Material for forming organic film, substrate for manufacturing semiconductor device, method for forming organic film, patterning method, and compound
The organic film forming material with a specific compound and solvent combination addresses the challenges of heat resistance and planarization in semiconductor manufacturing, enhancing device yield and process reliability.
Patent Information
- Application Number
- JP2023063361
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2043-04-10
AI Technical Summary
Existing semiconductor manufacturing processes face challenges in achieving high integration and speed without relying on miniaturization, as conventional organic film forming materials lack sufficient heat resistance, adhesion, and planarization properties, especially under inert gas conditions, leading to corrosion and reduced yield.
An organic film forming material containing a specific organic compound represented by general formula (1A) and an organic solvent, which can be cured in both air and inert gas conditions, providing high heat resistance, good adhesion, and advanced embedding/planarization properties.
The material enables the formation of organic films with excellent heat resistance and planarization, preventing substrate corrosion and improving the yield of semiconductor devices by ensuring uniform film thickness and pattern transfer accuracy.
Smart Images

Figure 2024150107000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a material for forming an organic film, a substrate for manufacturing a semiconductor device using the material, a method for forming an organic film, a pattern formation method by a multilayer resist method, and a compound that can be suitably used for the material. [Background technology]
[0002] Conventionally, the high integration and high speed of semiconductor devices have been achieved by miniaturizing the pattern dimensions by shortening the wavelength of the light source in the lithography technology (photolithography) using light exposure as a general-purpose technology. In order to form such fine circuit patterns on a substrate for manufacturing a semiconductor device (substrate to be processed), a method is used in which the substrate to be processed is processed by dry etching using a photoresist film on which a pattern is usually formed as an etching mask. However, in reality, there is no dry etching method that can achieve perfect etching selectivity between the photoresist film and the substrate to be processed, so in recent years, substrate processing using a multilayer resist method has become common. In this method, an intermediate film having an etching selectivity different from that of the photoresist film (hereinafter also referred to as the resist upper layer film) is interposed between the resist upper layer film and the substrate to be processed, and after obtaining a pattern on the resist upper layer film, the pattern is transferred to the intermediate film by dry etching using the resist upper layer film pattern as a dry etching mask, and the pattern is further transferred to the substrate to be processed by dry etching using the intermediate film as a dry etching mask.
[0003] One of the multilayer resist methods is a three-layer resist method that can be performed using a general resist composition used in a single-layer resist method. In this method, an organic underlayer film (hereinafter also referred to as an organic film) is formed on a substrate to be processed by applying and baking an organic underlayer film material (hereinafter also referred to as an organic film) made of an organic resin-containing composition, and a silicon-containing film (hereinafter also referred to as a silicon-containing resist intermediate film) is formed on the organic underlayer film by applying and baking a resist intermediate film material (hereinafter also referred to as a silicon-containing resist intermediate film) made of a silicon-containing resin-containing composition on the organic underlayer film, and a general organic photoresist film (resist upper layer film) is formed on the resist intermediate film. After patterning the resist upper layer film, dry etching with fluorine-based gas plasma is performed, and since the organic resist upper layer film can have a good etching selectivity to the silicon-containing resist intermediate film, the resist upper layer film pattern can be transferred to the silicon-containing resist intermediate film. According to this method, even if a resist top layer film that does not have a sufficient thickness to directly process a substrate to be processed or a resist top layer film that does not have sufficient dry etching resistance to process a substrate to be processed is used, the silicon-containing resist intermediate film usually has a thickness equal to or less than that of the resist top layer film, so that the pattern can be easily transferred to the silicon-containing resist intermediate film. Then, by using the silicon-containing resist intermediate film to which the pattern has been transferred as a dry etching mask and transferring the pattern to an organic film by dry etching with oxygen-based or hydrogen-based gas plasma, the pattern can be transferred to an organic film that has sufficient dry etching resistance to process the substrate. This organic film pattern that has been transferred to the pattern can be transferred to a substrate by dry etching using a fluorine-based gas or a chlorine-based gas.
[0004] On the other hand, miniaturization in the manufacturing process of semiconductor devices is approaching an essential limit due to the wavelength of the light source for photolithography. Therefore, in recent years, high integration of semiconductor devices without relying on miniaturization has been considered, and as one of the methods, semiconductor devices having complex structures such as multi-gate structures have been considered, and some have already been put to practical use. When such a structure is formed by a multi-layer resist method, it is possible to apply an organic film forming material that can fill micropatterns such as holes, trenches, and fins formed on a substrate to be processed with a film without gaps, or fill steps, densely patterned areas, and areas without patterns with a film to perform planarization. By forming a flat organic film surface on a stepped substrate using such an organic film forming material, it is possible to suppress the film thickness fluctuation of the silicon-containing resist intermediate film and resist top layer film formed thereon, and to suppress the focal tolerance of photolithography and the margin reduction in the subsequent processing process of the substrate to be processed. This makes it possible to manufacture semiconductor devices with a high yield. On the other hand, in the single-layer resist method, in order to fill in steps or patterns on a processed substrate, the thickness of the top-layer resist film must be thick, which can lead to pattern collapse after exposure and development, or deterioration of the pattern shape due to reflection from the substrate during exposure, etc., and this narrows the pattern formation tolerance during exposure, making it difficult to manufacture semiconductor devices with a good yield.
[0005] Furthermore, as a method for increasing the speed of next-generation semiconductor devices, the application of precision materials such as new materials with high electron mobility using, for example, strained silicon or gallium arsenide, and ultra-thin polysilicon controlled in angstrom units has begun to be considered. However, in the case of a substrate to be processed to which such a new precision material is applied, the material is corroded by oxygen in the air under the conditions for forming a planarization film using the organic film forming material described above, for example, under film forming conditions in air at 300° C. or higher, and the semiconductor device cannot achieve the performance as designed for the high speed of the material, and there is a possibility that the yield for industrial production cannot be achieved. Therefore, in order to avoid the decrease in yield caused by the corrosion of the substrate by air under such high temperature conditions, an organic film forming material that can be formed in an inert gas is expected.
[0006] Conventionally, condensation resins using carbonyl compounds such as ketones and aldehydes or aromatic alcohols as condensation agents for phenolic or naphtholic compounds are known as organic film forming materials for multilayer resist methods. For example, fluorene bisphenol novolac resin described in Patent Document 1, bisphenol compounds and their novolac resins described in Patent Document 2, adamantane phenol compound novolac resins described in Patent Document 3, and bisnaphthol compounds and their novolac resins described in Patent Document 4 can be exemplified. Such materials are formed as a film having solvent resistance against the coating film material used in the next process by crosslinking with a methylol compound as a crosslinking agent, oxidation at the α-position of the aromatic ring by the action of oxygen in the air, and curing action by crosslinking reaction by condensation thereafter. However, since the driving force for developing this solvent resistance is oxidation, it is not possible to satisfy various performances such as sufficient heat resistance and flatness in an inert gas. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2005-128509 A [Patent Document 2] JP 2006-293298 A [Patent Document 3] JP 2006-285095 A [Patent Document 4] JP 2010-122656 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in view of the above circumstances, and aims to provide a compound capable of forming an organic film which is cured not only in air but also under film-forming conditions in an inert gas, and which is excellent in heat resistance, filling and flattening properties of a pattern formed on a substrate, as well as excellent adhesion to the substrate, and a material for forming an organic film containing the compound.Furthermore, the present invention aims to provide a substrate for manufacturing a semiconductor device, a method for forming an organic film, and a method for forming a pattern using the material. [Means for solving the problem]
[0009] In order to solve the above problems, the present invention provides a material for forming an organic film, comprising: The present invention provides a material for forming an organic film, which comprises (A) a compound for forming an organic film represented by the following general formula (1A), and (B) an organic solvent. [ka] (In the formula, Y is an n1-valent organic group, a trivalent nitrogen atom or a tetravalent carbon atom, n1 is an integer of 3 to 8, and X is a partial structure represented by the following general formula (1B).) [ka] (In the formula, the dashed line represents a bond. R1 and R2 represent a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkyloxy group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms, and a hydrogen atom on a carbon atom constituting the alkyl group, alkyloxy group, alkynyl group, or alkenyl group may be substituted with a fluorine atom. In addition, aromatic rings that may be substituted with R1 may form a bridged structure via a single bond or a divalent group obtained by removing one hydrogen atom from R1. n4 and n5 represent integers of 0 to 2. Ar1 and Ar2 represent a benzene ring or a naphthalene ring, respectively. n2 represents 0 or 1, n3 represents 1 or 2, and R3 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms.)
[0010] Such an organic forming material will harden not only in air but also under film formation conditions in an inert gas, and will be an organic film forming material capable of forming an organic film that has high heat resistance, good adhesion to the substrate, and advanced filling / planarization properties.
[0011] In this case, it is preferable that R3 in the general formula (1B) is any of those represented by the following formula (1C). [ka] (The dashed lines in the above formula represent bonds.)
[0012] It is preferable to introduce such an end structure into the organic film-forming compound, which is the component (A), from the viewpoint of imparting excellent curability, flatness, embedding properties, and adhesion to the substrate.
[0013] In addition, n1 in the general formula (1A) is preferably 3 or 4.
[0014] It is preferable to adjust the number of substituents in the organic film-forming compound, which is the component (A), within an appropriate range in order to prevent loss of thermal fluidity due to rapid curing.
[0015] In addition, n2 in the general formula (1B) is preferably 1.
[0016] By introducing the above-mentioned structure into the organic film-forming compound, which is component (A), the carbon density can be increased, thereby imparting etching resistance, and further, shrinkage of the film due to heat is suppressed, making it possible to form a film with good heat resistance and flatness.
[0017] Moreover, it is preferable that Y in the general formula (1A) is any of the partial structures shown in the following formula (1D). [ka] (The dashed lines in the above formula represent bonds, and R4 represents a hydrogen atom or a methyl group.)
[0018] It is preferable that the organic film-forming compound, which is the component (A), has the above-mentioned structure from the viewpoint of improving various physical properties such as heat resistance, solvent solubility, and flatness.
[0019] The ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn of the component (A) in terms of polystyrene measured by gel permeation chromatography is preferably 1.00≦Mw / Mn≦1.10.
[0020] By controlling the Mw / Mn of the organic film-forming compound, which is the component (A), within such a range, an organic film having excellent filling properties and flatness can be formed.
[0021] The (B) organic solvent is preferably a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher.
[0022] The organic film-forming material containing the above-mentioned mixture of organic solvents can provide an organic film having higher embedding / flattening properties by adding a high-boiling point solvent to give it thermal fluidity. Note that in the present invention, the boiling point is the value at 1 atmosphere (1013 hPa).
[0023] The organic film-forming material of the present invention may further contain one or more of (C) an acid generator, (D) a surfactant, (E) a crosslinking agent, and (F) a plasticizer.
[0024] The organic film-forming material of the present invention may contain one or more of the above components (C) to (F) depending on the purpose.
[0025] The present invention also provides a substrate for manufacturing a semiconductor device, characterized in that the substrate has an organic film formed on it by curing the organic film-forming material of the present invention.
[0026] Such a substrate includes an organic film that has high heat resistance, good adhesion to the substrate, and high-level filling / planarization properties, and therefore, when used in the manufacturing process of a semiconductor device, the yield of the semiconductor device is improved.
[0027] The present invention further provides a method for forming an organic film to be applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material of the present invention onto a substrate to be processed, and subjecting the substrate to which the organic film-forming material has been applied to a heat treatment in an inert gas atmosphere at a temperature of 50°C or higher and 600°C or lower for a period of 5 to 7200 seconds to obtain a cured film.
[0028] The organic film formed by the method of the present invention and applied in the manufacturing process of a semiconductor device hardens even when formed in an inert gas, and has high heat resistance and advanced filling / planarization properties, and its use in the manufacturing process of a semiconductor device improves the yield of the semiconductor device.
[0029] The present invention also provides a method for forming an organic film that is applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material of the present invention onto a substrate to be processed, heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 50°C or higher and 300°C or lower for a period of 5 to 600 seconds to form a coating film, and subsequently heat-treating the substrate in an inert gas atmosphere at a temperature of 200°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a cured film.
[0030] The organic film formed by the method of the present invention and applied in the manufacturing process of a semiconductor device hardens even when formed in a partially inert gas, has high heat resistance and advanced filling / planarization properties, and its use in the manufacturing process of a semiconductor device improves the yield of the semiconductor device.
[0031] In the method for forming an organic film of the present invention, the oxygen concentration in the inert gas is preferably 1% by volume or less.
[0032] The organic film forming material of the present invention can be sufficiently cured without generating sublimates even when heated in such an inert gas atmosphere, and can form an organic film with excellent adhesion to the substrate. In addition, by heating in such an inert gas atmosphere, corrosion of the substrate to be processed can be prevented. In the present invention, the oxygen concentration is expressed on a volume basis.
[0033] In the present invention, the substrate to be processed may be a substrate having a structure or step having a height of 30 nm or more.
[0034] The method for forming an organic film of the present invention is particularly useful for forming a flat organic film on such a substrate.
[0035] The present invention also provides a pattern forming method, comprising the steps of forming an organic film on a workpiece using the organic film-forming material of the present invention, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming a resist top layer film on the silicon-containing resist intermediate film using a photoresist composition, forming a circuit pattern on the resist top layer film, transferring the pattern to the silicon-containing resist intermediate film by etching using the resist top layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film to which the pattern has been transferred as a mask.
[0036] The present invention also provides a pattern formation method, comprising the steps of forming an organic film on a workpiece using the organic film-forming material of the present invention, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming an organic antireflective film on the silicon-containing resist intermediate film, forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film and the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film to which the pattern has been transferred as a mask.
[0037] The present invention also provides a pattern formation method, comprising the steps of forming an organic film on a workpiece using the organic film-forming material of the present invention, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming a resist upper layer film on the inorganic hard mask using a photoresist composition, forming a circuit pattern on the resist upper layer film, transferring the pattern to the inorganic hard mask by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.
[0038] The present invention also provides a pattern formation method, comprising the steps of forming an organic film on a workpiece using the organic film-forming material of the present invention, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming an organic antireflective film on the inorganic hard mask, forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film and the inorganic hard mask by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.
[0039] The organic film-forming material of the present invention can be suitably used in various pattern forming methods, such as a three-layer resist process using a silicon-containing resist intermediate film or an inorganic hard mask, and a four-layer resist process using an organic anti-reflective film in addition to these. In the manufacturing process of a semiconductor device, if a circuit pattern is formed by such a pattern forming method of the present invention, the semiconductor device can be manufactured with a high yield.
[0040] When the inorganic hard mask is used, it is preferable to form it by a CVD method or an ALD method.
[0041] In the pattern formation method of the present invention, for example, an inorganic hard mask can be formed by such a method.
[0042] In the present invention, the circuit pattern is preferably formed by lithography using light having a wavelength of 10 nm or more and 300 nm or less, direct drawing with an electron beam, nanoimprinting, or a combination of these.
[0043] In forming the circuit pattern, it is preferable to develop the circuit pattern using an alkali developer or an organic solvent.
[0044] In the pattern forming method of the present invention, such a circuit pattern forming means and developing means can be suitably used.
[0045] In addition, it is preferable to use, as the workpiece, a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.
[0046] The workpiece preferably contains silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
[0047] According to the pattern forming method of the present invention, a pattern can be formed by processing the above-mentioned workpiece.
[0048] The present invention also provides a compound represented by the following general formula (1A): [ka] (In the formula, Y is an n1-valent organic group, a trivalent nitrogen atom or a tetravalent carbon atom, n1 is an integer of 3 to 8, and X is a partial structure represented by the following general formula (1B).) [ka] (In the formula, the dashed line represents a bond. R1 and R2 represent a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkyloxy group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms, and a hydrogen atom on a carbon atom constituting the alkyl group, alkyloxy group, alkynyl group, or alkenyl group may be substituted with a fluorine atom. In addition, aromatic rings that may be substituted with R1 may form a bridged structure via a single bond or a divalent group obtained by removing one hydrogen atom from R1. n4 and n5 represent integers of 0 to 2. Ar1 and Ar2 represent a benzene ring or a naphthalene ring, respectively. n2 represents 0 or 1, n3 represents 1 or 2, and R3 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms.)
[0049] Compounds with three or more cardo structures in one molecule can be cured not only in air but also in inert gas due to the substituents introduced into the terminal structures, and can form organic films that have high heat resistance, good adhesion to substrates, and advanced filling / flattening properties. In addition, the introduction of multiple cardo structures into the molecule can reduce the crystallinity of the compound, improving its solubility in solvents without impairing its heat resistance, and further making it possible to achieve both thermal fluidity and heat resistance, which are contradictory properties.
[0050] In this case, it is preferable that R3 in the general formula (1B) is any of those represented by the following formula (1C). [ka] (The dashed lines in the above formula represent bonds.)
