Sustained-release aromatic composition and method for producing the same

A three-dimensional network structure with specific pore sizes stabilizes fragrance compositions, maintaining scent consistency and supporting aromatic components effectively, addressing the issue of fragrance tone changes in conventional compositions.

JP2024151010APending Publication Date: 2024-10-24DPS INC

Patent Information

Application Number
JP2023064114
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional fragrance compositions fail to maintain a consistent fragrance tone over a long period due to the volatility differences between top, middle, and base notes, leading to a change in scent over time.

Method used

A sustained-release aroma composition utilizing a three-dimensional continuous network structure with macropores and mesopores, where macropores have a diameter of 0.1 μm to 100 μm and mesopores have a diameter of 0.1 nm to less than 100 nm, supported by a silica or silicon oxide framework, allowing for a two-stage hierarchical porous structure.

Benefits of technology

The composition maintains a stable fragrance tone over a long period without significant changes, supporting a larger amount of aromatic components and allowing for uniform evaporation, thus enhancing versatility in applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151010000001_ABST
    Figure 2024151010000001_ABST
Patent Text Reader

Abstract

To provide a sustained-release aromatic compound having fragrance which is less likely to change over a longer time than a conventional sustained-release aromatic compound.SOLUTION: A sustained-release aromatic compound is provided, comprising: a skeletal body 20 having a gap and three-dimensional continuous network structure; and a sustained-release liquid existing in at least a part of the gap. The gap is: a plurality of macropores 30 which extend inward from a surface 22 of the skeletal body and exist while dispersed on the surface of the skeletal body; and a plurality of mesopores which extend to the inside of the skeletal body from the surface of the skeletal body and an inner surface 32 of the macropores and exist while dispersed on the surface of the skeletal body and the inner surface of the macropores, and at least a part of the plurality of mesopores is a through-hole.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sustained release fragrance composition and a method for making the same. [Background technology]

[0002] Fragrances are added to various products such as cosmetics and detergents. Fragrances are classified into top notes, middle notes, and base notes in order of increasing volatility. Usually, multiple fragrances are mixed together to create complex fragrances or fragrances that change over time.

[0003] It is a universal challenge to make a fragrance last for a long time, especially to maintain a fragrance tone for a long time. Specifically, the top note is highly volatile and determines the initial impression of the fragrance, but evaporates in a short time. On the other hand, the middle note and base note are less volatile than the top note, so they continue to smell even after the top note evaporates. In this way, the fragrance tone changes over time depending on the difference in volatility of each fragrance. Patent Document 1 discloses a fragrance-containing capsule that can stably encapsulate a fragrance. According to this technology, a fragrance including a top note can be appropriately realized by friction or the like. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-237761 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the conventional technology, it is possible to realize a scent containing a top note temporarily, but it is not possible to maintain the fragrance tone for a long period of time. Therefore, the object of the present invention is to provide a sustained-release fragrance composition whose fragrance tone is less likely to change for a long period of time than conventional ones and which is highly versatile. [Means for solving the problem]

[0006] As a result of extensive investigations, the present inventors have found that the above-mentioned problems can be solved by using a specific framework as a carrier for sustained release liquid, and have thus completed the present invention.

[0007] According to the present invention, the following is provided: [1] A sustained release fragrance composition comprising: A framework having a three-dimensional continuous network structure with voids; A sustained release liquid present in at least a portion of the void; Equipped with the voids are a plurality of macropores extending from the surface of the framework toward the inside and distributed on the surface of the framework, and a plurality of mesopores extending from the surface of the framework and the inner surfaces of the macropores toward the inside of the framework and distributed on the surface of the framework and the inner surfaces of the macropores, and A sustained-release fragrance composition, wherein at least a portion of the plurality of mesopores are through-pores. [2] The most frequent pore size of the macropores is 0.1 μm or more and 100 μm or less, and The sustained-release fragrance composition according to [1], wherein the most frequent pore size of the mesopores is 0.1 nm or more and less than 100 nm. [3] The sustained-release aroma composition according to [1] or [2], wherein the skeleton is a granular skeleton, and the longest diameter of the granular skeleton is 500 μm or less. [4] The sustained-release fragrance composition according to [1] or [2], wherein the framework is a silicon oxide complex mainly containing silica or silicon oxide. [5] The sustained-release fragrance composition according to [1] or [2], wherein the sustained-release liquid is an oil containing an aromatic component. Effect of the Invention

