryl group, a tetrahydropyranyl group, -CH2CH2-OH, -CH2CH(CH3)-OH, and -CH2CH2-NCO. 5 Examples of compounds having an epoxy group include the following: The compound having a (meth)acrylic group and an epoxy group may be an oligomer.

[0057] Specific examples of the compound having one (meth)acrylic group and a molecular weight of 72 to 1,000 include 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, acrylic acid, butyl acrylate, methyl acrylate, and ethyl acrylate.

[0058] A specific example of the compound having a (meth)acrylic group and an epoxy group is 4-hydroxybutyl acrylate glycidyl ether.

[0059] Specific examples of copolymers having two (meth)acrylic groups and a molecular weight of 200 to 1,000 include tetraethylene glycol diacrylate, nonaethylene glycol diacrylate, tetradecanyl ethylene glycol diacrylate, tricyclodecane dimethanol diacrylate, 1,10-decanediol diacrylate, 1,6-hexanediol diacrylate, 1,9-nonanediol diacrylate, dipropylene glycol diacrylate, heptapropylene glycol diacrylate, and trimethylolpropane triacrylate.

[0060] When (C-2) organopolysiloxane is used as component (C), it is preferable that it does not have an aliphatic unsaturated bond other than the (meth)acrylic group. Here, the (meth)acrylic group means an acrylic group or a methacrylic group. Among them, it is preferable that it has an acrylic group. It is more preferable that at least one of the (meth)acrylic groups exists as a substituent on the difunctional siloxane unit and / or the trifunctional siloxane unit.

[0061] The organopolysiloxane includes cyclic siloxanes and organopolysiloxanes having linear and branched structures.

[0062] The organopolysiloxane (C-2) preferably has 3 or more siloxane units having (meth)acrylic groups, more preferably 3 to 6. Furthermore, it is preferable that the organopolysiloxane has no Si-H groups and no alkenyl groups.

[0063] The cyclic siloxane is preferably one represented by the following structural formula (6). D 1A d' (6) (In the formula, D 1A is R 6 ASiO 2 / 2 and R 6 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, or an alkoxy group, a hydrogen atom, a hydroxyl group, an epoxy group, or a polyoxyalkylene group, and A is CH2=CR 1 COR2 - and R 1 is a hydrogen atom or a methyl group, R 1 OR 3 Or R 3 and R 3 is a divalent group having 1 to 20 carbon atoms, which may have a branched or cyclic structure, and may contain an epoxy group, an ester bond, a urethane bond, an ether bond, an isocyanate bond, or a hydroxyl group. d' is 3 to 6.

[0064] As the organopolysiloxane having a linear or branched structure, an organopolysiloxane having three or more (meth)acrylic groups on the side chain, represented by the following formula (7), is preferred. M 1 a M 1A b D 1 c D 1A d T 1 e T 1A f Q 1 g (7) (In the formula, M 1 is R 6 3SiO 1 / 2 , M 1A is R 6 2ASiO 1 / 2 , D 1 is R 6 2SiO 2 / 2 , D 1A is R 6 ASiO 2 / 2 , T 1 is R 6 SiO 3 / 2 , T 1A ASiO 3 / 2 , Q 1 SiO 4 / 2 and R 6 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, an alkoxy group, a hydrogen atom, a hydroxyl group, an epoxy group, or a polyoxyalkylene group. A is CH2=CR 1 COR 2 - and R 1is a hydrogen atom or a methyl group, R 2 OR 3 Or R 3 and R 3 is a divalent group having 1 to 20 carbon atoms, which may have a branched or cyclic structure and may contain an epoxy group, an ester bond, a urethane bond, an ether bond, an isocyanate bond, or a hydroxyl group. a is an integer from 0 to 20, b is an integer from 0 to 5, and when a is 0, b is an integer from 2 to 5, when a is 1, b is an integer from 1 to 5, and when a is 2 to 20, b is an integer from 0 to 5. c is an integer from 0 to 300, d is an integer from 0 to 200, e and f are both integers from 0 to 10, g is 0 to 5, and b+d+f is 3 or more.

[0065] In the above formulas (6) and (7), R 6 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, or an alkoxy group, a hydrogen atom, a hydroxyl group, an epoxy group, or a polyoxyalkylene group, preferably having 1 to 12 carbon atoms, and more preferably having 1 to 8 carbon atoms. Specific examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, and dodecyl groups; alkenyl groups such as vinyl, allyl, butenyl, propenyl, 5-hexenyl, octenyl, and decenyl groups; cycloalkyl groups such as cyclohexyl groups; aryl groups such as phenyl, naphthyl, and tolyl groups; aralkyl groups such as benzyl and phenethyl groups; and groups in which a portion of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with halogen atoms, epoxy groups, amino groups, polyether groups, cyano groups, and hydroxyl groups. Specific examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, etc. Examples of the polyoxyalkylene group include a polyoxyethylene group, a polyoxypropylene group, etc.

[0066] Here, R 1 R is a hydrogen atom or a methyl group, and preferably a hydrogen atom. 2 OR 3 Or R 3 and R 3R is a divalent group having 1 to 20 carbon atoms, which may have a branched or cyclic structure, and may contain an epoxy group, an ester bond, a urethane bond, an ether bond, an isocyanate bond, or a hydroxyl group. 3 Specific examples of the divalent hydrocarbon groups include linear alkylene groups such as methylene, ethylene, propylene, butylene, hexamethylene, octamethylene, and decylene, branched alkylene groups such as methylethylene and methylpropylene, cyclic alkylene groups such as cyclohexylene, alkenylene groups such as propenylene, arylene groups such as phenylene, and aralkylene groups such as methylenephenylene and methylenephenylenemethylene. These divalent hydrocarbon groups may be mediated by ester bonds, urethane bonds, ether bonds, and isocyanate bonds, and these may also be used in combination. Furthermore, some or all of the hydrogen atoms of these divalent hydrocarbon groups may be substituted with epoxy groups or hydroxyl groups. Among these, R 3 As the alkyl group, a propylene group is preferable.

[0067] In formula (7), a is an integer of 0 to 20, and b is an integer of 0 to 5, and when a is 0, b is an integer of 2 to 5, when a is 1, b is an integer of 1 to 5, and when a is 2 to 20, b is an integer of 0 to 5. a is preferably 2 or 3, and in that case, b is preferably 0.

[0068] c is an integer of 0 to 300, preferably an integer of 5 to 200, more preferably an integer of 10 to 100, and even more preferably an integer of 15 to 70.

[0069] d is an integer of 0 to 200, preferably an integer of 3 to 50, more preferably an integer of 3 to 30, and further preferably an integer of 3 to 20. Although the invention can be carried out even if d is less than 3, the curability may decrease depending on other conditions, such as a small amount of catalyst. Also, if d exceeds 200, the curability may decrease.

[0070] Both e and f are integers of 0 to 10, preferably integers of 0 to 6, and more preferably integers of 0 to 3. When e is 10 or more, the curing property may decrease, although the reason is not clear. Similarly, when f is 10 or more, the curing property may decrease.

[0071] g is 0 to 5, and is preferably 0 or 1. When g exceeds 5, it is not preferable because it becomes difficult to control the viscosity during production and the peeling force becomes large.

[0072] Specific examples of (C-2) organopolysiloxane compounds having three or more (meth)acrylic groups and a molecular weight of 500 or more include the following. D 1A 3. D 1A 4. D 1A 5. M 1 2D 1A 3D 1 2. M 1 3D 1A 3T 1 1. M 1 3D 1A 2T 1A , M 1 2D 1 5D 1A 3. M 1 2D 1 20 D 1A 5、 M 1Vi 2D 1 20 D 1A 5、 M 1 2D 1 30 D 1A 7. M 1φ 2D 1 30 D 1A 7、 M 1 2D 1 25 D 1φ 5D 1A 7、 M 1 2D 1 65 D 1A 15 , M1Vi 2D 1 65 D 1A 15、 M 1 2D 1 61 D 1OH 4D 1A 15、 M 1 2D 1 63 D 1OSiR’ 2D 1A 15、 M 1H 2D 1 65 D 1A 15、 M 1 1M 1A 1D 1 10 D 1A 3、M 1OSiR’ 2D 1 20 D 1A 5、M 1 2D 1 20 D 1A 5、M 1 2D 1 32 D 1A 5、 M 1A 2D 1 37 D 1A 8、 M 1 3D 1 20 D 1A 5T 1 1、M 1 3D 1 110 D 1A 6T 1 1、M 1 2D 1 170 D 1A 22 、M 1 2D 1 170 D 1A 20 Q 1 1、M 1 3D 1 180 D 1A 18 T1 1 (In the formula, M 1Vi is R 7 2(CH2=CH)SiO 1 / 2 , M 1φ is R 7 2(C6H5)SiO 1 / 2 , M 1H is R 7 2(H)SiO 1 / 2 , M 1OSiR’ is R 7 2(OSiR 8 3) SiO 1 / 2 , D 1φ is R 7 (C6H5)SiO 2 / 2 , D 1OH is R 7 (OH)SiO 2 / 2 , D 1OSiR’ is R 7 (OSiR 8 3) SiO 2 / 2、 T 1 is R 7 SiO 3 / 2 , T 1A ASiO 3 / 2 , Q 1 SiO 4 / 2 and R 7 , R 8 is an alkyl group having 1 to 6 carbon atoms, such as a methyl group or an ethyl group, and (C6H5) represents a phenyl group. A is the same as in the above formula (7).