[0051] By introducing such a terminal structure, it is possible to achieve crosslinking properties, good adhesion to the substrate, and high-level filling / planarization properties.
[0052] In the compound of the present invention, n1 in the general formula (1A) is preferably 3 or 4.
[0053] It is preferable to adjust the number of substituents in the compound to an appropriate range in order to prevent loss of thermal fluidity due to rapid curing.
[0054] In addition, n2 in the general formula (1B) is preferably 1.
[0055] By introducing the above-mentioned structure into the compound, the carbon density can be increased, thereby imparting etching resistance, and further, shrinkage of the film due to heat can be suppressed, making it possible to form a film with good heat resistance and flatness.
[0056] Moreover, it is preferable that Y in the general formula (1A) is any of the partial structures shown in the following formula (1D). [ka] (The dashed lines in the above formula represent bonds, and R4 represents a hydrogen atom or a methyl group.)
[0057] The compound of the present invention preferably has the above-mentioned structure from the viewpoint of improving various physical properties such as heat resistance, solvent solubility, and flatness. Effect of the Invention
[0058] As described above, the compound of the present invention is hardened without generating by-products even when formed in an inert gas that prevents corrosion of the substrate, and is a useful compound for forming an organic film having high heat resistance, good adhesion to the substrate, and high embedding and planarization properties. In addition, an organic film forming material containing this compound (compound for forming an organic film) is a material for forming an organic film having excellent embedding / planarization properties and various properties such as heat resistance and etching resistance. Therefore, an organic film obtained by the organic film forming material of the present invention has high embedding / planarization properties, and is an organic film without micropores due to poor embedding or unevenness on the organic film surface due to insufficient flatness. Therefore, the organic film forming material of the present invention is extremely useful as an organic film forming material in a multilayer resist method such as a two-layer resist method, a three-layer resist method using a silicon-containing intermediate film, and a four-layer resist method using a silicon-containing intermediate film and an organic anti-reflective film, or as a planarization material for manufacturing a semiconductor device. In addition, the organic film formed from the organic film-forming material of the present invention has excellent heat resistance, so that even when a CVD hard mask is formed on the organic film, there is no film thickness variation due to thermal decomposition, making it suitable for pattern formation. Furthermore, the semiconductor device substrate planarized with the organic film of the present invention has a wide process margin during patterning, making it possible to manufacture semiconductor devices with high yields. Furthermore, if a circuit pattern is formed by the pattern formation method of the present invention in the manufacturing process of a semiconductor device, semiconductor devices can be manufactured with high yields. [Brief description of the drawings]
[0059] [Figure 1] FIG. 4 is an explanatory diagram of flattening characteristics in the present invention. [Diagram 2] FIG. 2 is an explanatory diagram of an example of a pattern forming method using a three-layer resist method according to the present invention. [Diagram 3] FIG. 2 is an explanatory diagram of a method for evaluating embedding characteristics in an embodiment. [Figure 4] FIG. 4 is an explanatory diagram of a method for evaluating flattening characteristics in an embodiment. [Diagram 5] FIG. 2 is an explanatory diagram of a method for measuring adhesion in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0060] As described above, in order to prevent corrosion of the substrate, there has been a demand for the development of a compound for forming an organic film that can form an organic film that does not generate by-products even under film formation conditions in an inert gas, for example, at 300° C. or higher, has excellent filling and flattening properties for a pattern formed on a substrate, and also has good resistance to dry etching during substrate processing. Furthermore, there has been a demand for the development of a material for forming an organic film that does not cause a change in the thickness of the organic film due to thermal decomposition, even when a CVD hard mask is formed on the organic film, and a compound for forming an organic film that is useful for a pattern formation method using the material.
[0061] Usually, when forming an organic film, a compound for forming an organic film is dissolved in an organic solvent to form a composition, which is applied to a substrate on which the structure and wiring of a semiconductor device are formed, and baked to form an organic film. Immediately after application of the composition, a coating film is formed that conforms to the shape of the step structure on the substrate, but when the coating film is baked, most of the organic solvent evaporates before it hardens, and the organic film is formed by the compound for forming an organic film remaining on the substrate. The present inventors have conceived that if the compound for forming an organic film remaining on the substrate at this time has sufficient thermal fluidity, it is possible to flatten the step shape immediately after application by thermal fluidity and form a flat film.
[0062] The present inventors further conducted intensive research and found that an organic film-forming compound having a fluorene-type substituent represented by the following general formula (1A) has the same thermosetting properties as conventional organic film-forming materials not only in air but also in an inert gas due to the action of the substituent introduced at the end, and has good thermal fluidity, thereby exhibiting advanced filling / flattening properties. Since the curing mechanism does not depend on oxidation, there is no deterioration in etching resistance due to oxidation of the organic film-forming compound, and the compound has good dry etching resistance. In addition, since the compound has multiple rigid fluorene structures, it can provide an organic film-forming material having heat resistance without variation in coating thickness due to thermal decomposition even when forming a CVD hard mask, and thus completed the present invention.
[0063] That is, the present invention is a material for forming an organic film, characterized in that it contains (A) a compound for forming an organic film represented by the following general formula (1A) and (B) an organic solvent. [ka] (In the formula, Y is an n1-valent organic group, a trivalent nitrogen atom or a tetravalent carbon atom, n1 is an integer of 3 to 8, and X is a partial structure represented by the following general formula (1B).) [ka] (In the formula, the dashed line represents a bond. R1 and R2 represent a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkyloxy group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms, and a hydrogen atom on a carbon atom constituting the alkyl group, alkyloxy group, alkynyl group, or alkenyl group may be substituted with a fluorine atom. In addition, aromatic rings that may be substituted with R1 may form a bridged structure via a single bond or a divalent group obtained by removing one hydrogen atom from R1. n4 and n5 represent integers of 0 to 2. Ar1 and Ar2 represent a benzene ring or a naphthalene ring, respectively. n2 represents 0 or 1, n3 represents 1 or 2, and R3 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms.)
[0064] The present invention also relates to a compound represented by the above general formula (1A) that can be used as a material for forming an organic film.
[0065] The present invention will be described in detail below, but the present invention is not limited thereto.
[0066] The organic film-forming material of the present invention is characterized by containing an organic film-forming compound (A component) represented by the above general formula (1A) and an organic solvent (B component). The organic film-forming material may contain a compound (organic film-forming compound) represented by the above general formula (1A) and an organic solvent, and may contain other components as necessary. Each component will be described below.
[0067] <Compounds for organic film formation> The compound for forming an organic film of the present invention is a compound for forming an organic film represented by the following general formula (1A). [ka] (In the formula, Y is an n1-valent organic group, a trivalent nitrogen atom or a tetravalent carbon atom, n1 is an integer of 3 to 8, and X is a partial structure represented by the following general formula (1B).) [ka] (In the formula, the dashed line represents a bond. R1 and R2 represent a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkyloxy group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms, and a hydrogen atom on a carbon atom constituting the alkyl group, alkyloxy group, alkynyl group, or alkenyl group may be substituted with a fluorine atom. In addition, aromatic rings that may be substituted with R1 may form a bridged structure via a single bond or a divalent group obtained by removing one hydrogen atom from R1. n4 and n5 represent integers of 0 to 2. Ar1 and Ar2 represent a benzene ring or a naphthalene ring, respectively. n2 represents 0 or 1, n3 represents 1 or 2, and R3 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms.)
[0068] By introducing three or more cardo structures into the molecule as in the above general formula (1B), the crystallinity of the compound can be reduced, and the solubility in a solvent can be improved without impairing the heat resistance, making it possible to achieve a trade-off between thermal fluidity and heat resistance. In addition, OR3 can be cured in air or in an inert gas by selecting a substituent, and the chain length can be adjusted appropriately from the viewpoint of flatness and curability. In addition, it is possible to impart high adhesion to the substrate by mixing it with a compound partially having an ether group or a hydroxyl group. In addition, various physical properties such as etching resistance and optical properties can be adjusted by appropriately selecting the structure forming the main skeleton represented by Y. These compounds prevent film peeling when forming an inorganic hard mask directly on an organic film using the CVD method or the ALD method, making it possible to form an organic film with excellent process tolerance.
[0069] Examples of the n1-valent organic group among Y in the above general formula (1A) include the following, which may have a substituent when they have an aromatic ring. Examples of such groups include an alkyl group having 1 to 10 carbon atoms, an alkynyl group and an alkenyl group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, a nitro group, a halogen group, a nitrile group, an alkoxycarbonyl group having 1 to 10 carbon atoms, and an alkanoyloxy group having 1 to 10 carbon atoms.
[0070] [ka]
[0071] [ka]
[0072] [ka]
[0073] [ka]
[0074] Among the compounds represented by the above general formula (1A), examples of when the substituent R1 on the aromatic ring in general formula (1B) forms a bridge structure with a hydrogen atom in another aromatic ring (R1 in another aromatic ring is bonded to each other to form a bridge structure) include the following: Ar1, Ar2, n1, n2, n3, n5, R1, R2, and R3 are the same as above. [ka]
[0075] Among the above, from the viewpoint of adjusting the number of substituents in the compound within an appropriate range to prevent loss of thermal fluidity due to rapid curing, and from the viewpoint of loss of thermal fluidity due to an increase in the molecular weight of the compound caused by an increase in the number of substituents represented by X, it is preferable that n1=3 or 4 is satisfied, that is, Y is a trivalent or tetravalent organic group, and from the viewpoint of ease of availability of raw materials, n1=3 is more preferable.
[0076] Furthermore, from the viewpoints of availability of raw materials, heat resistance, and thermal fluidity, Y is more preferably any of the partial structures represented by the following formula (1D). [ka] (The dashed lines in the above formula represent bonds, and R4 represents a hydrogen atom or a methyl group.)
[0077] In the above general formula (1A), X is represented by the following general formula (1B). [ka] (In the formula, the dashed line represents a bond. R1 and R2 represent a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkyloxy group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms, and a hydrogen atom on a carbon atom constituting the alkyl group, alkyloxy group, alkynyl group, or alkenyl group may be substituted with a fluorine atom. In addition, aromatic rings that may be substituted with R1 may form a bridged structure via a single bond or a divalent group obtained by removing one hydrogen atom from R1. n4 and n5 represent integers of 0 to 2. Ar1 and Ar2 represent a benzene ring or a naphthalene ring, respectively. n2 represents 0 or 1, n3 represents 1 or 2, and R3 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms.)
[0078] Examples of the partial structure represented by the above general formula (1B) include the following: R1, R2, R3, n3, n4, and n5 are the same as above. [ka]
[0079] [ka]
[0080] [ka]
[0081] [ka]
[0082] [ka]
[0083] As the partial structure represented by Ar1 and Ar2 in the above general formula (1B), it is preferable that Ar1 and Ar2 are benzene rings, or that Ar1 and Ar2 are a combination of a benzene ring and a naphthalene ring. When Ar1 and Ar2 are benzene rings, improvement in heat resistance can be expected from the viewpoint of symmetry, and when Ar1 and Ar2 are a combination of a benzene ring and a naphthalene ring, an asymmetric structure is formed, which further improves the solubility of the compound in a solvent. Among these, it is more preferable that Ar1 and Ar2 are benzene rings from the viewpoint of ease of obtaining raw materials.
[0084] Examples of the substituents R1 and R2 on the aromatic ring in the above general formula (1B) include halogen atoms such as fluorine, chlorine, bromine and iodine, alkyl groups having 1 to 4 carbon atoms such as methyl, ethyl, propyl, isopropyl, butyl, s-butyl and t-butyl, alkoxy groups having 1 to 4 carbon atoms such as methoxy, ethoxy, propyloxy, n-butoxy, s-butoxy and t-butoxy, alkynyl groups having 2 to 4 carbon atoms such as vinyl, allyl and butenyl, and alkenyl groups having 2 to 4 carbon atoms such as ethynyl, propargyl and butynyl. In the case of an alkyloxy group, an alkyl group, an alkenyl group, and an alkynyl group, some or all of the hydrogen atoms on the carbon atoms may be substituted with fluorine substituents such as fluorine atoms. For example, in the case of a methyl group, a trifluoromethyl group, a difluoromethyl group, a monofluoromethyl group, etc. may be used. Among these, from the viewpoints of heat resistance and etching resistance, it is preferable that n4 and n5 are 0, and from the viewpoints of flatness and solubility, it is preferable that R1 is a trifluoromethyl group.
[0085] R3 in the above general formula (1B) is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkynyl or alkenyl group having 2 to 4 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a s-butyl group, and a t-butyl group. Examples of the alkenyl group having 2 to 4 carbon atoms include a vinyl group, an allyl group, and a butenyl group. Examples of the alkenyl group having 2 to 4 carbon atoms include an ethynyl group, a propargyl group, and a butynyl group. Among these, the structure represented by the following (1C) is preferred, and a propargyl group is more preferred from the viewpoint of thermosetting properties. [ka]
[0086] In the above general formula (1B), n2 is an integer of 0 or 1. From the viewpoint of heat resistance and etching resistance, it is preferable that n2=1, that is, a naphthalene ring.
[0087] In the above general formula (1B), n3 is an integer of 1 or 2. From the viewpoint of curability, it is preferable that n3=2, and in particular, when a substituent represented by -OR3 similar to catechol is adjacent as in the partial structure below, it is particularly preferable from the viewpoint of adhesion and heat resistance. [ka]
[0088] Furthermore, in the above general formula (1B), it is preferable that n2=1 and n3 is an integer of 1 or 2 as shown below, and it is more preferable that n3=2 from the viewpoint of curability. In particular, it is particularly preferable from the viewpoint of adhesion and heat resistance when a substituent represented by -OR3 similar to catechol is adjacent, as in the partial structure shown below. [ka]
[0089] Furthermore, when the partial structure having a substituent represented by OR3 has a propargyloxy group at the β-position on the naphthalene ring shown below, the propargyloxy group forms a cyclized product by baking, and then polymerizes to exhibit thermosetting properties. In this case, the propargyloxy group imparts fluidity before cyclization, and after cyclization, it not only acts as a curable group but also contributes to improving heat resistance by forming a ring structure. In this case, the curing reaction does not generate decomposable additives such as thermal acid generators that become outgassing components, or by-products such as condensation reactions, so that it is possible to suppress sublimate components during baking and film shrinkage. These actions make it possible to achieve both heat resistance and filling / flattening properties, which are contradictory properties, which is even more preferable.
[0090] [ka]
[0091] Furthermore, when the ratio of hydrogen atoms in the structure constituting R3 is a and the ratio of alkyl groups having 1 to 4 carbon atoms, alkynyl groups having 2 to 4 carbon atoms, and alkenyl groups having 2 to 4 carbon atoms is b, the ratio of hydrogen atoms, which can be expected to have an effect on adhesion to the substrate and film-forming properties, and alkyl groups having 1 to 4 carbon atoms, alkynyl groups having 2 to 4 carbon atoms, and alkenyl groups, which can be expected to have heat resistance and thermal fluidity, can be adjusted at any ratio to adjust the ratio according to the desired performance. When adjusting to any ratio, it is also possible to adjust the introduction rate of the substituent by reaction, and it is also possible to separately prepare a compound in which R3 is a hydrogen atom and a compound substituted with an alkyl group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group, and mix them to adjust to the desired ratio.
[0092] In addition, the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn in terms of polystyrene as measured by gel permeation chromatography (GPC) of the compound represented by general formula (1A) is preferably 1.00≦Mw / Mn≦1.10. By definition, if it is a monomolecular compound, Mw / Mn is 1.00, but due to the separation property of the gel permeation chromatography method, the measured value may exceed 1.00. In general, it is extremely difficult for a polymer having a repeating unit to approach Mw / Mn=1.00 unless a special polymerization method is used, and Mw / Mn has a distribution of Mw and exceeds 1. In the present invention, 1.00≦Mw / Mn≦1.10 is defined as an index showing monomolecularity in order to distinguish between monomolecular compounds and polymers. The average molecular weight and dispersity in the present invention are the weight average molecular weight (Mw), number average molecular weight (Mn) and dispersity (Mw / Mn) in terms of polystyrene measured by the GPC method using tetrahydrofuran as an eluent.
[0093] By controlling the Mw / Mn of the compound for the organic film-forming composition within such a range, an organic film having excellent filling properties and flatness can be formed.
[0094] [Method of manufacturing organic film-forming compound] An example of a method for producing a compound represented by the general formula (1A) of the present invention includes a step (STEP 1) of obtaining intermediate fluorenols by addition reaction of ketones having Ar1 and Ar2 with an organometallic reagent having metal M, followed by a dehydration condensation reaction (STEP 2) using an acid catalyst with benzene or naphthalenes having OR3 as a substituent as a raw material to obtain a target product. The reactions used in STEP 1 and STEP 2 can use one or more raw materials, which can be appropriately combined depending on the required properties.
