Surface treatment liquid, surface treatment method of nickel-containing layer, and method for manufacturing nickel-containing layer
A surface treatment liquid with ferrous and ferric ions, hydrogen chloride, and other compounds addresses smut and pinhole issues in nickel-containing layers, enhancing adhesion and etching stability.
Patent Information
- Application Number
- JP2023063309
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
AI Technical Summary
Existing surface treatment agents for nickel-containing layers, such as Invar material and austenitic stainless steel, fail to effectively suppress the formation of smut and pinholes, and improve adhesion with resist patterns, leading to potential peeling and device performance degradation.
A surface treatment liquid containing ferrous and ferric ions, hydrogen chloride, triammonium citrate, and other compounds in an aqueous solution is used to treat nickel-containing layers, effectively suppressing smut and pinhole formation while removing surface oxide films.
The treatment liquid significantly reduces smut and pinhole formation, enhances adhesion between the nickel-containing layer and resist patterns, and improves device performance by ensuring stable etching processes.
Smart Images

Figure 2024150077000001 
Figure 2024150077000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface treatment solution, a surface treatment method for a nickel-containing layer, and a method for producing a nickel-containing layer. [Background technology]
[0002] The nickel-containing layer is used in precision electronic components such as printed wiring boards, lead frames, connector terminals, and package substrates, as well as high-definition display components such as shadow masks, etc. Among these, Invar is preferably used for these components, etc., because of its small thermal expansion coefficient.
[0003] There is a known technology for forming fine lines by processing a metal material on which a resist pattern has been formed using a wet etching method. In the wet etching method, fine powder-like foreign matter called "smut" may be formed on the surface of the metal material, which may reduce the adhesion between the metal material and the resist pattern. In addition, a natural oxide film may be formed on the surface of the nickel-containing layer, which may reduce device performance. Therefore, a method has been developed for treating the surface of the metal material using a surface treatment liquid to suppress the formation of smut and improve the adhesion between the metal material and the resist pattern, as well as a method for removing the surface oxide film.
[0004] For example, Patent Document 1 discloses a surface treatment agent containing hydrogen peroxide, a mineral acid, an azole, silver ions, and halogen ions as a surface treatment agent for improving the adhesion between a copper-plated substrate and a dry film resist. Patent Document 2 discloses a surface treatment agent for copper or copper alloys containing a nitrogen-containing heterocyclic compound and an acid such as an inorganic acid or an organic acid. Patent Document 3 discloses a surface treatment liquid for silicon substrates containing sulfuric acid and ammonium fluoride. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-003283 A [Patent Document 2] JP 2008-045156 A [Patent Document 3] Japanese Patent Application Publication No. 9-246255 Summary of the Invention [Problem to be solved by the invention]
[0006] The surface treatment agents disclosed in Patent Documents 1 and 2 were effective to some extent for copper. However, even if these surface treatment agents were applied to nickel-containing layers such as Invar materials and austenitic stainless steel, it was difficult to suppress the formation of smut, and the adhesion between the nickel-containing layer and the resist pattern after wet etching could not be improved. If the adhesion between the substrate such as the nickel-containing layer and the resist pattern is low, the resist pattern is easily peeled off, making it difficult to form fine wiring according to the resist pattern. In addition, when the surface treatment liquid containing sulfuric acid disclosed in Patent Document 3 is applied to the nickel-containing layer, pinholes are easily generated, and device performance may be reduced.
[0007] For this reason, there has been a demand for a surface treatment liquid that can suppress the formation of smut and the occurrence of pinholes, and can also remove a native oxide film to improve adhesion between a nickel-containing layer and a resist pattern, and in particular, a surface treatment liquid that can suppress the occurrence of pinholes.
[0008] The present invention has been made to solve these problems, and an object of the present invention is to provide a surface treatment liquid for a nickel-containing layer that can suppress the formation of smut and the occurrence of pinholes while removing a surface oxide layer. Another object of the present invention is to provide a surface treatment method for a nickel-containing layer using the surface treatment liquid, and a method for producing a surface-treated nickel-containing layer. [Means for solving the problem]
[0009] As a result of extensive investigations, the present inventors have found that an aqueous solution containing a specific component can solve the above problems, and have completed the present invention.
