Magnetic steel sheet having insulating coating

The electrical steel sheet with a Si and Mn-based insulating coating addresses cracking and sticking issues by maintaining film integrity during strain relief annealing, ensuring effective adhesion and reducing electrical shorts.

JP2024150349AActive Publication Date: 2024-10-23JFE STEEL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023063726
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

Conventional electrical steel sheets with insulating coatings face issues of cracking and poor sticking resistance during strain relief annealing, leading to potential electrical short circuits and decreased adhesion.

Method used

The insulating coating on the electrical steel sheet contains specific ratios of Si and Mn, with a mass ratio of Mn/Si between 0.010 and 0.100, along with an organic component, to enhance bonding and prevent cracking and sticking.

Benefits of technology

The coating effectively suppresses cracking and ensures excellent sticking resistance, maintaining the integrity of the insulating film during high-temperature annealing, thereby preventing electrical shorts and improving magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150349000001
    Figure 2024150349000001
  • Figure 2024150349000002
    Figure 2024150349000002
  • Figure 2024150349000003
    Figure 2024150349000003
Patent Text Reader

Abstract

To provide a magnetic steel sheet having an insulating coating, capable of suppressing the cracks of an insulating coating after annealing for removing strain and excellent even in sticking resistance.SOLUTION: A magnetic steel sheet having an insulating coating includes a magnetic steel sheet and an insulating coating formed on at least one surface of the magnetic steel sheet. The insulating coating includes Si and Mn, and the mass ratio Mn / Si in the insulating coating is 0.010 or more and 0.100 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrical steel sheet with an insulating coating. [Background technology]

[0002] Insulating coatings for magnetic steel sheets used in motors, transformers, etc., are required to have various properties, such as interlaminar resistance, convenience during processing and molding, and stability during storage and use. In particular, insulating coatings with excellent punchability can reduce the number of times dies need to be replaced during punching. Since magnetic steel sheets are used for a variety of purposes, various insulating coatings have been developed according to the purpose. In addition, when magnetic steel sheets are subjected to punching, shearing, bending, etc., residual strain causes deterioration of the magnetic properties, so in order to eliminate this, they are often subjected to stress relief annealing at temperatures of about 700 to 800°C. Therefore, in this case, the insulating coating must be able to withstand stress relief annealing.

[0003] The insulating coating of electromagnetic steel sheets can be broadly divided into (1) Inorganic coating that emphasizes weldability and heat resistance and can withstand stress relief annealing. (2) Resin-containing inorganic coating (i.e., semi-organic coating) that can withstand stress relief annealing in order to achieve both punchability and weldability; (3) Organic coatings for special purposes that cannot be annealed for distortion relief Among these, the coatings that can withstand stress relief annealing as general-purpose products are those containing inorganic components as shown in (1) and (2) above, both of which generally contain chromium compounds. In particular, chromium-based insulating coatings of type (2) are widely used because they can be manufactured in a one-coat, one-bake process, and therefore have significantly improved punchability compared to inorganic insulating coatings.

[0004] However, in recent years, environmental awareness has increased, and in the field of electrical steel sheets, chromate-free products with insulating coatings that do not contain chromium compounds are desired by customers etc. The following are technologies for forming insulating coatings that fall under the above (2) by applying a surface treatment liquid that does not contain chromium compounds and that contains both organic and inorganic components to the surface of electrical steel sheets.

[0005] Patent Document 1 describes an electrical steel sheet with an insulating coating, which has an insulating coating formed by applying to at least one side of an electrical steel sheet and drying a surface treatment agent containing trialkoxysilane and / or dialkoxysilane (A), in which the substituents bonded to Si are at least one non-reactive substituent selected from hydrogen, an alkyl group, and a phenyl group, a silane coupling agent (B), and plate-like silica (C). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2013 / 031200 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in conventional electrical steel sheets with an insulation coating, such as that described in Patent Document 1, there is a risk of cracks occurring in the insulation coating after stress relief annealing. If cracks occur in the insulation coating, it is thought that the adhesion of the coating will decrease due to a decrease in the bonding strength within the coating. If the adhesion of the coating decreases due to a decrease in the bonding strength within the coating, the insulation coating may peel off, causing various problems.

