Composition for additive manufacturing and method of additive manufacturing, particularly nuclear reactor component
The use of surrogate slurries and iterative protocols in additive manufacturing, coupled with in-situ volumetric testing, addresses the challenges of producing complex nuclear reactor components with uranium-containing materials, enhancing quality control and compliance.
Patent Information
- Application Number
- JP2024107361
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-03-31
AI Technical Summary
Existing additive manufacturing processes face challenges in producing complex nuclear reactor components with precise quality control and defect detection, particularly in the integration of uranium-containing materials, which require stringent manufacturing standards and inspection methods.
The development of a surrogate slurry composition for additive manufacturing, combined with iterative protocol adjustment, allows for the production of nuclear reactor components using nuclear fuel slurry, incorporating uranium-containing materials, and enables in-situ volumetric testing through light-activated dyes for defect detection.
This approach facilitates the efficient manufacturing of complex nuclear reactor components with improved quality assurance and defect identification, ensuring compliance with stringent manufacturing standards and regulatory requirements.
Smart Images

Figure 2024150486000001_ABST
Abstract
Description
[Technical field]
[0001] Technical Field and Industrial Applicability The present disclosure generally relates to compositions and additive manufacturing methods for use in additive manufacturing. In particular, the disclosed compositions can be used as surrogate slurries in additive manufacturing processes to manufacture parts, whereby additive manufacturing protocols are developed that are then used with appropriate materials, such as fuel assembly structural materials (e.g., Ni, W, Mo, or NW-Mo alloys), moderator materials (e.g., graphite, boron, or carbon-based materials), and nuclear fuel slurry materials (e.g., uranium or uranium-molybdenum-based materials), to additively manufacture semi-finished or finished parts, such as parts for use in nuclear reactors. In the case of nuclear reactor parts, the surrogate slurry includes 30% to 70% by volume of a plurality of surrogate particles selected to represent uranium-containing materials, and these surrogate particles are then replaced in the nuclear fuel slurry with particles having a composition that includes the uranium-containing material (e.g., uranium metal, uranium alloy, uranium ceramic, or uranium-molybdenum alloy). In a related aspect, the disclosed slurries and additive manufacturing processes can be used for in-situ volumetric inspection, where an additively manufactured product includes a light-activated dye component that is exposed to a light source, for example, an ultraviolet-activated dye component that is activated by exposure to ultraviolet light to generate a signal that can be inspected to identify manufacturing defects. The present disclosure also relates to the composition of the surrogate slurry, and to the composition of the nuclear fuel slurry itself. [Background technology]
[0002] In the discussion that follows, certain structures and / or methods are described. However, nothing below should be construed as an admission that these structures and / or methods constitute prior art. Applicant expressly reserves the right to demonstrate that such structures and / or methods are not prior art against the present invention.
[0003] Various processes can be used to create three-dimensional objects, for example by adding materials together (e.g., fusing liquid molecules or powder particles together) and then bonding or solidifying materials under computer control. Many different techniques exist based on melt / deposition or deposition / curing techniques, and these techniques can be used to manufacture objects of almost any shape or geometry, using digital model data from, for example, a 3D model or other electronic data source, such as a computer-aided design (CAD) model or an Additive Manufacturing File (AMF) file (usually in successive layers).
[0004] A number of these manufacturing processes are available. The main difference between the processes is in the method and materials used to deposit layers to form the part, with each method / material having its advantages and disadvantages. Some methods melt or soften a material to produce the layers. An example is fused filament fabrication (FFF), also known as fused deposition modeling (FDM), fused particle fabrication (FPF) or fused granular fabrication (FGF). It produces parts by extruding small beads or streams of material and immediately hardening the layers. Other methods harden liquid materials with various techniques, each of which uses a layer-by-layer approach to harden the liquid material to create the object being manufactured. An example is stereolithography (SL), which uses various optical or chemical curing processes (with associated photo-reactive or chemically reactive materials). In each example, the product produced has properties based on the material it is manufactured from. Summary of the Invention
[0005] In general, the present disclosure relates to compositions and methods used in additive manufacturing. Due to the continuous layer-by-layer manufacturing process, the disclosed additive manufacturing process is suitable for manufacturing complex parts. In the case of nuclear reactor components, examples of complex parts include fuel assemblies (e.g., the arrangement of fuel elements (containing fuel and combustible poison), mechanical supports of the fuel assembly structure, spacer grids (ensuring spacing between components and guiding of the fuel elements), and non-fuel tubes (also known as fuel bundles), such as control rods or core instrumentation. The complexity of the structure extends to other systems of the reactor, including various components of the primary system (meaning the system that is exposed to, in contact with, or exposed to the primary coolant), such as piping, pumps, instrumentation (or gauges), heat exchangers, and steam generators, depending on the design. Thus, the construction of fuel elements, fuel assemblies, cores, and reactor systems (or reactor systems) all require precise design and manufacturing standards, as well as extensive controls before, during, and after manufacturing, such as controls on material supply, handling, installation, inspection, and testing.
[0006] Utilizing the disclosed additive manufacturing methods has proven advantageous in the manufacture of these complex structures, particularly fuel elements and fuel assemblies, improving both the manufacturing process itself and the complex structures manufactured, including quality assurance of such structures. Utilizing the disclosed additive manufacturing methods in combination with the disclosed compositions has proven particularly advantageous for these purposes.
[0007] Embodiments disclosed herein include methods of additively manufacturing components, particularly nuclear fission reactor components, and compositions of slurries used in the additive manufacturing of such components, during additive manufacturing process development and prototype development, and in the final production of working parts.
[0008] An embodiment of a method for manufacturing a component of a nuclear reactor system includes iteratively developing an additive manufacturing protocol using a surrogate slurry, substituting the surrogate slurry with a nuclear fuel slurry in the developed additive manufacturing protocol, and manufacturing a green body (or unfired body or green body) of the component of the nuclear reactor system using the nuclear fuel slurry in the developed additive manufacturing protocol.
[0009] An embodiment of the nuclear fuel slurry for additive manufacturing includes: 30% to 45% by volume of monomer resin, 45% to 60% by volume of multiple particles; >0% to 7% by volume of dispersant, greater than 0% by volume of a photoactivated dye; greater than 0% by volume of a light absorber; greater than 0% by volume of a photoinitiator, and 0% to 20% by volume (balance) diluent The particles have a composition comprising a uranium-containing material. In some embodiments, the uranium-containing material is uranium metal, uranium alloy, uranium ceramic, or uranium-molybdenum alloy. In some embodiments, the uranium-containing material is uranium oxide, uranium dioxide, uranium carbide, uranium carbonate, uranium nitride, uranium silicide, uranium fluoride, uranium chloride, uranium oxide and tungsten cermet, uranium dioxide and tungsten cermet, uranium oxide and molybdenum cermet, or uranium dioxide and molybdenum cermet, Zr or Si-based ceramic composite (e.g., ZrC-UC or SiC-UN). In addition, other uranium-containing materials can be used, including those that include inorganic species and those that include organic ligands / anion species.
[0010] The enrichment of U235 in the uranium-containing material is greater than 0%. For some NTP applications, the enrichment is less than 20%, preferably 19.75% or less. For other NTP applications, the enrichment is 90%-98%. For some CANDU applications, the enrichment is at natural levels. For some land-based nuclear power reactor applications, the enrichment is less than 20%, preferably 4%-15%. In alternative embodiments, the enrichment of the uranium-containing material can use other fissile materials, such as thorium-based.
