Method for manufacturing magnetic toner
By employing a collection process with optimized magnetic force and flow conditions, the method significantly reduces empty beads in magnetic toner, improving image quality and reducing contamination in one-component development systems.
Patent Information
- Application Number
- JP2023061807
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
AI Technical Summary
Existing methods for producing magnetic toner in one-component development systems result in a significant number of 'empty beads' that contain little or no magnetic material, which negatively impact image quality and can cause in-machine contamination, despite efforts to optimize binder resin dissolution viscosity.
A method involving a collection step where magnetic toner particles are collected from an aqueous medium using a collecting section with a magnetic force within a flow path, optimizing parameters such as surface magnetic flux density, flow velocity, and concentration to reduce empty beads.
The method effectively reduces the number of empty beads in magnetic toner, enhancing image quality and minimizing contamination by selectively collecting magnetic toner particles.
Smart Images

Figure 2024148574000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a magnetic toner with fewer empty particles. [Background technology]
[0002] Magnetic toners used in one-component development generally contain a large amount of magnetic material (magnetic iron oxide particles) as a toner component compared to other components such as colorants, but during the production of magnetic toner, a certain number of particles called "empty particles" that contain little or no magnetic material are generated. If this is a small amount, it has little effect on printing, but from the standpoint of further improving image quality, it is preferable to have as few as possible. Conventionally, as a method for reducing empty particles in a magnetic toner, optimizing the dissolution viscosity of a binder resin has been proposed (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5517505 Summary of the Invention [Problem to be solved by the invention]
[0004] By using the methods described above, it is possible to reduce empty balls to a certain extent and also has the effect of suppressing contamination inside the machine. However, from the perspective of achieving even higher image quality, there is a demand for technology that can further reduce empty balls in the toner. [Means for solving the problem]
[0005] The present invention provides a method for producing a magnetic toner, comprising a recovery step of recovering magnetic toner particles from a magnetic toner particle dispersion liquid containing an aqueous medium and magnetic toner particles dispersed in the aqueous medium, the recovery step includes a collecting step of collecting the magnetic toner particles in a collecting section having a magnetic force and provided in a flow path through which the magnetic toner particle dispersion flows, The present invention relates to a method for producing a magnetic toner. Effect of the Invention
[0006] According to the present invention, a magnetic toner with fewer empty particles can be provided. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is an explanatory diagram showing an example of a recovery step in the production method of the present invention. [Diagram 2] 4 is a schematic cross-sectional view showing an example of a collection section in a recovery process. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In the present disclosure, the description of a numerical range such as "XX or more and YY or less" or "XX to YY" means a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined.
[0009] When the embodiments for carrying out the present invention are specifically illustrated with reference to the drawings, the dimensions, materials, shapes, and relative positions of the components described in the embodiments should be appropriately changed depending on the configuration of the members to which the present invention is applied and various conditions. In other words, it is not intended to limit the scope of the present invention to the following embodiments.
[0010] [Features of the present invention] The present invention is a method for producing a magnetic toner, which includes a recovery step of recovering magnetic toner particles from a magnetic toner particle dispersion liquid containing an aqueous medium and magnetic toner particles dispersed in the aqueous medium, and is characterized in that the recovery step includes a collection step of collecting the magnetic toner particles in a magnetic collecting section provided in a flow path through which the magnetic toner particle dispersion liquid flows.
[0011] The present inventors consider the reason why the effects of the present invention are manifested as follows.
[0012] In the present invention, the magnetic toner particles are collected in a collecting section having a magnetic force provided in a flow path through which an aqueous medium and a magnetic toner particle dispersion liquid containing magnetic toner particles dispersed in the aqueous medium flow. By collecting the magnetic toner particles in a magnetic section provided in the flow path, the magnetic toner particles can be selectively collected by the flow rate of the aqueous medium and the magnetic force, and the number of empty particles can be reduced.
[0013] FIG. 1 shows an example of a recovery process having a collection step according to the present invention. A more detailed description will be given in the following examples. First, a magnetic toner particle dispersion liquid with a properly adjusted magnetic toner particle concentration is introduced into a pre-recovery tank 1. Next, the magnetic toner particle dispersion liquid is transferred from the pre-recovery tank 1 to a pipe 3 provided in a flow path through which the dispersion liquid flows, using a pump 2. A magnetic collector is provided in the pipe 3, through which the magnetic toner particles are collected and the magnetic toner particles are collected with reduced empty particles. On the other hand, the processing liquid containing mainly empty particles after the collection process is transferred to a post-recovery tank 4 connected to the secondary side of the pipe 3. The processing liquid transferred to the post-recovery tank 4 may be discarded, or if magnetic toner particles are contained in the processing liquid, it may be returned to the upstream side of the pipe 3 for reprocessing. The pipe 3 may be provided in multiple stages.
[0014] FIG. 2 shows a specific embodiment of the collection section, in which a magnet 5 held by a fixing bracket 6 is provided within a pipe 3, and the toner particles collected by the magnet 5 are recovered by, for example, peeling them off, and then dried to obtain the desired magnetic toner particles.
[0015] It is also possible to provide the collection section in a tank (corresponding to tank 1 in FIG. 1) rather than in the flow path (corresponding to pipe 3 in FIG. 1), but this makes it difficult to obtain a sufficient effect of reducing empty particles.
[0016] Here, the surface magnetic flux density B (mT) of the collection portion is preferably 500 mT or more and 1300 mT or less. If the surface magnetic flux density B (mT) of the collection portion is 500 mT or more, it is preferable because it is easy to collect the magnetic toner particles to be collected. If the surface magnetic flux density B (mT) of the collection portion is 1300 mT or less, it is preferable because it reduces the erroneous collection of empty particles. The surface magnetic flux density B (mT) of the collection portion is more preferably 700 mT or more and 1200 mT or less, and even more preferably 900 mT or more and 1100 mT or less.
[0017] The flow velocity V (m / s) of the magnetic toner particle dispersion at the portion where the magnetic toner particle dispersion comes into contact with the collecting unit is preferably 0.01 m / s or more and 0.15 m / s or less. If the flow velocity V (m / s) of the magnetic toner particle dispersion is 0.01 m / s or more, it is preferable because it reduces the erroneous collection of empty particles into a portion having a magnetic force. If the flow velocity V (m / s) of the magnetic toner particle dispersion is 0.15 m / s or less, it is preferable because it is easy to collect the magnetic toner particles. The flow velocity V (m / s) of the magnetic toner particle dispersion at the portion where the magnetic toner particle dispersion comes into contact with the collecting unit is more preferably 0.02 m / s or more and 0.10 m / s or less, and even more preferably 0.03 m / s or more and 0.08 m / s or less.
