Multilayer electronic component

The core-double shell structure in dielectric crystal grains of multilayer ceramic capacitors addresses insulation resistance issues by preventing oxygen vacancy movement, enhancing high-temperature life and TCC performance for 5G applications.

JP2024149333APending Publication Date: 2024-10-18SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023129263
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-07
Filing Date
2023-08-08
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Multilayer ceramic capacitors face challenges with insulation resistance deterioration due to oxygen vacancies generated during firing in a reducing atmosphere, and they struggle to meet the demanding conditions of high-frequency applications like 5G technology.

Method used

The use of dielectric crystal grains with a core-double shell structure, where the first shell has a higher molar ratio of Sn to Ti and the second shell has a higher molar ratio of rare earth elements to Ti, acts as a barrier to prevent oxygen vacancy movement and enhance high-temperature life characteristics.

Benefits of technology

The core-double shell structure improves high-temperature life characteristics and temperature coefficient of capacitance (TCC) performance, ensuring stability under harsh conditions and meeting X6S standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149333000001_ABST
    Figure 2024149333000001_ABST
Patent Text Reader

Abstract

To provide a multilayer electronic component that has improved high temperature life characteristics, meets X6S temperature characteristics, and has excellent room temperature dielectric constant.SOLUTION: A multilayer electronic component includes a body including a dielectric layer including a plurality of dielectric crystal grains and an internal electrode alternately arranged with the dielectric layer, and an external electrode arranged on the body and connected to the internal electrode. At least one of the plurality of dielectric crystal grains includes Ba, Ti, Sn, and a rare earth element (RE), and has a core-double shell structure. For example, the core-double shell structure includes a core C, a first shell SH1 arranged on at least a part of the core, and a second shell SH2 arranged on at least a part of the first shell, and when the average molar ratios of Sn to Ti included in the first shell and the second shell are S1 and S2, respectively, and the average molar ratios of the rare earth element to Ti included in the first shell and the second shell are R1 and R2, respectively, S1>S2 and R2>R1 are satisfied.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer electronic component. [Background technology]

[0002] Multi-layered ceramic capacitors (MLCCs), which are one type of multi-layered electronic component, are chip-type capacitors that are mounted on printed circuit boards of various electronic products such as visual devices such as liquid crystal displays (LCDs) and plasma display panels (PDPs), computers, smartphones, and mobile phones, and serve to charge and discharge electricity.

[0003] Such multilayer ceramic capacitors have the advantages of being small yet high capacitance and easy to mount, and can be used as components of various electronic devices. As various electronic devices such as computers and mobile devices become smaller and have higher output, there is an increasing demand for multilayer ceramic capacitors to be smaller and have higher capacitance.

[0004] Generally, the body of a multilayer ceramic capacitor is made up of dielectric layers containing BaTiO3 as a main component and internal electrodes containing conductive metals that are alternately laminated together. Such a body must be fired in a reducing atmosphere, and the material forming the dielectric layers must be resistant to reduction.

[0005] However, due to the inherent characteristics of oxides, oxygen may be released from the oxide during firing in a reducing atmosphere, generating oxygen vacancies and electrons. The movement of the oxygen vacancies may cause a problem in that the insulation resistance of the multilayer ceramic capacitor may deteriorate.

[0006] To solve this problem, it is possible to suppress the generation of oxygen vacancies by adding rare earth elements to the dielectric layer. However, with the recent development of 5G (Fifth-generation) mobile communication technology that uses high frequency bands, there is a need for research into multilayer ceramic capacitors with excellent high-temperature life characteristics and temperature coefficient of capacitance (TCC). Summary of the Invention [Problem to be solved by the invention]

[0007] One of several objects of the present invention is to provide a multilayer electronic component having improved high temperature life characteristics.

[0008] One of several objects of the present invention is to provide a multilayer electronic component that meets X6S temperature characteristics.

[0009] One of several objects of the present invention is to provide a multilayer electronic component having an excellent room temperature dielectric constant.

[0010] However, the scope of the present invention is not limited to the above, and can be more easily understood in the course of describing specific embodiments of the present invention. [Means for solving the problem]

[0011] An embodiment of the present invention provides a multilayer electronic component comprising: a body including a dielectric layer having a plurality of dielectric crystal grains and internal electrodes alternately arranged with the dielectric layers; and an external electrode arranged on the body and connected to the internal electrode, at least one of the plurality of dielectric crystal grains including Ba, Ti, Sn, and a rare earth element, and having a core-double shell structure, the core-double shell structure including a core, a first shell arranged on at least a portion of the core, and a second shell arranged on at least a portion of the first shell, wherein, when average molar ratios of Sn to Ti contained in the first shell and second shell are S1 and S2, respectively, and average molar ratios of the rare earth element to Ti contained in the first shell and second shell are R1 and R2, respectively, S1>S2 and R2>R1 are satisfied.

[0012] According to an embodiment of the present invention, there is provided a multilayer electronic component comprising: a body including a dielectric layer having a plurality of dielectric crystal grains and internal electrodes alternately arranged with the dielectric layer; and an external electrode arranged on the body and connected to the internal electrode, at least one of the plurality of dielectric crystal grains includes Ba, Ti, Sn, and a rare earth element, and has a core-double shell structure, the core-double shell structure including a core, a first shell arranged on at least a portion of the core, and a second shell arranged on at least a portion of the first shell, wherein, when average molar ratios of Sn to Ti contained in the core, first shell, and second shell are respectively Sc, S1, and S2, and average molar ratios of rare earth elements to Ti contained in the core, first shell, and second shell are respectively Rc, R1, and R2, the following relationships are satisfied: S1>S2, S1>Sc, R2>S2, R2>Sc, and R2>Rc. Effect of the Invention

[0013] One of the various effects of the present invention is that it can provide a multilayer electronic component having improved high-temperature life characteristics.

[0014] One of the various effects of the present invention is that it can provide a multilayer electronic component that satisfies the X6S temperature characteristics.