[0010] That is, according to the present invention, there is provided a surface treatment liquid used for treating the surface of a nickel-containing layer, the surface treatment liquid being an aqueous solution containing: (A) 0.5 to 15 mass % of at least one component selected from the group consisting of ferrous ions and ferric ions; (B) 0.01 to 0.4 mass % of hydrogen chloride; (C) 1 to 20 mass % of at least one compound selected from the group consisting of triammonium citrate, ammonium lactate, ammonium formate, diammonium hydrogen citrate, ammonium glycolate, and diammonium malate; and water.
[0011] The present invention also provides a method for treating the surface of a nickel-containing layer, comprising the step of contacting the surface of the nickel-containing layer with the above-mentioned surface treatment liquid.
[0012] Furthermore, according to the present invention, there is provided a method for producing a surface-treated nickel-containing layer, comprising the step of contacting the surface of a nickel-containing layer with the above-mentioned surface treatment liquid. Effect of the Invention
[0013] According to the present invention, it is possible to provide a surface treatment liquid for a nickel-containing layer that can suppress the formation of smut and the occurrence of pinholes while removing a surface oxide layer. Also, according to the present invention, it is possible to provide a surface treatment method for a nickel-containing layer using the above surface treatment liquid, and a method for producing a surface-treated nickel-containing layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The following is a detailed description of an embodiment of the present invention. The surface treatment liquid according to one embodiment of the present invention is a liquid composition used to treat the surface of a nickel-containing layer, and is an aqueous solution containing: (A) 0.5 to 15 mass% of at least one component selected from the group consisting of ferrous ions and ferric ions; (B) 0.01 to 0.4 mass% of hydrogen chloride; (C) 1 to 20 mass% of at least one compound selected from the group consisting of triammonium citrate, ammonium lactate, ammonium formate, diammonium hydrogen citrate, ammonium glycolate, and diammonium malate; and water.
[0015] In this specification, the term "nickel-containing layer" refers to a metal material containing at least 1% by mass of nickel. Examples of the nickel-containing layer include nickel alone; low thermal expansion iron-nickel alloys (also called "Invar materials") such as Fe-Ni36%, Fe-Ni32%-Co5%, Fe-Ni29%-Co17%, Fe-Ni42%-Cr-Ti, and Ni-Mo28%-Fe2%; austenitic stainless steels such as SUS301, SUS304, and SUS316; copper-nickel alloys such as cupronickel and nickel silver; nickel-titanium alloys; nickel-zinc alloys; nickel-chromium alloys; and nickel-cobalt alloys. As the nickel-containing layer to be the surface-treated body, the above-mentioned Invar materials and stainless steel are preferable, and Invar materials are particularly preferable.
[0016] The surface treatment liquid contains at least one component (A) selected from the group consisting of ferrous ions and ferric ions (hereinafter, also referred to as "component (A)"). The component (A) may be any compound capable of supplying (generating) at least one component selected from the group consisting of ferrous ions and ferric ions to the surface treatment liquid. An iron (II) compound can be used as a source of ferrous ions. Examples of iron (II) compounds include iron chloride (II), iron bromide (II), iron iodide (II), iron sulfate (II), iron nitrate (II), and iron acetate (II). Examples of iron (III) compounds can be used as a source of ferric ions. Examples of iron (III) compounds include iron chloride (III), iron bromide (III), iron iodide (III), iron sulfate (III), iron nitrate (III), and iron acetate (III).
[0017] As the supply source of component (A), iron chloride (II) or iron chloride (III) is preferred because it can more effectively suppress the formation of smut and the generation of pinholes and can more effectively remove the surface oxide film, which is a natural oxide film, and it is particularly preferred to use iron chloride (II) and iron chloride (III) in combination. The supply source of component (A) may be either anhydrous or hydrated.
[0018] The concentration of component (A) in the surface treatment liquid is 0.5 to 15% by mass. Since this can more effectively suppress the formation of smut and the occurrence of pinholes and can more effectively remove natural oxide films, the concentration of component (A) in the surface treatment liquid is preferably 1 to 10% by mass, and more preferably 2 to 6% by mass. The "concentration of component (A)" refers to the concentration of at least one component selected from the group consisting of ferrous ions and ferric ions. For example, in the case of a surface treatment liquid containing 10% by mass of iron (II) chloride, the concentration of component (A) is about 4.4% by mass.
