Composite fiber for cool-feeling fabric, manufacturing method thereof, cool-feeling fabric, and textile product

A composite fiber with a high-density polyethylene core and nylon 6 sheath, produced via co-extrusion and stretching, addresses the lack of hygroscopicity, quick drying, and flexibility in existing fibers, offering enhanced dyeability and cooling sensation.

JP2024151101AActive Publication Date: 2024-10-24QINGDAO SHAZHI TEXTILE TECH CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023064236
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-24
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

Existing core-sheath composite fibers lack high hygroscopicity, quick drying properties, flexibility, and dyeability, while providing a cooling sensation.

Method used

A composite fiber with a core containing high-density polyethylene and a sheath made of nylon 6, having an irregular cross-section and specific mass content, is produced through co-extrusion, stretching, and optionally twisting, to enhance hygroscopicity, quick drying, flexibility, and dyeability.

Benefits of technology

The resulting fiber exhibits high hygroscopicity, quick drying, flexibility, and dyeability, providing a cooling sensation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151101000003
    Figure 2024151101000003
  • Figure 2024151101000001
    Figure 2024151101000001
  • Figure 2024151101000002
    Figure 2024151101000002
Patent Text Reader

Abstract

To provide a fiber that has a high moisture absorption property, a quick drying property, and flexibility, is dyeable, and gives a cool feeling.SOLUTION: There is provided a composite fiber for a cool-feeling fabric with a core-sheath structure, wherein a core of the composite fiber for the cooling fabrics with a core-sheath structure contains high-density polyethylene, and the sheath contains nylon 6. A manufacturing method of the composite fiber for the cool-feeling fabric includes a co-extrusion step in which high density polyethylene constituting the core and nylon 6 constituting the sheath are co-extruded; and a stretching step for stretching filaments obtained in the co-extrusion step. The composite fiber for cool-feeling fabrics is used in a cool-feeling fabrics. The cool-feeling fabric is used in a textile product.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite fiber for cooling sensation fabric, a manufacturing method thereof, a cooling sensation fabric, and a textile product. [Background technology]

[0002] Composite fibers having a core-sheath structure are known. Cited Document 1 discloses a nonwoven fabric containing a core-sheath type composite fiber in which the core and the sheath are made of components with different dielectric tangents and melting points. Currently, there are commercially available core-sheath type composite fibers that give a cool feeling. The core of the commercially available core-sheath type composite fibers is made of nylon 6, and the sheath is made of polyethylene. Due to the characteristics of polyethylene, the moisture absorption and dyeability of the commercially available core-sheath type composite fibers are low. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-231592 A Summary of the Invention [Problem to be solved by the invention]

[0004] Recently, there has been a demand for fibers that have high moisture absorption, quick drying, flexibility, dyeability, and a cool feel.

[0005] The problem to be solved by the present invention is to provide a fiber which has high moisture absorption, quick drying properties, flexibility, is dyeable, and provides a cool feel. [Means for solving the problem]

[0006] The present inventors have conducted extensive research in light of the above problems and have found that a composite fiber having a core containing high density polyethylene and a sheath containing nylon 6 has high moisture absorption, quick drying properties, flexibility, is dyeable, and provides a cool feel. The present invention has been completed based on these findings.

[0007] The present invention relates to a composite fiber for cooling fabrics having a core-sheath structure, the core comprising high-density polyethylene and the sheath comprising nylon 6. Preferably, the content of the core in the composite fiber for cooling fabric is 20 to 60% by mass, and the content of the sheath in the composite fiber for cooling fabric is 40 to 80% by mass. The cross-sectional shape of the core and the sheath is preferably an irregular cross section having irregularities on the outer periphery. Preferably, the composite fiber for cooling fabric has a fineness of 8-400 tex and a filament count of 10-250.

[0008] The present invention relates to a method for producing a composite fiber for cooling fabric, the method including a co-extrusion step of co-extruding the high-density polyethylene constituting the core and the nylon 6 constituting the sheath, and a drawing step of drawing the filaments obtained in the co-extrusion step. The method for producing a composite fiber for cooling fabric preferably further includes a twisting step of twisting the filaments obtained in the co-extrusion step.

[0009] The present invention also relates to a cooling fabric in which the above-mentioned composite fiber for cooling fabric is used.