[0011] In one particular embodiment, the nuclear fuel slurry for additive manufacturing comprises: 30% to 45% by volume of an acrylate monomer resin; a plurality of particles having a composition comprising 45% to 60% by volume of a uranium-containing material; >0% to 7% by volume of a dispersant suitable for dispersing a plurality of particles in a nuclear fuel slurry; greater than 0% by volume of a photoactivated dye for activation during subsequent quality control testing; greater than 0% by volume of a light absorber that inhibits free radical polymerization of the slurry, thereby reducing crosslinking; 0% by volume of a photoinitiator selected to match the wavelength of light used to cure the slurry composition, and 0% to 18% by volume of methylnaphthalene as a diluent (balance) The composition comprises:
[0012] In one particular embodiment, the surrogate slurry for additive manufacturing comprises: 30% to 45% by volume of an acrylate monomer resin; a plurality of surrogate particles having a composition comprising 45% to 60% by volume of yttria-stabilized zirconia (YSZ); >0% to 7% by volume of a dispersant suitable for dispersing a plurality of particles in a nuclear fuel slurry; greater than 0% by volume of a photoactivated dye for activation during subsequent quality control testing; greater than 0% by volume of a light absorber that inhibits free radical polymerization of the slurry, thereby reducing crosslinking; a photoinitiator selected to match the wavelength of light used to cure the slurry composition, or vice versa, in an amount greater than 0% by volume; and 0% to 18% by volume of methylnaphthalene as a diluent (balance) A composition comprising:
[0013] Additive manufacturing protocols, such as stereolithography additive manufacturing protocols, can be developed using surrogate slurries by iteratively adjusting additive manufacturing parameters until the additive manufacturing protocol produces a desired part of a desired quality. An example embodiment of a method for developing additive manufacturing protocols using surrogate slurries includes preparing a first surrogate slurry for additive manufacturing, preparing a first green body (or body) from the first surrogate slurry by a first additive manufacturing technique, identifying defects present in the first green body, adjusting a composition of the first surrogate slurry or parameters of the first additive manufacturing technique based on the one or more identified defects, and producing a second green body (a) by an additive manufacturing technique from the adjusted first surrogate slurry, or (b) by the first additive manufacturing technique adjusted from the first surrogate slurry, or (c) by the first additive manufacturing technique adjusted from the adjusted first surrogate slurry.
[0014] Additionally, the embodiments disclosed herein can be used to qualify the design and verify acceptable manufacture of nuclear fission reactors or individual components of nuclear fission reactors. For example, the methods of manufacturing nuclear reactor components disclosed herein can also be used to measure and verify the performance and integrity of the fabricated structures. As such, the methods can serve as a means of verifying the qualification or providing acceptance criteria information for a nuclear reactor or reactor components by a third party, such as, for example, a government regulatory body, a government agency or department, or a commercial entity such as a power utility.
[0015] An example of such an embodiment of an in-situ volumetric inspection method includes exposing an additively manufactured product to a light source, such as light having a wavelength of 300 nm to 750 nm or ultraviolet light, where the additively manufactured product includes a photoactivatable dye component, the exposure step activating the photoactivatable dye component to generate a signal, optically inspecting the exposed additively manufactured product, and identifying manufacturing defects in the additively manufactured product based on a comparison of the signal generated by the activated photoactivatable dye component to a standard. In one particular embodiment, the additively manufactured product is a green body (or unfired body or green body) of a component of a nuclear reactor system (or system), and the additively manufactured product is produced by a stereolithography additive manufacturing protocol using a nuclear fuel slurry.
[0016] Although the disclosed reactors and cores have components with complex mechanical geometries, the integral and repeatable manufacturing, including fissile fuel material, allows the components to be manufactured more easily. Other advantages include the possibility of inspecting the components in situ or layer by layer.
[0017] The above summary, as well as the following detailed description of the embodiments, can be better understood when read in conjunction with the appended drawings, in which: It is to be understood that the described embodiments are not limited to the precise arrangements and instrumentalities shown in the drawings. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 illustrates steps in an exemplary method for manufacturing a component of a nuclear reactor system. [Diagram 2] FIG. 2 shows steps in an example of an iterative process for developing an additive manufacturing protocol using a surrogate slurry. [Diagram 3] FIG. 3 illustrates the steps in one example of an in situ volumetric inspection method. [Figure 4A] FIG. 4A includes photographs relating to visual inspection of parts produced by the methods and surrogate slurries disclosed herein. [Figure 4B]FIG. 4B includes photographs relating to visual inspection of parts produced by the methods and surrogate slurries disclosed herein. [Diagram 5] FIG. 5 is an image of a green body produced using an additive manufacturing process and a surrogate slurry consistent with those disclosed herein. [Figure 6] FIG. 6 is an image of a group of second green bodies produced using additive manufacturing processes and surrogate slurries consistent with those disclosed herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] 1 illustrates steps in an exemplary method (100) for manufacturing a component of a nuclear reactor system. The exemplary method (100) includes iteratively developing an additive manufacturing protocol (preferably a stereolithography additive manufacturing protocol) using a surrogate slurry (110), substituting a nuclear fuel slurry for the surrogate slurry in the developed additive manufacturing protocol (120), and manufacturing a green body of the component of the nuclear reactor system using the nuclear fuel slurry in the developed additive manufacturing protocol (130).
[0020] Additive manufacturing protocols can be developed and / or adapted for use with any suitable additive manufacturing process. Examples of suitable additive manufacturing processes are disclosed in ISO / ASTM 52900-15, which defines categories of additive manufacturing processes including binder jetting, directed energy deposition, material extrusion, material jetting, powder bed fusion, sheet lamination, and photopolymerization. The contents of ISO / ASTM 52900-15 are incorporated herein by reference. Stereolithography is a form of additive manufacturing that uses a photopolymerization process. In exemplary embodiments, stereolithography additive manufacturing techniques include photoinitiation (or photoinitiation) from exposure to ultraviolet or beta radiation. In some exemplary embodiments, the ultraviolet radiation is generated in a digital light processor (DLP) or stereolithography apparatus (SLA). In other exemplary embodiments, the beta radiation is generated in an electron beam (EBeam) or electron bombardment (EBI) device. Although the methods and compositions disclosed herein are described in connection with stereolithography, it is expressly contemplated that such methods and compositions may be applicable and / or adapted to other additive manufacturing processes.
[0021] In an exemplary method (100), an additive manufacturing protocol is iteratively developed (110) using a surrogate slurry. The surrogate slurry is a surrogate for the nuclear fuel slurry. In this regard, the surrogate slurry has a composition designed to mimic the behavior of the nuclear fuel slurry in an additive manufacturing process. This is accomplished by using surrogate particles for the nuclear fuel particles, and in particular by using surrogate particles selected to represent uranium-containing materials. Details regarding the surrogate slurry and its composition as well as the nuclear fuel slurry and its composition are provided below.