[0018] The concentration of the magnetic toner particles in the magnetic toner particle dispersion liquid during the recovery process is preferably 0.02% by mass or more and 35.00% by mass or less. If the concentration of the magnetic toner particles in the magnetic toner particle dispersion liquid is 0.02% by mass or more, the magnetic toner particles can be collected by magnetic force, and if the concentration of the magnetic toner particles in the magnetic toner particle dispersion liquid is 35.00% by mass or less, it is preferable because it is easy to separate empty toner particles. The concentration of the magnetic toner particles is more preferably 0.05% by mass or more and 10.00% by mass or less, and even more preferably 0.10% by mass or more and 5.00% by mass or less.
[0019] It is preferable that the recovery process includes the collection process and, after the collection process, a separation process of reducing the magnetic force of the collection section and separating the magnetic toner particles from the collection section. By providing the separation process, the collected magnetic toner particles can be easily recovered. FIG. 2(b) shows an example of this embodiment, in which a magnet 5 is housed in a sheath tube 7. After the magnetic toner particles are collected, the magnet 5 is removed from the piping 3 together with the sheath tube 7, and the magnet 5 is then removed from the sheath tube 7, allowing the toner particles to be separated from the magnet.
[0020] The relationship between the surface magnetic flux density B (mT) of the collecting portion and the flow velocity V (m / s) of the magnetic toner particle dispersion at a portion where the magnetic toner particle dispersion contacts the collecting portion is as follows: 10000≦B / V≦75000 It is preferred that 12000≦B / V≦45000 is more preferred, 14000≦B / V≦35000 is more preferred.
[0021] The recovery step is preferably carried out in a state where the magnetic toner particles are coated with an inorganic dispersant, since the inorganic dispersant makes it difficult for problems such as fusion of the toner particles to occur.
[0022] The magnetic collector may be an electromagnet, a permanent magnet, etc., as long as it has a predetermined magnetic force. From the viewpoint of power consumption, a permanent magnet, particularly a neodymium magnet, is preferred.
[0023] [Magnetic Toner Constituent Materials] As the raw materials used in the production of the magnetic toner particles of the present invention, any other known raw materials may be used as long as they are magnetic substances.
[0024] <Crystalline materials> The crystalline material is a material that shows a clear melting point in differential scanning calorimetry, and the crystalline material is not particularly limited, but examples thereof include a release agent, a crystalline polyester resin, etc. The melting point of the crystalline material is preferably 50.0°C or more and 85.0°C or less.
[0025] Examples of the release agent include the following: aliphatic hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, microcrystalline wax, Fischer-Tropsch wax, and paraffin wax; oxides of aliphatic hydrocarbon waxes such as oxidized polyethylene wax, or block copolymers thereof; waxes mainly composed of fatty acid esters such as carnauba wax and montanic acid ester wax, and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax; saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and parinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bismuth Examples of such amides include saturated fatty acid bisamides such as stearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, and hexamethylene bisstearic acid amide; unsaturated fatty acid amides such as ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipic acid amide, and N,N'-dioleyl sebacic acid amide; aromatic bisamides such as m-xylene bisstearic acid amide and N,N'-distearyl isophthalic acid amide; fatty metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; waxes obtained by grafting aliphatic hydrocarbon waxes with vinyl monomers such as styrene and acrylic acid; partial esterification products of fatty acids and polyhydric alcohols, such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats.
[0026] When a wax containing fatty acid ester as a main component (hereinafter referred to as ester wax) is used as a release agent, it is easy to plasticize the binder resin and improve low-temperature fixability.
[0027] In the present invention, the crystalline material preferably contains a monoester compound. The monoester compound means an ester compound having one ester group in one molecule.
[0028] The melting point of the monoester compound is preferably 60° C. or more and 72° C. or less, more preferably 60° C. or more and 70° C. or less. When the melting point is in the above-mentioned range, it is possible to effectively improve the low-temperature fixing property of the toner. In addition, by controlling the charge decay rate of the toner after heating to a predetermined range, the sticking problem can be easily solved at the same time.
[0029] Examples of aliphatic alcohols that can be used for the monoester compound include the following: 1-hexanol, 1-heptanol, 1-octanol, 1-nonanol, 1-decanol, undecyl alcohol, lauryl alcohol, myristyl alcohol, 1-hexadecanol, stearyl alcohol, arachidyl alcohol, behenyl alcohol, and lignoceryl alcohol.
[0030] On the other hand, examples of aliphatic carboxylic acids include pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid.
[0031] The average number of carbon atoms per molecule of the monoester compound is preferably 36 or more and 42 or less. A monoester compound having an average number of carbon atoms of 36 or more has a lamellar structure due to a relatively long alkyl chain, and tends to have high electrical conductivity. Therefore, it is easy to control the charge decay rate of the toner after heating to a specific range. In addition, a monoester compound having an average number of carbon atoms of 42 or less is preferable because the monoester compound easily plasticizes the binder resin sufficiently when the toner is subjected to heat. The average number of carbon atoms is more preferably 36 or more and 40 or less.
[0032] As the monoester compound, a condensation product of an aliphatic alcohol having 6 to 24 carbon atoms and a long-chain carboxylic acid, or a condensation product of an aliphatic carboxylic acid having 4 to 24 carbon atoms and a long-chain alcohol can be used. Any long-chain carboxylic acid or long-chain alcohol can be used, but a combination that satisfies the above melting point is preferred.
[0033] The content of the monoester compound is preferably 13 parts by mass or more and 40 parts by mass or less, and more preferably 15 parts by mass or more and 35 parts by mass or less, relative to 100 parts by mass of the binder resin.
[0034] Hydrocarbon waxes are known to crystallize in a form in which linear hydrocarbon chain portions are stacked, and examples of such waxes include paraffin wax and Fischer-Tropsch wax.
[0035] In the suspension polymerization method, the hydrocarbon wax tends to form a large domain near the center of the toner particle, which makes it easier to locally distribute the small domains near the surface of the toner particle, making it easier to control the 25% ratio within the above range.