[0010] The present invention further relates to a textile product in which the cooling fabric is used. The textile product is preferably a futon, a futon cover, a pillow, a mattress, a seat cushion, a cushion, a rug, or clothing. Effect of the Invention

[0011] The composite fiber for cooling sensation fabrics having a core-sheath structure of the present invention provides a fiber that has high moisture absorption, quick-drying properties and flexibility, is dyeable, and gives a cooling sensation. The manufacturing method for the composite fiber for cooling sensation fabrics of the present invention provides a manufacturing method for the composite fiber for cooling sensation fabrics. The cooling sensation fabric of the present invention provides a cooling sensation fabric that has high moisture absorption, quick-drying properties and flexibility, and gives a cooling sensation. The textile product of the present invention provides a textile product that has high moisture absorption, quick-drying properties and flexibility, and gives a cooling sensation. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram showing one embodiment of a conjugate fiber for cooling fabric of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will now be described in further detail. In addition, unless otherwise specified, "~" in a numerical range means from above to below, and both ends of the range are included. In addition, when a numerical range is indicated, the upper limit and the lower limit can be appropriately combined, and the numerical range obtained by combining them is also disclosed. In addition, in the description of the drawings, the same elements are denoted by the same reference numerals, and duplicated description will be omitted. Also, the dimensional ratios of the drawings are exaggerated for the convenience of explanation, and may differ from the actual ratios.

[0014] <Composite fiber for cooling fabrics> The core of the composite fiber for cooling fabric having a core-sheath structure of the present invention contains high density polyethylene, and is preferably made of high density polyethylene. The sheath of the composite fiber for cooling fabric of the present invention contains nylon 6, and is preferably made of nylon 6. Since nylon 6 has a polar group, the composite fiber for cooling fabric of the present invention having a sheath containing nylon 6 has high hygroscopicity. However, since nylon 6 is a hydrophobic resin, the composite fiber for cooling fabric of the present invention has high quick-drying properties. Furthermore, due to the flexibility of high density polyethylene and nylon 6, the composite fiber for cooling fabric of the present invention has high flexibility.

[0015] Since nylon 6 is a dyeable resin, the composite fiber for cooling fabric of the present invention can be dyed. Furthermore, since the melting point of nylon 6 is 200°C or higher, the heat-resistant temperature of the composite fiber for cooling fabric of the present invention is 100°C or higher. On the other hand, when the commercially available core-sheath type composite fiber is heated to 100°C or higher, the polyethylene constituting the sheath melts, and its heat-resistant temperature is less than 100°C.

[0016] The content of the core in the composite fiber for cooling sensation fabric of the present invention is preferably 20 to 60% by mass, and the content of the sheath in the composite fiber for cooling sensation fabric of the present invention is preferably 40 to 80% by mass. When the contents of the core and sheath in the composite fiber for cooling sensation fabric of the present invention are within the above ranges, the moldability and ability to provide a cooling sensation of the composite fiber for cooling sensation fabric of the present invention are further improved.

[0017] One embodiment of the conjugate fiber for cooling fabric of the present invention is shown in Figure 1. The conjugate fiber for cooling fabric 1 has a core 2 and a sheath 3. The cross-sectional shapes of the core 2 and the sheath 3 are not limited to a specific shape. The cross-sectional shapes of the core 2 and the sheath 3 may be different. Examples of the cross-sectional shapes include a circle, an ellipse, a triangle, a rectangle, a star, a cross, a Y-shape, and the like. The cross-sectional shapes of the core 2 and the sheath 3 are preferably irregular cross sections having irregularities on the periphery, such as a star, a cross, or a Y-shape. When the cross-sectional shapes of the core 2 and the sheath 3 are irregular cross sections having irregularities on the periphery, the quick-drying property of the composite fiber for cooling fabric of the present invention is further improved.

[0018] The fineness of the conjugate fiber for cooling sensation fabric of the present invention is preferably 8 to 400 tex, and the number of filaments is preferably 10 to 250. When the fineness and the number of filaments of the conjugate fiber for cooling sensation fabric of the present invention are within the above ranges, the moisture absorption, quick-drying properties, flexibility, and ability to provide a cooling sensation of the conjugate fiber for cooling sensation fabric of the present invention are improved.

[0019] <Method of manufacturing composite fiber for cooling fabric> The manufacturing method of the composite fiber for cool-feeling fabric of the present invention includes a co-extrusion step of co-extruding the high-density polyethylene constituting the core and the nylon 6 constituting the sheath. The co-extrusion step is carried out under normal co-extrusion conditions in the spinning process of synthetic resins. Dried pellets of high-density polyethylene and nylon 6 are melted and extruded by a screw extruder, and the melts are fed into a spinning module at a preset discharge rate through a metering pump. Next, the high-density polyethylene and nylon 6 in the spinning module are filtered, pressurized, and co-extruded uniformly and continuously from a spinning plate. Preferably, the initial pressure of the spinning module is adjusted to about 110 kg, and sintered stainless steel metal filter sand of 80 to 100 mesh is used in the filtration.

[0020] The co-extrudate extruded from the spinning plate may be uniformly cooled to about 120 to 140°C, wound on a roll, and molded. The winding may be repeated about 8 times, and the heat shrinkage rate of the molded product is about 9%. After the molding, the molded product is oiled in a tanker and then subjected to a stretching process described below.

