High temperature superconducting tape sheet for multi-turn coils, multi-turn coil therewith, superconducting flux transformer, and superconducting magnetometer
The superconducting tape sheet with overlapping planar coil sections addresses the limitations of existing methods by enabling low-profile, multi-turn coils with efficient magnetic flux transmission without bonding, suitable for superconducting flux transformers and magnetometers.
Patent Information
- Application Number
- JP2023064605
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing multi-turn superconducting coils using high-temperature superconducting tape wires require lengthy processing times, large joint shapes, and are limited by wire width, making it difficult to create low-profile coils with a sufficient number of turns.
A high-temperature superconducting tape sheet with planar coil sections connected by a wiring section forms a closed circuit, allowing planar coil sections to be stacked and overlapped in the same direction without bonding, enabling a multi-turn coil structure.
This approach allows for the creation of a multi-turn coil that maintains a superconducting state at liquid nitrogen temperatures without bonding, facilitating low-profile coils with increased turns and improved magnetic flux transmission efficiency.
Smart Images

Figure 2024151395000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a high-temperature superconducting tape sheet for a multi-turn coil, a multi-turn coil using the same, a superconducting flux transformer, and a superconducting magnetometer. [Background technology]
[0002] Multi-turn coils using metallic superconducting wires have been put to practical use as superconducting flux transformers for precision magnetic measurements. Since superconducting flux transformers use persistent supercurrents, it is essential to make the coils into superconducting closed circuits by joining the ends of the wires or other methods.
[0003] Meanwhile, tape wires made of high-temperature superconducting ceramic materials that have a superconducting transition temperature above the boiling point of liquid nitrogen (77 K at 1 atmosphere) and have excellent properties such as critical current density are commercially available, and techniques for joining tape wires are known (for example, see Non-Patent Documents 1 and 2).
[0004] According to Figure 2 of Non-Patent Document 1, the superconducting layer of the tape wire is exposed, melted and diffused under high temperature and pressure, and annealed in an oxygen atmosphere for 350 hours, enabling a bond with good superconducting properties at the boiling point of liquid nitrogen. Also, according to Figure 1 of Non-Patent Document 2, a bonding technology for tape wires using a superconducting bulk body is reported. However, all of these methods have limitations, such as requiring a long processing time and making the shape of the bonded part large.
[0005] A technique for fabricating a superconducting closed circuit in a tape wire without using a joint has been reported (see, for example, Patent Documents 1 and 2). Patent Document 1 discloses a method for fabricating a superconducting closed circuit by providing a slit along the length direction of the tape wire and bending it. According to this method, since no joints are used to fabricate the closed circuit, the entire closed circuit can be maintained in a superconducting state at the boiling point of liquid nitrogen. By adopting this method, a coil with a large diameter and a multi-winding structure can be provided, but the height of the coil is limited by the width of the flat tape wire used. Therefore, in order to fabricate a low-profile coil, it is necessary to perform slit processing on a tape wire with a very narrow width, which requires high-precision processing. In addition, it is difficult to fabricate a small-diameter coil due to the bending resistance of the processed thin wire.
[0006] Patent Document 2 discloses a method for fabricating a superconducting closed circuit without using any bonding, by patterning a closed circuit on a flat substrate such as a tape wire by ion milling. This method can provide a low-profile coil that maintains the entire closed circuit in a superconducting state at the boiling point of liquid nitrogen. However, the number of windings is limited to one turn, and the outer diameter of the coil is small, not exceeding the width of the substrate.
[0007] Furthermore, Patent Documents 1 and 2 disclose the use of the above-mentioned coil in a superconducting flux transformer. In a superconducting flux transformer used in combination with a magnetic sensor, a structure in which the distance between the magnetic sensor and the superconducting flux transformer is small is advantageous in order to reduce leakage of the transmitted magnetic flux. In particular, in combination with a superconducting flux transformer and a high-temperature superconducting SQUID having a small loop shape, a structure in which the superconducting flux transformer, which is a low-profile planar superconducting coil, is placed closely to the SQUID loop is desirable. In addition, a superconducting flux transformer using a small-diameter multi-turn coil is effective in improving the efficiency of magnetic flux transmission.
