Method for producing catalyst for methanol production, catalyst for methanol production and method for producing methanol

A catalyst production method using copper, zinc, and optional aluminum in an alcohol solvent enhances methanol production efficiency by reducing crystallite diameters and agglomeration, addressing the need for improved activity and efficiency in existing catalysts.

JP2024148550APending Publication Date: 2024-10-18NIPPON STEEL CORPORATION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023061760
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing methanol production catalysts based on copper and zinc require improvements in efficiency and activity to meet demands for higher energy and economic efficiency.

Method used

A catalyst production method using a copper compound, zinc nitrate, and oxalic acid in an alcohol solvent to form a precipitate, followed by drying and calcination, resulting in a composite oxide with controlled crystallite diameters and specific component ratios, including the option of adding aluminum, to enhance activity and efficiency.

Benefits of technology

The method produces a catalyst with increased active sites and reduced agglomeration, leading to higher methanol production efficiency and activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148550000001
    Figure 2024148550000001
  • Figure 2024148550000002
    Figure 2024148550000002
  • Figure 2024148550000003
    Figure 2024148550000003
Patent Text Reader

Abstract

To provide a method for producing a catalyst for methanol production that enables the production of methanol with increased activity and enhanced efficiency, a catalyst for methanol production and a method for producing methanol.SOLUTION: A method for producing a catalyst for methanol production includes mixing a copper compound, zinc nitrate, and oxalic acid in an alcohol solvent to form a precipitate, which is subjected to drying and firing, resulting in the production of a catalyst composed of a complex oxide containing copper and zinc. A catalyst for methanol production is composed of a complex oxide containing copper and zinc and has a CuO crystallite size of 14 nm or smaller, before catalytic reduction, as determined from the half-width of the X-ray diffraction pattern. Also provided is a method for producing methanol using the catalyst.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a catalyst for methanol production, a catalyst for methanol production, and a method for producing methanol. [Background technology]

[0002] Methanol is used as a raw material for a wide range of chemical products, including the starting material for olefins (ethylene, propylene, etc.), which are used to make general-purpose resins (polyethylene, polypropylene, etc.), as well as a raw material for phenolic resins, synthetic fibers, paints, pharmaceuticals and agrochemicals, fuel additives, and a raw material for basic chemicals (acetic acid, formaldehyde, etc.).

[0003] For example, Patent Document 1 discloses a "copper oxide and / or copper-containing catalyst for methanol synthesis, characterized in that gallium is blended therein." Furthermore, Patent Document 2 discloses "a catalyst for synthesizing formate esters and methanol, which synthesizes formate esters and methanol via formate esters from a raw material gas containing one or both of carbon monoxide and carbon dioxide and hydrogen in the presence of an alcohol as a solvent, the catalyst for synthesizing formate esters and methanol, characterized in that it contains Cu and Zn simultaneously as main components and contains one or more components selected from Groups 4, 6, 7, and 13 of the periodic table and lanthanoids as promoters." [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 06-312138 [Patent Document 2] JP 2005-246261 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0005] Here, as disclosed in Patent Documents 1 and 2, methanol is produced efficiently in the production of methanol using a catalyst made of a composite oxide containing copper and zinc. However, the production of methanol is extremely important in the chemical industry, and there is a constant demand for higher efficiency in terms of energy saving, economic efficiency, etc., and there is currently a demand for even higher catalyst activity.

