Method for joining base material, joining device, and laminate
The use of methylglycine and UV irradiation forms a crosslinked layer for low-temperature bonding of base materials, addressing cost and performance issues in flexible circuit boards and semiconductor wafer stacking, enhancing bonding strength and reducing transmission loss.
Patent Information
- Application Number
- JP2023062066
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Current methods for joining base materials, such as those used in flexible printed circuit boards and semiconductor wafer stacking, face challenges with high costs, difficulty in forming fine patterns, increased transmission loss, and potential for current leakage due to roughened surfaces and polarity issues, especially in high-frequency applications.
A method involving the use of methylglycine as a crosslinking agent, combined with ultraviolet irradiation, to form a precursor layer at controlled oxygen and moisture concentrations, allowing base materials to be joined at low temperatures through a crosslinked layer, ensuring electrical neutrality and hydrophobicity.
This approach enables strong, low-temperature bonding of various materials, including copper foil and polymer films, with improved bonding strength and reduced transmission loss, suitable for high-frequency circuits and sensitive environments.
Smart Images

Figure 2024148702000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for bonding substrates, a bonding apparatus, and a laminate. [Background technology]
[0002] Polyimide (PI) films are used as insulating materials for flexible printed circuit boards (FPCs) due to their excellent heat resistance, flexibility, and electrical insulation. Flexible copper-clad laminates (FCCLs) are used to fabricate flexible printed circuit boards, and in flexible printed circuit boards that require fine circuit formation, the dry sputtering method is used as one of the methods for metallizing the polyimide surface. In commercially available metallized two-layer FCCLs, a seed layer of Ni / Cr alloy and Cu is formed on the polyimide surface by sputtering, and a conductor layer is formed on top of that by electrolytic Cu plating. This FCCL is advantageous for forming fine circuits because it is easy to make thin polyimide and conductor layers. However, the formation of a seed layer by sputtering is very expensive, and the price of FCCL is also high, limiting its use.
[0003] With the miniaturization and high performance of mobile information terminals such as smartphones, there is a strong demand for lighter, thinner, shorter, smaller flexible printed wiring boards, fine pattern circuit formation, and cost reduction. Current flexible printed wiring boards use inexpensive laminated or cast type FCCLs, which have a rough surface to ensure adhesion to the copper foil because the interface between the polyimide and conductor layer is not smooth and it is difficult to make the copper foil thin. In addition, it is difficult to make the flexible printed wiring board thin because the copper foil is thick. When forming FCCLs using these laminate or cast methods, roughening is required to ensure adhesion to the copper foil. However, in high-frequency applications, the current density of the outermost layer of the conductor increases due to the skin effect, so there is a problem that roughening the outermost layer increases transmission loss and heat generation. In addition, since the lands are large, the wiring formation area between the lands is small, making it difficult to miniaturize flexible printed wiring boards. In order to meet the market demand for lighter, thinner, shorter, and smaller flexible printed wiring boards, it is necessary to use metallized two-layer FCCLs, but this is difficult to adopt due to its high cost, and the emergence of cheaper materials and processes is desired.
[0004] On the other hand, a technology using an organic adhesive has been developed to bond and laminate polymer films at low temperatures (Patent Document 1). When using an organic adhesive, in a special environment such as a vacuum, the organic solvent may evaporate or escape from the adhesive layer of the final product over time, which may cause a decrease in the mechanical strength of the bonded portion. In addition, there is a risk of defects such as bubbles occurring, which reduces the yield and increases the final cost.
[0005] Furthermore, stacking of silicon wafers has become an important technology in the manufacturing of semiconductors, which are becoming increasingly miniaturized. Currently, bonding is performed using water, a method called fusion bonding. However, this method requires reheating at high temperatures after bonding, which can cause problems when managing the temperature history or when peeling is required. Surface activated bonding is being attempted as a method for bonding at room temperature. This method uses a bonding technique in which an intermediate layer of silicon is formed on the bonding surface. However, with this method, a silicon film, which is a semiconductor, is attached to both the insulating and conductive parts that make up the semiconductor circuit surface, making it prone to current leakage. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2008-150550 A [Patent Document 2] Patent No. 7018223 Summary of the Invention [Problem to be solved by the invention]
[0007] In order to solve the above problems, an object of the present invention is to provide a method for joining substrates, which firmly joins substrates together at low temperatures, a joining apparatus, and a laminate. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention employs the following means. That is, the method of the present invention for bonding a first substrate and a second substrate includes irradiating a first ultraviolet ray to one or both of a bonding surface of the first substrate and a bonding surface of the second substrate in the presence of a certain concentration of methylglycine to form a precursor layer, and abutting the first substrate and the second substrate to bond the first substrate and the second substrate via the precursor layer. According to this invention, a precursor layer is formed by irradiating the bonding surface of the first substrate and / or the bonding surface of the second substrate with the first ultraviolet light in the presence of a certain concentration of methylglycine, and the first substrate and the second substrate can be firmly bonded by contacting them with each other through this precursor layer.