[0008] According to the present invention, it is possible to provide a sustained-release fragrance composition whose fragrance tone is less likely to change over a long period of time than conventional compositions and which is highly versatile. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of a granular framework according to the present embodiment. [Diagram 2] FIG. 2 is a partially enlarged schematic cross-sectional view of the framework according to this embodiment. [Diagram 3] FIG. 3 is an electron microscope photograph of the aggregated porous body. [Figure 4] FIG. 4 is an enlarged electron microscope photograph of a portion of the massive porous body. [Diagram 5] FIG. 5 shows the pore size distribution of the massive porous body measured by BJH measurement using nitrogen adsorption measurement. [Figure 6] FIG. 6 is an electron microscope photograph of the granular skeleton A. [Figure 7] FIG. 7 is a graph showing the amount of aromatic oil carried per gram of each sample. [Figure 8] FIG. 8 is a graph showing the evaluation of the fragrance tone of each sample over time. [Figure 9] FIG. 9 is a graph showing the amount of support over time for each sample. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. The framework and the method for producing the framework and the sustained-release fragrance composition according to the present invention will be described in that order.

[0011] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the present embodiment and the drawings related to the present embodiment, components with the same reference numerals have the same structure or function. In addition, each drawing is exaggerated for the purpose of explanation, and the scale may not be the same as the actual scale.

[0012] <Skeletal body> FIG. 1 is a schematic cross-sectional view of a granular skeleton 10 according to one embodiment. FIG. 2 is a schematic enlarged cross-sectional view of a skeleton 20 according to this embodiment. The granular skeleton 10 according to this embodiment is made of a skeleton 20 having a three-dimensional continuous network structure. The skeleton 20 has voids. The voids are made of a plurality of macropores 30 and a plurality of mesopores 40. The macropores 30 are dispersed on the surface 22 of the skeleton 20 and extend from the surface 22 of the skeleton 20 toward the inside. The macropores 30 according to this embodiment may be non-penetrating pores (non-penetrating macropores 30a), or may be penetrating pores (penetrating macropores 30b), or may include non-penetrating pores (non-penetrating macropores 30a) and penetrating pores (penetrating macropores 30b). The mesopores 40 are dispersed on the surface 22 of the skeleton 20 and the inner surface 32 of the macropores 30, and extend from the surface 22 of the skeleton 20 and the inner surface 32 of the macropores 30 toward the inside of the skeleton 20. Thus, the framework 20 according to this embodiment has a two-stage hierarchical porous structure.

[0013] The substrate of the skeleton 20 according to the present embodiment is not particularly limited as long as it can support the sustained release liquid described later. The substrate of the skeleton 20 according to the present embodiment is typically an inorganic compound, and is preferably a metal oxide or a metal oxide complex. The substrate of the skeleton 20 according to the present embodiment is particularly preferably a silicon oxide complex mainly containing silica (silica gel or silica glass) or silicon oxide. Such a substrate makes it easy to manufacture the skeleton 20. In addition, as the substrate of the skeleton 20 according to the present embodiment, a metal oxide complex containing typical metal elements such as aluminum, phosphorus, germanium, and tin, and transition metal elements such as titanium, zirconium, vanadium, chromium, iron, cobalt, nickel, palladium, platinum, copper, silver, gold, and zinc can also be used. Furthermore, as the substrate of the skeleton 20 according to the present embodiment, a metal oxide complex containing alkali metal elements such as lithium and sodium, alkaline earth metal elements such as magnesium and calcium, and lanthanum-based elements such as lanthanum and cerium can also be used.