[0006] Therefore, an object of the present invention is to provide a method for producing a catalyst for methanol production, which is highly active and capable of producing methanol more efficiently, a catalyst for methanol production, and a method for producing methanol. [Means for solving the problem]

[0007] Means for solving the above problems include the following aspects. <1> A method for producing a catalyst for methanol production, comprising mixing a copper compound, zinc nitrate, and oxalic acid in an alcohol solvent to form a precipitate, and then drying and calcining the precipitate to produce a catalyst made of a composite oxide containing copper and zinc. <2> further mixing an aluminum compound into the alcohol solvent to produce a catalyst made of a composite oxide containing copper, zinc and aluminum; <1> 2. A method for producing the catalyst for methanol production according to claim 1 . <3> The surface tension of the alcohol solvent is 48 mN m -1 is less than or equal to <1> 2. A method for producing the catalyst for methanol production according to claim 1 . <4> A catalyst for methanol production, which is composed of a composite oxide containing copper and zinc, and has a CuO crystallite size of 14 nm or less before catalytic reduction, as calculated from the half-width of the X-ray diffraction pattern. <5> The component ratios in the composite oxide are, in terms of metal, copper: 30% by mass or more and 70% by mass or less, and zinc: 30% by mass or more and 70% by mass or less. <4> 2. The catalyst for methanol production according to claim 1 . <6> The composite oxide further contains aluminum. <4> or <5> 2. The catalyst for methanol production according to claim 1 . <7> The component ratios in the composite oxide are, in terms of metal, copper: 30% by mass or more and 60% by mass or less, zinc: 30% by mass or more and 60% by mass or less, and aluminum: 1% by mass or more and 10% by mass or less. <6> 2. The catalyst for methanol production according to claim 1 . <8> The crystallite size of Cu after catalytic reduction is 14 nm or less, as calculated from the half-width of the X-ray diffraction pattern. <4> ~ <7> 2. The catalyst for methanol production according to claim 1 . <9> <1> ~ <3> A catalyst for methanol production produced by the method for producing a catalyst for methanol production according to any one of claims 1 to 5, or <4> ~ <8> 1. A method for producing methanol, comprising introducing a raw material gas containing hydrogen and carbon dioxide, or a raw material gas containing hydrogen, carbon monoxide and carbon dioxide, into a reaction field in which the catalyst for methanol production according to any one of claims 1 to 9 is present, to produce methanol. Effect of the Invention

[0008] According to the present invention, it is possible to provide a method for producing a catalyst for methanol production, which is highly active and capable of producing methanol more efficiently, a catalyst for methanol production, and a method for producing methanol. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will now be described. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In numerical ranges described in stages, the upper limit or lower limit value described in a certain numerical range may be replaced with the upper limit or lower limit value of another numerical range described in stages. In a numerical range, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples. When a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. The term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. A "combination of preferred aspects" is a more preferred aspect.

[0010] Additionally, "room temperature" refers to a temperature within the range of 23°C ± 3°C. In addition, the "methanol production catalyst" will also be referred to simply as "catalyst."

[0011] (Method of manufacturing a catalyst for methanol production) The method for producing a catalyst for methanol production of the present invention comprises mixing a copper compound, zinc nitrate, and oxalic acid in an alcohol solvent to form a precipitate, and then drying and calcining the precipitate to produce a catalyst made of a composite oxide containing copper and zinc.

[0012] The catalyst production method of the present invention is capable of producing methanol with high activity and high efficiency by the above-mentioned technique. The reason for this is presumed to be as follows.

[0013] Conventionally, Cu / Zn-based catalysts for methanol production are produced by mixing metal oxide precursors in water using a solid-phase precipitation method, forming a precipitate, and then drying and calcining the precipitate. However, in order to further increase the activity of the catalyst, it is necessary to micronize the resulting catalyst in order to increase the active sites of the catalyst.

[0014] Therefore, in the method for producing a catalyst of the present invention, a metal oxide precursor is mixed in an alcohol solvent, a precipitate is formed, and the precipitate is dried and calcined to produce a catalyst. The alcohol solvent has a lower surface tension than water, and when the precipitate is dried, the aggregation of the precipitate is suppressed. As a result, the catalyst obtained is finer and the active sites of the catalyst are increased.

[0015] Therefore, it is presumed that the method for producing a catalyst of the present invention is capable of producing methanol with high activity and high efficiency. In addition, the catalyst manufacturing method of the present invention makes it possible to produce a catalyst without adding a pH adjuster, which saves a large amount of water required to wash away residual ions of the pH adjuster before drying, thereby reducing costs.