[0015] One of the various effects of the present invention is that it can provide a multilayer electronic component having an excellent room temperature dielectric constant. [Brief description of the drawings]

[0016] [Figure 1] 1 is a perspective view showing a multilayer electronic component according to an embodiment of the present invention; [Diagram 2] 2 is a cross-sectional view that illustrates a cross section taken along line II' in FIG. 1. [Diagram 3] 2 is a cross-sectional view that shows a schematic cross section taken along line II-II' in FIG. 1. [Figure 4] 1 is an exploded perspective view showing a schematic exploded view of a main body of a multilayer electronic component according to an embodiment of the present invention; [Diagram 5] FIG. 3 is an enlarged view of the K1 region in FIG. [Figure 6] 1 shows a schematic diagram of a dielectric grain having a core-double shell structure. [Figure 7] 1 is a schematic diagram showing a molar ratio of Sn to Ti and a molar ratio of rare earth elements to Ti in each region of a dielectric crystal grain having a core-double shell structure. [Figure 8] 1 is a graph showing the results of accelerated life testing (HALT) for experimental examples and comparative examples. [Figure 9] 1 is a graph showing the results of accelerated life testing (HALT) for experimental examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, the embodiments of the present invention will be described with reference to specific embodiments and the accompanying drawings. However, the embodiments of the present invention can be modified into various other forms, and the scope of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those skilled in the art. Therefore, the shape and size of elements in the drawings may be exaggerated for clearer explanation, and elements indicated by the same reference numerals in the drawings are the same elements.

[0018] In order to clearly explain the present invention in the drawings, parts that are not relevant to the explanation are omitted, and the size and thickness of each component shown in the drawings are arbitrarily shown for convenience of explanation, so the present invention is not necessarily limited to those shown in the drawings. Components having the same function within the same concept are described using the same reference numerals. Furthermore, throughout the specification, when a part is said to "include" a certain component, this does not mean that other components are excluded, but that the part may further include other components, unless otherwise specified.

[0019] In the drawings, the first direction can be defined as a thickness T direction, the second direction can be defined as a length L direction, and the third direction can be defined as a width W direction.

[0020] [Multilayer electronic components] FIG. 1 is a perspective view showing a multilayer electronic component according to an embodiment of the present invention, FIG. 2 is a cross-sectional view showing a cross section taken along line I-I' in FIG. 1, FIG. 3 is a cross-sectional view showing a cross section taken along line II-II' in FIG. 1, FIG. 4 is an exploded perspective view showing a main body of a multilayer electronic component according to an embodiment of the present invention, FIG. 5 is an enlarged view of region K1 in FIG. 2, FIG. 6 is a schematic view of dielectric crystal grains having a core-double shell structure, and FIG. 7 is a schematic view showing the molar ratio of Sn to Ti and the molar ratio of rare earth elements to Ti by region of dielectric crystal grains having a core-double shell structure.

[0021] A multilayer electronic component 100 according to one embodiment of the present invention will be described in detail below with reference to Figures 1 to 7. Also, a multilayer ceramic capacitor will be described as an example of a multilayer electronic component, but the present invention is not limited thereto and can be applied to various multilayer electronic components, such as an inductor, a piezoelectric element, a varistor, or a thermistor.

[0022] A multilayer electronic component 100 according to an embodiment of the present invention includes a body 110 including a dielectric layer 111 including a plurality of dielectric crystal grains 10a, 10b, and 10c and internal electrodes 121 and 122 alternately arranged with the dielectric layer, and external electrodes 131 and 132 arranged on the body and connected to the internal electrodes, at least one of the plurality of dielectric crystal grains includes Ba, Ti, Sn, and a rare earth element and has a core-double shell structure, the core-double shell structure includes a core C, a first shell SH1 arranged on at least a portion of the core, and a second shell SH2 arranged on at least a portion of the first shell, where S1 and S2 are average molar ratios of Sn to Ti included in the first and second shells SH1 and SH2, respectively, and R1 and R2 are average molar ratios of the rare earth element to Ti included in the first and second shells SH1 and SH2, respectively, and S1>S2 and R2>R1 may be satisfied.

[0023] Although there is no particular limitation on the specific shape of the body 110, as shown in the drawing, the body 110 may have a hexahedral shape or a shape similar thereto. Due to shrinkage of the ceramic powder contained in the body 110 during the firing process and grinding of the corners, the body 110 may have a substantially hexahedral shape, although it is not a hexahedral shape with perfect straight lines.

[0024] The main body 110 may have first and second surfaces 1, 2 facing in a first direction, third and fourth surfaces 3, 4 connected to the first and second surfaces 1, 2 and facing in the second direction, and fifth and sixth surfaces 5, 6 connected to the first to fourth surfaces 1, 2, 3, 4 and facing in the third direction.

[0025] The body 110 may be formed by alternately stacking dielectric layers 111 and internal electrodes 121, 122. The plurality of dielectric layers 111 forming the body 110 may be in a fired state, and the boundaries between adjacent dielectric layers 111 may be integrated to such an extent that they are difficult to see without using a scanning electron microscope (SEM).

[0026] Referring to FIG. 5, the dielectric layer 111 includes a plurality of dielectric crystal grains 10a, 10b, and 10c, and at least one of the plurality of dielectric crystal grains may be a dielectric crystal grain 10a including Ba, Ti, Sn, and a rare earth element and having a core-shell structure.

[0027] Referring to FIG. 6, the core-dual shell structure may include a core C, a first shell SH1 disposed on at least a portion of the core, and a second shell SH2 disposed on at least a portion of the first shell.

[0028] Multilayer ceramic capacitors, which are one type of multilayer electronic component, can suffer from the problem of deterioration of insulation resistance due to the movement of oxygen vacancies generated during firing. In order to solve this problem, a method of forming a dielectric layer containing dielectric crystal grains having a core-shell structure by adding rare earth elements to a BaTiO3-based main component is considered. The rare earth elements basically form a shell region by substituting the A site or B site of the perovskite structure represented by ABO3, and such a shell region can act as a barrier to block the flow of oxygen vacancies and play a role in preventing leakage current.

[0029] However, with the recent development of 5G mobile communication technology that uses high frequency bands, the environment in which multilayer ceramic capacitors are used is becoming more severe, which has led to the problem that multilayer ceramic capacitors that meet the X6S standard (capacitance change rate within ±22% in the temperature range of -55°C to 105°C) cannot be stably provided using only dielectric crystal grains with a simple core-shell structure.

[0030] On the one hand, in the multilayer electronic component 100 according to an embodiment of the present invention, the dielectric layer 111 includes dielectric crystal grains 10a having a core-double shell structure including a core C, a first shell SH1 disposed on at least a part of the core, and a second shell SH2 disposed on at least a part of the first shell. When the average molar ratios of Sn to Ti contained in the first and second shells SH1 and SH2 are S1 and S2, respectively, and the average molar ratios of rare earth elements to Ti contained in the first and second shells SH1 and SH2 are R1 and R2, respectively, by satisfying S1 > S2 and R2 > R1, a multilayer electronic component excellent in high-temperature life characteristics and satisfying the X6S standard can be provided.