[0009] In one embodiment of the present invention, the method includes irradiating one or both of the bonding surface of the first base material and the bonding surface of the second base material with a second ultraviolet ray before forming the precursor layer. In this embodiment, before forming the precursor layer, the bonding surface of the first substrate and / or the bonding surface of the second substrate are irradiated with a second ultraviolet ray, so that the surface on which the precursor layer is to be formed can be cleaned.
[0010] In one aspect of the present invention, the forming of the precursor layer and the bonding are performed in an environment in which oxygen concentration and moisture concentration are controlled. In this embodiment, the formation of the precursor layer and the bonding are performed in an environment in which the oxygen concentration and the moisture concentration are controlled, so that an appropriate environment can be prepared for each step.
[0011] In one aspect of the present invention, the oxygen concentration and water concentration are controlled in a vacuum or in an inert gas atmosphere. In this embodiment, the oxygen concentration and moisture concentration are controlled in a vacuum or in an inert gas atmosphere, so that an appropriate environment for controlling the oxygen concentration and moisture concentration can be created.
[0012] In one embodiment of the present invention, the first substrate and / or the second substrate is a laminate of any one or any combination of copper foil, glass, a semiconductor, a polymer film, a Si wafer, SiC, or any of these with circuits formed on the surface thereof. In this embodiment, a desired material can be selected as the substrate. Here, the semiconductor includes, for example, gallium nitride, gallium arsenide, and the like, which can be used in integrated circuits, solar cells, and the like.
[0013] In one embodiment of the present invention, the first substrate and / or the second substrate is any one of polymer films selected from the group consisting of LCP (liquid crystal polymer), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), PTFE (polytetrafluoroethylene), COP (cycloolefin polymer), PPS (polyphenylene sulfide), PEEK (polyether ether ketone), PI-based films (including PI (polyimide) and MPI (modified polyimide)), and PPE-based films (including PPE (polyphenylene ether) and mPPE (modified polyphenylene ether)), or a laminate of a combination of any one of these polymer films. In this embodiment, an appropriate material can be selected for the polymer film.
[0014] In one embodiment of the present invention, the first ultraviolet light and the second ultraviolet light have a dominant wavelength of any one of 126 nm, 146 nm, 156 nm, 172 nm, 185 nm, 206 nm, 222 nm, 254 nm, 283 nm, and 308 nm, or any combination thereof. In this embodiment, the first ultraviolet light and the second ultraviolet light can be selected to have appropriate dominant wavelengths.
[0015] The bonding apparatus of the present invention includes a chamber whose air pressure can be freely controlled, an inert gas supply source that supplies an inert gas to the chamber, and an ultraviolet ray irradiation mechanism and a methylglycine spray mechanism that are disposed within the chamber. According to this invention, it is possible to provide a bonding device capable of firmly bonding a first base material and a second base material.
[0016] The laminate of the present invention comprises a first substrate, a crosslinked layer made of methylglycine, and a second substrate laminated in this order. According to this invention, it is possible to provide a laminate having desired characteristics. Effect of the Invention
[0017] According to the present invention, it is possible to provide a method for joining substrates, which firmly joins substrates together at low temperatures, a joining device, and a laminate. [Brief description of the drawings]
[0018] [Figure 1] 5A to 5C are schematic diagrams illustrating a bonding step of base materials according to an embodiment of the present invention. [Diagram 2] 5A to 5C are schematic diagrams illustrating a bonding step of base materials according to an embodiment of the present invention. [Diagram 3] 5A to 5C are schematic diagrams illustrating a bonding step of base materials according to an embodiment of the present invention. [Figure 4] 5A to 5C are schematic diagrams illustrating a bonding step of base materials according to an embodiment of the present invention. [Diagram 5] 5A to 5C are schematic diagrams illustrating a bonding step of base materials according to an embodiment of the present invention. [Figure 6] 5A to 5C are schematic diagrams illustrating a bonding step of base materials according to an embodiment of the present invention. [Figure 7] FIG. 1 is a schematic plan view of a bonding device according to an embodiment of the present invention. [Figure 8] 1 is a process schematic diagram according to an embodiment of the present invention. [Figure 9] FIG. 13 is a diagram showing results according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] <Technology underlying the present invention> Before describing the embodiments of the present invention, a technology on which the present invention is based will be described.