[0008] Up to now, examples of fabricating multi-turn planar coils by interlayer wiring using multi-layer superconducting thin films have been reported (see, for example, Non-Patent Document 3). According to Non-Patent Document 3, there are many process constraints for coil fabrication, such as the need for vacuum processes and single crystal substrates. There have also been reports of coils using flexible tape wires without using vacuum processes (see, for example, Non-Patent Document 4). According to Non-Patent Document 4, a superconducting gradiometer has been reported in which a superconducting closed circuit including multiple planar coil parts in the same circuit formed on a flexible tape wire is formed, and the tape wire is bent to arrange two planar coil parts apart so that the current flows in opposite directions. In this superconducting gradiometer, the number of turns of each planar coil part is one. Also, since the current flows in opposite directions, a multi-turn coil with an increased number of turns cannot be realized even if the planar coil parts are stacked. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2013-175577 A [Patent Document 2] JP 2011-181559 A [Non-patent literature]
[0010] [Non-Patent Document 1] YJPark et al.,Supercond.Sci.Technol.27 085008 (2014). [Non-Patent Document 2] X.Jin et al.,Supercond.Sci.Technol.28 075010 (2015). [Non-Patent Document 3] AHMiklich et al.,Appl.Phys.Lett.59, 988 (1991). [Non-Patent Document 4] M. Bick et al., IEEE Trans. Appl. Supercond., 15(2), 765(2005). Summary of the Invention [Problem to be solved by the invention]
[0011] An object of the present invention is to provide a high-temperature superconducting tape sheet for a multi-turn coil that does not require joining and is a closed circuit, a multi-turn coil using the same, a superconducting flux transformer using the same, and a superconducting magnetometer. [Means for solving the problem]
[0012] The high-temperature superconducting tape sheet for multi-turn coils according to the present invention solves the above-mentioned problems by comprising a plurality of planar coil sections, each having one turn, and a wiring section connecting each of the plurality of planar coil sections, the plurality of planar coil sections and the wiring section forming a closed circuit, and at least some (at least two or more) of the plurality of planar coil sections being overlapped with each other so that the direction of current flow is the same. At least some of the planar coil portions may be overlapped with each other by bending the tape sheet in an in-plane direction. At least some of the planar coil portions may be overlapped with each other by forming three-dimensional loops by bending the tape sheet in a direction perpendicular to the surface of the tape sheet. The high temperature superconducting tape sheet may have a width of 2 mm or more and 20 mm or less. The high temperature superconducting tape sheet may have a length of 50 mm or more and 1 m or less. The ratio of an outer diameter of the at least some planar coil sections to a width of the high temperature superconducting tape sheet may be between 0.2 and 1.0. The at least some planar coil portions may have an inner diameter of 0.1 mm or more and 10 mm or less. The at least some planar coils may be in number between 2 and 5, inclusive. The shape of the plurality of planar coil portions may be at least one selected from the group consisting of a circle, an ellipse, and a polygon. The superconducting layer of the high-temperature superconducting tape sheet contains a general formula REBa a Cu3O b which may be a material represented by. Here, RE is at least one element selected from the group consisting of yttrium (Y), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), and ytterbium (Yb), a satisfies 0 < a ≤ 2, and b satisfies 6.2 ≤ b ≤ 7. The multi-layer coil according to the present invention is made of the high-temperature superconducting tape, thereby solving the above problems. In the multi-layer coil, among the plurality of planar coil portions in the high-temperature superconducting tape sheet, at least some of the planar coil portions may be overlapped so that the direction of current flow is the same. The superconducting flux transformer according to the present invention includes the multi-layer coil, thereby solving the above problems. The superconducting magnetometer according to the present invention includes the superconducting flux transformer and one or more magnetic sensors selected from the group consisting of a high-temperature superconducting SQUID, an AMR element, a TMR element, an MR element including a GMR element, an MI element, a flux gate, and a Hall element, thereby solving the above problems.
Advantages of the Invention
[0013] The high-temperature superconducting tape sheet according to the present invention includes a plurality of planar coil portions with one turn each and wiring portions connecting them, which form a closed circuit. Further, some (at least two or more) of the plurality of planar coil portions are overlapped so that the direction of current flow is the same, so that a multi-layer coil that does not require bonding and is a closed circuit can be provided. By using such a multi-layer coil, a superconducting flux transformer and a superconducting magnetometer can be provided.
Brief Description of the Drawings
[0014] [Figure 1] FIG. 1 is a top view of the high-temperature superconducting tape sheet for a multi-turn coil according to the present invention. [Diagram 2] Cross-sectional view of the high-temperature superconducting tape sheet for multi-turn coils of the present invention. [Diagram 3] FIG. 2 is an enlarged view of the planar coil portion 121 of FIG. 1. [Figure 4] FIG. 13 is a schematic diagram showing another shape of a planar coil portion; [Diagram 5] 2 is a diagram showing a procedure for producing a multi-turn coil from the tape sheet 100 of FIG. 1. [Figure 6] FIG. 1 is a top view of another high-temperature superconducting tape sheet for a multi-turn coil according to the present invention. [Figure 7] A diagram showing a multi-turn coil made using the tape sheet shown in Figure 6. [Figure 8] FIG. 1 is a top view of another high-temperature superconducting tape sheet for a multi-turn coil according to the present invention. [Figure 9] A diagram showing a multi-turn coil made using the tape sheet of Figure 8. [Figure 10] Schematic diagram showing a superconducting gradiometer using a multi-turn coil according to the present invention. [Figure 11] Schematic diagram showing a superconducting magnetometer according to the present invention. [Figure 12] Photograph of the high-temperature superconducting tape sheet for multi-turn coils in Example 1 [Figure 13] Photograph showing the high-temperature superconducting flux transformer of Example 2 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that like elements are given like reference numerals and their description will be omitted.