[0095] [ka] (In the above formula, Y, Ar1, Ar2, n1, n2, n3, n4, n5, R1, R2, and R3 are the same as above, M represents a metal such as Li or MgX1, and X1 represents a halogen atom.)
[0096] Examples of the organometallic reagent used in Step 1 include Grignard reagents, organolithium reagents, organozinc reagents, organotitanium reagents, etc., with Grignard reagents and organolithium reagents being particularly preferred. Grignard reagents and organolithium reagents may be prepared by direct metallation of the corresponding halide with metallic magnesium or metallic lithium, respectively, or by a metal-halogen exchange reaction with an aliphatic organometallic compound such as isopropylmagnesium halide, methyllithium, or butyllithium.
[0097] In addition, organozinc reagents and organotitanium reagents can be prepared from the corresponding Grignard reagents or organolithium reagents by reaction with zinc halide, titanium(IV) halide, alkoxytitanium(IV), etc. Metal salt compounds may be present during the preparation of the organometallic reagents or during the reaction of the organometallic reagents with sumanene oxide. In this case, the reaction proceeds in the presence of a transition metal catalyst such as palladium or nickel.
[0098] Examples of the metal salt compound include cyanides, halides, and perhalogenates. Preferred examples of the metal salt compound include lithium salts such as lithium chloride, lithium bromide, lithium iodide, and lithium perchlorate, and copper salts such as copper(I) cyanide, copper(II) cyanide, copper(I) chloride, copper(II) chloride, and dilithium tetrachlorocuprate.
[0099] The above metal salt compound can be added in an amount of 0.01 to 5.0 equivalents, preferably 0.2 to 2.0 equivalents, to the organometallic reagent to increase the solubility of the organometallic reagent and facilitate its preparation, and can also adjust the nucleophilicity and Lewis acidity of the reagent.
[0100] As the solvent used in the preparation of the above-mentioned organometallic reagent and the reaction with the sumanene oxide, ethers such as diethyl ether, dibutyl ether, tetrahydrofuran, 1,4-dioxane, cyclopentyl methyl ether, etc., hydrocarbons such as benzene, toluene, xylene, mesitylene, hexane, heptane, octane, isooctane, etc., and aprotic polar solvents such as N,N,N',N'-tetramethylethylenediamine, hexamethylphosphoric triamide, N,N-dimethylformamide, etc. can be used alone or in combination.
[0101] The reaction temperature depends on the type and reaction conditions of the ketones and organometallic reagents having Ar1 and Ar2, but is preferably −70 to 150° C. For example, when the organometallic reagent is an organozinc reagent or a Grignard reagent, it can be selected from various temperatures depending on the reaction, such as room temperature to reflux at the boiling point of the solvent. The reaction time is usually preferably 30 minutes to 48 hours.
[0102] The reaction method includes a method of charging the organometallic reagent and ketones having Ar1 and Ar2 prepared in advance all at once in a solvent, or a method of dispersing or dissolving either the organometallic reagent or the ketones having Ar1 and Ar2 in a solvent, and then dropping the other one that has been dispersed or dissolved in the solvent. The intermediate fluorenols obtained can be quenched with water or the like and then directly proceeded to the dehydration condensation reaction in STEP 2, but they can also be diluted in an organic solvent to remove unreacted raw materials and catalysts that exist in the system as reaction intermediates, and then crystallized with a poor solvent or separated for recovery as a powder.
[0103] As the acid catalyst used in the dehydration condensation reaction shown in STEP 2, inorganic acids such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, heteropolyacids, etc., organic acids such as oxalic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, trifluoromethanesulfonic acid, etc., and Lewis acids such as aluminum trichloride, aluminum ethoxide, aluminum isopropoxide, boron trifluoride, boron trichloride, boron tribromide, tin tetrachloride, tin tetrabromide, dibutyltin dichloride, dibutyltin dimethoxide, dibutyltin oxide, titanium tetrachloride, titanium tetrabromide, titanium (IV) methoxide, titanium (IV) ethoxide, titanium (IV) isopropoxide, titanium (IV) oxide, etc. can be used. The amount of these catalysts used can be in the range of 0.1 to 20 moles, preferably 0.2 to 10 moles, relative to the number of moles of the intermediate fluorenols.
[0104] The solvent to be used is not particularly limited, and examples thereof include alcohols such as methanol, ethanol, isopropyl alcohol, butanol, ethylene glycol, propylene glycol, diethylene glycol, glycerol, ethylene glycol monomethyl ether, and propylene glycol monomethyl ether; ethers such as diethyl ether, dibutyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, and 1,4-dioxane; chlorine-based solvents such as methylene chloride, chloroform, dichloroethane, and trichloroethylene; hydrocarbons such as hexane, heptane, benzene, toluene, xylene, and cumene; nitriles such as acetonitrile; ketones such as acetone, ethyl methyl ketone, and isobutyl methyl ketone; esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate; and aprotic polar solvents such as dimethyl sulfoxide, N,N-dimethylformamide, and hexamethylphosphoric triamide. These can be used alone or in combination of two or more. These solvents can be used in the range of 0 to 2000 parts by mass per 100 parts by mass of the reaction raw materials, and the reaction temperature is preferably from −50° C. to the boiling point of the solvent, more preferably from room temperature to 150° C. The reaction time is appropriately selected from 0.1 to 100 hours.
[0105] The reaction method includes a method of charging fluorenols, benzene or naphthalenes and an acid catalyst all at once, a method of dispersing or dissolving fluorenols, benzene or naphthalenes, and then adding the catalyst all at once or in portions, or diluting with a solvent and adding dropwise, a method of dispersing or dissolving the catalyst, and then adding fluorenols, benzene or naphthalenes all at once or in portions, or diluting with a solvent and adding dropwise. In this case, depending on the reactivity of benzene or naphthalenes, it is preferable to use 2 moles or more of benzene or naphthalenes when fluorenols are 1 mole. After the reaction is completed, the catalyst used in the reaction is removed by diluting with an organic solvent, and then performing separation and washing to recover the target product.
[0106] The organic solvent used at this time is not particularly limited as long as it can dissolve the target substance and separate into two layers when mixed with water, but examples thereof include hydrocarbons such as hexane, heptane, benzene, toluene, and xylene, esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate, ketones such as methyl ethyl ketone, methyl amyl ketone, cyclohexanone, and methyl isobutyl ketone, ethers such as diethyl ether, diisopropyl ether, methyl-t-butyl ether, and ethylcyclopentyl methyl ether, chlorine-based solvents such as methylene chloride, chloroform, dichloroethane, and trichloroethylene, and mixtures thereof. The washing water used at this time may be what is usually called deionized water or ultrapure water. The number of washings may be one or more times, but since washing 10 or more times does not necessarily provide the effect of washing alone, it is preferably about 1 to 5 times.
[0107] In order to remove acidic components in the system during separation washing, washing may be performed with a basic aqueous solution. Specific examples of the base include alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates, ammonia, and organic ammonium.
[0108] Furthermore, in order to remove metal impurities or base components in the system during separation washing, washing with an acidic aqueous solution may be performed. Specific examples of the acid include inorganic acids such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, and heteropolyacids, and organic acids such as oxalic acid, fumaric acid, maleic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid.
[0109] The above-mentioned separation washing with a basic aqueous solution and an acidic aqueous solution may be performed either alone or in combination. From the viewpoint of removing metal impurities, the separation washing is preferably performed in the order of a basic aqueous solution and an acidic aqueous solution.
[0110] After the above-mentioned separation washing with the basic aqueous solution or acidic aqueous solution, washing with neutral water may be performed successively. The number of washings may be one or more times, but is preferably about 1 to 5 times. As the neutral water, the above-mentioned deionized water or ultrapure water may be used. The number of washings may be one or more times, but if the number of washings is too few, the basic components and acidic components may not be removed. Even if washing is performed 10 times or more, the effect of washing alone may not be obtained, so it is preferably about 1 to 5 times.
[0111] Furthermore, the reaction product after the liquid separation operation can be recovered as a powder by concentrating the solvent to dryness or crystallizing it under reduced pressure or normal pressure, but it can also be left in a solution state of a moderate concentration in order to improve operability when preparing an organic film-forming material. The concentration at this time is preferably 0.1 to 50 mass%, more preferably 0.5 to 30 mass%. At such a concentration, the viscosity is unlikely to increase, so that the operability is prevented from being impaired, and the amount of solvent is not excessive, so that it is economical.
[0112] The solvent used in this case is not particularly limited as long as it can dissolve the compound, and specific examples include ketones such as cyclohexanone and methyl-2-amyl ketone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; and esters such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol mono tert-butyl ether acetate. These can be used alone or in combination of two or more.
[0113] [Alternative methods for producing compounds] In addition, when R3 of the compound represented by the above general formula (1A) used in the organic film-forming material of the present invention is other than a hydrogen atom, an alternative manufacturing method includes a process (STEP1-1) in which an intermediate is obtained by a dehydration condensation reaction using an acid catalyst with fluorenols and benzenes or naphthalenes having a hydroxyl group, i.e., phenols or naphthols, as shown below. The monomolecular compound can be obtained by a method of performing a substitution reaction (STEP2-1) using a base catalyst with a raw material represented by R3-X2 having a leaving group X2 that converts the hydroxyl group to OR3. In this case, it is possible to use one or more types of R3-X2, and further, it is possible to control the ratio of hydroxyl groups and OR3 by controlling the reaction rate. It is also possible to control the film-forming properties and the adhesion of the film to the substrate by partially introducing a polar structure such as a hydroxyl group.
[0114] [ka] (In the above formula, Y, Ar1, Ar2, n1, n2, n3, n4, n5, R1, R2, and R3 are the same as above, and X2 represents a halogen atom, tosylate, or mesylate.)
[0115] The dehydration condensation reaction of (STEP1-1) can be carried out by the method described in the method for producing the compound of the above general formula (1A). The reaction method and the method for recovering the compound can be carried out by the method described in the method for producing the compound of the above general formula (1A).
[0116] Examples of the base catalyst used in the substitution reaction of (STEP2-1) include inorganic base compounds such as sodium hydrogen carbonate, sodium carbonate, potassium carbonate, calcium carbonate, cesium carbonate, sodium hydroxide, potassium hydroxide, sodium hydride, and potassium phosphate; and organic amine compounds such as triethylamine, pyridine, and N-methylmorpholine. These may be used alone or in combination of two or more kinds.
[0117] The solvent used in this case is not particularly limited as long as it is a solvent inert to the above reaction. For example, ether solvents such as diethyl ether, tetrahydrofuran, dioxane, etc., aromatic solvents such as benzene, toluene, xylene, etc., acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, N-methylpyrrolidone, water, etc., can be used alone or in combination.
[0118] The reaction method and the method for recovering the compound or polymer can be carried out by the method described in the above-mentioned method for producing the compound represented by the general formula (1A).
[0119] In preparing the compounds or polymers used in the organic film-forming materials obtained by this method, various halides, tosylates, and mesylates can be used alone or in combination according to the required performance. For example, compounds having a side chain structure that contributes to improving planarization characteristics, or a rigid aromatic ring structure that contributes to etching resistance and heat resistance can be combined in any ratio. Therefore, organic film-forming materials using these polymers can achieve both filling / planarization characteristics and etching resistance at a high level.
[0120] As described above, the compound for forming an organic film of the present invention provides a material for forming an organic film that can form an organic film that hardens without generating by-products even when formed in an inert gas in which corrosion of the substrate is prevented, has good adhesion to the substrate, and has heat resistance of, for example, 400° C. or more and high-level filling / planarizing properties.
[0121] In the present invention, the planarization property refers to the ability to planarize the surface of a substrate. For example, as shown in FIG. 1, a material (composition) containing the organic film-forming compound of the present invention can reduce a 100 nm step in the substrate 1 to 30 nm or less by applying an organic film-forming material 3' onto the substrate 1 and heating it to form an organic film 3. The step shape shown in FIG. 1 shows a typical example of the step shape in a substrate for manufacturing a semiconductor device, and the step shape of a substrate that can be planarized by the material containing the organic film-forming compound of the present invention is not limited to this.
[0122] <Materials for organic film formation> The present invention also provides a material for forming an organic film, which contains (A) the above-mentioned compound for forming an organic film of the present invention and (B) an organic solvent. In the material for forming an organic film of the present invention, the above-mentioned compound for forming an organic film of the present invention can be used alone or in combination of two or more. The material for forming an organic film of the present invention can also be called a composition for forming an organic film.
[0123] Further, in the present invention, as described above, a method of using only two or more kinds of substituents represented by R3 in combination, or a method of intentionally controlling the substitution rate of the substituent R3 so that the desired performance is obtained. Specifically, when the ratio of hydrogen atoms in the structure constituting R3 in the compound is a, and the ratio of alkyl groups having 1 to 4 carbon atoms, alkynyl groups having 2 to 4 carbon atoms, and alkenyl groups having 2 to 4 carbon atoms, which are expected to have an effect on adhesion to the substrate and film-forming properties, and alkyl groups having 1 to 4 carbon atoms, alkynyl groups having 2 to 4 carbon atoms, and alkenyl groups which are expected to have heat resistance and thermal fluidity, are adjusted at an arbitrary ratio, and the substitution introduction rate of b is adjusted so that a+b=100 according to the desired performance can be used. When controlling the substitution introduction rate, a desired compound can be obtained by carrying out a reaction using a compound having one or more leaving groups X2 according to the method described in the above [Alternative method for producing a compound].
[0124] <Organic solvent> The organic solvent usable in the organic film-forming material of the present invention is not particularly limited as long as it dissolves the organic film-forming compound of the present invention, as well as the optional components of the acid generator, crosslinking agent, and other additives. Specifically, solvents having a boiling point of less than 180° C., such as those described in paragraphs (0091) to (0092) of JP-A-2007-199653, can be used. Among them, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, 2-heptanone, cyclopentanone, cyclohexanone, and mixtures of two or more of these are preferably used.
[0125] Such a material can be applied by spin coating, and since it contains the compound for forming an organic film of the present invention as described above, it becomes a material for forming an organic film that has both heat resistance of 400°C or more and high-level filling / planarization properties.
[0126] Furthermore, in the organic film forming material of the present invention, it is possible to add a high boiling point solvent having a boiling point of 180° C. or more to the above-mentioned solvent having a boiling point of less than 180° C. (a mixture of a solvent having a boiling point of less than 180° C. and a solvent having a boiling point of 180° C. or more). The high boiling point organic solvent is not particularly limited as long as it can dissolve the organic film forming compound, and may be any of hydrocarbons, alcohols, ketones, esters, ethers, chlorine-based solvents, etc., but specific examples include 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecanol, ethylene glycol, 1,2-propylene glycol, 1,3-butylene glycol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 2,4-heptanediol, 2-ethyl-1,3-Hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerin, n-nonyl acetate, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoisobutyl ether, diethylene glycol monohexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, triethylene glycol monomethyl ether, triethylene glycol-n-butyl ether, triethylene glycol butyl methyl ether, triethylene Glycol diacetate, tetraethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tripropylene glycol mono-n-propyl ether, tripropylene glycol mono-n-butyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, triacetin, propylene glycol diacetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol methyl-n-propyl ether, dipropylene glycol methyl ether acetate, 1,4-butanediol diacetate, 1,3-butylene glycol diacetate, 1,Examples of the monomer include 6-hexanediol diacetate, triethylene glycol diacetate, γ-butyrolactone, dihexyl malonate, diethyl succinate, dipropyl succinate, dibutyl succinate, dihexyl succinate, dimethyl adipate, diethyl adipate, and dibutyl adipate, and these may be used alone or in combination.
[0127] The boiling point of the high boiling point solvent may be appropriately selected according to the temperature at which the organic film-forming material is heat-treated, and the boiling point of the high boiling point solvent to be added is preferably 180°C to 300°C, and more preferably 200°C to 300°C. If the boiling point is too low, there is no risk of the solvent volatilizing too quickly during baking (heat treatment), and sufficient thermal fluidity can be obtained. In addition, if the boiling point is high, there is no risk of the solvent remaining in the film after baking without volatilizing, and there is no risk of adversely affecting the film properties such as etching resistance.
[0128] Furthermore, when the above-mentioned high boiling point solvent is used, the blending amount of the high boiling point solvent is preferably 1 to 30 parts by mass per 100 parts by mass of the solvent having a boiling point of less than 180° C. If the blending amount is such, there is no risk that the blending amount is too small to impart sufficient thermal fluidity during baking, or that the blending amount is too large to remain in the film, leading to deterioration of film properties such as etching resistance. The amount of the organic solvent to be added is preferably 200 to 10,000 parts, more preferably 300 to 5,000 parts, based on 100 parts (parts by mass; the same applies hereinafter unless otherwise specified) of the compound (A).