[0022] The additive manufacturing protocol is developed (or created) in an iterative process. For example, (a) additive manufacturing process parameters such as movement of deposition stages (spatial and temporal), temperatures associated with deposition, sequencing of steps, and (b) repeating the additive manufacturing process while adjusting the components of the slurry composition and their composition such as concentration or volume percent are adjusted in subsequent process iterations. The adjustments of (a) and (b) can be based on parameters determined from the manufactured parts. Such parameters include, for example, one or more mechanical properties, one or more chemical properties, and identification of one or more physical and / or chemical defects. The adjustments of (a) and (b) can be made separately or together to arrive at a final additive manufacturing protocol (also referred to as a developed additive manufacturing protocol). The final additive manufacturing protocol thereby includes both the slurry composition information and the digital model data. The digital model data may be, for example, a 3D model or other electronic data source such as a computer-aided design (CAD) model or an Additive Manufacturing File (AMF) file or a stereolithography contour (SLC) file.
[0023] An exemplary iterative process for developing an additive manufacturing protocol using a surrogate slurry is illustrated in FIG. 2. In the exemplary iterative process (200), a first surrogate slurry for additive manufacturing is prepared (210). The first surrogate slurry has a composition as disclosed herein. Using the first surrogate slurry, a first green body is formed by a first additive manufacturing technique (220). The first additive manufacturing technique may be any of the additive manufacturing techniques disclosed herein. The first green body is then inspected and / or tested to identify defects and other deviations from a desired final product (230). This inspection and / or testing may include any suitable inspection and testing, including mechanical, visual, and chemical.
[0024] Based on one or more identified defects and / or deviations, the composition of the first surrogate slurry or the parameters of the first additive manufacturing technique can be adjusted (240). For example, the components of the composition can be adjusted (either the material chemistry or the amounts of the components) and can be varied within the compositional ranges disclosed herein. As another example, one or more parameters of the first additive manufacturing technique can be adjusted and changed (e.g., the movement (spatial and temporal) of the deposition stage, the temperature associated with the deposition, and the sequencing of the steps, etc.). Other process parameters that can be adjusted include, for example: increasing the temperature of the resin bath to a higher temperature, reducing the viscosity, producing a more uniform printed layer thickness, adjusting the delay before irradiation to allow proper leveling of the additively manufactured printed layer, adjusting the movement speed to reduce hydraulic bearing forces and delamination of the printing window, providing multiple light exposures per layer to limit scattering and increase the depth of cure, and continuously varying the exposure intensity to optimize the desired properties (movie). Other design parameters that can be adjusted include: changing the design for thin geometries below printability, increasing / reducing pores that are too small and can be blocked by diffusion during exposure, adding drain or wash holes to the part to remove trapped resin, and combining spiral and lattice bodies to support delicate features with structurally and neutronically useful materials. The composition and / or parameter adjustments may be performed independently or in combination. Also, the composition and / or parameter adjustments can be performed in subsequent iterations of the ongoing iterative process (200) or in subsequent iterative processes (200). Alternatively, the composition of the first surrogate slurry or the parameters of the first additive manufacturing technique can be adjusted to measure (or determine) the effect of changing such composition / parameters. Such causal information can be developed (or developed) and used in subsequent iterations of the ongoing iterative process (200) or in subsequent iterative processes (200).
[0025] After adjusting the composition of the first surrogate slurry or the parameters of the first additive manufacturing technique, the exemplary iterative process (200) prepares a second green body (250). The second green body (and subsequent green bodies in the iterative process) are adjusted in one or more ways. The adjustments can include: (a) adjusting the first (or subsequent) surrogate slurry and using the adjusted surrogate slurry in the additive manufacturing technique, (b) utilizing the first surrogate slurry (i.e., the unadjusted surrogate slurry) in the adjusted first (or subsequent) additive manufacturing technique, or (c) adjusting the first (or subsequent) surrogate slurry and using the adjusted slurry in the adjusted first (or subsequent) additive manufacturing technique.
[0026] The process of preparing green bodies from surrogate slurries by additive manufacturing, identifying defects in the green bodies, and adjusting the surrogate slurry composition or additive manufacturing parameters can be repeated as necessary until an additive manufacturing protocol is arrived at that produces a green body having desired properties. The additive manufacturing protocol can then be used with the nuclear fuel slurry to produce green bodies of desired components, such as components of a nuclear reactor.
[0027] In the exemplary method 100, once the developed additive manufacturing protocol is obtained, the nuclear fuel slurry is substituted for the surrogate slurry in the developed additive manufacturing protocol (120). A green body of a component of the nuclear reactor system is then manufactured using the nuclear fuel slurry in the developed additive manufacturing protocol (130). Because the surrogate slurry resembles the nuclear fuel slurry in an additive manufacturing process, the use of the nuclear fuel slurry in the developed additive manufacturing protocol produces a green body of the component that is at least substantially (or materially) the same (or within manufacturing tolerances) as, if not identical to, that manufactured using the surrogate slurry, except for the substitution of the surrogate particles with nuclear fuel particles, e.g., uranium-containing material.
[0028] The manufactured (or shaped) green body can then be sintered to form a manufactured (or shaped) part, such as a manufactured (or shaped) part of a nuclear reactor system. Other suitable forms of hardening (or strengthening or consolidation) can also be used to form the manufactured part, including, for example, combinations of temperature, pressure, and atmosphere. The hardened manufactured part can be further processed, for example, by one or more of machining, grinding, polishing, coating, carburizing, nitriding, oxidizing, and etching.
[0029] An example of a surrogate slurry for additive manufacturing has a composition including a monomer resin, a plurality of surrogate particles, a dispersant, a photoactivated dye, a light absorber, a photoinitiator, and a diluent. An example of a nuclear fuel slurry for additive manufacturing has a composition including a monomer resin, a plurality of uranium-containing particles, a dispersant, a photoactivated dye, a light absorber, a photoinitiator, and a diluent.
[0030] Both the surrogate slurry and the nuclear fuel slurry include a monomer resin present in an amount of 30% to 45% by volume, or 35% to 40% by volume. In a particular example, the monomer resin is an acrylate (or acrylic acid ester) based monomer resin or a methacrylate (or methacrylic acid ester) based monomer, or a mixture thereof. In some embodiments, the monomer resin may be at least 50% acrylate-based, or 70% to 90% acrylate-based. In other embodiments, the acrylate-based monomer resin has functionality, e.g., monofunctional, difunctional, trifunctional, or tetrafunctional, or a mixture thereof. The acrylate-based monomer resin may be at least 50% difunctional, or at least 80% difunctional, or 70% to 90% difunctional. A particular example of a suitable acrylate-based monomer resin is hexanediol diacrylate (available under the trade name SR 238 from Sartomer (Arkema Group)). Another specific example of a suitable acrylate-based monomer resin is ethoxylated (4) pentaerythritol tetraacrylate (available under the trade name SR 494 from Sartomer (Arkema Group). Alternatively, an oligomeric resin can replace the acrylate-based monomer resin. The use of an oligomeric resin can provide improvements in the areas of shrinkage control, polymerization rate, and viscosity compared to monomeric resins.
[0031] The nuclear fuel slurry includes particles of uranium-containing material present in an amount of 30% to 70% by volume, or 30% to 60% by volume, or 45% to 60% by volume, or 50% to 55% by volume, while the surrogate slurry includes substitute particles present in an amount of 30% to 70% by volume, or 30% to 60% by volume, or 45% to 60% by volume, or 50% to 55% by volume, where the substitute particles are selected to substitute for the uranium-containing material. However, the amount of substitute particles in the surrogate slurry varies based on the interaction characteristics (e.g., absorption) of the substitute particles with the curing radiation and the substitute selection parameters. In an exemplary embodiment, the substitute particles are doped zirconia phases, carbides, nitrides, or borides, or silicon or zirconium, that sufficiently match the neutron absorption cross section and refractive index of uranium oxide. The amount of substitute particles in the substitute slurry is between 40% and 60% by volume, or between 40% and 55% by volume.