[0073] The amount of component (C) is 0.01 to 5.0 parts by mass, and preferably 0.1 to 2.0 parts by mass, per 100 parts by mass of component (A). If it is less than 0.01 part by mass, the cure acceleration effect is not clear, while if it exceeds 5.0 parts by mass, the amount of migrating components increases, and a decrease in the residual adhesion rate and deterioration of adhesion may be observed.

[0074] The manufacturing method of component (C) is 1 2. M 1 2D 1 3. M 1A 2. D 1A 4. D 1 4(M 1 , M 1A , D 1 , D1A is the same as the above formula (6). It can be obtained by blending raw materials such as dimethyl ether, ...

[0075] [(D) component] The platinum group metal catalyst (D) of the present invention can be known as an addition reaction catalyst.Such platinum group metal catalyst can be, for example, platinum, palladium, rhodium, ruthenium, etc., and among these, platinum catalyst is particularly preferably used.This platinum catalyst can be, for example, platinum compound, platinum and vinylsiloxane complex, chloroplatinic acid alcohol solution or aldehyde solution, chloroplatinic acid and various olefin complex salts, chloroplatinic acid and vinylsiloxane complex, etc.

[0076] The amount of component (D) is a catalytic amount. Usually, the platinum group metal concentration in the organopolysiloxane composition for release paper or film for producing a cured film is 100 to 500 ppm by mass in the organopolysiloxane composition for release paper or film. The amount of platinum group metal catalyst in the present invention is 1 to 100 ppm, preferably 1 to 60 ppm, more preferably 1 to 40 ppm, and most preferably 1 to 30 ppm, calculated as platinum group metal mass relative to the total mass of the organopolysiloxane composition (total mass of components (A) to (D)).

[0077] [(E) component] The dilution solvent for component (E) is an optional component and is not used when the composition of the present invention is used as a solventless type, but when component (A) is a high-viscosity organopolysiloxane, the dilution solvent reduces the viscosity of the composition, making it easier to apply a thin film onto a substrate. In addition, it acts as a compatibilizer and solvent to prevent the separation of the multiple different components that make up the organopolysiloxane composition, providing a coating solution with a uniform composition, and imparts good leveling and wettability to the organopolysiloxane composition layer applied to various substrates, making it possible to form a silicone cured coating of uniform thickness and with a smooth and highly smooth surface.

[0078] In particular, it is often an essential component when coating on plastic film substrates, which require surface smoothness and a highly transparent appearance.

[0079] Dilution solvents include various organic solvents, aromatic solvents such as toluene and xylene, aliphatic solvents such as hexane and heptane, ketone solvents such as acetone and methyl ethyl ketone (also known as 2-butanone), ester solvents such as ethyl acetate, and ether solvents such as diethyl ether. These solvents are soluble in organopolysiloxanes (not including siloxane solvents), as well as low-viscosity cyclic siloxanes such as octamethyltetrasiloxane and decamethylpentasiloxane, M2D p (wherein M and D are the same as those in the above formula (2), and p is a number from 0 to 200, preferably from 1 to 50), 2+q D p T q (wherein M, D, and T are the same as in formula (2) above, p is 0 to 200, preferably 1 to 50, and q is 1 to 10, preferably 1 to 3) or other branched-chain siloxanes (siloxane solvents) can be used.

[0080] When a dilution solvent is used, it is 1 to 100,000 parts by mass per 100 parts by mass of the organopolysiloxane of component (A), and if it is less than 1 part by mass, the viscosity is too high, and if it exceeds 100,0000 parts by mass, the viscosity is too low and the coatability is reduced. It is more preferable that it is 1,000 to 10,000 parts by mass.

[0081] [Component (F)] The addition reaction inhibitor (F) of the present invention is a component that is added as necessary to control the catalytic activity of the platinum group metal catalyst. Examples of such an inhibitor include various organic nitrogen compounds, organic phosphorus compounds, acetylene compounds, oxime compounds, and organic chloro compounds. Specific examples of the compound include acetylenic alcohols such as 1-ethynyl-1-cyclohexanol, 3-methyl-1-butyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 3-methyl-1-penten-3-ol, and phenylbutynol; acetylenic compounds such as 3-methyl-3-1-penten-1-yne and 3,5-dimethyl-1-hexyn-3-yne; reaction products of acetylenic compounds such as 1,1-dimethylpropynyloxytrimethylsilane with alkoxysilanes, siloxanes, or hydrogensilanes; vinyl siloxanes such as tetramethylvinylsiloxane cyclic compounds; organic nitrogen compounds such as benzotriazole and other organic phosphorus compounds; oxime compounds; maleic acid compounds such as diallyl maleate; and organic chloro compounds.

[0082] The amount of the component (F), when blended, is preferably 0.01 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the component (A).

[0083] [(G) component] As the component (G), a component that improves the adhesion to the substrate can be blended. The component (G) has at least two alkenyl groups, and R 10 (3-g1) R 9 g1 SiO 1 / 2 Siloxane unit (M R9R10 Units), R 10 SiO 3 / 2 Siloxane unit (T R10 Units) (wherein R 9 are each independently an alkenyl group; R 10 are each independently an unsubstituted or halogen- or cyano-substituted monovalent hydrocarbon group that does not contain an aliphatic unsaturated bond, and g1 is an integer of 1 to 3.R9R10 Unit / T R10 The molar ratio of units is 2 / 8 to 8 / 2, the viscosity at 25°C is in the range of 1 to 1,000 mPa s, and the molecular terminal is M R9R10 Unit or M R9R10 It is an organopolysiloxane in which the units and some of the units are silanol groups or alkoxy groups. The molecular terminals are M R1R2 It is preferable that the units are bonded, but some of them may be silanol groups or alkoxy groups to form terminals.

[0084] In the above formula, R 9 R can be exemplified by the same alkenyl groups as P in the above formula (2), and among these, vinyl groups are industrially preferred. 10 Specific examples of g1 include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, and dodecyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, naphthyl, and tolyl; and aralkyl groups such as benzyl and phenethyl. Of these, methyl and phenyl are industrially preferred. g1 is an integer of 1 to 3, and preferably 1 or 2.

[0085] The component (G) is the above M R9R10 Unit / T R10 The molar ratio of the units in this organopolysiloxane is 2 / 8 to 8 / 2, and preferably 3 / 7 to 7 / 3. If the molar ratio is less than 2 / 8, the effect of improving adhesion may be small, and if it exceeds 8 / 2, industrial production becomes difficult.

[0086] In addition, bifunctional R 10 (2-g2) R 9 g2 SiO 2 / 2 Siloxane units (wherein g2 is 0, 1 or 2. D R9R10 (denoted as unit), tetrafunctional SiO 4 / 2 Siloxane units (Q units) may be included, but when stronger adhesion is required, particularly in release films, M units not including them are preferred.R9R10 Unit / T R10 Siloxanes with a molar ratio of units of 2 / 8 to 8 / 2 are preferred. R9R10 If a unit or Q unit is included, M must be included. R9R10 Units and T R10 Use a small amount relative to any one unit.

[0087] The (G) component is T R10 The unit is D R9R10 It differs from component (A) in that it contains more than units.

[0088] The amount of alkenyl groups in the organopolysiloxane of component (G) is preferably 0.01 to 2.5 mol / 100 g, more preferably 0.03 to 2.0 mol / 100 g, and even more preferably 0.05 to 1.5 mol / 100 g. If this content is too low, the effect of improving adhesion may be reduced, and if it is too high, the pot life may be shortened.

[0089] The organopolysiloxane of component (G) preferably has a viscosity at 25°C of 1 to 1,000 mPa·s, particularly preferably 5 to 500 mPa·s, more preferably 10 to 100 mPa·s, and even more preferably 10 to 50 mPa·s, and it is preferable that the organopolysiloxane has a degree of polymerization within this viscosity range. If the viscosity is less than 1 mPa·s, the effect of improving adhesion may be small, and if it exceeds 1,000 mPa·s, solubility or dispersibility in the composition may decrease.

[0090] Specific examples of the component (G) include the following: [ka] (In the formula, Me represents a methyl group, Vi represents a vinyl group, and Ph represents a phenyl group.)

[0091] When component (G) is used, the amount is preferably 0.1 to 20 parts by mass, and more preferably 0.15 to 10 parts by mass, per 100 parts by mass of component (A). If the amount is less than 0.1 part by mass, the effect of improving adhesion to the substrate may be reduced, whereas if the amount is more than 20 parts by mass, the release properties of the cured coating may decrease.

[0092] When adding component (G), it is desirable to add component (C) in an amount such that the ratio of the number of moles of SiH groups in component (C) to the number of moles of alkenyl groups in component (G) (SiH groups / alkenyl groups) is 1 or more, and particularly 1 to 5, in order to prevent a decrease in the release properties of the cured coating.

[0093] [Optional ingredients] The organopolysiloxane composition of the present invention may contain components that are usually added to organopolysiloxane compositions for release papers or films, provided that the effects of the present invention are not impaired.

[0094] The properties are not deteriorated even when the composition is diluted with an organic solvent.