[0016] (Embodiment 1) In the first embodiment, a high temperature superconducting tape sheet for a multi-turn coil of the present invention, a manufacturing method thereof, and a multi-turn coil and a superconducting flux transformer obtained thereby will be described.
[0017] FIG. 1 is a top view of the high temperature superconducting tape sheet for a multi-turn coil of the present invention. FIG. 2 is a cross-sectional view of the high temperature superconducting tape sheet for a multi-turn coil of the present invention.
[0018] The high-temperature superconducting tape sheet for multi-turn coils (hereinafter sometimes simply referred to as the tape sheet) 100 of the present invention comprises a plurality of planar coil sections 121-123, each of which has one turn, and a wiring section 130 connecting the plurality of planar coil sections 121-123, which as a whole form an electrically closed closed circuit 110.
[0019] The tape sheet 100 of the present invention has a high-temperature superconducting layer 230 made of a high-temperature superconductor having a superconducting transition temperature equal to or higher than the boiling point of liquid nitrogen (77 K at 1 atmosphere) and is not limited as long as it has the above-mentioned closed circuit 110 in a tape-like sheet, but illustratively it may be a sheet having a substrate 210, an intermediate layer 220 thereon, a high-temperature superconducting layer 230 thereon, and a metal cover layer 240 thereon, as shown in FIG. 2.
[0020] The substrate 210 is a tape-shaped metal substrate, and illustratively, a known tape substrate such as a nickel alloy represented by Hastelloy (registered trademark), a copper alloy, a silver alloy, stainless steel, etc. The substrate 210 preferably has a thickness in the range of 10 μm to 500 μm.
[0021] The intermediate layer 220 is located between the substrate 210 and the high-temperature superconducting layer 230, and may be one or more layers such as a diffusion prevention layer, a bed layer, a buffer layer, etc. The diffusion prevention layer is a layer that suppresses the diffusion of components of the substrate 210 into the high-temperature superconducting layer 230. An exemplary diffusion prevention layer is Si3N4, Al2O3, etc., and has a thickness in the range of 10 nm to 500 nm. The bed layer is a layer that suppresses an interface reaction between the substrate 210 and the high-temperature superconducting layer 230. An exemplary bed layer is a rare earth oxide, and has a thickness in the range of 10 nm to 150 nm. Here, the rare earth oxide means a compound that is usually represented by RE2O3 when rare earth elements such as yttrium (Y) and erbium (Er) are RE, and is represented by REO2 with a few exceptions such as cerium (Ce). The buffer layer is a layer that controls the orientation of the high-temperature superconducting layer 230. Exemplary buffer layers are metal oxides such as CeO2, Y2O3, Al2O3, Gd2O3, Zr2O3, Gd2Zr2O7, MgO, ZrO2-Y2O3 (YSZ), SrTiO3, etc. formed by the IBAD method and have a thickness in the range of 50 nm to 500 nm.
[0022] The high-temperature superconducting layer 230 may preferably be a bismuth-based superconducting ceramic or a rare earth-based superconducting ceramic. These are known as high-temperature superconductors and can be deposited by physical vapor deposition, chemical vapor deposition, or coating. An example of a bismuth-based superconducting ceramic is the well-known Bi2Sr2Ca2Cu3O 10 , Bi2Sr2CaCu2O 10 The rare earth-based superconducting ceramics may preferably be represented by the general formula REBa containing rare earth elements (RE), barium (Ba), copper (Cu), and oxygen (O): a CuO bIt is represented by [formula], where RE is at least one element selected from the group consisting of yttrium (Y), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), and ytterbium (Yb), a satisfies 0 < a ≤ 2, and b satisfies 6.2 ≤ b ≤ 7. By using such a rare-earth-based superconducting oxide, a high-temperature superconducting tape sheet excellent in characteristics such as critical current density can be provided. The high-temperature superconducting layer 230 preferably has a thickness in the range of 100 nm or more and 1 μm or less.
[0023] The metal cover layer 240 protects the high-temperature superconducting layer 230 and is, for example, silver (Ag). The metal cover layer 240 preferably has a thickness in the range of 500 nm or more and 5 μm or less. In addition, although not shown, there may be a cover layer 240 also under the base material 210, and on the outer side of one or both of the metal cover layers 240, there may be a plating layer, which is, for example, copper (Cu), as a stabilizing layer.
[0024] In FIG. 2, the portions where the high-temperature superconducting layer 230 remains become the planar coil portions 121 to 123 and the wiring portion 130 shown in FIG. 1. For the other portions, in FIG. 2, the intermediate layer 220 is exposed, but it is not limited to this. The base material 210 may be exposed.
[0025] Returning to FIG. 1 again. The arrow in FIG. 1 indicates the direction of the current flowing in the closed circuit 110. In the tape sheet 100, the plurality of planar coil portions 121 to 123 are overlapped with each other so that the direction of the current flowing through them is the same. Thereby, joining is not required, and a multi-wound coil that is a closed circuit can be provided.