[0008] Furthermore, if electrical steel sheets stick to each other during stress relief annealing, an electrical short circuit occurs, causing a problem of increased iron loss. For this reason, electrical steel sheets with an insulating coating are required to not stick to each other during stress relief annealing, i.e., to have excellent sticking resistance.

[0009] In view of the above problems, an object of the present invention is to provide an electrical steel sheet with an insulation coating in which cracking of the insulation coating is suppressed after stress relief annealing and which also has excellent sticking resistance. [Means for solving the problem]

[0010] As a result of intensive research conducted by the present inventors in order to achieve this object, it was discovered that, in an insulating coating containing a Si compound, when the Mn in the insulating coating is in a certain range in terms of mass ratio Mn / Si, cracking of the insulating coating after stress relief annealing can be suppressed and excellent sticking resistance can be achieved.

[0011] The gist and configuration of the present invention, which has been completed based on the above findings, are as follows. [1] A magnetic coil assembly comprising an electromagnetic steel sheet and an insulating coating formed on at least one surface of the electromagnetic steel sheet, An electrical steel sheet with an insulation coating, wherein the insulation coating contains Si and Mn, and a mass ratio Mn / Si in the insulation coating is 0.010 or more and 0.100 or less.

[0012] [2] The insulating coating contains an organic component, and the ratio of the organic component (mass%) in the insulating coating to Si is SiO 2 The electrical steel sheet with an insulation coating according to the above [1], wherein the converted amount (mass%) is 0.70 or less.

[0013] [3] A motor having an iron core formed by laminating the insulating coated electrical steel sheets according to [1] or [2] above.

[0014] [4] A transformer having an iron core formed by laminating the insulating coating-coated electrical steel sheets according to [1] or [2] above. Effect of the Invention

[0015] The electrical steel sheet with an insulating coating of the present invention is inhibited from cracking in the insulating coating after stress relief annealing, and also has excellent sticking resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] An electrical steel sheet with an insulating coating according to one embodiment of the present invention comprises an electrical steel sheet and an insulating coating formed on at least one side of the electrical steel sheet.

[0017] [Electromagnetic steel sheet] The electromagnetic steel sheet (base steel sheet) that serves as the base of the insulating coating is not limited to a specific electromagnetic steel sheet. For example, an electromagnetic steel sheet having a general composition can be used. General components include Si, Mn, Al, etc., with the balance being Fe and unavoidable impurities. Usually, the Si content is 0.05 to 7.0 mass%, the Mn content is 0.05 to 10.0 mass%, and the Al content is 2.0 mass% or less.

[0018] The type of electrical steel sheet is not particularly limited, and any of so-called soft iron sheets (electrical steel sheets) with high magnetic flux density, general cold-rolled steel sheets such as SPCC, non-oriented electrical steel sheets containing Si or Al to increase resistivity, etc. Non-oriented electrical steel sheets conforming to JIS C2552:2014 and oriented electrical steel sheets conforming to JIS C2553:2019 can be preferably used.

[0019] [Insulating coating] In this embodiment, the insulating coating contains Si and Mn, and optionally further contains an organic component.

[0020] Coating weight is 0.05g / m 2 More than 1.50g / m 2 It is preferable that the coating weight is 0.05 g / m or less. 2 If the coating thickness is more than 1.50g / m, corrosion resistance can be ensured. 2 The coating adhesion can be obtained by measuring the weight of the electrical steel sheet before the insulating coating is formed and the weight of the electrical steel sheet with the insulating coating, and calculating the difference between the weights.

[0021] The components contained in the insulating coating will be described below.