[0095] Examples of optional added components include high molecular weight linear organopolysiloxanes other than components (A) to (C) for the purpose of imparting slip properties, silicone resins having aryl groups other than components (A) to (C) for the purpose of adjusting release force, silicone resins, silica, and low molecular weight organopolysiloxanes having neither hydrogen atoms bonded to silicon atoms nor alkenyl groups.

[0096] [Manufacturing method] The organopolysiloxane composition of the present invention can be obtained by mixing the above-mentioned components (A) to (D) and, if necessary, the components (E) to (G) and any optional components in predetermined amounts.

[0097] The viscosity of the resulting organopolysiloxane composition at 25° C., as measured with an Ostwald viscometer, is preferably from 1 to 100 mPa·s, and more preferably from 5 to 50 mPa·s.

[0098] [Applications / How to use] The organopolysiloxane composition of the present invention is applied to a sheet-like substrate such as paper or plastic film using a coating roll (three-roll, five-roll, gravure roll, offset gravure roll, etc.), and then cured by heating in a conventional manner. In this way, a silicone cured coating of the organopolysiloxane composition of the present invention is formed on one side of the sheet-like substrate, and is suitably used as a release sheet, etc.

[0099] Examples of the paper substrate include glassine paper, polyethylene laminated paper, polyvinyl alcohol resin-coated paper, clay-coated paper, etc. Examples of the plastic film substrate include films of polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate, etc.

[0100] The amount of the organopolysiloxane composition applied may be an amount sufficient to form a silicone cured film on the surface of the sheet-like substrate, and may be, for example, 0.1 to 50.0 g / m 2 Applying too much of the adhesive may result in a decrease in the peeling performance.

[0101] The conditions for heat curing vary depending on the type of substrate and the amount of coating, but a cured coating can be formed on the substrate by heating at 80 to 200°C, preferably 100 to 180°C, for 1 to 60 seconds, preferably 2 to 30 seconds.

[0102] The peeling force for tesa7475 tape (tesa UK Ltd.) is preferably 0.4 N or less, more preferably 0.10 to 0.40 N. The peeling force for the BPS-5127 transfer method is preferably 0.1 N or less, more preferably 0.04 to 0.1 N.

[0103] The residual adhesion rate is preferably 91% or more, and more preferably 94% or more. EXAMPLES

[0104] The present invention will be described in detail below with reference to examples and comparative examples. However, the present invention is not limited to the following examples. The average molecular weights shown below are 29 The viscosity was determined by Si-NMR, and the viscosity was measured at 25°C using a rotational viscometer. The kinetic viscosity was measured at 25°C using an Ostwald type viscometer.

[0105] [Raw materials used] Component (A) Methylvinylpolysiloxane (A1) Polysiloxane with the following structure, vinyl value of 0.0073 mol / 100 g, and viscosity of 30% by mass toluene solution at 25°C of 20,000 mPa s {(CH2=CH)3SiO 1 / 2}2{(CH2=CH)(CH3)SiO 2 / 2} 48 {(CH3)2SiO 2 / 2} 10000 Methylvinylpolysiloxane (A2): No siloxane unit represented by formula (1) Polysiloxane with the following structure, vinyl value of 0.0067 mol / 100 g, and viscosity of 30% by weight toluene solution at 25°C of 20,000 mPa s {(CH2=CH)(CH3)2SiO 1 / 2}2{(CH2=CH)(CH3)SiO 2 / 2} 48 {(CH3)2SiO 2 / 2} 10000 Methylvinylpolysiloxane (A3) Polysiloxane with the following structure, vinyl value of 0.051 mol / 100 g, and viscosity of 400 mPa s at 25°C {(CH2=CH)3SiO 1 / 2}2{(CH3)2SiO 2 / 2} 155 Methylvinylpolysiloxane (A4): No siloxane unit represented by formula (1) Polysiloxane with the following structure, vinyl value of 0.017 mol / 100 g, and viscosity of 400 mPa s at 25°C {(CH2=CH)(CH3)2SiO 1 / 2}2{(CH3)2SiO 2 / 2} 155 Methylphenylvinylpolysiloxane (A5): No siloxane unit represented by formula (1) Polysiloxane with the following structure, vinyl value of 0.002 mol / 100 g, phenyl group content of 2 mol%, and viscosity of 30 mass% toluene solution at 25°C of 800 mPa s {(CH2=CH)(CH3)2SiO 1 / 2}2{(CH2=CH)(CH3)SiO 2 / 2}6 {(CH3)2SiO 2 / 2} 5000 {(C6H5)2SiO 2 / 2} 77 Methylphenylvinylpolysiloxane (A6) Polysiloxane with the following structure, vinyl value of 0.018 mol / 100 g, phenyl group content of 10 mol %, and viscosity of 30 mass % toluene solution at 25°C of 10,000 mPa s {(CH2=CH)3SiO 1 / 2}2{(CH2=CH)(CH3)SiO 2 / 2} 80 {(CH3)2SiO 2 / 2} 5000 {(C6H5)2SiO 2 / 2} 550

[0106] (B) Component Methylhydrogenpolysiloxane (B1) Both ends of the molecular chain are capped with trimethylsiloxy groups, (CH3)HSiO 2 / 2 Units and (CH3)2SiO 2 / 2 The Si-H group content consisting of units is 1.42 mol / 100 g and the kinetic viscosity is 110 mm 2 / s Methyl hydrogen polysiloxane {(CH3)3SiO1 / 2}2{(CH3)HSiO 2 / 2} 90 {(CH3)2SiO 2 / 2} 10 Methylhydrogenpolysiloxane (B2) Both ends of the molecular chain are blocked with trimethylsiloxy groups, and all units except for the ends are (CH3)HSiO units. The Si-H group content is 1.59 mol / 100 g, and the kinetic viscosity is 35 mm. 2 / s Methyl hydrogen polysiloxane {(CH3)3SiO 1 / 2}2{(CH3)HSiO 2 / 2} 60 Methylphenylhydrogenpolysiloxane (B3) Both ends of the molecular chain are blocked with trimethylsiloxy groups, and all units other than the ends are (CH3)HSiO units and (C6H5)2SiO units. The Si-H group content is 1.19 mol / 100 g, the phenyl group content is 10 mol%, and the kinetic viscosity is 100 mm 2 / s Methylphenylhydrogenpolysiloxane {(CH3)3SiO 1 / 2}2{(CH3)HSiO 2 / 2} 73 {(C6H5)2SiO 2 / 2}8 Methylphenylhydrogenpolysiloxane (B4) Both ends of the molecular chain are blocked with trimethylsiloxy groups, and all units other than the ends are (CH3)HSiO units and (C6H5)2SiO units. The Si-H group content is 0.84 mol / 100 g, the phenyl group content is 22 mol%, and the kinetic viscosity is 120 mm 2 / s Methylphenylhydrogenpolysiloxane {(CH3)3SiO 1 / 2}2{(CH3)HSiO 2 / 2} 70 {(C6H5)2SiO 2 / 2} 20

[0107] (C) Component Acrylic acid (C1): HOOCH=CH2; molecular weight 72 2-Ethylhexyl acrylate (C2): CH2=CH-(CO)-O-CH2CH(C2H5)C4H9; molecular weight 213.5 2-Hydroxyethyl acrylate (C3): CH2=CH-(CO)-O-CH2CH2OH; molecular weight 116 4-Hydroxybutyl acrylate glycidyl ether (C4): A compound having an acrylic group at one end and a glycidyl ether group at the other end, represented by the following formula: Molecular weight: 200 [ka] Polysiloxanes with (meth)acrylic groups M 3 2D 3 170 D 3A 22 (C5); Weight average molecular weight 16,526 M 3 3D 3 110 D 3A 6T 3 1(C6); Weight average molecular weight 9,482 M 3 3D 3 180 D 3A 18 T 3 1(C7); Weight average molecular weight 16,726 M 3A 2D 3 37 D 3A 8(C8); Weight average molecular weight 4,472 M 3 2D 3 20 D 3A 5(C9); Weight average molecular weight 2,502 M 3 2D 3 20 D 3MA 5(C10); Weight average molecular weight 2,516 D 3A4(C11); Weight average molecular weight 689 T 3 0.6 T 3A 4.4 (OR 11 )7(C12); Weight average molecular weight 928 (M in the chemical formula 3 is R 11 3SiO 1 / 2 , M 3A is R 11 2A 1 SiO 1 / 2 , D 3 is R 11 2SiO 2 / 2 , D 3A is R 11 A 1 SiO 2 / 2 , D 3MA is R 11 (MA)SiO 2 / 2 , T 3 is R 11 SiO 3 / 2、 T 3A A 1 SiO 3 / 2 and R 11 is a methyl group, A 1 is CH2=CHCOO(CH2)3-, and MA is CH2=CCH3COO(CH2)3-.)

[0108] Other additives (comparison examples) M 3A 2D 3 1(C13); Weight average molecular weight 432 (M in the chemical formula 3A is R 11 2A 1 SiO 1 / 2 , D 3 is R 11 2SiO 2 / 2 and R 11 is a methyl group, A 1 is CH2=CHCOO(CH2)3-.)