[0014] The most frequent pore size of the macropores 30 according to the present embodiment (hereinafter, simply referred to as "macropore size") is preferably 0.1 μm or more and 100 μm or less, and may be within any two values ​​of 0.1, 0.5, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, and 100 μm. Here, the "most frequent pore size" in this specification means the most frequent value (mode value) of the pore size distribution measured by a well-known method. As a method for measuring the pore size distribution, for example, mercury intrusion porosimetry can be mentioned. The most frequent pore size of the macropores 30 is equivalent to the average pore size obtained by measuring the pore sizes of about 20 to 30 macropores 30 in an electron microscope photograph of the skeleton 20 and calculating the average value. When the most frequent pore size of the macropores 30 is in such a range, a sufficient amount of sustained release liquid can be contained, and the fragrance can be sustained for a long time.

[0015] The most frequent pore size of the mesopores 40 according to this embodiment (hereinafter, simply referred to as "mesopore size") is preferably 0.1 nm or more and less than 100 nm, and may be within any two values ​​of 0.1, 0.5, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, or 90 nm. Thus, in this specification, "mesopores" may also include pores (micropores) with a most frequent pore size of 2 nm or less. In addition, as the pore size distribution of the mesopores 40 when determining the most frequent pore size of the mesopores 40, a pore size distribution derived by the well-known BJH method using nitrogen adsorption measurement may be used. At least a part of the mesopores 40 according to this embodiment is preferably a through hole. When a sustained-release aromatic composition is prepared using a framework 20 having mesopores 40 with such a structure, convection of the sustained-release liquid is less likely to occur in the mesopores 40, so that even a sustained-release liquid containing a highly volatile substance such as a top note is likely to be sustained-released while maintaining a constant concentration ratio. In other words, when a sustained-release aromatic composition is produced using the framework 20 according to this embodiment, the sustained-release liquid can transpire uniformly.

[0016] The macropore diameter according to this embodiment is preferably 5 times or more, and may be 10 times or more, 20 times or more, 30 times or more, 40 times or more, 50 times or more, 100 times or more, or 150 times or more, based on the mesopore diameter. When the framework 20 has such a structure, a stable two-stage hierarchical porous structure is formed.

[0017] The skeleton 20 according to this embodiment is a granular skeleton 10. The longest diameter of the granular skeleton 10 according to this embodiment is preferably 500 μm or less, more preferably 200 μm or less, 100 μm or less, or 50 μm or less. When the longest diameter of the granular skeleton 10 is in such a range, the granular skeleton 10 can be used to prepare a sustained-release aromatic composition, and can be used for various purposes while maintaining the effect of maintaining the fragrance tone.

[0018] <Method of manufacturing the skeleton> The method for producing the granular skeleton 10 according to this embodiment is described in detail below. The method for producing the granular skeleton 10 according to this embodiment includes a synthesis step of synthesizing a massive porous body by a sol-gel method, and a granulation step of producing the granular skeleton 10 by pulverizing the massive porous body before or after sintering.

[0019] The synthesis process according to this embodiment is typically a sol-gel method involving spinodal decomposition, and includes a sol preparation process, a gelation process, and a removal process.

[0020] The sol preparation step according to the present embodiment includes an adding step of adding raw materials and a mixing step of mixing the raw materials to obtain a uniform precursor sol. The raw materials according to the present embodiment include, for example, a silica precursor, which is a raw material for silica gel or silica glass, and a coexisting substance that has the function of inducing sol-gel transition and phase separation in parallel, in an acid or alkaline aqueous solution.

[0021] The acid or alkaline aqueous solution according to this embodiment is preferably an aqueous solution in which an acid or base that functions as a catalyst for promoting the hydrolysis reaction of silica precursor is dissolved in water as a solvent.Acids according to this embodiment include acetic acid, hydrochloric acid, sulfuric acid, nitric acid, formic acid, oxalic acid and citric acid, and bases according to this embodiment include amines such as sodium hydroxide, potassium hydroxide, ammonia water, sodium carbonate, sodium bicarbonate and trimethylammonium, ammonium hydroxides such as tert-butylammonium hydroxide, and alkali metal alkoxides such as sodium methoxide.Note that the solvent according to this embodiment may be alcohols such as ethanol and methanol if the hydrolysis reaction of silica precursor proceeds.

