Window, door and / or facade structure and method for producing corner joint of window, door and / or facade structure

Laser welding of coated metal profiles with corner connectors addresses the issues of unsightly weld seams and coating damage in conventional methods, providing aesthetically pleasing and functional corner joints with reduced re-coating needs.

JP2024149431APending Publication Date: 2024-10-18SCHUECO INTERNATIONAL KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024060603
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-05
Filing Date
2024-04-04
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Conventional welded corner joints in window, door, and facade structures result in unsightly weld seams and require extensive re-coating due to annealing colors and damage to coatings, complicating the manufacturing process.

Method used

Laser welding of coated metal profiles with precise heat input to form joints that minimize visible damage and allow for coated profiles, using indirect connections via corner connectors to maintain dimensional accuracy and stability.

Benefits of technology

The solution results in visually appealing, dimensionally accurate, and mechanically stable corner joints with minimal protrusion, reducing re-coating efforts and ensuring smooth operation of windows and doors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149431000001_ABST
    Figure 2024149431000001_ABST
Patent Text Reader

Abstract

To provide an attractive welded corner joint with little labor.SOLUTION: Regarding a window, door and / or facade structure comprising a corner joint (50, 60, 70) with two metal profiles (1, 2) connected to each other by one or more welded joints, the welded joint is configured as a laser-welded joint. The welded joint indirectly connects the profiles (1, 2) by means of a corner angle connector (12, 16, 32), particularly preferably the profiles (1, 2) each having profile chambers (8, 9), the corner angle connector (12, 16, 32) having at least two legs which are inserted into the profile chambers (8, 9). This invention relates to a method of producing a corner joint (50, 60, 70) of a window, door, and / or facade structure.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a window, door and / or facade construction having a corner joint and to a method for manufacturing the corner joint. [Background technology]

[0002] Constructions of the aforementioned type having welded corner joints are well known: in most cases, uncoated metallic profiles are joined together using a fuel-based welding process with a filler metal. Metal profiles usually show an annealing color due to the large heat input, which is hidden by the subsequent coating. Coating large frames or doors is significantly more complicated than coating individual profiles.

[0003] Additionally, the aforementioned welding process results in wide, unsightly weld seams that overhang adjacent areas.

[0004] The excess can be removed by grinding, but if there is a coating, this should also be removed completely - in this case a second coating is absolutely essential.

[0005] Lack of sanding will result in corner joints that are visually and tactilely unappealing. Sanding requires that the appropriate coating material be applied over a large area of ​​the corner joint area, significantly increasing the amount of recoating work. Summary of the Invention [Problem to be solved by the invention]

[0006] SUMMARY OF THE PRESENT EMBODIMENT It is therefore an object of the present invention to provide an attractive welded corner joint that requires less labor. [Means for solving the problem]

[0007] The object of the present invention is solved by a window, door and / or facade structure having the features of claim 1 and by a method for manufacturing a corner joint having the features of claim 11.

[0008] The window, door and / or facade structure according to the invention comprises at least two metal profiles, preferably coated metal profiles, with a corner joint which are connected to each other by one or more weld joints, the weld joint being formed as one laser welded joint or, in case of multiple weld joints, as multiple laser welded joints.

[0009] Laser welding allows for dimensional accuracy and precise heat input, making it possible to weld coated metallic profiles with little visible damage to the profile, especially the profile's coating.

[0010] Thus, uncoated metallic profiles such as steel, non-ferrous metals, aluminum and stainless steel can be used as metallic profiles. However, it is also possible, which is particularly advantageous, to use already painted metallic profiles. Any systems such as powders, anodized surfaces and / or wet paint coatings and / or galvanic coatings and / or foils can be used as coating systems.

[0011] Laser welding can be advantageously realized without the use of filler metal, without which no additional material is applied to the material of the metallic profile, and burning of the coating material due to contact with the filler metal is advantageously avoided.

[0012] It is often necessary for windows, doors or facades to maintain a particularly good dimensional accuracy relative to the frame, e.g. the door or window frame. If the weld joint protrudes too much, the closing of the window or door may be hindered. Furthermore, the seal may be compressed particularly strongly locally during closing, with the result that the mechanical stresses on the seal at this point are undesirably increased. This is also avoided by using laser weld joints, which are designed in such a way that they do not protrude or only slightly protrude relative to the neighboring areas.

[0013] The welded joint indirectly connects the profiles to one another by means of corner connectors, the profiles each having a profile chamber and the corner connectors having at least two legs, the legs being inserted into the profile chambers.

[0014] Advantageous embodiments of the invention are the subject matter of the dependent claims.

[0015] The weld joint is configured as a welded joint or surface weld shape with a protrusion of less than 1 mm, preferably less than 0.5 mm, relative to the adjacent areas. The corner joint is therefore tactilely appealing and, due to its good dimensional accuracy, presents few obstructions in relation to the frame or wall opening.