[0032] Examples of uranium-containing materials include uranium metal, uranium alloys, uranium ceramics, and uranium-molybdenum alloys. In some embodiments, the uranium-containing materials replaced with the substitute particles are uranium oxide, uranium dioxide, uranium carbide, uranium oxycarbide, uranium nitride, uranium silicide, uranium fluoride, uranium chloride, cermets of uranium oxide and tungsten, cermets of uranium dioxide and tungsten, cermets of uranium oxide and molybdenum, and cermets of uranium dioxide and molybdenum. In other embodiments, the uranium-containing materials can be represented by the chemical formula U(C,O,N,Si,F,Cl), where any one or more of carbon (C), oxygen (O), nitrogen (N), silicon (Si), fluorine (F), chlorine (Cl), and combinations thereof may be present in stoichiometric or non-stoichiometric amounts with the uranium.
[0033] Other non-limiting examples of uranium-containing materials include inorganic species such as U(OH, B, Sb, P, As, S, Se, Te, Cl, Br, I); uranium hydroxides and hydrates; uranium bromides; uranium iodides; uranium selenides; uranium tellurides; uranium chlorides; uranium sulfides; uranium borides; uranium phosphides; uranium arsenides and antimony compounds. Organic ligand / anionic species may also be used as uranium-containing materials. However, as the size of these polyatomic ions increases, there will be a limit beyond which a reduction in the concentration of uranium mass is no longer favorable for fabrication into structures for nuclear fuel-related applications. Non-limiting examples of uranium-containing materials include organic ligand / anionic species such as ammonium urinate (or ammonium uranate), uranyl carbonyl; uranyl nitrate; uranyl oxalate; uranyl peroxide; uranyl acetate; uranyl benzoate; uranyl tannate; and uranyl quinolate.
[0034] Additionally, uranium-containing materials may be additively manufactured in one form and then subsequently converted to another uniform form, for example, by nitridation, oxidation, reduction, carburization (or carbonization) during a sintering process. For example, uranium in a uranium-containing material formed during additive manufacturing can be converted to uranium oxide by an oxidation process.
[0035] In certain embodiments, the composition of the uranium-containing material that the surrogate particles are selected to replace in the surrogate slurry corresponds to the composition of the particles of the uranium-containing material in the nuclear fuel slurry. Properties that contribute to the selection of the surrogate particles include those shown in Table 1. The properties in Table 1 are listed in order of decreasing importance and are categorized into three tiers, Tier I, Tier II, and Tier III. Where applicable, the upper / lower limits included in the Selection Criteria column in Table 1 are for the value of that property for the surrogate particles in the surrogate slurry compared to (or based on) the value for that property of the uranium-containing material in the nuclear fuel slurry.
[0036] [Table 1]
[0037] The selection of surrogate particles for the surrogate slurry is a balance of the properties in Table 1. In that regard, Tier I properties have been found to be more relevant to the performance of the surrogate slurry than Tier II properties, and similarly Tier II properties have been found to be more relevant to the performance of the surrogate slurry than Tier III properties. Additionally, as a first approximation, Tier I properties can be utilized in selecting an appropriate surrogate particle. In certain examples, the surrogate particle has a composition including yttria stabilized zirconia (YSZ), alumina (Al2O3), zirconia (ZrO2), ceria (CeO2), silica (SiO2), fused silica, zirconia toughened alumina (ZTA) (Al2O3-ZrO2), alumina toughened zirconia (ATZ) (ZrO2-Al2O3), or kaolinite (Al2O3·2SiO2·2H2O). In yet another example, the surrogate particles have a composition including carbides, nitrides, borides, carbonitrides, carboborides, nitroborides, or carbonitroborides of transition metals such as silicon (Si) or zirconium (Zr), which are represented by the formula M(C,N,B) where M is a transition metal and one or more of the elements C, N, and B are present in stoichiometric or non-stoichiometric amounts. Specific examples include ZrC, ZrN, ZrB, ZrB 2、 Examples include SiC, SiN, SiB, and SiB2.
[0038] Other characteristics of the surrogate particles include a D10 particle size of 1 nm to 10μ, alternatively 40 nm to 1μ, in another embodiment the D50 particle size is 1 nm to 10μ, alternatively 40 nm to 1μ, and the D90 particle size is 1 nm to 20μ, alternatively 1 nm or 40 nm to 1μ or 12μ or 15μ.
[0039] Both the surrogate slurry and the nuclear fuel slurry include a dispersant present in an amount of >0% to 7% by volume, or 3% to 7% by volume, or 4% to 6% by volume. The particulate dispersant is selected for its ability to disperse both the surrogate particles and the particles of the uranium-containing material in the slurry composition. The amount of dispersant must be at least sufficient to adequately coat the particles, and sufficient to produce a well-dispersed, shear-thinning, non-Newtonian fluid that is not thixotropic. In one example, the slurry has a viscosity of 100,000 centipoise (cP) or less, or alternatively has a viscosity of 10,000 cP or less. If the viscosity is too high, the slurry will exhibit shear thickening.
[0040] In one aspect, the dispersant is selected such that the electrostatic affinity of the dispersant is within 20% or within 10% of the value of the electrostatic affinity of the surrogate particle. In a particular example, the dispersant is a composition containing a quaternary ammonium chloride, such as VARIQUAT® CC-9 or VARIQUAT® CC-42 (both available from Evonik Industries AG, Germany), or a high molecular weight dispersant, such as TEGO® Dispers 660 C or TEGO® Dispers 670 (both available from Evonik Industries AG, Germany). In yet another particular example, two different dispersants or a mixture of dispersants can be used. For example, the dispersant of the first composition and the dispersant of the second composition can be mixed such that the ratio of the first component to the second component (first component:second component) is in the range of 2 to 2.5, or 2.15 to 2.35.
[0041] Both the surrogate slurry and the nuclear fuel slurry include a photoactivated dye, a photoabsorber, and a photoinitiator, each present in an amount greater than 0% by volume, or between 0.05% and 0.10% by volume. In some embodiments, the photoactivated dye, photoabsorber, and photoinitiator are selected to be effective for the radiation source, for example, the photoactivated dye, photoabsorber, and photoinitiator are selected to be effective between 300 nm and 750 nm, or between 300 nm and 600 nm, or between 400 nm and 560 nm. In one example, the photoactivated dye, photoabsorber, and photoinitiator are selected to be effective in the range of 620 nm and 640 nm.
[0042] The photoactivated dye changes color upon curing, thereby providing visualization of the cured layer. Such visualization can be detected under certain wavelengths, such as ultraviolet light, and can be used for defect detection or other inspection purposes. In a particular example, the photoactivated dye is a triarylmethane dye, preferably C 25 H 30 ClN3 (available from Sigma-Aldrich Corp., USA under the trade name Crystal violet). Crystal violet is a blue aniline derivative dye. In another specific example, the photoactivated dye is present in an amount of 0.002 moles / L of monomer resin.
[0043] The light absorber absorbs incident radiation within certain wavelengths and inhibits or reduces free radical polymerization of the slurry resulting from those wavelengths, thereby reducing crosslinking. In a particular example, the light absorber is a triazine light absorber, preferably 2-hydroxyphenyl-s-triazine with 18-20% 2-methoxy-1-propyl acetate (e.g., Tinuvin® 477 available from BASF, which is a liquid triazine light absorber based on a red-shifted tris-resorcinol-triazine chromophore that exhibits high thermal stability, excellent lightfastness, and minimal interaction with metal crystals and amine crosslinkers).