[0022] The main component of the silica precursor according to this embodiment can be, for example, water glass (aqueous sodium silicate solution) or an inorganic or organic silane compound. The inorganic silane compound according to this embodiment can be, for example, tetraalkoxysilanes such as tetramethoxysilane, tetraethoxysilane, tetraisopropoxysilane, tetra-n-butoxysilane, and tetra-t-butoxysilane. In addition, examples of the organic silane compound according to this embodiment include trialkoxysilanes such as trimethoxysilane, triethoxysilane, triisopropoxysilane, and triphenoxysilane, which have substituents such as methyl, ethyl, propyl, butyl, hexyl, octyl, decyl, hexadecyl, octadecyl, dodecyl, phenyl, vinyl, hydroxyl, ether, epoxy, aldehyde, carboxyl, ester, thionyl, thio, and amino, dialkoxysilanes such as methyldiethoxysilane, methyldimethoxysilane, ethyldiethoxysilane, and ethyldimethoxysilane, and monoalkoxysilanes such as dimethylethoxysilane and dimethylmethoxysilane. Furthermore, examples of the silica precursor according to this embodiment include alkoxysilicates containing crosslinking reaction rate control group substitutes such as monoalkyl, dialkyl, and phenyltriethoxy, and oligomers such as disilane, which is a dimer, and trisilane, which is a trimer. The above-mentioned various hydrolyzable silanes are commercially available and can be easily and inexpensively obtained.

[0023] Examples of coexisting substances according to this embodiment include block copolymers such as polyethylene glycol, polyethylene oxide, polypropylene glycol, polypropylene oxide, polyacrylic acid, and polyethylene oxide-polypropylene oxide block copolymers, cationic surfactants such as cetyltrimethylammonium chloride, anionic surfactants such as sodium dodecyl sulfate, and nonionic surfactants such as polyoxyethylene alkyl ethers.

[0024] The mixing step according to this embodiment can be carried out by stirring at a low temperature (for example, 5° C. or lower) at which the sol-gel transition does not easily proceed. This allows the hydrolysis reaction of the silica precursor to proceed, and a uniform precursor sol is prepared.

[0025] The gelation step according to this embodiment includes a heating step. The precursor sol prepared in the above-mentioned sol preparation step is poured into a gelation vessel and allowed to stand at a temperature at which the sol-gel transition is likely to proceed (for example, about 40°C). As described above, the precursor sol contains a coexisting substance that induces the sol-gel transition and phase separation in parallel, and thus spinodal decomposition is induced. As a result, a bicontinuous structure of a silica hydrogel (wet gel) phase and a solvent phase having a three-dimensional continuous network structure is gradually formed.

[0026] In the heating step according to this embodiment, even after the silica hydrogel phase is formed, the polycondensation reaction of the wet gel proceeds slowly, causing the gel to shrink. Therefore, in the gelling step according to this embodiment, it is preferable to further carry out a hydrothermal treatment step in which the above-mentioned co-continuous structure is immersed in a basic aqueous solution such as ammonia water and heated after the heating step. This allows the hydrolysis reaction, polycondensation reaction, and dissolution and reprecipitation reaction of the silica hydrogel phase to proceed further, making it possible to further strengthen the skeletal structure of the silica hydrogel phase. It is preferable to carry out the hydrothermal treatment in a pressurized container or a sealed container. This makes it possible to prevent harmful components such as ammonia from being released into the environment due to heating. Thus, it is preferable to carry out the gelling step according to this embodiment by two-stage heating treatment, that is, a heating step and a hydrothermal treatment step.