[0022] The insulating coating containing Si can be formed by using a Si compound as a raw material. Examples of the Si compound include colloidal silica, fumed silica, alkoxysilane, silane coupling agent, and siloxane, and one or more selected from these can be used.

[0023] The alkoxysilane is not particularly limited, but one or more selected from trialkoxysilanes and dialkoxysilanes can be used.

[0024] The type of trialkoxysilane is not particularly limited, and is represented by the general formula R1Si(OR') 3 and one or more of them can be used. R1 is a non-reactive substituent selected from hydrogen, an alkyl group, and a phenyl group. When R1 is an alkyl group, it is preferably a linear or branched alkyl group having 1 to 6 carbon atoms, more preferably a linear or branched alkyl group having 1 to 3 carbon atoms. R' is an alkyl group, preferably a linear or branched alkyl group having 1 to 4 carbon atoms, more preferably a linear or branched alkyl group having 1 to 2 carbon atoms. For example, methyltrimethoxysilane, ethyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, phenyltriethoxysilane, phenyltrimethoxysilane, and hydrolysates thereof can be used. Among them, trialkoxysilanes in which R1 is an alkyl group are preferred from the viewpoint of providing more excellent corrosion resistance of the electrical steel sheet.

[0025] The type of dialkoxysilane is not particularly limited, and has the general formula R2R3Si(OR'') 2 and one or more of them can be used. Here, R2 and R3 are non-reactive substituents selected from hydrogen, an alkyl group, and a phenyl group, and are preferably linear or branched alkyl groups having 1 to 6 carbon atoms, and more preferably linear or branched alkyl groups having 1 to 3 carbon atoms. R'' is an alkyl group, and is preferably linear or branched alkyl groups having 1 to 4 carbon atoms, and more preferably linear or branched alkyl groups having 1 to 2 carbon atoms. For example, dimethyldimethoxysilane, dimethyldiethoxysilane, diphenyldimethoxysilane, and hydrolysates thereof can be used. Among them, dialkoxysilanes in which R2 and R3 are alkyl groups are preferred from the viewpoint of providing more excellent corrosion resistance of the electrical steel sheet.

[0026] The type of silane coupling agent is not particularly limited, and may be represented by the general formula XSi(R4): n(OR) 3-n (wherein n ranges from 0 to 2), and one or more of these groups may be used. X is at least one reactive functional group selected from an active hydrogen-containing amino group, an epoxy group, a mercapto group, and a methacryloxy group. R4 is an alkyl group, preferably a linear or branched alkyl group having 1 to 4 carbon atoms, and more preferably a linear or branched alkyl group having 1 to 2 carbon atoms. OR is any hydrolyzable group, and R is, for example, an alkyl group, preferably a linear or branched alkyl group having 1 to 4 carbon atoms, and more preferably a linear or branched alkyl group having 1 to 2 carbon atoms. R is, for example, an acyl group (-COR5), and R5 is preferably a linear or branched alkyl group having 1 to 4 carbon atoms, and more preferably a linear or branched alkyl group having 1 to 2 carbon atoms. Examples of silane coupling agents that can be used include N-2-(aminoethyl)3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, vinyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, and hydrolyzates thereof. Among these, silane coupling agents having an amino group or an epoxy group are preferred from the viewpoint of providing superior corrosion resistance to the electromagnetic steel sheet.

[0027] The type of siloxane is not particularly limited, and can be represented by the general formula R 3 SiO-(R 2 SiO) n -SiR 3 and one or more of these can be used. Each R is an alkyl group or an amino group, preferably a linear or branched alkyl group having 1 to 4 carbon atoms, and more preferably a linear or branched alkyl group having 1 to 2 carbon atoms. n is not particularly limited, but is within the range of 1 to 10, for example.

[0028] As the Si compound, it is preferable to use in combination one or more types selected from the group consisting of colloidal silica and fumed silica and one or more types selected from the group consisting of alkoxysilanes, silane coupling agents, and siloxanes.