[0036] The content of the hydrocarbon wax is preferably from 0.5 to 20 parts by mass, and more preferably from 1 to 15 parts by mass, relative to 100 parts by mass of the binder resin.
[0037] The content of the crystalline material is preferably 3 parts by mass or more and 40 parts by mass or less, more preferably 20 parts by mass or more and 35 parts by mass or less, relative to 100 parts by mass of the binder resin. By making it 3 parts by mass or more, the low-temperature fixing property is improved, and it becomes easier to control the charge decay rate of the toner after heating. In addition, by making it 35 parts by mass or less, it is possible to maintain good hot offset resistance and storage stability.
[0038] <Binding resin> Examples of binder resins used in toners include homopolymers of styrene and its substitutes, such as polystyrene and polyvinyltoluene; styrene-propylene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-methyl acrylate copolymers, styrene-ethyl acrylate copolymers, styrene-butyl acrylate copolymers, styrene-octyl acrylate copolymers, styrene-dimethylaminoethyl acrylate copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-butyl methacrylate copolymers, styrene-dimethylaminoethyl methacrylate copolymers, styrene-vinyl methyl ether copolymers, styrene-vinyl ethyl ether copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-maleic acid copolymers, and styrene-maleic acid ester copolymers; and styrene-based copolymers, such as polymethyl methacrylate, polybutyl methacrylate, polyvinyl acetate, polyethylene, polypropylene, polyvinyl butyral, silicone resins, polyester resins, polyamide resins, epoxy resins, and polyacrylic acid resins.
[0039] These can be used alone or in combination of two or more kinds. Among these, styrene-based copolymers, such as styrene-butyl acrylate, are particularly preferred in terms of development characteristics, fixability, etc. The binder resin can also be used in combination with other known resins.
[0040] Examples of the styrene-based polymerizable monomer include styrene; α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, and p-methoxystyrene.
[0041] Examples of the acrylic polymerizable monomer include acrylic polymerizable monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, iso-propyl acrylate, n-butyl acrylate, iso-butyl acrylate, tert-butyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, and cyclohexyl acrylate.
[0042] Examples of the methacrylic polymerizable monomer include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, iso-propyl methacrylate, n-butyl methacrylate, iso-butyl methacrylate, tert-butyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, and n-octyl methacrylate.
[0043] The method for producing the styrene copolymer is not particularly limited, and any known method can be used.
[0044] <Coloring agent> The colorant may include the following organic pigments, organic dyes, and inorganic pigments.
[0045] Cyan colorants include copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds.
[0046] Examples of magenta colorants include the following: condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds.
[0047] Examples of yellow colorants include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds.
[0048] Examples of black colorants include carbon black, the above-mentioned yellow colorants, magenta colorants, cyan colorants, and colorants toned to black using magnetic materials.
[0049] These colorants can be used alone or in a mixture, or in the form of a solid solution. The colorant is selected in terms of hue angle, chroma, brightness, light resistance, OHP transparency, and dispersibility in toner particles. The content of the colorant is preferably 0.1 parts by mass or more and 60.0 parts by mass or less, more preferably 0.5 parts by mass or more and 50.0 parts by mass or less, based on 100 parts by mass of the binder resin.
[0050] <Magnetic material> The toner is made of a magnetic material. The magnetic material is mainly composed of magnetic iron oxide such as iron oxide or γ-iron oxide, and may contain elements such as phosphorus, cobalt, nickel, copper, magnesium, manganese, aluminum, and silicon. These magnetic materials have a BET specific surface area of 2 m2 or less as measured by the nitrogen adsorption method. 2 / g or more 30m 2 / g or less, and 2 / g or more 28m 2 / g or less. Also, the Mohs hardness is preferably 5 to 7. The shape of the magnetic material may be polyhedral, octahedral, hexahedral, spherical, needle-like, scale-like, etc., and those with less anisotropy such as polyhedral, octahedral, hexahedral, and spherical shapes are preferred in terms of increasing image density.
[0051] The magnetic material preferably has a number-average particle size of 0.10 μm or more and 0.40 μm or less. In general, the smaller the particle size of the magnetic material, the higher the coloring power, but the magnetic material tends to aggregate, so the above range is preferable from the viewpoint of the balance between coloring power and aggregation properties.
[0052] The number-average particle size of the magnetic material can be measured using a transmission electron microscope. Specifically, the toner to be observed is thoroughly dispersed in an epoxy resin, and then the resin is cured for two days in an atmosphere at a temperature of 40°C to obtain a cured product. The cured product is cut into a thin-section sample using a microtome, and the particle sizes of 100 magnetic particles in the field of view are measured using a transmission electron microscope (TEM) at a magnification of 10,000 to 40,000. The number-average particle size is calculated based on the equivalent diameter of a circle that is equal to the projected area of the magnetic material. It is also possible to measure the particle size using an image analyzer.
[0053] The magnetic material can be produced, for example, by the following method. An alkali such as sodium hydroxide is added to an aqueous solution of a ferrous salt in an amount equivalent or greater to the iron component to prepare an aqueous solution containing ferrous hydroxide. Air is blown into the aqueous solution while maintaining the pH of the prepared solution at pH 7 or higher, and the aqueous solution is heated to 70°C or higher to carry out an oxidation reaction of the ferrous hydroxide, thereby first producing seed crystals that will become the cores of the magnetic iron oxide powder.
[0054] Next, an aqueous solution containing about 1 equivalent of ferrous sulfate is added to the slurry liquid containing the seed crystals based on the amount of alkali added previously. The reaction of ferrous hydroxide is allowed to proceed while air is blown in while maintaining the pH of the liquid at 5 to 10, and magnetic iron oxide powder is grown around the seed crystals as a core. At this time, the shape and magnetic properties of the magnetic material can be controlled by selecting any pH, reaction temperature, and stirring conditions. As the oxidation reaction progresses, the pH of the liquid shifts to the acidic side, but it is preferable not to make the pH of the liquid less than 5. The magnetic material thus obtained can be obtained by filtering, washing, and drying it by a standard method.
[0055] In addition, when producing a toner in an aqueous medium, it is highly preferable to subject the magnetic material surface to a hydrophobic treatment. When performing surface treatment in a dry manner, the washed, filtered and dried magnetic material is treated with a coupling agent. When performing surface treatment in a wet manner, the dried material is redispersed after the oxidation reaction is completed, or the magnetic material obtained by washing and filtering after the oxidation reaction is redispersed in another aqueous medium without drying, and then the coupling treatment is performed. Either the dry method or the wet method can be appropriately selected.