[0016] It is particularly preferred that the weld joint is substantially flat relative to the adjacent areas, ie protrudes less than 0.1 mm.

[0017] The welded joint can be configured as a closed weld seam, or as a row of spot welds, or as a surface weld profile. The average weld diameter of the spot welds and / or the diameter of the weld seam perpendicular to its longitudinal extension is preferably at least 2 mm.

[0018] The linear row of weld seams or spot welds may have a maximum extension of more than 15 mm, preferably more than 20 mm.

[0019] Alternatively, the weld joint may even be formed as a slight recess compared to adjacent areas by locally altering the metal structure. This has the particular advantage that any subsequent coating of the welded area results in a flattening compared to adjacent areas, creating an overall flat surface without any visual or tactile awareness of the welded area.

[0020] Adjacent to the laser welded joint, the painted area may form as a burnt area, which contains the pyrolysis products of the paint of the painted area, beyond which the metallic profile can also be painted, but without the pyrolysis products being quantitatively contained in the paint composition and in the weld pool composition of the laser welded joint.

[0021] The burnt area is advantageously less than 2 mm wide, preferably less than 1 mm wide, away from the laser weld joint. Such small burnt areas are desirable and can be achieved by laser welding, especially when using fiber laser welding equipment.

[0022] In addition to the indirect welded joint, the corner joint has a second welded joint that connects the metal profiles of the corner joint directly to each other.

[0023] The direct connection is a welded joint with a welded area on each of the two profiles.

[0024] The second weld joint is advantageously arranged along the miter joint, at least in some areas, along the visible side of the corner joint, for a particularly stable connection. The visible side has a particularly large contact surface of both metal profiles, which allows a very extensive connection over the entire width of the visible side. It is particularly preferred that the welded joints are arranged along the miter joints of the corner joints, i.e. around the entire outer connection area of ​​the two profiles.

[0025] Advantageously, the second weld joint is disposed perpendicular to the visible side of the corner joint along at least one outer side, which is particularly attractive to end users as it is substantially invisible after installation.

[0026] The welded joints connect the profiles indirectly by means of corner connectors. In particular, the connections can be located along the aforementioned perpendicular outer side to the visible side. The indirect connection by corner connectors can create a wider and therefore more stable connection between the two profiles.

[0027] The weld joint advantageously has a longitudinal weld seam running parallel to the longitudinal axis A of the respective metal profile. Similarly, the surface weld geometry can also have a main direction running parallel to the longitudinal axis A of the respective metal profile. In this case, a particularly large contact surface of the profile wall with the leg of the corner angle connector can be assumed.

[0028] The corner connectors can be configured in such a way that when the corner joint is installed, a pretension is created between the two contact surfaces in the contact area of ​​the metal profiles, as a result of which the profiles are pressed together even more and the ingress of dirt and liquids, e.g. rainwater, is further prevented in the area of ​​the corner joint.

[0029] The longitudinal axes of the legs of the corner angle connector can define a first angle, where an angled inner surface formed from both legs has a recess at a contact area of ​​both legs.

[0030] Alternatively or additionally, the angled inner surface can define a second angle that is less than the first angle. As with the recess, the angled inner surface configuration creates a pretension by clamping the material as the weld joint cools. In this variation, for example, the corner angle connector can be particularly preferably configured as a solid material corner angle connector.

[0031] Alternatively or additionally, the two legs of the corner connector can be configured as spring legs for supporting against the profile wall. This support allows for a large area to be fused during full penetration welding, for example by directing the laser beam at the profile wall from the side opposite to the side on which the spring legs are supported. In particular, the spring legs can be formed via two contact walls, between which a spring web is formed. When pressure is applied to the contact walls, reducing the distance between them, the spring web undergoes a bending deformation and forms a restoring force.

[0032] The weld joint is advantageously arranged in the groove of the profile, preferably along the base of the groove, particularly preferably along the groove of the weatherstrip. The weld joint may have a slightly rough surface. This forms a natural stop during installation and when threading the weatherstrip seam on the sealing strip. For long profiles it is often difficult for the mechanic to find the end of the groove. The weatherstrip is usually cut to the length of the profile at both ends. If the profile has a natural stop, the mechanic knows that he no longer needs to thread the weatherstrip seal through the groove. The welded joint provides a further installation advantage here.

[0033] The weld joint can be configured as a through-hole weld joint such that at least one of the profile walls forms a solidified molten pool throughout the thickness of the profile wall. If corner angle connectors are used, a portion of the corner angle connector also forms part of the molten pool. In this regard, both direct and indirect connection of metal profiles with corner connectors using laser welding can result in a weld joint with a corresponding solidified melt pool throughout the entire thickness of the profile wall.

