Adsorbent composition comprising plant material residue and method for use thereof

By densifying and grinding plant material residues into small pieces, the compositions achieve enhanced oil adsorption and resistance, addressing the need for additional uses of agricultural by-products like flax shive, offering a sustainable and safe solution for oil spill cleanup.

JP2024150738AInactive Publication Date: 2024-10-23エスダブリュエム ホルコ ルクセンブルク
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024126142
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-03-20
Filing Date
2024-08-01
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

There is a need for additional uses and applications of plant material by-products such as flax shive, which is generated in large quantities during agricultural processes, as they are traditionally used for animal bedding, fuel, or disposed of through landfills.

Method used

Densifying and grinding plant material residues, such as flax shive, into small pieces to create compositions with enhanced adsorption properties for oily substances, particularly suitable for cleaning up oil spills.

Benefits of technology

The compositions exhibit improved oil adsorption capabilities, are fire-resistant, generate minimal dust, and can be safely stored and incinerated, providing a sustainable solution for oily substance cleanup.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150738000013
    Figure 2024150738000013
  • Figure 2024150738000014
    Figure 2024150738000014
  • Figure 2024150738000015
    Figure 2024150738000015
Patent Text Reader

Abstract

To provide a method for remediating oil spills using plant material residues, an oil remediation composition, and a method for producing an oil remediation composition.SOLUTION: A remedial composition disclosed here is made from plant material residues that have been densified and then reduced into discrete pieces. The remedial composition disclosed here can be made from various different plant species and can be particularly made from agricultural crop byproducts, such as flax shives. The remedial composition disclosed here is particularly well suited for use as a remediation product for cleaning up and / or removing oily substances, such as petroleum products.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (Related Applications) This application claims priority to U.S. Provisional Application No. 62 / 821,100, filed March 20, 2019, and U.S. Provisional Application No. 62 / 757,404, filed November 8, 2018, the disclosures of which are incorporated herein by reference. [Background technology]

[0002] Large amounts of plant material residues are generated annually as by-products of agricultural and / or industrial processes. For example, in one embodiment, the plant material residues may include by-products of agricultural crops. Examples of plant material residues that are generated annually in large amounts include flax shive, corn stover, wheat straw, barley straw, switchgrass, bagasse, and the like.

[0003] For example, flax straw is grown as a commercial crop for the extraction of fiber from the plant. Flax fiber can be used for a variety of applications. When flax fiber is extracted from flax straw, the remaining non-fibrous plant material residue is called flax shive. Flax shive represents 20-85% of the total weight of flax straw. Thus, flax shive is the main by-product of flax straw processing. Traditionally, flax shive has been used to make animal bedding, burned as fuel, or disposed of by land use or disposal in sanitary landfills.

[0004] However, there is a need for additional uses and applications of plant material by-products such as flax shive. Summary of the Invention [Means for solving the problem]

[0005] In general, the present disclosure relates to the production of novel and useful products from plant material residues, particularly from agricultural by-products. According to the present disclosure, the plant material residues are densified and then broken into individual pieces. The compositions of the present disclosure thus produced have been found to have a unique combination of physical properties. For example, the compositions of the present disclosure have been found to be suitable for adsorbing and / or absorbing oily substances for use in cleaning up oily spills.

[0006] For example, in one embodiment, the present disclosure relates to a method for cleaning up an oil spill. The method of the present disclosure includes contacting an oily material with an oil sorbent composition. The oil sorbent composition includes, for example, densified pieces of plant material residue. The plant material residue can include non-fibrous plant material. According to the present disclosure, the densified pieces of plant material residue can have a density of about 0.2-0.5 g / cm. 3 , for example, about 0.25 to 0.4 g / cm 3 It has a bulk density of.