[0029] SiO of Si in the insulating film 2 The converted amount (mass %) is preferably 50 mass % or more and 90 mass % or less. 2 When the converted amount is 50 mass % or more, the insulating property is excellent. The reason for this is that SiO 2 This is because it can be considered that a certain proportion of Si exists in the insulating film. 2 If the converted amount is 90 mass % or less, cracks are unlikely to occur in the insulating coating. The reason for this is unclear, but it is thought that the Si-O bond formed in the insulating coating is strong, and the SiO 2 If the converted amount exceeds 90 mass %, the stress applied to the insulating coating is large, and it is believed that cracks will occur in the insulating coating.

[0030] SiO of Si in the insulating film 2 The converted amount (mass%) was calculated by measuring the Si content (mass%) of the coating portion by EDX analysis using a transmission electron microscope, and converting this into SiO 2 It is desirable to convert the amount into the equivalent amount (mass%). The analysis points should be about 10 points, and the average value should be used.

[0031] The insulating coating containing Mn can be formed by using a Mn compound as a raw material. Examples of Mn compounds include MnO 2 and Mn 2 O 3 One or both of these can be used.

[0032] In this embodiment, it is important that the mass ratio Mn / Si in the insulating coating is 0.010 or more and 0.100 or less.

[0033] When the mass ratio Mn / Si is 0.010 or more, the Mn content in the insulating coating is sufficient, and the effect of suppressing cracking of the insulating coating after stress relief annealing can be obtained. Although it is not clear why cracking can be suppressed when the mass ratio Mn / Si is 0.010 or more, the inventors believe that the root cause is high reactivity between Si compounds and Mn. In other words, when the mass ratio Mn / Si is 0.010 or more, it is believed that a chemical reaction is likely to occur within the insulating coating, bonds are formed between molecules, and as a result, cracking is suppressed.

[0034] On the other hand, if the mass ratio Mn / Si exceeds 0.100, the magnetic steel sheets are stuck together during stress relief annealing, resulting in poor sticking resistance. This is thought to be because the insulating coating applied to the magnetic steel sheets is highly reactive, forming new chemical bonds between the laminated magnetic steel sheets, resulting in sticking. Therefore, from the viewpoint of obtaining excellent sticking resistance, the mass ratio Mn / Si is set to 0.100 or less, preferably 0.090 or less. Here, in the past, stress relief annealing was often performed at a temperature of about 700 to 800 ° C., but recently, in order to further improve magnetic properties, stress relief annealing has been aimed at increasing the temperature, and stress relief annealing at a temperature of about 900 ° C. has been considered. In this embodiment, by setting the mass ratio Mn / Si to 0.100 or less, a remarkable effect of excellent sticking resistance in stress relief annealing at a high temperature of 900 ° C. is achieved.

[0035] In this specification, the mass ratio Mn / Si in the insulating coating is determined by Auger electron spectroscopy, which will be described below. In the case of Auger electron spectroscopy, which performs analysis in the depth direction while sputtering, the average values ​​of the Mn and Si intensities are determined from the sputtering start point to the point where the Si intensity is reduced to half from the maximum point when analyzing in the depth direction, and the average Mn intensity is divided by the average Si intensity. In this case, the number of analysis points on the insulating coating is 10 or more, and the average value of the average Mn intensity / average Si intensity of all analysis points is the "mass ratio Mn / Si" in the present invention. The part up to the point where the Si intensity is reduced to half is the "insulating coating". Needless to say, the part deeper than the point where the Si intensity is reduced to half is the "electromagnetic steel sheet".

[0036] In this embodiment, the insulating coating may contain an organic component from the viewpoint of improving various coating properties such as corrosion resistance and punchability. When the Si compound contains one or more selected from the group consisting of alkoxysilane, silane coupling agent, and siloxane, the organic component is contained in the Si compound. In addition, the organic component may be contained in the insulating coating by using an organic resin as a raw material in addition to the Si compound. There is no particular limitation on the organic resin, and any known or arbitrary resin can be used. For example, aqueous resins (emulsion, dispersion, water-soluble) such as acrylic resin, alkyd resin, polyolefin resin, styrene resin, vinyl acetate resin, epoxy resin, phenol resin, polyester resin, urethane resin, and melamine resin can be mentioned, and one or more selected from these can be used.

