Glass composition, glass fiber, glass cloth, and glass fiber production method
A tailored glass composition with specific oxide ratios addresses the challenge of achieving low dielectric constant and mass production suitability, resulting in high-performance glass fibers for printed circuit boards.
Patent Information
- Application Number
- JP2024133361
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-06-21
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-06-19
AI Technical Summary
Existing glass compositions struggle to achieve a low dielectric constant while being suitable for mass production, particularly in the context of producing glass fibers with smaller diameters required for thinner printed circuit boards and high-speed data transmission.
A glass composition is formulated with specific ranges of SiO2, B2O3, Al2O3, and RO (where RO includes Li2O, Na2O, K2O, MgO, CaO, and SrO) to achieve a low dielectric constant and suitable characteristic temperatures for mass production, ensuring homogeneity and preventing devitrification and bubble inclusion.
The solution provides glass fibers with a dielectric constant of 4.4 or less and a dielectric loss tangent of 0.007 or less, suitable for mass production with reduced fiber breakage and bubble inclusion, enhancing the performance of printed circuit boards.
Smart Images

Figure 2024149728000001 
Figure 2024149728000002 
Figure 2024149728000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass composition, a glass fiber and a glass cloth made of the composition, and a method for producing a glass fiber. [Background technology]
[0002] A type of printed circuit board that is equipped on electronic devices, made of resin, glass, There are substrates that are made of fibers and inorganic fillers, and, if necessary, further materials such as hardeners and modifiers. There are also printed wiring boards (PCBs) on which electronic components are mounted. There are also printed circuit boards that have a similar structure to the substrate. In the following description, both printed circuit boards and printed wiring boards are collectively referred to as "printed boards." In the printed circuit board, the glass fiber functions as an insulator, a heat resistant material, and a reinforcing material for the board. The glass fiber is included in the printed circuit board, for example, as glass cloth woven from glass yarns (glass yarns) made of a plurality of glass fibers. In addition, the glass cloth is usually used in the printed circuit board as a prepreg impregnated with resin. In recent years, in order to meet the demand for miniaturization of electronic devices and the demand for high mounting of printed circuit boards for the purpose of high functionality, the printed circuit boards have been made thinner. In order to make the printed circuit boards thinner, glass fibers with smaller fiber diameters are required. In addition, due to the reason that the demand for high-speed transmission and processing of large amounts of data is rapidly increasing, the glass fibers used in the printed circuit boards are required to have a low dielectric constant.
[0003] Glass is also used as an inorganic filler for printed circuit boards. A typical example is flake glass. When a glass molded body such as flake glass is used as an inorganic filler for printed circuit boards, the molded body is required to have the same properties as glass fibers used in printed circuit boards, such as a low dielectric constant.
[0004] Patent documents 1 to 5 disclose glass fibers made of a glass composition having a low dielectric constant. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 62-226839 [Patent Document 2] Special Publication No. 2010-508226 [Patent Document 3] JP 2009-286686 A [Patent Document 4] International Publication No. 2017 / 187471 [Patent Document 5] International Publication No. 2018 / 216637 Summary of the Invention [Problem to be solved by the invention]
[0006] The glass composition is required to have a characteristic temperature suitable for mass production as well as a low dielectric constant. The characteristic temperature of the glass composition important for mass production of glass fibers is the temperature T3, which is a guideline for the spinning temperature, that is, the temperature at which the viscosity is 10 3 dPas. Temperature T2 , T2.5, and even the devitrification temperature TL are indicators for determining whether a glass composition is suitable for mass production of glass fibers. However, it is not easy to adjust the characteristic temperature of a glass composition with a low dielectric constant.
[0007] In view of the above, an object of the present invention is to provide a novel glass composition that has a low dielectric constant and is suitable for mass production. [Means for solving the problem]
[0008] The present invention relates to Expressed as weight percent, 40≦SiO2≦60 25≦B2O3≦45 5≦Al2O3≦15 0 <R2O≦5 0 <RO<15 Including, SiO2+B2O3≧80 and / or SiO2+B2O3≧78 and 0 <RO<10 The present invention provides a glass composition, in which the following holds true: In this specification, R2O is at least one oxide selected from Li2O, Na2O, and K2O, and RO is at least one oxide selected from MgO, CaO, and SrO.
[0009] From another aspect, the present invention provides Expressed as weight percent, 40≦SiO2≦60 25≦B2O3≦45 0 <Al2O3≦18 0 <R2O≦5 0≦RO≦12 Including, i) SiO2 + B2O3 ≧ 80, and SiO2 + B2O3 + Al2O3 ≦ 99.9, and ii) SiO2+B2O3≧78, SiO2+B2O3+Al2O3≦99.9, and 0 <RO<10 The present invention provides a glass composition, in which at least one of the following conditions is satisfied.
[0010] From another aspect, the present invention provides Expressed as weight percent, 40≦SiO2≦60 25≦B2O3≦45 0 <Al2O3≦18 0 <R2O≦5 3 <RO<8 Including, SiO2+B2O3≧75, and SiO2+B2O3+Al2O3<97 The present invention provides a glass composition, in which the following holds true:
[0011] The present invention is, from another aspect, When expressed by weight, SiO2+B2O3≧77 is satisfied. The dielectric constant at a frequency of 1 GHz is 4.4 or less, The dielectric tangent at a frequency of 1 GHz is 0.007 or less, viscosity 10 2 The temperature T2 at which dPas occurs is 1700°C or less. The present invention provides a glass composition,
[0012] The present invention is, from another aspect, Expressed in weight percent, 40≦SiO2≦49.95 25≦B2O3≦40 10≦Al2O3≦20 0.1≦R2O≦2 1≦RO≦10 Including, SiO2+B2O3≧70, and SiO2+B2O3+Al2O3≦97 The present invention provides a glass composition, in which the following holds true:
[0013] The present invention is, from another aspect, Expressed in weight percent, 40≦SiO2≦49.95 25≦B2O3≦29.9 10≦Al2O3≦20 0.1≦R2O≦1 2≦RO≦8 Including, SiO2+B2O3≧70, and SiO2+B2O3+Al2O3≦97 The present invention provides a glass composition, in which the following holds true:
[0014] The present invention is, from another aspect, Expressed as weight percent, 40≦SiO2≦49.95 31≦B2O3≦40 8≦Al2O3≦18 0.1≦R2O≦1 1≦RO≦10 Including, SiO2+B2O3≧77, and SiO2+B2O3+Al2O3≦97 The present invention provides a glass composition, in which the following holds true:
[0015] From another aspect, the present invention provides A glass fiber composed of the glass composition according to the present invention is provided.
[0016] From another aspect, the present invention provides A glass cloth made from the glass fibers according to the present invention is provided.