[0034] The invention also relates to a method for manufacturing a corner joint for a window, door and / or facade structure, which is advantageously a window, door and / or facade structure according to the invention described above.

[0035] In a first step, two metallic profiles, preferably coated metallic profiles, are provided. A particular advantage of using laser welding is that due to the very limited heating, there is no or only slight localized damage to the coating, making repairs easy. Existing laser welding equipment can also be used to rework the coating in the weld area. For example, the laser can melt the coating particles and distribute them in a liquid state in the weld area.

[0036] The method includes the step of inserting respective legs of the corner angle connector into profile chambers of respective metal profiles, such that a respective leg of the corner angle connector is disposed within each of the two metal profiles.

[0037] The particles can originate from an existing coating or from a coating material that is subsequently applied to the weld joint, for example by localized sputtering.

[0038] Positioning two metallic profiles at an angle to each other may for example involve placing two contact surfaces of the two metallic profiles next to each other, at which point a contact area is formed.

[0039] In a further step, the two metal profiles are welded to one another using a laser welding device, in particular a fiber laser welding device, where the welding takes place directly in the contact area of ​​the two metal profiles or outside the contact area, in particular using corner connectors as an aid.

[0040] In order to create a mechanically stable connection, the power of the laser welding device is set in such a way that a penetration weld joint is provided through the profile wall and / or along the penetration welded weld joint at the contact area of ​​the two profile walls.

[0041] The welded joints are applied in such a way that the profiles are indirectly connected to each other by corner angle connectors.

[0042] Advantageous embodiments of the method are the subject matter of the dependent claims.

[0043] The welding can be carried out in particular according to the following advantageous variants:

[0044] This is done by inserting one leg of the corner angle connector into the profile chamber of each metal profile so that one leg of the corner angle connector is located on each of the two metal profiles. In this case, the corner angle connector has the widest possible contact surface with the inside of the profile wall of the profile chamber, so that the heat flow is transferred to the corner angle connector when the profile chamber is heated. This leads to a particularly wide and complete fusion of both components during the welding process.

[0045] Between each metal profile and the corner connector, a through weld joint is formed, preferably with the formation of a pretension. The pretension can be achieved by utilizing the linear expansion during heating and the material shortening as the molten material cools. The configuration of the corner connector can further support the creation of the pretension. The pretension can be formed particularly well with two mitred cut metal profiles.

[0046] The weld joint is preferably made in particular outside the contact area, and is particularly preferably located outside the visible sides of the two metallic profiles.

[0047] However, it is also possible to form a weld joint according to the first variant of welding and, having provided a weld joint in the contact area, additionally produce a weld joint via a corner connector according to the second variant.

[0048] The method according to both variants described above can also include reprocessing, which comprises further laser processing to form a coating by melting the coating components and / or by radiation activated crosslinking of the coating material and / or by evaporating the coating components.

[0049] Rework can also include the application of additional coating material in the area of ​​the weld joint, which can be done in a variety of ways, for example, as a solvent-based coating composition, as a solventless polymeric coating, and / or as a particulate coating composition.

[0050] However, it is also possible to fuse existing coating material from the area adjacent the weld joint to form a closed coating surface.

[0051] Furthermore, the metal profiles are advantageously pre-fixed (pre-fixed) to the respective corner profiles.

[0052] The pre-fixing can be done by drilling holes in the corner connector and the metal profile, or the pre-fixing can be done by deforming and / or punching one or especially both metal profiles in certain areas.

[0053] Mechanical fixing means, for example rods and / or pins and / or screws inserted into holes, can be used for pre-fixation.

[0054] During welding, the pre-fixture is maintained according to step b).

[0055] It is also possible to provide an opening in the metal profile and direct the laser beam through the outer profile chamber to the lower profile wall where the welding is performed. The opening can also be configured as a slot hole for better alignment of the laser beam. Furthermore, the hole can be optionally closed in a post-processing operation after welding, for example by welding. [Brief description of the drawings]

