Method of producing nitride or oxynitride
By optimizing the pressure increase rate and raw material layer thickness in the combustion synthesis method, the method addresses the challenges of mass production in nitrides and oxynitrides, enhancing crushability and productivity.
Patent Information
- Application Number
- JP2023061801
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
AI Technical Summary
The combustion synthesis method for nitrides and oxynitrides faces challenges in achieving mass production due to issues with unreacted substances, internal sintering, and poor crushability, which are exacerbated when scaling up from laboratory-scale fabrication to mass production.
The method optimizes the pressure increase rate during nitrogen gas pressurization in the combustion synthesis process, adjusting it to 0.1 kPa/sec to 1.5 kPa/sec, and adjusts the raw material layer thickness to 50 mm to 300 mm, using specific diluents and bedding powders to enhance synthesis efficiency and crushability.
This approach improves the crushability and enables mass production of nitrides and oxynitrides by reducing unreacted materials and internal sintering, ensuring high productivity and product stability.
Smart Images

Figure 2024148571000001 
Figure 2024148571000002 
Figure 2024148571000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for synthesizing a nitride or oxynitride by combustion synthesis. [Background technology]
[0002] It has been reported that the synthesis of nitrides such as Si3N4, BN, AlN, and MgSiN2, and oxynitrides such as SiAlON, AlON, and Si2N2O can be performed using the combustion synthesis method. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-23406 A [Non-patent literature]
[0004] [Non-Patent Document 1] T. Sakurai, Y. Miyamoto, O. Yamada, Combustion synthesis of fine and high-purity AlN powder and its reaction control, J. Soc. Mater. Sci. Jpn., 54 (2005) 574-579. Summary of the Invention [Problem to be solved by the invention]
[0005] Combustion synthesis is an excellent method as an energy-saving synthesis method and as a technology that addresses environmental issues, but mass production technology for nitrides or oxynitrides has not yet been established.
[0006] Therefore, the present invention has been made in consideration of the above problems, and has an object to provide a method for producing a nitride or oxynitride that is excellent in mass productivity by optimizing the pressure increase step. [Means for solving the problem]
[0007] The method for producing a nitride or oxynitride according to the present invention is a method for obtaining a nitride or oxynitride by a combustion synthesis method, characterized in that in a nitrogen gas pressure increasing step, the pressure increase rate from 0 kPa to 100 kPa is adjusted to be 0.1 kPa / sec or more and 1.5 kPa or less, and after the pressure increase, the nitride or oxynitride is synthesized by the combustion synthesis method in a nitrogen atmosphere.
[0008] In the present invention, the pressure increase rate is preferably set to 0.6 kPa or less. In the present invention, it is preferable to adjust the layer thickness of the raw material to 50 mm or more and 300 mm or less, and then carry out the pressure increasing step. Effect of the Invention
[0009] According to the method for producing a nitride or oxynitride of the present invention, the crushability can be improved by adjusting the pressure increase rate, making mass production possible. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] An embodiment of the present invention (hereinafter, abbreviated as "embodiment") will be described in detail below. Note that the present invention is not limited to the following embodiment, and can be practiced with various modifications within the scope of the gist. Note that the notation "~" includes both the lower limit and the upper limit.
[0011] <Problems with the conventional technology> Combustion synthesis is known as a process for synthesizing inorganic compounds using the heat of reaction generated during chemical bonding of substances. Because combustion synthesis is a synthesis method that utilizes the heat generated by a reaction, basically, except for the energy required to start (ignite) the combustion reaction, synthesis is possible without any subsequent energy input, and the reaction proceeds quickly, making it a highly productive synthesis method.
[0012] By the way, it has been reported that the nitrides Si3N4, BN, and AlN, and the oxynitride SiAlON can be synthesized by the combustion synthesis method. Although the combustion synthesis method is an excellent method as an energy-saving synthesis method and as a technology that addresses environmental issues, it has also been pointed out that the mass production process of the above-mentioned compositions is difficult.
[0013] The main reason for this is the difficulty of controlling the reaction. That is, when moving from the lab-scale production in a laboratory to the mass-production scale in a mass-production facility, problems such as an increase in unreacted materials and internal sintering occur, leading to problems such as a deterioration in the stability and pulverizability of the product. Since the nitrides and oxynitrides are synthesized by gas-solid reactions, these phenomena occur significantly, posing a challenge for mass production. However, no definitive solutions to the above problems have been reported to date.