[0017] From another aspect, the present invention provides A prepreg comprising the glass cloth according to the present invention is provided.
[0018] From another aspect, the present invention provides A printed circuit board comprising the glass cloth according to the present invention is provided.
[0019] From another aspect, the present invention provides The present invention provides a method for producing glass fibers, which comprises a step of melting the glass composition according to the present invention at a temperature of 1400° C. or higher to obtain glass fibers having an average fiber diameter of 1 to 6 μm. Effect of the Invention
[0020] According to the present invention, it is possible to provide a glass composition having a lower dielectric constant and a characteristic temperature suitable for mass production. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] In the following, all "%" indications of the content of each component are by weight. "Substantially free" means that the content is less than 0.1% by weight, preferably less than 0.07% by weight, and more preferably less than 0.05% by weight. In this context, "substantially" means that impurities that are inevitably mixed in from industrial raw materials are allowed up to the above-mentioned limits. The preferred ranges of the content, characteristics, and other properties of each component can be understood by any combination of the upper and lower limits described individually below.
[0022] In the following, the characteristic temperature of the glass composition is n The temperature at which dPas is Tn (For example, T2.5 means that the viscosity of the glass composition is 10 2.5 Temperature at which dPas occurs (Strictly speaking, the dielectric constant means the relative dielectric constant, but in this specification, it is simply referred to as the dielectric constant according to the conventional practice. The dielectric constant and the dielectric loss tangent are values at room temperature (25° C.). The following description is presented for the purpose of showing a preferred embodiment of the present invention, without the intention of limiting the present invention.
[0023] [Components of the composition] (SiO2) SiO2 is a component that forms the network structure of glass. SiO2 has the effect of lowering the dielectric constant of the glass composition. If the SiO2 content is too low, the dielectric constant of the glass composition cannot be sufficiently increased. If the SiO2 content is too high, the viscosity at the time of melting becomes too high and the melting temperature becomes too high. When the homogeneity of the glass composition is decreased, fiber breakage is induced during spinning of glass fibers, particularly glass fibers having a small fiber diameter. The SiO2 content is 40% or more, 45% or more, 46% or more, or even 48% or more, particularly 49% or more. % or more, and in some cases, it may be 50% or more, further 50.5% or more, 51% or more, 52% or more, or 53% or more. The SiO2 content is 60% or less, less than 58%, The content of SiO2 is preferably 56% or less, more preferably less than 55%, particularly preferably 54.5% or less, and in some cases may be 54% or less, 53% or less, 52% or less, or 51% or less. An example of a preferable range is 40% or more and less than 58%, and further 40% or more and less than 55%. The SiO2 content can also be 40% or more and 49.95% or less.
[0024] (B2O3) B2O3 is a component that forms a network structure of glass. B2O3 reduces the dielectric constant of the glass composition, reduces the viscosity of the glass composition when melted, improves defoaming (bubble removal), and has the effect of suppressing the inclusion of bubbles in the formed glass fiber. On the other hand, B2O3 is easily volatilized when the glass composition is melted, and if its content is excessive, it may be difficult to obtain sufficient homogeneity as a glass composition, the inclusion of bubbles in the formed glass fiber may be insufficiently suppressed, or B2O3 volatilized from the glass may adhere to the tip of a bushing used in spinning, causing so-called thread breakage. The content of B2O3 is preferably 25% or more, 27% or more, 29% or more, 30% or more, or even more than 30%, and may be 30.5% or more, or even 31% or more, 32% or more, 33% or more, or 34% or more in some cases. The content of B2O3 is preferably 45% or less, 43% or less, 41% or less, or even 39% or less, and may be 38% or less, further 36% or less, 35% or less, 34% or less, or 32% or less in some cases. An example of a preferred range of the content of B2O3 is more than 30% and 45% or less. The content of B2O3 may be 25% or more and 40% or less, 25% or more and 29.9% or less, or 31% or more and 40% or less.
[0025] (SiO2+B2O3), (SiO2+B2O3+Al2O3) In order to obtain a glass composition with a sufficiently low dielectric constant, the SiO2 content and the B2O3 content must be If the total (SiO2+B2O3) is adjusted to 77% or more, 78% or more, or even 80% or more, (SiO2+B2O3) is preferably 81% or more, 82% or more, or even 83% or more. In some cases, it may be 84% or more, or even 85% or more. (SiO2+B2O 3) may be 90% or less, or even 87.5% or less. If the value of (SiO2+B2O3) is too high, the tendency of the glass composition to undergo phase separation is promoted. + B2O3) can be 70% or more. The SiO2 content, the B2O3 content, and The total content of Al2O3 (SiO2+B2O3+Al2O3) is 100% to allow for other components. Therefore, 99.9% or less is preferable. (SiO2+B2O3+Al2O3) is 98% or less, It may be 97% or less, less than 97%, or even 96% or less. (SiO2+B2O3) and A preferred example of a combination with (SiO2+B2O3+Al2O3) is that (SiO2+B2O3) is 82% or more and (SiO2+B2O3+Al2O3) is 98% or less. Also, (SiO2+B2O3+Al2O3) can be 90% or more and 98% or less, or 90% or more and 97% or less.
[0026] The ratio of (SiO2+B2O3+Al2O3) to (SiO2+B2O3), i.e., (SiO2+B2O3+Al2O3) / (SiO2+B2O3), is preferably 1.05 or more, and may be 1.12 or more, 1.13 or more, 1.15 or more, or even 1.20 or more. As this ratio increases, defects such as fluffing of glass fibers are suppressed. This effect becomes more pronounced in the fifth combination of the contents of SiO2 and B2O3 described later.
[0027] (Preferable combination of SiO2 and B2O3) In order to obtain a glass composition with a lower dielectric constant and easier melting, the content of SiO2 and B2O3 is There are preferred range combinations of SiO2 content. The first combination is The second combination is a combination of SiO2 content of 50 to 53%, preferably 51 to 52%, and B2O3 content of 33 to 35%, preferably 34 to 35%. The third combination is a combination in which the SiO2 content is 52 to 54%, preferably 52.5 to 54%, and the B2O3 content is 32 to 35%, and preferably 32 to 34%. The fourth combination is a combination in which the SiO2 content is 52 to 55%, preferably 53 to 55%, and the B2O3 content is 30 to 35%. This is a 2% combination.