[0019] The surface treatment solution contains (B) hydrogen chloride (hereinafter also referred to as "component (B)"). The source of hydrogen chloride may be either concentrated hydrochloric acid or dilute hydrochloric acid. Commercially available hydrochloric acid may be used as is or after appropriate dilution.
[0020] The concentration of component (B) in the surface treatment liquid is 0.01 to 0.4% by mass. The concentration of component (B) in the surface treatment liquid is 0.05 to 0.3% by mass, and more preferably 0.1 to 0.25% by mass, in order to more effectively suppress the formation of smut and the occurrence of pinholes and to more effectively remove a native oxide film.
[0021] The surface treatment liquid contains (C) at least one compound selected from the group consisting of triammonium citrate, ammonium lactate, ammonium formate, diammonium hydrogen citrate, ammonium glycolate, and diammonium malate (hereinafter also referred to as "component (C)"). As component (C), a commercially available product can be used. It is particularly preferable that component (C) is triammonium citrate, since this can more effectively suppress the formation of smut and the occurrence of pinholes, and can more effectively remove a natural oxide film.
[0022] The concentration of component (C) in the surface treatment liquid is 1 to 20% by mass. The concentration of component (C) in the surface treatment liquid is preferably 3 to 17% by mass, and particularly preferably 5 to 14% by mass, because this makes it possible to more effectively suppress the formation of smut and the occurrence of pinholes and to more effectively remove a native oxide film.
[0023] The surface treatment solution preferably further contains (D) a nickel compound (hereinafter also referred to as "component (D)"). By containing component (D), the formation of smut and the occurrence of pinholes can be more effectively suppressed, and the native oxide film can be more effectively removed.
[0024] Examples of the component (D) (nickel compound) include nickel halides such as nickel chloride (II), nickel fluoride (II), and nickel bromide (II), and nickel salts such as nickel sulfate (II) and nickel nitrate (II). The concentration of the component (D) in the surface treatment liquid is preferably 0.01 to 5 mass%, more preferably 0.1 to 3 mass%, and particularly preferably 0.3 to 2 mass%.
[0025] The surface treatment liquid is an aqueous solution in which each component is dissolved in water. Therefore, the surface treatment liquid contains water as a solvent. The amount of water in the surface treatment liquid is preferably the remainder depending on the concentrations of the above-mentioned components (A) to (C) and the component (D) used as necessary. When additives, etc. described below are used, the content of water in the surface treatment liquid is preferably the remainder depending on the concentrations of the components (A) to (D) and the additives, etc. The content of water in the surface treatment liquid is preferably about 60 to 99 mass%.
[0026] In addition to the above-mentioned components and water, the surface treatment liquid may further contain well-known additives within a range that does not impair the effects of the present invention. Examples of the additives include stabilizers, solubilizers for each component, antifoaming agents, pH adjusters, specific gravity adjusters, viscosity adjusters, wettability improvers, chelating agents, oxidizing agents, reducing agents, and surfactants. The concentrations of these additives are generally in the range of 0.001 to 10% by mass.
[0027] The surface treatment method of a nickel-containing layer according to one embodiment of the present invention (hereinafter, also simply referred to as the "surface treatment method") includes a step of contacting the surface of the nickel-containing layer with the above-mentioned surface treatment liquid. By contacting the surface with the surface treatment liquid to perform surface treatment, it is possible to obtain a nickel-containing layer that can be etched while suppressing the formation of smut and the occurrence of pinholes. The method of contacting the surface of the nickel-containing layer with the surface treatment liquid is not particularly limited, and a general pretreatment method can be adopted. Specifically, the surface treatment liquid can be contacted with the surface of the nickel-containing layer by a pretreatment method such as a dip type, a spray type, or a spin type.
[0028] When the surface of the nickel-containing layer is treated by the dipping method, the nickel-containing layer may be immersed for about 1 to 600 seconds in a surface treatment solution adjusted to a temperature range of, for example, 10 to 90° C. When the surface of the nickel-containing layer is treated by the spraying method, the surface treatment solution adjusted to a temperature range of, for example, 10 to 90° C. may be sprayed onto the surface of the nickel-containing layer at a pressure range of 0.01 to 1.0 MPa.