[0031] The core C can play a role in maintaining the dielectric constant and realizing the capacitance of the multilayer electronic component 100. The core C is BaTiO3 or (Ba 1-x Ca x )TiO3 (0 < x < 1) in which Ca, Zr, Sn, etc. are partially solid-solved in BaTiO3, Ba(Ti 1-y Ca y )O3 (0 < y < 1), (Ba 1-x Ca x )(Ti 1-y Zr y )O3 (0 < x < 1, 0 < y < 1), Ba(Ti 1-y Zr y )O3 (0 < y < 1), and (Ba 1-x- Ca x )(Ti 1-y Sn y )O3 (0 < x < 1, 0 < y < 1), and can include one or more of them, but the present invention is not limited thereto.

[0032] The first shell SH1 can contain Sn. Sn is doped into the B site of BaTiO3 and has the effect of increasing the band gap energy at which other rare earth elements diffuse into the interior of the dielectric crystal grains. Therefore, it can serve as a barrier to suppress the diffusion of other rare earth elements into the interior of the dielectric crystal grains. Thereby, the breakdown voltage and high-temperature reliability characteristics of the multilayer electronic component 100 can be improved.

[0033] The second shell SH2 can contain rare earth elements. Here, the rare earth element may be one or more of La, Y, Ac, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, and more preferably one or more of Dy, Tb, Y, Gd, and Ho. The rare earth element contained in the second shell SH2 can play a role in suppressing the generation of oxygen vacancies and reducing the mobility of oxygen vacancies.

[0034] On the other hand, according to an embodiment of the present invention, the average molar ratio S1 of Sn to Ti contained in the first shell SH1 is greater than the average molar ratio S2 of Sn to Ti contained in the second shell SH2, and the average molar ratio R2 of the rare earth element to Ti contained in the second shell SH2 can be greater than the average molar ratio R1 of the rare earth element to Ti contained in the first shell SH1. Here, the molar ratio of the rare earth element to Ti can mean the ratio of the total molar number of the rare earth element to the molar number of Ti, and for example, it can mean the (Dy + Tb + Y + Gd + Ho / Ti) value based on the molar number.

[0035] One or more of the plurality of dielectric crystal grains 10a, 10b, 10c have a robust double shell structure composed of the first shell SH1 and the second shell SH2 with different Sn and rare earth element concentrations, so that the high temperature life characteristics and TCC characteristics can be further improved.

[0036] The ratio of S1 and S2 does not need to be particularly limited. For example, it can satisfy 3 < S1 / S2 ≤ 10. When S1 / S2 is 3 or less, the improvement effect of the high temperature life or the improvement effect of the TCC characteristics may be slight. Also, when S1 / S2 exceeds 10, there may be problems such as a decrease in the room temperature dielectric constant or a decrease in the TCC characteristics.

[0037] The ratio of R1 and R2 does not particularly need to be limited either. For example, it can satisfy 4 < R2 / R1 ≤ 12. When R2 / R1 is 4 or less, the high-temperature life characteristics may deteriorate. When R2 / R1 exceeds 12, there may be a problem that the TCC characteristics deteriorate.

[0038] S1, S2, R1, and R2 can be measured, for example, by performing line analysis through EDS (Energy Disperse X-Ray Spectrometer) installed in a transmission electron microscope (TEM, Transmission Electron Microscope) on the dielectric crystal grains of the dielectric layer 111 located in the central regions in the first and second directions in a cross-section cut from the center in the third direction of the main body 110 in the first and second directions.

[0039] First, as shown in FIG. 7, by performing TEM-EDS line analysis along the major axis passing through the center α of the core-double shell structure, the molar ratios of Sn and rare earth elements (RE) to Ti can be represented in a graph. At this time, the boundary between the first shell SH1 and the core C and the boundary between the first shell SH1 and the second shell SH2 can be defined as the points where the molar ratio of Sn to Ti is 10% of the maximum value Smax of the molar ratio of Sn to Ti contained in the first shell SH1.

[0040] Based on the boundary, the molar ratios of Sn and rare earth elements (RE) to Ti at a plurality of equally spaced points (P4, P5, P6, ...) located in the first shell SH1, for example, at three equally spaced points, are measured, and then averaged to measure S1 and R1. In addition, the molar ratios of Sn and rare earth elements (RE) to Ti at a plurality of equally spaced points (P7, P8, P9, ...) located in the second shell SH2, for example, at three equally spaced points, are measured, and then averaged to measure S2 and R2. In addition, the molar ratios of Sn and rare earth elements (RE) to Ti at a plurality of equally spaced points (P1, P2, P3, ...) located in the core C, for example, at three equally spaced points, are measured, and then averaged to measure the average molar ratio of Sn to Ti (Sc) and the average molar ratio of rare earth elements (RE) to Ti (Rc) contained in the core C. Moreover, if the measurement of such an average value is extended to 10 or more dielectric crystal grains 10a having a core-double shell structure and the average value is measured, a more generalized average molar ratio can be measured.

[0041] Referring to FIG. 7, the molar ratio of Sn to Ti contained in the first shell SH1 may gradually decrease inside the first shell SH1 toward the boundary with the core C and / or the second shell SH2. That is, a Sn concentration peak may exist in the first shell SH1. Since Sn is mainly dissolved in the first shell SH1, there is a possibility that Sn is almost absent in the core C and the second shell SH2, and S2 and Sc may each be 0.1×Smax or less. As a result, the S1 and Sc may satisfy S1>Sc. Furthermore, since there is almost no Sn in the second shell SH2, S2 and R2 may satisfy R2>S2. Similarly, since there is almost no Sn in the core C, R2>Sc may be satisfied.

[0042] The Sn concentration peak in the first shell SH1 can act as a barrier to suppress the rare earth element (RE) from diffusing into the inside of the dielectric crystal grain, so that the rare earth element (RE) is absent or present in only a trace amount in the core C. That is, R2>Rc can be satisfied.

[0043] The core-dual shell structure has the above-mentioned Sn concentration gradient because, as described below, a BaTiO3-based powder pre-doped with Sn is mixed with additives containing rare earth elements to form a ceramic slurry, and the first shell SH1 containing Sn is formed before the second shell SH2 in the process of manufacturing and firing a ceramic green sheet using the ceramic slurry.

[0044] Meanwhile, the dielectric crystal grains 10a having a core-double shell structure may further contain other accessory elements in addition to Sn and rare earth elements.

[0045] For example, the second shell SH2 of the dielectric crystal grain 10a having a core-double shell structure may include a first element. The first element may include at least one of a variable valence acceptor element and a fixed valence acceptor element. Here, the variable valence acceptor may include at least one of Mn, V, Cr, Fe, Ni, Co, Cu, and Zn, and the fixed valence acceptor may include at least one of Mg and Zr. The variable valence acceptor element and the fixed valence acceptor element may serve to reduce the electron concentration, and may serve to lower the firing temperature of the multilayer electronic component and improve the high-temperature withstand voltage characteristics. The content of the first element included in the second shell SH2 may be 0.01 mol to 2.0 mol with respect to 100 mol of Ti included in the second shell SH2, but the present invention is not limited thereto.