[0026] The tape sheet 100 may have cuts or notches in portions other than the closed circuit 110. This makes it easier to stack multiple planar coil portions. Specifically, the presence of the notches 140 in the tape sheet 100 makes it easier to stack the multiple planar coil portions 121-123 on top of each other by bending the tape sheet 100 in the in-plane direction so that all of the currents flow in the same direction.
[0027] In FIG. 1, three planar coil sections 121-123 are shown as at least some (at least two or more) planar coil sections, but there is no particular limit to the number of planar coil sections included in the closed circuit. The number of planar coil sections to be overlapped is preferably 2 or more and 5 or less. Within this range, distortion due to deformation occurring during overlapping can be reduced, and deterioration of superconducting properties can be suppressed. More preferably, the number of planar coil sections is 3 or more and 4 or less. Within this range, a multi-turn coil with a necessary and sufficient number of coil turns can be supplied.
[0028] 1 shows a state in which a current flows counterclockwise in the closed circuit 110, but a current may flow clockwise. In this case, it goes without saying that the planar coil portions 121 to 123 are overlapped so that the current flows in the same direction.
[0029] The width W of the tape sheet 100 and the length L of the tape sheet are appropriately set according to the dimensions of the desired multi-winding coil, but preferably, the width W of the tape sheet 100 is 2 mm or more and 20 mm or less. Within this range, it is easy to select from commercially available wires, and the dimensions of a particularly low-profile multi-winding coil can be realized. From the viewpoint of processing, if the width W is in the range of 10 mm or more and 15 mm or less, a low-profile multi-winding coil can be provided with good yield. In addition, preferably, the length L of the tape sheet is 50 mm or more and 1 meter or less. Within this range, the number of turns of a generally required multi-winding coil can be realized.
[0030] FIG. 3 is an enlarged view of the planar coil portion 121 of FIG.
[0031] The maximum length of the inner side of the coil of the planar coil part 121, excluding the wiring, is defined as the inner diameter d, and the maximum length of the outer side of the coil, including the wiring, is defined as the outer diameter D. The outer diameter D of the planar coil part 121 does not exceed the width W of the tape sheet 100, but may be appropriately set within that range according to the dimensions of the desired multi-turn coil. The ratio (D / W) of the outer diameter D of the planar coil part to the width W of the tape sheet 100 is preferably 0.2 or more and 1.0 or less. Within this range, the dimensions of a multi-turn coil generally required can be realized. More preferably, D / W may be 0.45 or more and 1.0 or less. This makes it possible to provide a low-profile multi-turn coil. The inner diameter d of the planar coil part 121 is preferably 0.1 mm or more and 10 mm or less. Within this range, it is easy to couple with a magnetic sensor element such as a high-temperature superconducting SQUID, and a generally required area of a multi-turn coil can be realized. The width of the wiring is, for example, in the range of 0.2 mm or more and 1 mm or less.
[0032] FIG. 4 is a schematic diagram showing the shape of another planar coil portion.
[0033] 1 has circular planar coil parts 121-123, but the shape of the planar coil parts is not limited to circular and any shape can be selected. The shape of the multiple planar coil parts may be exemplarily selected from the group consisting of a circle, an ellipse, and a polygon, as shown in FIG. 4. For example, when the multi-turn coil of the present invention is used as a superconducting magnetic flux transformer, the shape of the planar coil parts can be selected so that the shape of the multi-turn coil is the same as the area to be detected.
[0034] In addition, when the shape of the planar coil portion is an ellipse, the inner diameter d and the outer diameter D are the major axis excluding the wiring and the major axis including the wiring, respectively, and when the shape of the planar coil portion is a polygon, the inner diameter d and the outer diameter D are the diameter or major axis excluding the wiring and the diameter or major axis including the wiring, respectively, when a circle or an ellipse inscribed in the polygon and a circle or an ellipse circumscribed the polygon are drawn.
[0035] A method for producing the closed circuit 110 on the tape sheet 100 will be described. By removing the high temperature superconducting layer 230 only from the portion of the tape sheet 100 other than the closed circuit 110, it is possible to make it possible for a current to flow in the closed circuit 110 on the tape sheet 100 and to make it possible for a current to not flow in the portion of the tape sheet 100 other than the closed circuit 110.
[0036] When removing the high temperature superconducting layer 230 from the portion other than the closed circuit 110 of the tape sheet 100, the method may also be a method of removing other laminated layers. For example, the method may be a method of removing the metal cover layer 240 and the high temperature superconducting layer 230, or a method of removing from the metal cover layer 240 to the base material 210.
[0037] Methods for removing the high temperature superconducting layer 230 from the portion of the tape sheet 100 other than the closed circuit 110 include cutting, milling, and chemical etching. Also, a combination of these methods may be selected.