[0056] The invention is explained in more detail with reference to exemplary embodiments in the following figures. The individual details of the exemplary embodiments are not to be considered as limiting the subject matter of the invention. On the contrary, the exemplary embodiments provide the skilled person with numerous other variants that also form part of the invention. [Figure 1] FIG. 1 shows a first perspective view of a corner joint of two profiles of a window, door or facade structure. [Diagram 2] FIG. 2 shows a second perspective view of a corner joint between two profiles of a window, door or facade structure. [Diagram 3] FIG. 2 shows a side view of a first corner connector. [Figure 4] A side view of a second corner connector is shown. [Figure 5a] 1 shows a schematic diagram of multiple welding lines for manufacturing a corner angle connector. [Figure 5b] 1 shows a schematic diagram of multiple welding lines for manufacturing a corner angle connector. [Figure 5c] 1 shows a schematic diagram of multiple welding lines for manufacturing a corner angle connector. [Figure 5d] 1 shows a schematic diagram of multiple welding lines for manufacturing a corner angle connector. [Figure 5e] 1 shows a schematic diagram of multiple welding lines for manufacturing a corner angle connector. [Figure 5f] 1 shows a schematic diagram of multiple welding lines for manufacturing a corner angle connector. [Figure 6]FIG. 2 shows a schematic cross-sectional view of a profile with corner connectors inserted at the start of welding. [Figure 7] FIG. 2 shows a schematic cross-sectional view of a profile with a corner angle connector inserted at the end of a weld. [Figure 8] Shows a cross section through the walls of two profiles to be connected. [Figure 9] FIG. 9 is a cross-sectional view of FIG. 8 after the joint has been formed. [Figure 10] FIG. 10 is a cross-sectional view of FIG. 8 and FIG. 9, showing the state after welding. [Figure 11a] 1 shows perspective and cross-sectional views of all four variants for pre-fixing the profile before welding. [Figure 11b] 1 shows perspective and cross-sectional views of all four variants for pre-fixing the profile before welding. [Figure 11c] 1 shows perspective and cross-sectional views of all four variants for pre-fixing the profile before welding. [Figure 11d] 1 shows perspective and cross-sectional views of all four variants for pre-fixing the profile before welding. [Figure 11e] 1 shows perspective and cross-sectional views of all four variants for pre-fixing the profile before welding. [Figure 11f] 1 shows perspective and cross-sectional views of all four variants for pre-fixing the profile before welding. [Figure 11g] 1 shows perspective and cross-sectional views of all four variants for pre-fixing the profile before welding. [Figure 11h] 1 shows perspective and cross-sectional views of all four variants for pre-fixing the profile before welding. [Figure 12a] FIG. 13 is a diagram showing four modified examples of welding patterns. [Figure 12b] FIG. 13 is a diagram showing four modified examples of welding patterns. [Figure 12c] FIG. 13 is a diagram showing four modified examples of welding patterns. [Figure 12d] FIG. 13 is a diagram showing four modified examples of welding patterns. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0057] The present invention relates to a method for manufacturing a corner joint between two metal profiles of a window, door or facade construction.

[0058] The method is carried out by welding through a profile wall or by a joint between two profile walls. The welding is carried out by a laser welding process. Laser welding is known per se and is described, for example, in EP 0 238 171 A1.

[0059] In contrast to other welding techniques, laser welding is in particular performed without filler metals, which would cause undesirable material strengthening of the weld joint.

[0060] Metal profiles are the starting material for the manufacture of corner joints. These can be, for example, stainless steel profiles or aluminum profiles.

[0061] It is particularly preferred that the metallic profile is coated at least on the outside, however in the region of the contact surfaces the metallic profile is preferably not coated in a manner known per se. Laser welding can be performed in two ways, which are described below. A first variant is described by indirect welding of the profiles 1 and 2 using corner connectors 12, 16 or 32. This variant is illustrated in particular in figures 1 to 7.

[0062] A second variant is achieved by direct welding of the profiles 1 and 2 by means of a material-locking connection of the contact surfaces of both profiles 1 and 2. This is explained in particular with reference to figures 8 to 10.

[0063] Fig. 1 shows a corner joint 50 consisting of a first profile 1 and a second profile 2. Profiles 1 and 2 are profiles of a door, window or facade structure. This therefore relates in particular to both the corner joint of the respective door or window leaf and to the corner joint of the respective door or window frame, which in a conventional configuration have several profile chambers, such as profile chambers 8 and 9.

[0064] The contact surfaces form a contact area 3. However, the contact surfaces do not necessarily have to touch and small distances between the profiles, especially distances less than 1 mm, are undesirable but may occur in case of manufacturing imprecision. The profiles of Figures 1 and 2 are mitered such that the contact surfaces form an angle of 45° with respect to the longitudinal axis A of the respective profiles 1 and 2. However, other configurations of the contact area are also possible, for example configurations with contact surfaces perpendicular to the longitudinal axis A of the respective profiles.

[0065] The profiles 1 and 2 have grooves 4, 5, in particular weatherstrip grooves, to accommodate the weatherstrip joints of the sealing strip. When the sealing strip is mounted or screwed on, there are usually no end stops for the sealing strip. This means that additional assembly steps are required when positioning and removing the sealing strip during assembly. Furthermore, the sealing strip can move linearly within the groove.

[0066] In the corner joint 50 of Fig. 1, profiles 1 and 2 each have a profile wall with a visible side S and a rear side R. As shown in Figs. 1 and 2, each profile can also have two visible sides S and S' and two corresponding rear sides R and R'.