[0028] The fifth combination has a SiO2 content of 47 to 52%, preferably 48 to 51%, and more preferably The fifth combination is a combination in which the content of B2O3 is 25-30%, preferably 26-29.5%, and more preferably 26-29%. In the fifth combination, the sum of the content of MgO and the content of CaO (MgO+CaO) is 3.5% or more, more preferably 4% or more, and is suitably 8% or less. In the sixth combination, the content of SiO2 is 48-53%, preferably 49 and the B2O3 content is 28-35%, preferably 30-33%, and sometimes 30.5-32.5%. In the sixth combination, (MgO+CaO) is 1% or more and less than 3.5%, preferably 1-3%, more preferably 1-2.5%, and sometimes 1.5-2.5%.
[0029] (Al2O3) Al2O3 is a component that forms the network structure of glass. Al2O3 has the effect of increasing the chemical durability of the glass composition. On the other hand, Al2O3 makes the glass composition more susceptible to devitrification during spinning. The content of Al2O3 is preferably 5% or more, 7.5% or more, 8% or more, 9% or more, or even 10% or more, and may be 10.5% or more, 12% or more, or 13% or more in some cases. The content of Al2O3 is preferably 20% or less, 18% or less, 17% or less, or even 15% or less, and may be 14% or less, or even 13% or less, or 12.5% or less in some cases. An example of the content of Al2O3 suitable for the case where it is desired to reliably control the devitrification temperature TL to a range lower than the temperature T3 is 12.3% or less. Al2O3 is generally It is understood to be a component that increases the viscosity of the glass composition during melting. However, SiO2 + B2O3 In a glass composition having a high value of , Al2O3 can specifically act to reduce the viscosity during melting.
[0030] A preferred range of the Al2O3 content is, for example, 8 to 12.5%, particularly 10 to 12.5%. When the first to fourth combinations of the SiO2 and B2O3 contents described above are adopted, These ranges are particularly suitable.
[0031] Another example of a preferable range of the content of Al2O3 is 13 to 17%. When the fifth combination of the content of B2O3 is used, the content of Al2O3 is particularly preferably 13 to 17%. Another example of a preferable range of the content of Al2O3 is 12 to 15%. When the sixth combination of the content of SiO2 and B2O3 is used, the content of Al2O3 is preferably 13 to 17%. A prevalence of 12-15% is particularly suitable.
[0032] Alkali metal oxides are well known as components that act to reduce viscosity during melting, but increasing the content of alkali metal oxides simultaneously increases the dielectric constant. In contrast, in the preferred glass composition of the present invention, Al2O3 specifically acts to reduce viscosity during melting, but has only a slight side effect of increasing the dielectric constant.
[0033] (MgO) MgO is an optional component that reduces the viscosity of the glass composition during melting, suppresses the mixing of bubbles into the glass fibers, and improves the homogeneity of the glass composition. The content of MgO may be 0.1% or more, 0.2% or more, further 0.5% or more, 0.6% or more, and in some cases 0.8% or more, or even 1% or more. The content of MgO is preferably less than 10%, 8% or less, 7% or less, or 5% or less, and in some cases 3% or less, further 2% or less, and particularly 1.6% or less. In order to set the ratio to the CaO content in an appropriate range, the content of MgO may be preferably 1.7% or less, 1.5% or less, further 1.2% or less, or 1% or less. However, depending on the content of other components, the optimal content of MgO may be 2% or more, for example, 2 to 8%, or even 2 to 5%, or 3 to 5%. Note that MgO has a large effect of lowering the devitrification temperature, and yet is not as effective as the alkali metal oxide R2O. In order not to increase the dielectric constant, it is preferable to add it preferentially over R2O, in other words, so that its content is higher than that of R2O.
[0034] The preferred range of the content of MgO is, for example, 0.5 to 2%. When the first to fourth combinations of the content of SiO2 and B2O3 are adopted, the content of MgO is preferably 0.5 to 2%, more preferably 0.5 to 1.6%. When using SiO2 and B2O3, the content of MgO is preferably 0.5 to 2%, more preferably 1 to 2%. Another example of a preferred range of the content of MgO is 0.1 to 1%. Content of SiO2 and B2O3 When the sixth combination is employed, the content of MgO is particularly suitably 0.1 to 1%, and more preferably 0.1% or more and less than 1%.
[0035] (CaO) CaO is an optional component that improves the solubility of glass raw materials and reduces the viscosity of the glass composition during melting. The effect of CaO is greater than that of MgO. The CaO content may be 0.1% or more, 0.5% or more, or even 1% or more, and in some cases 1.5% or more, or even 2% or more. The CaO content is preferably less than 10%, 7% or less, or 5% or less, and in some cases 4% or less, 3.5% or less, 3% or less, or even 2.5% or less. CaO has a greater effect of increasing the dielectric constant of the glass composition than MgO and ZnO. For the same reason as MgO, CaO is also more effective than the alkali metal oxide R2O. It is preferred to add it preferentially, in other words, so that its content is higher than that of R2O.
[0036] The preferred range of the CaO content is, for example, 2 to 5%, and more preferably 2 to 3.5%. When the first to fifth combinations of the content of SiO2 and B2O3 are adopted, the CaO content is particularly suitable to be 2 to 5%, and the first to fourth combinations are more suitable to be 2 to 3.5%, and the fifth combination is more suitable to be 2.5 to 5%. Another example of a preferred range of the CaO content is 0.5 to 2%. When the sixth combination of the content of SiO2 and B2O3 is adopted, the CaO A content of 0.5 to 2% is particularly suitable.
[0037] An example of a particularly preferred combination of the MgO content and the CaO content is 1-2% MgO and 2-5% CaO, which is particularly suitable when the fifth combination of the SiO2 and B2O3 contents is used.
[0038] (SrO) SrO is also an optional component that improves the solubility of glass raw materials and reduces the viscosity of the glass composition during melting. However, since SrO increases the dielectric constant of the glass composition compared with MgO and CaO, it is desirable to limit the content of SrO. The content of SrO is preferably 1% or less, 0.5% or less, or even 0.1% or less. SrO may not be substantially contained.
[0039] When the first to fifth combinations of the content of SiO2 and B2O3 are adopted, the content of SrO A content of 0.1% or less is particularly suitable. In this case, SrO may not be substantially contained. However, SrO may be added so that its content is 0.1 to 5%, or even 1 to 3.5%. When the sixth combination of SiO2 and B2O3 contents is adopted, For this combination, the SrO content is preferably 0.1-5%, more preferably 1-3.5%. In particular, in the sixth combination, it has been found that SrO, contrary to the common technical knowledge of those skilled in the art, can effectively act to reduce dielectric loss, in other words, to reduce dielectric tangent. In the sixth combination, the ratio SrO / CaO of the SrO content to the CaO content may exceed 1. In this case, the ratio CaO / MgO of the CaO content to the MgO content may also exceed 1.