[0056] Examples of coupling agents that can be used in the surface treatment of the magnetic material include silane coupling agents, titanium coupling agents, etc. Silane coupling agents are more preferably used.
[0057] When using a silane coupling agent, it is possible to use a single type of silane coupling agent or a combination of multiple types of silane coupling agents. When using a combination of multiple types of silane coupling agents, the treatment may be performed with each coupling agent individually or simultaneously.
[0058] The total amount of coupling agent used for treatment is preferably 0.9 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of the magnetic material, and it is important to adjust the amount of treatment agent depending on the surface area of the magnetic material, the reactivity of the coupling agent, etc.
[0059] In addition to the magnetic material, other colorants may be used in combination. Colorants that can be used in combination include the above-mentioned known dyes and pigments, as well as magnetic or non-magnetic inorganic compounds. Specifically, ferromagnetic metal particles such as cobalt and nickel, or alloys of these with chromium, manganese, copper, zinc, aluminum, rare earth elements, etc., particles such as hematite, titanium black, nigrosine dyes / pigments, carbon black, phthalocyanine, etc. are also included. It is preferable to treat the surface of these before use.
[0060] The amount of the magnetic material added is preferably 40 parts by mass or more and 200 parts by mass or less, more preferably 90 parts by mass or more and 160 parts by mass or less, relative to 100.0 parts by mass of the binder resin.
[0061] <Charge control agent> A charge control agent can be used in the toner as necessary. Known charge control agents can be used, but charge control agents that have a high triboelectric charging speed and can stably maintain a constant triboelectric charge amount are preferred. Furthermore, when the toner particles are produced by a suspension polymerization method, charge control agents that have low polymerization inhibition properties and are substantially free of solubilized substances in aqueous media are preferred.
[0062] Charge control agents include those that control the toner to be negatively charged and those that control the toner to be positively charged. Examples of charge control agents that control the toner to be negatively charged include the following: monoazo metal compounds, acetylacetone metal compounds, aromatic oxycarboxylic acids, aromatic dicarboxylic acids, oxycarboxylic acid or dicarboxylic acid-based metal compounds, aromatic oxycarboxylic acids, aromatic mono- or polycarboxylic acids or their metal salts, anhydrides, or esters, phenol derivatives such as bisphenol, urea derivatives, metal-containing salicylic acid-based compounds, metal-containing naphthoic acid-based compounds, boron compounds, quaternary ammonium salts, calixarene, and charge control resins.
[0063] The charge control agents can be used alone or in combination of two or more kinds.
[0064] Among these charge control agents, metal-containing salicylic acid compounds are preferred, and those in which the metal is aluminum or zirconium are particularly preferred.
[0065] The amount of the charge control agent added is preferably 0.01 parts by mass or more and 20.0 parts by mass or less, and more preferably 0.5 parts by mass or more and 10.0 parts by mass or less, relative to 100.0 parts by mass of the binder resin.
[0066] As the charge control resin, it is preferable to use a polymer or copolymer having a sulfonic acid group, a sulfonate group, or a sulfonate ester group. As the polymer having a sulfonic acid group, a sulfonate group, or a sulfonate ester group, it is preferable to contain a sulfonic acid group-containing acrylamide monomer or a sulfonate group-containing methacrylamide monomer in a copolymerization ratio of 2% by mass or more. More preferably, it is preferable to contain a sulfonic acid group-containing acrylamide monomer in a copolymerization ratio of 5% by mass or more.
[0067] The charge control resin preferably has a glass transition temperature (Tg) of 35° C. or more and 90° C. or less, a peak molecular weight (Mp) of 10,000 or more and 30,000 or less, and a weight average molecular weight (Mn) of 25,000 or more and 50,000 or less. When this charge control resin is used, it is possible to impart preferable triboelectric charging characteristics without affecting the thermal characteristics required for the toner particles. Furthermore, since the charge control resin contains a sulfonic acid group, the dispersibility of the charge control resin itself in the dispersion of the colorant and the dispersibility of the colorant are improved, and the coloring power, transparency, and triboelectric charging characteristics can be further improved.
[0068] <Particle size of magnetic toner> The weight average particle diameter (D4) of the magnetic toner is preferably 3.0 μm or more and 12.0 μm or less, more preferably 4.0 μm or more and 10.0 μm or less. When the weight average particle diameter (D4) is in the above range, good fluidity is obtained, and the latent image can be developed faithfully.
[0069] [Method of Manufacturing Magnetic Toner] The magnetic toner to be subjected to the recovery step according to the present invention may be produced by any known method.
[0070] For example, in the case of production by a pulverization method, the magnetic material, and optionally the binder resin, colorant, crystalline material, and other additives are thoroughly mixed in a mixer such as a Henschel mixer, a ball mill, etc. Thereafter, the various materials are melt-kneaded using a thermal kneader such as a heating roll, a kneader, or an extruder to disperse or dissolve them, and the magnetic toner particles are obtained through a cooling and solidifying step, a pulverization step, a classification step, and optionally a surface treatment step.
[0071] In the pulverization step, a known pulverization device such as a mechanical impact type or a jet type may be used. The order of the classification step and the surface treatment step is not important. In the classification step, it is preferable to use a multi-division classifier in terms of production efficiency.
[0072] The magnetic toner particles can be dispersed in an aqueous medium at any time after the pulverization step, and the recovery step according to the present invention can be carried out.
[0073] As a method for producing magnetic toner particles, suspension polymerization and emulsion aggregation can be preferably exemplified. When the toner particles are produced using the suspension polymerization and emulsion aggregation methods, the toner particles are produced in an aqueous medium, so that the toner particles can be easily incorporated into the production process. These production methods can easily sharpen the particle size distribution of the toner particles and increase the average circularity of the toner particles. It is also possible to produce toner particles having a core-shell structure.
[0074] Examples of the production of toner particles using the suspension polymerization method will be described in detail below, but the present invention is not limited to these.
[0075] The method for producing magnetic toner particles using the suspension polymerization method is as follows.
[0076] First, a polymerizable monomer composition is obtained by uniformly dissolving or dispersing a magnetic material, a polymerizable monomer capable of forming a binder resin as required, a colorant, a crystalline material, a polymerization initiator, a crosslinking agent, a charge control agent, and other additives.