[0129] In the case of such an organic film-forming material, by imparting thermal fluidity to the above-mentioned organic film-forming compound by adding a high-boiling point solvent, the organic film-forming material becomes one having both high-level filling / planarizing properties.
[0130] <Other ingredients> The organic film-forming material of the present invention may further contain one or more of (C) an acid generator, (D) a surfactant, (E) a crosslinking agent, and (F) a plasticizer, depending on the purpose.
[0131] ((C) Acid Generator) In the organic film-forming material of the present invention, an acid generator can be added as component (C) to further promote the curing reaction. The acid generator may be one that generates an acid by thermal decomposition or one that generates an acid by light irradiation, and either one may be added. Specifically, the materials described in paragraphs (0061) to (0085) of JP-A-2007-199653 may be added, but are not limited thereto.
[0132] The acid generators may be used alone or in combination of two or more. When an acid generator is added, the amount of the acid generator added is preferably 0.05 to 50 parts, more preferably 0.1 to 10 parts, based on 100 parts of the compound.
[0133] (D) Surfactant To improve the coating property in spin coating, a surfactant can be added as component (D) to the organic film-forming material of the present invention. For example, the surfactants described in (0142) to (0147) of JP-A-2009-269953 can be used.
[0134] The above surfactants can be used alone or in combination of two or more. When a surfactant is added, the amount of the surfactant added is preferably 0.01 to 10 parts, more preferably 0.05 to 5 parts, based on 100 parts of the compound.
[0135] ((E) Crosslinking Agent) In order to enhance the curability and further suppress intermixing with the upper layer film, a crosslinking agent may be added as component (E) to the organic film-forming material of the present invention. The crosslinking agent is not particularly limited, and various known crosslinking agents may be widely used. Examples include melamine-based crosslinking agents, glycoluril-based crosslinking agents, benzoguanamine-based crosslinking agents, urea-based crosslinking agents, β-hydroxyalkylamide-based crosslinking agents, isocyanurate-based crosslinking agents, aziridine-based crosslinking agents, oxazoline-based crosslinking agents, and epoxy-based crosslinking agents.
[0136] Specific examples of the melamine-based crosslinking agent include hexamethoxymethylated melamine, hexabutoxymethylated melamine, alkoxy and / or hydroxyl-substituted derivatives thereof, and partial self-condensates thereof. Specific examples of the glycoluril-based crosslinking agent include tetramethoxymethylated glycoluril, tetrabutoxymethylated glycoluril, alkoxy and / or hydroxyl-substituted derivatives thereof, and partial self-condensates thereof. Specific examples of the benzoguanamine-based crosslinking agent include tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, alkoxy and / or hydroxyl-substituted derivatives thereof, and partial self-condensates thereof. Specific examples of the urea-based crosslinking agent include dimethoxymethylated dimethoxyethyleneurea, alkoxy and / or hydroxyl-substituted derivatives thereof, and partial self-condensates thereof. Specific examples of the β-hydroxyalkylamide-based crosslinking agent include N,N,N',N'-tetra(2-hydroxyethyl)adipic acid amide. Specific examples of the isocyanurate crosslinking agent include triglycidyl isocyanurate and triallyl isocyanurate.Specific examples of the aziridine crosslinking agent include 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate]. Specific examples of the oxazoline-based crosslinking agent include 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tertbutyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymer.Specific examples of epoxy crosslinking agents include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether.
[0137] Specific examples of polynuclear phenol-based crosslinking agents include compounds represented by the following general formula (1E). [ka] (In the formula, Q is a single bond or a hydrocarbon group having 1 to 20 carbon atoms and a valence of s. 10 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. s is an integer of 1 to 5.
[0138] Q is a single bond or a hydrocarbon group having 1 to 20 carbon atoms and a valence of s. s is an integer of 1 to 5, and is more preferably 2 or 3. Specific examples of Q include groups in which s hydrogen atoms have been removed from methane, ethane, propane, butane, isobutane, pentane, cyclopentane, hexane, cyclohexane, methylpentane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, benzene, toluene, xylene, ethylbenzene, ethylisopropylbenzene, diisopropylbenzene, methylnaphthalene, ethylnaphthalene, and eicosane. R 10 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specific examples of the alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a pentyl group, an isopentyl group, a hexyl group, an octyl group, an ethylhexyl group, a decyl group, and an eicosanyl group, and a hydrogen atom or a methyl group is preferable.
[0139] Specific examples of the compound represented by the general formula (1E) include the following compounds. Among these, from the viewpoint of improving the curability and thickness uniformity of the organic film, hexamethoxymethylated products of triphenolmethane, triphenolethane, 1,1,1-tris(4-hydroxyphenyl)ethane, and tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene are preferred. 10 is the same as above.
[0140] [ka]
[0141] [ka]
[0142] The above acid crosslinking agents may be used alone or in combination of two or more. The amount of the crosslinking agent added is preferably 1 to 100 parts, more preferably 5 to 50 parts, based on 100 parts of the compound.
[0143] ((F) Plasticizer) In addition, in order to further improve the flattening / filling properties, a plasticizer can be added as component (F) to the organic film-forming material of the present invention. The plasticizer is not particularly limited, and various known plasticizers can be widely used. Examples include low molecular weight compounds such as phthalates, adipic esters, phosphates, trimellitates, and citrates, polyethers, polyesters, and polymers such as the polyacetal polymers described in JP-A-2013-253227. When a plasticizer is added, the amount of the plasticizer is preferably 1 to 100 parts, more preferably 5 to 30 parts, based on 100 parts of the compound.
[0144] In addition, in the organic film-forming material of the present invention, as an additive for imparting filling / flattening properties in the same manner as a plasticizer, for example, a liquid additive having a polyethylene glycol or polypropylene glycol structure, or a thermally decomposable polymer having a weight loss rate of 40% by mass or more between 30°C and 250°C and a weight average molecular weight of 300 to 200,000 is preferably used. This thermally decomposable polymer preferably contains a repeating unit having an acetal structure represented by the following general formula (DP1) or (DP1a). When these thermally decomposable polymers are added, the amount of addition is preferably 1 to 100 parts, more preferably 5 to 30 parts, based on 100 parts of the compound.
[0145] [ka] (In the formula, Ra is a hydrogen atom or an optionally substituted saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms. L is a saturated or unsaturated divalent organic group having 2 to 30 carbon atoms.)
[0146] [ka] (In the formula, Rb is an alkyl group having 1 to 4 carbon atoms. Z is a saturated or unsaturated divalent hydrocarbon group having 4 to 10 carbon atoms, which may have an ether bond. t represents the average number of repeating units and is 3 to 500.)
[0147] Furthermore, the following flowability promoters can be used as additives for improving the filling / flattening properties as described above. As the flowability promoter, one or more compounds selected from the following general formulas (i) to (iii) can be used. When these flowability promoters are added, the amount added is preferably 1 to 100 parts, more preferably 5 to 30 parts, based on 100 parts of the compound. [ka] (In the formula, each Ra is independently a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms which may be substituted. W1 is a phenylene group or a divalent group represented by the following general formula (i-1). W2 and W3 are each a single bond or a divalent group represented by the following general formula (i-2). m1 is an integer of 1 to 10, and na is an integer of 0 to 5.) [ka] (In the formula, * indicates a bonding position, and Rb, Rc, Rd, and Re are a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms. W10 and W11 each independently represent a single bond or a carbonyl group. m10 and m11 are integers of 0 to 10, and m10+m11≧1.) [ka] (In the formula, * indicates the bond position.)
[0148] [ka] (In the formula, Rf is each independently a hydrogen atom or an organic group having 1 to 10 carbon atoms which may be substituted. W4 is a divalent group represented by the following general formula (ii-1). W5 is a single bond or a divalent group represented by the following general formula (ii-2). m2 is an integer of 2 to 10, and nc is an integer of 0 to 5.) [ka] (In the formula, * indicates a bonding position, and Rg, Rh, Ri, and Rj each represent a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms. m20 and m21 each represent an integer of 0 to 10, and m20+m21≧1.)
[0149] [ka] (In the formula, Rk and Rl are a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms which may be substituted, and may be bonded to form a cyclic structure. Rm and Rn are organic groups having 1 to 10 carbon atoms, and Rm is a group containing either an aromatic ring or a divalent group represented by the following general formula (iii-1). W6 and W7 are a single bond or a divalent group represented by the following general formula (iii-2), and at least one of them is a divalent group represented by any of (iii-2).) [ka] (In the formula, * indicates a bonding position, and W30 is an organic group having 1 to 4 carbon atoms.) [ka] (In the formula, * indicates the bond position.)
[0150] As described above, the organic film-forming material of the present invention is a material for forming an organic film that hardens without generating by-products even when formed in an inert gas that prevents corrosion of the substrate, has good adhesion to the substrate, and has heat resistance of, for example, 400 ° C. or more and high filling / flattening properties. Therefore, the organic film-forming material of the present invention is extremely useful as a material for forming an organic film in a multilayer resist method such as a two-layer resist method, a three-layer resist method using a silicon-containing resist intermediate film or an inorganic hard mask (e.g., a silicon-containing inorganic hard mask), and a four-layer resist method using a silicon-containing resist intermediate film or an inorganic hard mask and an organic anti-reflective film. In addition, the organic film-forming material of the present invention does not generate by-products even when formed in an inert gas, and has excellent filling / flattening properties, so it can be suitably used as a flattening material in semiconductor device manufacturing processes other than the multilayer resist method. That is, the organic film-forming material of the present invention can be suitably used in a semiconductor device manufacturing process.
[0151] <Substrates for manufacturing semiconductor devices> The present invention also provides a substrate for manufacturing a semiconductor device, characterized in that the substrate has an organic film formed on it by curing the organic film-forming material of the present invention.
[0152] The substrate for manufacturing a semiconductor device of the present invention can also be said to comprise a substrate and an organic film which is a cured product of the organic film-forming material of the present invention formed on the substrate.
[0153] Such a substrate for manufacturing a semiconductor device includes an organic film that has high heat resistance, good adhesion to the substrate, and high-level filling / planarization properties, and therefore when used in the manufacturing process of a semiconductor device, the yield of the semiconductor device is improved.
[0154] <Organic film formation method> The present invention further provides a method for forming an organic film, which is applied to a manufacturing process of a semiconductor device, using the organic film-forming material of the present invention. (One-stage bake method (in inert gas)) A method for forming an organic film applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material of the present invention on a substrate to be processed, and subjecting the substrate to which the organic film-forming material has been applied to a heat treatment in an inert gas atmosphere at a temperature of 50°C or higher and 600°C or lower for a period of 5 to 7200 seconds to obtain a cured film. (Two-stage baking method (in air and inert gas)) The method for forming an organic film is applied in a manufacturing process of a semiconductor device, and is characterized in that the organic film-forming material of the present invention is spin-coated on a substrate to be processed, the substrate to be processed on which the organic film-forming material has been coated is heat-treated in air at a temperature of 50°C or higher and 300°C or lower for a period of 5 to 600 seconds to form a coating film, and then heat-treated in an inert gas atmosphere at a temperature of 200°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a cured film.
[0155] In the method for forming an organic film of the present invention, first, the above-mentioned organic film-forming material of the present invention is spin-coated onto a substrate to be processed.
[0156] In the organic film forming method of the present invention, the substrate to be processed on which the organic film forming material has been applied is then subjected to a heat treatment (heated film forming step) to obtain a cured film.
[0157] The heating film-forming step for forming a cured film can employ one-stage baking, two-stage baking, or three or more stages of multi-stage baking, but one-stage baking or two-stage baking is economically preferred.
[0158] The film formation by one-stage baking is preferably performed at a temperature of 50°C to 600°C for 5 to 7200 seconds, preferably at a temperature of 150°C to 500°C for 10 to 7200 seconds (more preferably 10 to 3600 seconds). By performing heat treatment under such conditions, flattening and crosslinking reaction due to thermal flow can be promoted. In the multi-layer resist method, a coating type silicon-containing resist intermediate film or a CVD hard mask may be formed on the obtained film. When a coating type silicon-containing resist intermediate film is applied, it is preferable to form the film at a temperature higher than the temperature at which the silicon-containing resist intermediate film is formed. Usually, the silicon-containing resist intermediate film is formed at a temperature of 100°C to 400°C, preferably 150°C to 350°C. When the organic film is formed at a temperature higher than this temperature, it is possible to prevent dissolution of the organic film by the silicon-containing resist intermediate film material and form an organic film that does not mix with the material.
[0159] When a CVD hard mask is used, it is preferable to form the organic film at a temperature higher than the temperature at which the CVD hard mask is formed, for example, a temperature of 150° C. or higher and 500° C. or lower.
[0160] Examples of the atmosphere during baking include inert gases such as nitrogen, argon, and helium. The material of the present invention can form a sufficiently cured organic film without generating sublimates even when baked in such an inert gas atmosphere. Furthermore, the material of the present invention can be cured without generating by-products even when formed in an inert gas that prevents corrosion of the substrate.
[0161] That is, one embodiment of the organic film forming method of the present invention is a method for forming an organic film applied in a manufacturing process of a semiconductor device, which is characterized by spin-coating the organic film forming material of the present invention onto a substrate to be processed, and heat-treating the substrate to which the organic film forming material has been applied in an inert gas atmosphere at a temperature of 50°C or higher and 600°C or lower for a period of 5 to 7200 seconds to obtain a cured film.
[0162] On the other hand, in film formation by two-stage baking, for example, a first stage of baking can be performed in which a substrate to be processed coated with the organic film-forming material of the present invention is heat-treated in air, followed by a second stage of baking in an inert gas atmosphere.
[0163] Considering the influence of oxygen in the air on the substrate, the first stage of baking is performed for 5 to 600 seconds at a treatment temperature of 300° C. or less, preferably 250° C. or less in air. The lower limit of the treatment temperature in air can be, for example, 50° C.
[0164] The atmosphere during the second baking step can be exemplified by inert gases such as nitrogen, argon, and helium. The material of the present invention can form a sufficiently cured organic film without generating sublimates even when baked in such an inert gas atmosphere. Furthermore, the material of the present invention can be cured without generating by-products even when formed in an inert gas that prevents corrosion of the substrate.
[0165] The second stage baking temperature is higher than the first stage baking temperature, for example, 200°C or higher, and 600°C or lower, preferably 500°C or lower, and is preferably performed for 10 to 7200 seconds. In the multilayer resist method, a coating type silicon-containing resist intermediate film or a CVD hard mask may be formed on the obtained film. When a coating type silicon-containing resist intermediate film is applied, it is preferable to form the film at a temperature higher than the temperature at which the silicon-containing resist intermediate film is formed. Usually, the silicon-containing resist intermediate film is formed at 100°C or higher and 400°C or lower, preferably 150°C or higher and 350°C or lower. When the organic film is formed at a temperature higher than this temperature, it is possible to prevent the organic film from being dissolved by the silicon-containing resist intermediate film material and form an organic film that does not mix with the material.
[0166] When a CVD hard mask is applied in two-stage baking, it is preferable to form the organic film at a temperature higher than the temperature at which the CVD hard mask is formed. Examples of the temperature at which the CVD hard mask is formed include a temperature of 150° C. or higher and 500° C. or lower.
[0167] That is, one embodiment of the organic film forming method of the present invention is a method for forming an organic film applied in a manufacturing process of a semiconductor device, which comprises spin-coating the organic film forming material of the present invention onto a substrate to be processed, heat-treating the substrate to which the organic film forming material has been applied in air at a temperature of 50°C or higher and 300°C or lower for a period of 5 to 600 seconds to form a coating film, and subsequently heat-treating the substrate in an inert gas atmosphere at a temperature of 200°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a cured film.
[0168] The oxygen concentration in the inert gas is preferably 1% by volume or less. The organic film-forming material of the present invention can be sufficiently cured without generating sublimates even when heated (heat-treated) in such an inert gas atmosphere, and can form an organic film having excellent adhesion to a substrate. In addition, by heating in such an inert gas atmosphere, corrosion of the substrate to be processed can be prevented.
[0169] That is, the present invention provides a method for forming an organic film that functions as an organic film used in the manufacturing process of a semiconductor device, in which the heat treatment under the inert gas atmosphere is performed by heat treating the substrate to be processed in an atmosphere having an oxygen concentration of 1% by volume or less to form a hardened film in order to prevent corrosion of the substrate to be processed.
[0170] In this method for forming an organic film, first, the organic film forming material of the present invention is spin-coated on a substrate to be processed. After spin-coating, in a two-stage bake, the material is first baked in air at 300°C or less, and then the second stage bake is performed in an atmosphere with an oxygen concentration of 1% by volume or less. In the case of a one-stage bake, the first stage bake in air may be skipped. Examples of the atmosphere during baking include inert gases such as nitrogen, argon, and helium. If the material of the present invention is used, it is possible to form a sufficiently hardened organic film without generating sublimates even when fired in such an inert gas atmosphere.