[0029] The surface of the nickel-containing layer is treated by contacting the surface with a surface treatment solution, and then washed with pure water and dried. Next, a resist pattern is formed on the surface of the nickel-containing layer by a conventional method, and then the layer is etched with an etching solution, whereby fine wiring having good adhesion to the resist pattern can be formed.
[0030] The above-mentioned surface treatment liquid and the surface treatment method using this surface treatment liquid can be suitably used, for example, when processing nickel-containing layers for electrodes and wiring of devices such as liquid crystal displays, plasma displays, touch panels, organic EL devices, solar cells, and lighting fixtures.
[0031] <Other> The disclosure of this embodiment includes the following aspects. [1] A surface treatment solution used to treat a surface of a nickel-containing layer, comprising: (A) 0.5 to 15 mass % of at least one component selected from the group consisting of ferrous ions and ferric ions; (B) 0.01 to 0.4 mass% hydrogen chloride; (C) 1 to 20% by mass of at least one compound selected from the group consisting of triammonium citrate, ammonium lactate, ammonium formate, diammonium hydrogen citrate, ammonium glycolate, and diammonium malate; and The surface treatment solution is an aqueous solution containing water. [2] The surface treatment solution according to [1], wherein the nickel-containing layer is an Invar material. [3] (D) The surface treatment liquid according to [1] or [2], further comprising 0.01 to 5 mass % of a nickel compound. [4] A surface treatment method for a nickel-containing layer, comprising the step of contacting a surface of the nickel-containing layer with the surface treatment liquid according to any one of [1] to [3]. [5] A method for producing a surface-treated nickel-containing layer, comprising a step of contacting a surface of a nickel-containing layer with the surface treatment liquid according to any one of [1] to [3]. EXAMPLES
[0032] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited thereto.
[0033] <Component (A)> As the component (A), the following a-1 and a-2 were prepared. a-1: Iron(II) chloride a-2: Iron(III) chloride
[0034] <(B) component> As component (B) and its comparative components, b-1 and b-2 shown below were prepared. b-1: Hydrogen chloride b-2: Sulfuric acid
[0035] <(C) component> As component (C) and its comparative components, c-1 to c-6 shown below were prepared. C-1: Triammonium citrate C-2: Ammonium lactate C-3: Ammonium formate C-4: Diammonium hydrogen citrate C-5: Ammonium sulfate C-6: Citric acid
[0036] <(D) component> As component (D), d-1 shown below was prepared. d-1: Nickel(II) chloride
[0037] <Surface treatment liquid> (Examples 1 to 8 and Comparative Examples 1 to 4) The components were mixed to obtain the compositions shown in Table 1, to obtain treatment solutions Nos. 1 to 8 and comparative treatment solutions 1 to 4. In Table 1, the concentration of component (A) represents the concentration of ferrous ions and ferric ions, and the concentration of component (B) represents the concentration of hydrogen chloride or sulfuric acid. Water was added so that the total of the components was 100 mass %.
[0038] TIFF2024150077000001.tif184170
[0039] <Surface treatment of nickel-containing layer> Example 9 An Fe-Ni 36% foil (hereinafter also referred to as "(untreated) substrate") having a length of 100 mm, width of 100 mm, and thickness of 0.030 mm was prepared. Treatment solution No. 1 was sprayed on the surface of the substrate by a spray method under conditions of 35°C and a spray pressure of 0.1 MPa, and then the substrate was washed successively with 3 mass% hydrochloric acid and ion-exchanged water. A resist pattern with a line / space of 10 μm / 10 μm was formed at 30 locations on the substrate using a dry film resist. Next, a ferric chloride-based pattern etching solution (trade name "ADEKA CHELMIC IN-654", manufactured by ADEKA Corporation) was sprayed (50°C, 150 seconds) under conditions of a spray pressure of 0.1 MPa to perform etching, and then the substrate was washed successively with 3 mass% hydrochloric acid and ion-exchanged water to obtain Example substrate No. 1.
[0040] (Examples 10 to 16) Example substrates Nos. 2 to 8 were obtained in the same manner as in Example 9 above, except that Treatment Liquid No. 1 was replaced with Treatment Liquid Nos. 2 to 8, respectively.