[0016] The process for producing the catalyst of the present invention will be described in detail below.

[0017] First, in the method for producing a catalyst of the present invention, specifically, a catalyst is produced, for example, as follows. 1) As metal oxide precursors, a copper compound and a zinc compound are dissolved in an alcohol solvent at room temperature to obtain solution A. 2) Solution B is obtained by dissolving oxalic acid in an alcohol solvent. 3) After mixing solution B and solution A, the mixed solution is stirred at room temperature and normal pressure (1 atm) for 0.5 to 15 hours (preferably 2 to 8 hours) to form a precipitate by coprecipitation of the copper compound and the zinc compound. 4) The precipitate is separated from the alcohol solvent by a separation method such as centrifugation or filtration. Before drying, the precipitate after separation may be left to stand for 5 to 500 hours for aging. Furthermore, before drying, the precipitate after separation or aging may be washed with ion-exchanged water or the like. 5) The obtained precipitate is dried under an air atmosphere or an inert gas atmosphere at a drying temperature of 100 to 150° C. (preferably 100 to 120° C.) for a drying time of 10 to 24 hours (preferably 15 to 20 hours). 6) The resulting dried product is calcined under an air atmosphere or an inert gas atmosphere at a calcination temperature of 300 to 500° C. (preferably 350 to 400° C.) for a calcination time of 3 to 8 hours (preferably 4 to 6 hours).

[0018] By the above operations, a catalyst made of a composite oxide containing copper and zinc is obtained. The catalyst obtained by calcination may be subjected to activation treatment such as reduction (for example, in a hydrogen stream) after particle size adjustment, if necessary. In addition, when the catalyst is handled in air, the surface of the catalyst may be subjected to a passivation treatment.

[0019] Here, when producing a catalyst made of a composite oxide containing copper, zinc, and aluminum, in addition to a copper compound and a zinc compound, an aluminum compound is also dissolved in an alcohol solvent to obtain solvent A. That is, in addition to a copper compound, a zinc compound, and oxalic acid, an aluminum compound is mixed in an alcohol solvent to form a precipitate by coprecipitation of the copper compound, the zinc compound, and the aluminum compound.

[0020] When a promoter other than aluminum (such as gallium) is contained in the catalyst, a compound containing the promoter metal is mixed in the alcohol solvent.

[0021] -Metal oxide precursor- When producing a catalyst made of a composite oxide containing copper and zinc, a copper compound and a zinc compound are used as the metal oxide precursor. When producing a catalyst made of a composite oxide containing copper, zinc and aluminum, a copper compound, a zinc compound and an aluminum compound are used as the metal oxide precursor.

[0022] These metal oxide precursors are applied as compounds that dissolve in the alcohol solvent to be applied. Specifically, the metal oxide precursor is, for example, a compound that dissolves in an amount of 14 g or more (preferably 16 g or more) in 100 g of an alcohol solvent at room temperature.

[0023] Examples of metal oxide precursors include metal nitrates, metal acetates, metal chlorides, metal bromides, and ammonium heavy metal salts. That is, examples of copper compounds include copper nitrate, copper acetate, copper chloride, copper bromide, and ammonium bicuprate. Examples of zinc compounds include zinc nitrate, zinc acetate, zinc chloride, zinc bromide, and ammonium bizincate. Examples of the aluminum compound include aluminum nitrate, aluminum acetate, aluminum chloride, aluminum bromide, and ammonium bialuminate. Each metal oxide precursor may be used alone or in combination of two or more kinds.

[0024] The metal oxide precursor may be a non-hydrate or a hydrate, but is preferably a hydrate from the viewpoints of solubility in a solvent and ease of handling.

[0025] The ratio of the copper compound, zinc compound, and aluminum compound is selected according to the component ratio (mass %) of the catalyst to be produced.