[0067] Inside the grooves 4 and 5 of each profile 1 and 2, a weld joint 6, 7, 6', 7' is provided in the form of a weld line or a surface weld profile consisting of several weld lines. A person skilled in the art will distinguish between such spot welds and weld lines. The weld line is commonly referred to as the weld bead, and usually refers to the pronounced bead of material formed by the fusion deformation, particularly the filler metal.

[0068] This bead of material is disadvantageous for several reasons: in the visible area, it reduces the visual appearance of the corner joint; furthermore, it is susceptible to rust and other environmental influences, and it must be reworked, usually by material-removal processes such as grinding or milling. In most applications, profiles machined with corner joints are coated. If the weld bead is too strong due to surface stresses, the coating can peel off or be removed during further processing.

[0069] On mounting surfaces intended for mounting to frame facing surfaces, leaf facing surfaces, or recessed wall surfaces, weld beads may interfere with accurate mounting location and may prevent windows or doors from closing or sealing In grooves 4 and 5, particularly in the location within the weatherstrip groove as shown in Figures 1 and 2, a pronounced weld bead would cause the weatherstrip seal to become clogged and make the window more difficult to close. However, the weld bead shown in Figures 1 and 2 is very low in height, preferably less than 1 mm, and more preferably less than 0.5 mm. As a result, the height of the weld bead is low and the above-mentioned disadvantages do not occur.

[0070] 2 shows the arrangement of the weld beads along the inside of the corner joint 50. The weld joints 10, 10', 11, 11' are in the form of weld beads and extend parallel to the longitudinal axis A of the respective profiles 1 and 2.

[0071] The location and longitudinal extension of the weld joints 6, 7 and 10, 11 as weld beads is explained by the fact that the two profiles 1 and 2 are indirectly welded together via corner angle connectors. Each weld bead connects a corner connector, not shown in FIGS. 1 and 2, to the profile wall, which closes the bottom of the respective groove 4 and 5 by a material connection. The laser beam is applied to the outer surfaces of the profile walls of profiles 1 and 2 and heats them to such an extent that a material connection is made with the corner angle connectors on the opposite sides of the profile walls, which is commonly called a through weld joint.

[0072] To achieve the low weld seam height or low weld bead height, no filler metal is used. It is particularly preferred that the weld seam, when viewed from the outer surface of the profile, is level with the adjacent areas or recessed relative to the adjacent areas.

[0073] During rework, a laser can be used to smooth out the weld seam so it is more flush. If subsidence occurs, additional coating material can be applied, for example by sputtering, which can be further melted by the laser to create adjacent regions and planar features, where the thickness of the coating layer is correspondingly greater than in the adjacent regions.

[0074] Using a fiber laser as the laser welding device allows for even lower weld joint heights with very precise heat input. The fiber laser can be configured as a so-called multi-head fiber laser, whereby two or more weld seams are applied simultaneously, such as for example weld seams 6 and 7 or 10 and 11 .

[0075] As a connecting aid, the legs of the corner angle connector are placed in the corresponding profile chambers 8 of the two profiles 1 and 2 and further stabilize the corner joint 50. The corner angle connector used should ideally be able to lie flat against the profile wall surface. This can be achieved using a corner angle connector with spring legs or using the corner angle connector as a moulded body made from solid material.

[0076] Figures 3 and 4 show two exemplary variations on corner angle connectors 12 and 16. Figure 3 shows corner angle connector 12 with two compressible spring legs 15, which are configured to be compressible perpendicular to their longitudinal extension.

[0077] The spring leg 15 comprises two contact walls 13a and 13b which contact the walls of the profiled chambers 8 and 9, respectively, and an elastically deformable web 14 arranged with a predefined buckling point between the two contact walls. The spring leg is tapered at its ends, which allows it to be inserted more easily into the respective profiled chambers. The distance between the contact walls 13a and 13b can shorten under the effect of a force, forming a restoring force. As a result, the spring leg 15 is inserted into the profile chamber 8 or 9 with a reduced distance between the contact walls 13a and 13b and is pressed against the profile chamber wall after resetting. This ensures optimal contact with the profile chamber wall during laser welding.

[0078] As an alternative to the elastically deformable web 14, other elastically deformable means can also be provided. This can be another form of web, for example an elastomer between the contact walls 13a and 13b. Also, the very precise heat input of laser welding allows the use of plastics that are not thermally stable at the temperature of the weld zone, but can be placed outside the weld area as part of the corner connector.

[0079] 4 shows a second of several variations of a corner connector 16 having two spring legs 19. Again, the spring legs 19 have two contact walls 20a, 20b that are variable in distance from each other and provide a restoring force.

[0080] Here, the two contact walls 20a and 20b are connected to one another via a spring web 18, which bears against a stop 17 which undergoes a bending deformation when the distance between the contact walls 20a and 20b decreases. In Fig. 4, this stop 17 is configured as a spherical cap on which the spherical end of the spring web 18 rests.