[0046] Furthermore, the second shell SH2 of the dielectric crystal grain 10a having a core-double shell structure may contain a second element including at least one of Si and Al. The second element may play a role in lowering the firing temperature of the multilayer electronic component and improving the high-temperature withstand voltage characteristics. The content of the second element contained in the second shell SH2 may be 0.5 mol to 4.0 mol per 100 mol of Ti contained in the second shell SH2, but the present invention is not limited thereto. Meanwhile, it is preferable that the second shell SH2 further contains at least one of Si, Al, Mn, and Mg among the first and second elements.

[0047] 5, the dielectric layer 111 may include dielectric crystal grains 10b having a core-shell structure in addition to the dielectric crystal grains 10a having a core-double shell structure. The dielectric crystal grains 10b having the core-shell structure may include a core 10b1 and a shell 10b2 disposed on at least a portion of the core. The dielectric layer 111 may also include dielectric crystal grains 10c that do not have a separate shell.

[0048] The ratio of the number of dielectric crystal grains 10a having the core-double shell structure among the plurality of dielectric crystal grains 10a, 10b, 10c may be, for example, 50% or more. The ratio of the number of dielectric crystal grains 10a having the core-double shell structure may be measured from an image obtained by scanning a cross section of the dielectric layer 111 with a transmission electron microscope (TEM). When the ratio of the number of dielectric crystal grains 10a having the core-double shell structure is 50% or more, the effect of improving high temperature life and TCC characteristics may be more significant.

[0049] 6, the first shell SH1 may be disposed to cover the entire surface of the core C, and the second shell SH2 may be disposed to cover the entire surface of the first shell SH1. However, the first shell SH1 may not cover a portion of the surface of the core C, and the second shell SH2 may exist in a form in which it does not cover a portion of the surface of the first shell SH1.

[0050] In this case, the first shell SH1 may be arranged to cover 90% or more of the area of ​​the surface of the core C, and the second shell SH2 may be arranged to cover 90% or more of the area of ​​the surface of the first shell SH1. When the first shell SH1 is arranged to cover 90% or more of the area of ​​the core surface, and the second shell SH2 is arranged to cover 90% or more of the area of ​​the surface of the first shell SH1, the effects of improving the high-temperature life and the TCC characteristics according to the present invention may become more pronounced.

[0051] There is no need to particularly limit the lengths of the core C, the first shell SH1, and the second shell SH2, but referring to Fig. 6, when the center of the core-double shell structure in the cross section of the core-double shell structure is defined as α and the point on the surface of the second shell SH2 farthest from the α is defined as β, the length LC of the straight line connecting the α and β, which corresponds to the core C, may be 70 nm to 100 nm. If the length LC of the straight line connecting the α and β, which corresponds to the core C, is less than 70 nm, it may be difficult to achieve the target dielectric characteristics, and if it exceeds 100 nm, there is a risk of degrading the DC-bias characteristics and reliability.

[0052] In addition, the length LS2 of the straight line connecting α and β, which corresponds to the second shell SH2, may be greater than the length LS1 of the straight line connecting the first shell SH1 and the core-dual shell structure may have a more significant effect on improving reliability.

[0053] In one embodiment, the length LS1 of the straight line connecting α and β, which corresponds to the first shell SH1, may be 20 nm or less. If LS1 exceeds 20 nm, the dielectric properties may be degraded. There is no need to particularly limit the lower limit of LS1, and it may exceed 0 nm.

[0054] In one embodiment, the length LS2 of the straight line connecting α and β, which corresponds to the second shell SH2, may be 25 nm or more and 50 nm or less. If the LS2 is less than 25 nm, the reliability improvement effect of the present invention may be small. Also, if the LS2 is more than 50 nm, there is a risk that the high temperature life characteristics or the TCC characteristics may be deteriorated.

[0055] The average grain size of the dielectric crystal grains 10a, 10b, and 10c does not need to be particularly limited, but may be, for example, 130 nm to 300 nm. If the average grain size is less than 130 nm, it may be difficult to realize capacitance due to a decrease in dielectric constant, and if it exceeds 300 nm, there is a risk of reliability decreasing due to a decrease in the number of dielectric crystal grains per dielectric layer, and there is a risk of DC-bias characteristics decreasing.

[0056] The average crystal grain size may refer to an average value of the dielectric crystal grain size obtained by, for example, obtaining an image of the dielectric layer 111 arranged in the central region in the first and second directions in a cross section in the first and second directions cut at the center in the third direction of the body 110 by magnifying it 50,000 times with a scanning electron microscope (SEM) and then analyzing the image using an image analysis program, for example, Zootos Program by Zootos Corporation.

[0057] The average thickness td of the dielectric layer 111 is not particularly limited, but may be, for example, 10 μm or less, and more preferably 0.6 μm to 2.0 μm. Generally, the thinner the dielectric layer 111, the lower the reliability, and the properties such as insulation resistance and breakdown resistance may be deteriorated. On the other hand, in the case of the multilayer electronic component according to one embodiment of the present invention, by including the dielectric crystal grains 10a having the above-mentioned core-double shell structure, the reliability of the multilayer electronic component can be ensured even when the average thickness td of the dielectric layer 111 is 0.6 μm to 2.0 μm.

[0058] Here, the average thickness td of the dielectric layer 111 means the size in the first direction of the dielectric layer 111 disposed between the internal electrodes 121 and 122. The average thickness of the dielectric layer 111 may be measured by scanning the cross sections of the body 110 in the first and second directions with a scanning electron microscope (SEM) at a magnification of 10,000. More specifically, the thickness may be measured at a number of points of one dielectric layer 111, for example, 30 points equally spaced in the second direction, and an average value may be measured. The 30 equally spaced points may be designated by a capacitance forming unit Ac, which will be described later. Furthermore, if such an average value measurement is extended to 10 dielectric layers 111 to measure the average value, the average thickness of the dielectric layer 111 may be further generalized.

[0059] The internal electrodes 121, 122 may be alternately arranged with the dielectric layer 111, and for example, a first internal electrode 121 and a second internal electrode 122, which are a pair of electrodes having different polarities, may be arranged to face each other with the dielectric layer 111 interposed therebetween. That is, the first internal electrode 121 and the second internal electrode 122 may be electrically isolated from each other by the dielectric layer 111 arranged therebetween.