[0014] <Problems with manufacturing methods listed in patent and non-patent documents> Patent Document 1 discloses a method for synthesizing silicon nitride by combustion synthesis. Specifically, the dilution ratio is optimized to control the temperature of the reaction field in the combustion reaction to a desired temperature, making it easy to control the nitriding reaction. However, the diluent is silicon nitride, and as the diluent ratio increases, the product yield decreases, resulting in problems with poor mass productivity.
[0015] Non-Patent Document 1 proposes a method for synthesizing AlN by a combustion synthesis method. Specifically, it is proposed to add a diluent and a halide such as NHF or NH4Cl to the raw material of AlN to refine the primary crystal particles of the composite. However, when NHF or NH4Cl is used, toxic HF and HCl gases are generated. For this reason, there are problems such as high costs due to safety management and anti-corrosion measures for facilities, and difficulty in mass production. For these reasons, it has been difficult to effectively improve mass productivity in either case.
[0016] <Method of Manufacturing Nitride or Oxynitride in the Present Embodiment> When the amount of raw material is increased for mass production, the calorific value increases and the grindability decreases. This is thought to be due to the increase in the calorific value per volume, which leads to the primary crystals becoming larger. When considering mass production, it is desirable to increase the layer thickness of the raw material with a low dilution rate, but as mentioned above, this leads to a decrease in grindability, which is an issue.
[0017] Therefore, the inventors of the present invention have conducted extensive research and have discovered that the above problem occurs when the raw materials are compressed during the gas pressure increase process during vacuum nitrogen replacement before combustion synthesis, resulting in a decrease in volume. When performing combustion synthesis, the raw materials are filled into a heat-resistant container. At that time, gas exchange with the atmosphere mainly occurs at the top surface of the powder. Therefore, if the pressure increase rate in the pressure increase process exceeds the gas diffusion rate into the raw materials, the raw materials are compressed from the top surface of the powder, and the powder surface decreases, resulting in a decrease in volume. Therefore, the present invention was made with the aim of finding a pressure increase rate that can suppress the compression of the raw material.
[0018] That is, the method for producing a nitride or oxynitride in this embodiment is characterized in that, in the nitrogen gas pressure increasing step, the pressure increase rate from 0 kPa to 100 kPa is adjusted to be 0.1 kPa / sec or more and 1.5 kPa or less, and after the pressure increase, the nitride or oxynitride is synthesized by a combustion synthesis method in a nitrogen atmosphere.
[0019] As a result, even at a low dilution rate, good synthesis properties are exhibited and grindability can be improved. It was also found that good synthesis can be achieved even if the layer thickness of the raw material is made thicker than before. Conventionally, the layer thickness of the raw material was about 50 to 70 mm, but in the experiment described below, the layer thickness was set to 100 mm and good results were obtained. As a result, the problem of reduced pulverizability, which was an issue with the combustion synthesis method, can be improved, making mass production possible.
[0020] Each step of the method for producing the nitride or oxynitride will now be described. A raw material containing an element contained in the nitride or oxynitride and a diluent is filled into an insulating crucible. For example, a heat-resistant insulating material with a thermal conductivity of 0.2 W / m·K or less is used for the crucible, but is not limited thereto. The insulating material to be used can be determined depending on the raw material to be filled into the crucible. Examples of insulating materials that can be used include carbon, alumina fiber, and zirconia. For example, when synthesizing silicon nitride, if alumina fiber is used, Al and O form a solid solution, which reduces the thermal conductivity, and therefore effective insulating effects cannot be expected, so it is preferable to use carbon as the insulating material.
[0021] In this embodiment, the layer thickness of the raw material is adjusted to 50 mm or more and 300 mm or less. The "layer thickness" can be determined by measuring the layer thickness at multiple points and averaging them. In this embodiment, productivity can be increased by making the layer thickness of the raw material thicker. However, if the layer thickness is made too thick, the powder will be packed tightly together due to its own weight, resulting in poor combustion. In this embodiment, the layer thickness is preferably set to 100 mm or more and 200 mm or less.