[0027] In the heating step according to the present embodiment, the dissolution and reprecipitation reaction of the silica fine particles forming the framework of the silica hydrogel phase proceeds, so that the pore size of the mesopores 40 is enlarged. Furthermore, the hydrothermal treatment step repeats the dissolution and reprecipitation reaction, so that the pore size of the mesopores 40 can be further enlarged. The hydrothermal treatment step is preferably performed at a temperature in the range of 25°C or higher and lower than 100°C, and may be within any two of the following temperatures: 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, or 95°C. The treatment time of the hydrothermal treatment step is preferably, for example, 1 hour or higher and 100 hours or higher, and may be within any two of the following temperatures: 3 hours, 5 hours, 10 hours, 20 hours, 50 hours, or 80 hours. By performing the hydrothermal treatment under such conditions, the mesopores 40 become through-holes. The pore size of the mesopores 40 can also be controlled by further adding urea to the precursor sol. Urea is hydrolyzed at a temperature of 60° C. or higher to generate ammonia, and the ammonia expands the pore size of the mesopores 40 formed in the skeleton of the wet gel.

[0028] On the other hand, the structure and pore size of the macropores 30 according to this embodiment can be controlled by adjusting the amounts of the solvent and silica precursor added to the precursor sol in the sol preparation step, or the composition and amounts of the coexisting substances added.

[0029] The removal step according to this embodiment includes a drying step in which the wet gel is dried to form a dry gel. This makes it possible to remove the solvent phase containing additives and unreacted substances. The drying step according to this embodiment may be natural drying, but in order to eliminate distortion and cracks that occur when drying the wet gel, drying is preferably performed after replacing the solvent in the wet gel with a low surface tension solvent such as isopropanol, acetone, hexane, or hydrofluorocarbon, which has a lower surface tension than water, drying by freeze sublimation, or supercritical drying is preferably performed in a surface tension-free state after replacing the solvent in the wet gel with carbon dioxide in a supercritical state.

[0030] The removal step according to the present embodiment preferably further includes a washing step of washing the wet gel before the drying step. This can eliminate the surface tension during drying caused by additives and unreacted substances remaining in the solvent phase, and suppress the gel from being distorted or cracked during drying. The washing step according to the present embodiment preferably uses a liquid such as an organic solvent or an aqueous solution. The liquid according to the present embodiment may be a liquid in which an organic compound or an inorganic compound is dissolved, or may be a solution containing an acid or a base and having a pH different from the isoelectric point of the gel. Examples of acids that may be contained in the liquid according to the present embodiment include hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, acetic acid, formic acid, carbonic acid, citric acid, and phosphoric acid, and examples of bases that may be contained in the liquid according to the present embodiment include sodium hydroxide, potassium hydroxide, ammonia, water-soluble amines, sodium carbonate, and sodium bicarbonate.

[0031] In the synthesis process according to this embodiment, a baking process may be further included after the removing process, in which the dry gel is baked. This allows the dry gel to be sintered into silica glass. Note that if the baking temperature is lower than the glass transition temperature of silica (about 1000°C), the gel will not become silica glass.

[0032] The synthesis process according to this embodiment can provide a massive porous body having a three-dimensional continuous network structure with voids. The massive porous body according to this embodiment has a two-stage hierarchical porous structure having macropores and mesopores. That is, the scope of the framework 20 of the present invention also includes a massive porous body that has not been subjected to the granulation process described below. In addition, the scope of the framework 20 of the present invention also includes a massive porous body that has been shaped into an arbitrary shape by cutting or the like after the synthesis process. At this time, it does not matter if some of the macropores 30 are blocked. The pore size distribution of the framework 20 according to this embodiment may be measured after the synthesis process. The pore sizes of the macropores and mesopores are determined depending on the conditions of the synthesis process.

[0033] In this embodiment, it is preferable to further include a granulation step in which the aggregated porous body is pulverized to form a granular skeleton 10 after the synthesis step. The pulverization method according to this embodiment is not particularly limited. It may be performed manually, or a mortar or the like may be used, or a crushing device such as a ball mill may be used. In addition, when the granulation step includes a sintering step in which the dried gel obtained in the removal step is sintered, it may be performed either before or after the sintering step. At this time, it does not matter if some of the macropores 30 are blocked. Even if some of the macropores 30 are blocked, the granular skeleton 10 according to this embodiment allows uniform evaporation of the sustained-release liquid when it is made into a sustained-release aromatic composition by the method described below.