[0020] Patent Document 2 discloses a bonding method and a laminate for performing organic-inorganic hybrid bonding at low temperature and atmospheric pressure and improving water resistance reliability. This document discloses the invention of a "Vapor-Assisted Vacuum Ultraviolet (V-VUV) method in a nitrogen atmosphere containing lower alcohol vapor" in order to achieve general-purpose bonding properties for dissimilar materials at low temperature and atmospheric pressure. In this method, lower alcohol vapor is decomposed by VUV light, and the action of radical species generated causes the following: a) Removal of the initial contamination layer using VUV light; b) The effect of partial reduction of inorganic oxides and the formation of alkyl chains terminated with carboxy or hydroxyl groups; After that, when the hydrophilic functional groups at the ends come into contact with each other at room temperature, they form hydrogen bonds, and then they are heated at a low temperature of up to about 150°C to undergo dehydration condensation, resulting in the bond.
[0021] The crosslinks obtained by this method, as in the present embodiment described below, are multidentately coordinated with the cations of the parent material at the inorganic material side base of the alkyl chain, and can maintain a dynamic equilibrium state of the hydrolysis reaction, which is a cause of deterioration when moisture reaches the interface due to moisture absorption of the organic material, and exhibit water resistance. As an experimental example, it was confirmed that a joint between aluminum and polyimide maintained a strong bond even after six months of holding test at 85°C and 85% RH.
[0022] Afterwards, in the process of forming bonded bodies of various combinations using the V-VUV method, it was found that while the above-mentioned bridge formation itself is basically not selective about the target materials, there were cases where bonding was difficult depending on the combination of materials. When bonding glass or quartz substrates together, the surfaces with the bridged layer formed by the V-VUV method became charged, and electrostatic repulsion prevented full contact between the samples (approaching to the level of atomic distance between the surfaces), resulting in occasional instances where sufficient bonding strength could not be obtained. To solve this problem, 1) To make the surface on which the cross-links are formed electrically neutral 2) In order to enhance the bonding ability at the site of physical contact at room temperature, a functional group that has a higher hydrogen supplying ability (easier to form hydrogen bonds) than CH is formed at the end of the alkyl chain. These are the main technical requirements of this application. In addition, the lamination process of semiconductor wafer processing requires simultaneous bonding of the conductive copper circuit and the insulating part, so bonding that makes the surface electrically neutral is required so that it is not affected by polarity. Furthermore, a process that is not affected by polarity is also necessary for bonding glass interposers and Si wafers, which will likely become mainstream in the future.
[0023] Secondary technology requirements include: a) The crosslinking ends must have functional groups that bond with the opposing material, but the entire surface must maintain hydrophobicity (pseudo hydrophobicity), reducing the adsorption of contaminants when transporting the surface-modified sample to bonding or other processes. b) Considering that the bonded body obtained by this method is likely to be used in the living environment of the human body, such as in a flexible sensor device, the entire surface modification and bonding process has a low biological and environmental load. Hereinafter, an embodiment of the present invention that satisfies the above technical requirements will be described.
[0024] First Embodiment 1 to 5 are schematic diagrams illustrating a process for bonding a first base material and a second base material according to the first embodiment of the present invention. The process for bonding a first base material and a second base material according to this embodiment will be described with reference to these drawings. (Joining process 1-1. Preparation of first and second substrates) As shown in FIG. 1, a first substrate 2 and a second substrate 3 are prepared.
[0025] (Bonding process 1-2. Formation of precursor layer by ultraviolet light) Next, as shown in FIG. 2, the first ultraviolet ray 5 is irradiated to either or both of the bonding surface 21 of the first substrate 2 and the bonding surface 31 of the second substrate 3 in an environment in which a certain concentration of methylglycine 4 is present. In this embodiment, the first ultraviolet ray 5 is irradiated to both of the bonding surface 21 of the first substrate 2 and the bonding surface 31 of the second substrate 3 in an environment in which a certain concentration of methylglycine 4 is present. As shown in FIG. 3, a precursor layer 22 of the first substrate 2 and a precursor layer 32 of the second substrate 3 are formed by the irradiation of the first ultraviolet ray 5. The formed precursor layers 22 and 32 have a thickness of, for example, 10 nm or less. The atmosphere in which the first ultraviolet ray 5 is irradiated in the presence of a certain concentration of methylglycine 4 may be the air or an atmosphere filled with an inert gas such as nitrogen or argon.