[0081] Figures 5a to 5f show several variations of weld shapes that can be used as part of the laser welding process, as weld lines to connect the profiles to the legs of corner connectors as shown in Figures 3 and 4, or as surface weld shapes.

[0082] FIG. 5a shows a single weld line 21 in a spiral weld configuration. FIG. 5b shows a single weld line 22 having a serpentine weld shape. FIG. 5c shows the cross pattern 23 as a flat weld joint consisting of multiple intersecting weld lines. FIG. 5d shows the weld pattern 24 as a surface weld joint consisting of multiple weld lines 25 arranged parallel to one another. FIG. 5e shows a single straight weld line 25, while FIG. 5f shows two weld lines 26 running parallel to each other.

[0083] Figure 6 shows a corner joint 50, as may be present, for example, in the region of the profile chamber 8 of figures 1 and 2. Figure 6 shows a further variant of the corner connector 32 for this purpose, which is made of solid material in order to better stabilize the corner joint.

[0084] In FIG. 6, an initial weld joint 33 is formed at the material connection between the profile wall of the profile chamber 8 and the corner angle connector 32 of the corner joint 60 . The distance 34 between the corner angle connector 32 and the profile wall 8 of the profile chamber 8 is not uniform, but increases gradually or abruptly in the direction of the leg transition or in the contact area 3 of the two profiles 1 and 2 . This is because the inner angle surface 36 defines an angle that is smaller than the longitudinal axes of the two legs of the corner corner connector, at least in the contact area of ​​the two legs of the corner corner connector, and therefore the diameter and / or cross section of the corner corner connector 32 decreases from the end of the legs in the direction of transition from one leg to the other.

[0085] 6 also shows the welding directions for making the weld seams of the corner joints 60. These run parallel to the longitudinal axis A from a start point remote from the contact area 3 to an end point close to the contact area 3.

[0086] The reason for this unusual structure of the corner angle connector 32 is the initial welded state in Figure 6 and the final welded state in Figure 7. The weld joint 33 further expands in area 35. During cooling due to material contraction due to temperature, the distance 34 in the area of ​​the weld joint 33 decreases. During cooling due to material contraction due to temperature, the distance 34 in the area of ​​the weld joint 33 decreases. During cooling, the material bond between the metallic profile and the corner angle connector 32 shrinks, placing the profiles in the contact area 3 under pretension, which causes them to be pressed together by this additional force. This tightening of the corner angle connector 32 by the pretension obtained as a result of observing the welding sequence makes the tightness of the contact area 3 more secure.

[0087] The variants shown in figures 1 to 7 can be carried out without opening the profile wall by welding through it. However, it is also possible to drill a through hole in the profile wall, through which the laser beam is guided directly into the weld area between the profile wall and the corner connector. This technique, also known as the keyhole method, allows a more targeted energy input, but requires a rather unfavorable opening of the profile, which can result in sealing off the through hole.

[0088] 8 to 10 describe a further variant of the welding of two profiles 1 and 2 to form a corner joint 70. In the embodiment shown in FIG. In this case, the profile wall 1 or 2 is chamfered at the ends in preparation for welding in the first step 101, so that the end faces 27 and 28 of the respective opposing profile walls 1 and 2 are not flat as usual, but taper towards each other in the contact area 3.

[0089] In a second step 102, the two end faces 27 and 28 are pressed together to form second beaded edges 29 and 30 when a corresponding contact pressure is applied across the contact area 3. This enlarges the joint to support a more stable connection. Finally, in a third step 103, the materials are welded by directing a laser beam onto the contact area.

[0090] This forms the weld seam 31, which in Fig. 10 protrudes from the visible side relative to the adjacent surface. Of course, the weld seam 31 can also protrude along the rear side R when it is beveled in the opposite direction to that shown in Fig. 8 in the first step 101. This protrusion of the weld seam 31 is not an inevitable result of the laser welding, but is merely a result of the material protrusion of the beaded edges 29 and 30.

[0091] The height of the weld seam can be reduced by post-treatment, e.g. by repeated laser irradiation. Furthermore, if the coating is damaged, the weld seam can be recoated by localized application of a coating material, e.g. by sputtering of paint particles. Laser processing can also be used to fuse particulate coating components together. Overall, the above-described method for forming a corner joint 70 directly between the profiles 1 and 2 using a laser melting process results in only slight bulges in the contact area and at the same time only slight burning of the coating in the area of ​​the weld seam.

[0092] 11a and 11b respectively show a perspective view and a cross-sectional view of a variant of the pre-fixing before the actual welding. A hole 81 with a straight drill groove is drilled through the two metal profiles 1, 2 and through the corner angle connector 12.

[0093] Pre-fixing is achieved by inserting mechanical fixing means 82, such as rods, screws and / or pins, into the holes.