[0021] The method for producing the composite fiber for cooling sensation fabric of the present invention includes a drawing step of drawing the filament obtained in the co-extrusion step. The oiled molded product is taken up on a take-up roller and drawn. The draw ratio is preferably 4 to 5 times, and the draw temperature is preferably 40 to 50°C. When the draw ratio and the draw temperature are within the above ranges, fluffing and entanglement with the take-up roller of the composite fiber for cooling sensation fabric of the present invention are further prevented, and the moisture absorption, quick-drying, flexibility, and ability to give a cooling sensation are further improved.

[0022] The manufacturing method of the conjugate fiber for cooling fabric of the present invention preferably further includes a twisting step of twisting the filaments obtained in the co-extrusion step. Therefore, the conjugate fiber for cooling fabric of the present invention may have an interlace part 4. The interlace part 4 makes the conjugate fiber for cooling fabric of the present invention less likely to be cut.

[0023] <Application of composite fibers for cool-feeling fabrics> The composite fiber for cool feeling fabric of the present invention is used as a material for cool feeling fabrics such as fabrics and knits. The cool feeling fabric is used as a material for fiber products such as futons, futon covers, pillows, mattresses, zabutons, cushions, rugs, and clothes.

Example

[0024] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited thereto.

[0025] In the examples and comparative examples, various physical properties were measured as follows. <Q-MAX value (cool feeling value)> In accordance with JIS L1927, the cool feeling provided by each knit fabric was measured using a Thermo Lab II contact cool and warm feeling measuring device manufactured by Kato Tech Co., Ltd. That is, the sensor was heated by bringing the sensor into contact with the hot plate, the temperature difference between the knit fabric and the sensor was set to 10 ° C, and the two were brought into contact, and the heat transfer amount (Q-MAX value) was measured. The larger the value, the stronger the cool feeling the knit fabric gives to human skin.

[0026] <Quick drying property> The quick drying property of each knit fabric was measured under the conditions of 20 ° C and 65% RH based on the ISO I7617 A-1 method.

[0027] [Example 1] Dried high-density polyethylene pellets were melt-extruded in an extruder set at extrusion temperatures of 230°C, 245°C, and 249°C. Dried nylon 6 pellets were melt-coextruded in an extruder set at extrusion temperatures of 246°C, 250°C, and 268°C. The coextruded melt was placed in a spinning module set at 269°C. Next, each of the high-density polyethylene and nylon 6 in the spinning module was filtered with 80-100 mesh sintered stainless steel metal filter sand, and was uniformly and continuously coextruded from the spinning plate at an initial pressure of 110 kg in the spinning module. The filaments extruded from the spinning plate had a core consisting of 30% by mass of high-density polyethylene and a sheath consisting of 70% by mass of nylon 6. The filaments were cooled with air at 26°C at a wind speed of 0.7 m / s and dropped 2.2 m. The dropped filaments were oiled in a tanker so that the mass of the oil agent (oil supply rate) relative to the mass of the filaments and the oil agent was 1.2% by mass. The oiled filaments were uniformly cooled to 132°C, wound six times on a roll, and molded. The molded product was wound on a winding roller, fuzz was removed, and stretched to a stretch ratio of 4.9 and a stretch temperature of 46°C. The heat shrinkage of the produced composite fiber for cooling fabric was 9%, its fineness was 80 tex, and its filament number was 48. The composite fiber for cooling fabric was woven to produce a knit fabric, and its Q-MAX value was measured. The results are shown in Tables 1 and 2.

[0028] [Example 2] Dried high-density polyethylene pellets were melt-extruded in an extruder set at extrusion temperatures of 230°C, 245°C, and 249°C. Dried nylon 6 pellets were melt-coextruded in an extruder set at extrusion temperatures of 246°C, 250°C, and 268°C. The coextruded melt was placed in a spinning module set at 269°C. Next, each of the high-density polyethylene and nylon 6 in the spinning module was filtered with 80-100 mesh sintered stainless steel metal filter sand, and was uniformly and continuously coextruded from the spinning plate at an initial pressure of 110 kg in the spinning module. The filaments extruded from the spinning plate had a core consisting of 40% high-density polyethylene by mass and a core consisting of 60% nylon 6 by mass. The filaments were cooled with air at 26°C at a wind speed of 0.7 m / s and dropped 2.2 m. The dropped filaments were oiled in a tanker so that the mass of the oil agent (oil supply rate) relative to the mass of the filaments and the oil agent was 1.2% by mass. The oiled filaments were uniformly cooled to 133°C, wound around a roll seven times, and molded. The molded product was wound around a winding roller, fuzz was removed, and stretched to a stretch ratio of 4.9 and a stretch temperature of 46°C. The heat shrinkage of the composite fiber for cooling fabric produced was 9%, its fineness was 100 tex, and its filament number was 48. The composite fiber for cooling fabric was woven to produce a knit fabric, and its Q-MAX value was measured. The results are shown in Tables 1 and 2.