[0026] (Joining process 1-3. Joining of first base material and second base material) The first substrate 2 on which the precursor layer 22 is formed and the second substrate 3 on which the precursor layer 32 is formed are brought into contact with each other so that the precursor layers 22 and 32 face each other as shown in FIG. 4. As shown in FIG. 5, the precursor layers 22 and 32 come into contact with each other to form a cross-linked layer 41, and the first substrate 2 and the second substrate 3 are bonded by the cross-linked layer 41. Thus, a laminate 1 can be obtained in which the first substrate 2, the cross-linked layer 41, and the second substrate 3 are laminated in this order. During the bonding process, the laminate 1 may be heated. By heating, water molecules can be removed and the bonding strength can be further improved. The heating temperature may be, for example, 150° C. or less.
[0027] (Process environment) The formation of the precursor layers 22, 32 and the bonding of the first substrate 2 and the second substrate 3 are performed in an environment in which the oxygen concentration and the moisture concentration are controlled. The oxygen concentration and the moisture concentration may be controlled in a vacuum or a nitrogen atmosphere. Alternatively, other inert gases may be selected instead of nitrogen. Examples of the inert gas that may be selected include nitrogen, helium, neon, argon, and mixtures thereof.
[0028] (First substrate, second substrate) In this embodiment, the first substrate and / or the second substrate may be a laminate of any of copper foil, glass, semiconductor, polymer film, Si wafer, SiC, or any of these with circuits formed on the surface thereof, or any combination thereof. Note that the semiconductor here includes, for example, gallium nitride, gallium arsenide, etc., which can be used in integrated circuits, solar cells, etc.
[0029] Alternatively, the first substrate and / or the second substrate may be any of the following polymer films or a laminate of a combination of polymer films: LCP (liquid crystal polymer), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), PTFE (polytetrafluoroethylene), COP (cycloolefin polymer), PPS (polyphenylene sulfide), PEEK (polyether ether ketone), PI-based (including PI (polyimide) and MPI (modified polyimide)), PPE-based (including PPE (polyphenylene ether) and mPPE (modified polyphenylene ether)). These materials may be selected based on the desired high-frequency circuit characteristics, gas permeability characteristics, moisture-proof characteristics, and the like.
[0030] (Crosslinked substance) In this embodiment, the cross-linking substance present at the time of ultraviolet irradiation includes a certain concentration of methylglycine. The state of the cross-linking substance at the time of ultraviolet irradiation may be gaseous, mist (droplets), or a mixture thereof.
[0031] (UV rays) The first ultraviolet ray 5 irradiated in the presence of a certain concentration of a crosslinking substance may have a dominant wavelength of any one of 126 nm, 146 nm, 156 nm, 172 nm, 185 nm, 206 nm, 222 nm, 254 nm, 283 nm, and 308 nm. As a source of ultraviolet ray having these wavelengths, a source having a desired wavelength, such as a low pressure mercury lamp, a high pressure mercury lamp, an excimer lamp, or a deep ultraviolet LED, can be appropriately selected.
[0032] (Precursor layer and crosslinked layer) Methylglycine supplied during the formation of the precursor layer has the structure shown in Chemical Formula 1 below. In the presence of a certain concentration of methylglycine, a precursor layer 22 formed on a first base material 2 having metal atoms by irradiation with a first ultraviolet ray 5 has a structure of a metal carboxylate compound formed by bonding a carboxylate with a metal atom, for example, as shown in Chemical Formula 2 below. In Chemical Formula 2, the dashed line RR represents the vicinity of the metal surface. Here, M represents a metal atom.
[0033] [ka]
[0034] [ka]
[0035] Here, in the area indicated by the dashed line H1, i.e., in the vicinity of the surface of the cross-linked layer, H3N + AEON and COO - ions are present. This part contributes to bonding with the opposing material, and amphoteric ions are generated predominantly in a neutral environment, + in a basic environment, and - in an acidic environment, making it possible to balance with the surrounding environment, so that electrical neutrality is maintained on the surface of the crosslinked layer. Here, the C1 part is an alkyl chain (hydrophobic) region, which keeps the entire crosslink pseudo-hydrophobic. The M1 region is a region on the base material surface, and the atom is shown by the symbol M as a schematic, but in reality, it represents the coordination by the base material cation, and the actual coordination number is not limited to this and varies depending on the base material.