[0026] -Oxalic acid- Oxalic acid may be in the form of a non-hydrate or a hydrate. From the viewpoints of solubility in a solvent and ease of handling, however, a hydrate (ie, oxalic acid dihydrate) is preferred. The amount of oxalic acid mixed relative to the total amount of the metal oxide precursors is preferably 20 to 50 mass %, more preferably 32 to 43 mass %, from the viewpoint of forming a sufficient precipitate.

[0027] -Alcohol solvent- The alcohol solvent may be either a monohydric alcohol or a polyhydric alcohol, and the alcohol may be either an aliphatic alcohol or an aromatic alcohol. Specific examples of the alcohol solvent include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 1-pentanol, ethylene glycol, and benzyl alcohol. The alcohol solvent may be used alone or in combination of two or more kinds.

[0028] However, in order to obtain a catalyst that can produce methanol more efficiently by miniaturizing the catalyst and making it more active, the alcohol solvent must have a surface tension of 48 mN m -1 Less than or equal to 25mN m -1 Less than or equal to 23 mN m is preferable.-1 It is advisable to use an alcohol solvent such as that described below.

[0029] Here, the surface tension of the alcohol solvent is a value measured using a surface tensiometer at a liquid temperature of 23°C. In addition, when the alcohol solvent is a mixed solvent in which two or more alcohol solvents are mixed, the surface tension is the surface tension of the mixed solvent.

[0030] (Catalyst for methanol production) The catalyst for methanol production of the present invention comprises a composite oxide containing copper and zinc, and has a CuO crystallite size of 14 nm or less before catalytic reduction, calculated from the half-width of the X-ray diffraction pattern. The catalyst of the present invention has a small CuO crystallite size of 14 nm or less before catalytic reduction, and therefore has many active sites, making it highly active and capable of producing methanol more efficiently. The catalyst of the present invention is, for example, a catalyst produced by the above-mentioned method for producing a catalyst of the present invention.

[0031] The catalyst of the present invention will be described in detail below. The catalyst of the present invention is made of a composite oxide containing copper and zinc. The composite oxide may further contain aluminum in addition to copper and zinc.

[0032] -Crystallite size- In the catalyst of the present invention, the crystallite size of CuO before reduction of the catalyst is preferably 14 nm or less, and more preferably 10 nm or less. However, from the viewpoint of suppressing a decrease in activity due to aggregation, the crystallite size of CuO before reduction of the catalyst is preferably 6 nm or more.

[0033] From the viewpoint of active and more efficient methanol production, the crystallite size of Cu after catalytic reduction, calculated from the half-width of the X-ray diffraction pattern, is preferably 14 nm or less, more preferably 12 nm or less, and even more preferably 10 nm or less. However, from the viewpoint of suppressing a decrease in activity due to aggregation, the crystallite size of Cu after catalyst reduction is also preferably 6 nm or more. The catalyst reduction conditions were a reduction temperature of 260° C. and a reduction time of 4 hours.

[0034] The method for measuring the crystallite sizes of CuO and Cu is as follows. X-ray diffraction (XRD) measurement is performed on the catalyst before reduction (i.e., the composite oxide) or the catalyst after reduction to be measured, and an X-ray diffraction pattern is obtained. In the X-ray diffraction pattern, the diffraction peaks of CuO or Cu are identified by checking against the database (CuO PDF-#48-1548 or Cu PDF-#04-0836). Then, the crystallite size of CuO or Cu is calculated from the half-width of the identified CuO or Cu diffraction peak using the following formula (Debye-Scherrer formula). Formula: D = 0.9λ / βcosθ D: Crystallite diameter (n,) λ: X-ray (CuK α1 line) wavelength 1.541051 Å β: Half-width (rad) θ: Diffraction angle at the apex of the diffraction peak (degrees)