[0077] Next, the polymerizable monomer composition is dispersed in a continuous layer (e.g., an aqueous medium) containing a dispersant using an appropriate stirrer, and particles of the polymerizable monomer composition are formed in the aqueous medium. Next, the polymerizable monomer contained in the particles of the polymerizable monomer composition is polymerized to obtain toner particles having a desired particle size. The stirring strength of the stirrer is preferably selected in consideration of material dispersibility, productivity, and the like.
[0078] The polymerization initiator may be added at the same time as the polymerizable monomer and other additives are added, or may be mixed immediately before dispersing the polymerizable monomer composition in the aqueous medium. Also, the polymerization initiator dissolved in the polymerizable monomer or solvent may be added immediately after forming particles of the polymerizable monomer composition and before starting the polymerization reaction.
[0079] When the above polymerizable monomers are polymerized, the polymerization temperature is usually 40°C or higher, preferably 50°C or higher and 90°C or lower.
[0080] As the polymerizable monomer, those exemplified as the polymerizable monomers forming the above-mentioned styrene-based copolymer are preferable.
[0081] The polymerization initiator preferably has a half-life of 0.5 to 30 hours during the polymerization reaction. When the polymerization reaction is carried out using an initiator in an amount of 0.5 to 20 parts by mass relative to 100 parts by mass of the polymerizable monomer, a polymer having a molecular weight maximum of 5,000 to 50,000 can be easily obtained.
[0082] Specific examples of the polymerization initiator include azo or diazo polymerization initiators such as 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, and azobisisobutyronitrile; and peroxide polymerization initiators such as benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, t-butyl peroxy 2-ethylhexanoate, and t-butyl peroxypivalate.
[0083] As the crosslinking agent, a compound having two or more polymerizable double bonds is mainly used. For example, aromatic divinyl compounds such as divinylbenzene and divinylnaphthalene; carboxylic acid esters having two double bonds such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, and 1,3-butanediol dimethacrylate; divinyl compounds such as divinylaniline, divinyl ether, divinyl sulfide, and divinyl sulfone; and compounds having three or more vinyl groups. These are used alone or as a mixture of two or more kinds.
[0084] The amount of the crosslinking agent added is preferably 0.1 parts by mass or more and 10.0 parts by mass based on 100 parts by mass of the polymerizable monomer.
[0085] The dispersant may be a known surfactant, an organic dispersant, or a poorly water-soluble inorganic dispersant. Examples of the inorganic dispersant include polyvalent metal phosphates such as tricalcium phosphate, magnesium phosphate, aluminum phosphate, zinc phosphate, and hydroxyapatite, carbonates such as calcium carbonate and magnesium carbonate, inorganic salts such as calcium metasilicate, calcium sulfate, and barium sulfate, and inorganic compounds such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide.
[0086] Examples of the surfactant include sodium dodecylbenzene sulfate, sodium tetradecyl sulfate, sodium pentadecyl sulfate, sodium octyl sulfate, sodium oleate, sodium laurate, sodium stearate, and potassium stearate.
[0087] The amount of inorganic dispersant added is preferably 0.2 parts by mass or more and 20.0 parts by mass or less with respect to 100 parts by mass of polymerizable monomer. The dispersant may be used alone or in combination with a plurality of kinds. Furthermore, a surfactant may be used in combination in an amount of 0.1 parts by mass or more and 10.0 parts by mass or less.
[0088] When an inorganic dispersant is used, it may be used as it is, but in order to obtain finer particles, inorganic dispersant particles may be generated in an aqueous medium and used. For example, in the case of tricalcium phosphate, a sodium phosphate aqueous solution and a calcium chloride aqueous solution are mixed under high speed stirring to generate water-insoluble calcium phosphate, which enables more uniform and fine dispersion.
[0089] The magnetic toner particles that have undergone the above steps can be filtered, washed and dried by known methods.
[0090] The recovery step can be performed at any timing after the polymerization reaction. After filtration or drying, the recovery step can be performed by dispersing the toner particles in the aqueous medium again.
[0091] The obtained toner particles may be used as they are as a toner. If necessary, an external additive may be added and mixed to adhere to the surface of the toner particles to form a toner. The external additive may be mixed by a known method such as a Henschel mixer.
[0092] In addition, a classification process can be added to the manufacturing process (before mixing with external additives) to remove coarse and fine powder. It is Noh.
[0093] As the external additive, inorganic fine particles having a number average particle size of primary particles of 4 nm or more and 80 nm or less (more preferably 6 nm or more and 40 nm or less) are preferable.
[0094] The number average particle size of the primary particles of the inorganic fine particles may be measured using a magnified photograph of the toner taken with a scanning electron microscope.
[0095] Inorganic fine particles are added to improve the fluidity of the toner and to make the chargeability of the toner uniform, but it is also possible to impart functions such as adjusting the charge amount of the toner and improving environmental stability by subjecting the inorganic fine particles to a hydrophobic treatment. Examples of treatment agents used in the hydrophobic treatment include silicone varnish, various modified silicone varnishes, silicone oil, various modified silicone oils, silane compounds, silane coupling agents, and other treatment agents such as organic silicon compounds and organic titanium compounds. These may be used alone or in combination of two or more.
[0096] Examples of inorganic fine particles include silica fine particles, titanium oxide fine particles, alumina fine particles, etc. As the silica fine particles, for example, both dry silica fine particles called dry method or fumed silica, which are produced by vapor phase oxidation of silicon halide, and wet silica fine particles produced from water glass or the like, can be used.
[0097] In addition, in the case of dry silica fine particles, it is also possible to obtain composite fine particles of silica and other metal oxides by using other metal halide compounds such as aluminum chloride and titanium chloride together with the silicon halide compound in the production process, and these are also included.
[0098] The amount of inorganic fine particles added is preferably 0.1 parts by mass or more and 3.0 parts by mass or less with respect to 100 parts by mass of toner particles.
[0099] The weight average particle diameter (D4) of the magnetic toner can be determined, for example, by the following measurement method.
[0100] <Method of measuring weight-average particle size (D4) of toner (particles)> The weight average particle size (D4) of the toner (particles) is measured with an effective measurement channel count of 25,000 channels using a precision particle size distribution measuring device equipped with a 100 μm aperture tube and a fine hole electrical resistance method called "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.) and the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.) for setting measurement conditions and analyzing measurement data, and the weight average particle size (D4) is calculated by analyzing the measurement data.