[0036] For example, when the second base material 3 is polyimide, the precursor layer 32 of the second base material 3 has a structure containing a crosslinkable polymer as shown in the following [Chemical formula 3]. In the figure, the dashed line RR represents the vicinity of the surface of the second base material 3. The end of A in the figure represents -C(=O)-OH or -CH3.
[0037] [ka]
[0038] As shown in [Chemical formula 2] and [Chemical formula 3], most of the ends of the alkyl chain bridge are -C(=O)-OH or -CH3. As shown in the following [Chemical formula 4] (A-1), when one end D and the other end E approach each other, H2O is released and the two ends are bonded through an O atom (B-1). Also, as shown in (A-2), in the case of a CH3 group, it bonds with an OH group coming from the other side, H2O is released in the same way, and the two ends are bonded through an O atom (B-1). The dashed lines in the formula represent hydrogen bonds. The bonds by oxygen O in formula (B-1) can be hydrolyzed, but they are reversible because they are decomposed into -C(=O)-OH or -CH3. Therefore, even if decomposition occurs, recombination occurs at the same time, and the mutual bonds are maintained.
[0039] [ka]
[0040] As described above, in the method for bonding the first and second substrates in this embodiment, ultraviolet light is irradiated in an environment where a certain concentration of a crosslinking substance made of methylglycine is present, forming a precursor layer. By abutting these precursor layers, a crosslinked layer is formed, and the first and second substrates are bonded through this crosslinked layer, so that a bonding method for firmly bonding the first and second substrates at low temperatures can be provided. The second substrate can be selected from any of polymer films or laminates of combinations of any of polymer films, such as LCP (liquid crystal polymer), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), PTFE (polytetrafluoroethylene), COP (cycloolefin polymer), PPS (polyphenylene sulfide), PEEK (polyether ether ketone), PI-based (including PI (polyimide) and MPI (modified polyimide)), and PPE-based (including PPE (polyphenylene ether) and mPPE (modified polyphenylene ether)), so that one that can be used in high-frequency circuits can be appropriately selected. Since the crosslinking substance made of methylglycine has the property of being electrically neutral, it can be well bonded to the polymer film even if the first substrate is copper foil, glass, a semiconductor, etc. Therefore, it is possible to provide a method for bonding substrates that can be used in high-frequency circuits, which firmly bonds the first substrate and the second substrate at low temperature.
[0041] In this embodiment, the precursor layer is formed by irradiating the first ultraviolet light in a state where a certain concentration of methylglycine is present, but the substance present when irradiating the first ultraviolet light is not limited to methylglycine, and may be an amino acid having a zwitterion, that is, a structure having both an amino group and a carboxy group. For example, glutamic acid may be considered as a candidate. The same applies to the following embodiments.
[0042] <Second embodiment> Next, a second embodiment of the present invention will be described. The second embodiment differs from the first embodiment in that, before forming the precursor layer 22 of the first base material 2 and the precursor layer 32 of the second base material 3 as shown in Fig. 2 and Fig. 3, the bonding surface 21 of the first base material 2 and the bonding surface 31 of the second base material 3 are irradiated with the second ultraviolet light 8 as shown in Fig. 6. In this embodiment, the bonding surface 21 of the first base material 2 and the bonding surface 31 of the second base material 3 are both irradiated with the second ultraviolet light 8. The other steps are the same as those of the first embodiment. By adding this step to the first embodiment, in addition to the effects of the first embodiment, the surface state is improved by removing moisture and impurities from the bonding surface 21 of the base material 2 and the bonding surface 31 of the second base material 3 before the formation of the precursor layers 22 and 32, and the bonding between the first base material 2 and the precursor layer 22 and between the second base material 3 and the precursor layer 32, and the film quality of the precursor layers 22 and 32 is improved, and as a result, the bonding strength between the first base material 2 and the second base material 3 can be improved. The second ultraviolet ray 8 may have a dominant wavelength of 156 nm, 172 nm, 185 nm, 206 nm, 222 nm, 254 nm, 283 nm, or 308 nm. As an ultraviolet ray source including these wavelengths, a source having a desired wavelength, such as a low-pressure mercury lamp, a high-pressure mercury lamp, an excimer lamp, or a deep ultraviolet LED, can be appropriately selected.