[0171] In addition, the organic film forming method of the present invention can use a substrate to be processed having a structure or step having a height of 30 nm or more. As described above, the organic film forming material of the present invention has excellent filling / flattening properties, so that even if the substrate to be processed has a structure or step (unevenness) having a height of 30 nm or more, a flat cured film can be formed. In other words, the organic film forming method of the present invention is particularly useful when forming a flat organic film on such a substrate to be processed.
[0172] The thickness of the organic film to be formed may be appropriately selected, but is preferably 30 to 20,000 nm, and more preferably 50 to 15,000 nm.
[0173] The above-mentioned method for forming an organic film can be applied to both the case of forming an organic film for an organic film using the organic film-forming material of the present invention and the case of forming an organic film for a planarizing film.
[0174] For example, one variation of the organic film forming method of the present invention is a method for forming an organic film capable of planarizing the surface of a stepped substrate used in the manufacturing process of a semiconductor device, which comprises spin-coating the above-mentioned organic film forming material of the present invention onto a substrate to be processed, heat-treating the substrate to which the organic film forming material has been applied in air at a temperature of 50°C or higher and 300°C or lower for a period of 5 to 600 seconds, and subsequently heat-treating the substrate to which the organic film forming material has been applied in an inert gas atmosphere at a temperature of 200°C or higher and 600°C or lower for 10 to 7200 seconds, thereby forming a cured film.
[0175] In this method for forming an organic film, first, the organic film forming material of the present invention is spin-coated onto a substrate to be processed. By using the spin-coating method, good embedding properties can be obtained. After spin-coating, baking (heat treatment) is performed to promote flattening by thermal flow and crosslinking reaction. This baking can evaporate the solvent in the material, so mixing can be prevented even when a resist top layer or a silicon-containing resist intermediate layer is formed on the organic film.
[0176] <Pattern formation method> The organic film-forming material of the present invention can be suitably used in various pattern-forming methods, such as a three-layer resist process using a silicon-containing resist intermediate film or an inorganic hard mask, and a four-layer resist process using an organic anti-reflective film in addition to these. In the manufacturing process of a semiconductor device, if a circuit pattern is formed by such a pattern-forming method of the present invention, the semiconductor device can be manufactured with a high yield. Below, an example of a pattern-forming method using the organic film-forming material of the present invention is given.
[0177] (1) A method for forming a pattern, comprising the steps of forming an organic film on a workpiece using the organic film-forming material of the present invention, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming a resist top layer film on the silicon-containing resist intermediate film using a photoresist composition, forming a circuit pattern on the resist top layer film, transferring the pattern to the silicon-containing resist intermediate film by etching using the resist top layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask. (2) A pattern forming method comprising the steps of forming an organic film on a workpiece using the organic film-forming material of the present invention, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming an organic antireflective film on the silicon-containing resist intermediate film, forming a resist top layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist top layer film, transferring the pattern to the organic antireflective film and the silicon-containing resist intermediate film by etching using the resist top layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask. (3) A method for forming a pattern, comprising the steps of: forming an organic film on a workpiece using the organic film-forming material of the present invention; forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film; forming a resist upper layer film on the inorganic hard mask using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the inorganic hard mask by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask. (4) A method for forming a pattern, comprising the steps of forming an organic film on a workpiece using the organic film-forming material of the present invention, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming an organic antireflective film on the inorganic hard mask, forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist upper layer film, transferring the pattern to the organic antireflective film and the inorganic hard mask by etching using the resist upper layer film on which the pattern has been formed as a mask, transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask, and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask. The pattern formation method will be described below with examples, but is not limited to these.
[0178] [Three-layer resist method using silicon-containing resist intermediate film] The present invention also provides a pattern formation method, which comprises forming an organic film on a workpiece using the organic film-forming material of the present invention described above, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming a resist upper layer film on the silicon-containing resist intermediate film using a photoresist composition, forming a circuit pattern on the resist upper layer film, etching the silicon-containing resist intermediate film using the resist upper layer film on which the pattern has been formed as a mask to transfer the pattern to the silicon-containing resist intermediate film, etching the organic film using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask to transfer the pattern to the organic film, and further etching the workpiece using the organic film to which the pattern has been transferred as a mask to transfer the pattern to the workpiece.
[0179] As the workpiece, it is preferable to use a semiconductor device substrate, or the semiconductor device substrate on which any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film is formed. More specifically, although not limited to, a substrate such as Si, α-Si, p-Si, SiO2, SiN, SiON, W, TiN, Al, or the like, or a substrate on which the above-mentioned metal film or the like is formed as a workpiece layer, may be used.
[0180] As the processed layer, various low-k films such as Si, SiO2, SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si, and their stopper films are used, and can be formed to a thickness of usually 50 to 10,000 nm, particularly 100 to 5,000 nm. When forming the processed layer, the substrate and the processed layer are made of different materials.
[0181] The metal constituting the workpiece preferably contains silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
[0182] Furthermore, the workpiece may be a substrate having a structure or steps with a height of 30 nm or more.
[0183] When forming an organic film on a workpiece using the organic film-forming material of the present invention, the above-mentioned organic film-forming method of the present invention may be applied.
[0184] Next, a resist intermediate film (silicon-containing resist intermediate film) is formed on the organic film using a resist intermediate film material containing silicon atoms. As the silicon-containing resist intermediate film material, a polysiloxane-based intermediate film material is preferable. By imparting an anti-reflection effect to the silicon-containing resist intermediate film, reflection can be suppressed. In particular, for 193 nm exposure, if a material containing many aromatic groups and having high etching selectivity with the substrate is used as the organic film forming material, the k value becomes high and the substrate reflection becomes high, but by imparting absorption to an appropriate k value as the silicon-containing resist intermediate film, it becomes possible to suppress reflection, and the substrate reflection can be reduced to 0.5% or less. As the silicon-containing resist intermediate film having an anti-reflection effect, anthracene is preferably used for 248 nm and 157 nm exposure, and polysiloxane having a phenyl group or a light-absorbing group having a silicon-silicon bond in a pendant structure or polysiloxane structure for 193 nm exposure, which is crosslinked by acid or heat.
[0185] Next, a resist upper layer film is formed on the silicon-containing resist intermediate film using a resist upper layer film material consisting of a photoresist composition. The resist upper layer film material may be either positive or negative, and the same as a commonly used photoresist composition can be used. After spin-coating the resist upper layer film material, it is preferable to perform pre-baking at 60 to 180°C for 10 to 300 seconds. Thereafter, exposure is performed according to a conventional method, and further post-exposure baking (PEB) and development are performed to obtain a resist upper layer film pattern. The thickness of the resist upper layer film is not particularly limited, but is preferably 30 to 500 nm, and particularly preferably 50 to 400 nm.
[0186] Next, a circuit pattern (resist upper layer film pattern) is formed on the resist upper layer film. In forming the circuit pattern, it is preferable to form the circuit pattern by lithography using light having a wavelength of 10 nm or more and 300 nm or less, direct drawing with an electron beam, nanoimprinting, or a combination of these.
[0187] Examples of the exposure light include high-energy rays with a wavelength of 300 nm or less, specifically far ultraviolet rays, KrF excimer laser light (248 nm), ArF excimer laser light (193 nm), F2 laser light (157 nm), Kr2 laser light (146 nm), Ar2 laser light (126 nm), soft X-rays (EUV) of 3 to 20 nm, electron beams (EB), ion beams, X-rays, and the like.
[0188] In forming the circuit pattern, it is preferable to develop the circuit pattern with an alkali or an organic solvent.
[0189] Next, the silicon-containing resist intermediate film is etched using the resist top layer film on which the circuit pattern is formed as a mask, and the pattern is transferred to the silicon-containing resist intermediate film. The etching of the silicon-containing resist intermediate film using the resist top layer film pattern as a mask is preferably performed using a fluorocarbon gas. This forms a silicon-containing resist intermediate film pattern.
[0190] Next, the silicon-containing resist intermediate film with the transferred pattern is used as a mask to etch the organic film, and the pattern is transferred to the organic film. The silicon-containing resist intermediate film exhibits higher etching resistance to oxygen gas or hydrogen gas than the organic film, so the etching of the organic film using the silicon-containing resist intermediate film pattern as a mask is preferably performed using an etching gas mainly composed of oxygen gas or hydrogen gas. This allows the organic film pattern to be formed.
[0191] Next, the workpiece is etched using the organic film with the transferred pattern as a mask, and the pattern is transferred to the workpiece. The next etching of the workpiece (working layer) can be performed by a conventional method. For example, if the workpiece is SiO2, SiN, or a silica-based low dielectric constant insulating film, etching is performed mainly with fluorocarbon gas, and if it is p-Si, Al, or W, etching is performed mainly with chlorine or bromine gas. If the substrate is processed by etching with fluorocarbon gas, the silicon-containing resist intermediate film pattern is peeled off at the same time as the substrate is processed. On the other hand, if the substrate is processed by etching with chlorine or bromine gas, a separate dry etching stripping with fluorocarbon gas must be performed after the substrate is processed in order to strip the silicon-containing resist intermediate film pattern.
[0192] An organic film obtained by using the organic film-forming material of the present invention can have excellent etching resistance when etching the workpiece as described above.
[0193] [Four-layer resist method using silicon-containing resist intermediate film and organic anti-reflective film] The present invention also provides a pattern formation method, which comprises forming an organic film on a workpiece using the organic film-forming material of the present invention described above, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming an organic antireflective film on the silicon-containing resist intermediate film, forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist upper layer film, etching the organic antireflective film and the silicon-containing resist intermediate film using the resist upper layer film on which the pattern has been formed as a mask to transfer the pattern to the organic antireflective film and the silicon-containing resist intermediate film, etching the organic film using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask to transfer the pattern to the organic film, and further etching the workpiece using the organic film to which the pattern has been transferred as a mask to transfer the pattern to the workpiece.
[0194] This method can be carried out in the same manner as the three-layer resist method using the silicon-containing resist intermediate film described above, except that an organic antireflective coating (BARC) is formed between the silicon-containing resist intermediate film and the resist top layer film.
[0195] The organic anti-reflection film can be formed by spin coating using a known organic anti-reflection film material.
[0196] [Three-layer resist method using inorganic hard mask] The present invention also provides a pattern formation method by a three-layer resist method using the above-mentioned organic film-forming material of the present invention, which comprises forming an organic film on a workpiece using the organic film-forming material of the present invention, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming a resist upper layer film on the inorganic hard mask using a photoresist composition, forming a circuit pattern on the resist upper layer film, etching the inorganic hard mask using the resist upper layer film on which the pattern has been formed as a mask to transfer the pattern to the inorganic hard mask, etching the organic film using the inorganic hard mask on which the pattern has been transferred as a mask to transfer the pattern to the organic film, and further etching the workpiece using the organic film on which the pattern has been transferred as a mask to transfer the pattern to the workpiece.
[0197] This method can be carried out in the same manner as the three-layer resist method using the silicon-containing resist intermediate film described above, except that an inorganic hard mask is formed on the organic film instead of the silicon-containing resist intermediate film.
[0198] The inorganic hard mask selected from silicon oxide film, silicon nitride film, and silicon oxide nitride film (SiON film) can be formed by CVD method, ALD method, etc. Methods for forming silicon nitride film are described in, for example, JP 2002-334869 A and WO 2004 / 066377 A. The thickness of the inorganic hard mask is preferably 5 to 200 nm, more preferably 10 to 100 nm. As the inorganic hard mask, a SiON film having a high effect as an anti-reflection film is most preferably used. Since the substrate temperature when forming the SiON film is 300 to 500° C., the organic film needs to withstand a temperature of 300 to 500° C. The organic film formed using the organic film forming material of the present invention has high heat resistance and can withstand high temperatures of 300 to 500° C., so that it is possible to combine an inorganic hard mask formed by CVD method or ALD method with an organic film formed by spin coating method.
[0199] The inorganic hard mask selected from a titanium oxide film and a titanium nitride film can also be formed by a CVD method, an ALD method, or the like.
[0200] [Four-layer resist method using inorganic hard mask and organic anti-reflective coating] The present invention also provides a pattern formation method by a four-layer resist method using the organic film-forming material of the present invention, which comprises forming an organic film on a workpiece using the organic film-forming material of the present invention, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming an organic antireflective film on the inorganic hard mask, forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure, forming a circuit pattern on the resist upper layer film, etching the organic antireflective film and the inorganic hard mask using the resist upper layer film on which the pattern has been formed as a mask to transfer the pattern to the organic antireflective film and the inorganic hard mask, etching the organic film using the inorganic hard mask on which the pattern has been transferred as a mask to transfer the pattern to the organic film, and further etching the workpiece using the organic film on which the pattern has been transferred as a mask to transfer the pattern to the workpiece.
[0201] This method can be carried out in the same manner as the above-mentioned three-layer resist method using an inorganic hard mask, except that an organic antireflective coating (BARC) is formed between the inorganic hard mask and the resist top layer.
[0202] In particular, when a SiON film is used as the inorganic hard mask, the two-layer anti-reflection coating of the SiON film and BARC makes it possible to suppress reflections even in immersion lithography with a high NA exceeding 1.0. Another advantage of forming a BARC is that it has the effect of reducing the tailing of the resist top layer pattern directly above the SiON film.
[0203] Here, an example of a pattern forming method by the three-layer resist method of the present invention is shown in Figures 2(A) to (F). In the case of the three-layer resist method, as shown in Figure 2(A), an organic film 3 is formed on a workpiece layer 2 formed on a substrate 1 using the organic film forming material of the present invention, and then a silicon-containing resist intermediate film 4 is formed thereon, and a resist upper layer film 5 is formed thereon. Then, as shown in Figure 2(B), an exposed portion 6 of the resist upper layer film 5 is exposed to light, and PEB (post exposure bake) is performed. Then, as shown in Figure 2(C), development is performed to form a resist upper layer film pattern 5a. Then, as shown in Figure 2(D), the silicon-containing resist intermediate film 4 is dry-etched using a fluorocarbon gas with the resist upper layer film pattern 5a as a mask, to form a silicon-containing resist intermediate film pattern 4a. Then, as shown in Figure 2(E), after removing the resist upper layer film pattern 5a, the organic film 3 is oxygen plasma etched with the silicon-containing resist intermediate film pattern 4a as a mask, to form an organic film pattern 3a. Furthermore, as shown in FIG. 2(F), after removing the silicon-containing resist intermediate film pattern 4a, the process layer 2 is etched using the organic film pattern 3a as a mask to form a pattern 2a.
[0204] When forming an inorganic hard mask, the silicon-containing resist intermediate film 4 may be changed to an inorganic hard mask, and when forming a BARC, the BARC may be formed between the silicon-containing resist intermediate film 4 and the resist upper layer film 5. Etching of the BARC may be performed consecutively prior to etching of the silicon-containing resist intermediate film 4, or etching of only the BARC may be performed, and then etching of the silicon-containing resist intermediate film 4 may be performed by changing the etching device, for example.
[0205] As described above, the pattern forming method of the present invention makes it possible to form a fine pattern on a workpiece with high precision by a multi-layer resist method. EXAMPLES
[0206] The present invention will be described in more detail below with reference to Synthesis Examples, Comparative Synthesis Examples, Examples, and Comparative Examples, but the present invention is not limited thereto. Note that, as for the molecular weight and dispersity, the weight average molecular weight (Mw) and number average molecular weight (Mn) in terms of polystyrene were determined by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent, and the dispersity (Mw / Mn) was determined.
[0207] Synthesis example: Synthesis of compounds for forming organic films The following fluorenols (B1) to (B7), phenols and naphthols (C1) to (C4) were used in the synthesis of the organic film-forming compounds (A1) to (A13).
[0208] Fluorenols: [ka]
[0209] Phenols or naphthols: [ka]
[0210] As an example of the synthesis of fluorenols, a synthesis example of (B1) is shown below. [Synthesis Example 1] Synthesis of fluorenols (B1) [ka] A mixture of 189.9g of tris(4-bromophenyl)amine (D1), 1000mL of MTBE (t-butyl methyl ether), and 1000mL of THF (tetrahydrofuran) cooled to -20°C under N2 atmosphere was added with 500mL of 2.60M n-butyllithium hexane solution, and stirred at -20°C for 20 minutes. 191.7g of 9-fluorenone was dissolved in THF to prepare a 25wt% THF solution, which was slowly added dropwise, gradually raised to room temperature, and stirred at room temperature for 4 hours. After adding 1000ml of saturated ammonium chloride aqueous solution to stop the reaction, 2000ml of MTBE was added and the separated aqueous layer was removed. The organic layer was washed five times with 500ml of pure water, and the solvent was distilled off. After distillation, 500g of THF was added, and then 2000g of methanol was added to perform recrystallization. The precipitated crystals were separated by filtration, washed twice with 500g of methanol, and collected. The collected crystals were dried in vacuum at 70° C. to obtain compound (B1).