[0040] (RO) The content of RO, i.e., the total content of MgO, CaO and SrO, is preferably less than 15%, 12% or less, 10% or less, 9.5% or less, 8% or less, or even less than 7%, particularly preferably 6% or less, and in some cases may be 5% or less, or even 4% or less. If the content of RO is too high, the dielectric constant may not be sufficiently reduced. Each component constituting RO is an optional component individually, but it is preferable that at least one of them is included, that is, the total content exceeds 0%. The content of RO is preferably 1% or more, 1.5% or more, 2% or more, or even 2.5% or more, and in some cases may be 3% or more, or even 3.5% or more.
[0041] A preferred example of the range of the RO content is 2 to 7%, particularly 2 to 4%.
[0042] (MgO / RO) MgO / RO, i.e., the ratio of the MgO content to the RO content, is preferably less than 0.8, further preferably less than 0.7, and may be 0.5 or less, or 0.4 or less in some cases. When MgO / RO is large, the glass composition tends to undergo phase separation more significantly, and the homogeneity of the glass composition may be impaired. In addition, the mixture of phases with different physical properties may make spinning difficult. On the other hand, in order to suppress the dielectric constant of the glass composition, MgO / RO is preferably 0.1 or more, further preferably 0.14 or more, and may be 0.19 or more in some cases. MgO / RO is preferably 0.1 to 0.5.
[0043] (MgO / (MgO+CaO)) The ratio of MgO / (MgO+CaO), i.e., the ratio of the content of MgO to the total content of MgO and CaO, may be within any range of the above upper and lower limits for MgO / RO. MgO / (MgO+CaO) is preferably 0.1 to 0.5, and more preferably 0.1 to 0.4.
[0044] (LiO) Even a small amount of Li2O can reduce the viscosity of the glass composition during melting and improve the glass Li2O is an optional component that has the effect of suppressing the incorporation of bubbles into the fibers and also suppresses devitrification. In addition, the addition of an appropriate amount of Li2O significantly suppresses the tendency of the glass composition to undergo phase separation. However, Li2O increases the dielectric constant of the glass composition, although its effect is relatively weaker than that of other elements such as R2O. The content of Li2O is preferably 1.5% or less, 1% or less, or 0.5% or less. The Li2O content may be 0.01% or more, 0.03% or more, or even 0.05% or more. The preferred range of the Li2O content is, for example, 0.01 to 0.5%, and more preferably 0.0 5~0.4%.
[0045] (Na2O) Even a small amount of Na2O can be added to the glass composition to reduce its viscosity during melting. It is an optional component that has the effect of suppressing the incorporation of bubbles into the fibers and also has the effect of suppressing devitrification. From this viewpoint, the content of Na2O is 0.01% or more, 0.05% or more, and However, the addition of Na2O increases the dielectric constant of the glass composition. The Na2O content must be kept within a limited range so as not to increase the temperature. At most, 1% or less, 0.5% or less, and even 0.4% or less are preferable, and in some cases, it may be 0.2% or less, even 0.15% or less, and particularly 0.1% or less, 0.05% or less, and 0.01% or less. An example of a preferable range of the Na2O content is 0.01 to 0.4%.
[0046] (K2O) Even a small amount of K2O can reduce the viscosity of the glass composition during melting, and can also improve the glass fiber structure. It is an optional component that has the effect of suppressing the incorporation of bubbles into the fibers and also suppressing devitrification. However, K2O has a large effect of increasing the dielectric constant of the glass composition. The content of K2O is preferably 1% or less, 0.5% or less, or 0.2% or less, and may be 0.1% or less, 0.05% or less, or 0.01% or less in some cases. K2O is not substantially contained. This is also fine.
[0047] (R2O) The content of R2O and the total content of Li2O, Na2O and K2O is preferably 5% or less, 4% or less, 3% or less, 2% or less, or even 1.5% or less, and in some cases may be 1% or less, or even 0.6% or less, or 0.5% or less. Each component constituting R2O is individually Although these are optional components, it is preferable that at least one of them is contained, i.e., the total content exceeds 0%. The content of R2O is 0.03% or more, 0.05% or more, Further, it is preferably 0.1% or more, more preferably 0.15% or more, and even more preferably 0.2% or more.
[0048] Furthermore, when the content of Li2O is greater than the content of Na2O, the tendency of the glass composition to undergo phase separation may be more effectively suppressed.
[0049] When the Li2O content is 0.25% or more, or even 0.3% or more, the characteristic temperature is further increased. In particular, the first combination of the SiO2 and B2O3 contents can be adjusted to a desired range. When using this method, the Li2O content must be 0.25% or more, and preferably 0.3% or more. In this case, it is preferable to add Na2O so that the content is 0.05% or more. It may be added so that the content is less than the content of i2O.
[0050] (T-Fe2O3) T-Fe2O3 is an optional component that improves the solubility of glass raw materials by its heat ray absorption action and improves the homogeneity of the glass composition during melting. Due to the effect of improving homogeneity by T-Fe2O3, even when the fiber diameter of the formed glass fiber is small, the occurrence of glass fiber breakage during spinning is suppressed, and spinning operability is improved. The content of T-Fe2O3 is preferably 0.01% or more, 0.02% or more, 0.05% or more, or even 0.10% or more. The effect of improving solubility is remarkable when the content of T-Fe2O3 is 0.01% or more, but the effect of improving homogeneity is particularly remarkable when the content of T-Fe2O3 is 0.02% or more. For the purpose of suppressing excessive heat ray absorption action by T-Fe2O3, the content of T-Fe2O3 is preferably 0.5% or less, 0.3% or less, or even 0.25% or less, and may be 0.20% or less in some cases. In this specification, according to the conventional practice, the total amount of iron oxide in a glass composition is expressed as FeO, etc. The value of iron oxide other than O3 converted to Fe2O3, i.e., the content of T-Fe2O3, is displayed. Therefore, at least a part of T-Fe2O3 can be contained as FeO. A preferable range of the content of T-Fe2O3 is, for example, 0.01 to 0.5%, and further 0.1 to 0.3%.
[0051] (ZnO) ZnO is an optional component that improves the solubility of glass raw materials and reduces the viscosity of the glass composition during melting. However, ZnO increases the dielectric constant of the glass composition. The content of ZnO is preferably 3.5% or less, 2% or less, 1% or less, or even 0.5% or less. ZnO may not be substantially contained.