[0109] Ingredient (F) 3-Methyl-1-butyn-3-ol (F1) 1-Ethynyl-1-cyclohexanol (F2) (G) Component Its viscosity at 25°C is 30 mPa·s, and its molecular chain ends are mainly capped with dimethylvinylsilyl groups, (CH3)2CH2=CHSiO 1 / 2 Unit 50 mol% and CH3SiO 3 / 2 Organopolysiloxane (G1) composed of 50 mol% units (vinyl group content = 0.6 mol / 100 g)

[0110] (H) Component Perhexa C (manufactured by NOF Corporation, 1,1-di(t-butylperoxy)cyclohexane (H1), 10-hour half-life temperature 90.7°C, exothermic onset temperature 134°C)

[0111] 1) Comparison of the effects of C ingredients 1-1) Evaluation of solvent-based composition [Example 1] 100 parts by mass of methylvinylpolysiloxane (A1) as component (A), 1.54 parts by mass of methylhydrogenpolysiloxane (B1) as component (B), and polysiloxane D having an acrylic group on the side chain as component (C). 3A 4. Add 1.3 parts by mass of (C11), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F) and stir until homogenous. Then, add a platinum and vinylsiloxane complex as component (D) so that the platinum atomic mass equivalent is 80 ppm relative to the total mass of components (A), (B), (C), and (D), and stir until homogenous. Then, add 1.3 parts by mass of (C11), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F). Stir until homogenous. Add 1.3 parts by mass of (C11), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F). 2 An organopolysiloxane composition having a Si—H ratio of 3 / s and H / Vi (the ratio of Si—H groups in component (B) to alkenyl groups in component (A) (the same applies hereinafter)) was prepared.

[0112] [Example 2] A viscosity of 10 mm was obtained by the same method as in Example 1, except that the component (C) was changed to 1.3 parts by mass of 4-hydroxybutyl acrylate glycidyl ether (C4). 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0113] [Example 3] Component (C) is a polysiloxane M having an acrylic group on the side chain. 3 2D 3 170 D 3A 22 (C5) was changed to 1.3 parts by mass, and the same method as in Example 1 was used to prepare a 10 mm viscosity 1000 ml syrup. 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0114] [Example 4] Component (C) is a polysiloxane M having an acrylic group on the side chain. 3 3D 3 180 D 3A 18 T 3 The same method as in Example 1 was used except that the amount of 1 (C7) was changed to 1.3 parts by mass. 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0115] [Example 5] The component (C) is a polysiloxane M having acrylic groups at the terminals and side chains. 3A 2D 3 37 D 3A The same procedure as in Example 1 was repeated except that the amount of 1.3 parts by mass of 8 (C8) was changed to 10 mm viscosity. 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0116] [Example 6] Component (C) is a polysiloxane M having an acrylic group on the side chain. 3 2D 3 20 D 3A The same procedure as in Example 1 was repeated except that the amount of 5(C9) was changed to 4 parts by mass. 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0117] [Example 7] Component (C) is a polysiloxane M having an acrylic group on the side chain. 3 2D 320 D 3A The same method as in Example 1 was used, except that the amount of 5(C9) was changed to 0.3 parts by mass. 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0118] [Example 8] (C) component is acrylic group-containing polysiloxane T 3 0.6 T 3A 4.4 (OR 7 The same procedure as in Example 1 was repeated except that the amount of 7(C12) was changed to 0.3 parts by mass. 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0119] [Example 9] A platinum / vinylsiloxane complex was added as component (D) to give a platinum atomic mass equivalent of 30 ppm relative to the total mass of components (A), (B), (C), (D), and (E), and the mixture was stirred until homogenous. 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0120] [Reference example 1] 100 parts by mass of methylvinylpolysiloxane (A1) as component (A), 1.54 parts by mass of methylhydrogenpolysiloxane (B1) as component (B), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F) were added and stirred until uniform, and then a platinum and vinylsiloxane complex was added as component (D) so that the platinum atomic mass equivalent was 160 ppm relative to the total mass of components (A), (B), (C), and (D), and the mixture was stirred until uniform. The mixture had a viscosity of 10 mm. 2 An organopolysiloxane composition having a Si—H ratio of 3 / s and H / Vi (the ratio of Si—H groups in component (B) to alkenyl groups in component (A) (the same applies hereinafter)) was prepared.

[0121] [Comparative Example 1] 100 parts by mass of methylvinylpolysiloxane (A1) as component (A), 1.54 parts by mass of methylhydrogenpolysiloxane (B1) as component (B), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F) were added and stirred until uniform, and then a platinum and vinylsiloxane complex was added as component (D) so that the platinum atomic mass equivalent was 80 ppm relative to the total mass of components (A), (B), (C), and (D), and the mixture was stirred until uniform, and the viscosity was reduced to 10 mm. 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0122] [Comparative Example 2] Component (C) is an organosiloxane M having acrylic groups at both ends. 3A 2D 3 Add 1.3 parts by mass of 1 (C13) and measure the temperature in the same manner as in Example 1. 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0123] [Comparative Example 3] A 100-part polysiloxane having a viscosity of 10 mm was prepared in the same manner as in Example 1, except that 100 parts by mass of methylvinylpolysiloxane (A2) was used as the component (A) and 1.42 parts by mass of methylhydrogenpolysiloxane (B1) was used as the component (B). 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0124] The organopolysiloxane compositions obtained in the above examples (Examples 1 to 9, Reference Example 1, Comparative Examples 1 to 3) were evaluated as follows. These results are shown in Tables 1 to 3 together with the above blended compositions.

[0125] [Peeling Force] The organopolysiloxane composition was applied to a polyester film using a No. 14 bar coater, and then heated in a hot air dryer at 120°C for 20 seconds to produce a film with a thickness of 0.3 g / m 2 Thus, a release film having a cured coating of the organopolysiloxane composition was obtained. The obtained release film was aged at 25°C for 24 hours, after which tesa-7475 tape (tesa UK Ltd.) was attached to the cured coating surface of the release film and cut to a size of 2.5 cm x 18 cm to prepare a test piece. This test piece was sandwiched between glass plates and heated to 70°C with a pressure of 20 g / cm 2 After 20 hours of compression under a load of 100 mm, one end of the test piece was peeled off, and the end of the adhesive-backed substrate of the tape was pulled in a direction at an angle of 180 degrees to the polyester film at a peeling speed of 0.3 m / min, and the force required to peel it off (i.e., the "peeling force") (N / 25 mm) was measured using a tensile testing machine (Shimadzu Corporation, Model AGS-50G).

[0126] [Residual adhesion rate] After measuring the peel force as described above, the tesa-7475 tape (tesa UK Ltd.) was attached to a suspension plate, and a 2 kg tape roller was rolled back and forth once to press it down. After leaving it for 30 minutes, one end of the tesa-7475 tape was peeled off, and the end was pulled in a direction at an angle of 180 degrees to the suspension plate and peeled off at a peeling speed of 0.3 m / min. The force required to peel was measured as adhesive strength A (N / 25 mm). As a blank, unused tesa-7475 tape was attached to a suspension plate, and a 2 kg tape roller was used to press it back and forth once as above, and after leaving it for 30 minutes, one end of the tesa-7475 tape was peeled off, and the end was pulled in a direction at an angle of 180 degrees to the suspension plate, and peeled off at a peeling speed of 0.3 m / min. The force required to peel was measured as adhesive strength B (N / 25 mm). The residual adhesion rate (%) was calculated as (A / B) x 100.

[0127] [Curability] The organopolysiloxane composition was applied to a polyester film using a No. 14 bar coater, and then heated in a hot air dryer at 120°C for 20 seconds to produce a film with a thickness of 0.3 g / m 2 A release film having a cured coating of the organopolysiloxane composition was obtained. The release film was removed from the dryer and the cured coating surface was immediately rubbed vigorously with the index finger ten times, and then red oil-based ink was applied to observe the degree of ink absorption and the condition of the cured coating. The results were expressed as "X" if the finger marks were dark, "△" if they were light, and "O" if they were barely visible.

[0128] [Silicone (organopolysiloxane) migration] In the same manner as in the peel strength measurement, a polyester film was placed on the surface of the cured film of the organopolysiloxane composition formed on the polyester film surface, and after 20 hours of pressure bonding at room temperature under a pressure of 0.98 MPa, the polyester film was removed from the cured film. Red oil-based ink was applied to the surface of the polyester film that had been in contact with the cured film, and silicone migration was evaluated based on the degree of repelling. The results were expressed as follows: no ink repellency: no or very little silicone migration (◯); partial ink repellency: slight silicone migration (△); ink repellency: significant silicone migration (×).

[0129] [Adhesion] The release film prepared in the same manner as in the peel force measurement was left to stand for 3 days at 25°C and 50% RH, after which the cured film of organopolysiloxane composition formed on the surface of the polyester film was rubbed strongly with the index finger 10 times, and red oil-based ink was applied to observe the degree of ink absorption and the condition of the cured film. The results were expressed as follows: no ink staining: good adhesion (◯); partial ink staining: partial dropout (Δ); and complete ink staining: complete dropout (×). The release film was left for one day at 60°C and 90% RH conditions to promote a decrease in adhesion under more severe conditions, and then the adhesion was evaluated in the same manner. If there was no staining by the ink, the adhesion was evaluated as being particularly good and marked with "◎".