[0044] The photoinitiator is selected to match the incident radiation used to cure the slurry composition (or vice versa). In a particular example, the photoinitiator is a Type I or Type II photoinitiator, preferably bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (e.g., OmniRad 819 (formerly Irgacure 819), available from IGM Resins, USA, which is a photoinitiator for the radical polymerization of unsaturated resins by exposure to ultraviolet light).
[0045] Both the surrogate slurry and the nuclear fuel slurry include a diluent present in an amount of 4% to 40% by volume, or 4% to 20% by volume, or 4% to 6% by volume, or 8% to 40% by volume, or 8% to 20% by volume, or 8% to 15% by volume. A suitable diluent is liquid at room temperature and has a boiling point low enough that it can be removed at a temperature below 400°C, or below 300°C. When the diluent is removed, small voids (or holes) remain in the manufactured parts, and in nuclear reactor components, the small voids provide an outgassing volume that helps minimize or prevent cracking of the components. In a particular example, the diluent is methylnaphthalene.
[0046] The disclosed nuclear fuel slurry can be used in additive manufacturing processes. Suitable additive manufacturing equipment can be used that can be adapted to the specific requirements of the materials used in the manufacture of the parts (e.g., chemical resistance), the specific requirements for the use of the equipment itself (e.g., specific atmospheric or vacuum requirements), as well as the dimensions and shapes of the parts to be manufactured. Examples of suitable additive manufacturing equipment include SLA and DLP machines, electron beam-based additive manufacturing equipment, and DLP stereolithography equipment, any of which can be modified or adapted for specific requirements.
[0047] An exemplary method of additive manufacturing may include providing a concept (or design or blueprint) of a part to be manufactured to a controller of an additive manufacturing device. Such concept may be incorporated into an additive manufacturing protocol.
[0048] In an exemplary method, a supply volume of nuclear fuel slurry composition, such as a bath or reservoir, is established. A base portion of the green body of the part is then formed by hardening a portion of the slurry composition in contact with a movable base of an additive manufacturing apparatus. Alternatively, the base portion can be prefabricated before the additive manufacturing process begins. An additional portion of the green body of the part is formed layer-by-layer by first hardening a portion of the slurry composition in contact with the base portion to form a first layer of the green body, and then hardening a portion of the slurry composition in contact with a previously deposited layer of the green body to form the additional portion, while simultaneously moving (or translating) the movable base relative to the interface between the surface of the supply volume and the most recently formed additional (laminate) portion. The movement of the movable base is generally governed by the additive manufacturing protocol, according to the design of the part. In an exemplary embodiment, the movement of the movable base relative to the interface between the surface of the supply volume and the most recently formed additional portion of the green body has an X-axis resolution and a Y-axis resolution of 50μ or better, and a Z-axis resolution of 20μ or better. In an exemplary embodiment, each additional portion of the part green body that is formed layer by layer has a thickness of at least 25 μm, alternatively between 25 μm and 50 μm. Once layer-by-layer fabrication of the part green body is complete, the part green body can be removed from the additive manufacturing apparatus and sintered (or processed by other debinding / hardening techniques) to form a densified ceramic.
[0049] The disclosed methods and slurries can be incorporated into or enable in-situ volumetric inspection methods. FIG. 3 shows steps in an exemplary method (300) of in-situ volumetric inspection. The exemplary method (300) includes exposing an additively manufactured product containing a UV dye component to ultraviolet light (310). The exposure step activates the UV dye component to generate a signal, and the exposed additively manufactured product is then optically inspected (320), for example, using a magnifying device. The magnifying device, such as a stereo microscope, can include imaging capabilities as well as image analysis. Defects in the additively manufactured product can be identified (330) based on comparing the signal generated by the activated UV dye component to a standard.
[0050] As described herein, the photoactivated dye provides visualization of the cured layer by changing color upon curing. Such visualization can be detected under ultraviolet light and can be used for defect detection or other inspection purposes. Figures 4A-B include photographs for visual inspection of parts manufactured according to the methods and surrogate slurries disclosed herein. Figure 4A shows a part 410 exposed to an ultraviolet light source 420. Figure 4B shows an image 450 of the part 400 of Figure 4A. The part 410 has a test pattern in which a first region includes the photoactivated dye and a second region does not include the photoactivated dye. The distribution of the photoactivated dye is reflected in the image 450 of Figure 4B, in which the dark regions 460 correlate with the first region including the photoactivated dye and the light regions 470 correlate with the second region not including the photoactivated dye. By comparing the shape of the first region in the manufactured part to a standard of the test pattern, the quality of the manufacturing, e.g., density and shape, as well as any defects in such manufacturing can be detected. 4A-4B are shown using test patterns, similar in-situ inspection procedures can be applied to more complex parts and other quality parameters in the as-manufactured parts. Although in-situ volumetric inspection has been described herein with ultraviolet light, any suitable radiation source can be used so long as it produces a detectable signal from the structure being inspected.
[0051] Examples of slurries: Two examples of substitute slurry compositions are shown in Table 2. Both ingredients and amounts (volume % of the slurry) are provided. Substitute Slurry A is an acrylate-based slurry composition and does not contain methacrylate; Substitute Slurry B is a mixed acrylate- and methacrylate-based slurry composition. In both Substitute Slurry A and Substitute Slurry B, the substitute particles are yttria-stabilized zirconia. Substitute Slurry A has a separate diluent component, namely polyethylene glycol. Substitute Slurry B does not have a separate diluent component, but rather incorporates a diluent component in the monomer resin in the form of polyethylene glycol from the methacrylate monomer solution.
[0052] [Table 2]
[0053] One exemplary nuclear fuel slurry composition is shown in Table 3. Both ingredients and amounts (volume % of the slurry) are provided. Nuclear fuel slurry X is an acrylate-based composition and does not contain methacrylate; nuclear fuel slurry Y is a mixed acrylate- and methacrylate-based slurry composition. In both nuclear fuel slurry X and nuclear fuel slurry Y, the uranium-containing material is UO2. Nuclear fuel slurry X has a separate diluent component, namely polyethylene glycol. Nuclear fuel slurry Y does not have a separate diluent component, but rather incorporates its component in the monomer resin in the form of polyethylene glycol from a methacrylate monomer solution.
[0054] [Table 3]
[0055] Of the above examples of surrogate slurries and nuclear fuel slurries, surrogate slurries A and B had the capability to produce the green bodies of exemplary parts using AM. For example, Figure 5 is an image of a green body produced using additive manufacturing, specifically a digital light processor, using surrogate slurry A disclosed herein. The green body shown is in the form of a test structure, but can be formed into any configuration using appropriate additive manufacturing protocols.
[0056] However, when the substitute slurries were substituted for nuclear fuel slurries X and Y, the layer thickness was insufficient to form green bodies of substantial volume, i.e., green bodies of 2 mm or less were formed. Thus, while the nuclear fuel slurries of the above examples were capable of producing green bodies, the relatively small layer thicknesses and small volumes formed per layer made the production process inefficiently long.