[0060] The first internal electrode 121 may be disposed to be spaced apart from the fourth surface 4 and connected to the third surface 3. In addition, the second internal electrode 122 may be disposed to be spaced apart from the third surface 3 and connected to the fourth surface 4.

[0061] The conductive metal contained in the internal electrodes 121, 122 may be one or more of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof, but the present invention is not limited thereto.

[0062] The average thickness te of the internal electrodes 121, 122 does not need to be particularly limited, but may be, for example, 3 μm or less. The average thickness te of the internal electrodes 121, 122 can be set arbitrarily according to the desired characteristics and applications. For example, in the case of electronic components for high-voltage electrical equipment, the average thickness te of the internal electrodes 121, 122 may be less than 1 μm, and in the case of electronic components for small IT devices, the average thickness te of the internal electrodes 121, 122 may be 0.4 μm or less in order to achieve miniaturization and high capacity, but the present invention is not limited thereto.

[0063] The average thickness te of the internal electrodes 121, 122 means the size of the internal electrodes 121, 122 in the first direction. Here, the average thickness of the internal electrodes 121, 122 may be measured by scanning the cross sections of the body 110 in the first and second directions with a scanning electron microscope (SEM) with a magnification of 10,000. More specifically, the thickness may be measured at a number of points of one internal electrode 121, 122, for example, 30 points equally spaced in the second direction, and an average value may be measured. The 30 equally spaced points may be designated by a capacitance forming unit Ac, which will be described later. In addition, if the measurement of such an average value is extended to 10 internal electrodes 121, 122 and the average value is measured, the average thickness of the internal electrodes 121, 122 may be further generalized.

[0064] The body 110 may include a capacitance forming part Ac that is disposed inside the body 110 and includes first and second internal electrodes 121, 122 that are alternately disposed with a dielectric layer 111 therebetween to form a capacitance, and a first cover part 112 and a second cover part 113 that are disposed on both end faces of the capacitance forming part Ac that face each other in a first direction. The cover parts 112, 113 may basically serve to prevent damage to the internal electrodes due to physical or chemical stress. The cover parts 112, 113 may have the same configuration as the dielectric layer 111, except that they do not include internal electrodes.

[0065] The average thickness tc of the cover parts 112, 113 does not need to be particularly limited. However, in order to reduce the size and increase the capacity of the multilayer electronic component, the average thickness tc of the cover parts 112, 113 may be 100 μm or less, 30 μm or less, or 20 μm or less. Here, the average thickness of the cover parts 112, 113 means the average thickness of each of the first cover part 112 and the second cover part 113.

[0066] The average thickness tc of the cover parts 112, 113 may mean the average size of the cover parts 112, 113 in the first direction, and may be the average value of the size in the first direction measured at five equally spaced points on the cross sections of the body 110 in the first and second directions.

[0067] The body 110 may include a first margin portion 114 and a second margin portion 115 disposed on both end surfaces of the capacitance forming portion Ac facing the third direction, respectively. The margin portions 114 and 115 may refer to regions between both ends of the internal electrodes 121 and 122 and the boundary surface of the body 110 in a cross section obtained by cutting the body 110 in the first and third directions.

[0068] The margin portions 114, 115 may include the same material as the dielectric layer 111, except that they do not include the internal electrodes 121, 122. The margin portions 114, 115 may essentially serve to prevent damage to the internal electrodes 121, 122 due to physical or chemical stress.

[0069] The margin portions 114, 115 may be formed by applying a conductive paste for internal electrodes to the ceramic green sheets and firing the sheets, except for the portions where the margin portions are to be formed. Alternatively, in order to suppress steps due to the internal electrodes 121, 122, the internal electrodes 121, 122 after lamination are cut so as to be connected to the fifth and sixth surfaces 5, 6 of the main body, and then a single dielectric layer or two or more dielectric layers are laminated on both end surfaces of the capacitance forming portion Ac that face the third direction, thereby forming the margin portions 114, 115.

[0070] There is no need to particularly limit the average thickness of the margin portions 114, 115. However, in order to reduce the size and increase the capacity of the multilayer electronic component, the average thickness of the margin portions 114, 115 may be 100 μm or less, 30 μm or less, or 20 μm or less. Here, the average thickness of the margin portions 114, 115 means the average thickness of each of the first margin portion 114 and the second margin portion 115.

[0071] The average thickness of the margin portions 114, 115 may mean the average size of the margin portions 114, 115 in the third direction, and may be the average value of the sizes in the third direction measured at five equally spaced points in the cross sections of the body 110 in the first and third directions.

[0072] The external electrodes 131, 132 may be disposed on the third and fourth surfaces 3, 4 of the body 110 and may extend onto parts of the first, second, fifth and sixth surfaces. In addition, the external electrodes 131, 132 may include a first external electrode 131 connected to the first internal electrode 121 and a second external electrode 132 connected to the second internal electrode 122.

[0073] The external electrodes 131, 132 are disposed on the third and fourth surfaces 3, 4 of the body 110 and may include electrode layers 131a, 132a connected to the internal electrodes 121, 122 and plating layers 131b, 132b disposed on the electrode layers. That is, the first external electrode 131 is disposed on the third surface 3 and includes a first electrode layer 131a connected to the first internal electrode 121 and a first plating layer 131b disposed on the first electrode layer, and the second external electrode 132 is disposed on the fourth surface 4 and includes a second electrode layer 132a connected to the second internal electrode 122 and a second plating layer 132b disposed on the second electrode layer.

[0074] The electrode layers 131a and 132a may include a conductive metal and glass. The conductive metal included in the electrode layers 131a and 132a may serve to ensure electrical connectivity with the internal electrodes 121 and 122, and the glass may serve to improve the bonding strength with the body 110.

[0075] The metal included in the electrode layers 131a and 132a may be any conductive material, and a specific material may be determined in consideration of electrical characteristics, structural stability, etc. For example, the conductive metal included in the electrode layers 131a and 132a may be one or more selected from the group consisting of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof, and more preferably may include copper (Cu).

[0076] The electrode layers 131a and 132a may be composed of only one layer including a conductive metal and glass, but the present invention is not limited to this, and the electrode layers 131a and 132a may have a multi-layer structure.

[0077] For example, the electrode layers 131a and 132a may include a first layer that is a fired electrode containing a conductive metal and glass, and a second layer that is disposed on the first layer and contains a conductive metal and a resin. The second layer that contains a conductive metal and a resin may play a role in improving the bending strength of the multilayer electronic component.

[0078] The metal contained in the second layer is not particularly limited, and may include one or more selected from the group consisting of nickel (Ni), copper (Cu), palladium (Pd), silver (Ag), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), and alloys thereof.