[0130] [Table 1]

[0131] [Table 2]

[0132] [Table 3] *No siloxane unit represented by formula (1) above

[0133] 1-2) Evaluation of solvent-free composition (organic (C) component) [Example 10] 60 parts by mass of methylvinylpolysiloxane (A3) and 40 parts by mass of methylvinylpolysiloxane (A4) as component (A), 4.23 parts by mass of methylhydrogenpolysiloxane (B2) as component (B), 0.5 parts by mass of acrylic acid (C1) as component (C), and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F) were added and stirred until uniform, and then a platinum and vinylsiloxane complex was added as component (D) so that the platinum atomic mass equivalent was 80 ppm relative to the total mass of components (A), (B), (C), and (D), and the mixture was stirred until uniform. 2 A composition having a Si-H ratio of 1.8 / s and H / Vi (ratio of Si-H groups in the composition to alkenyl groups in the composition) was prepared.

[0134] [Example 11] A kinetic viscosity of 403 mm was obtained by the same method as in Example 11, except that the component (C) was changed to 0.5 parts by mass of 2-ethylhexyl acrylate (C2). 2 A composition having a viscosity of 1.8 / s and H / Vi was prepared.

[0135] [Example 12] A kinetic viscosity of 400 mm was obtained in the same manner as in Example 11, except that the component (C) was changed to 0.5 parts by mass of 2-hydroxyethyl acrylate (C3). 2 A composition having a viscosity of 1.8 / s and H / Vi was prepared.

[0136] [Example 13] The same method as in Example 1 was used except that the component (C) was changed to 0.5 parts by mass of 4-hydroxybutyl acrylate glycidyl ether (C4). 2A composition having a viscosity of 1.8 / s and H / Vi was prepared.

[0137] [Reference example 2] 60 parts by mass of methylvinylpolysiloxane (A3) and 40 parts by mass of methylvinylpolysiloxane (A4) as component (A), 3.98 parts by mass of methylhydrogenpolysiloxane (B2) as component (B), and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F) were added and stirred until uniform, and then a platinum and vinylsiloxane complex was added as component (D) so that the platinum atomic mass equivalent was 120 ppm relative to the total mass of components (A), (B), and (D), and the mixture was stirred until uniform. 2 A composition having a viscosity of 1.7 / s and H / Vi was prepared.

[0138] [Comparative Example 4] 60 parts by mass of methylvinylpolysiloxane (A3) and 40 parts by mass of methylvinylpolysiloxane (A4) as component (A), 4.23 parts by mass of methylhydrogenpolysiloxane (B2) as component (B), and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F) were added and stirred until uniform, and then a platinum and vinylsiloxane complex was added as component (D) so that the platinum atomic mass equivalent was 80 ppm relative to the total mass of components (A), (B), and (D), and the mixture was stirred until uniform. 2 A composition having a viscosity of 1.8 / s and H / Vi was prepared.

[0139] [Comparative Example 5] 100 parts by mass of methylvinylpolysiloxane (A4) as component (A), 1.92 parts by mass of methylhydrogenpolysiloxane (B2) as component (B), 0.5 parts by mass of acrylic acid (C1) as component (C), and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F) were added and stirred until uniform, and then a platinum and vinylsiloxane complex was added as component (D) so that the platinum atomic mass equivalent was 80 ppm relative to the total mass of components (A), (B), (C), and (D), and the mixture was stirred until uniform. 2A composition having a Si-H ratio of 1.8 / s and H / Vi (ratio of Si-H groups in the composition to alkenyl groups in the composition) was prepared.

[0140] The organopolysiloxane compositions obtained in the above examples (Examples 10 to 15, Reference Example 2, Comparative Examples 4 to 5) were evaluated as follows. These results are shown in Tables 4 to 6 together with the above blended compositions.

[0141] [Peeling Force] The organopolysiloxane composition was applied onto the metal roll of an RI tester (manufactured by IHI Machinery Systems Co., Ltd.), and the two rolls in contact with the rubber roll were rotated for 45 seconds to spread the composition evenly onto the rolls, after which the composition was transferred from the rubber roll to a polyethylene-laminated paper. The polyethylene-laminated paper to which the composition had been transferred was heated in a hot air dryer at 120°C for 20 seconds to form a sheet having a thickness of 0.9 to 1.1 g / m. 2 Thus, a release paper having a cured coating of the organopolysiloxane composition was obtained. In this state, after aging for 24 hours at 25°C, a solvent-based acrylic adhesive BPS-5127 (manufactured by Toyo Ink Co., Ltd.) was applied to the cured film surface of this release paper (the side transferred from the rubber roll) to a thickness of 130 μm, and then dried in a dryer at 100°C for 180 seconds. After drying, it was left at room temperature for 10 minutes or more, and then a wood-free paper was attached and cut into a size of 5.0 cm x 18 cm. A load was applied to the cut piece by rolling a 2 kg roller back and forth once, and after aging for 24 hours at room temperature, one end of the test piece was peeled off, and the end of the adhesive-attached substrate of the tape was pulled in a direction at an angle of 180 degrees to the polyethylene laminated paper at a peeling speed of 0.3 m / min, and the force required for peeling (i.e., "peeling force") (N / 50 mm) was measured using a tensile tester (Shimadzu Corporation AGS-50G type).

[0142] [Residual adhesion rate] In the same manner as in the case of the release force described above, the silicone composition was transferred to polyethylene laminated paper and cured in a dryer to obtain a release paper. After aging for 24 hours at 23°C, Nitto Denko NO31B tape was laminated onto the release paper. Similarly, Nitto Denko NO31B tape was laminated onto a Teflon (registered trademark) plate for comparison. Next, these laminated samples were heated at 70°C with 20 g / cm 2 After storage at 23°C for 30 minutes or more, the tape was peeled off, attached to a stainless steel plate, and pressed back and forth with a 2 kg roller once, after which the adhesive strength was measured using a tensile tester (Shimadzu Corporation AGS-50G type). The adhesive strength of the Teflon (registered trademark) plate lamination tape was taken as a blank value, and the ratio (%) of the measured value of the sample to the blank value was taken as the residual adhesive rate (%).

[0143] [Curability] Using the same method as for the release force described above, the silicone composition was transferred to polyethylene-laminated paper and heated in a hot air dryer at 120°C for 20 seconds to produce a film with a thickness of 0.9 to 1.1 g / m 2 This resulted in a release paper having a cured coating of the organopolysiloxane composition of Example 1. The release paper was removed from the dryer and the cured coating surface was immediately rubbed vigorously with the index finger ten times, and then red oil-based ink was applied and the degree of ink absorption and the condition of the cured coating were observed. The results were expressed as "X" if the finger marks were dark, "△" if they were light, and "O" if they were barely visible.

[0144] [Silicone (organopolysiloxane) migration] A polyester film was placed on the surface of the cured coating of the organopolysiloxane composition formed on the release paper obtained in the same manner as in the peel force measurement, and the polyester film was pressed at room temperature under a pressure of 0.98 MPa for 20 hours, after which the polyester film was separated from the cured coating. Red oil-based ink was applied to the surface of the polyester film that had been in contact with the cured coating, and silicone migration was evaluated based on the degree of repelling. The results were expressed as follows: no ink repellency: no or very little silicone migration (◯); partial ink repellency: slight silicone migration (△); ink repellency: significant silicone migration (×).

[0145] [Adhesion] The release paper prepared in the same manner as in the peel force measurement was left to stand for 3 days at 25°C and 50% RH, after which the cured film of organopolysiloxane composition formed on the surface of the polyester film was rubbed strongly with the index finger 10 times, and red oil-based ink was applied to observe the degree of ink absorption and the condition of the cured film. The results were expressed as follows: no ink staining: good adhesion (◯); partial ink staining: partial dropout (Δ); and complete ink staining: complete dropout (×). The release film was left for one day at 60°C and 90% RH conditions to promote a decrease in adhesion under more severe conditions, and then the adhesion was evaluated in the same manner. If there was no staining by the ink, the adhesion was evaluated as being particularly good and marked with "◎".

[0146] [Table 4] *No siloxane unit represented by formula (1) above

[0147] [Table 5] *No siloxane unit represented by the following formula (1)

[0148] 1-3) Evaluation of solvent-free composition (silicone-based (C) component) [Example 14] Component (C) is an organosiloxane M having a methacryl group on the side chain. 3 2D 3 20 D 3MAA viscosity of 401 mm was obtained by the same method as in Example 10, except that 1 part by mass of (C10) was added, and a platinum-vinylsiloxane complex was added as component (D) so that the platinum atomic mass was 20 ppm based on the total mass of components (A), (B), (C), and (D). 2 An organopolysiloxane composition having a viscosity of 1.8 / s and H / Vi was prepared.

[0149] [Example 15] Component (C) is a polysiloxane M having an acrylic group on the side chain. 3 3D 3 110 D 3A 6T 3 The same procedure as in Example 14 was repeated except that the amount of 1 (C6) was changed to 1 part by mass. 2 An organopolysiloxane composition having a viscosity of 1.8 / s and H / Vi was prepared.

[0150] [Reference example 3] 60 parts by mass of methylvinylpolysiloxane (A3) and 40 parts by mass of methylvinylpolysiloxane (A4) as component (A), 3.98 parts by mass of methylhydrogenpolysiloxane (B2) as component (B), and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F) were added and stirred until uniform, and then a platinum and vinylsiloxane complex was added as component (D) so that the platinum atomic mass equivalent was 120 ppm relative to the total mass of components (A), (B), and (D), and the mixture was stirred until uniform. 2 A composition having a viscosity of 1.7 / s and H / Vi was prepared.