[0052] (Other Ingredients) Other components that may be included in the glass composition include P2O5, BaO, PbO, TiO2 , ZrO2, La2O3, Y2O3, MoO3, WO3, Nb2O5, Cr2O3, SnO2, CeO2, As2O3, Sb2O3, and SO3 can be exemplified. Other components that the glass composition may contain are, for example, precious metal elements such as Pt, Rh, and Os, and halogen elements such as F and Cl. The allowable content of each of these components is preferably less than 2%, further less than 1%, and particularly less than 0.5%, and the total content is preferably less than 5%, further less than 3%, particularly less than 2%, and especially less than 1%. However, the glass composition may be substantially free of each of the other components described above. TiO2 may be added in a small amount for the reasons described below. ZrO2 may be present, but may not be present substantially. It is preferable that BaO and PbO are not substantially contained. It is also preferable that P2O5 is not substantially contained. This is because BaO and PbO have a large effect of increasing the dielectric constant of the glass composition, and P2O5 induces phase separation. However, even in this case, the glass composition should contain components effective for promoting fining during melting, preferably SO3, F, and Cl, each in an amount of less than 2%. It is okay to do so.
[0053] Contrary to the common technical knowledge of a person skilled in the art, the addition of a small amount of TiO2 has a large effect on the dielectric constant and dielectric constant of the glass composition. It was found that the electric loss tangent may decrease. From this viewpoint, the content of TiO2 is The sixth combination of the content of SiO2 and B2O3 may be more than 0% and less than 1%. When using this material, TiO2 may be added in an amount of more than 0% and not more than 1%.
[0054] (Example of a preferred composition) In one preferred embodiment, the glass composition of the present invention comprises the following components: 40≦SiO2<58 25≦B2O3≦40 7.5≦Al2O3≦18 0 <R2O≦4 0≦Li2O≦1.5 0≦Na2O≦1.5 0≦K2O≦1 1≦RO<10 0≦MgO<10 0≦CaO<10 0≦SrO≦5 0≦T-Fe2O3≦0.5
[0055] In one embodiment containing the above components, 7.5≦Al2O3≦15 and 0≦SrO≦1 may be satisfied.
[0056] At the end of the above 0≦ZnO≦3.5 A glass composition containing the above is also another preferred embodiment.
[0057] These types of glass compositions preferably further satisfy 40≦SiO2<55. In addition, SiO2+B2O3≧80 may be satisfied, and preferably SiO2+B2O3+Al2 The glass may further satisfy O3≦99.9. MgO / RO<0.8 may also be used in the above-mentioned form. This is another condition that the composition may meet.
[0058] [Characteristics] (Dielectric constant) In a preferred embodiment, the dielectric constant of the glass composition according to the present invention at a measurement frequency of 1 GHz is 4.65 or less, 4.4 or less, 4.35 or less, 4.30 or less, 4.25 or less, or even 4.20 or less, and in some cases 4.18 or less. The dielectric constant at a measurement frequency of 5 GHz is 4.63 or less, 4.4 or less, 4.31 or less, 4.27 or less, 4.22 or less, or even 4.17 or less, and in some cases 4.15 or less. The dielectric constant at a measurement frequency of 10 GHz is 4.55 or less, 4.4 or less, 4.22 or less, 4.18 or less, 4.14 or less, or even 4.08 or less, and in some cases 4.06 or less.
[0059] (Dielectric tangent: tan δ) In a preferred embodiment, the dielectric loss tangent of the glass composition according to the present invention at a measurement frequency of 1 GHz is 0.007 or less, 0.005 or less, 0.004 or less, or even 0.003 or less, and in some cases 0.002 or less. The dielectric loss tangent at a measurement frequency of 1 GHz may be 0.001 or less, less than 0.001, 0.0009 or less, 0.0008 or less, or even 0.0007 or less. The dielectric loss tangent at a measurement frequency of 5 GHz is 0.007 or less, 0.005 or less, 0.004 or less, or even 0.003 or less, and in some cases 0.002 or less. The dielectric loss tangent at a measurement frequency of 10 GHz is 0.007 or less, 0.006 or less, 0.005 or less, 0.004 or less, or even 0.003 or less, and in some cases 0.002 or less.
[0060] (characteristic temperature) In a preferred embodiment, T2 of the glass composition according to the present invention is 1700°C or less, 1650°C or less, 1640°C or less, 1620°C or less, or even 1610°C or less, and in some cases is less than 1600°C, 1550°C or less, or even 1520°C or less, and particularly 1510°C or less. T2 is a temperature that is an indication of the melting temperature of the glass melt. An excessively high T2 requires an extremely high temperature to melt the glass melt, resulting in high energy costs and high costs for equipment that can withstand high temperatures. It is high. At the same temperature, a glass with a lower T2 has a lower viscosity of the melt, so it is effective in clarifying and homogenizing the glass melt, while a glass with a lower T2 can be melted at a lower temperature when melted at the same viscosity, and is suitable for mass production. T2.5 is preferably 1590°C or less, 1550°C or less, or even 1500°C or less, and in some cases 1450°C or less, or even 1400°C or less. T3 is preferably 1450°C or less, 1420°C or less, 1400°C or less, or even 1365°C or less, particularly 1360°C or less, and in some cases 1330°C or less, or even 1300°C or less. T3 is a temperature that is a guideline for the spinning temperature of glass fibers. An excessively high T3 causes a lot of B2O3 to volatilize from the glass at the tip of the bushing, which may adhere to the tip and increase the risk of so-called thread breakage.
[0061] In a preferred embodiment, T3 of the glass composition according to the present invention is higher than the devitrification temperature TL. In a more preferred embodiment, T3 is higher than the TL by 10° C. or more, further 50° C. or more, and in some cases 100° C. or more. In a preferred embodiment, T2.5 of the glass composition according to the present invention is higher than the devitrification temperature TL by 50° C. or more. In a more preferred embodiment, T2.5 is higher than the TL by 100° C. or more. T3 and T2.5 that are sufficiently higher than the TL greatly contribute to the stable production of glass fibers.
[0062] The fifth combination of SiO2 and B2O3 contents is particularly suitable for achieving favorable characteristic temperatures. Preferred characteristic temperatures are, for example, T2 below 1520°C, in particular below 1510°C, and T3 above TL below 1300°C. In the first combination, the glass composition having a Li2O content of 0.25% or more is also , which is suitable for achieving the above-mentioned preferable characteristic temperature.
[0063] [Application] The use of the glass composition according to the present invention is not limited. Examples of the use are glass fiber and glass molded body. An example of the glass molded body is flaky glass. That is, the glass composition of the present invention can be a glass composition for glass fiber, a glass composition for glass molded body, or a glass composition for flaky glass.
[0064] The glass composition according to the present invention is a glass composition that can further suppress the occurrence of devitrification and the inclusion of bubbles in the glass fibers even when the fiber diameter of the glass fibers to be formed is small. Here, "glass fibers having a small fiber diameter" means, for example, glass fibers having an average fiber diameter of 1 to 6 μm. That is, the glass composition according to the present invention can be a glass composition for glass fibers with a small fiber diameter, and more specifically, a glass composition for glass fibers having an average fiber diameter of 1 to 6 μm. In addition, as described above, when the glass fibers produced from the glass composition according to the present invention are used for printed circuit boards, the effect of the present invention becomes more remarkable. From this viewpoint, the glass composition according to the present invention can be a glass composition for glass fibers used for printed circuit boards (printed wiring boards, printed circuit boards).