[0007] The densified plant material residue pieces may include various plant materials. For example, the densified plant material residue may include flax shive, corn stover, hemp hurd, bagasse, wheat straw, barley straw, switchgrass, etc. In one embodiment, the oil sorbent composition of the present disclosure contains densified plant material residue in an amount greater than about 70% by weight of the composition, such as greater than about 80% by weight, such as greater than about 90% by weight, or such as greater than about 95% by weight.

[0008] The oil sorbent composition of the present disclosure can be used to purify any type of oily material. For example, in one embodiment, the oil sorbent composition of the present disclosure can be used to purify petroleum-based products or petroleum-derived materials. In addition, the oil sorbent composition of the present disclosure can be used to adsorb various types of liquid hydrocarbons. The oil sorbent composition of the present disclosure has excellent oil adsorption properties. For example, the oil sorbent composition has a volume-based D5 average oil adsorption ratio (cm) of greater than about 0.7, e.g., in the range of about 0.75 to 1.00, when tested according to ASTM test F726-17. 3 / cm3 ) can be shown.

[0009] The present disclosure also relates to oil purification compositions comprising densified pieces of plant material residue. The plant material residue may include, for example, flax shive, corn stover, hemp hurd, bagasse, wheat straw, barley straw, switchgrass, etc. The densified plant material pieces generally have a density of about 0.7-1 g / cm. 3 , for example, about 0.75 to 0.95 g / cm 3 The densified plant material residue particles may have a density of about 0.2 to 0.5 g / cm. 3 , for example, about 0.25 to about 0.4 g / cm 3 The bulk density may be

[0010] In one embodiment, the oil purifying composition of the present disclosure is prepared from linseeds, for example, the oil purifying composition of the present disclosure contains linseeds in an amount greater than about 70% by weight of the composition, such as greater than about 80% by weight, or for example greater than about 90% by weight.

[0011] The present disclosure also relates to a method for producing an oil purification composition as described above. The method of the present disclosure includes a step of densifying a plant material residue to form a briquette. For example, the plant material residue may be densified to form a briquette having a density of about 0.6 g / cm. 3 Density above 0.7 to 1 g / cm 3 The plant material residue is subjected to a pressure sufficient to form briquettes having a density in the range of about 17.24 mPa (about 2,500 psi), such as greater than about 20.68 mPa (about 3,000 psi), or, for example, greater than about 24.13 mPa (about 3,500 psi). The plant material residue is typically subjected to a pressure of less than about 344.74 mPa (about 50,000 psi). In accordance with the present disclosure, the briquettes are then broken into individual pieces. The size of the individual pieces may be such that more than 50% of the pieces have a maximum dimension of about 1.27 to 12.7 cm (about 0.5 to 5 inches), such as about 1.27 to 7.62 cm (about 0.5 to 3 inches).

[0012] The briquettes can be broken into individual pieces using various methods and techniques. In one embodiment, for example, the briquettes can be fed through a gap formed between two rotating rollers. The briquettes can be fed through a gap formed between the two rotating rollers by positioning the two rotating rollers at a predetermined distance from each other. The gap distance between the two rotating rollers can be about 0.5 to 2 inches. However, in another embodiment, the individual pieces are formed from the briquettes by feeding the briquettes through a roller mill or a hammer mill.

[0013] The crushed individual pieces or crumbles provide various benefits and advantages. For example, the crumbles generate little to no harmful dust. The crumbles are also lighter than many other oil or chemical cleanup products. The crumbles of the present disclosure have been unexpectedly found to be more ignition resistant, especially compared to the plant material residues prior to densification. The crushed plant material of the present disclosure is ignition resistant, does not generate harmful dust, and is lighter than other cleanup products, enhancing worker safety. After the individual pieces or crumbles are used to clean up an oil or chemical spill, the used pieces or crumbles can be incinerated instead of disposed of in a landfill.