[0034] The granular skeleton 10 after the granulation step can be classified by sieving through a sieve with a predetermined mesh size, so that only the granular skeleton 10 within a desired particle size range can be collected. The size of the granular skeleton 10 according to this embodiment can be appropriately adjusted depending on the application of the granular skeleton 10.

[0035] <Sustained release aroma composition> The sustained-release aromatic composition according to this embodiment includes a skeleton 20 (granular skeleton 10 or aggregate porous body) prepared by the above-mentioned method, and a sustained-release liquid present in at least a part of the voids of the skeleton 20. The sustained-release aromatic composition according to this embodiment can be prepared by contacting (e.g., immersing) the above-mentioned skeleton 20 with the sustained-release liquid. The skeleton 20 according to this embodiment has a plurality of macropores 30 and a plurality of mesopores 40 formed and dispersed on the surface 22 of the skeleton, so that the sustained-release liquid penetrates into the inside of the skeleton 20 from the surface 22 of the skeleton.

[0036] The sustained-release aromatic composition according to this embodiment has a two-stage hierarchical porous structure and can hold a larger amount of sustained-release liquid. In addition, since at least a part of the mesopores 40 of the sustained-release aromatic composition according to this embodiment are through-holes, even if the sustained-release liquid is a mixture of liquids with different volatilities, the fragrance tone is less likely to change over a long period of time than in the past.

[0037] Oil containing aromatic components such as essential oils can be used as the sustained release liquid according to this embodiment. The sustained release aromatic composition according to this embodiment is less likely to change its fragrance tone over a long period of time than conventional compositions. Therefore, the sustained release liquid according to this embodiment does not need to be artificially manipulated (e.g., chemically modified) to change its volatility.

[0038] The sustained release fragrance composition according to the present embodiment can be used, for example, in sanitary products and cosmetics. When the sustained release fragrance composition according to the present embodiment uses a block porous body, it can be used, for example, as a stationary fragrance. When the sustained release fragrance composition according to the present embodiment uses a granular framework 10, it can be mixed as a fragrance in various products such as detergents and cosmetics, and is highly versatile. EXAMPLES

[0039] The present invention will be described in more detail below with reference to examples. Note that the examples described below are representative examples of the present invention, and the scope of the present invention should not be construed as being narrowed by these examples.

[0040] 1. Preparation of granular scaffold Granular skeletons A and B were prepared by a sol-gel method involving spinodal decomposition. Specifically, 0.9 g of polyethylene glycol (molecular weight 10,000) was dissolved in 10 mL of 0.01 mol / L aqueous acetic acid solution. Next, 5 mL of tetramethoxysilane was added to the above solution and stirred to obtain a homogeneous solution. The above homogeneous solution was then left to stand in an incubator set at 40°C to gel it.

[0041] The gel was immersed in 0.1M ammonia water and heated in a closed container at a set temperature of 30°C to 80°C for 24 hours. The gel was then sintered at a set temperature of 600°C or higher for 5 hours to obtain a massive porous body. Electron microscope photographs of the obtained massive porous body are shown in Figs. 3 and 4. As shown in Fig. 3, the massive porous body was a skeleton having a three-dimensional continuous network structure with voids, and had a plurality of macropores extending from the surface of the skeleton toward the inside and distributed on the surface of the skeleton. The most frequent pore size of the macropores was about 1 μm from the electron microscope photograph (see Fig. 4). In addition, the results of the pore size distribution measured by the BJH measurement using nitrogen adsorption measurement for the massive porous body are shown in Fig. 5. As shown in Fig. 5, the massive porous body had a plurality of mesopores extending from the surface of the skeleton and the inner surface of the macropores toward the inside of the skeleton and distributed on the surface of the skeleton and the inner surface of the macropores. The most frequent pore size of the mesopores was about 8 nm, and at least some of them were through-pores. Thus, the porous aggregate obtained by the above-mentioned method had a two-stage hierarchical porous structure having macropores and mesopores.