[0065] Similarly, the glass composition according to the present invention is a glass composition that can further suppress the occurrence of devitrification and the inclusion of bubbles in a glass molded body even when the formed glass molded body, for example, a flake-shaped glass, has a small thickness. Here, "thickness is small" means, for example, 0.1 to 2.0 μm. As described above, the effect of the present invention becomes more remarkable when a glass molded body manufactured from the glass composition of the present invention (a glass molded body composed of the glass composition of the present invention) is used for a printed circuit board. From this viewpoint, the glass composition according to the present invention can be a glass composition for a glass molded body used for a printed circuit board.
[0066] When focusing on use for printed circuit boards, the glass composition according to the present invention can be a glass composition for printed circuit boards.
[0067] [Glass fiber] The glass fiber according to the present invention is composed of the glass composition according to the present invention. The specific composition of the glass fiber is not particularly limited, and as long as it is composed of the glass composition according to the present invention, it can have the same composition as conventional glass fibers. However, as described above, the glass composition according to the present invention is a glass composition with a low dielectric constant, and even when the fiber diameter of the formed glass fiber is small, it is a composition that can further suppress the occurrence of devitrification and the inclusion of bubbles in the glass fiber, so that the glass fiber according to the present invention can be a glass fiber with a small fiber diameter. Moreover, such a glass fiber with a small fiber diameter and a low dielectric constant is one form of the glass fiber according to the present invention.
[0068] The average fiber diameter of the glass fibers may be, for example, 1 to 10 μm, or further 6 to 10 μm, or may be 1 to 6 μm. The average fiber diameter may be 3 μm or more, 10 μm or less, 5.1 μm or less, 4.6 μm or less, or further 4.3 μm or less. A glass composition having a characteristic temperature suitable for mass production is suitable for stable production as a thin glass fiber. In a preferred embodiment, the average fiber diameter is further thinner, for example, 3.9 μm or less, or further 3.5 μm or less. The glass fibers are, for example, long glass fibers (filaments).
[0069] A preferred application of the glass fiber according to the present invention is a printed circuit board. Glass fibers having a low dielectric constant and a small fiber diameter are suitable for use in printed circuit boards. However, the application is not limited to printed circuit boards.
[0070] The glass fiber may be a glass yarn. The glass yarn may contain glass fibers other than the glass fiber of the present invention, but may be composed only of the glass fiber of the present invention, specifically, the long glass fiber. This glass yarn is highly productive because it is suppressed from causing defects such as thread breakage and fluffing of the glass fiber.
[0071] The number of long glass fibers (filament number) contained in the glass yarn is, for example, 30 to 400. When used for a printed circuit board, the number of filaments may be, for example, 30 to 120, 30 to 70, or even 30 to 60. An appropriate number is advantageous in forming the glass cloth more easily and reliably and in making the printed circuit board thinner. However, the configuration and uses of the glass yarn are not limited to these examples.
[0072] The glass yarn containing glass fibers may have a count of, for example, 0.7 to 6 tex, 0.9 to 5 tex, or even 1 to 4 tex, or even 1 to 3 tex, or may be 10 to 70 tex. An appropriate count is advantageous in that a thin glass cloth can be formed more easily and reliably, and a printed circuit board can be made thinner.
[0073] The glass yarn may have a strength of 0.4 N / tex or more, further 0.6 N / tex or more, particularly 0.7 N / tex or more.
[0074] The glass fiber according to the present invention can be produced by applying a known method. For example, when producing glass fibers having an average fiber diameter of about 1 to 6 μm, the following example method can be adopted. That is, the glass composition according to the present invention is charged into a glass melting furnace, melted to form molten glass, and then the molten glass is drawn out from a number of spinning nozzles provided at the bottom of a heat-resistant bushing in a spinning furnace and formed into a filament. In this way, glass fibers composed of the glass composition according to the present invention can be produced. The glass fiber can be a long glass fiber (filament). The melting temperature in the melting furnace is, for example, 1300 to 1700° C., preferably 1400 to 1700° C., and more preferably 1500 to 1700° C. In these cases, even when the fiber diameter of the formed glass fiber is small, the occurrence of minute devitrification and the inclusion of bubbles in the glass fiber can be further suppressed, and the spinning tension can be prevented from becoming excessively high, and the obtained glass fiber can be produced. The properties (e.g. strength) and quality of the fibres can be ensured.
[0075] In order to manufacture glass fibers with a small fiber diameter, it is possible to consider a method of increasing the drawing speed of molten glass from a spinning furnace or decreasing the temperature of a spinning nozzle. However, the former method may not be able to secure enough time to promote degassing of molten glass in a spinning furnace. For this reason, thread breakage during spinning due to the inclusion of bubbles, a decrease in fiber strength, etc. may occur. In addition, the tension (spinning tension) generated in the fiber during spinning increases with an increase in the spinning speed, which may also be a factor in thread breakage during spinning, a decrease in fiber strength, a decrease in fiber quality, etc. Normally, a winding rotor device called a collet is used to wind glass fibers, and if the spinning tension increases excessively, a thread habit due to the recess between the fingers occurs in the wound glass fiber, which leads to a decrease in the quality of the glass fiber. The collet is a device that has a plurality of fingers on the outer periphery of the collet body that move radially outward during rotation and sink into the collet body side when stopped. The deterioration of the quality of the glass fibers may lead to, for example, a poor appearance and / or poor fiber opening in the glass cloth. On the other hand, in the latter method, it is necessary to lower the melting temperature in the melting furnace, which brings the melting temperature closer to the devitrification temperature of the glass composition, and the viscosity of the molten glass may increase, making it impossible to perform sufficient degassing. The increase in viscosity may also increase the spinning tension, which may cause the above-mentioned problems.
[0076] The above problems can be alleviated by using the glass composition according to the present invention and melting it in the above-mentioned temperature range. The improved quality of the glass fiber also improves the appearance and / or spreadability of the glass cloth using the glass fiber.
[0077] A glass strand can be formed by applying a bundling agent to the surface of the glass fiber formed by spinning and bundling a plurality of glass fibers, for example, 10 to 120 glass fibers. This strand contains the glass fiber according to the present invention. The strand is wound up on a tube (for example, a paper tube) on a collet rotating at high speed to form a cake, and then the strand is unwound from the outer layer of the cake, air-dried while being twisted, and then rewound on a bobbin or the like to be twisted, thereby forming a glass yarn.