[0037] From the viewpoint of sufficiently improving the coating performance, the organic component (mass%) / Si ratio in the insulating coating is SiO 2 The converted amount (mass%) is preferably 0.05 or more. On the other hand, since organic components are more easily permeable to oxygen than Si compounds, if there is an excess of organic components, the corrosion resistance deteriorates. From this point of view, the SiO ratio of organic components (mass%) / Si in the insulating coating is 2 The converted amount (mass %) is preferably 0.70 or less.

[0038] The ratio of organic components (mass%) in the insulating coating to Si is SiO 2 The converted amount (mass%) is determined by the following method. The C and Si contents (mass%) of the coating are measured by EDX analysis using a transmission electron microscope. The C content (mass%) is used as the organic component (mass%). The Si content (mass%) is used as the SiO 2 Convert to the equivalent amount (mass%). Then, the organic component (mass%) / Si SiO 2 Calculate the converted amount (mass%). It is advisable to analyze about 10 points and use the average value.

[0039] In this embodiment, the insulating coating preferably comprises a Si compound serving as a Si source, a Mn compound serving as a Mn source, optionally further comprising an organic resin, and optionally further comprising other components described below.

[0040] Furthermore, in this embodiment, in addition to the above-mentioned components, the inclusion of commonly used additives such as surfactants, rust inhibitors, lubricants, and antioxidants, inorganic compounds such as boric acid and pigments, and organic compounds is not prevented. The organic compound may contain an organic acid as a contact inhibitor between the inorganic component and the organic resin. Examples of the organic acid include a polymer or copolymer containing acrylic acid. These other components can be added to an extent that does not impair the effects of the present invention, but the total solid content (mass%) of the additives / SiO 2 If the converted amount (mass%) exceeds 1.0, unreacted substances remain in the coating and reduce water resistance, so the content should be the total solid content of additives (mass%) / SiO 2 The converted amount (mass %) is preferably 1.0 or less, and more preferably 0.5 or less.

[0041] In this embodiment, impurities such as Hf and HfO are contained in the inorganic components. 2 , TiO 2 However, the total amount of these impurities is SiO 2 If the amount is 5% by mass or less based on the converted amount, no particular problem will occur.

[0042] The method for producing an insulating coated electrical steel sheet is described below. There are no particular limitations on the pretreatment of the electrical steel sheet. That is, the electrical steel sheet may be left untreated, but it is advantageous to subject the sheet to a degreasing treatment using an alkali or the like, or an acid pickling treatment using hydrochloric acid, sulfuric acid, phosphoric acid, or the like.

[0043] Next, a treatment liquid for forming an insulating coating is prepared by adding the Si compound, the Mn compound, optionally the organic resin, and optionally further the other components to deionized water and mixing them.

[0044] The treatment solution is then applied to the surface of the electrical steel sheet by any method, including roll coating, bar coating, immersion, spray coating, etc., and the most suitable method is selected depending on the shape of the electrical steel sheet to be treated, etc.

[0045] Next, the treatment liquid applied to the magnetic steel sheet is baked to form the applied treatment liquid into an insulating coating. The baking method is not particularly limited, and commonly used methods such as hot air heating, infrared heating, and induction heating can be used. The maximum sheet temperature is not particularly limited, and may be about 150 to 350°C. The heating time is not particularly limited, and may be appropriately set within a range of 1 second to 10 minutes.

[0046] Through the above steps, the electrical steel sheet with an insulation coating according to this embodiment can be manufactured.

[0047] It is preferable to form the insulating coating on both sides of the electromagnetic steel sheet, but it may be formed on only one side depending on the purpose. Also, depending on the purpose, the insulating coating of this embodiment may be formed on one side of the electromagnetic steel sheet and another insulating coating may be formed on the other side.