[0022] The thickness of the powder is preferably 10 mm to 40 mm, more preferably 20 mm to 30 mm. In this embodiment, the temperature inside the raw material is high due to the combustion synthesis, and the thickness of the powder is adjusted to the above range in order to suppress the raw material reaction caused by the evaporation of the insulating material. By using the powder, the insulating effect can be increased more effectively.
[0023] The powder is spread, for example, on the side and bottom of the crucible. The powder may also be spread on the top surface of the raw material. The material of the powder is not limited, but for example, an inorganic material is used. Among the inorganic materials, nitrides, oxides, or carbides are preferable. For example, Si3N4 powder, AlN powder, BN powder, etc. can be used as the nitride. Furthermore, Al2O3 powder can be used as the oxide. Furthermore, SiC can be used as the carbide.
[0024] When the nitride is Si3N4, the dilution ratio of the diluent is preferably 3 wt% to 10 wt%, more preferably 4 wt% to 8 wt%, and even more preferably 4 wt% to 6 wt%. When the nitride is AlN, the dilution ratio is preferably 42 wt% to 60 wt%. When the nitride is BN, the dilution ratio is preferably 30 wt% to 50 wt%. In this way, the amount of unreacted Al and B can be reduced by increasing the dilution ratio of AlN and BN, which have a large calorific value, compared to Si3N4. Furthermore, the dilution ratio of the diluent is preferably 50 wt% or more and 60 wt% or less when the oxynitride is α-SiAlON, and is preferably 10 wt% or more and 30 wt% or less when the oxynitride is β-SiAlON.
[0025] When the diluent is Si3N4, the particle diameter of the Si3N4 powder is preferably about 0.1 to 1 μm, and more preferably about 0.4 to 0.8 μm. Here, the "particle diameter" refers to the "average particle diameter D50" that can be measured, for example, by a laser diffraction particle size distribution measuring device (HORIBA LA-950). "D50" is the particle diameter at which the cumulative number is 50% of the total number of particles. The particle diameter may be a manufacturer catalog value.
[0026] When the diluent is AlN, it is preferable to use a mixed powder of fine particles and coarse particles. Although not limited thereto, it is preferable that the particle size of the fine particles is 8 μm or less, and the particle size of the coarse particles is 100 to 150 μm. It is also preferable to use a mixture in which the fine particles and the coarse particles are mixed in a ratio of about 1:1. Therefore, the particle size distribution is a wide distribution with two peaks.
[0027] When the diluent is BN, the particle size of the BN powder is preferably about 1 to 20 μm, and more preferably about 5 to 10 μm. The definition of "particle size" is the same as that of the particle size of the Si3N4 powder described above.
[0028] The smaller the raw material particle size, the higher the combustion temperature tends to be. On the other hand, if the raw material particle size is too small, oxygen impurities increase, the combustion temperature decreases, and the amount of oxygen impurities in the composite increases, which tends to reduce performance. Therefore, it is preferable to maintain a certain size.
[0029] When the nitride is Si3N4, the particle size of Si contained in the raw material is preferably about 3 to 20 μm, more preferably 5 to 15 μm. Note that the particle size here is the size before mixing and pulverizing. After mixing the raw material components and pulverizing and mixing, the particle size of Si is about 1 to 5 μm, more preferably about 2 to 3 μm.
[0030] When the nitride is AlN, the particle size of Al contained in the raw material is preferably about 5 to 25 μm, more preferably about 6 to 20 μm. If the particle size is adjusted to be near the lower limit of the range, a problem occurs in which oxygen impurities increase, so the particle size of Al is more preferably about 10 to 15 μm. In addition, in the synthesis of AlN, pulverization is not performed after mixing the raw material components.
[0031] When the nitride is BN, the particle size of B contained in the raw material is preferably 5 μm or less, and more preferably the particle size of B after the raw material components are mixed, pulverized and mixed is about 1 to 2 μm.
[0032] The higher the nitrogen gas pressure, the higher the diffusion of nitrogen into the raw material, and the better the synthesis (the less sintering and unreacted products). However, in synthesis equipment that can handle high pressure, the equipment becomes more robust and the processing volume (reaction volume) becomes smaller, resulting in lower productivity. For this reason, the nitrogen gas pressure is preferably about 0.5 MPa to 3 MPa, more preferably about 0.8 MPa to 3 MPa, and even more preferably about 0.95 MPa to 2.5 MPa.