[0078] [Glass cloth] The glass cloth according to the present invention is composed of the glass fiber according to the present invention. The glass cloth according to the present invention may also have the above-mentioned properties such as a low dielectric constant possessed by the glass composition according to the present invention. The weave structure of the glass cloth according to the present invention is, for example, a plain weave, a satin weave, a twill weave, a basket weave, or a rib weave, and is preferably a plain weave. However, the weave structure is not limited to these examples. The glass yarn may contain glass fibers other than the glass fiber according to the present invention, but may be composed only of the glass fiber according to the present invention, specifically, the long glass fiber. The glass cloth according to the present invention is suppressed in occurrence of defects such as thread breakage and fluffing of the glass fiber, and has high productivity.
[0079] In a preferred embodiment, the thickness of the glass cloth is preferably 200 μm or less, more preferably 7 to 150 μm, even more preferably 7 to 30 μm, and particularly preferably 8 to 15 μm, as measured in accordance with the provisions of item 7.10.1 of JIS R3420: 2013. This preferred embodiment of the glass cloth is suitable for making thin printed circuit boards.
[0080] In a preferred embodiment, the mass of the glass cloth is preferably 250 g / m2, expressed by the cloth mass measured in accordance with the provisions of JIS R3420:2013, item 7.2. 2 Less than 150 g / m 2 Less than 50 g / m, more preferably 50 g / m 2 , particularly preferred Approximately 15g / m 2 The preferred embodiment of the glass cloth is a thin-walled prism. Suitable for use on PCBs.
[0081] In a preferred embodiment, the number of glass fibers (weave density) per unit length (25 mm) of the glass cloth is, for example, preferably 40 to 130, more preferably 60 to 120, and even more preferably 90 to 120 per 25 mm length for both warp and weft. The glass cloth of this preferred embodiment is suitable for reducing the thickness and increasing the number of intertwining points of the warp and weft to prevent the glass cloth from bending and suppressing the generation of pinholes when impregnated with resin.
[0082] In a preferred embodiment, the air permeability of the glass cloth is, for example, 400 cm 3 / (cm 2 sec) or less, preferably 300 cm 3 / (cm 2 ·sec) or less, preferably 250 cm 3 / (cm 2 The preferred embodiment of the glass cloth has a small thickness and In order to open the glass cloth so that it has the above-mentioned degree of air permeability, it is preferable to obtain glass fibers by applying the above-mentioned melting temperature, i.e., 1400° C. or higher, preferably 1400 to 1650° C., to the glass composition according to the present invention or a glass raw material prepared to obtain the glass composition according to the present invention.
[0083] The glass cloth according to the present invention can be produced by a known method using the glass fiber according to the present invention. One example of the production method is a method in which a glass yarn is subjected to a warping process and a sizing process, and then the warp yarn is used to drive a glass yarn weft. Various looms, such as a jet loom, a Sulzer loom, and a rapier loom, can be used to drive the weft. Specific examples of jet looms include an air jet loom and a water jet loom. However, the looms used to produce the glass cloth are not limited to these.
[0084] The glass cloth according to the present invention may be subjected to a fiber-opening treatment. The fiber-opening treatment is advantageous for making the glass cloth thinner. The specific method of the fiber-opening treatment is not particularly limited, and for example, fiber-opening by the pressure of a water flow, fiber-opening by high-frequency vibration using water or the like as a medium, and fiber-opening by pressure using a roll or the like can be applied. As the water used as the medium for fiber-opening, deaerated water, ion-exchanged water, deionized water, electrolytic cation water, electrolytic anion water, etc. can be used. The fiber-opening treatment may be carried out simultaneously with the weaving of the glass cloth or after the weaving. The fiber-opening treatment may be carried out simultaneously with various treatments such as heat cleaning and surface treatment, or after various treatments.
[0085] When a substance such as a sizing agent is attached to the woven glass cloth, a removal treatment of the substance, typically a heat cleaning treatment, may be further carried out. The glass cloth that has been subjected to the removal treatment has excellent impregnation with a matrix resin and adhesion to the resin when used for a printed circuit board. After the removal treatment, or separately from the removal treatment, the woven glass cloth may be surface-treated with a silane coupling agent or the like. The surface treatment can be carried out by a known means, specifically, by a method of impregnating, applying, or spraying the silane coupling agent into the glass cloth.
[0086] The glass cloth according to the present invention is suitable for printed circuit boards. When used for printed circuit boards, the characteristics of the glass cloth, such as a low dielectric constant and the ability to be made of glass fibers with a small fiber diameter, can be effectively utilized. However, the application is not limited to printed circuit boards.
[0087] [Prepreg] The prepreg according to the present invention may be composed of the glass cloth according to the present invention. The prepreg according to the present invention may also have the above-mentioned properties such as a low dielectric constant possessed by the glass composition according to the present invention. The method for producing the prepreg according to the present invention is not particularly limited, and any conventionally known production method may be adopted. The resin impregnated into the prepreg according to the present invention is not particularly limited as long as it is a synthetic resin that can be compounded with the glass cloth of the present invention, and examples thereof include thermosetting resins, thermoplastic resins, etc. Resins having a low dielectric constant suited to the glass cloth according to the present invention having a low dielectric constant can be used.
[0088] [Printed circuit board] The printed circuit board according to the present invention may be made of the glass cloth according to the present invention. The printed circuit board according to the present invention may also have the above-mentioned properties such as a low dielectric constant possessed by the glass composition according to the present invention. The method for producing the substrate of the present invention is not particularly limited, and any conventionally known manufacturing method may be adopted. For example, a method in which a prepreg containing a resin impregnated in a glass cloth is produced and then cured may be mentioned. EXAMPLES
[0089] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0090] Glass raw materials were weighed to obtain each composition shown in Tables 1 to 6 (the unit of the content of the components is weight %), and mixed to obtain a homogeneous state to prepare a glass raw material mixed batch. Next, the prepared mixed batch was put into a platinum-rhodium crucible, and heated in an indirect heating electric furnace set at 1600°C in an air atmosphere for 3 hours or more to obtain molten glass. Next, the obtained molten glass was poured into a refractory mold for casting, and the obtained molded body was slowly cooled to room temperature in a slow cooling furnace to obtain a glass composition sample to be used for evaluation.
[0091] The glass samples thus prepared were evaluated for characteristic temperatures T2, T2.5 and T3, devitrification temperature TL, and dielectric constant and dielectric loss tangent at frequencies of 1 GHz, 5 GHz and 10 GHz. The evaluation method was as follows.
[0092] (characteristic temperature) The viscosity was measured using the platinum ball pull method, and the viscosity was 10 2 dPa·s, 10 2.5 dPa·s, 10 3 The temperatures at which the viscosity becomes dPa·s were defined as T2, T2.5, and T3, respectively.