[0211] Other fluorenols (B2) to (B7) were synthesized using the following fluorenol sources. Specifically, the compound corresponding to the raw material (D1) used in Synthesis Example 1 was replaced with the corresponding bromides (D2) to (D7) according to the target structure, and the molar ratio of n-butyllithium solution and 9-fluorenone was the same as in Synthesis Example 1, to synthesize (B2) to (B7), respectively. Note that (B5) was synthesized using the ketone (D8) instead of 9-fluorenone.
[0212] Fluorenol Sources: [ka]
[0213] [Synthesis Example 2] Synthesis of compound (A1) [ka] Under a nitrogen atmosphere, 30.0 g of compound (B1), 55.0 g of compound (C1), and 400 g of 1,2-dichloroethane were added to obtain a homogeneous dispersion at an internal temperature of 60°C. 22.0 g of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 1 hour. After the reaction was completed, the mixture was cooled to room temperature, 1000 ml of MIBK (methyl isobutyl ketone) was added, and the mixture was washed six times with 200 ml of pure water, and the organic layer was dried under reduced pressure. 200 g of THF was added to the residue to obtain a homogeneous solution, and then crystallized in 2000 g of IPE (diisopropyl ether). The precipitated crystals were separated by filtration, washed twice with 500 g of IPE, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A1). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A1): Mw = 1350, Mw / Mn = 1.04
[0214] [Synthesis Example 3] Synthesis of compound (A2) [ka] Under a nitrogen atmosphere, 30.0 g of compound (B2), 19.9 g of compound (C1), and 250 g of 1,2-dichloroethane were added to obtain a homogeneous dispersion at an internal temperature of 60°C. 20.4 g of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, 1000 ml of MIBK was added, and the mixture was washed six times with 200 ml of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and then crystallized in 1000 g of IPE (diisopropyl ether). The precipitated crystals were separated by filtration, washed twice with 300 g of IPE, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A2). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A2): Mw = 1520, Mw / Mn = 1.04
[0215] [Synthesis Example 4] Synthesis of compound (A3) [ka] Under a nitrogen atmosphere, 10.0 g of compound (A1), 10.3 g of potassium carbonate, and 60 g of DMF (N,N-dimethylformamide) were added to obtain a homogeneous dispersion at an internal temperature of 50°C. 8.8 g of propargyl bromide was slowly added, and the reaction was carried out at an internal temperature of 50°C for 16 hours. After the reaction was completed, 150 ml of MIBK was added, washed six times with 50 ml of pure water, and the organic layer was dried under reduced pressure. 40 g of MIBK was added to the residue to obtain a homogeneous solution, which was then crystallized in 200 g of MeOH (methanol). The precipitated crystals were separated by filtration, washed twice with 100 g of MeOH, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A3). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A3): Mw=1590, Mw / Mn=1.04
[0216] [Synthesis Example 5] Synthesis of compound (A4) [ka] Under a nitrogen atmosphere, 10.0 g of compound (A2), 9.8 g of potassium carbonate, and 60 g of DMF were added to obtain a uniform dispersion at an internal temperature of 50°C. 8.4 g of propargyl bromide was slowly added, and the reaction was carried out at an internal temperature of 50°C for 16 hours. After the reaction was completed, 150 ml of MIBK was added, washed six times with 50 ml of pure water, and the organic layer was dried under reduced pressure. 40 g of MIBK was added to the residue to obtain a uniform solution, which was then crystallized in 200 g of MeOH. The precipitated crystals were separated by filtration, washed twice with 100 g of MeOH, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A4). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A4): Mw=1830, Mw / Mn=1.04
[0217] [Synthesis Example 6] Synthesis of compound (A5) [ka] Under a nitrogen atmosphere, 20.0 g of compound (B3), 21.5 g of compound (C1), and 200 g of 1,2-dichloroethane were added to obtain a homogeneous dispersion at an internal temperature of 60°C. 12.9 g of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, 1000 ml of MIBK was added, and the mixture was washed six times with 200 ml of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and 300 g of hexane was added dropwise while stirring to precipitate a mochi-like precipitate. After leaving the mixture to stand for a while, the clear supernatant was decanted. 100 g of THF was added again to obtain a homogenized solution, and 300 g of hexane was added to precipitate a mochi-like precipitate, and the mixture was left to stand, and the supernatant was decanted. DMF was added to the precipitate to obtain a homogeneous solution, and then the mixture was distilled under reduced pressure, and DMF was added to adjust the yield to 30 wt% DMF solution. 23.9g of potassium carbonate was added to the obtained DMF solution, and a uniform dispersion was obtained at an internal temperature of 50°C under a nitrogen atmosphere. 20.6g of propargyl bromide was slowly added, and the reaction was carried out at an internal temperature of 50°C for 16 hours. After the reaction was completed, 300ml of MIBK was added, washed six times with 100ml of pure water, and the organic layer was dried under reduced pressure. 80g of MIBK was added to the residue to obtain a uniform solution, which was then crystallized in 400g of MeOH. The precipitated crystals were separated by filtration, washed twice with 200g of MeOH, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A5). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A5): Mw=1750, Mw / Mn=1.05
[0218] [Synthesis Example 7] Synthesis of compound (A6) [ka] Under a nitrogen atmosphere, 20.0 g of compound (B4), 17.5 g of compound (C1), and 190 g of 1,2-dichloroethane were added to obtain a homogeneous solution at an internal temperature of 60°C. 10.5 g of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, 1000 ml of MIBK was added, and the mixture was washed six times with 200 ml of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and 300 g of hexane was added dropwise while stirring to precipitate a mochi-like precipitate. After leaving the mixture to stand for a while, the clear supernatant was decanted. 100 g of THF was added again to obtain a homogenized solution, and 300 g of hexane was added to precipitate a mochi-like precipitate, and the mixture was left to stand, and the supernatant was decanted. DMF was added to the precipitate to obtain a homogeneous solution, and then the mixture was distilled under reduced pressure, and DMF was added to adjust the yield to 30 wt% DMF solution. 22.6 g of potassium carbonate was added to the obtained DMF solution, and a uniform dispersion was obtained under a nitrogen atmosphere at an internal temperature of 50°C. 19.5 g of propargyl bromide was slowly added, and the reaction was carried out for 16 hours at an internal temperature of 50°C. After the reaction was completed, 300 ml of MIBK was added, washed six times with 100 ml of pure water, and the organic layer was dried under reduced pressure. 80 g of MIBK was added to the residue to obtain a uniform solution, which was then crystallized in 400 g of MeOH. The precipitated crystals were separated by filtration, washed twice with 200 g of MeOH, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A6). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A6): Mw=1870, Mw / Mn=1.03
[0219] [Synthesis Example 8] Synthesis of compound (A7) [ka] Under a nitrogen atmosphere, 20.0 g of compound (B5), 12.8 g of compound (C1), and 160 g of 1,2-dichloroethane were added to obtain a homogeneous solution at an internal temperature of 60°C. 7.7 g of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, 1000 ml of MIBK was added, and the mixture was washed six times with 200 ml of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and 300 g of hexane was added dropwise while stirring to precipitate a mochi-like precipitate. After leaving the mixture to stand for a while, the clear supernatant was decanted. 100 g of THF was added again to obtain a homogenized solution, and 300 g of hexane was added to precipitate a mochi-like precipitate, and the mixture was left to stand, and the supernatant was decanted. DMF was added to the precipitate to obtain a homogeneous solution, and then the mixture was distilled under reduced pressure, and DMF was added to adjust the yield to 30 wt% DMF solution. 16.6g of potassium carbonate was added to the obtained DMF solution, and a uniform dispersion was obtained under a nitrogen atmosphere at an internal temperature of 50°C. 14.3g of propargyl bromide was slowly added, and the reaction was carried out for 16 hours at an internal temperature of 50°C. After the reaction was completed, 300ml of MIBK was added, washed six times with 100ml of pure water, and the organic layer was dried under reduced pressure. 80g of MIBK was added to the residue to obtain a uniform solution, which was then crystallized in 400g of MeOH. The precipitated crystals were separated by filtration, washed twice with 200g of MeOH, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A7). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A7): Mw=2320, Mw / Mn=1.05
[0220] [Synthesis Example 9] Synthesis of compound (A8) [ka] In a nitrogen atmosphere, 20.0 g of compound (B6), 18.5 g of compound (C1), and 200 g of 1,2-dichloroethane were added to obtain a homogeneous dispersion at an internal temperature of 60°C. 11.1 g of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, 1000 ml of MIBK was added, and the mixture was washed six times with 200 ml of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and 300 g of hexane was added dropwise while stirring to precipitate a mochi-like precipitate. After leaving the mixture to stand for a while, the clear supernatant was decanted. 100 g of THF was added again to obtain a homogenized solution, and 300 g of hexane was added to precipitate a mochi-like precipitate, and the mixture was left to stand, and the supernatant was decanted. DMF was added to the precipitate to obtain a homogeneous solution, and then the mixture was distilled under reduced pressure, and DMF was added to adjust the yield to 30 wt% DMF solution. 26.5 g of potassium carbonate was added to the obtained DMF solution, and a uniform dispersion was obtained at an internal temperature of 50°C under a nitrogen atmosphere. 23.2 g of allyl bromide was slowly added, and the reaction was carried out at an internal temperature of 50°C for 16 hours. After the reaction was completed, 300 ml of MIBK was added, washed six times with 100 ml of pure water, and the organic layer was dried under reduced pressure. 80 g of MIBK was added to the residue to obtain a uniform solution, and then crystallized in MeOH (400 g). The precipitated crystals were separated by filtration, washed twice with 200 g of MeOH, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A8). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A8): Mw=2110, Mw / Mn=1.05
[0221] [Synthesis Example 10] Synthesis of compound (A9) [ka] Under a nitrogen atmosphere, 20.0 g of compound (B1), 41.7 g of compound (C2), and 300 g of 1,2-dichloroethane were added to obtain a homogeneous dispersion at an internal temperature of 60°C. 22.0 g of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 1 hour. After the reaction was completed, the mixture was cooled to room temperature, 1000 ml of MIBK (methyl isobutyl ketone) was added, and the mixture was washed six times with 200 ml of pure water, and the organic layer was dried under reduced pressure. 200 g of THF was added to the residue to obtain a homogeneous solution, and then crystallized in 2000 g of IPE (diisopropyl ether). The precipitated crystals were separated by filtration, washed twice with 500 g of IPE, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A9). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A9): Mw=1300, Mw / Mn=1.02
[0222] [Synthesis Example 11] Synthesis of compound (A10) [ka] Under a nitrogen atmosphere, 10.0 g of compound (A2), 6.5 g of potassium carbonate, and 60 g of DMF were added to obtain a uniform dispersion at an internal temperature of 50°C. 2.8 g of propargyl bromide was slowly added, and the reaction was carried out at an internal temperature of 50°C for 16 hours. After the reaction was completed, 150 ml of MIBK was added, washed six times with 50 ml of pure water, and the organic layer was dried under reduced pressure. 40 g of MIBK was added to the residue to obtain a uniform solution, which was then crystallized in 200 g of MeOH. The precipitated crystals were separated by filtration, washed twice with 100 g of MeOH, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A10). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A10): Mw = 1690, Mw / Mn = 1.07
[0223] [Synthesis Example 12] Synthesis of compound (A11) [ka] In a nitrogen atmosphere, 20.0 g of compound (B3), 25.2 g of compound (C3), and 200 g of 1,2-dichloroethane were added to obtain a homogeneous dispersion at an internal temperature of 60°C. 12.9 g of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, 1000 ml of MIBK was added, and the mixture was washed six times with 200 ml of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and 300 g of hexane was added dropwise while stirring to precipitate a mochi-like precipitate. After leaving the mixture to stand for a while, the clear supernatant was decanted. 100 g of THF was added again to obtain a homogenized solution, and 300 g of hexane was added to precipitate a mochi-like precipitate, and the mixture was left to stand, and the supernatant was decanted. DMF was added to the precipitate to obtain a homogeneous solution, and then the mixture was distilled under reduced pressure, and DMF was added to adjust the yield to 30 wt% DMF solution. 15.4 g of potassium carbonate was added to the obtained DMF solution, and a uniform dispersion was obtained under a nitrogen atmosphere at an internal temperature of 50°C. 13.3 g of propargyl bromide was slowly added, and the reaction was carried out for 16 hours at an internal temperature of 50°C. After the reaction was completed, 300 ml of MIBK was added, washed six times with 100 ml of pure water, and the organic layer was dried under reduced pressure. 80 g of MIBK was added to the residue to obtain a uniform solution, which was then crystallized in 400 g of MeOH. The precipitated crystals were separated by filtration, washed twice with 200 g of MeOH, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A11). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A11): Mw = 1330, Mw / Mn = 1.06
[0224] [Synthesis Example 13] Synthesis of compound (A12) [ka] Under a nitrogen atmosphere, 20.0 g of compound (B4), 12.0 g of compound (C4), and 160 g of 1,2-dichloroethane were added to obtain a homogeneous solution at an internal temperature of 60°C. 10.5 g of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, 1000 ml of MIBK was added, and the mixture was washed six times with 200 ml of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue to obtain a homogeneous solution, and 300 g of hexane was added dropwise while stirring to precipitate a mochi-like precipitate. After leaving the mixture to stand for a while, the clear supernatant was decanted. 100 g of THF was added again to obtain a homogenized solution, and 300 g of hexane was added to precipitate a mochi-like precipitate, and the mixture was left to stand, and the supernatant was decanted. DMF was added to the precipitate to obtain a homogeneous solution, and then the mixture was distilled under reduced pressure, and DMF was added to adjust the yield to 30 wt% DMF solution. 22.6 g of potassium carbonate was added to the obtained DMF solution, and a uniform dispersion was obtained under a nitrogen atmosphere at an internal temperature of 50°C. 19.5 g of propargyl bromide was slowly added, and the reaction was carried out for 16 hours at an internal temperature of 50°C. After the reaction was completed, 300 ml of MIBK was added, washed six times with 100 ml of pure water, and the organic layer was dried under reduced pressure. 80 g of MIBK was added to the residue to obtain a uniform solution, which was then crystallized in 400 g of MeOH. The precipitated crystals were separated by filtration, washed twice with 200 g of MeOH, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A12). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A12): Mw = 1540, Mw / Mn = 1.03
[0225] [Synthesis Example 14] Synthesis of compound (A13) [ka] In a nitrogen atmosphere, 20.0 g of compound (B7), 15.1 g of compound (C1), and 200 g of 1,2-dichloroethane were added to obtain a homogeneous solution at an internal temperature of 60°C. 9.1 g of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, 1000 ml of MIBK was added, and the mixture was washed six times with 200 ml of pure water, and the organic layer was dried under reduced pressure. 120 g of THF was added to the residue to obtain a homogeneous solution, and 350 g of hexane was added dropwise while stirring to precipitate a mochi-like precipitate. After leaving the mixture to stand for a while, the clear supernatant was decanted. 120 g of THF was added again to obtain a homogenized solution, and 350 g of hexane was added to precipitate a mochi-like precipitate, and the mixture was left to stand, and the supernatant was decanted. DMF was added to the precipitate to obtain a homogeneous solution, and then the mixture was distilled under reduced pressure, and DMF was added to adjust the yield to 30 wt% DMF solution. 29.3 g of potassium carbonate was added to the obtained DMF solution, and a uniform dispersion was obtained under a nitrogen atmosphere at an internal temperature of 50°C. 25.2 g of propargyl bromide was slowly added, and the reaction was carried out for 16 hours at an internal temperature of 50°C. After the reaction was completed, 400 ml of MIBK was added, washed six times with 100 ml of pure water, and the organic layer was dried under reduced pressure. 100 g of MIBK was added to the residue to obtain a uniform solution, which was then crystallized in 500 g of MeOH. The precipitated crystals were separated by filtration, washed twice with 200 g of MeOH, and collected. The collected crystals were dried in a vacuum at 70°C to obtain compound (A13). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (A13): Mw = 1810, Mw / Mn = 1.04
[0226] The comparative compounds (R1) to (R3) were synthesized using the following compounds (a1) to (a3). [ka]
[0227] [Comparative Synthesis Example 1] Synthesis of Comparative Compound (R1) [ka] Under a nitrogen atmosphere, 10.00 g of compound (a1), 4.76 g of potassium carbonate, and 50 g of DMF were made into a uniform dispersion at an internal temperature of 50°C under a nitrogen atmosphere. 3.72 g of propargyl bromide was slowly dropped, and the reaction was carried out at an internal temperature of 50°C for 16 hours. After cooling to room temperature, 100 g of methyl isobutyl ketone and 50 g of pure water were added to make a uniform solution, and then the water layer was removed. The organic layer was further washed twice with 30 g of 3.0% aqueous nitric acid solution and five times with 30 g of pure water, and the organic layer was dried under reduced pressure. 30 g of THF was added to the residue, and crystals were crystallized with 100 g of methanol. The crystals that were crystallized were separated by filtration, washed twice with 60 g of methanol, and collected. The collected crystals were dried in a vacuum at 70°C to obtain (R1). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (R1): Mw=960, Mw / Mn=1.07
[0228] [Comparative Synthesis Example 2] Synthesis of Comparative Compound (R2) [ka] Under a nitrogen atmosphere, 78.8 g of compound (a2), 21.6 g of 37% formalin solution, and 250 g of 1,2-dichloroethane were mixed at a liquid temperature of 70°C to prepare a homogeneous solution, and then 5 g of methanesulfonic acid was slowly added and stirred at a liquid temperature of 80°C for 12 hours. After cooling to room temperature, 500 g of MIBK was added, and the organic layer was washed five times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 300 mL of THF was added to the residue, and the polymer was reprecipitated with 2000 mL of hexane. The precipitated polymer was separated by filtration and dried under reduced pressure to obtain compound (R2). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (R2): Mw=2720, Mw / Mn=1.55
[0229] [Comparative Synthesis Example 3] Synthesis of Comparative Compound (R3) [ka] Under a nitrogen atmosphere, 90.1 g of compound (a3), 10.5 g of 37% formalin solution, and 270 g of 2-methoxy-1-propanol were made into a homogeneous solution at a liquid temperature of 80 ° C., and then 18 g of a 20% solution of paratoluenesulfonic acid in 2-methoxy-1-propanol was slowly added and stirred at a liquid temperature of 110 ° C. for 8 hours. After cooling to room temperature, 600 g of MIBK was added, and the organic layer was washed five times with 200 g of pure water, and then the organic layer was dried under reduced pressure. 320 g of THF was added to the residue, and the polymer was reprecipitated with 1350 g of hexane. The precipitated polymer was separated by filtration and dried under reduced pressure to obtain compound (R3). The weight average molecular weight (Mw) and dispersity (Mw / Mn) were determined by GPC, and the results were as follows: (R3): Mw=3700, Mw / Mn=2.82
[0230] The structural formulas, weight average molecular weight (Mw) and dispersity (Mw / Mn) of the compounds obtained above are shown in Tables 1 and 2-1. The structural formulas, Mw and Mw / Mn of the compounds (R1) to (R3) used in the comparative examples are also shown in Table 2-2.