[0033] At this time, in this embodiment, the pressure increase rate from 0 kPa to 100 kPa is adjusted to 0.1 kPa / sec or more and 1.5 KPa or less. In this way, the pressure increase rate at the beginning of the pressure increase process is specified. That is, in this embodiment, the gas flow rate is constant, but the pressure increase rate starts to gradually decrease from a plateau after 100 kPa. In this way, the pressure increase rate fluctuates depending on the timing of measuring the pressure increase range, so it is specified as the pressure increase rate from 0 kPa to 100 kPa. In this embodiment, it is preferable to adjust the rate of pressure rise from 0 kPa to 100 kPa in the range of 0.1 kPa / sec to 0.6 kPa / sec.
[0034] After the pressure increase is completed, nitrides or oxide nitrides are obtained by a combustion synthesis method under a nitrogen atmosphere. In this embodiment, by regulating the pressure increase rate as described above, the sinking depth of the upper surface of the raw material can be reduced, preferably to 0 mm, and compression of the raw material can be suppressed, resulting in good pulverizability after synthesis. Specifically, the particle size (D50) of the pulverized powder can be reduced to 3.5 μm or less, preferably to 3.0 μm or less.
[0035] In the present embodiment, the nitrides produced by combustion synthesis are, for example, AlN, Si3N4, BN, MgSiN2, etc., but are not limited thereto, and can also be applied to GaN and InN in group 13 and Ge3N4 in group 14, which have similar properties in the periodic table. Also, the oxynitrides produced by combustion synthesis are, for example, SiAlON, AlON, Si2N2O, etc., but are not limited thereto. EXAMPLES
[0036] The present invention will be described in detail below with reference to examples carried out to clarify the effects of the present invention, but the present invention is not limited to the following examples.
[0037] <Experiment 1: Experiment on powder surface height according to pressure rise speed> [Raw materials] The raw materials used in this experiment are as follows: Si (element in nitrides): purity 4N, particle size 6μm α-Si3N4 (diluent): Purity 2N, particle size 1μm, dilution rate 8wt%
[0038] The above raw materials were pulverized and mixed in a vibration ball mill equipped with a urethane pot and silicon nitride balls of φ10 mm until the average particle diameter D50 of Si was 3 μm or less, and the bulk density was adjusted to 0.68 g / cc. The "average particle diameter D50" can be measured, for example, by a laser diffraction particle size distribution measuring device (HORIBA LA-950), and "D50" is the particle diameter at which the cumulative number is 50% of the total number of particles.
[0039] [Experimental Method] 1000g of the above raw materials were placed in a heat-resistant carbonaceous container measuring 100mm square x 200mm deep. After smoothing the top surface of the powder, vacuum replacement with nitrogen gas was performed up to 900kPa at each pressure increase rate. After that, the pressure was slowly reduced at a rate of 7.5kPa / min (2 hours) and returned to normal pressure, and the sinking depth from the top surface of the powder was measured.
[0040] The pressure rise rate was set to values between 0 and 100 kPa. Four pressure rise rates were used in the experiment: 0.30 kPa / sec, 0.60 kPa / sec, 1.05 kPa / sec, and 1.92 kPa / sec. When the gas pressure reached 800 kPa or higher, the pressure rise rate dropped significantly from the above rate, but no operation was performed to return the pressure rise rate to the above rate (i.e., the gas flow rate was always constant). The experimental results of the sinking depth are shown in Table 1.
[0041] [Table 1]
[0042] As shown in Table 1, when the pressure increase rate was made slower than 1.92 kPa, the sinking depth could be made smaller than 10 mm, and in particular, when the pressure increase rate was made 0.60 kPa or less, no sinking was observed (sinking depth = 0 mm).
[0043] <Experiment 2: Synthesis and crushing test> Combustion synthesis was started with each raw material used in experiment 1, and after the combustion synthesis was completed, the composite (β-Si3N4) was removed from the crucible and coarsely crushed using a jaw crusher and a hammer crusher. After that, 100 g of the coarse powder was dry-ground for 120 minutes in a planetary ball mill, and the particle size of each was measured.