[0101] The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).
[0102] Before performing measurements and analysis, the dedicated software is set up as follows.
[0103] In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check the aperture tube flush after measurement.
[0104] In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.
[0105] The specific measurement method is as follows. (1) Pour about 200 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "Aperture Tube Flush" function of the dedicated software to remove dirt and air bubbles from inside the aperture tube. (2) Approximately 30 mL of the electrolyte solution is placed in a 100 mL flat-bottom glass beaker, and approximately 0.3 mL of a solution prepared by diluting "Contaminon N" (a 10% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7 consisting of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) three times by weight with ion-exchanged water is added as a dispersant. (3) A specified amount of ion-exchanged water is placed in the water tank of an ultrasonic disperser "Ultrasonic Dispersion System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two oscillators with an oscillation frequency of 50 kHz built in with a phase shift of 180 degrees and an electrical output of 120 W, and approximately 2 mL of Conaminon N is added to this water tank. (4) Set the beaker (2) in the beaker fixing hole of the ultrasonic disperser, operate the ultrasonic disperser, and adjust the height of the beaker so that the resonance state of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner (particles) is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, add the electrolytic solution (5) in which the toner (particles) is dispersed to the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the Analysis / Volume Statistics (Arithmetic Mean) screen is the weight-average particle size (D4).
[0106] In addition, the measurement of the "number of empty balls" in the examples described later was carried out by the following measurement method.
[0107] <Method of measuring the number of empty balls> Weigh 0.30 g of dried toner into a 50 ml beaker in 20% Contaminon RO water. Ultrasonicate and place the beaker on a neodymium magnet (anisotropic ferrite magnet, φ20 mm, thickness 10 mm, surface magnetic flux density 133 mT) for 3 minutes.
[0108] The number of empty balls is calculated as follows. The measuring device used is a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000.
[0109] The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).
[0110] Before carrying out the measurements and analyses, the dedicated software was set up as follows.
[0111] In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement."
[0112] In the "Pulse to particle size conversion setting" screen of the dedicated software, the bin interval is set to logarithmic particle size, the particle size bin is set to 256 particle size bins, and the particle size range is set to 2 μm to 60 μm.
[0113] The specific measurement method is as follows. (1) Pour 55.0 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the dedicated software to remove dirt and air bubbles from inside the aperture tube. (2) Into a 100 ml flat-bottom glass beaker, add 30.0 ml of a diluted solution obtained by diluting "Contaminon N" (a 10% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7 consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) approximately 5 times by weight with ion-exchanged water, and then add 0.3 g of dried toner particles. (3) Prepare an ultrasonic disperser "Ultrasonic Dispension System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees, and has an electrical output of 120 W. Place approximately 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank, and add approximately 2 mL of Conaminon N to this tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) The beaker from (4) is irradiated with ultrasonic waves and ultrasonic dispersion treatment is continued for 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) The beaker from (5) is removed from the ultrasonic disperser and placed on top of a neodymium magnet (anisotropic ferrite magnet φ20t10, surface magnetic flux density 133mT) for 3 minutes. (7) Using a micropipette, add 3.00 ml of the supernatant of the aqueous solution (6) in which the toner has been dispersed to the round-bottom beaker (1) placed in the sample stand, and start the measurement. The number of particles counted 50 seconds after the start of the measurement is regarded as the number of empty particles.
[0114] [Configuration included in the embodiment of the present invention] The disclosure of this embodiment includes the following configuration. (Configuration 1) A method for producing a magnetic toner, comprising a recovery step of recovering magnetic toner particles from a magnetic toner particle dispersion liquid containing an aqueous medium and magnetic toner particles dispersed in the aqueous medium, the recovery step includes a collecting step of collecting the magnetic toner particles in a collecting section having a magnetic force and provided in a flow path through which the magnetic toner particle dispersion flows, 2. A method for producing a magnetic toner comprising the steps of: (Configuration 2) The method for producing a magnetic toner according to Configuration 1, wherein the flow path has a pipe provided with the magnetic collector, through which the magnetic toner particle dispersion transferred from a tank prior to the recovery process passes. (Configuration 3) The method for producing a magnetic toner according to configuration 1 or 2, wherein the surface magnetic flux density B (mT) of the collecting portion is 500 mT or more and 1300 mT or less. (Configuration 4) The method for producing a magnetic toner according to any one of Configurations 1 to 3, wherein the flow velocity V (m / s) of the magnetic toner particle dispersion at a portion where the magnetic toner particle dispersion contacts the collecting portion is 0.01 m / s or more and 0.15 m / s or less. (Configuration 5) The method for producing a magnetic toner according to any one of Configurations 1 to 4, wherein the concentration of the magnetic toner particles in the magnetic toner particle dispersion before the collection step is 0.02% by mass or more and 35.00% by mass or less. (Configuration 6) The recovery step The collection step, and a separating step of reducing the magnetic force of the collecting section and separating the magnetic toner particles from the collecting section after the collecting step; 6. The method for producing a magnetic toner according to any one of Configurations 1 to 5, comprising: (Configuration 7) The relationship between the surface magnetic flux density B (mT) of the collecting portion and the flow velocity V (m / s) of the magnetic toner particle dispersion at a portion where the magnetic toner particle dispersion contacts the collecting portion is as follows: 10000≦B / V≦75000 7. The method for producing a magnetic toner according to any one of Configurations 1 to 6, which satisfies the above. EXAMPLES
[0115] The present invention will be described in more detail below with reference to Production Examples and Examples, which are not intended to limit the present invention in any way. In the following formulations, the number of parts refers to parts by mass unless otherwise specified.
[0116] <Production of magnetic iron oxide> Fe 2+ 50 L of an aqueous solution of ferrous sulfate containing 2.0 mol / L was mixed with 55 L of an aqueous solution of sodium hydroxide containing 4.0 mol / L, and stirred to obtain an aqueous solution of ferrous salt containing ferrous hydroxide colloid. This aqueous solution was kept at 85°C and an oxidation reaction was carried out while blowing in air at 20 L / min, to obtain a slurry containing core particles.