[0057] Based on the above examples, further examples have been made and discussed. These further exemplary nuclear fuel slurry M and nuclear fuel slurry N are shown in Table 4. Both components and amounts (volume % of slurry) are provided. Nuclear fuel slurry M is an acrylate-based slurry composition and does not contain methacrylic acid; nuclear fuel slurry N is an acrylate-based slurry composition. In both nuclear fuel slurry M and nuclear fuel slurry N, the uranium-containing material is UO2. Both nuclear fuel slurry M and nuclear fuel slurry N use an independent diluent component, namely polyethylene glycol or PRO14388 (a blend of SR238 monomer / PEG-like diluent, commercially available from Sartomer).
[0058] [Table 4]
[0059] Both the nuclear fuel slurry M and the nuclear fuel slurry N were used in an additive manufacturing process, in particular using a digital light processor. The nuclear fuel slurry N produced second green bodies, three of which are shown in FIG. 6. The second green bodies shown in FIG. 6 are in the form of test structures, but can be formed into any desired structure by using the appropriate additive manufacturing protocol. The second green body shown in FIG. 6 was formed using layers (each having a thickness of about 15μ), with a height of 10 mm and a volume of UO2 material of 0.92 cm. 3 2.3cm 3 The results of the nuclear fuel slurry M and the nuclear fuel slurry N showed that the mixture of SR238 and SR494 in the nuclear fuel slurry N with respect to the monomer resins promoted improved adhesion (or cohesion) between the layers and contributed to improved mechanical properties of the hardened layers (compared to the monomers in the nuclear fuel slurry N). However, nuclear fuel slurry M did not result in a satisfactory green body because the amount and type of monomer resin (i.e., 36.7 vol. %, SR238) did not provide sufficient mechanical strength to facilitate the layer-by-layer formation process. The layers made with nuclear fuel slurry M showed brittle fracture and were only partially cohesive. From the results with nuclear fuel slurry M and nuclear fuel slurry N, it was concluded that the mixture of SR238 and SR494 in the nuclear fuel slurry N with respect to the monomer resins promoted improved adhesion (or cohesion) between the layers and contributed to improved mechanical properties of the hardened layers (compared to the monomers in the nuclear fuel slurry N).
[0060] Various embodiments disclosed herein have uranium-based materials as the fissile component, however, it should be understood that other fissile materials may be used in place of or in combination with uranium, including plutonium, thorium, americium, curium, neptunium, and combinations thereof.
[0061] Although described in the context of additively manufactured parts for nuclear reactors, the additive manufacturing methods and in-situ inspection methods disclosed herein can be applied in the manufacture of other technologies, such as the petrochemical industry (e.g., manufacturing chemical reactors), the aerospace industry (e.g., manufacturing turbine parts and housings, including turbine blades, combustion chambers, nozzles, valves, and cooling tubes, missile and rocket parts, as well as adapted to the manufacture of other complex articles. In addition, developing additive manufacturing protocols using surrogate slurries (which are then utilized with non-surrogate slurries) can also be applied to the manufacture of other technologies, such as in the petrochemical and aerospace industries mentioned above.
[0062] Although particular embodiments have been referenced, it will be apparent that other embodiments and variations may be devised by others skilled in the art without departing from the spirit and scope thereof, and it is intended that the appended claims be interpreted to include all such embodiments and equivalent variations.
Claims
1. 1. An additive manufacturing slurry comprising: 30% to 45% by volume of a monomer resin; 30% to 70% by volume of a plurality of substitute particles; >0% to 7% by volume of a dispersant; greater than 0% by volume of a photoactivated dye; greater than 0 volume percent light absorber; greater than 0% by volume of a photoinitiator, and 0% to 18% by volume of diluent as the balance (Volume % is based on the total volume of the slurry), the photoactivated dye, the photoabsorber and the photoinitiator function within an incident wavelength range of 300 nm to 750 nm; the surrogate particle is selected to substitute for the uranium-containing material by having (i) a refractive index within ±20% of the refractive index of the uranium-containing material, and (ii) an absorption cross section for the incident wavelength within ±10% of the absorption cross section of the uranium-containing material; Additive manufacturing slurries.
2. 2. The additive manufacturing slurry of claim 1, wherein the uranium-containing material substituted by the substitute particles is uranium metal, a uranium alloy, a uranium ceramic, or a uranium-molybdenum alloy.
3. 2. The additive manufacturing slurry of claim 1, wherein the uranium-containing material substituted by the substitute particles is uranium oxide, uranium dioxide, uranium carbide, uranium carbonate, uranium nitride, uranium silicide, uranium fluoride, uranium chloride, a cermet of uranium oxide and tungsten, a cermet of uranium dioxide and tungsten, a cermet of uranium oxide and molybdenum, or a cermet of uranium dioxide and molybdenum.
4. 4. The additive manufacturing slurry of claim 3, wherein the uranium-containing material substituted by the substitute particles is uranium oxide or uranium dioxide.
5. 2. The additive manufacturing slurry of claim 1, wherein the uranium-containing material substituted by the substitute particles is U(C,O,N,Si,F,Cl).
6. 6. The additive manufacturing slurry of any one of claims 1 to 5, wherein the plurality of substitute slurries have a D50 particle size of 40 nm to 10 μm.
7. 7. The additive manufacturing slurry of any one of claims 1 to 6, wherein the proxy particles have a D50 particle size value that is within ±10% of a D50 particle size of the uranium-containing material.
8. 8. The additive manufacturing slurry of claim 7, wherein the surrogate particles have a D90 particle size value that is within ±10% of a D90 particle size of the uranium-containing material.
9. 9. The additive manufacturing slurry of claim 8, wherein the surrogate particles have a D10 particle size value that is within ±10% of a D10 particle size of the uranium-containing material.
10. The plurality of surrogate particles have a specific surface area within ±10% of the specific surface area of the uranium-containing material, where the specific surface area is N 2 The slurry for additive manufacturing according to any one of claims 1 to 9, wherein the BET specific surface area is obtained from an adsorption isotherm.
11. 11. The additive manufacturing slurry of any one of claims 1 to 10, wherein the plurality of proxy particles has a morphology within ±10% of the morphology of the uranium-containing material.
12. 12. The additive manufacturing slurry of any one of claims 1 to 11, wherein the monomer resin is an acrylate based monomer resin or a methacrylate based monomer resin, or a mixture thereof.
13. 13. The additive manufacturing slurry of claim 12, wherein said monomer resin is at least 50% acrylate-based.
14. 13. The additive manufacturing slurry of claim 12, wherein the monomer resin is 70-90% acrylate based.
15. 15. The additive manufacturing slurry of any one of claims 1 to 14, wherein the acrylate based monomer resin is mono-, di-, tri- or tetra-functional, or a mixture thereof.
16. 16. The additive manufacturing slurry of claim 15, wherein the acrylate based monomer resin is at least 50% difunctional.
17. 17. The additive manufacturing slurry of claim 16, wherein said acrylate based monomer resin is at least 80% difunctional.
18. 17. The additive manufacturing slurry of claim 16, wherein the acrylate based monomer resin is 70-90% difunctional.