[0043] In the above-mentioned embodiments, the first base material 2 and the second base material 3 are expressed as a single plate-like body in order to explain the principle of the bonding process, but in reality, as will be explained in the following embodiments, the base material 2 such as copper foil and the second base material 3 can both be wound in a roll and supplied. The base material 2 such as copper foil may be supplied with a thickness of 10 μm to 50 μm. The second base material 3 may be supplied with a thickness of 5 μm to 100 μm.
[0044] <Third embodiment> 7 is a schematic plan view of a bonding device 100 according to a sixth embodiment of the present invention. In this embodiment, the first substrate corresponds to a roll-shaped copper foil film 2a, and the second substrate corresponds to a roll-shaped supporting substrate film 3a. The bonding apparatus 100 includes a chamber 101 whose air pressure can be freely controlled, an inert gas supply source 102 that supplies an inert gas to the chamber 101, and ultraviolet ray irradiation mechanisms 103a and 103b, cross-linking material spray mechanisms 104a and 104b, and a roll-to-roll bonding mechanism 105, which are arranged in the chamber 101. The roll-to-roll bonding mechanism 105 includes unwinding and winding rollers 106a, 106b, 106c, and 106d, forward encoders 107a and 107b, reverse encoders 108a and 108b, forward tension controllers 109a and 109b, reverse tension controllers 110a and 110b, cooling rollers 111a and 111b, press rollers 112a and 112b, guide rollers 113a-113f, and a cutting mechanism 114. In the figure, M represents a driving source, and an electric motor is used as the driving source. The inert gas supply source 102 communicates with the chamber 101 through an inert gas supply pipe 102a having an automatic control valve. The air pressure control source 115 communicates with the chamber 101 through an air pressure control pipe 115a. The air pressure control source 115 is composed of, for example, a vacuum pump, an exhaust valve, etc., and freely controls the air pressure inside the chamber 101.
[0045] The roll-shaped copper foil film 2a and the roll-shaped supporting substrate film 3a are wound around the unwinding / winding rollers 106a, 106b, 106c, and 106d, and by controlling the rotation of the rollers, the rolls are unwound and wound in the forward direction indicated by the arrow S or the reverse direction indicated by the arrow G. The cross-linking substance spraying mechanisms 104a and 104b spray the cross-linking substance 4 toward the roll-shaped copper foil film 2a and the roll-shaped supporting substrate film 3a. Here, the cross-linking substance 4 contains a certain concentration of methylglycine as described in the first embodiment. The ultraviolet ray irradiation mechanisms 103a and 103b irradiate ultraviolet rays from an ultraviolet ray irradiation source toward the roll-shaped copper foil film 2a and the roll-shaped supporting substrate film 3a. The ultraviolet ray used here is the same as the first ultraviolet ray described in the first embodiment, and a low-pressure mercury lamp or the like is used as the ultraviolet ray irradiation source.
[0046] The forward rotation encoders 107a, 107b and the reverse rotation encoders 108a, 108b monitor the forward and reverse conveying speeds of the rolled copper foil film 2a and the rolled supporting substrate film 3a, respectively. The rotation speeds of the unwinding / winding rollers 106a, 106b, 106c, 106d are controlled based on the monitored conveying speeds so that the conveying speeds become predetermined values. The forward rotation tension controllers 109a, 109b and the reverse tension controllers 110a, 110b control the tensions of the rolled copper foil film 2a and the rolled supporting substrate film 3a to appropriate values during forward and reverse rotations of the rolled copper foil film 2a and the rolled supporting substrate film 3a, respectively.
[0047] The cooling rollers 111a and 111b are disposed between the ultraviolet irradiation mechanisms 103a and 103b, respectively, and cool the copper foil film 2a and the supporting base film 3a whose temperatures have risen due to ultraviolet irradiation. The press rollers 112a and 112b are rollers that bring the copper foil film 2a and the supporting base film 3a into contact with each other, and the press roller 112b moves to the position shown by the dashed line to bring the copper foil film 2a into contact with the supporting base film 3a, thereby bonding the copper foil film 2a and the supporting base film 3a together. The cutting mechanism 114 cuts the copper foil film 2a when the bonding device 100 starts the bonding operation (when the press roller 112b moves to the position shown by the dashed line).