[0151] [Comparative Example 6] 60 parts by mass of methylvinylpolysiloxane (A3) and 40 parts by mass of methylvinylpolysiloxane (A4) as component (A), 4.23 parts by mass of methylhydrogenpolysiloxane (B2) as component (B), and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F) were added and stirred until uniform, and then a platinum and vinylsiloxane complex was added as component (D) so that the platinum atomic mass equivalent was 20 ppm relative to the total mass of components (A), (B), and (D), and the mixture was stirred until uniform. 2 A composition having a viscosity of 1.8 / s and H / Vi was prepared.

[0152] [Comparative Example 7] The component (A) was 100 parts by mass of methylvinylpolysiloxane (A4), the component (B) was 1.92 parts by mass of methylhydrogenpolysiloxane (B2), and the component (C) was an organosiloxane M having a methacryl group on the side chain. 3 2D 3 20 D 3MA 5. Add 1 part by mass of (C10) and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F) and stir until homogenous. Then, add a platinum and vinylsiloxane complex as component (D) so that the platinum atom mass equivalent is 20 ppm relative to the total mass of components (A), (B), (C), and (D). Stir until homogenous. Then, adjust the kinetic viscosity to 420 mm. 2 A composition having a Si-H ratio of 1.8 / s and H / Vi (ratio of Si-H groups in the composition to alkenyl groups in the composition) was prepared.

[0153] The organopolysiloxane compositions obtained in the above examples (Examples 14 to 15, Reference Example 3, Comparative Examples 6 to 7) were evaluated as follows. These results are shown in Table 6 together with the above blended compositions.

[0154] [Peeling Force] The composition obtained above was applied onto the metal roll of an RI tester (manufactured by IHI Machinery Systems Co., Ltd.), and the two rolls consisting of a metal roll and a rubber roll were rotated for 45 seconds to uniformly spread the composition, and then the composition was transferred from the rubber roll to glassine paper ASP (manufactured by Ahlstrom-Munksjo). The glassine paper to which the composition was transferred was heated in a hot air dryer at 120°C for 20 seconds to a thickness of 0.9 to 1.1 g / m 2 A release paper having a cured coating of the above composition was obtained. After aging for 24 hours at 25°C in this state, tesa-7475 tape (tesa UK Ltd.) was attached to the surface of the cured coating of this release paper (the side transferred from the rubber roll) and cut into a size of 2.5 cm x 18 cm. This was sandwiched between glass plates and heated to 70°C with 20 g / cm 2 After aging for 24 hours under the load, one end of the test piece was peeled off and the adhesive-backed end of the tape was pulled at an angle of 180 degrees to the glassine paper at a peeling rate of 0.3 m / min, and the force required to peel it off (i.e., the "peeling force") (N / 50 mm) was measured using a tensile testing machine (AGS-50G, manufactured by Shimadzu Corporation).

[0155] [Residual adhesion rate] After measuring the peeling force, the tesa-7475 tape (tesa UK Ltd.) was attached to a polyester film, and a 2 kg roller was moved back and forth once to apply a load. After leaving it for 30 minutes, one end of the tesa-7475 tape was peeled off, and the end was pulled in a direction at an angle of 180 degrees to the polyester film, and peeled off at a peeling speed of 0.3 m / min. The force required to peel off at this time: peeling force A (N / 25 mm) was measured. As a blank, unused tesa-7475 tape was applied to a polyester film, and a 2 kg roller was rolled back and forth once to apply a load in the same manner as above. After leaving it for 30 minutes, one end of the tesa-7475 tape was peeled off, and the end was pulled in a direction at an angle of 180 degrees to the polyester film at a peeling speed of 0.3 m / min. The force required to peel at this time: peel force B (N / 25 mm) was measured. The residual adhesion rate (%) was calculated by (A / B) x 100.

[0156] [Curability] The release paper prepared in the same manner as in the peel force measurement was removed from the dryer and the cured film surface was immediately rubbed vigorously with the index finger 10 times, and red magic marker was applied to observe the ink thickness and the condition of the cured film. The results were expressed as "X" if the finger marks were dark, "△" if they were light, and "O" if they were barely visible.

[0157] [Silicone (organopolysiloxane) migration] A 36 μm thick polyethylene terephthalate film was placed on the surface of the release paper prepared in the same manner as in the case of peeling force measurement, and after pressing for 20 hours under a pressure of 0.98 MPa at room temperature, the polyethylene terephthalate film was removed from the cured film. An oil-based ink (trade name: Magic Ink, manufactured by Teranishi Chemical Industry Co., Ltd.) was applied to the surface of the polyethylene terephthalate film that had been in contact with the cured film, and the silicone migration was evaluated according to the following criteria based on the degree of repelling. The results were expressed as follows: no ink repellency: no or very little silicone migration (◯); ink repellency: considerable silicone migration (×).

[0158] [Adhesion] The release paper prepared in the same manner as in the peel force measurement was left to stand for 3 days under conditions of 25°C and 50% RH, after which the cured film of organopolysiloxane composition formed on the surface of the polyethylene laminated paper was rubbed strongly with the index finger 10 times, and red oil-based ink was applied to observe the degree of ink absorption and the condition of the cured film. The results were expressed as follows: no ink staining: good adhesion (◯); partial ink staining: partial dropout (Δ); entire surface ink staining: complete dropout (×).

[0159] [Table 6] *No siloxane unit represented by the following formula (1)

[0160] 2) Effects of phenyl-containing ingredients [Example 16] The component (A) was 100 parts by mass of methylvinylpolysiloxane (A1), the component (B) was 1.04 parts by mass of methylhydrogenpolysiloxane (B1) and 0.60 parts by mass of methylphenylhydrogenpolysiloxane (B3), and the component (C) was a polysiloxane M having an acrylic group on the side chain. 3 2D 3 20 D 3A Add 1.3 parts by mass of (C9), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F), and 0.60 parts by mass of organopolysiloxane (G1) as component (G) and stir until uniform. Then, add a platinum and vinylsiloxane complex as component (D) so that the platinum atomic mass equivalent is 80 ppm relative to the total mass of components (A), (B), (C), and (D), and stir until uniform. Then, add a mixture having a viscosity of 10 mm. 2 / An organopolysiloxane composition having a viscosity of 1000 psig and H / Vi=2 was prepared.

[0161] [Example 17] The component (A) was 60 parts by mass of methylvinylpolysiloxane (A1), 40 parts by mass of methylphenylvinylpolysiloxane (A5), and the component (B) was 1.46 parts by mass of methylhydrogenpolysiloxane (B1), and the component (C) was polysiloxane M having an acrylic group on the side chain. 3 2D 3 20 D 3A 5. Add 1.3 parts by mass of (C9), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F) and stir until homogenous. Then, add a platinum and vinylsiloxane complex as component (D) so that the platinum atomic mass equivalent is 80 ppm relative to the total mass of components (A), (B), (C), and (D), and stir until homogenous. Then, add 1.3 parts by mass of (C9), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F). Stir until homogenous. Add 1.3 parts by mass of (C9), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F). 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=4 was prepared.

[0162] [Example 18] The component (A) was 60 parts by mass of methylvinylpolysiloxane (A1) and 40 parts by mass of methylphenylvinylpolysiloxane (A5), the component (B) was 0.70 parts by mass of methylhydrogenpolysiloxane (B1) and 0.47 parts by mass of methylphenylhydrogenpolysiloxane (B3), and the component (C) was polysiloxane M having an acrylic group on the side chain. 3 2D 3 20 D 3A Add 1.3 parts by mass of (C9), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F), and 0.60 parts by mass of organopolysiloxane (G1) as component (G) and stir until uniform. Then, add a platinum and vinylsiloxane complex as component (D) so that the platinum atomic mass equivalent is 80 ppm relative to the total mass of components (A), (B), (C), and (D), and stir until uniform. Then, add a mixture having a viscosity of 10 mm. 2 An organopolysiloxane composition having a viscosity of 1.7 / s and H / Vi was prepared.

[0163] [Example 19] 100 parts by mass of methylphenylvinylpolysiloxane (A6) as component (A), 4.29 parts by mass of methylphenylhydrogenpolysiloxane (B4) as component (B), and polysiloxane M having an acrylic group on the side chain as component (C). 3 2D 3 20 D 3A Add 1.3 parts by mass of (C9), 1,200 parts by mass of toluene and 1,200 parts by mass of hexane as component (E), 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F), and 0.60 parts by mass of organopolysiloxane (G1) as component (G) and stir until uniform. Then, add a platinum and vinylsiloxane complex as component (D) so that the platinum atomic mass equivalent is 80 ppm relative to the total mass of components (A), (B), (C), and (D), and stir until uniform. Then, add a mixture having a viscosity of 10 mm. 2 An organopolysiloxane composition having a viscosity of 1.7 / s and H / Vi was prepared.

[0164] The organopolysiloxane compositions obtained in the above examples (Examples 16 to 19) were evaluated using the same methods and conditions as those used in the above 1-1) Evaluation of Solvent-Based Compositions. These results are shown in Table 7 together with the above blended compositions.