[0042] The above-mentioned blocky porous body was crushed using a crushing device to obtain granular skeletons of various sizes. The granular skeletons were classified using a sieve with a specified mesh size to obtain granular skeletons A and B. An electron microscope photograph of granular skeleton A is shown in FIG. 6. At this time, depending on the mesh size of the sieve, the longest diameter of granular skeleton A was about 45 μm or more and 63 μm or less, and the longest diameter of granular skeleton B was 20 μm or less.

[0043] 2. Preparation of sustained release fragrance composition In a 20 mL glass bottle, 1 g each of the granular skeleton A and granular skeleton B prepared in 1. and a commercially available porous silica gel (hereinafter also referred to as the "conventional product"; YMC Gel SIL-HG, particle size 10 μm, mesopore size 12 nm; manufactured by YMC Corporation) and 10 g each of four types of aroma oils (fragrances A, B, C, and D) were placed and stirred for about 20 minutes until homogenized. After stirring, the mixture was left to stand for 8 hours or more. After standing, the mixture was transferred to filter paper and suction filtered. The mass of the solid remaining on the filter paper was measured, and the amount of aroma oil carried by each sample was calculated (n=5). The results are shown in FIG. 7. As shown in FIG. 7, it was found that the granular skeleton A and the granular skeleton B had a higher amount of aroma oil carried per 1 g of sample than the conventional product.

[0044] 3. Evaluation of scent change and sustained release A sensory test was conducted on each sample after filtration in step 2 to check for changes in aroma. Specifically, each sample was transferred to a petri dish without a lid and placed in a draft chamber. After each specified time, the petri dish was removed and evaluated by five testers according to the evaluation criteria in Table 1. The mass of each sample was also measured after each specified time.

[0045] [Table 1]

[0046] The average evaluation score of the fragrance tone for each elapsed time is shown in Figure 8. As shown in Figure 8, it was found that granular skeleton A and granular skeleton B showed less change in fragrance tone over a long period of time compared to the conventional product.

[0047] The measurement results of the sample mass over time are shown in Figure 9. As shown in Figure 9, it was found that granular skeleton A and granular skeleton B were able to support the flavoring for a longer period of time compared to the conventional product. [Explanation of symbols]

[0048] 10 Granular skeleton 20 Skeleton 22 Skeletal Surface 30 Macropores 30a Non-penetrating macropores 30b Through macropores 32 Inner surface of macropore 40 Mesopores

Claims

1. 1. A sustained release fragrance composition comprising: A framework having a three-dimensional continuous network structure having voids; A sustained release liquid present in at least a portion of the void; Equipped with the voids are a plurality of macropores extending from the surface of the framework toward the inside and distributed on the surface of the framework, and a plurality of mesopores extending from the surface of the framework and the inner surfaces of the macropores toward the inside of the framework and distributed on the surface of the framework and the inner surfaces of the macropores, and A sustained-release fragrance composition, wherein at least a portion of the plurality of mesopores are through-pores.

2. The most frequent pore size of the macropores is 0.1 μm or more and 100 μm or less, and The sustained-release fragrance composition according to claim 1, wherein the most frequent pore size of the mesopores is 0.1 nm or more and less than 100 nm.

3. 3. The sustained-release aroma composition according to claim 1, wherein the skeleton is a granular skeleton, and the longest diameter of the granular skeleton is 500 μm or less.

4. 3. The sustained-release fragrance composition according to claim 1, wherein the framework is silica or a silicon oxide complex mainly containing silicon oxide.

5. The sustained-release fragrance composition according to claim 1 or 2, wherein the sustained-release liquid is an oil containing a fragrance component.

Citation Information

Patent Citations

  • Fragrance encapsulated capsule and cosmetic blended therewith

    JP2014237761A

Cited By

  • Method for producing porous body

    WO2026141532A1