[0035] Here, the X-ray diffraction is carried out under the following conditions. X-ray diffraction equipment: Rigaku "RINT 2200" ·Radiation source:CuKα1 Voltage 40kV ·Current: 20mA Specimen rotation speed: No rotation Divergence slit: 1.00mm, Vertical limit divergence slit: 10mm Scattering slit: open Receiving slit: open Scanning mode: FT Counting time: 2.0 seconds Step width: 0.020° ·Operation axis: 10.0000°~80.0000°

[0036] -Ingredient ratio- In the catalyst of the present invention, when the catalyst is made of a composite oxide containing copper and zinc, the component proportions in the composite oxide, in terms of metal, are preferably copper: 30% by mass or more and 70% by mass or less, and zinc: 30% by mass or more and 70% by mass or less, and more preferably copper: 40% by mass or more and 60% by mass or less, and zinc: 40% by mass or more and 60% by mass or less.

[0037] In the catalyst of the present invention, when the catalyst is made of a composite oxide containing copper, zinc, and aluminum, the component proportions in the composite oxide, in terms of metal, are preferably from 30% by mass to 60% by mass of copper, from 30% by mass to 60% by mass of zinc, and from 1 to 10% by mass of aluminum, and more preferably from 35% by mass to 55% by mass of copper, from 35% by mass to 55% by mass of zinc, and from 4 to 6% by mass of aluminum.

[0038] In the catalyst of the present invention, when the component ratio in the composite oxide is within the above range, the efficiency of methanol production is improved.

[0039] The composite oxide may contain a promoter other than aluminum (such as gallium). The catalyst of the present invention may contain impurities that are mixed in during the catalyst production process, etc. However, from the viewpoint of improving the catalytic activity, the smaller the amount of impurities, the more preferable it is, and it is preferable to prevent impurities from being mixed in as much as possible.

[0040] The component ratios in the composite oxide are determined quantitatively by scanning high-frequency inductively coupled plasma spectrometry (ICP-AES method). Specifically, a sample is obtained by crushing a catalyst to be measured. An alkali melting agent (e.g., sodium carbonate, sodium borate, etc.) is added to the sample, which is then heated and melted in a platinum crucible. After cooling, the entire amount is dissolved in a hydrochloric acid solution under heating. The obtained sample solution is injected into an ICP analyzer. When the device is operated, the sample solution is atomized and thermally excited in the high-temperature plasma state inside the device, and when this returns to the ground state, an emission spectrum with wavelengths specific to the element is generated. The type and amount of contained elements are qualitatively and quantitatively determined from the emission wavelength and intensity. The component ratio of each metal is calculated by using the total amount of Cu and Zn, or the total amount of Cu, Zn, and Al as the denominator and the mass of each metal as the numerator.

[0041] -Other specifics- The catalyst of the present invention may be in the form of a powder or a molded body having any shape. However, the size of the catalyst is preferably 10 μm to 1 mm in average particle size. The size of the catalyst of the present invention is adjusted, for example, by crushing, sieving, or the like. When the catalyst has an average particle size of 10 μm or more, the efficiency of the solid-liquid separation operation between the catalyst and the product is improved. When the catalyst of the present invention has an average particle size of 1 mm or less, the surface area of ​​the catalyst is sufficiently large to fully exert catalytic activity. The average particle size of the catalyst is determined by obtaining a particle size distribution by a laser diffraction method (wet method), and is the cumulative 50% diameter (volume average particle size) accumulated from the smallest particle size on a volume basis.

[0042] The specific surface area of ​​the catalyst of the present invention is, for example, 1 to 400 m 2 / g. Generally, in order to achieve good catalytic activity, the larger the specific surface area of ​​the catalyst, the more advantageous it is. The specific surface area of ​​the catalyst is 400m 2 / g or less, the catalyst strength is improved. 2 When the catalytic activity is 1.0 to 1.5 carbon atoms / g or more, the contribution efficiency of the active metal to the reaction is improved, and sufficient catalytic activity is easily obtained. The specific surface area of ​​the catalyst is a measured value determined by the BET method using nitrogen gas adsorption and desorption.