[0014] Other features and aspects of the present invention are described in detail below. [Brief description of the drawings]

[0015] A full and enabling disclosure of the present invention, directed to one skilled in the art, is set forth in more detail in the remainder of the specification, which refers to the accompanying drawings, in which:

[0016] [Figure 1] 1 is a graph showing test results for various oils. [Diagram 2] 1 is a graph showing test results for various oils. [Diagram 3]1 is a graph showing test results for various oils. [Figure 4] 1 is a graph showing test results for various oils.

[0017] Repeat use of reference characters in the present specification and drawings is intended to represent same or analogous features or elements of the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Those skilled in the art will appreciate that this disclosure is a description of exemplary embodiments only and is not intended to limit the broader aspects of the invention.

[0019] In general, the present disclosure relates to a effluent cleaning composition made from plant material residue. For example, the effluent cleaning composition can be made from agricultural by-products. According to the present disclosure, the plant material residue is densified and then broken down (disintegrated) into individual pieces. This process dramatically and unexpectedly increases the adsorption and absorption properties of the plant material residue on a volumetric basis. The effluent cleaning composition of the present disclosure can absorb or adsorb any type of liquid material, but is particularly suitable for adsorbing oily materials, such as petroleum-based materials or hydrocarbon liquids. For example, through the process of the present disclosure, the oil adsorption properties of the plant material residue can be increased by more than 100%, for example more than 150%, on a volumetric basis.

[0020] In addition to having excellent oil absorption, the plant material residue of the present disclosure has been unexpectedly found to be resistant to ignition. This unique property was surprising given that untreated plant material residues are commonly used as fuel components. Because the plant material residue of the present disclosure is resistant to ignition, it is very safe to store at industrial sites, providing a great advantage in places where flammable materials such as oil and other chemicals are commonly present. In addition to being resistant to ignition, the plant material residue of the present disclosure also contributes to worker safety by generating little harmful dust.

[0021] Various plant material residues can be incorporated into the composition of the present disclosure.In one particular embodiment, for example, the composition of the present disclosure contains flax shive.Flannel shive is a by-product remaining after extracting fiber components from flax straw.Flannel shive includes all materials remaining after fiber extraction from flax straw.

[0022] In addition to flax shive, plant material residues that can be incorporated into the compositions of the present disclosure include corn stover, hemp herd, bagasse, wheat straw, barley straw, switchgrass, or any combination thereof. Corn stover generally refers to the residue or by-product left after harvesting with a combine. Corn stover includes corn cobs, mesophyll, stalks, etc.

[0023] Hemp hurd, like flax shives, is a by-product left over after the fiber is extracted from the hemp plant, while bagasse refers to the vegetable residue or by-product left over after sugar is extracted in sugarcane factories, while wheat straw, barley straw, and switchgrass refer to any part of a particular plant, including agricultural by-products.

[0024] Generally, to produce a effluent cleaning composition according to the present disclosure, the plant material residue is first densified. For example, the plant material residue can be densified by subjecting it to a high pressure sufficient to form briquettes. After the plant material residue is densified, the densified plant material residue is crushed (broken down) into individual pieces. For example, in one embodiment, briquettes formed from the densified plant material residue can be crushed by feeding them to a crushing device, thereby breaking the briquettes into pieces having a size that enhances their ability to absorb and / or adsorb liquids, such as oily substances, and a size that facilitates handling and transportation.

[0025] Any suitable compression device can be used to densify the plant material residue. In one embodiment, for example, a briquetting press can be used. For example, in one embodiment, the plant material residue, such as flax shive, is fed into a compression chamber provided in the briquetting press. In the compression chamber, the plant material residue is compressed into briquettes, for example using a piston or plunger. After the densified plant material residue is compressed, it is fed through a die and cooled.