[0165] [Table 7] *No siloxane unit represented by the following formula (1)

[0166] 3) Effects of Component (H) 3-1) Evaluation of solvent-based composition [Example 20] The component (A) was 100 parts by mass of methylvinylpolysiloxane (A1), the component (B) was 1.54 parts by mass of methylhydrogenpolysiloxane (B1), and the component (C) was a polysiloxane M having an acrylic group on the side chain. 3 2D 3 20 D 3A Add 1 part by mass of (C9), 1,561 parts by mass of toluene as component (E), 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F), and 1 part by mass of Perhexa C (H1) as component (H) and stir until homogenous. Then, add a platinum and vinylsiloxane complex as component (D) so that the platinum atom mass equivalent is 80 ppm relative to the total mass of components (A), (B), (C), and (D), and stir until homogenous. Then, adjust the kinetic viscosity to 10 mm. 2 A composition having a Si—H ratio (ratio of Si—H groups in the composition to alkenyl groups in the composition) of 3 was prepared.

[0167] [Example 21] The component (A) was 100 parts by mass of methylvinylpolysiloxane (A1), the component (B) was 1.54 parts by mass of methylhydrogenpolysiloxane (B1), and the component (C) was a polysiloxane M having an acrylic group on the side chain. 3 2D 3 20 D 3A5. Add 1 part by mass of (C9), 1,561 parts by mass of toluene as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F) and stir until homogenous. Then, add a platinum and vinylsiloxane complex as component (D) so that the platinum atom mass equivalent is 80 ppm relative to the total mass of components (A), (B), (C), and (D), and stir until homogenous. Then, adjust the kinetic viscosity to 10 mm. 2 A composition having a Si—H ratio (ratio of Si—H groups in the composition to alkenyl groups in the composition) of 3 was prepared.

[0168] [Reference example 4] 100 parts by mass of methylvinylpolysiloxane (A1) as component (A), 1.54 parts by mass of methylhydrogenpolysiloxane (B1) as component (B), 1,561 parts by mass of toluene as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F) were added and stirred until uniform, after which a platinum and vinylsiloxane complex as component (D) was added in an amount equivalent to 160 ppm of platinum atomic mass relative to the total mass of components (A), (B), (C), and (D), and the mixture was stirred until uniform, and the viscosity reached 10 mm. 2 An organopolysiloxane composition having a Si—H ratio of 3 / s and H / Vi (the ratio of Si—H groups in component (B) to alkenyl groups in component (A) (the same applies hereinafter)) was prepared.

[0169] [Comparative Example 8] 100 parts by mass of methylvinylpolysiloxane (A1) as component (A), 1.54 parts by mass of methylhydrogenpolysiloxane (B1) as component (B), 1,561 parts by mass of toluene as component (E), and 3 parts by mass of 3-methyl-1-butyn-3-ol (F1) as component (F) were added and stirred until uniform, after which a platinum and vinylsiloxane complex as component (D) was added in an amount equivalent to 80 ppm by platinum atomic mass relative to the total mass of components (A), (B), (C), and (D), and the mixture was stirred until uniform, and the viscosity was reduced to 10 mm. 2 An organopolysiloxane composition having a viscosity of 1000 s / s and H / Vi=3 was prepared.

[0170] The organopolysiloxane compositions obtained in the above examples (Examples 20 to 21, Reference Example 4, Comparative Example 8) were evaluated as follows. These results are shown in Table 8 together with the above blended compositions.

[0171] [Peeling Force] The organopolysiloxane composition was applied to polyethylene laminated paper using a No. 14 bar coater, and then heated in a hot air dryer at 100°C for 30 seconds to produce a coating with a thickness of 0.9 to 1.1 g / m. 2 Thus, a release paper having a cured coating of the organopolysiloxane composition was obtained. In this state, after aging for 24 hours at 25°C, a solvent-based acrylic adhesive BPS-5127 (manufactured by Toyo Ink Co., Ltd.) was applied to the cured film surface side of the release paper, and then dried in a dryer at 100°C for 180 seconds. After drying, the paper was left at room temperature for 10 minutes or more, and then a wood-free paper was attached and cut into a size of 5.0 cm x 18 cm. A load was applied to the cut piece by rolling a 2 kg roller back and forth once, and after aging for 24 hours at room temperature, one end of the test piece was peeled off, and the adhesive-attached substrate end of the tape was pulled at an angle of 180 degrees to the polyethylene laminated paper at a peeling speed of 0.3 m / min, and the force required for peeling (i.e., "peeling force") (N / 50 mm) was measured using a tensile tester (Shimadzu Corporation AGS-50G type).

[0172] [Residual adhesion rate] The silicone composition was applied to polyethylene laminated paper and cured in the same manner as in the case of the above-mentioned release force to obtain a release paper. After aging at 23°C for 24 hours, tesa-7475 tape (tesa UK Ltd.) was laminated onto the release paper and cut into a size of 2.5 cm x 18 cm. This was sandwiched between glass plates and heated to 70°C with 20 g / cm 2 After aging for 24 hours under a load of 1000 g, the tape was peeled off, attached to a stainless steel plate, pressed with a 2 kg roller once, and left for 30 minutes. One end of the tesa-7475 tape was peeled off, and the end was pulled in a direction at an angle of 180 degrees to the suspension plate and peeled off at a peeling speed of 0.3 m / min. The force required to peel off was measured as adhesive strength A (N / 25 mm). It was measured using a tensile tester (Shimadzu Corporation AGS-50G type). As a blank, unused tesa-7475 tape was attached to a suspension plate, and a 2 kg tape roller was used to press it back and forth once as above, and after leaving it for 30 minutes, one end of the tesa-7475 tape was peeled off, and the end was pulled in a direction at an angle of 180 degrees to the suspension plate, and peeled off at a peeling speed of 0.3 m / min. The force required to peel was measured as adhesive strength B (N / 25 mm). The residual adhesion rate (%) was calculated as (A / B) x 100.

[0173] [Curability] Using the same method as for the release force described above, the silicone composition was applied to polyethylene-laminated paper and heated in a hot air dryer at 100°C for 30 seconds to give a film thickness of 0.9 to 1.1 g / m 2 This resulted in a release paper having a cured coating of the organopolysiloxane composition of Example 1. The release paper was removed from the dryer and the cured coating surface was immediately rubbed vigorously with the index finger ten times, and then red oil-based ink was applied and the degree of ink absorption and the condition of the cured coating were observed. The results were expressed as "X" if the finger marks were dark, "△" if they were light, and "O" if they were barely visible.

[0174] [Silicone (organopolysiloxane) migration] A polyester film was placed on the surface of the cured coating of the organopolysiloxane composition formed on the release paper obtained in the same manner as in the peel force measurement, and the polyester film was pressed at room temperature under a pressure of 0.98 MPa for 20 hours, after which the polyester film was separated from the cured coating. Red oil-based ink was applied to the surface of the polyester film that had been in contact with the cured coating, and silicone migration was evaluated based on the degree of repelling. The results were expressed as follows: no ink repellency: no or very little silicone migration (◯); partial ink repellency: slight silicone migration (△); ink repellency: significant silicone migration (×).

[0175] [Table 8]

[0176] 3-2) Evaluation of solvent-free composition [Example 22] As the component (A), 60 parts by mass of methylvinylpolysiloxane (A3), 40 parts by mass of methylvinylpolysiloxane (A4), as the component (B), 4.23 parts by mass of methylhydrogenpolysiloxane (B2), as the component (C), polysiloxane M having an acrylic group on the side chain, 3 2D 3 20 D 3A Add 1 part by mass of (C9), 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F), and 1 part by mass of Perhexa C (H1) as component (H) and stir until homogenous. Then, add a platinum and vinylsiloxane complex as component (D) so that the platinum atomic mass equivalent is 60 ppm relative to the total mass of components (A), (B), (C), and (D). Stir until homogenous. Then, adjust the kinetic viscosity to 406 mm. 2 A composition having a Si-H ratio of 1.8 / s and H / Vi (ratio of Si-H groups in the composition to alkenyl groups in the composition) was prepared.

[0177] [Example 23] As the component (A), 60 parts by mass of methylvinylpolysiloxane (A3), 40 parts by mass of methylvinylpolysiloxane (A4), as the component (B), 4.23 parts by mass of methylhydrogenpolysiloxane (B2), as the component (C), polysiloxane M having an acrylic group on the side chain, 3 2D 3 20 D 3A 5. Add 1 part by mass of (C9) and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F) and stir until homogenous. Then, add a platinum and vinylsiloxane complex as component (D) so that the platinum atom mass equivalent is 60 ppm relative to the total mass of components (A), (B), (C), and (D). Stir until homogenous. Then, adjust the kinetic viscosity to 405 mm. 2 A composition having a Si-H ratio of 1.8 / s and H / Vi (ratio of Si-H groups in the composition to alkenyl groups in the composition) was prepared.

[0178] [Reference example 5] 60 parts by mass of methylvinylpolysiloxane (A3) and 40 parts by mass of methylvinylpolysiloxane (A4) as component (A), 4.23 parts by mass of methylhydrogenpolysiloxane (B2) as component (B), and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F) were added and stirred until uniform, and then a platinum and vinylsiloxane complex was added as component (D) so that the platinum atomic mass equivalent was 120 ppm relative to the total mass of components (A), (B), (C), and (D), and the mixture was stirred until uniform. 2 A composition having a Si-H ratio of 1.8 / s and H / Vi (ratio of Si-H groups in the composition to alkenyl groups in the composition) was prepared.