[0038] The cutting method is a method of physically separating the entire layer, including the high-temperature superconducting layer 230, from the closed circuit in the portion of the tape sheet 100 other than the closed circuit 110. To cut, a tool commonly used for cutting can be used, and may be one that utilizes a shearing force such as scissors or a cutting machine, or one that utilizes a tearing force such as a cutter, a knife, or a hole punch.
[0039] The cutting method is a method of physically removing the layer including the high temperature superconducting layer 230 by scraping off the portion of the tape sheet 100 other than the closed circuit 110. Examples of the cutting method include ion milling, laser processing, mechanical (milling) processing using a diamond mill bit, electric discharge processing, and processing by water jet. It is desirable to use a method that does not generate excessive force or large thermal stress so that necessary laminated layers (for example, the high temperature superconducting layer 230 of the closed circuit 110) do not peel off during processing.
[0040] The chemical etching method is a method in which the layers including the high temperature superconducting layer 230 are removed by chemically dissolving them in the areas other than the closed circuit 110 on the tape sheet 100 .
[0041] In chemical etching, first, a masking process is performed to protect the closed circuit 110 on the tape sheet 100 from etching. A photosensitive material called photoresist is applied onto the tape sheet 100, and an exposure process is performed through a photomask on which the pattern of the closed circuit 110 is printed. For exposure, a halogen lamp, a semiconductor laser, ultraviolet light, or an electron beam can be used depending on the material of the photoresist. As a result of the exposure process, the amount of exposure irradiated to the photoresist in the part that becomes the closed circuit 110 on the tape sheet 100 and the photoresist in the part other than the closed circuit 110 on the tape sheet 100 is significantly different. The photoresist may be either negative type or positive type, and a photomask suitable for each type may be prepared. Since the solubility of the photoresist in the developer changes due to exposure, if the photoresist is immersed in the developer after the exposure process, the excess photoresist, that is, the photoresist in the part other than the closed circuit 110 on the tape sheet 100, can be removed.
[0042] With the photoresist remaining only on the portion of the closed circuit 110 on the tape sheet 100, the tape sheet 100 is subjected to an etching process. The etching may be either wet etching or dry etching. The metal cover layer 240 and the high-temperature superconducting layer 230 are removed by the etching process from the portion of the tape sheet 100 other than the closed circuit 110 where there is no photoresist. Even if the intermediate layer 220 and the base material 210 remain, they do not constitute the closed circuit 110 and therefore have no effect. As for the closed circuit 110 on the tape sheet 100, since the photoresist remains on the surface, the metal cover layer 240 and the high-temperature superconducting layer 230 are protected from etching, and as a result, they remain together with the intermediate layer 220 and the base material 210. After chemical etching, the unnecessary photoresist can be removed by a solvent.
[0043] The closed circuit 110 can be formed on the tape sheet 100 by any of the above methods.
[0044] Next, a method for producing a multi-turn coil using the tape sheet 100 will be described.
[0045] FIG. 5 is a diagram showing a procedure for producing a multi-turn coil from the tape sheet 100 of FIG.
[0046] The planar coil parts 121-123 are overlapped with each other by bending stress in the in-plane direction of the tape sheet 100. Simply overlapping the planar coil parts 121-123 is undesirable because it may cause wrinkles in the high-temperature superconducting tape sheet 100 for multi-winding coils. To prevent this, the parts in which there is no closed circuit in the high-temperature superconducting tape sheet 100 for multi-winding coils in FIG. 1 and which will become wrinkles when the planar coil parts 121-123 are overlapped are notched in advance or cut off, so that overlapping can be achieved with less wrinkles. Even after overlapping, each of the planar coil parts 121-123 forms a closed circuit 110 through the wiring part 130, and the direction of the current flowing through the planar coil parts 121-123 overlapped vertically is the same. In this way, the multi-winding coil 500 is obtained. Naturally, the multi-winding coil 500 forms a closed circuit.
[0047] FIG. 6 is a top view of another high temperature superconducting tape sheet for a multi-turn coil according to the present invention.
[0048] Another tape sheet 600 includes a plurality of planar coil parts 621-624, each of which has one turn, and a wiring part 630 that connects the plurality of planar coil parts 621-624, which together form an electrically closed circuit 610. In Fig. 6 as well, a state in which a current flows counterclockwise in the closed circuit 610 is shown, and the planar coil parts 621-624 are overlapped with each other so that the current flows in the same direction.
[0049] FIG. 7 is a diagram showing a multi-turn coil produced using the tape sheet shown in FIG.
[0050] In the multi-turn coil of Fig. 7, the tape sheet forms a three-dimensional loop by bending in a direction perpendicular to the surface of the tape sheet 600, and the planar coil portions 621-624 are overlapped so that all currents flow in the same direction to form the multi-turn coil 701. The tape sheet 600 of Fig. 6 differs from the tape sheets of Fig. 1 and Fig. 5 that utilize bending in the in-plane direction in that it utilizes bending stress in a direction perpendicular to the surface of the tape sheet, but other than that, it may be the same as the configuration described with reference to Fig. 1 and Fig. 5, and therefore description thereof will be omitted.