[0048] The electrical steel sheet with the insulation coating of this embodiment can be subjected to stress relief annealing to remove stress due to punching, for example. A preferred stress relief annealing atmosphere is N 2An atmosphere in which iron is less likely to be oxidized, such as a DX gas atmosphere, is applied. Here, the dew point is set high, for example, Dp: about 5 to 60°C, and the surface and cut end surface are slightly oxidized to further improve corrosion resistance. Generally, the preferred stress relief annealing temperature is 700 to 900°C, more preferably 700 to 800°C, but the insulation coating according to this embodiment can be stress relief annealed even at 900°C. The retention time of the stress relief annealing temperature is preferably long, more preferably 1 hour or more.

[0049] A motor according to one embodiment of the present invention is characterized in that it has an iron core formed by laminating the above-mentioned insulating coated magnetic steel sheets. Also, a transformer according to one embodiment of the present invention is characterized in that it has an iron core formed by laminating the above-mentioned insulating coated magnetic steel sheets.

[0050] That is, the electrical steel sheet with an insulating coating of this embodiment is suitable for use, for example, in the rotor core of a motor with built-in permanent magnets (IPM motor). In recent years, the drive motors used in hybrid electric vehicles (HEVs) and electric vehicles (EVs) have become much faster, and during high-speed rotation, strong centrifugal forces act on the bridge parts in which the permanent magnets are embedded. The electrical steel sheet with an insulating coating of this embodiment can withstand such centrifugal forces. Note that the application of the electrical steel sheet with an insulating coating of this embodiment is not limited to rotor cores, and it can also be used, for example, in the core of a stator (fixed part) or the like.

[0051] Using the same insulating coated steel sheet for both the rotor core component and the stator core component is advantageous in terms of yield, since the approximately circular region in the center of the stator core component, which is punched out into an approximately annular shape, can be used as the material for the rotor core component; this type of cutting is known as "common cutting" and is common.

[0052] It is preferable to perform stress relief annealing on a member punched from an insulating coated steel sheet for use as a stator core, or a stator core formed by laminating such a member. Since high strength is not required for a material for a stator core, and low core loss is important, it is preferable to release processing strain that adversely affects core loss.

[0053] Whether the steel sheets are for rotor cores or stator cores, assuming that they are to be produced in the same process, stress relief annealing is carried out to remove the processing strain imposed on the electromagnetic steel sheet when the insulating coated steel sheet is punched out, and according to the present invention, an electromagnetic steel sheet with good sticking resistance can be obtained.

[0054] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples. Not limited to this. EXAMPLES

[0055] In each test example shown in Table 1, a treatment liquid was prepared by adding a Si compound, a Mn compound, and in some cases, an organic resin to deionized water and mixing them. In Table 1, S1 to S7 representing Si compounds are shown in Table 2, M1 and M2 representing Mn compounds are shown in Table 3, and R1 and R2 representing organic resins are shown in Table 4. The total solid content concentration of each component relative to the amount of deionized water was 50 g / L.

[0056] In each test example, a test piece was cut from a 0.35 mm thick electrical steel sheet (A360 (JIS C 2552 (2000))) to a width of 200 mm and a length of 290 mm. One side of the test piece was coated with the treatment liquid using a roll coater, and the test piece was baked in a hot air baking oven at a maximum plate temperature of 200°C for a heating time of 30 seconds. After that, the test piece was allowed to cool to room temperature, and the coating adhesion weight was 0.50 g / m 2 An insulating coating of 1000 nm was obtained.

[0057] <SiO 2 Conversion amount (mass%)> The Si content (mass%) of the coating was measured by EDX analysis using a transmission electron microscope, and this was calculated as SiO 2 The amount of Si was calculated as SiO 2 Therefore, the Si content in the insulation coating is SiO 2 The analysis was performed at 10 points, and the average value was calculated as the "SiO 2 The converted amount (mass %) is shown in the table.