[0029] [Example 3] The dried high density polyethylene pellets were melt extruded in an extruder set at extrusion temperatures of 230°C, 248°C, and 252°C. The dried nylon 6 pellets were melt co-extruded in an extruder set at extrusion temperatures of 276°C, 272°C, 271°C, and 270°C. The co-extruded melt was placed in a spinning module set at 269°C. Next, each of the high density polyethylene and nylon 6 in the spinning module was filtered with 80-100 mesh sintered stainless steel metal filter sand, and was co-extruded uniformly and continuously from the spinning plate at an initial pressure of 110 Kg in the spinning module. The filaments extruded from the spinning plate had a core consisting of 50% high density polyethylene by mass and a sheath consisting of 50% nylon 6 by mass. The filaments were cooled with air at 28°C at a wind speed of 0.75 m / s and dropped 2.3 m. The dropped filaments were oiled in a tanker so that the mass of the oil with respect to the mass of the filaments and the oil (oiling rate) was 1.2% by mass. The oiled filaments were uniformly cooled to 123°C, wound around a roll 7 times, and molded. The molded product was wound around a winding roller, fuzz was removed, and the product was stretched to a stretch ratio of 4.9 times and a stretching temperature of 42°C. The heat shrinkage rate of the manufactured composite fiber for cooling fabric was 9%, its fineness was 100 tex, and its filament number was 48. The composite fiber for cooling fabric was woven to prepare a knit fabric, and its Q-MAX value was measured. The results are shown in Tables 1 and 2.

[0030] [Comparative Example 1] Except for using low-density polyethylene instead of high-density polyethylene, the same procedure as in Example 1 was carried out. The knit fabric produced by weaving the obtained composite fiber had a hard feel and was unsuitable as a material for textile products.

[0031] [Table 1]

[0032] [Table 2]

[0033] The knit fabrics produced by weaving the composite fibers for cooling fabrics of Examples 1 to 3, in which the core and sheath contain a specific resin, have high quick-drying properties, and furthermore, each knit fabric provides a high cooling sensation. Since nylon 6 has a polar group, the knit fabrics produced by weaving the composite fibers for cooling fabrics of Examples 1 to 3, which have a sheath containing nylon 6, have high moisture absorption. Furthermore, due to the flexibility of high-density polyethylene and nylon 6, the knit fabrics produced by weaving the composite fibers for cooling fabrics of Examples 1 to 3 have high flexibility. [Explanation of symbols]

[0034] 1... Composite fiber for cooling fabric, 2... Core, 3... Sheath, 4... Interlaced part.

Claims

1. A composite fiber for cooling fabrics having a core-sheath structure, the core comprises high density polyethylene; The composite fiber for cool-feeling fabrics is characterized in that the sheath contains nylon 6.

2. The composite fiber for cooling fabric according to claim 1, characterized in that the content of the core in the composite fiber for cooling fabric is 20 to 60% by mass, and the content of the sheath in the composite fiber for cooling fabric is 40 to 80% by mass.

3. The composite fiber for cooling fabric according to claim 1, characterized in that the cross sections of the core and the sheath are irregular cross sections having irregularities on the outer periphery.

4. 2. The composite fiber for cooling fabrics according to claim 1, characterized in that the fiber has a fineness of 8 to 400 tex and a filament count of 10 to 250.

5. a co-extrusion step of co-extruding the high density polyethylene constituting the core and the nylon 6 constituting the sheath; The method for producing a composite fiber for cooling fabric according to any one of claims 1 to 4, comprising a drawing step of drawing the filaments obtained in the co-extrusion step.

6. The method for producing a composite fiber for cooling fabric according to claim 5, further comprising a twisting step of twisting the filaments obtained in the co-extrusion step.

7. A cooling fabric using the composite fiber for cooling fabric according to any one of claims 1 to 4.

8. A textile product using the cooling fabric according to claim 7.

9. 9. The textile product according to claim 8, which is a futon, a futon cover, a pillow, a mattress, a cushion, a rug, or clothing.

Citation Information

Patent Citations

  • Fiber and application method and application thereof, and textile

    CN111172619A

  • Multi-component fibers

    JP2010538171A

  • Heat-shielding composite fiber with excellent cool sensation

    JP2014077214A

  • Heat insulating material provided with thermal storage properties

    JP2019143270A

  • Sanitary nonwoven fabric and manufacturing method therefor

    JP2023065155A