[0026] The amount of pressure applied to the plant material residue during the densification process varies depending on the particular plant material and the desired results. Typically, the amount of pressure applied to the plant material residue is greater than about 2,000 psi, such as greater than about 2,500 psi, such as greater than about 3,000 psi, such as greater than about 3,500 psi, or such as greater than about 4,000 psi. In other embodiments, the amount of pressure applied to the plant material residue is greater than about 10,000 psi, such as greater than about 15,000 psi, such as greater than about 20,000 psi, or such as greater than about 25,000 psi. The amount of pressure applied to the plant material residue is generally less than about 75,000 psi, such as less than about 50,000 psi, or such as less than about 40,000 psi. Applying pressure of these amounts to the plant material residue can cause cell disintegration and release of cellular material.

[0027] In one embodiment, the temperature of the plant material residue increases due to mechanical friction during densification. For example, the temperature in the compression chamber is greater than about 50°C, such as greater than about 60°C, such as greater than about 70°C, such as greater than about 80°C, such as greater than about 90°C, or such as greater than about 100°C. Also, the temperature in the compression chamber is generally less than about 130°C. In one embodiment, for example, the temperature in the compression chamber is in the range of about 105-115°C. The above temperatures evaporate the moisture in the plant material residue. Generally, the plant material residue fed to the process should contain a sufficient amount of moisture to facilitate the densification process when forming the briquettes. However, the moisture content of the plant material residue should not be too high so as to form harmful amounts of steam. Generally, the moisture content of the plant material residue should be greater than about 6% by weight, such as greater than about 10% by weight, or such as greater than about 12% by weight. Also, the moisture content of the plant material residue should generally be less than about 20% by weight, such as less than about 15% by weight.

[0028] The dimensions of the briquettes after densification are generally not critical. Thus, briquettes of any size can be formed according to the present disclosure. In one embodiment, the briquettes can have a cylindrical shape after being discharged from the die. For illustrative purposes only, cylindrical briquettes having a diameter of more than about 40 mm, such as more than about 50 mm, such as more than about 60 mm, or such as more than about 70 mm, and generally less than about 110 mm, such as less than about 100 mm, such as less than about 90 mm, or such as less than about 80 mm, can be formed according to the present disclosure.

[0029] The density of the plant material residue is increased by an amount sufficient to improve the adsorption properties of the plant material. For example, the density of densified plant material residue is typically about 0.6 g / cm. 3 For example, about 0.7 g / cm 3 For example, about 0.75 g / cm 3 For example, about 0.8 g / cm 3 More than, or for example, about 0.85 g / cm 3The density of densified plant material residues is typically greater than 1 g / cm 3 For example, less than about 0.95 g / cm 3 is less than.

[0030] The initial density of plant material residues is typically around 0.1 g / cm 3 Thus, densification may increase the density of the residual plant material by more than about 6 fold, such as by more than about 7 fold, or such as by more than about 8 fold.

[0031] According to the present disclosure, after densifying the plant material residue, the densified plant material residue is crushed into small pieces. The pieces thus formed can be large enough to increase the surface area for adsorbing or absorbing substances without generating a large amount of fines. Generally, the pieces should be of a size that facilitates handling of the plant material. For example, in one embodiment, more than 50% of the pieces of the densified plant material residue have a maximum dimension of more than about 0.25 inches, such as more than about 0.5 inches, such as more than about 0.75 inches, such as more than about 1 inch, such as more than about 1.25 inches, such as more than about 1.5 inches, such as more than about 1.75 inches, such as more than about 5.0 inches. The particles have a maximum dimension of more than about 2 inches, such as more than about 2.25 inches, for example more than about 2.5 inches, such as more than about 2.75 inches, for example more than about 3 inches, such as more than about 3.25 inches, for example more than about 3.5 inches, such as more than about 3.75 inches, or for example more than about 4 inches. Also, more than 50% of the particles of the densified plant material residue generally have a maximum dimension of less than about 20 inches, such as less than about 10 inches, for example less than about 8 inches, or for example less than about 4 inches. Particle size can be determined using an ASTM standard test sieve. For example, ASTM standard test sieves are commercially available from a number of sources, including Custom Advanced Connections, Webster, Texas, USA. Unless otherwise stated, the dimensions of more than 50% of the particles are based on the total weight of the sample. However, in other embodiments, the particle size and particle size distribution of the particles may be based on volume.