19. The substitute particles are alumina (Al 2 O 3 ), yttria-stabilized zirconia (YSZ), zirconia (ZrO 2 ), Celia (CeO 2 ), titania (TiO 2 ), silica (SiO 2 ), fused silica, zirconia-toughened alumina (ZTA) (Al 2 O 3- ZrO 2 ), alumina-toughened zirconia (ATZ) (ZrO 2 -Al 2 O 3 ), or kaolinite (Al 2 O 3 ・2SiO 2 ・H 2 19. The additive manufacturing slurry of any one of claims 1 to 18, having a composition comprising:
20. The substitute particles are alumina (Al 2 O 3 ), yttria-stabilized zirconia (YSZ), ceria (CeO 2 ), titania (TiO 2 20. The additive manufacturing slurry of claim 19 having a composition comprising:
21. 20. The additive manufacturing slurry of any one of claims 1 to 19, wherein the proxy particles have a composition comprising M(C,N,B), where M is a transition metal and one or more of the elements C, N and B are present in stoichiometric or non-stoichiometric amounts.
22. 22. The additive manufacturing slurry of claim 21 , wherein the transition metal is silicon or zirconium.
23. 23. The additive manufacturing slurry of any one of claims 1 to 22, wherein the diluent has a refractive index that is the same as or higher than the refractive index of the monomer resin.
24. 24. The additive manufacturing slurry of claim 23, wherein the diluent is inert.
25. 24. The additive manufacturing slurry of claim 23, wherein the diluent is methylnaphthalene.
26. The photoactivated dye is a triarylmethane dye, preferably 25 H 30 ClN 3 26. The additive manufacturing slurry of any one of claims 1 to 25, wherein the photoabsorber is a triazine based photoabsorber, preferably 2-hydroxyphenyl-s-triazine with 18-20% 2-methoxy-1-propyl acetate, and the photoinitiator is a Type I or Type II photoinitiator, preferably bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide.
27. 27. The additive manufacturing slurry of any one of claims 1 to 26, wherein the composition is curable by photoinitiation or electron beam irradiation.
28. A slurry for additive manufacturing, comprising: 30% to 45% by volume of a monomer resin; 30% to 70% by volume of the plurality of particles; >0% to 7% by volume of a dispersant; greater than 0% by volume of a photoactivated dye; greater than 0 volume percent light absorber; greater than 0% by volume of a photoinitiator, and 0% to 18% by volume of diluent as the balance (Volume % is based on the total volume of the slurry), the particles having a composition including a uranium-containing material; Additive manufacturing slurries.
29. 30. The additive manufacturing slurry of claim 28, wherein the uranium containing material is uranium metal, a uranium alloy, a uranium ceramic, or a uranium-molybdenum alloy.
30. 29. The additive manufacturing slurry of claim 28, wherein the uranium containing material is uranium oxide, uranium dioxide, uranium carbide, uranium carbonate, uranium nitride, uranium silicide, uranium fluoride, uranium chloride, a cermet of uranium oxide and tungsten, a cermet of uranium dioxide and tungsten, a cermet of uranium oxide and molybdenum, or a cermet of uranium dioxide and molybdenum.
31. 31. The additive manufacturing slurry of claim 30, wherein the uranium-containing material represented by the proxy particles is uranium oxide or uranium dioxide.
32. 32. The additive manufacturing slurry of any one of claims 28 to 31, wherein the plurality of particles has a D50 particle size of 40 nm to 10 μm.
33. 32. The additive manufacturing slurry of any one of claims 28 to 31, wherein the monomer resin is an acrylate based monomer resin or a methacrylate based monomer resin, or a mixture thereof.
34. 34. The additive manufacturing slurry of claim 33, wherein said monomer resin is at least 50% acrylate based.
35. 34. The additive manufacturing slurry of claim 33, wherein the monomer resin is 70-90% acrylate based.
36. 36. The additive manufacturing slurry of any one of claims 28 to 35, wherein the acrylate based monomer resin is mono-, di-, tri-, or tetra-functional, or a mixture thereof.
37. 37. The additive manufacturing slurry of claim 36, wherein said acrylate based monomer resin is at least 50% difunctional.
38. 38. The additive manufacturing slurry of claim 37, wherein said acrylate based monomer resin is at least 80% difunctional.
39. 38. The additive manufacturing slurry of claim 37, wherein the acrylate based monomer resin is 70-90% difunctional.
40. The photoactivated dye is a triarylmethane dye, preferably 25 H 30 ClN 3 40. The additive manufacturing slurry of any one of claims 28 to 39, wherein the photoabsorber is a triazine based photoabsorber, preferably 2-hydroxyphenyl-s-triazine with 18-20% 2-methoxy-1-propyl acetate, and the photoinitiator is a Type I or Type II photoinitiator, preferably bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide.
41. 41. The additive manufacturing slurry of any one of claims 28 to 40, wherein the diluent has a refractive index that is the same as or higher than the refractive index of the monomer resin.
42. 42. The additive manufacturing slurry of claim 41 , wherein the diluent is inert.
43. 42. The additive manufacturing slurry of claim 41 , wherein the diluent is methylnaphthalene.
44. The additive manufacturing slurry of any one of claims 28 to 43, wherein the composition is curable by photoinitiation.
45. 1. A method of manufacturing a component of a nuclear reactor system, comprising the steps of: Iteratively developing additive manufacturing protocols using surrogate slurries; replacing the surrogate slurry with a nuclear fuel slurry in the developed additive manufacturing protocol; and producing a green body for a component of a nuclear reactor system using said nuclear fuel slurry in said developed additive manufacturing protocol; Including, The substitute slurry is 30% to 45% by volume of a monomer resin; 30% to 70% by volume of a plurality of substitute particles; >0% to 7% by volume of a dispersant; greater than 0% by volume of a photoactivated dye; greater than 0 volume percent light absorber; greater than 0% by volume of a photoinitiator, and 0% to 18% by volume of diluent as the balance (Volume percentages are based on the total volume of the surrogate slurry), the photoactivated dye, the photoabsorber and the photoinitiator function within an incident wavelength range of 300 nm to 750 nm; the surrogate particle is selected to substitute for the uranium-containing material by having (i) a refractive index within ±20% of the refractive index of the uranium-containing material, and (ii) an absorption cross section for the incident wavelength within ±10% of the absorption cross section of the uranium-containing material; The nuclear fuel slurry comprises: 30% to 45% by volume of a monomer resin; 30% to 70% by volume of the plurality of particles; >0% to 7% by volume of a dispersant; greater than 0% by volume of a photoactivated dye; greater than 0% by volume of a light absorber; greater than 0% by volume of a photoinitiator, and 0% to 18% by volume of diluent as the balance (Volume percentages are based on the total volume of the nuclear fuel slurry), the particles having a composition including a uranium-containing material; A method for manufacturing nuclear reactor system components.
46. 46. The method of claim 45, wherein the uranium-containing material is uranium metal, a uranium alloy, a uranium ceramic, or a uranium-molybdenum alloy.
47. 46. The method of claim 45, wherein the uranium-containing material is uranium oxide, uranium dioxide, uranium carbide, uranium carbonate, uranium nitride, uranium silicide, uranium fluoride, uranium chloride, a cermet of uranium oxide and tungsten, a cermet of uranium dioxide and tungsten, a cermet of uranium oxide and molybdenum, or a cermet of uranium dioxide and molybdenum.
48. 48. The method of claim 47, wherein the uranium-containing material substituted by the substitute particles is uranium oxide or uranium dioxide.
49. 46. The method of claim 45, wherein the uranium-containing material substituted by the proxy particles is U(C,O,N,Si,F,Cl).
50. The method of any one of claims 45 to 49, further comprising sintering the green body to form a component of the nuclear reactor system.