[0041] (Comparative Examples 5 to 8) Comparative Example Substrates 1 to 4 were obtained in the same manner as in Example 9 above, except that Comparative Treatment Solutions 1 to 4 were used, respectively, instead of Treatment Solution No. 1.
[0042] <Evaluation Examples 1 to 8 and Comparative Evaluation Examples 1 to 4> (Smut rating) The maximum thicknesses of smut precipitated on the surfaces of Example Substrates Nos. 1 to 8 and Comparative Substrates Nos. 1 to 4 were measured using an X-ray photoelectron spectrometer and evaluated according to the following evaluation criteria. The results are shown in Table 2. +++: Maximum thickness of smut is less than 10 nm ++: The maximum thickness of smut is 10 nm or more and less than 30 nm +: Maximum thickness of smut is 30nm or more and less than 50nm -: Maximum thickness of smut is 50nm or more and less than 100nm --: Maximum thickness of smut is 100nm or more and less than 300nm ---: Maximum thickness of smut is 300 nm or more
[0043] (Pinhole evaluation) Surface 1 cm of Example Substrates Nos. 1 to 8 and Comparative Substrates Nos. 1 to 4 2 The range was observed and the number of pinholes was evaluated according to the following evaluation criteria. The results are shown in Table 2. +++: Fewer than 10 pinholes with a diameter of 3 μm or more were observed. ++: 10 or more but less than 30 pinholes having a diameter of 3 nm or more were observed. +: 30 to less than 50 pinholes with a diameter of 3 nm or more were observed. -: Between 50 and 70 pinholes with a diameter of 3 nm or more were observed. --: Between 70 and 100 pinholes with a diameter of 3 nm or more were observed. ---: More than 100 pinholes with a diameter of 3 nm or more were observed.
[0044] (Evaluation of surface oxide film) Using an X-ray photoelectron spectrometer, the presence or absence of an oxide film on the surfaces of Example Substrates Nos. 1 to 8 and Comparative Example Substrates 1 to 4 was confirmed and evaluated according to the following evaluation criteria. The results are shown in Table 2. +++: No surface oxide film ---: Surface oxide film present
[0045] TIFF2024150077000002.tif103170
[0046] As shown in Table 2, it can be seen that the occurrence of pinholes is sufficiently suppressed in Example Substrates Nos. 1 to 8 compared to Comparative Example Substrates 1 to 4. Furthermore, it can be seen that the formation of smut is sufficiently suppressed in Example Substrates Nos. 1 to 8 compared to Comparative Example Substrates 2 and 3, and the surface oxide film is sufficiently removed.
[0047] As described above, according to the present invention, it is possible to provide a surface treatment liquid capable of suppressing the formation of smut and the occurrence of pinholes when etching a nickel-containing layer and capable of removing a surface oxide film, a surface treatment method for a nickel-containing layer, and a manufacturing method for a nickel-containing layer.
Claims
1. A surface treatment solution used to treat a surface of a nickel-containing layer, comprising: (A) 0.5 to 15 mass % of at least one component selected from the group consisting of ferrous ions and ferric ions; (B) 0.01 to 0.4% by mass of hydrogen chloride; (C) 1 to 20% by mass of at least one compound selected from the group consisting of triammonium citrate, ammonium lactate, ammonium formate, diammonium hydrogen citrate, ammonium glycolate, and diammonium malate; and The surface treatment solution is an aqueous solution containing water.
2. 2. The surface treatment solution according to claim 1, wherein the nickel-containing layer is an Invar material.
3. The surface treatment solution according to claim 1, further comprising (D) 0.01 to 5 mass % of a nickel compound.
4. A surface treatment method for a nickel-containing layer, comprising a step of contacting the surface of the nickel-containing layer with the surface treatment liquid according to any one of claims 1 to 3.
5. A method for producing a surface-treated nickel-containing layer, comprising a step of contacting the surface of a nickel-containing layer with the surface treatment liquid according to any one of claims 1 to 3.
Citation Information
Patent Citations
Surface treating liquid for semiconductor device and wet processing of semiconductor device
JP1997246255A
Surface treatment agent for copper and copper alloy
JP2003003283A
Surface treatment agent for copper or copper alloy surface, and treatment method thereof
JP2008045156A