[0048] The operation of the bonding device 100 configured as above will be described. With the copper foil film 2a and the supporting base film 3a set as shown in FIG. 7, the air pressure inside the chamber 101 is first adjusted to a desired pressure by the air pressure control source 115. Next, an inert gas is supplied from the inert gas supply source 115 and controlled simultaneously with the air pressure control source to adjust the inside of the chamber 101 to a desired state. The desired state includes a state in which the desired oxygen concentration and moisture concentration are achieved. After the environment inside the chamber 101 is prepared, the unwinding / winding rollers 106a, 106b, 106c, and 106d transport the copper foil film 2a and the supporting base film 3a in the forward direction (the direction of the arrow S).
[0049] The copper foil film 2a and the supporting substrate film 3a unwound by the unwinding / winding rollers 106a and 106b have their surfaces sprayed with methylglycine 4 by the crosslinking substance spraying mechanisms 104a and 104b. Next, the surfaces are irradiated with ultraviolet light by the ultraviolet light irradiation mechanisms 103a and 103b in an environment where a certain concentration of methylglycine 4 is present. The copper foil film 2a and the supporting substrate film 3a, whose temperatures have been raised by the ultraviolet light irradiation, are cooled by the cooling rollers 111a and 111b. By this ultraviolet light irradiation, the precursor layer described in the above embodiment is formed on the surfaces of the copper foil film 2a and the supporting substrate film 3a.
[0050] When the copper foil film 2a and the supporting base film 3a on which the precursor layer has been formed are transported to the press rollers 112a and 112b, the press roller 112b moves to the position indicated by the dashed line, and the copper foil film 2a and the supporting base film 3a are brought into contact with each other and joined by the press rollers 112a and 112b. At that time, the cutting mechanism 114 cuts the copper foil film 2a. The joined laminate of the copper foil film 2a and the supporting base film 3a is taken up by the unwinding / winding roller 106c, and the joining is performed continuously to produce a laminate. The press rollers 112a and 112b each have a built-in heater, and may be heated to an appropriate temperature based on the desired characteristics and joining strength of the laminate to be produced.
[0051] As described above, in the bonding apparatus 100 of the present embodiment, spraying of methylglycine as a cross-linking substance, irradiation of ultraviolet rays, and bonding of the copper foil film 2a and the supporting substrate 3a are continuously performed in a roll-to-roll manner in the chamber 101 where the air pressure, moisture concentration, etc. are adjusted, so that a laminate that can be used in a high-frequency circuit and has a guaranteed bonding strength can be efficiently produced. Therefore, a bonding apparatus that firmly bonds the copper foil film and the supporting substrate film at a low temperature can be provided. In this embodiment, the copper foil film 2a is cut by the cutting mechanism 114, but the present invention is not limited to this, and it is also possible to replace the copper foil film 2a and the supporting substrate 3a in FIG. 7. EXAMPLES
[0052] Examples of the present invention are shown below, but the contents of the present invention should not be construed as being limited to these examples.
[0053] In order to make the surface on which a crosslinked layer of several nm thick is formed electrically neutral and hydrophobic, and the formation process is non-toxic, the present invention proposes a "vacuum ultraviolet light irradiation method (MG-VUV) in a nitrogen atmosphere containing methylglycine (MG) aqueous solution vapor." In the MG-VUV method, an L-methylglycine aqueous solution, which is an amino acid derivative and has low toxicity to humans, is used. The process of the MG-VUV method has been described above in the embodiment (outlined in FIG. 8). Due to the action of radical species generated by decomposition of MG molecules by VUV, an alkyl chain ultrathin crosslink is formed on the base of a multidentate carboxylate salt, which has an amine at the end in addition to conventional hydrophilic functional groups. Glycine ions are zwitterionic (amphoteric) and can achieve electrical neutralization, and NH has a higher hydrogen donating ability than conventional CH. In addition, a structure similar to methanol can be generated by decomposition of MG molecules, but this is also decomposed by VUV and contributes to alkyl chain elongation by the mechanism described in the embodiment. In other words, the crosslink formation process proceeds, including the reaction product.
[0054] The same type of alkali-free glass sample (20 x 20 mm 2 ) are shown in Fig. 9, which shows top optical microscope images of samples bonded by the V-VUV method (ethanol vapor, surface charging) of the aforementioned Patent Document 1 and the MG-VUV method of the present invention (methylglycine vapor, electrically neutral) and the results of shear tests. In both cases, the bonding process conditions other than the type of vapor introduced are the same as follows: 1) Introduce solution vapor into high-purity nitrogen so that the relative humidity is about 20% (approximately 27°C). 2) Place the sample in the atmosphere of 1 and irradiate it with VUV. The light source wavelength is 172 nm, and the distance between the light source and the sample is 70 mm. 3) After contacting the samples at room temperature, apply a load of 400N (1MPa converted into sample area). 4) Immediately after applying the load, heat to 150℃ and hold for 10 minutes 5) Immediately after heating, remove the load and allow the temperature to drop to room temperature. Preliminary X-ray photoelectron spectroscopy measurements have confirmed that a cross-linked layer of approximately 10 nm thickness is formed in both the V-VUV method of the above patent and the MG-VUV method of the present invention, thus eliminating the possibility of bonding failure due to insufficient cross-link formation.