51. 1. A method for developing an additive manufacturing protocol using a surrogate slurry, comprising: Preparing a first surrogate slurry for additive manufacturing; creating a first green body from the first surrogate slurry by a first additive manufacturing technique; identifying defects present in the first substrate body; adjusting the composition of the first surrogate slurry or the first additive manufacturing technique based on the one or more identified defects; and producing a second green body (a) from the adjusted first surrogate slurry by said additive manufacturing technique, (b) from the first surrogate slurry by the adjusted first additive manufacturing technique, or (c) from the adjusted first surrogate slurry by the adjusted first additive manufacturing technique. Including, The first substitute slurry comprises: 30% to 45% by volume of a monomer resin; 30% to 70% by volume of a plurality of substitute particles; >0% to 7% by volume of a dispersant; greater than 0% by volume of a photoactivated dye; greater than 0% by volume of a light absorber; greater than 0% by volume of a photoinitiator, and 0% to 18% by volume of diluent as the balance (Volume percentages are based on the total volume of the first substitute slurry), the photoactivated dye, the photoabsorber and the photoinitiator function within an incident wavelength range of 300 nm to 750 nm; the surrogate particle is selected to substitute for the uranium-containing material by having (i) a refractive index within ±20% of the refractive index of the uranium-containing material, and (ii) an absorption cross section for the incident wavelength within ±10% of the absorption cross section of the uranium-containing material; method.
52. 52. The method of claim 51, wherein the uranium-containing material substituted by the surrogate particles is uranium metal, a uranium alloy, a uranium ceramic, or a uranium-molybdenum alloy.
53. 52. The method of claim 51, wherein the uranium-containing material substituted by the substitute particles is uranium oxide, uranium dioxide, uranium carbide, uranium carbonate, uranium nitride, uranium silicide, uranium fluoride, uranium chloride, a cermet of uranium oxide and tungsten, a cermet of uranium dioxide and tungsten, a cermet of uranium oxide and molybdenum, or a cermet of uranium dioxide and molybdenum.
54. 54. The method of claim 53, wherein the uranium-containing material substituted by the substitute particles is uranium oxide or uranium dioxide.
55. 52. The method of claim 51 , wherein the uranium-containing material substituted by the substitute particles is U(C,O,N,Si,F,Cl).
56. 56. The method of any one of claims 51 to 55, wherein the first additive manufacturing technique comprises photoinitiation.
57. 1. A method of manufacturing a component of a nuclear reactor system, comprising the steps of: using an additive manufacturing protocol with the nuclear fuel slurry to produce a green body for a component of a nuclear reactor system; The additive manufacturing protocol is developed using a surrogate slurry; The nuclear fuel slurry comprises: 30% to 45% by volume of a monomer resin; 30% to 70% by volume of the plurality of particles; >0% to 7% by volume of a dispersant; greater than 0% by volume of a photoactivated dye; greater than 0 volume percent light absorber; greater than 0% by volume of a photoinitiator, and 0% to 18% by volume of diluent as the balance (Volume percentages are based on the total volume of the nuclear fuel slurry), the particles having a composition including a uranium-containing material; method.
58. 58. The method of claim 57, wherein the uranium-containing material is uranium metal, a uranium alloy, a uranium ceramic, or a uranium-molybdenum alloy.
59. 58. The method of claim 57, wherein the uranium-containing material is uranium oxide, uranium dioxide, uranium carbide, uranium carbonate, uranium nitride, uranium silicide, uranium fluoride, uranium chloride, a cermet of uranium oxide and tungsten, a cermet of uranium dioxide and tungsten, a cermet of uranium oxide and molybdenum, or a cermet of uranium dioxide and molybdenum.
60. 60. The method of claim 59, wherein the uranium-containing material is uranium oxide or uranium dioxide.
61. 58. The method of claim 57, wherein the uranium-containing material is U(C,O,N,Si,F,Cl).
62. The method of any one of claims 57 to 61, further comprising sintering the green body to form the component of a nuclear reactor system.
63. 1. A method for in-situ volumetric inspection, comprising: exposing an additively manufactured product that includes a photoactivated dye component to a light source, the exposure step activating the photoactivated dye component to form a signal; optically inspecting the exposed additively manufactured product; and Identifying manufacturing defects in the additively manufactured product based on a comparison of a signal generated by the activated photoactivated dye component to a standard. The method includes:
64. 64. The method of claim 63, wherein the additively manufactured product is a substrate body for a component of a nuclear reactor system.
65. 65. The method of claim 64, wherein the additively manufactured product is manufactured by an additive manufacturing protocol using a nuclear fuel slurry.
66. The nuclear fuel slurry comprises: 30% to 45% by volume of a monomer resin; 30% to 70% by volume of the plurality of particles; >0% to 7% by volume of a dispersant; greater than 0% by volume of a photoactivated dye; greater than 0% by volume of a light absorber; greater than 0% by volume of a photoinitiator, and 0% to 18% by volume of diluent as the balance (Volume percentages are based on the total volume of the nuclear fuel slurry), the particles have a composition including a uranium-containing material; 66. The method of claim 65.
67. 67. The method of claim 66, wherein the uranium-containing material is uranium metal, a uranium alloy, a uranium ceramic, or a uranium-molybdenum alloy.
68. 67. The method of claim 66, wherein the uranium-containing material is uranium oxide, uranium dioxide, uranium carbide, uranium carbonate, uranium nitride, uranium silicide, uranium fluoride, uranium chloride, a cermet of uranium oxide and tungsten, a cermet of uranium dioxide and tungsten, a cermet of uranium oxide and molybdenum, or a cermet of uranium dioxide and molybdenum.
69. 67. The method of claim 66, wherein the uranium-containing material is uranium oxide or uranium dioxide.
70. 67. The method of claim 66, wherein the uranium-containing material is U(C,O,N,Si,F,Cl).
71. 66. The method of claim 65, wherein the additive manufacturing protocol is developed using a surrogate slurry.
72. The additive manufacturing protocol comprises: 30% to 45% by volume of a monomer resin; 30% to 70% by volume of a plurality of substitute particles; >0% to 7% by volume of a dispersant; greater than 0% by volume of a photoactivated dye; greater than 0 volume percent light absorber; greater than 0% by volume of a photoinitiator, and 0% to 18% by volume of diluent as the balance (Volume percentages are based on the total volume of the nuclear fuel slurry), a surrogate slurry, the surrogate particles being selected to represent uranium-containing material; The method of claim 65, wherein the method is developed using
73. 73. The method of claim 72, wherein the uranium-containing material is uranium metal, a uranium alloy, a uranium ceramic, or a uranium-molybdenum alloy.
74. 73. The method of claim 72, wherein the uranium-containing material is uranium oxide, uranium dioxide, uranium carbide, uranium carbonate, uranium nitride, uranium silicide, uranium fluoride, uranium chloride, a cermet of uranium oxide and tungsten, a cermet of uranium dioxide and tungsten, a cermet of uranium oxide and molybdenum, or a cermet of uranium dioxide and molybdenum.
75. 73. The method of claim 72, wherein the uranium-containing material is uranium oxide or uranium dioxide.
76. 73. The method of claim 72, wherein the uranium-containing material is U(C,O,N,Si,F,Cl).
Citation Information
Patent Citations
Aqueous additive production method for the fabrication of ceramic and / or metallic bodies
EP3287213A1
Photocurable liquid composition, three-dimensional article, and method for producing them
JP2007291393A
Process for quality control for a powder based layer building up process
US20040173946A1
System and method for detecting defects in three-dimensional printed parts
WO2019051048A1