[0079] The conductive metal contained in the second layer may include one or more of spherical powder and flaky powder. That is, the conductive metal contained in the second layer may be composed of only flake-shaped powder, may be composed of only spherical powder, or may be in a form in which flake-shaped powder and spherical powder are mixed. Here, the spherical powder may include a form that is not completely spherical, for example, a form in which the length ratio of the major axis to the minor axis (major axis / minor axis) is 1.45 or less. The flake-shaped powder means a powder having a flat and elongated shape, and is not particularly limited, but may be, for example, a length ratio of the major axis to the minor axis (major axis / minor axis) of 1.95 or more. The lengths of the major axis and minor axis of the spherical powder and the flake-shaped powder can be measured from an image obtained by scanning the cross sections in the first and second directions cut at the center of the third direction of the laminated electronic component 100 with a scanning electron microscope (SEM).

[0080] The resin contained in the second layer may play a role of ensuring adhesion and absorbing shock. The resin is not particularly limited as long as it has adhesion and shock absorption properties and can be mixed with the conductive metal powder to form a paste, and may include at least one selected from the group consisting of epoxy resin, acrylic resin, ethyl cellulose, etc.

[0081] In addition, the second layer may include a plurality of metal particles, an intermetallic compound, and a resin. By including the intermetallic compound, electrical connectivity with the first layer may be further improved. The intermetallic compound may function to connect the plurality of metal particles to improve electrical connectivity, and may function to surround the plurality of metal particles to connect them to each other.

[0082] At this time, the intermetallic compound may include a metal having a melting point lower than the curing temperature of the resin. That is, since the intermetallic compound includes a metal having a melting point lower than the curing temperature of the resin, the metal having a melting point lower than the curing temperature of the resin melts during the drying and curing process, and forms an intermetallic compound with a part of the metal particles to surround the metal particles. At this time, the intermetallic compound may include a low melting point metal of preferably 300° C. or less.

[0083] In one embodiment, the second layer may include Sn. During the drying and curing process, Sn melts, and the molten Sn wets high melting point metal particles such as Ag, Ni, or Cu by capillary action, and reacts with some of the Ag, Ni, or Cu metal particles to form intermetallic compounds such as Ag3Sn, Ni3Sn4, Cu6Sn5, and Cu3Sn. Ag, Ni, or Cu that is not involved in the reaction remains in the form of metal particles.

[0084] Thus, the metal particles may include one or more of Ag, Ni, and Cu, and the intermetallic compound may include one or more of Ag3Sn, Ni3Sn4, Cu6Sn5, and Cu3Sn.

[0085] The plating layers 131b and 132b can improve mounting characteristics. The type of the plating layers 131b and 132b is not particularly limited, and may be a plating layer containing nickel (Ni), tin (Sn), palladium (Pd) and / or an alloy containing these, or may be formed of multiple layers. The plating layers 131b and 132b may be, for example, a nickel (Ni) plating layer or a tin (Sn) plating layer, or may be a form in which a nickel (Ni) plating layer and a tin (Sn) plating layer are formed in sequence. The plating layers 131b and 132b may also include multiple nickel (Ni) plating layers and / or multiple tin (Sn) plating layers.

[0086] In the drawings, the multilayer electronic component 100 is shown to have a structure having two external electrodes 131, 132, but this is not limited to this, and the number and shape of the external electrodes 131, 132 can be changed depending on the shape of the internal electrodes 121, 122 or other purposes.

[0087] A method for manufacturing the multilayer electronic component 100 will now be described.

[0088] First, a ceramic powder for forming the dielectric layer 111 is prepared. The ceramic powder may be, for example, BaTiO3 powder. BaTiO3 can generally be synthesized by reacting a titanium raw material such as titanium dioxide with a barium raw material such as barium carbonate. Methods for synthesizing BaTiO3 include, for example, a solid phase method, a sol-gel method, and a hydrothermal synthesis method.

[0089] Next, SnO2 is preferentially added to the synthesized ceramic powder, and then the Sn-doped ceramic powder can be mixed with additives containing rare earth elements, such as oxides containing one or more of La, Y, Ac, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, oxides containing one or more of Mn, V, Cr, Fe, Ni, Co, Cu, and Zn, Mg, and Zr, and / or oxides containing one or more of Al and Sn.

[0090] That is, since BaTiO3 is preferentially doped with Sn, during the grain growth process of the dielectric crystal grains 10a, a first shell SH1 having a high molar ratio of Sn to Ti is formed first on the core C containing a BaTiO3-based main component, and then a second shell SH2 having a high molar ratio of rare earth elements to Ti is formed.

[0091] Next, the prepared ceramic powder may be dried and pulverized, and then mixed with an organic solvent such as ethanol and a binder such as polyvinyl butyral to prepare a ceramic slurry. The ceramic slurry may be coated on a carrier film and dried to provide a ceramic green sheet.

[0092] Next, a conductive paste for internal electrodes containing a conductive metal, a binder, etc. is printed on the ceramic green sheet to a predetermined thickness by a screen printing method, a gravure printing method, etc., to form an internal electrode pattern.

[0093] Then, the ceramic green sheet on which the internal electrode pattern is printed is peeled off from the carrier film and cut, and then a predetermined number of ceramic green sheets on which the internal electrode pattern is printed are stacked so that the internal electrode patterns are alternately exposed at both ends in the second direction of the chip, and the stacked ceramic green sheets are cut to have a predetermined chip size.

[0094] The binder contained in the cut chips may be preferably removed by a debinding process. The conditions of the debinding process may vary depending on the type of binder used, but are not particularly limited. For example, the debinding process may be performed at a temperature of 180° C. to 450° C. for a period of 0.5 hours to 24 hours. The debinding-treated chips may then be fired at a temperature of 1100° C. to 1300° C. to form the body 110 including the dielectric layer 111 and the internal electrodes 121 and 122.

[0095] Next, the third and fourth surfaces 3, 4 of the body 110 where the internal electrodes 121, 122 are exposed may be dipped into a conductive paste for external electrodes containing conductive metal and glass, and then fired to form the electrode layers 131a, 132a. Alternatively, the electrode layers 131a, 132a may be formed by transferring a sheet containing conductive metal and glass. In addition, when the electrode layers 131a, 132a are composed of a first layer which is a fired electrode containing conductive metal and glass, and a second layer which contains conductive metal and resin, the method may further include a process of applying and curing a conductive resin composition containing conductive metal and resin on the first layer.

[0096] There is no need to limit the method for forming the plating layers 131b and 132b in particular, and for example, the plating layers 131b and 132b can be formed by using an electrolytic plating method and / or an electroless plating method.