[0032] In one embodiment, the densified plant material residue pieces have an average maximum dimension of about 0.25 to 20 inches, such as about 0.5 to 15 inches, or such as about 1 to 4 inches.

[0033] Generally, any suitable method or technique can be used to break down the densified plant material residue to form individual pieces. For example, in one embodiment, a roller mill can be used to break down the densified plant material residue to form individual pieces. In another embodiment, a hammer mill can be used to break down the densified plant material residue to form individual pieces.

[0034] In one embodiment, the densified plant material residue or briquettes are fed into a gap (nip) formed between two rotating rollers. For example, the two rotating rollers are arranged at a predetermined distance from each other, and the densified plant material residue is fed into the gap thus formed between the two rotating rollers. The distance of the gap between the two rotating rollers is more than about 0.5 inches, such as more than about 0.75 inches, such as more than about 1 inch, or such as more than about 1.25 inches. Also, the distance of the gap between the two rotating rollers is generally less than about 3 inches, such as less than about 2 inches, such as less than about 1.75 inches, or such as less than about 1.5 inches. By feeding the briquettes through the gap formed between the two rotating rollers, the briquettes are broken into pieces having a desired size. To ensure that the effluent cleaning composition of the present disclosure thus produced has the desired size and size distribution, the gap distance between the two rotating rollers, the rotation speed of the two rotating rollers, and various other parameters can be varied and adjusted.

[0035] In one embodiment, the compositions of the present disclosure produced by the above process may be particles having an average maximum dimension of about 0.5 to 2 inches. In one embodiment, the plant material residue may be densified and then ground into small pieces, such that the compositions of the present disclosure thus produced have a bulk density that provides improved absorption and adsorption properties. The bulk density of the compositions of the present disclosure is generally about 0.2 g / cm. 3 For example, about 0.25 g / cm 3 or, for example, about 0.275 g / cm 3 The bulk density of the compositions of the present disclosure is generally greater than about 0.5 g / cm 3 For example, less than about 0.4 g / cm 3 Less than about 0.35 g / cm 3 Less than, or for example, about 0.3 g / cm 3 In one embodiment, for example, the composition of the present disclosure has a bulk density of about 0.26 to 0.29 g / cm 3 The bulk density can be determined according to EN15103:2009.

[0036] The composition of the present disclosure may be made entirely from plant material residue. Also, the composition of the present disclosure does not require binders or other materials to produce a product with excellent absorption and adsorption properties, especially for oily substances. Thus, the composition of the present disclosure may contain more than about 70% by weight of the plant material residue, such as more than about 80% by weight, such as more than about 90% by weight, such as more than about 95% by weight, or such as more than about 98% by weight of the plant material residue. In one embodiment, the composition of the present disclosure is made entirely from plant material residue.

[0037] However, if desired, various other additives and ingredients can be incorporated into the compositions of the present disclosure. For example, in one embodiment, additional absorbent materials can be incorporated into the compositions of the present disclosure.

[0038] The compositions of the present disclosure have a variety of uses and applications. In an embodiment, for example, the compositions of the present disclosure can be used as cleaning compositions to absorb or adsorb various types of chemical spills. For example, the compositions of the present disclosure can be used to clean up various types of hydrocarbons, ammonia, and various other chemicals. In an embodiment, the compositions of the present disclosure are used to absorb and / or adsorb oily substances. The oily substances can be, for example, vegetable oils, animal oils, or petroleum-based oils. For example, the oily substances can include petroleum or petroleum-derived substances. The oily substances can include any liquid hydrocarbon. To clean up an oily substance, the composition of the present disclosure can simply be contacted with the oily substance, allowing the composition of the present disclosure to absorb and / or adsorb the oily substance.