[0051] Next, a method for producing multiple multi-turn coils in one closed circuit will be described.
[0052] FIG. 8 is a top view of another high temperature superconducting tape sheet for a multi-turn coil according to the present invention.
[0053] Another tape sheet 800 includes a plurality of planar coil parts 821-827, each of which has one turn, and a wiring part 830 that connects the plurality of planar coil parts 821-827, which together constitute an electrically closed circuit 810. FIG. 8 also shows a state in which a current flows counterclockwise in the closed circuit 810, and the planar coil parts 821-827 are overlapped with each other so that the current flows in the same direction. More specifically, among the plurality of planar coil parts 821-827, the planar coil parts 821-823 and the planar coil parts 825-827 are overlapped with each other by bending the tape sheet 800 in the in-plane direction, so that the current flows in the same direction. In this way, by separately providing a plurality of parts in which the planar coil parts are overlapped to form a multi-turn coil, it is possible to have two or more multi-turn coils in the same closed circuit. Here, when the same closed circuit includes at least one multi-turn coil in which multiple planar coil sections are overlapped, for convenience, a planar coil section that is not overlapped, i.e., a one-turn coil such as planar coil section 824, will also be treated as a multi-turn coil.
[0054] FIG. 9 is a diagram showing a multi-turn coil made using the tape sheet of FIG.
[0055] Fig. 9 shows three multi-turn coils 901 to 903. The multi-turn coil 901 in Fig. 9 is a three-turn multi-turn coil formed by overlapping multiple planar coil portions 821 to 823, the multi-turn coil 902 is a one-turn multi-turn coil formed by planar coil portion 824, and the multi-turn coil 903 is a three-turn multi-turn coil formed by overlapping multiple planar coil portions 825 to 827, which are connected by the same closed circuit.
[0056] Naturally, it is also possible to have two or more multi-turn coils in the same closed circuit when the tape sheet is bent in a direction perpendicular to the surface of the tape sheet to form a three-dimensional loop and then overlapped, as shown in Figure 7.
[0057] A closed circuit including a multi-turn coil according to the present invention can function as a superconducting flux transformer for the purpose of transforming the strength of an applied magnetic field and transmitting it to a remote location, utilizing the conversion between magnetic field and electric current.
[0058] For example, in a superconducting flux transformer consisting of a closed circuit with at least two or more multi-turn coils, at least one of the multi-turn coils in the same closed circuit is used as an input coil that couples with a magnetic sensor, and the remaining multi-turn coils are used as pickup coils that capture signals. When a magnetic field is applied to the pickup coil, a shielding current is generated in the closed circuit to cancel the change in magnetic flux, and this shielding current creates a magnetic field in the input coil.
[0059] When it includes three or more multi-turn coils, it can provide a superconducting gradiometer, which is a type of superconducting magnetic flux transformer. In a superconducting gradiometer, two or more pickup coils are placed apart by changing the direction of the current flow so as to eliminate low-order components of the magnetic flux. When the pickup coil is a multi-turn coil, it can be divided into multiple coil sections, which allows a higher-order gradiometer structure that measures the second and third derivatives of the magnetic field change.
[0060] (Embodiment 2) In the second embodiment, a superconducting gradiometer and a superconducting magnetometer will be described as applications of a multi-turn coil made from the high-temperature superconducting tape sheet for a multi-turn coil described in the first embodiment.
[0061] FIG. 10 is a schematic diagram showing a superconducting gradiometer (magnetic gradient meter) using the multi-turn coil of the present invention.
[0062] In FIG. 10, in a closed circuit with three multi-turn coils, two of the multi-turn coils function as pickup coils 1011 and 1012, and the remaining multi-turn coil functions as an input coil 1020. When the magnetic fields detected by the pickup coils 1011 and 1012 are different, the currents flowing through the respective coils are different, and the difference in current generates a magnetic field in the input coil 1020. Therefore, the structure in FIG. 10 is a first-order superconducting gradiometer. Although not shown, a second-order or third-order superconducting gradiometer may be provided by using further multi-turn coils, i.e., by increasing the number of pickup coils and removing low-order components of the magnetic flux change. Thus, the type of magnetic field detected differs depending on the arrangement of the multi-turn coils, but in either case, a current flows through the superconducting flux transformer according to the detected magnetic field, and a magnetic field is generated in the input coil 1020.
[0063] FIG. 11 is a schematic diagram showing a superconducting magnetometer according to the present invention.