[0043] (Method of producing methanol) In the method for producing methanol of the present invention, a raw material gas containing hydrogen and carbon dioxide, or a raw material gas containing hydrogen, carbon monoxide and carbon dioxide, is introduced into a reaction field in which a catalyst for methanol production produced by the method for producing a catalyst for methanol production of the present invention or the catalyst for methanol production of the present invention is present, to produce methanol.

[0044] The methanol production process of the present invention will be described in detail below.

[0045] -reaction- In the method for producing methanol of the present invention, for example, after a catalyst is placed in a reaction field (specifically, after a reaction vessel is filled with the catalyst), a raw material gas is passed through the reaction field (specifically, the reaction vessel) to bring the raw material gas into contact with the catalyst. It is preferable that the catalyst is heated under an inert gas (nitrogen, etc.) atmosphere and brought into contact with hydrogen gas to carry out a reduction treatment before bringing the raw material gas into contact with the catalyst (i.e., before methanol is synthesized). As for the type of reaction vessel, any of a fixed bed, an entrained bed, and a fluidized bed can be suitably used.

[0046] From the viewpoint of highly efficient methanol production, the raw material gas is preferably introduced into the reaction field (specifically, the reaction vessel) at a rate of 10 to 1000 mL / min (preferably 50 to 600 mL / m) per 1 g of catalyst. In particular, the raw material gas is preferably introduced so that the pressure of the methanol gas in the reaction field is constant.

[0047] - Raw material gas - In the method for producing methanol of the present invention, the raw material gas used is a raw material gas containing hydrogen and carbon dioxide, or a raw material gas containing hydrogen, carbon monoxide and carbon dioxide.

[0048] When a raw material gas containing hydrogen and carbon dioxide is used as the raw material gas, the molar ratio of hydrogen to carbon dioxide (hydrogen / carbon dioxide) in the raw material gas is preferably 1 / 1 to 10 / 1, and more preferably 2 / 1 to 5 / 1, from the viewpoint of highly efficient methanol production.

[0049] When a raw material gas containing hydrogen, carbon monoxide, and carbon dioxide is used as the raw material gas, the molar ratio of hydrogen to carbon monoxide and carbon dioxide in the raw material gas (hydrogen / (carbon monoxide+carbon dioxide)) is preferably 1 / 1 to 10 / 1, and more preferably 2 / 1 to 5 / 1, from the viewpoint of highly efficient methanol production. Moreover, the molar ratio of carbon monoxide to carbon dioxide (carbon monoxide / carbon dioxide) in the raw material gas is preferably 0.5 / 1 to 10 / 1, and more preferably 3 / 1 to 7 / 1, from the viewpoint of highly efficient methanol production.

[0050] The raw material gas may contain an inert gas, provided that the total amount of hydrogen, carbon monoxide, and carbon dioxide in the raw material gas is within the range of 90 mol % or more.

[0051] From the viewpoint of highly efficient methanol production, the raw material gas is preferably introduced into the reaction field (specifically, the reaction vessel) at a gaseous rate of 10 to 200 mL / min (preferably 50 to 100 mL / min) per 1 g of catalyst.

[0052] -others- In the method for producing methanol of the present invention, methanol may be introduced into the reaction field in the presence of the catalyst together with the raw material gas. By introducing methanol, methanol can be produced with even higher efficiency.

[0053] When methanol is introduced into the reaction field together with the raw material gas, the methanol introduced into the reaction field may be in a gas phase or a liquid phase. That is, the methanol hs introduced together with the raw material gas may be in a gas state or in a methanol liquid state. The number of methanol molecules that can exist in the same volume in both liquid and gas phases is smaller in the gas phase, so if the reaction proceeds in a reaction system supplied as a gas phase, the reaction will also proceed sufficiently in a reaction system supplied as a liquid phase. When supplied as a liquid phase, the reaction is carried out in the form of droplets. It may be sprayed upstream of the reaction field and vaporized in the reaction field.