[0097] (Experimental Example) <Reliability evaluation by sample chip size> 8 and 9 are graphs showing the results of accelerated life testing (HALT) for the experimental examples and the comparative examples.

[0098] First, SnO2 was added to BaTiO3, and then additives including oxides containing Dy, Tb, Y, Gd, and Ho and oxides containing Si, Al, Mn, and Mg were mixed in. Next, the prepared BaTiO3 powder was dried and pulverized, and then an organic solvent such as ethanol and a binder such as polyvinyl butyral were mixed to prepare a ceramic slurry, which was then applied to a carrier film and dried to prepare a ceramic green sheet.

[0099] Next, a conductive paste for internal electrodes containing Ni powder, a binder, etc. was printed on the ceramic green sheets to a predetermined thickness to form internal electrode patterns, and the ceramic green sheets on which the internal electrode patterns were formed were stacked and cut.

[0100] Next, a binder removal process and a firing process are performed to form the main body 110, and then the third and fourth surfaces 3, 4 of the main body 110 are dipped in a conductive paste for external electrodes containing a conductive metal and glass, and then fired to form electrode layers 131a, 132a. Plating layers 131b, 132b in which a Ni plating layer and a Sn plating layer are sequentially stacked on the electrode layers are formed, and a sample chip for an experimental example is prepared.

[0101] At this time, the sample chip of the comparative example was manufactured in the same manner as the sample chip of the experimental example, except that the step of doping BaTiO3 with Sn in advance was not carried out.

[0102] 8 and 9 are graphs showing the results of accelerated life testing (HALT) for the experimental examples and the comparative examples.

[0103] Specifically, in experimental example 1 and comparative example 1 in FIG. 8, sample chips were formed using the above-mentioned method, and the thickness of the dielectric layer after firing was set to 0.6 to 0.9 μm, and the size of the sample chip in the second direction was approximately 0.6 mm and the size in the third direction was approximately 0.3 mm.

[0104] In experimental example 2 and comparative example 2 in Figure 9, sample chips were formed using the method described above, and the thickness of the dielectric layer after firing was set to 1.3 to 2.0 μm. The size of the sample chip in the second direction was approximately 1.0 mm, and the size in the third direction was approximately 0.5 mm.

[0105] The accelerated life evaluation was carried out by measuring the life of 40 samples each of Experimental Example 1, Comparative Example 1, Experimental Example 2, and Comparative Example 2 under conditions of a temperature of 125° C. and 2×Vr (rated voltage).

[0106] Referring to FIGS. 8 and 9, it can be confirmed that Experimental Examples 1 and 2 are superior in reliability compared to Comparative Examples 1 and 2. This is because in the case of Experimental Examples 1 and 2, by pre-doping BaTiO3 with Sn, dielectric crystal grains 10a having a robust double-shell structure composed of a first shell SH1 and a second shell SH2 with different concentrations of Sn and rare earth elements are included.

[0107] <Characteristic Evaluation by S1 / S2 and R2 / R1> Next, the characteristics of the sample chips were evaluated based on the values of S1 / S2 and R2 / R1. That is, the sample chips were manufactured by the above-described method, and the amounts of SnO2 and rare earth oxides doped into BaTiO3 were adjusted. Specifically, for each sample number in Table 1 below, the amount of Sn doped into BaTiO3 was changed between 0.8 mol and 3.0 mol with respect to 100 mol of Ti to adjust the S1 / S2 value, and the rare earth element was changed between 0.8 mol and 2.0 mol with respect to 100 mol of Ti to adjust the R2 / R1 value.

[0108] Thereafter, in the cross-section cut from the center in the third direction of the main body 110 in the first and second directions, for the dielectric crystal grains of the dielectric layer 111 located in the central regions in the first and second directions, after observing with a transmission electron microscope (TEM) under the conditions of an acceleration voltage of 200 kV, an observation magnification of 79,000 times, and a beam diameter of 1.5 nm, line analysis was performed through the EDS installed in the transmission electron microscope. At this time, after measuring the molar ratios of Sn and rare earth elements (RE) to Ti at three equally spaced points located in the first shell SH1 and averaging them respectively to measure S1 and R1, and after measuring the molar ratios of Sn and rare earth elements (RE) to Ti at three equally spaced points located in the second shell SH2 and averaging them respectively to measure S2 and R2, the values of S1 / S2 and R2 / R1 were obtained. Also, the measurement of the above average values was extended to 10 dielectric crystal grains 10a having a core-double shell structure to measure the average values, and the values of S1 / S2 and R2 / R1 were further generalized.

[0109] In Table 1 below, if the S1 / S2 value is 3 or less, it is indicated as "-", if it is more than 3 and 10 or less, it is indicated as "○", and if it is more than 10, it is indicated as "+". If the R2 / R1 value is 4 or less, it is indicated as "-", if it is more than 4 and 12 or less, it is indicated as "○", and if it is more than 12, it is indicated as "+".

[0110] The room temperature capacitance and dissipation factor (DF) were measured by heat treating the sample chip at 150℃ for 2 hours using an LCR meter at 1kHz and AC1.14V / μm. The measured room temperature capacitance and the dielectric constant were calculated using the dielectric constant formula, and the results are shown in Table 1 below.

[0111] The satisfaction of X6S was judged by measuring the TCC at -55°C and the TCC at 125°C, and then indicating whether the TCC at -55°C and 125°C was within the range of ±22% with an "O" and whether it was outside the range of ±22% with an "X".

[0112] The mean time to failure (MTTF) in Table 1 below refers to the average time it takes for the insulation resistance of all sample chips to reach 1 kΩ or less when 400 sample chips for each sample number are subjected to a temperature of 125°C and a voltage twice the rated voltage.

[0113] The satisfaction of the DC effective capacitance was evaluated by applying a DC voltage of 100 kHz, 0.01 V, and maintaining it for 60 seconds. If the capacitance value at a voltage of 1 V was 80% or more of the capacitance when no DC was applied, it was indicated as "○", and if it was less than 80%, it was indicated as "X".

[0114] After that, the four characteristic conditions, 1) room temperature dielectric constant ≧ 3000, 2) whether X6S is satisfied, 3) MTTF ≧ 45, 4) whether DC effective capacitance is satisfied, were all evaluated as excellent (○); two to three were evaluated as average (△); and one or less was evaluated as poor (X). These are shown in Table 1 below.

[0115] [Table 1]

[0116] Referring to Sample Nos. 1-1 to 1-3 in Table 1 above, when S1 / S2 is 3 or less, it can be confirmed that the high-temperature life characteristic (MTTF) decreases or the TCC characteristic (X6S) decreases according to the R2 / R1 value.