[0064] The superconducting magnetometer 1100 of the present invention includes a superconducting flux transformer 1110 and a high-temperature superconducting SQUID 1140 (also called a SQUID element). The superconducting flux transformer 1110 is made of a closed circuit including the multi-turn coil described in the first embodiment, and here includes two multi-turn coils, each of which functions as a pickup coil 1120 and an input coil 1130. The input coil 1130 of the superconducting flux transformer 1110 is coupled to the SQUID element 1140 including a Josephson junction so as to have mutual inductance. This allows the magnetic field in the pickup coil 1120 to be measured. Preferably, the inductance of the pickup coil 1120 and that of the input coil 1130 are made equal. This maximizes the transmission rate of the signal received by the SQUID element 1140 with respect to the magnetic field measured by the pickup coil 1120. The inductance of the pickup coil 1120 and the input coil 1130 can be controlled by adjusting the number of turns of the overlapping multi-turn coils, the length of the coils, and the cross-sectional area of the coils.
[0065] The superconducting magnetometer according to the present invention may be configured to include a non-cooled general-purpose magnetic sensor, for example, an MR (magnetoresistance) element including an AMR element, a TMR element, or a GMR element, an MI element, a fluxgate, or a Hall element. In that case, the input coil 1130 may be used as an input to these general-purpose magnetic sensors.
[0066] Depending on the purpose, a superconducting gradiometer may be used as a superconducting flux transformer. Since a superconducting gradiometer can be made to be unaffected by a uniform magnetic field or a certain magnetic field gradient, magnetic noise from a distant source is eliminated. Therefore, it becomes easier to detect the required signal in an ordinary room instead of a special magnetically shielded room.
[0067] The present invention will now be described in detail with reference to specific examples, but it should be noted that the present invention is not limited to these examples. EXAMPLES
[0068] [Example 1] In Example 1, a high temperature superconducting tape sheet for a multi-turn coil having four planar coil portions was manufactured.
[0069] RE1Ba2Cu3O is used as the wire material for high-temperature superconducting tape sheets. y A flat tape wire (RE=Dy, manufactured by SuperPower, USA, model number SF12050-AP) was used. The flat tape wire has a Hastelloy-C alloy tape (thickness 50 μm) as the substrate 210 (FIG. 2), on which an oxide buffer layer (material MgO, thickness 0.2 μm) that has been subjected to crystal orientation treatment is formed as the intermediate layer 220 (FIG. 2), and a REBCO layer (REBaCuO y , RE=Dy, thickness 0.5 μm), and the whole was covered with an Ag layer (thickness 2 μm) as a metal cover layer 240. The width, length and thickness of the flat tape wire were 12 mm, 50 mm and 0.06 mm, respectively.
[0070] Four planar coil parts and wiring parts were formed by cutting the flat tape wire. In detail, a diamond blade, an Ichinen Access diamond drill 28576 1.0mm, and a Niigata Seiki SK diamond internal flat φ6 #200 F6 φ2.35mm were attached to a Proxxon mini router MM100, and the pattern was formed by cutting manually. Three circular washer-shaped planar coil parts with an outer diameter D=6mm and an inner diameter d=3mm and a circular planar coil part with an outer diameter D=8mm and an inner diameter d=6mm were formed, and these were connected by wiring parts with a line width of 0.5mm. The distance between the wiring parts was 0.2mm. The appearance of the high-temperature superconducting tape sheet for multi-turn coils of Example 1 obtained in this manner is shown in FIG. 12.
[0071] FIG. 12 is a photograph of the high temperature superconducting tape sheet for a multi-turn coil of Example 1.
[0072] As shown in Fig. 12, a tape sheet was obtained in which three serially connected planar coil parts (outer diameter D = 6 mm, inner diameter d = 3 mm) and one circular planar coil part (outer diameter D = 8 mm, inner diameter d = 6 mm) were connected with wiring parts (line width 0.5 mm). According to Fig. 12, the parts that were not electrically connected were cut off to make it easier to overlap the planar coil parts.
[0073] [Example 2] In Example 2, a high temperature superconducting magnetic flux transformer was manufactured using a multi-turn coil obtained from the tape sheet obtained in Example 1.
[0074] The three series-connected planar coil parts of the tape sheet obtained in Example 1 were overlapped on each other by bending stress in the in-plane direction of the tape sheet so that the current flow direction was the same. In this way, a high-temperature superconducting flux transformer including a multi-turn coil of 3 turns and 1 turn was manufactured. Figure 12 shows the appearance of the high-temperature superconducting flux transformer of Example 2.
[0075] FIG. 13 is a photograph showing the high temperature superconducting flux transformer of the second embodiment.
[0076] As shown in Figure 13, the three-turn multi-turn coil obtained by overlapping three planar coil sections was found to be low-profile at only 0.2 mm (2 mm including the curved wiring section). In addition, the three-turn multi-turn coil and the one-turn multi-turn coil are electrically connected by wiring sections, forming a high-temperature superconducting magnetic flux transformer with the one-turn multi-turn coil as the pickup coil and the three-turn multi-turn coil as the input coil.