[0044] The grinding conditions were a nylon pot and φ5mm silicon nitride balls. The particle size distribution was measured using a laser diffraction particle size distribution analyzer (HORIBA LA-950). The amount of unreacted silicon in the ground powder was quantified using XRD (Rigaku Mini Flex600-C). The particle size D50 and the amount of unreacted Si obtained by the crushing test are shown in Table 2 below.
[0045] [Table 2]
[0046] As shown in Table 2, it was found that the particle size D50 can be made smaller than 3.50 μm when the pressure increase rate is made smaller than 1.92 kPa. It was also found that the particle size D50 can be made 3 μm or less when the pressure increase rate is made 0.60 kPa or less, and the crushability can be improved. Furthermore, no unreacted Si was detected.
[0047] Based on the above experimental results, the pressure rise rate from 0 kPa to 100 kPa is set to 0.1 kPa / sec to 1.5 kPa / sec. The pressure rise rate from 0 kPa to 100 kPa is preferably set to 0.1 kPa / sec to 0.6 kPa / sec., and more preferably set to 0.3 kPa / sec to 0.6 kPa / sec.
[0048] <Experiment 3: Experiment on raw material layer thickness> Different amounts of the raw material (bulk density 0.68 g / cc) shown in Experiment 1 were placed in heat-resistant carbonaceous containers measuring 100 mm x 400 mm in depth. After smoothing the top surface of each raw material, the depth of the raw material was measured at four points, and the layer thickness was calculated from the average value.
[0049] The nitrogen gas was substituted by vacuum up to 900 KPa at a pressure increase rate of 0.60 KPa / sec (pressure increase rate from 0 kPa to 100 kPa).
[0050] Thereafter, the pressure was slowly reduced at a rate of 7.5 KPa / min over a period of 2 hours, and after the pressure was returned to normal, the depth to which the top surface of the raw material had sunk from the top surface of the powder was measured. Combustion synthesis was carried out under the same conditions as in Experiment 2.
[0051] After the synthesis was completed, the mixture was crushed coarsely using a jaw crusher and a hammer crusher. Then, 100 g of the coarse powder was dry-pulverized for 120 minutes using a planetary ball mill, and the particle size of each was measured.
[0052] The crushing conditions and the measurements of particle size D50 and the amount of unreacted Si by the crushing test were the same as in Experiment 2. The experimental results are shown in Table 3 below.
[0053] [Table 3]
[0054] As shown in Table 3, as the thickness of the raw material layer increases, the sinking depth increases, the particle size D50 becomes coarser, and unreacted Si is detected. This shows that the effect of the pressure rise rate decreases as the raw material layer thickness increases.
[0055] As shown in Table 3, when the raw material layer thickness exceeded 300 mm, unreacted Si was detected. In addition, when the raw material layer thickness reached about 220 mm, sinking of the raw material was observed, and it was found that the grindability began to decrease.
[0056] Based on the above, it is preferable to adjust the raw material layer thickness to 50 mm or more and 300 mm or less, more preferably to 50 mm or more and 200 mm or less, and even more preferably to 100 mm or more and 200 mm or less. [Industrial Applicability]
[0057] The nitride of the present invention can be effectively used not only as a heat dissipating filler but also as a material for ceramic substrates for heat dissipation, a reinforcing material for resins and glass, and the like.
Claims
1. A method for producing a nitride or oxynitride by combustion synthesis, comprising the steps of: In the nitrogen gas pressure increasing process, The pressure rise rate from 0 kPa to 100 kPa is adjusted to be 0.1 kPa / sec or more and 1.5 kPa or less, After the pressure is increased, the nitride or the oxynitride is synthesized by a combustion synthesis method in a nitrogen atmosphere.
2. A method for producing a nitride or oxynitride comprising the steps of:
2. 2. The method for producing a nitride or oxynitride according to claim 1, wherein the pressure increase rate is set to 0.6 kPa or less.
3. 2. The method for producing a nitride or oxynitride according to claim 1, wherein the layer thickness of the raw material is adjusted to 50 mm or more and 300 mm or less, and then the pressure increasing step is carried out.
Citation Information
Patent Citations
Method of producing high purity silicon nitride powder
JP2020023406A