[0179] [Comparative Example 9] 60 parts by mass of methylvinylpolysiloxane (A3) and 40 parts by mass of methylvinylpolysiloxane (A4) as component (A), 4.23 parts by mass of methylhydrogenpolysiloxane (B2) as component (B), and 0.3 parts by mass of 1-ethynyl-1-cyclohexanol (F2) as component (F) were added and stirred until uniform, and then a platinum and vinylsiloxane complex was added as component (D) so that the platinum atomic mass equivalent was 60 ppm relative to the total mass of components (A), (B), (C), and (D), and the mixture was stirred until uniform. 2 A composition having a Si-H ratio of 1.8 / s and H / Vi (ratio of Si-H groups in the composition to alkenyl groups in the composition) was prepared.

[0180] The organopolysiloxane compositions obtained in the above examples (Examples 22-23, Reference Example 5, Comparative Example 9) were evaluated using the same methods and conditions as those used in 1-3) Evaluation of Solventless Composition (Silicone-Based (C) Component) above. These results are shown in Table 9 together with the above blended compositions.

[0181] [Table 9]

[0182] Reference Example 1 is a case where component (C) is not used and the platinum concentration of the catalyst component (D) is high at 160 ppm. In this case, the cure proceeds sufficiently, so the hardening, silicone migration and adhesion are good, the peel force is light, the residual adhesion rate is high and the inherent properties of the release paper are observed.

[0183] In Comparative Example 1, the platinum concentration of the catalyst in component (D) of Reference Example 1 was reduced by half to 80 ppm, and in this case, even after heat treatment at 120°C for 30 seconds, curing was insufficient, so the peeling force was heavy, the residual adhesion rate was low, and the inherent properties of silicone were not obtained. When the coated surface was rubbed, finger marks were clearly left and the amount of migration was large, so the curing property, silicone migration property, and adhesion property were rated as ×, △, and ×.

[0184] Examples 1 to 9 have compositions in which a trace amount of a compound having an acrylic group, as component (C), has been added to the composition of Comparative Example 1. By adding component (C), despite the platinum concentration of the catalyst in component (D) being 80 ppm, curing proceeded sufficiently and there was no silicone migration. The peel strength and residual adhesion rate were not significantly different from those of Reference Example 1, and it can be confirmed that the curing reaction proceeded with a low platinum concentration due to the addition of component (C).

[0185] Comparing Comparative Example 2 with the Examples, when component (C) is a siloxane compound, the effect is more effective when the side chain is present than when the acrylic group is located at the end of the molecule, and Example 8 shows that the effect is similar not only when a (meth)acrylic group is present on a difunctional siloxane unit, but also when it is present on a trifunctional siloxane.

[0186] A comparison between Comparative Example 3 and Example 1 shows that the effect of component (C) is enhanced when the molecular terminal of component (A) has a trivinyl structure.

[0187] In Examples 10 to 13, the effect of a compound other than silicone as component (C) was evaluated using a composition that did not contain the solvent component (E).Comparison with Comparative Example 4 shows that component (C) acts to reduce the peel force and increase the residual adhesion rate, which is close to the characteristics of Reference Example 2, which contains a large amount of component (D), and therefore it can be confirmed that it promotes the curing reaction.

[0188] Comparison with the comparative examples shows that even in compositions that do not contain the solvent component (E), the effect of component (C) is enhanced when the molecular terminal of component (A) has a trivinyl structure.

[0189] Examples 14-15 are the results of evaluating the effect of a silicone compound as component (C) using a composition that does not contain the solvent component (E), but by reducing component (D) to 20 ppm and changing the substrate to glassine paper, the curing, migration, and adhesion were evaluated under stricter conditions. The same tendency as above was confirmed here, and the effect of component (C) in improving curing and adhesion and reducing migration was confirmed.

[0190] Examples 16 to 19 are the results of evaluating the effect of component (C) when a compound having a phenyl group is used as components (A) and (B). Compared with Examples 6 and 7, it can be seen that the effect of improving adhesion is greater.

[0191] In Examples 20 to 23, the effect of component (C) was evaluated by adding component (H), and it was confirmed that component (H) worked to reduce the peel force and increase the residual adhesion rate. This effect was the same for compositions that contained solvent and those that did not, but the solvent-based composition had a remarkable effect even under conditions where the curing temperature was as low as 100°C and it was difficult to obtain curing properties.

[0192] From the above results, it can be seen that the cure-accelerating effect of component (C) can be further enhanced by combining the molecular terminal trivinyl structure of component (A), the inclusion of phenyl groups in components (A) and / or (B), and the addition of peroxide (H).

Claims

1. A curable organopolysiloxane composition comprising the following components (A) to (D): (A) An organopolysiloxane having two or more silicon-bonded alkenyl groups per molecule, with an alkenyl group content of 0.001 to 0.7 mol / 100 g, and not having three or more (meth)acrylic groups per molecule, wherein at least 50 mass % of component (A) is a siloxane unit having at least one molecular terminal represented by the following formula (1): (CH 2 =CH-) 3 SiO 1/2 (1) It is blocked off by The viscosity at 25°C measured using a rotational viscometer is 7 mPa·s or more, and the viscosity of a 30% by weight toluene solution (the viscosity of a solution in which 30% by weight of organopolysiloxane is dissolved in toluene) is 70,000 mPa·s or less. Organopolysiloxane: 100 parts by mass, (B) an organohydrogenpolysiloxane having an average of two or more silicon-bonded hydrogen atoms (Si—H groups) per molecule and no more than three (meth)acrylic groups per molecule: an amount in which the number of moles of Si—H groups in component (B) corresponds to 1 to 10 times the number of moles of alkenyl groups in component (A); (C) one or more selected from the following (C-1) and (C-2): 0.01 to 5.0 parts by mass per 100 parts by mass of the (A) component, (C-1) A compound having one or more (meth)acrylic groups in one molecule, which is not an organopolysiloxane, and has a molecular weight of 72 to 1,000. (C-2) An organopolysiloxane having three or more (meth)acrylic groups in one molecule, the organopolysiloxane having a weight average molecular weight of 500 or more and 20,000 or less in terms of polystyrene, as determined by gel permeation chromatography (GPC) analysis (solvent: toluene). (D) Platinum group metal catalyst: an amount such that the platinum concentration in the total mass of the components (A), (B), (C), and (D) is 1 to 100 ppm by mass

2. 2. The curable organopolysiloxane composition according to claim 1, further comprising (E) 0 to 100,000 parts by mass of a dilution solvent per 100 parts by mass of component (A).

3. 2. The curable organopolysiloxane composition according to claim 1, further comprising 0.01 to 5.00 parts by mass of a reaction inhibitor (F) per 100 parts by mass of component (A).

4. 2. The curable organopolysiloxane composition according to claim 1, wherein in component (B), 5 to 30 mol % of the total number of substituents on silicon atoms are phenyl groups.

5. 2. The curable organopolysiloxane composition according to claim 1, wherein in component (A), 1 to 20 mol % of the total number of substituents on silicon atoms are phenyl groups.

6. Further, (G) at least two alkenyl groups, R 10 (3-g1) R 9 g1 SiO 1 / 2 Siloxane unit (M R9R10 Units), R 10 SiO 3 / 2 Siloxane unit (T R10 Units) (wherein R 9 are each independently an alkenyl group; R 10 are each independently an unsubstituted or halogen- or cyano-substituted monovalent hydrocarbon group that does not contain an aliphatic unsaturated bond, and g1 is an integer of 1 to 3. R9R10 Unit / T R10 The molar ratio of the units is 2 / 8 to 8 / 2, and the viscosity at 25°C is in the range of 1 to 1,000 mPa·s. R9R10 Unit or M R9R10 2. The curable organopolysiloxane composition according to claim 1, which contains 0.1 to 20.0 parts by mass of an organopolysiloxane in which the units and a portion of which are silanol groups or alkoxy groups are contained per 100 parts by mass of component (A).

7. 2. The curable organopolysiloxane composition according to claim 1, wherein component (C) is an organopolysiloxane having at least one difunctional and / or trifunctional siloxane unit having a (meth)acrylic group in one molecule.

8. 2. The curable organopolysiloxane composition according to claim 1, further comprising (H) 0.01 to 5.0 parts by mass of an organic peroxide per 100 parts by mass of component (A).

9. 9. The curable organopolysiloxane composition according to claim 8, wherein component (H) is a polyfunctional organic peroxide having two or more peroxide bonds in the molecule.

10. 2. The curable organopolysiloxane composition according to claim 1, further comprising (D) a platinum group metal catalyst in an amount such that the platinum concentration in the combined mass of components (A) to (D) is 1 to 40 ppm by mass.

11. The curable organopolysiloxane composition according to any one of claims 1 to 10, which is used for a release paper or release film.

12. A method for producing a release paper or a release film, which uses the organopolysiloxane composition for release paper or a release film according to claim 11.

Citation Information

Patent Citations

  • Organopolysiloxane composition for forming peelable cured film

    JP1997143371A

  • Silicone resin composition, and cured product thereof

    JP2011148981A

  • Silicone composition for release paper or release film, and release paper and release film

    WO2017010340A1

  • Organopolysiloxane composition for use in release paper or release film

    WO2020145151A1

  • Silicone composition for producing release paper or release film, and release paper and release film

    WO2021166653A1