[0058] <Mass ratio Mn / Si> The analysis was performed using an Auger electron spectrometer (manufactured by PHISICAL ELECTRONICS, Inc.) at an accelerating voltage of 10 keV and a sample current of 0.2 μA. The depth analysis was performed at a sputtering rate of 3 nm / min (SiO 2 The Mn / Si mass ratio was calculated based on the results of this analysis, and the values ​​are shown in Table 1.

[0059] < Organic component (mass%) / SiSiO 2 Conversion amount (mass%)> The SiO ratio of organic component (mass%) / Si was calculated using the method described above. 2 The converted amount (mass %) was calculated and the value is shown in Table 1.

[0060] The electrical steel sheets with insulation coating obtained in each test example were subjected to the following evaluations, and the results are shown in Table 1.

[0061] <Cracks in the insulation coating> The surface of the insulating coating was observed using a scanning electron microscope (ULTRA PLUS manufactured by Carl Zeiss) at an accelerating voltage of 5 kV to determine the presence or absence of cracks in the insulating coating. The magnification during observation was 1000 times. ◎ and ○ were deemed to be acceptable. (Judgment criteria) ◎: No cracks ○: Some cracks ×: Cracks on the entire surface

[0062] <Anti-sticking> Ten 50mm square test pieces are stacked together and the load is 20kPa (200g / cm 2 The specimens were annealed at 900°C for 2 hours in a nitrogen atmosphere while applying a 500g pressure. A 500g weight was then dropped onto the specimens, and the drop height at which the 10 bonded specimens were divided into 5 was measured. The lower the drop height, the better the sticking resistance. ◎ and ○ were deemed to be acceptable. (Judgment criteria) ◎: 10cm or less ○: More than 10cm, less than 15cm △: More than 15cm, less than 30cm ×: More than 30cm

[0063] <Corrosion resistance> The test specimens were subjected to a humidity test (50°C, relative humidity ≧98%), and the incidence of red rust after two weeks was observed and evaluated based on the area ratio. (Judgment criteria) ◎: Red rust area ratio less than 20% ○: Red rust area ratio 20% or more, less than 40% △: Red rust area ratio 40% or more, less than 60% ×: Red rust area ratio 60% or more

[0064] [Table 1] TIFF2024150349000002.tif245153TIFF2024150349000003.tif245157

[0065] [Table 2]

[0066] [Table 3]

[0067] [Table 4] [Industrial Applicability]

[0068] INDUSTRIAL APPLICABILITY The electrical steel sheet with an insulating coating of the present invention is extremely useful as parts for motors, transformers, etc., since cracking of the insulating coating is suppressed after stress relief annealing and the electrical steel sheet has excellent sticking resistance.

Claims

1. An electrical steel sheet and an insulating coating formed on at least one surface of the electrical steel sheet, An electrical steel sheet with an insulation coating, wherein the insulation coating contains Si and Mn, and a mass ratio Mn / Si in the insulation coating is 0.010 or more and 0.100 or less.

2. The insulating coating contains an organic component, and the organic component (mass %) in the insulating coating / Si is SiO 2 2. The electrical steel sheet with an insulation coating according to claim 1, wherein the converted amount (mass%) is 0.70 or less.

3. A motor having an iron core formed by laminating the insulating coated electrical steel sheets according to claim 1 or 2.

4. A transformer having an iron core formed by laminating the insulating-coated magnetic steel sheets according to claim 1 or 2.

Citation Information

Patent Citations

  • Insulation film treatment liquid for grain oriented electric steel sheet, and manufacturing method of grain oriented electric steel sheet with insulation film

    JP2009052060A

  • Treatment agent for forming chromium free insulating coating, grain oriented silicon steel sheet having insulating coating and method for manufacturing the same

    JP2020125537A

  • Grain-oriented electromagnetic steel sheet and method for manufacturing same

    WO2020149331A1

  • Oriented electromagnetic steel sheet