[0094] The fastening means 82 is here rod-shaped with its longitudinal axis arranged perpendicular to the miter of the corner joint. After welding, the drill grooves can optionally be closed by welding using weldable drill hole inserts.

[0095] 11c and 11d show a second variant of pre-fixing by punching or clamping. This is preferably carried out with a punching or clamping tool 83. The corner connector 12 has a recess 84 along its leg. The punching or clamping tool 83 deforms the wall of the metal profile, in particular by pressing it, so that it partially protrudes into the recess 84. This deformation, in particular by pressing and / or punching the metal profile, achieves a positive engagement with the corner connector 12. The metal profiles 1 and 2 are then welded to the corner connector 12.

[0096] Figures 11e and 11f disclose a further variant of pre-fixing, in which the corner angle connector 12 is fixed to the metal profiles 1 and 2 with a rod 85, in particular a mandrel. First, holes 86, e.g. nail holes, are made coaxially in the metal profile 1 or 2 and in the corner angle connector 12. Then, said rod 85 or another mechanical fastening means, e.g. a screw, is inserted into the holes 86. Two holes are provided for each corner connection. The longitudinal axes of the two mechanical fastening means are preferably perpendicular to each other and at an angle of 45 degrees to the miter joints of the metal profiles 1 and 2.

[0097] 11g and 11h disclose a further variant of pre-fixing, in which the metal profiles 1 and 2 are formed after the corner connectors have been inserted into the profiles. The forming is carried out by rolling the walls of the metal profiles in the direction of the corner connectors with a so-called press-rolling tool 87. This forming is reinforced by pressing the corner connectors into the corner receivers 88. The rollers of the tool move towards each other along the surfaces of the corner joints, as shown in Figs. 11g and 11h. Then the welding can be carried out again.

[0098] In the forming operations shown in Figures 11c and 11d, as in Figures 11g and 11h, the prefixture is maintained after welding.

[0099] The prefixing variants shown in Figures 11a to 11h have proven to be fundamentally favorable for producing well-defined welded connections with small gap dimensions. That a particularly easy-to-handle and at the same time optimal prefixing is achieved with the variants shown in Figures 11e and 11f has surprisingly been demonstrated by extensive comparative tests with non-illustrated variants of the prefixing.

[0100] To achieve pre-fixing, various punch geometries are possible, these are illustrated in Figures 12a to 12d. The method according to the invention makes it possible in particular to improve the sustainability and environmental protection of the profile and frame connections.

[0101] The replacement of conventional adhesives with mechanical connections simplifies the separation of materials by type. Time-limited pre-fixing combinations of nailing, crimping, screwing, punching, clamping (frame mounting) and welding processes, preferably laser, resistance spot, soldering and inert gas welding, are also particularly advantageous. Corner connectors have adapted geometries with regard to tolerances and position compensations.

[0102] The approach according to the invention provides for permanent metallurgical joining of unpainted or surface-treated profiles, e.g. anodized, painted and / or pre-treated color-coated metallic profiles, with a secondary visible surface, e.g. by energy-assisted material joining under the influence of heat.

[0103] This step makes it possible to increase the current cycle times of manual production in industrial processes.

[0104] The method according to the invention also allows for manual and / or partially automated or automated profile joining and frame manufacturing. Moreover, the method allows for static verification of these profile connections, in particular the mullion and transom connections. [Explanation of symbols]

[0105] 1 Profile 2 Profile 3 Contact area 4 grooves 5 grooves 6, 6' Welded joint 7, 7' Welded joint 8 Profile Room 9 Profile Room 10, 10' Welded joint 11, 11' Welded joint 12 Corner Connector 13a Contact wall 13b Contact wall 14 Elastically deformable web 15 Spring leg 16 Corner Connector 17 Stopper 18 Spring Web 19 Spring leg 20a contact wall 20b contact wall 21 Welding Line 22 Welding Line 23 Cross Pattern 24 Welding Pattern 25 Welding Line 26 Welding Line 27 End face 28 End face 29 Bead edge 30 Bead edge 31 Welded seams 32 Corner Connector 33 Welded joints 34 distance 35 areas 36 Interior Surfaces 50 Corner joint 60 Corner joint 70 Corner joint 81 holes 82 Fixing means 83 Punching and / or clamping tools 84 Recess 85 Rod 86 holes 87 Rolling Tools 88 Corner connector receiving part R, R' rear side S, S' visible side L Longitudinal axis (metal profile) 101 First Step 102 Second Step 103 Third Step

Claims

1. A window, door and / or facade construction comprising a corner joint (50, 60, 70) in which two metal profiles (1, 2) are connected to one another by one or more welded joints (6, 7, 6', 7', 10, 10', 11, 11', 33), the welded joints (6, 7, 6', 7', 10, 10', 11, 11', 33) being configured as laser welded joints, Window, door and / or facade construction, characterized in that the welded joint (6, 7, 6', 7', 10, 10', 11, 11', 33) indirectly connects the profiles (1, 2) by means of corner connectors (12, 16, 32), the profiles (1, 2) particularly preferably each having a profile chamber (8, 9), the corner connectors (12, 16, 32) having at least two legs which are inserted into the profile chambers (8, 9).