[0231] [Table 1]
[0232] [Table 2-1]
[0233] [Table 2-2]
[0234] Preparation of organic film-forming materials (UDL-1 to 19, Comparative Examples UDL-1 to 3) The compounds (A1) to (A13) and (R1) to (R3) were dissolved in a solvent containing 0.1 mass% of a surfactant FC-4430 (manufactured by Sumitomo 3M Limited) in the ratios shown in Table 3, and the resulting solution was filtered through a 0.1 μm fluororesin filter to prepare organic film-forming materials (UDL-1 to 19, Comparative Examples UDL-1 to 3). In the preparation of UDL-1 to 15, propylene glycol monomethyl ether acetate (PGMEA) was used as the solvent. In the preparation of UDL-16 to 19, a mixture of PGMEA and either (S1) 1,6-diacetoxyhexane: boiling point 260°C or (S2) tripropylene glycol monomethyl ether: boiling point 242°C as a high boiling point solvent was used as the solvent. In the preparation of Comparative UDL-1 to 3, PGMEA was used as the solvent.
[0235] [Table 3]
[0236] Example 1 Solvent Resistance Measurement (Examples 1-1 to 1-19, Comparative Examples 1-1 to 1-3) The organic film forming materials (UDL-1 to 19, comparative UDL-1 to 3) prepared above were applied onto silicon substrates, baked at 400°C for 60 seconds under a nitrogen flow with an oxygen concentration controlled to 0.2% by volume or less, and the film thickness (a [Å]) was measured. PGMEA solvent was dispensed onto the substrate, left for 30 seconds, spin-dried, and baked at 100°C for 60 seconds to evaporate the PGMEA, and the film thickness (b [Å]) was measured. The difference in film thickness before and after PGMEA treatment (residual film ratio: (b / a) x 100) was calculated. The results are shown in Table 4 below.
[0237] [Table 4]
[0238] As shown in Table 4, the organic film-forming materials of the present invention (Examples 1-1 to 1-19) have a residual film rate of 99.5% or more after PGMEA treatment, and a crosslinking reaction occurs even in a nitrogen atmosphere, demonstrating sufficient solvent resistance. In contrast, Comparative Example 1-3 does not have a substituent that serves as a crosslinking group, so the residual film rate after PGMEA treatment is less than 50%, and a curing reaction does not occur, so solvent resistance is not demonstrated. These results show that the substituent represented by OR3 introduced as a substituent effectively functions as a thermal crosslinking group.
[0239] Example 2 Evaluation of heat resistance characteristics (Examples 2-1 to 2-19, Comparative Examples 2-1 to 2-3) The above organic film-forming materials (UDL-1 to 19, Comparative UDL-1 to 3) were each coated on a silicon substrate and baked in air at 180°C to form a 200 nm coating film, and the film thickness (A (Å)) was measured. This substrate was further baked for 10 minutes at 400°C in a nitrogen stream with an oxygen concentration controlled to 0.2 volume % or less, and the film thickness (B (Å)) was measured. The remaining film ratio was calculated by dividing film thickness B by film thickness A. These results are shown in Table 5.
[0240] [Table 5]
[0241] As shown in Table 5, the organic film-forming material of the present invention (Examples 2-1 to 2-19) shows a film thickness reduction of less than 3% even after baking at 400°C for 10 minutes, and the organic film-forming material of the present invention maintains its film thickness even after baking at 400°C, and has high heat resistance. Among these, Examples 2-1 to 2-5, 2-11, and 2-16 to 2-18, which contain compounds having a structure of n2=1 and n3=2, show even less film thickness reduction. In contrast, Comparative Example 2-1, which is a divalent compound, and Comparative Example 2-2, which does not have a fluorene structure, show a large film thickness reduction of more than 10%, and Comparative Example 2-3, which does not have a crosslinking group, also shows a film thickness reduction of more than 10%. From the above results, it can be seen that a dense and highly heat-resistant film is formed by a compound having a polyvalent skeleton and a naphthalene structure.
[0242] Example 3: Evaluation of filling characteristics (Examples 3-1 to 3-19, Comparative Examples 3-1 to 3-3) As shown in FIG. 3, the above organic film forming materials (UDL-1 to 19, comparative UDL-1 to 3) were applied onto a SiO2 wafer substrate having a dense hole pattern (hole diameter 0.16 μm, hole depth 0.50 μm, distance between the centers of two adjacent holes 0.32 μm), and baked for 60 seconds at 400° C. under a nitrogen gas flow with an oxygen concentration controlled to 0.2 vol.% or less using a hot plate to form an organic film 8. The substrate used was a base substrate 7 (SiO2 wafer substrate) having a dense hole pattern as shown in FIG. 3(G) (overhead view) and (H) (cross-sectional view). The cross-sectional shape of each wafer substrate obtained was observed using a scanning electron microscope (SEM) to confirm whether the holes were filled with an organic film without voids (air gaps). The results are shown in Table 6. When an organic film forming material with poor filling properties was used, voids were generated inside the holes in this evaluation. When an organic film-forming material with good filling properties is used, the organic film fills the hole without leaving any voids, as shown in FIG. 3(I) in this evaluation.
[0243] [Table 6]
[0244] As shown in Table 6, it was confirmed that the organic film-forming material of the present invention (Examples 3-1 to 3-19) can fill a hole pattern without generating voids and has good filling properties. In Comparative Examples 3-1 and 3-2, although there was a lack of heat resistance as shown in the results of the heat resistance property evaluation, no voids were observed. On the other hand, in Comparative Example 3-3, it was confirmed that not only the heat resistance but also voids were generated due to a lack of crosslinking, resulting in poor filling properties. From these results, it was confirmed that the organic film-forming material of the present invention has good filling properties.
[0245] Example 4: Evaluation of planarization characteristics (Examples 4-1 to 4-19, Comparative Examples 4-1 to 4-3) Each of the organic film forming materials (UDL-1 to 19, comparative UDL-1 to 3) was applied onto a base substrate 9 (SiO2 wafer substrate) having a giant isolated trench pattern (FIG. 4(J), trench width 10 μm, trench depth 0.10 μm), and baked for 60 seconds at 400°C under a nitrogen flow with an oxygen concentration controlled to 0.2 vol% or less. The step (delta10 in FIG. 4(K)) between the trench portion and the non-trench portion of the organic film 10 was observed using an atomic force microscope (AFM) NX10 manufactured by Park Systems. The results are shown in Table 7. In this evaluation, the smaller the step, the better the planarization characteristics. In this evaluation, a trench pattern with a depth of 0.10 μm was planarized using an organic film forming material with a normal film thickness of about 0.2 μm, which is a strict evaluation condition for evaluating the superiority or inferiority of the planarization characteristics.
[0246] [Table 7]
[0247] As shown in Table 7, the organic film forming material of the present invention (Examples 4-1 to 4-19) had a smaller step between the organic film in the trench portion and the non-trench portion than Comparative Examples 4-1 to 4-3, and was confirmed to have excellent planarization characteristics. In Comparative Examples 4-1 to 4-2, the heat resistance was insufficient as shown in the heat resistance evaluation, and the filling property was ensured as shown in the filling property evaluation, but the film shrunk during high-temperature baking, resulting in deterioration of flatness. In Comparative Example 4-3, the crosslinking property was insufficient, so the flattening property was not good. In addition, when Examples 4-15 to 4-19 in which a high-boiling point solvent was added were compared with Examples 4-1, 4-2, 4-4, and 4-6 in which no high-boiling point solvent was added, it was found that the flatness was further improved by the addition of a high-boiling point solvent. From this result, it was found that the organic film forming material of the present invention has excellent heat resistance, so that film shrink during high-temperature baking is suppressed, and excellent flattening properties are exhibited.
[0248] Example 5 Adhesion Test (Examples 5-1 to 5-15, Comparative Examples 5-1 to 5-2) The organic film-forming materials (UDL-1 to 15, Comparative UDL-1 to 2) were applied onto a SiO2 wafer substrate, and baked at 400°C for 60 seconds under a nitrogen flow with an oxygen concentration controlled to 0.2% by volume or less to form an organic film with a thickness of 200 nm. The wafer with the organic film was cut into a square of 1 x 1 cm, and an aluminum pin with an epoxy adhesive was attached to the cut wafer using a special tool. Then, the aluminum pin was attached to the substrate by heating at 150°C for 1 hour using an oven. After cooling to room temperature, the initial adhesion was evaluated by resistance using a thin film adhesion strength measuring device (Sebastian Five-A). It should be noted that the adhesion test could not be performed on Comparative UDL-3, which did not have solvent resistance in Example 1.
[0249] Figure 5 shows an explanatory diagram of the adhesion measurement method. In Figure 5, 11 is the silicon wafer (substrate), 12 is the cured film, 13 is an aluminum pin with adhesive, 14 is the support base, 15 is the grip, and 16 indicates the tensile direction. The adhesion strength is the average value of 12 measurements, and the higher the value, the stronger the adhesion of the adhesive film to the substrate. The adhesion was evaluated by comparing the obtained values. The results are shown in Table 8.
[0250] [Table 8]
[0251] As shown in Examples 5-1 to 5-15 in Table 8, the organic film material using the compound of the present invention shows higher adhesion than Comparative Examples 5-1 and 5-2. Among them, Examples 5-1 to 5-6, 5-8, 5-10 to 5-15 including the structure of n3=2 showed high adhesion, and Examples 5-8, 5-12, and 5-13 including the structure of R3=H showed particularly high adhesion. On the other hand, Comparative Examples 5-1 and 5-2 showed low adhesion due to insufficient heat resistance. From these results, it can be seen that the compound of the present invention shows high heat resistance and adhesion to the substrate.
[0252] Example 6 Pattern formation test 1 (Examples 6-1 to 6-19, Comparative Example 6-1) The above organic film forming materials (UDL-1 to 19, comparative UDL-1) were each applied onto a silicon wafer substrate on which a 300 nm SiO2 film had been formed, and baked for 60 seconds at 400°C under a nitrogen flow with an oxygen concentration controlled to 0.2% by volume or less to form an organic film (resist underlayer film). A CVD-SiON hard mask was formed thereon, and an organic anti-reflective film material (ARC-29A: manufactured by Nissan Chemical Co., Ltd.) was further applied thereon and baked at 210°C for 60 seconds to form an organic anti-reflective film with a thickness of 80 nm, and a single layer resist for ArF of the resist upper layer film material was applied thereon and baked at 105°C for 60 seconds to form a photoresist film (resist upper layer film) with a thickness of 100 nm. An immersion protective film material (TC-1) was applied on the photoresist film and baked at 90°C for 60 seconds to form a protective film with a thickness of 50 nm. In addition, since comparative examples UDL-2 and UDL-3 had poor heat resistance and crosslinking property, it was not possible to form a CVD-SiON hard mask, and it was not possible to proceed to the subsequent pattern formation test.
[0253] The resist top layer material (ArF single layer resist) was prepared by dissolving a polymer (RP1), an acid generator (PAG1), and a basic compound (Amine1) in a solvent containing 0.1 mass% FC-430 (Sumitomo 3M Limited) in the proportions shown in Table 9, and filtering the solution through a 0.1 μm fluororesin filter.
[0254] [Table 9]
[0255] The polymer (RP1), acid generator (PAG1), and basic compound (Amine1) used are shown below.
[0256] [ka]
[0257] The immersion protective film material (TC-1) was prepared by dissolving the protective film polymer (PP1) in an organic solvent in the ratio shown in Table 10 and filtering through a 0.1 μm fluororesin filter.
[0258] [Table 10]
[0259] The polymer (PP1) used is shown below. [ka]
[0260] Next, the film was exposed using an ArF immersion exposure tool (Nikon Corporation; NSR-S610C, NA 1.30, σ 0.98 / 0.65, 35 degree dipole s-polarized illumination, 6% halftone phase shift mask), baked at 100°C for 60 seconds (PEB), and developed in a 2.38 mass% tetramethylammonium hydroxide (TMAH) aqueous solution for 30 seconds to obtain a 55 nm 1:1 positive line and space pattern.
[0261] Next, the organic anti-reflective film and the CVD-SiON hard mask were etched by dry etching using the resist pattern as a mask using a Tokyo Electron etching device, Telius, to form a hard mask pattern, the organic film was etched using the obtained hard mask pattern as a mask to form an organic film pattern, and the SiO2 film was etched using the obtained organic film pattern as a mask. The etching conditions are as follows:
[0262] Transfer conditions of resist pattern onto SiON hard mask. Chamber pressure 10.0Pa RF power: 1,500W CF4 gas flow rate: 75sccm O2 gas flow rate: 15sccm Time 15sec
[0263] Conditions for transferring hard mask patterns to organic films. Chamber pressure 2.0Pa RF power 500W Ar gas flow rate: 75sccm O2 gas flow rate: 45sccm Time 120sec
[0264] Transfer conditions of organic film pattern onto SiO2 film. Chamber pressure 2.0Pa RF power: 2,200W C5F 12 Gas flow rate: 20sccm C2F6 gas flow rate: 10sccm Ar gas flow rate: 300sccm O2 gas flow rate: 60sccm Time 90sec
[0265] The cross section of the pattern was observed using an electron microscope (S-4700) manufactured by Hitachi, Ltd. The results are shown in Table 11.
[0266] [Table 11]
[0267] As shown in Table 11, the results of the organic film forming material of the present invention (Examples 6-1 to 6-19) confirmed that in all cases, the resist upper layer film pattern was successfully transferred to the substrate, and the organic film forming material of the present invention is suitable for use in microfabrication by the multi-layer resist method. In Comparative Example 6-1, although the heat resistance was insufficient, a pattern could be formed.
[0268] In addition, the organic film forming material (UDL1-19) of the present invention can form an organic film that exhibits excellent adhesion to the substrate, and thus can suppress peeling of the CVD-SiON hard mask formed directly on the organic film and the resist upper layer film formed thereon. As a result, in Examples 6-1 to 6-19, as described above, the resist upper layer film pattern was finally transferred well to the substrate.
[0269] Example 7 Pattern formation test 2 (Examples 7-1 to 7-19, Comparative Example 7-1) The above organic film forming materials (UDL-1 to 19, Comparative UDL-1) were each applied onto a SiO2 wafer substrate having a trench pattern (trench width 10 μm, trench depth 0.10 μm) and baked at 400°C for 60 seconds under a nitrogen flow with an oxygen concentration controlled to 0.2 volume % or less. Except for this, a coating film was formed in the same manner as in Pattern Formation Test 1, followed by patterning and dry etching, and the shape of the resulting pattern was observed. The results are shown in Table 12.