[0093] (devitrification temperature) The sample glass was crushed, passed through a sieve with 2.83 mm openings, and the particles remaining on a sieve with 1.00 mm openings were sieved out. The particles were washed to remove fine powder adhering to the particles, and then dried to prepare a sample for measuring the devitrification temperature. 25 g of the sample for measuring the devitrification temperature was placed in a platinum boat (a rectangular platinum vessel without a lid) so that the thickness was approximately uniform, and after being held in a temperature gradient furnace for 2 hours, it was removed from the furnace, and the maximum temperature at which devitrification was observed inside the glass was taken as the devitrification temperature.
[0094] (Dielectric constant and dielectric loss tangent) The dielectric constant and dielectric loss tangent at each frequency were measured using a dielectric constant measuring device using a cavity resonator perturbation method. The measurement temperature was 25°C, and the dimensions of the measurement sample were a rectangular parallelepiped with a base of 1.5 cm on each side and a length of 10 cm.
[0095] The glass compositions of Examples 1 to 44 and 48 to 99 had a dielectric constant of 4.65 or less at a measurement frequency of 1 GHz, a T2 of 1700°C or less, and a T3 of 1450°C or less. Some of these glass compositions had a dielectric constant of 4.4 or less at a measurement frequency of 1 GHz, and the glass compositions of Examples 1 to 43, 48 to 81, 83 to 84, and 93 to 99 had a dielectric constant of 4.36 or less at a measurement frequency of 1 GHz. The glass compositions of Examples 1 to 41, 48 to 81, 83 to 84, and 94 to 99 had a dielectric constant of 4.35 or less at a measurement frequency of 1 GHz. In addition, the glass compositions of Examples 5 to 6, 66 to 67, and 83 to 92 had a T2 of 1520°C or less, and a T3 of 1300°C or less, which was higher than TL. The glass compositions of Examples 66 to 67 and Examples 83 to 92 have a B2O3 content of 35% or less, and in some cases 30% or less, and T2 The dielectric constant at a frequency of 1 GHz was less than 0.001, and T2 was less than 1600°C. The glass compositions of Examples 45 to 47 are comparative examples, and Example 45 had a T2 value exceeding 1700°C, and Examples 46 to 47 had a dielectric constant exceeding 4.7 at a measurement frequency of 1 GHz.
[0096] [Table 1]
[0097] [Table 2]
[0098] [Table 3]
[0099] [Table 4]
[0100] [Table 5]
[0101] [Table 6]
Claims
1. Expressed in weight percent, 40≦SiO 2 ≦60 30≦B 2 O 3 ≦45 5≦Al 2 O 3 ≦15 0<R 2 O≦5 1.5≦RO<15 Including, SiO 2 +B 2 O 3 ≧80, and / or SiO 2 +B 2 O 3 ≧78 and 1.5≦RO<10 The glass composition for glass fiber, However, R 2 O is Li 2 O, Na 2 O and K 2 RO is at least one oxide selected from MgO, CaO and SrO.
2. Expressed in weight percent, 40≦SiO 2 ≦60 30≦B 2 O 3 ≦45 5≦Al 2 O 3 ≦15 0<R 2 O≦5 0.01≦Li 2 O≦1.5 1.5≦RO<15 Including, SiO 2 +B 2 O 3 ≧80, and / or SiO 2 +B 2 O 3 ≧78 and 1.5≦RO<10 The glass composition according to claim 1, However, R 2 O is Li 2 O, Na 2 O and K 2 RO is at least one oxide selected from MgO, CaO and SrO.
3. Expressed in weight percent, SiO 2 +B 2 O 3 ≧81、 (SiO 2 +B 2 O 3 +Al 2 O 3 ) / (SiO 2 +B 2 O 3 ) ≧1.13; The dielectric constant at a frequency of 1 GHz is 4.4 or less, The dielectric tangent at a frequency of 1 GHz is 0.007 or less, Viscosity 10 2 The temperature T2 at which the viscosity becomes dPas is 1700° C. or less, Viscosity 10 3 The temperature T3 at which the viscosity becomes dPas is 1365° C. or lower, The glass composition for glass fiber.
4. Expressed in weight percent, 40≦SiO 2 ≦49.95 27≦B 2 O 3 ≦45 <h2 style=";text-align:left;direction:ltr">0<Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> ≦18 0<R 2 O≦5 3<RO<10 Including, 0.2≦MgO≦5 1≦CaO<10 0.1≦MgO / (MgO+CaO)≦0.5, SiO 2 + B 2 O 3 ≥ 75, and SiO 2 + B 2 O 3 + Al 2 O 3 < 97 The glass composition according to claim 1, However, R 2 O is Li 2 O, Na 2 O and K 2 RO is at least one oxide selected from MgO, CaO and SrO.
5. Expressed in weight percent, 45≦SiO 2 <58 25≦B 2 O 3 ≦40 7.5≦Al 2 O 3 ≦18 0<R 2 O≦4 0≦Li 2 O≦1.5 0≦Na 2 O≦1.5 0≦K 2 O≦1 1≦RO<10 0≦MgO<10 0≦CaO<10 0≦SrO≦5 0≦T-Fe 2 O 3 ≦0.5 0≦ZnO≦1 Including, SiO 2 +B 2 O 3 ≧80, and 0.1≦MgO / (MgO+CaO)≦0.5 is satisfied, TiO 2 A glass composition for glass fibers, which is substantially free of However, R 2 O is Li 2 O, Na 2 O and K 2 O, RO is at least one oxide selected from MgO, CaO and SrO, and T-Fe 2 O 3 is Fe 2 O 3 The total iron oxide in the glass composition is calculated as
6. 5. The glass composition according to claim 2, which is for glass fibers.
7. A glass fiber comprising the glass composition according to any one of claims 1 to 6.
8. A glass cloth made from the glass fiber according to claim 7.
9. A prepreg comprising the glass cloth according to claim 8.
10. A printed circuit board comprising the glass cloth according to claim 8.
11. A method for producing glass fibers, comprising the step of melting the glass composition according to any one of claims 1 to 6 at a temperature of 1400°C or higher to obtain glass fibers having an average fiber diameter of 1 to 6 µm.
Citation Information
Patent Citations
Glass fiber having low dielectric constant
JP1987226839A
Glass fiber having low dielectric loss tangent
JP1997002839A
Glass fiber and method for manufacturing the same
JP2020093959A
Glass composition, glass fiber, glass cloth, and method for manufacturing glass fiber
WO2017187471A1
Glass composition, glass fiber, glass cloth, and method for manufacturing glass fiber
WO2018216637A1