[0054] Specifically, from the viewpoint of highly efficient methanol production at low temperatures, it is advisable to introduce methanol into the reaction field of the raw material gas (specifically, the reaction vessel) at a rate of 15 mL / min or more (preferably 15 to 28 mL / min, more preferably 20 to 24 mL / min) per 1 g of catalyst. From the viewpoint of highly efficient methanol production, the ratio of the amount of introduced methanol to the amount of introduced raw material gas (amount of introduced methanol / amount of introduced raw material gas) is preferably 0.025 to 2.8, and more preferably 0.025 to 0.56.

[0055] Here, the molar ratio of methanol to the raw material gas (methanol / raw material gas) in the reaction field is preferably 1 / 14 to 1 / 2, and more preferably 1 / 7 to 1 / 4, from the viewpoint of highly efficient methanol production. EXAMPLES

[0056] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0057] <Example> (Catalyst Production) Cu(NO3)2·3H2O, Zn(NO3)2·6H2O, and Al(NO3)3·9H2O were dissolved in 40 mL of alcohol solution to prepare solution A. 2.791 g of H2C2O4·2H2O was dissolved in 33 mL of alcohol solution to prepare solution B. Here, the molar ratio of Cu / Zn / Al is the molar ratio that corresponds to the component ratio (mass%) of the catalyst shown in Table 1, and Cu 2+ , Zn 2+ , Al 3+ Solutions A and B were adjusted so that the total molar amount of was 0.021 mol and the H2C2O4 / (Cu+Zn+Al) ratio was 1.06 / 1. The alcohol solvent used was water (HO), methanol (MeOH), ethanol (EtOH), 1-propanol (n-PrOH), 2-propanol (i-PrOH), 1-butanol (n-BuOH), 2-butanol (s-BuOH), 1-pentanol (n-PeOH), ethylene glycol (EG), or benzyl alcohol (BNOH) according to Tables 1 to 4. Solution B was added to solution A, and the mixture was stirred at room temperature and atmospheric pressure for 6 hours to form a precipitate. The resulting precipitate was separated from the alcohol solvent by centrifugation. The precipitate was dried at 100°C for 15 h, and then calcined in air at 380°C for 4 h to obtain the catalyst.

[0058] (Methanol production) The reaction vessel of the fixed bed reactor was filled with 0.5 g or 2 g of catalyst. Before the reaction, the catalyst was reduced with H2 / Ar gas (volume ratio: 5 / 95) at 260°C for 4 hours, and the temperature was returned to room temperature after the reduction. Next, liquid methanol was vaporized and supplied to the reaction vessel at a supply rate of 0 mL / min (no supply), 0.002 or 0.003 mL / min together with raw material gas A (H2 / CO / CO2) with a volume ratio of H2 / CO / CO2 / Ar = 60 / 30 / 5 / 5.0 or raw material gas B (H2 / CO2) with a volume ratio of H2 / CO2 / Ar = 72 / 24 / 4. Under gas flow, the reaction temperature was set to 200°C, the pressure was set to 7 MPa, the raw material gas flow rate was set to 6 or 15 mL / min, and W / F (ratio of catalyst amount (W) to raw material gas supply rate (F)) was set to 12.4 or 124.4 g. cat Reactions were carried out as h / mol. The reaction conditions are shown in Tables 1 to 4.

[0059] The liquid components after the reaction were trapped using cooling water, and the gas components after the reaction were quantified online using a gas chromatograph (Shimadzu Gc-2014) equipped with a TCD (Thermal Conductivity Detector) detector, while the liquid components were quantified offline using a gas chromatograph (Shimadzu Gc-2014) equipped with an FID (Flame Ionization Detector) detector. And the total carbon conversion rate (A Total ), methanol (MeOH) selectivity (S MeOH ) was calculated using the following formula.