[0270] [Table 12]
[0271] As shown in Table 12, in the results of the organic film-forming material of the present invention (Examples 7-1 to 7-19), the resist upper layer film pattern was finally transferred to the substrate well in all cases, and it was confirmed that the organic film-forming material of the present invention is suitably used for microfabrication by the multilayer resist method. On the other hand, in Comparative Example 7-1, as shown in the results of the planarization characteristic evaluation, the planarization characteristic was poor, so that pattern collapse occurred during pattern processing, and ultimately a good pattern could not be obtained.
[0272] In addition, the organic film forming material of the present invention (Examples 7-1 to 7-19) can form an organic film that exhibits excellent adhesion to the substrate, and thus can suppress peeling of the CVD-SiON hard mask formed directly on the organic film and the resist upper layer film formed thereon. As a result, in Examples 7-1 to 7-19, as described above, the resist upper layer film pattern can be successfully transferred to the substrate.
[0273] From the above, it has become clear that the organic film-forming material of the present invention, which contains the organic film-forming compound of the present invention, has heat resistance of 400°C or more even under an oxygen-free inert gas, excellent adhesion to the substrate, and high-level filling / planarization properties, and is therefore extremely useful as an organic film-forming material for use in a multilayer resist method, and furthermore, that the pattern formation method of the present invention using this material makes it possible to form fine patterns with high precision even if the workpiece is a substrate having steps.
[0274] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
[0275] The present specification includes the following aspects. [1]: A material for forming an organic film, (A) an organic film-forming compound represented by the following general formula (1A), and (B) an organic solvent A material for forming an organic film, comprising: [ka] (In the formula, Y is an n1-valent organic group, a trivalent nitrogen atom or a tetravalent carbon atom, n1 is an integer of 3 to 8, and X is a partial structure represented by the following general formula (1B).) [ka] (In the formula, the dashed line represents a bond. R1 and R2 represent a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkyloxy group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms, and a hydrogen atom on a carbon atom constituting the alkyl group, alkyloxy group, alkynyl group, or alkenyl group may be substituted with a fluorine atom. In addition, aromatic rings that may be substituted with R1 may form a bridged structure via a single bond or a divalent group obtained by removing one hydrogen atom from R1. n4 and n5 represent integers of 0 to 2. Ar1 and Ar2 represent a benzene ring or a naphthalene ring, respectively. n2 represents 0 or 1, n3 represents 1 or 2, and R3 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms.) [2]: The material for forming an organic film according to [1], wherein R3 in the general formula (1B) is any one of those represented by the following formula (1C): [ka] (The dashed lines in the above formula represent bonds.) [3]: The material for forming an organic film according to [1] or [2], characterized in that n1 in the general formula (1A) is 3 or 4. [4]: A material for forming an organic film according to any one of [1] to [3], characterized in that n2 in the general formula (1B) is 1. [5]: A material for forming an organic film according to any one of [1] to [4], characterized in that Y in the general formula (1A) is any one of the partial structures shown in the following formula (1D). [ka] (The dashed lines in the above formula represent bonds, and R4 represents a hydrogen atom or a methyl group.) [6]: Any one of the organic film-forming materials of [1] to [5], characterized in that the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn of the component (A) in terms of polystyrene as determined by a gel permeation chromatography method is 1.00≦Mw / Mn≦1.10. [7]: The material for forming an organic film according to any one of [1] to [6], characterized in that the (B) organic solvent is a mixture of one or more organic solvents having a boiling point of less than 180°C and one or more organic solvents having a boiling point of 180°C or higher. [8]: The material for forming an organic film according to any one of [1] to [7], further comprising one or more of (C) an acid generator, (D) a surfactant, (E) a crosslinking agent, and (F) a plasticizer. [9]: A substrate for manufacturing a semiconductor device, characterized in that an organic film is formed on the substrate by hardening any one of the organic film-forming materials [1] to [8].
[10] : A method for forming an organic film applied in a manufacturing process of a semiconductor device, comprising spin-coating any one of the organic film-forming materials [1] to [8] onto a substrate to be processed, and subjecting the substrate to which the organic film-forming material has been applied to a heat treatment in an inert gas atmosphere at a temperature of 50°C or higher and 600°C or lower for a period of 5 to 7200 seconds to obtain a hardened film.
[11] : A method for forming an organic film applied in a manufacturing process of a semiconductor device, comprising spin-coating a substrate to be processed with any one of the organic film-forming materials [1] to [8], heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 50°C or higher and 300°C or lower for a period of 5 to 600 seconds to form a coating film, and subsequently heat-treating the substrate in an inert gas atmosphere at a temperature of 200°C or higher and 600°C or lower for a period of 10 to 7200 seconds to obtain a hardened film.
[12] : The method for forming an organic film according to
[10] or
[11] , wherein the oxygen concentration in the inert gas is 1 volume % or less.
[13] : The method for forming an organic film according to any one of
[10] to
[12] , characterized in that the substrate to be processed has a structure or step having a height of 30 nm or more.
[14] : A method for forming a pattern, comprising the steps of: forming an organic film on a workpiece using any one of the organic film-forming materials [1] to [8]; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming a resist top layer film on the silicon-containing resist intermediate film using a photoresist composition; forming a circuit pattern on the resist top layer film; transferring the pattern to the silicon-containing resist intermediate film by etching using the resist top layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.
[15] : A method for forming a pattern, comprising: forming an organic film on a workpiece using any one of the organic film-forming materials [1] to [8]; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming an organic antireflective film on the silicon-containing resist intermediate film; forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; transferring the pattern to the organic antireflective film and the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.
[16] : A pattern forming method comprising the steps of: forming an organic film on a workpiece using any one of the organic film-forming materials [1] to [8]; forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film; forming a resist upper layer film on the inorganic hard mask using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the inorganic hard mask by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.
[17] : A method for forming a pattern, comprising the steps of: forming an organic film on a workpiece using any one of the organic film-forming materials [1] to [8]; forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film; forming an organic antireflective film on the inorganic hard mask; forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; transferring the pattern to the organic antireflective film and the inorganic hard mask by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.
[18] : The pattern formation method according to
[16] or
[17] , wherein the inorganic hard mask is formed by a CVD method or an ALD method.
[19] : A pattern formation method according to any one of
[14] to
[18] , characterized in that in forming the circuit pattern, the circuit pattern is formed by lithography using light having a wavelength of 10 nm or more and 300 nm or less, direct drawing with an electron beam, nanoimprinting, or a combination of these.
[20] : The method for forming a pattern according to any one of
[14] to
[19] , characterized in that in forming the circuit pattern, the circuit pattern is developed using an alkaline developer or an organic solvent.
[21] : The pattern formation method according to any one of
[14] to
[20] , characterized in that the workpiece is a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.
[22] : The pattern formation method according to
[21] , characterized in that the workpiece contains silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
[23] : A compound represented by the following general formula (1A). [ka] (In the formula, Y is an n1-valent organic group, a trivalent nitrogen atom or a tetravalent carbon atom, n1 is an integer of 3 to 8, and X is a partial structure represented by the following general formula (1B).) [ka] (In the formula, the dashed line represents a bond. R1 and R2 represent a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkyloxy group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms, and a hydrogen atom on a carbon atom constituting the alkyl group, alkyloxy group, alkynyl group, or alkenyl group may be substituted with a fluorine atom. In addition, aromatic rings that may be substituted with R1 may form a bridged structure via a single bond or a divalent group obtained by removing one hydrogen atom from R1. n4 and n5 represent integers of 0 to 2. Ar1 and Ar2 represent a benzene ring or a naphthalene ring, respectively. n2 represents 0 or 1, n3 represents 1 or 2, and R3 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms.)
[24] : The compound according to
[23] , wherein R3 in the general formula (1B) is any one of those represented by the following formula (1C): [ka] (The dashed lines in the above formula represent bonds.)
[25] : The compound according to
[23] or
[24] , wherein n1 in the general formula (1A) is 3 or 4.
[26] : Any one of the compounds
[23] to
[25] , wherein n2 in the general formula (1B) is 1.
[27] : Any one of the compounds
[23] to
[26] , wherein Y in the general formula (1A) is any one of the partial structures shown in the following formula (1D). [ka] (The dashed lines in the above formula represent bonds, and R4 represents a hydrogen atom or a methyl group.) [Explanation of symbols]
[0276] 1...substrate, 2...processed layer, 2a...pattern formed on processed layer, 3...organic film, 3a...organic film pattern, 3'...material for forming organic film, 4...silicon-containing resist intermediate film, 4a...silicon-containing resist intermediate film pattern, 5...resist upper layer film, 5a...resist upper layer film pattern, 6...desired portion (exposed portion), 7...underlying substrate having dense hole pattern, 8...organic film, 9...underlying substrate having large isolated trench pattern, 10...organic film, delta 10...difference in film thickness of resist intermediate film between trench portion and non-trench portion, 11...silicon wafer, 12...cured film, 13...aluminum pin with adhesive, 14...support, 15...gripping, 16...tensile direction.
Claims
1. An organic film-forming material, (A) an organic film-forming compound represented by the following general formula (1A), and (B) an organic solvent A material for forming an organic film, comprising: 【Chemistry 1】 (In the formula, Y is an n1-valent organic group, a trivalent nitrogen atom, or a tetravalent carbon atom, n1 is an integer from 3 to 8, and X is a partial structure represented by the following general formula (1B).) 【Chemistry 2】 (In the formula, the dashed lines represent bonds. 1 , R 2 represents a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkyloxy group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms, and a hydrogen atom on a carbon atom constituting the alkyl group, alkyloxy group, alkynyl group, or alkenyl group may be substituted with a fluorine atom. 1 The aromatic rings which may be substituted with R 1 A bridge structure may be formed via a divalent group obtained by removing one hydrogen atom from R. n4 and n5 each represent an integer of 0 to 2. Ar1 and Ar2 each represent a benzene ring or a naphthalene ring. n2 represents 0 or 1, n3 represents 1 or 2, and R 3 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms.
2. R in the general formula (1B) 3 The material for forming an organic film according to claim 1, characterized in that it is any of those represented by the following formula (1C): 【Chemistry 3】 (The dashed lines in the above formula represent bonds.)
3. 2. The organic film-forming material according to claim 1, wherein n1 in the general formula (1A) is 3 or 4.
4. 2. The organic film-forming material according to claim 1, wherein n2 in the general formula (1B) is 1.
5. 2. The material for forming an organic film according to claim 1, wherein Y in the general formula (1A) is any of the partial structures shown in the following formula (1D): 【Chemistry 4】 (The dashed lines in the above formula represent bonds, and R 4 represents a hydrogen atom or a methyl group.)
6. 2. The organic film-forming material according to claim 1, wherein the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn of the component (A) in terms of polystyrene as determined by gel permeation chromatography is 1.00≦Mw / Mn≦1.
10.
7. 2. The organic film-forming material according to claim 1, wherein the organic solvent (B) is a mixture of one or more organic solvents having a boiling point of less than 180° C. and one or more organic solvents having a boiling point of 180° C. or higher.
8. The material for forming an organic film according to claim 1, further comprising one or more of (C) an acid generator, (D) a surfactant, (E) a crosslinking agent, and (F) a plasticizer.
9. A substrate for manufacturing a semiconductor device, comprising a substrate on which an organic film is formed by curing the organic film-forming material according to claim 1 .
10. A method for forming an organic film applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material according to any one of claims 1 to 8 onto a substrate to be processed, and subjecting the substrate to which the organic film-forming material has been applied to a heat treatment in an inert gas atmosphere at a temperature of 50°C or higher and 600°C or lower for a period of 5 to 7200 seconds to obtain a cured film.
11. A method for forming an organic film applied in a manufacturing process of a semiconductor device, comprising spin-coating the organic film-forming material according to any one of claims 1 to 8 onto a substrate to be processed, heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 50°C or higher and 300°C or lower for a period of 5 to 600 seconds to form a coating film, and subsequently heat-treating the substrate to which the organic film-forming material has been applied in air at a temperature of 200°C or higher and 600°C or lower for a period of 10 to 7200 seconds in an inert gas atmosphere to obtain a cured film.
12. 11. The method for forming an organic film according to claim 10, wherein the oxygen concentration in the inert gas is set to 1% by volume or less.
13. 11. The method for forming an organic film according to claim 10, wherein the substrate to be processed has a structure or step having a height of 30 nm or more.
14. A pattern forming method comprising the steps of: forming an organic film on a workpiece using the organic film-forming material according to any one of claims 1 to 8; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming a resist top layer film on the silicon-containing resist intermediate film using a photoresist composition; forming a circuit pattern on the resist top layer film; transferring the pattern to the silicon-containing resist intermediate film by etching using the resist top layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.
15. A pattern forming method comprising the steps of: forming an organic film on a workpiece using the organic film-forming material according to any one of claims 1 to 8; forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material; forming an organic antireflective film on the silicon-containing resist intermediate film; forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; transferring the pattern to the organic antireflective film and the silicon-containing resist intermediate film by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film to which the pattern has been transferred as a mask.
16. 9. A pattern forming method comprising the steps of: forming an organic film on a workpiece using the organic film-forming material according to claim 1; forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film; forming a resist upper layer film on the inorganic hard mask using a photoresist composition; forming a circuit pattern on the resist upper layer film; transferring the pattern to the inorganic hard mask by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.
17. 9. A pattern forming method comprising the steps of: forming an organic film on a workpiece using the organic film-forming material according to claim 1; forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxynitride film, a titanium oxide film, and a titanium nitride film on the organic film; forming an organic antireflective film on the inorganic hard mask; forming a resist upper layer film on the organic antireflective film using a photoresist composition to form a four-layer film structure; forming a circuit pattern on the resist upper layer film; transferring the pattern to the organic antireflective film and the inorganic hard mask by etching using the resist upper layer film on which the pattern has been formed as a mask; transferring the pattern to the organic film by etching using the inorganic hard mask on which the pattern has been transferred as a mask; and further transferring the pattern to the workpiece by etching using the organic film on which the pattern has been transferred as a mask.
18. 17. The pattern formation method according to claim 16, wherein the inorganic hard mask is formed by a CVD method or an ALD method.
19. 15. The pattern forming method according to claim 14, wherein the circuit pattern is formed by lithography using light having a wavelength of 10 nm or more and 300 nm or less, direct writing with an electron beam, nanoimprinting, or a combination thereof.
20. 15. The pattern forming method according to claim 14, wherein in forming the circuit pattern, the circuit pattern is developed with an alkali developer or an organic solvent.
21. 15. The pattern forming method according to claim 14, wherein the workpiece is a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.
22. 22. The pattern formation method according to claim 21, wherein the workpiece contains silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
23. A compound represented by the following general formula (1A): 【Chemistry 5】 (In the formula, Y is an n1-valent organic group, a trivalent nitrogen atom, or a tetravalent carbon atom, n1 is an integer from 3 to 8, and X is a partial structure represented by the following general formula (1B).) 【Chemistry 6】 (In the formula, the dashed lines represent bonds. 1 , R 2 represents a halogen atom, an alkyl group having 1 to 4 carbon atoms, an alkyloxy group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms, and a hydrogen atom on a carbon atom constituting the alkyl group, alkyloxy group, alkynyl group, or alkenyl group may be substituted with a fluorine atom. 1 The aromatic rings which may be substituted with R 1 A bridge structure may be formed via a divalent group obtained by removing one hydrogen atom from R. n4 and n5 each represent an integer of 0 to 2. Ar1 and Ar2 each represent a benzene ring or a naphthalene ring. n2 represents 0 or 1, n3 represents 1 or 2, and R 3 represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an alkynyl group having 2 to 4 carbon atoms, or an alkenyl group having 2 to 4 carbon atoms.
24. R in the general formula (1B) 3 The compound according to claim 23, characterized in that is any of those represented by the following formula (1C): 【Chemistry 7】 (The dashed lines in the above formula represent bonds.)
25. The compound according to claim 23, characterized in that n1 in the general formula (1A) is 3 or 4.
26. The compound according to claim 23, characterized in that n2 in the general formula (1B) is 1.
27. The compound according to claim 23, characterized in that Y in the general formula (1A) is any of the partial structures shown in the following formula (1D). 【Chemistry 8】 (The dashed lines in the above formula represent bonds, and R 4 represents a hydrogen atom or a methyl group.)
Citation Information
Patent Citations
Urethane (METH)acrylate compound and actinic energy ray curable resin composition using the same
JP2004196965A
Material for forming photoresist lower layer film and method for forming pattern
JP2005128509A
Resist lower layer film material and pattern forming method
JP2006285095A
Photoresist undercoat-forming material and patterning process
JP2006293298A
Method for forming resist underlayer film, patterning process using the same, and resist underlayer film material