[0117] The obtained slurry was filtered and washed using a filter press, and the core particles were dispersed again in water to reslurry. Sodium silicate was added to this reslurry in an amount of 0.20 mass% silicon equivalent per 100 parts of core particles, the pH of the slurry was adjusted to 6.0, and the mixture was stirred to obtain magnetic iron oxide particles with a silicon-rich surface. The obtained slurry was filtered and washed using a filter press, and then reslurried in ion-exchanged water.
[0118] 500 parts (10% by mass relative to the magnetic iron oxide) of ion exchange resin SK110 (manufactured by Mitsubishi Chemical) was added to this reslurry liquid (solid content 50 g / L) and stirred for 2 hours to carry out ion exchange. After that, the ion exchange resin was removed by filtration through a mesh, and the mixture was filtered and washed with a filter press, dried and crushed to obtain magnetic iron oxide with a number average particle size of 0.23 μm.
[0119] <Production of silane compounds> 30 parts of iso-butyltrimethoxysilane was dropped into 70 parts of ion-exchanged water while stirring. Then, this aqueous solution was kept at pH 5.5 and temperature 55°C, and dispersed for 120 minutes at a peripheral speed of 0.46 m / s using a dispersing blade to carry out hydrolysis. Then, the pH of the aqueous solution was adjusted to 7.0, and the solution was cooled to 10°C to stop the hydrolysis reaction. Thus, an aqueous solution containing a silane compound was obtained.
[0120] <Manufacture of magnetic body 1> 100 parts of the magnetic iron oxide was placed in a high-speed mixer (LFS-2 model, manufactured by Fukae Powtec Co., Ltd.), and while stirring at a rotation speed of 2000 rpm, 8.0 parts of the aqueous solution containing the silane compound was added dropwise over a period of 2 minutes. The mixture was then mixed and stirred for 5 minutes. Next, in order to increase the adhesion of the silane compound, it was dried at 40°C for 1 hour to reduce the moisture, and then the mixture was dried at 110°C for 3 hours to allow the condensation reaction of the silane compound to proceed. The mixture was then crushed and passed through a sieve with 100 μm openings to obtain magnetic material 1.
[0121] Example 1 450 parts of 0.1 mol / L-Na3PO4 aqueous solution was added to 720 parts of ion-exchanged water and heated to 60°C, after which 67.7 parts of 1.0 mol / L-CaCl2 aqueous solution was added to obtain an aqueous medium containing a dispersion stabilizer.
[0122] Styrene: 76.0 parts n-Butyl acrylate: 24.0 parts Divinylbenzene 0.2 parts Monoazo dye iron complex (T-77: manufactured by Hodogaya Chemical Co., Ltd.): 1.5 parts ·Magnetic material 1: 120.0 parts The above recipe was uniformly dispersed and mixed using an attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to obtain a monomer composition. This monomer composition was heated to 63°C, and 25 parts of crystalline polyester as crystalline material (1) and 11 parts of paraffin wax (melting point 77°C, crystallization temperature 75°C), which is a hydrocarbon wax, as crystalline material (2) were mixed therein and dissolved.
[0123] The monomer composition containing the crystalline material was added to the aqueous medium, and the suspension was granulated by stirring for 10 minutes at 24,000 rpm (dispersion step: condition 1) at 60°C under a N2 atmosphere using a modified motor of a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.). Then, 8.0 parts of the polymerization initiator t-butyl peroxypivalate was added while stirring with a paddle stirring blade, and the temperature was raised to 70°C and reacted for 4 hours. After the reaction was completed, the suspension was cooled to room temperature.
[0124] The cooled suspension was filtered, and the magnetic toner particles were mixed with the filtrate of the suspension so that the concentration of the magnetic toner particles was 0.2% by mass, to prepare a toner particle dispersion.
[0125] Next, recovery processing was performed according to the flow of Figure 1, including the collection process with the specifications shown in Figure 2(a). The toner particle dispersion liquid was charged into the pre-recovery process tank 1. The amount of the toner particle dispersion liquid charged into the pre-recovery process tank was 10.00 kg. While stirring with a paddle blade to the extent that the toner particles in the pre-recovery process tank 1 did not settle, the toner particle dispersion liquid was transferred from the pre-recovery process tank 1 using pump 2, passed through pipe 3 in which a neodymium magnet was installed, and a collection process was performed, and the entire amount of the treatment liquid was transferred to the post-recovery process tank 4 connected to the secondary side of pipe 3 in which a neodymium magnet was installed.
[0126] Here, the pipe 3 for delivering the suspension had an inner diameter of 50 mm, and a neodymium magnet 5 with a diameter of 25 mm, a length of 300 mm, and a surface magnetic flux of 1000 mT was installed at the center of the inside of the pipe using a fixing bracket 6.
[0127] The flow rate of pump 2 was adjusted to 5.3 L / min so that the flow rate of the suspension passing next to the neodymium magnet was 0.06 m / s.
[0128] Thereafter, the neodymium magnet was removed, and the toner particles captured by the neodymium magnet were peeled off to obtain magnetic toner particles.
[0129] The collected magnetic toner particles were dried, and the mass and number of empty particles were measured. The weight average particle size (D4) of the magnetic toner particles measured by the above-mentioned measuring method was 7.0 μm.
[0130] The number of empty balls, the mass of the collected magnetic toner particles, and the recovery rate (yield) are shown in Table 2. At this time, the B / V calculated using the magnetic force B and the flow velocity V was 16667.
[0131] The collected magnetic toner particles are dispersed in RO water, and the dispersion stabilizer is dissolved by adding hydrochloric acid and thoroughly washing. The particles are then filtered and dried, and the magnetic toner particles are mixed with 100 parts of the magnetic toner particles and the BET value is 300m. 2 / g and 0.8 parts of hydrophobic silica fine particles having a number average particle size of 8 nm were mixed in a Mitsui Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to produce a finished magnetic toner.
[0132] Example 2 The neodymium magnet was changed to one with a diameter of 24 mm and housed in a sheath tube 7 with an outer diameter of 25 mm and an inner diameter of 24 mm as shown in FIG. 2(b). After collecting the magnetic toner particles in the same manner as in Example 1, the neodymium magnet was removed from the piping together with the sheath tube, and a separation process was carried out in which the toner particles were separated from the neodymium magnet by removing the neodymium magnet from the sheath tube. By removing the neodymium magnet, it was possible to recover the toner particles collected in the sheath tube more easily than in Example 1. The neodymium magnet was selected to have a stronger magnetic force than in Example 1 so that the magnetic force was a magnetic flux of 1000 mT on the surface of the sheath tube. Apart from that, the magnetic toner was produced in the same manner as in Example 1.