[0060]

number

[0061] In formula (1), A CO indicates the conversion rate of CO. (CO / Ar) inlet indicates the volume ratio of CO to Ar in the raw gas supplied to the reaction vessel. (CO / Ar) outlet indicates the volume ratio of CO to Ar in the gas components discharged from the reaction vessel after the reaction. In formula (2), A CO indicates the conversion rate of CO2. (CO2 / Ar) inlet indicates the volume ratio of CO2 to Ar in the raw gas supplied to the reaction vessel. (CO2 / Ar) outlet indicates the volume ratio of CO2 to Ar in the gas components discharged from the reaction vessel after the reaction. In formula (3), Ca represents the ratio (volume %) of CO in the raw material gas supplied to the reaction vessel, and Cb represents the ratio (volume %) of CO2 in the raw material gas supplied to the reaction vessel.

[0062]

number

[0063] In formula (4), N MeOH is the molar amount of carbon that constitutes the liquid component methanol produced after the reaction and discharged from the reaction vessel, N total indicates the molar amount of carbon constituting the liquid and gas components produced after the reaction and discharged from the reaction vessel.

[0064] [Table 1]

[0065] [Table 2]

[0066] [Table 3]

[0067] [Table 4]

[0068] From the above results, it is understood that in this embodiment, the catalyst has high activity, the total carbon selectivity and the methanol selectivity are high, and methanol can be produced with high efficiency, as compared with the comparative example. It is also understood that the lower the surface tension of the alcohol solvent, the smaller the crystallite size of the CuO and the crystallite size of the Cu catalyst, and the higher the activation, the higher the total carbon selectivity and methanol selectivity, and the more efficiently methanol can be produced.

Claims

1. A method for producing a catalyst for methanol production, comprising mixing a copper compound, zinc nitrate, and oxalic acid in an alcohol solvent to form a precipitate, and then drying and calcining the precipitate to produce a catalyst made of a composite oxide containing copper and zinc.

2. 2. The method for producing a catalyst for methanol production according to claim 1, further comprising mixing an aluminum compound into the alcohol solvent to produce a catalyst made of a composite oxide containing copper, zinc and aluminum.

3. The surface tension of the alcohol solvent is 48 mN·m -1 2. The method for producing a catalyst for methanol production according to claim 1, wherein the catalyst is:

4. A catalyst for methanol production comprising a composite oxide containing copper and zinc, the crystallite size of CuO being 14 nm or less before catalytic reduction as calculated from the half-width of an X-ray diffraction pattern.

5. 5. The catalyst for methanol production according to claim 4, wherein the composite oxide has a component ratio, calculated as metal, of copper: 30% by mass or more and 70% by mass or less, and zinc: 30% by mass or more and 70% by mass or less.

6. 5. The catalyst for methanol production according to claim 4, wherein the composite oxide further contains aluminum.

7. 7. The catalyst for methanol production according to claim 6, wherein the composite oxide has component proportions, calculated as metals, of copper: 30% by mass or more and 60% by mass or less, zinc: 30% by mass or more and 60% by mass or less, and aluminum: 1% by mass or more and 10% by mass or less.

8. 5. The catalyst for methanol production according to claim 4, wherein the crystallite size of Cu after catalytic reduction is 14 nm or less, as calculated from the half-width of an X-ray diffraction pattern.

9. A method for producing methanol, comprising introducing a raw material gas containing hydrogen and carbon dioxide, or a raw material gas containing hydrogen, carbon monoxide and carbon dioxide, into a reaction field in which a catalyst for methanol production produced by the method for producing a catalyst for methanol production according to any one of claims 1 to 3 or the catalyst for methanol production according to any one of claims 4 to 8 is present, to produce methanol.

Citation Information

Patent Citations

  • Catalyst for synthesizing methanol

    JP1994312138A

  • Catalyst for synthesizing formate and methanol and method for producing formate and methanol