2. 2. The window, door and / or facade structure according to claim 1, wherein the welded joint (6, 7, 6', 7', 10, 10', 11, 11', 31, 33) is configured as a welded seam with a protrusion of less than 1 mm, preferably less than 0.5 mm, preferably less than 0.1 mm, as a line of multiple weld spots or as a surface weld profile or as a recess relative to the adjacent areas.

3. 3. A window, door and / or facade structure according to claim 1 or 2, wherein the painted areas adjacent to the laser welded joints are formed as burnt areas with pyrolysis products of the paint.

4. 4. A window, door and / or facade structure according to claim 3, wherein the painted area comprising pyrolysis products of the paint extends away from the laser welded joint as a burnt area over a width of less than 2 mm, preferably less than 1 mm.

5. 5. A window, door and / or facade structure according to any of claims 1 to 4, wherein the corner connector (12, 16, 32) is configured to build up a pretension between two contact surfaces resting against each other in the contact area (3) of the metal profiles (1, 2) in the assembled state of the corner joint (50, 60).

6. 6. A window, door and / or facade construction according to any one of claims 1 to 5, wherein the longitudinal axes of the legs of the corner angle connector (12, 16, 32) define a first angle and the inner angle surface (36) formed by both legs has a recess in the contact area of ​​both legs or defines a second angle smaller than the first angle.

7. 7. A window, door and / or facade construction according to any of the preceding claims, characterized in that the two legs of the corner connector (12, 16) are configured as spring legs (15, 19) for supporting against a profile wall.

8. 8. A window, door and / or facade structure according to any of the preceding claims, wherein the welded joints are arranged inside the grooves (4, 5) of the profiles (1, 2), preferably along their base, particularly preferably along the groove of the weatherstrip.

9. 9. The window, door and / or facade structure according to any of the preceding claims, wherein the welded joints (6, 7, 6', 7', 10, 10', 11, 11', 31, 33) are configured as full-thickness welded joints, such that at least one profile wall forms a solidified weld pool over the entire thickness of the profile wall, and, if corner connectors (12, 16, 32) are used, preferably a part of the corner connector (12, 16, 32) forms part of the molten pool.

10. 10. A window, door and / or facade structure according to any of the preceding claims, wherein the welded joints (6, 7, 6', 7', 10, 10', 11, 11', 31, 33) are constructed without filler metal.

11. A method for manufacturing a corner joint (50, 60, 70) for a window, door and / or facade structure according to any one of claims 1 to 10, comprising the steps of: a) providing two metal profiles (1, 2), preferably coated metal profiles, and positioning the two metal profiles (1, 2) at an angle to each other, the providing step being carried out by inserting each leg of the corner angle connectors (12, 16, 32) into the profile chambers (8, 9) of the respective metal profiles (1, 2) such that each leg of the corner angle connectors (12, 16, 32) is located in each of the metal profiles (1, 2); b) welding both metallic profiles (1, 2) together using a laser welding device, in particular a fiber laser welding device, The method is characterized in that the power of the laser welding device is set in such a way that through-welded weld joints (6, 7, 6', 7', 10, 10', 11, 11', 31, 33) are provided through the profile wall, and at least one, preferably through-welded weld joint (6, 7, 6', 7', 10, 10', 11, 11', 33) is arranged between each metal profile (1, 2) and a corner connector (12, 16, 32).

12. 12. The method according to claim 11, wherein at least one full penetration weld joint (6, 7, 6', 7', 10, 10', 11, 11', 33) is formed between each metal profile (1, 2) and the corner connector (12, 16, 32), preferably with the formation of a pretension, which full penetration weld joint is particularly preferably located outside the contact area (3), particularly preferably on the outside of the two metal profiles (1, 2).

13. 13. The method according to claim 11 or 12, wherein the method comprises re-processing consisting of a further laser processing to form a coating by melting a coating component or by radiation activated crosslinking of the coating material or by evaporating a coating component.

14. 14. The method according to claim 11, wherein the metal profiles (1, 2) are pre-fixed after the insertion of the corner connector (12) and before the welding according to step b), the pre-fixing being preferably formed by means of a positive fit between one of the metal profiles (1, 2) and the corner connector (12) or by introducing mechanical fixing means into holes (87) or apertures in one of the metal profiles (1, 2) and the corner connector (12).

15. 15. The method according to any of claims 11 to 14, wherein no filler metal is used to produce the weld joint in step b).