[0039] As mentioned above, the compositions of the present disclosure are particularly suitable for cleaning up oily materials. For example, when tested according to ASTM test F726-17, the compositions of the present disclosure have a D5 average oil adsorption ratio (cm) by volume of greater than about 0.7, such as greater than about 0.75, such as greater than about 0.8, or such as greater than about 0.8, and generally less than about 1. 3 / cm 3 The compositions of the present disclosure may also exhibit an N100 oil adsorption ratio (cm) of greater than about 0.85, such as greater than about 0.9, such as greater than about 0.95, or such as greater than about 1, and generally less than about 1.2. 3 / cm 3 The compositions of the present disclosure may also exhibit an N750 oil adsorption ratio (cm) of greater than about 0.85, such as greater than about 0.9, such as greater than about 0.95, such as greater than about 1, or such as greater than about 1.1, and generally less than about 1.4. 3 / cm 3 The compositions of the present disclosure may also exhibit a D7500 oil sorption ratio based on volume that is greater than about 0.9, such as greater than about 0.92, or such as greater than about 0.94, and generally less than about 1.2.

[0040] The above oil adsorption properties are dramatic and unexpected given the raw materials used to make the compositions of the present disclosure. For example, the oil adsorption properties of the plant material residue can be increased by more than about 30%, such as more than about 50%, such as more than about 70%, such as more than about 100%, or such as more than about 120%, or even such as more than about 150%, on a volume basis.

[0041] In addition to the oil adsorption properties described above, the plant material residue of the present disclosure has been unexpectedly found to be ignition resistant. The plant material residue of the present disclosure has ignition resistance, so it can be safely stored before use. The fire resistant properties of the plant material residue of the present disclosure are particularly advantageous when the composition of the present disclosure is stored around flammable liquids, gases and other materials. In addition, the composition of the present disclosure generates little harmful dust. Therefore, the composition of the present disclosure can be safely stored and used, as it does not pose a fire hazard or health hazard.

[0042] In one embodiment, the plant material residue of the present disclosure can be stored at an industrial site, such as on an oil platform. The plant material residue of the present disclosure can be used to collect oil spills and other chemical spills without generating harmful dust. After use to absorb or clean up oil or chemical spills, the used plant material residue of the present disclosure can be disposed of by burning. For example, the plant material residue of the present disclosure can be incinerated. The energy generated by burning can then be used to generate power or provide heat, if desired. In this way, the plant material residue of the present disclosure is completely sustainable and does not contribute to landfill disposal.

[0043] The present disclosure may be better understood with reference to the following examples. EXAMPLES

[0044] The following examples were conducted to demonstrate the oil adsorption properties of compositions made in accordance with the present disclosure.

[0045] Sample No. 1 below was produced in accordance with the present disclosure. To produce this sample, flax shive was first densified to a density of 0.883 g / cm 3 The briquettes were then densified to form briquettes having a diameter of 75 mm. A briquetting press manufactured by CF Nielsen A / S, model number BP6500, was used to densify the flax shivs. After the briquettes were formed, they were fed into a grinding device having two rollers positioned at a predetermined distance from each other. The briquettes were fed into a nip formed between the two rollers. The distance of the gap between the two rollers was about 1 inch. The grinding device produced particles having a size range of about 0.5 to 2 inches.

[0046] Compositions made according to the present disclosure were compared to nine other samples as follows: Sample No. 2: STARDUST absorbent sold by Stardust Spill Products, LLC Sample No. 3: Flax Shibu Sample No. 4: PIG DRI absorbent sold by New Pig Corporation Sample No. 5: ENVIRO-DRI absorbent available from Can-Ross Environmental Services Ltd. Sample No. 6: Corncob absorbent material Sample No. 7: OIL GATOR absorbent sold by Gator International Sample No. 8: Flax fiber Sample No. 9: Flax meal Sample No. 10: Wood mulch

[0047] The bulk density of each sample was as follows:

[0048] [Table 1]

[0049] Bulk density was measured according to EN15103:2009 "Solid biofuels - Determination of bulk density".