[0133] [Examples 3 to 25] A magnetic toner was produced in the same manner as in Example 1, except that the surface magnetic flux density B (mT) of the neodymium magnet, the flow velocity V (m / s) of the magnetic toner particle dispersion at the magnetic portion, the concentration (mass%) of the magnetic toner particle dispersion in the tank before the recovery process, and the amount of the toner particle dispersion to be treated (L) were changed as shown in Table 1.
[0134] The number of empty balls, the mass of the collected magnetic toner particles, and the recovery rate (yield) are shown in Table 2.
[0135] Example 26 After cooling to room temperature, 100 g of the suspension was transferred to a container, and while stirring the suspension, 10% hydrochloric acid was added to the container to adjust the suspension to pH = 1.4, and the suspension was stirred at room temperature for 2 hours to dissolve the dispersion stabilizer on the surface of the toner particles. After that, the suspension was filtered with a pressure filter and washed with 100 g of RO water, and this process was repeated three times.
[0136] The magnetic toner particles after filtration and washing were charged into a tank before the recovery process in the same manner as in Example 1, and mixed with RO water so that the toner particle concentration was 0.2% by mass, and the collection process was carried out.
[0137] When recovering the toner particles after collection, some toner particles were found adhering to the surface of the neodymium magnet, and the mass after collection was also reduced compared to Example 1. Since the toner particles had been washed once with hydrochloric acid, they were not washed with hydrochloric acid after collection. Other than that, the magnetic toner was produced in the same manner as in Example 1.
[0138] The number of empty balls, the mass of the collected magnetic toner particles, and the recovery rate (yield) are shown in Table 2.
[0139] Comparative Example 1 A magnetic toner particle dispersion liquid was prepared in the pre-recovery tank in the same manner as in Example 1, and after thorough stirring, the stirrer was stopped and the same neodymium magnet as in Example 1 was added to the pre-recovery tank. The neodymium magnet was observed from above the tank to confirm the state in which the toner particles were attracted to the neodymium magnet. 30 seconds after the neodymium magnet was added, almost no toner particles were seen to be attracted to the neodymium magnet, so the neodymium magnet was removed from the pre-recovery tank. The toner particles were peeled off from the removed neodymium magnet. Apart from that, a magnetic toner was produced in the same manner as in Example 1.
[0140] The number of empty balls, the mass of the collected magnetic toner particles, and the recovery rate (yield) are shown in Table 2.
[0141] Comparative Example 2 A magnetic toner particle dispersion liquid was prepared in the pre-recovery tank in the same manner as in Example 1, and after thorough stirring, a flow meter was inserted at a depth of 150 mm from the water surface at a location in the tank where the stirrer did not come into contact, and the stirrer rotation speed was adjusted so that the flow rate in the circumferential direction of the stirrer rotation was 0.06 m / s. The flow meter used was a simple propeller-type flow meter VR-401 manufactured by Kenec Co., Ltd. With the stirrer still running, the tip of the same neodymium magnet used in Example 1 was inserted at the location where the flow meter was inserted to a depth of 300 mm from the water surface, and was held in place. 30 seconds after the neodymium magnet was inserted, almost no adsorption of the toner particles to the neodymium magnet was observed, so the neodymium magnet was removed from the pre-recovery tank. The toner particles were peeled off from the removed neodymium magnet. Otherwise, a magnetic toner was produced in the same manner as in Example 1.
[0142] The number of empty balls, the mass of the collected magnetic toner particles, and the recovery rate (yield) are shown in Table 2.
[0143] [evaluation] The evaluation results of the number of empty balls based on the following evaluation ranks are shown in Table 3. (Evaluation criteria for number of empty balls) A: Less than 10,000 pieces B: More than 10,000 and less than 12,000 C: More than 12,000 and less than 15,000 D: More than 15,000 pieces
[0144] The evaluation results of the recovery rate based on the following evaluation ranks are shown in Table 3. (Yield Evaluation Criteria) A: 90.0% or more B: Less than 90.0% 80.0% or more C: Less than 80.0% 70.0% or more D: Less than 70.0%
[0145] [Table 1]
[0146] [Table 2]
[0147] [Table 3] [Explanation of symbols]
[0148] 1: tank before collection process, 2: pump, 3: piping for accommodating magnets (collection part with magnetic force), 4: tank after collection process, 5: magnet, 6: magnet fixing bracket, 7: sheath tube
Claims
1. A method for producing a magnetic toner, comprising: a recovery step of recovering magnetic toner particles from a magnetic toner particle dispersion liquid containing an aqueous medium and magnetic toner particles dispersed in the aqueous medium, the recovery step includes a collecting step of collecting the magnetic toner particles in a collecting section having a magnetic force and provided in a flow path through which the magnetic toner particle dispersion flows, 2. A method for producing a magnetic toner comprising the steps of:
2. The method for producing a magnetic toner according to claim 1 , wherein the flow path has a pipe provided with the magnetic collector, through which the magnetic toner particle dispersion liquid transferred from a tank before the recovery process passes.
3. 3. The method for producing a magnetic toner according to claim 1, wherein the surface magnetic flux density B (mT) of the collecting portion is 500 mT or more and 1300 mT or less.
4. 3. The method for producing a magnetic toner according to claim 1, wherein a flow velocity V (m / s) of the magnetic toner particle dispersion at a portion where the magnetic toner particle dispersion comes into contact with the collecting portion is 0.01 m / s or more and 0.15 m / s or less.
5. The method for producing a magnetic toner according to claim 1 or 2, wherein a concentration of the magnetic toner particles in the magnetic toner particle dispersion liquid before the collecting step is from 0.02% by mass to 35.00% by mass.
6. The recovery step comprises: The collection step, and a separating step of reducing the magnetic force of the collecting section and separating the magnetic toner particles from the collecting section after the collecting step; The method for producing a magnetic toner according to claim 1 or 2, comprising:
7. The relationship between the surface magnetic flux density B (mT) of the collecting portion and the flow velocity V (m / s) of the magnetic toner particle dispersion at a portion where the magnetic toner particle dispersion contacts the collecting portion is as follows: 10000≦B / V≦75000 The method for producing a magnetic toner according to claim 1 or 2, which satisfies the above condition.
Citation Information
Patent Citations
Electric material
JP1980017505A