[0117] Also, referring to Sample Nos. 3-1 to 3-3, when S1 / S2 exceeds 10, it can be confirmed that the room-temperature dielectric constant and DC effective capacitance decrease and the TCC characteristic decreases.

[0118] On the other hand, for Sample Nos. 2-1 to 2-3, when S1 / S2 exceeds 3 and satisfies 10 or less, it can be confirmed that the room-temperature dielectric constant and DC effective capacitance are good and both the high-temperature life characteristic and the TCC characteristic are improved.

[0119] Referring to Sample Nos. 1-1 to 1-3 and Sample Nos. 3-1 to 3-3, when the S1 / S2 values are similar, it can be confirmed that although the high-temperature life characteristic is improved as the R2 / R1 value increases, the TCC characteristic decreases.

[0120] However, referring to Sample No. 2-2, when both 3 < S1 / S2 ≤ 10 and 4 < R2 / R1 ≤ 12 are satisfied, it can be confirmed that the high-temperature life characteristic is significantly improved while ensuring the room-temperature dielectric constant, DC effective capacitance, and TCC characteristic.

[0121] The present invention is not limited by the above-described embodiments and the accompanying drawings, but is limited by the appended claims. Therefore, various forms of substitution, modification, and change can be made by those having ordinary knowledge in the technical field without departing from the technical idea of the present invention described in the claims, and it can be said that these also belong to the scope of the present invention.

[0122] In addition, the expression "one embodiment" does not mean the same embodiment, but is provided to emphasize and describe each unique feature that is different from the others. However, the one embodiment presented above does not exclude being realized in combination with the features of another embodiment. For example, even if a matter described in a specific embodiment is not described in another embodiment, it can be understood as a description related to the other embodiment, unless there is a description that is opposite or contradictory to the matter in the other embodiment.

[0123] Furthermore, expressions such as "first, second" are used to distinguish one component from another, and do not limit the order and / or importance of the components. In some cases, the first component may be named the second component, and similarly the second component may be named the first component, within the scope of the rights. [Explanation of symbols]

[0124] 100: Multilayer electronic components 110: Main unit 111: Dielectric layer 112, 113: Cover part 114, 115: Margin 121, 122: Internal electrode 131, 132: External electrode 10a, 10b, 10c: Dielectric crystal grains C: Core SH1: First shell SH2: Second shell

Claims

1. a body including a dielectric layer including a plurality of dielectric grains and internal electrodes arranged alternately with the dielectric layer; an outer electrode disposed on the body and connected to the inner electrode; At least one of the plurality of dielectric crystal grains includes Ba, Ti, Sn, and a rare earth element and has a core-double shell structure; the core-dual shell structure includes a core, a first shell disposed on at least a portion of the core, and a second shell disposed on at least a portion of the first shell; When average molar ratios of Sn to Ti contained in the first shell and the second shell are S1 and S2, respectively, and average molar ratios of rare earth elements to Ti contained in the first shell and the second shell are R1 and R2, respectively, A multilayer electronic component, satisfying S1>S2 and R2>R1.

2. 2. The multilayer electronic component according to claim 1, wherein the S1 and the S2 satisfy 3<S1 / S2≦10.

3. 3. The multilayer electronic component according to claim 1, wherein R1 and R2 satisfy 4<R2 / R1≦12.

4. 3. The multilayer electronic component according to claim 2, wherein R1 and R2 satisfy 4<R2 / R1≦12.

5. 3. The multilayer electronic component according to claim 1, wherein the S2 and the R2 satisfy R2>S2.

6. 3. The multilayer electronic component according to claim 1, wherein a molar ratio of Sn to Ti contained in the first shell gradually decreases inside the first shell toward the boundary with the core and / or the second shell.

7. 3. The multilayer electronic component according to claim 1, wherein the rare earth element is at least one of Dy, Tb, Y, Gd, and Ho.

8. The multilayer electronic component according to claim 1 , wherein the second shell further contains at least one of Si, Al, Mn, V, and Mg.

9. In a cross section of the core-double shell structure, the center of the core-double shell structure is defined as α, and the point on the surface of the second shell farthest from the α is defined as β.

3. The multilayer electronic component according to claim 1, wherein the length of the straight line connecting said α and said β, which corresponds to said core, is 70 nm to 100 nm.

10. In a cross section of the core-double shell structure, the center of the core-double shell structure is defined as α, and the point on the surface of the second shell farthest from the α is defined as β; Of the straight line connecting α and β, when the length corresponding to the first shell is LS1 and the length corresponding to the second shell is LS2, The multilayer electronic component according to claim 1 or 2, wherein LS2>LS1 is satisfied.

11. The multilayer electronic component according to claim 10 , wherein the LS1 is greater than 0 nm and less than 20 nm.

12. 11. The multilayer electronic component according to claim 10, wherein the LS2 is 25 nm or more and 50 nm or less.

13. When the average molar ratio of Sn to Ti contained in the core is Sc and the average molar ratio of rare earth element to Ti contained in the core is Rc, 3. The multilayer electronic component according to claim 1, wherein S1>Sc and R2>Rc are satisfied.

14. 3. The multilayer electronic component according to claim 1, wherein at least one of the dielectric layers has an average thickness of 0.6 μm to 2.0 μm.

15. a body including a dielectric layer including a plurality of dielectric grains and internal electrodes arranged alternately with the dielectric layer; an outer electrode disposed on the body and connected to the inner electrode; At least one of the plurality of dielectric crystal grains includes Ba, Ti, Sn, and a rare earth element and has a core-double shell structure; the core-dual shell structure includes a core, a first shell disposed over at least a portion of the core, and a second shell disposed over at least a portion of the first shell; When average molar ratios of Sn to Ti contained in the core, the first shell, and the second shell are respectively Sc, S1, and S2, and average molar ratios of rare earth elements to Ti contained in the core, the first shell, and the second shell are respectively Rc, R1, and R2, A multilayer electronic component that satisfies S1>S2, S1>Sc, R2>S2, R2>Sc, and R2>Rc.

16. 16. The multilayer electronic component according to claim 15, wherein the S1 and the S2 satisfy 3<S1 / S2≦10.

17. 17. The multilayer electronic component according to claim 15, wherein R1 and R2 satisfy 4<R2 / R1≦12.

18. 17. The multilayer electronic component according to claim 16, wherein R1 and R2 satisfy 4<R2 / R1≦12.

19. 17. The multilayer electronic component according to claim 15, wherein a molar ratio of Sn to Ti contained in the first shell gradually decreases inside the first shell toward the boundary with the core and / or the second shell.