[0050] The oil adsorption properties of each sample were tested. The oil adsorption rate was measured according to ASTM test F726-17.

[0051] Each sample for the adsorption test was conditioned in the laboratory at a temperature of 22 ± 2 °C and a relative humidity of 55 ± 5% for a minimum of 24 h.

[0052] The analysis was carried out using a universal viscosity reference standard obtained from Paragon Scientific Ltd. This viscosity reference standard is oil based, consisting of white oil and polybutene.

[0053] [Table 2]

[0054] Samples 1, 3-6, 8 and 10 were analyzed using a 210 micron / 70 mesh basket. Samples 2, 7 and 9 were analyzed using a 37 micron / 400 mesh basket.

[0055] A minimum weight of 4 g was used for each sorbent replica. The sorbents were placed in a labeled mesh basket and then lowered into the test cell pre-filled with the required oil (minimum liquid layer 2.5 cm). After 15 min ± 20 s, the basket with the sorbents was removed and allowed to drain on a wire rack for 30 ± 3 s (for high viscosity D7500 oil, the drainage time was 2 min ± 3 s). The sorbents were then transferred to a pre-weighed weighing dish to measure the sample weight and record the results. All tests were performed in triplicate.

[0056] Ratio of the volume of adsorbed oil to the dry volume of the adsorbent Oil adsorption ratio v=S SV / SOV During the ceremony S SV = Net oil adsorbed (S s ) / oil density. S OV = initial dry weight of adsorbent (S o ) / adsorbent storage density. Cubbage coefficient = the inverse of the ratio of the volume of adsorbed oil to the dry volume of the adsorbent.

[0057] The test results for various oils are shown in Tables 3-12 below and Figures 1-4.

[0058] [Table 3]

[0059] [Table 4]

[0060] [Table 5]

[0061] [Table 6]

[0062] [Table 7]

[0063] [Table 8]

[0064] [Table 9]

[0065] [Table 10]

[0066] [Table 11]

[0067] [Table 12]

[0068] Those skilled in the art will appreciate that the present invention can be modified or altered in various ways without departing from the spirit of the invention. In addition, it should be understood that aspects of the various embodiments can be interchanged in whole or in part. Furthermore, those skilled in the art will appreciate that the above detailed description and examples are for illustrative purposes only and are not intended to limit in any way the scope of the invention as set forth in the appended claims.

Claims

1. 1. A method for cleaning up an oil spill, comprising: Contacting an oily material with an oil sorbent composition, the oil sorbent composition comprises densified pieces of residual plant material; the plant material residue comprises non-fibrous plant material; The pieces of densified plant material residue have a density of 0.2 to 0.5 g / cm 3 having a bulk density of

2. 2. The method of claim 1 , The method of claim 1, wherein the densified plant material residue comprises flax shive.

3. 2. The method of claim 1 , The method, wherein the densified plant material residue comprises corn stover, hemp hurd, bagasse, wheat straw, barley straw, switchgrass, or any combination thereof.

4. The method according to any one of claims 1 to 3, wherein more than 50% of the particles of the densified plant material residue have a maximum dimension of between 1.27 and 12.7 cm, or between 1.27 and 7.62 cm.

5. The method according to any one of claims 1 to 4, The method of claim 1, wherein the oily material comprises petroleum or a petroleum-derived material.

6. The method according to any one of claims 1 to 4, The method, wherein the oily substance comprises a liquid hydrocarbon.

7. The method according to any one of claims 1 to 6, The oil sorbent composition has a volume-based D5 average oil sorption ratio (cm) of greater than 0.7, or from 0.75 to 1.00, when tested according to ASTM test F726-17. 3 / cm 3 ).