[0055] In the optical microscope images of the joints, the samples bonded by the V-VUV method clearly showed more optical interference fringes than the joints obtained by the MG-VUV method. Optical interference fringes are caused by a gap or intermediate layer between the material surfaces that is equivalent to the wavelength of the incident light (in this case, the halogen lamp light of the optical microscope), and therefore indicate that the front surface of the samples did not achieve closeness (contact) comparable to the interatomic distance. The shear test strength was also clearly greater for the samples obtained by the MG-VUV method, suggesting that the formation of an electrically neutral bridge surface and the suppression of electrical repulsion contribute to the jointability.
[0056] With regard to the above description of the specification, the claims encompass many modifications to the embodiments without departing from the technical idea of the present invention. Therefore, the embodiments disclosed in this specification are presented for illustrative purposes and should not be considered as limiting the scope of the present invention. [Explanation of symbols]
[0057] 1, 10 Laminate 2. First Substrate 21 Bonding surface of first base material 22 Precursor layer of first substrate 3 Second substrate 31 Bonding surface of second substrate 32 Precursor layer of second substrate 4. Methylglycine 41 Crosslinked layer 5. The First Ultraviolet Rays 7. Copper Thin Film 71 Precursor layer for thin copper film 8. The second ultraviolet ray 100 Joining equipment 101 Chamber 102 Inert gas supply source 103a, 103b Ultraviolet irradiation mechanism 104a, 104b Crosslinked substance spraying mechanism 105 Roll-to-roll bonding mechanism
Claims
1. 1. A method for bonding a first substrate and a second substrate, comprising: irradiating a first ultraviolet ray to one or both of the bonding surface of the first base material and the bonding surface of the second base material in a state in which methylglycine is present at a certain concentration, thereby forming a precursor layer; bringing the first base material and the second base material into contact with each other to bond the first base material and the second base material together via the precursor layer; A method for bonding substrates comprising the steps of:
2. irradiating one or both of a bonding surface of the first base material and a bonding surface of the second base material with a second ultraviolet ray before forming the precursor layer; The method of claim 1 , comprising:
3. The method for bonding substrates according to claim 1 or 2, wherein the forming of the precursor layer and the bonding are performed in an environment in which oxygen concentration and moisture concentration are controlled.
4. The method for bonding substrates according to claim 3 , wherein the oxygen concentration and the moisture concentration are controlled in a vacuum or an inert gas atmosphere.
5. 3. The method for joining substrates according to claim 1 or 2, wherein the first substrate and / or the second substrate is a laminate of any one of copper foil, glass, a semiconductor, a polymer film, a Si wafer, SiC, or any one of these substrates having a circuit formed on a surface thereof, or a combination thereof.
6. 3. The method for bonding substrates according to claim 1 or 2, wherein the first substrate and / or the second substrate is a polymer film selected from the group consisting of liquid crystal polymer, tetrafluoroethylene-perfluoroalkylvinylether copolymer, polytetrafluoroethylene, cycloolefin polymer, polyphenylene sulfide, polyetheretherketone, polyimide, polyimide-based films including modified polyimide, polyphenylene ether, and polyphenylene ether-based films including modified polyphenylene ether, or a laminate of a combination of any of the polymer films.
7. The method for bonding substrates according to claim 1 or 2, wherein the first ultraviolet light and the second ultraviolet light have a dominant wavelength of any one of 126 nm, 146 nm, 156 nm, 172 nm, 185 nm, 206 nm, 222 nm, 254 nm, 283 nm, and 308 nm, or any combination thereof.
8. A chamber capable of freely controlling air pressure; an inert gas source for supplying an inert gas to the chamber; disposed within the chamber; An ultraviolet irradiation mechanism; and a methylglycine spray mechanism.
9. A laminate comprising a first substrate, a cross-linked layer of methylglycine, and a second substrate, laminated in this order.
Citation Information
Patent Citations
Adhesive composition
JP2008150550A
Manufacturing method of laminate, laminate, and heated toilet seat device
JP7018223B2