8. A method according to any one of claims 1 to 7, comprising: The pieces of densified plant material residue have a density of 0.25 to 0.4 g / cm 3 having a bulk density of

9. The method according to any one of claims 1 to 8, wherein the sorbent composition comprises the densified plant material residue in an amount greater than 70%, greater than 80%, greater than 90%, or greater than 95% by weight of the composition.

10. A method according to any one of claims 1 to 9, comprising: The method further comprises, after the step of contacting the oily material with the oil sorbent composition, incinerating the oil sorbent composition that has been contacted with the oily material.

11. 1. An oil purification composition comprising: comprising small pieces of densified plant material residue; The plant material residue comprises non-fibrous plant material; The densified plant material residue comprises flax shives, corn stover, hemp hurd, bagasse, wheat straw, barley straw, switchgrass, or any combination thereof; The particles of the densified plant material residue have a density of 0.2 to 0.5 g / cm 3 and having a bulk density of The oil purification composition has a volume-based D5 average oil adsorption ratio (cm) of greater than 0.7 when tested according to ASTM test F726-17. 3 / cm 3 ).

12. 12. The oil purification composition of claim 11, The oil purification composition comprises linseed in an amount greater than 70% or greater than 80% by weight of the composition.

13. 13. The oil purification composition according to claim 11 or 12, The composition has a volume-based D5 average oil adsorption ratio (cm) of 0.75 to 1.00 when tested according to ASTM test F726-17. 3 / cm 3 ).

14. The oil purifying composition according to any one of claims 11 to 13, wherein more than 50% of the particles of the densified plant material residue have a maximum dimension of 1.27 to 12.7 cm, or 1.27 to 7.62 cm.

15. The oil purifying composition according to any one of claims 11 to 14, The pieces of densified plant material residue have a density of 0.25 to 0.4 g / cm 3 The composition has a bulk density of

16. The oil purifying composition according to any one of claims 11 to 15, A composition, wherein the pieces of the densified plant material residue have a higher resistance to ignition than the plant material residue before it is densified.

17. 1. A method for producing an oil purification composition, comprising: Densifying the plant material residue to form briquettes, the plant material residue having a density of 0.6 to 1 g / cm 3 applying sufficient pressure to form a briquette having a density of The briquettes are mixed with a slurry of 0.2 to 0.5 g / cm 3 and grinding the mixture into discrete pieces having a bulk density of A method comprising:

18. 20. The method of claim 17, The plant material residue has a density of 0.75 to 0.95 g / cm 3 and densifying the briquettes to a density of about 100%.

19. 19. The method of claim 17 or 18, The individual pieces have a density of 0.25 to 0.4 g / cm 3 having a bulk density of.

20. A method according to any one of claims 17 to 19, comprising the steps of: The method, wherein more than 50% of the individual pieces have a maximum dimension between 1.27 and 12.7 cm, or between 1.27 and 7.62 cm.

21. A method according to any one of claims 17 to 20, comprising the steps of: The briquettes are broken into the individual pieces by being fed through a gap formed between two rotating rollers; The two rotating rollers are spaced apart from each other by a distance of 1.27 to 5.08 cm to form a gap through which the briquettes are fed.

22. A method according to any one of claims 17 to 20, comprising the steps of: The method of claim 1, wherein the briquettes are broken into said individual pieces by feeding them through a roller mill or a hammer mill.

23. A method according to any one of claims 17 to 22, comprising the steps of: The method, wherein the pieces of the densified plant material residue have fire resistant properties and are more resistant to ignition than the plant material residue before it is densified.

Citation Information

Patent Citations

  • JP1973080491A

  • Cellulose absorbent product and manufacturing method

    JP1994507112A

  • Oil adsorbent

    JP1996131824A

  • An oxidative thermochemical drying process for altering the hydrophilic / hydrophobic properties of natural organic materials

    JP2004534653A

  • Agglomerated stover for use as a liquid absorbent

    US20120052298A1