[0077] Next, the operation of the high-temperature superconducting flux transformer of Example 2 was confirmed. In detail, the high-temperature superconducting flux transformer of Example 2 was cooled as a whole with liquid nitrogen in a situation where there was no magnetic field around it to cause a superconducting transition, and a static magnetic field was applied to the pickup coil (a planar coil part with an inner diameter of 6 mm), and the magnetic field generated in the input coil (three overlapping planar coil parts with an inner diameter of 3 mm) was measured by a magnetic sensor. The static magnetic field was applied by placing a magnetic field application coil, which was made of an air-core bobbin with a diameter of 6 mm and a length of 14 mm and 500 turns of polyurethane-coated copper wire of Φ0.2 mm, adjacent to the pickup coil with the same central axis, and passing a constant current through it.
[0078] When constant currents of 500 mA and 1000 mA were applied to the magnetic field application coil, the magnetic fields measured by the magnetic sensor were 0.47 μT and 0.94 μT, respectively. This confirmed that the magnetic field transmitted to the input coil increased in proportion to the magnetic field applied to the pickup coil, and that the device functions as a superconducting magnetic flux transformer.
[0079] [Comparative Example 1] Without installing the superconducting flux transformer of Example 2, the magnetic field application coil and the magnetic sensor were installed in the same position, the magnetic field application coil was cooled with liquid nitrogen, a constant current was passed through it, and the generated magnetic field was measured. When constant currents of 500 mA and 1000 mA were passed through the magnetic field application coil, the magnetic fields measured by the magnetic sensor were -0.26 μT and -0.54 μT, respectively. Due to the presence of a leakage magnetic field from the magnetic field application coil, a finite magnetic field proportional to the applied magnetic field was observed by the magnetic sensor, but the value was significantly smaller than that in the case where the superconducting flux transformer of Example 2 was installed, and the sign was reversed.
[0080] A comparison between Example 2 and Comparative Example 1 showed that a large magnetic signal was transmitted by installing the superconducting flux transformer of the present invention between the magnetic field application coil and the magnetic sensor. [Industrial Applicability]
[0081] By using the high-temperature superconducting tape sheet for multi-turn coils of the present invention, it is possible to provide a multi-turn coil that operates at liquid nitrogen temperature by utilizing the functions specific to a superconducting-connected closed circuit. As a result, the multi-turn coil of the present invention can be used in a superconducting flux transformer, or a highly sensitive magnetometer system that combines a superconducting flux transformer with a magnetic sensor such as a high-temperature superconducting SQUID or MI sensor. In particular, since a multi-turn coil with a low height and small diameter can be provided, it is advantageous for probe-type magnetic microscopes with a small detection head that is limited in size. [Explanation of symbols]
[0082] 100, 600, 800 High temperature superconducting tape sheet for multi-turn coils 110, 610, 810 closed circuit 121, 122, 123, 621, 622, 623, 624, 821, 822, 823, 824, 825, 826, 827 Planar coil section 130, 630, 830 wiring section 140 Cutout 210 Base material 220 Buffer Layer 230 High-Temperature Superconducting Layer 240 Metal Cover Layer 500, 701, 901, 902, 903 Multi-turn coil 1000 Superconducting Gradiometer 1011, 1012, 1120 Pickup coil 1020, 1130 Input coil 1100 Superconducting Magnetometer 1110 Superconducting flux transformer 1140 SQUID element
Claims
1. A plurality of planar coil portions each having one turn; a wiring portion connecting each of the plurality of planar coil portions; Equipped with the plurality of planar coil portions and the wiring portion form a closed circuit, A high temperature superconducting tape sheet for a multi-turn coil, wherein at least some of the planar coil sections of the plurality of planar coil sections are overlapped with each other so that the direction of current flow is the same.
2. 2. The high temperature superconducting tape sheet for a multi-turn coil according to claim 1, wherein at least some of the planar coil portions are overlapped with each other by bending the tape sheet in an in-plane direction.
3. 3. The high temperature superconducting tape sheet for a multi-turn coil according to claim 1 or 2, wherein at least some of the planar coil portions are overlapped with each other by forming three-dimensional loops by bending in a direction perpendicular to the surface of the tape sheet.
4. 4. The high temperature superconducting tape sheet for a multi-turn coil according to claim 1, wherein the high temperature superconducting tape sheet has a width of 2 mm or more and 20 mm or less.
5. 5. The high temperature superconducting tape sheet for a multi-turn coil according to claim 1, wherein the high temperature superconducting tape sheet has a length of 50 mm or more and 1 m or less.
6. 6. The high temperature superconducting tape sheet for a multi-turn coil according to claim 1, wherein the ratio of the outer diameter of at least some of the planar coil portions to the width of the high temperature superconducting tape sheet is 0.2 or more and 1.0 or less.
7. 7. The high temperature superconducting tape sheet for a multi-turn coil according to claim 1, wherein the inner diameter of at least some of the planar coil portions is 0.1 mm or more and 10 mm or less.
8. The high temperature superconducting tape sheet for a multi-turn coil according to any one of claims 1 to 7, wherein the number of said at least some planar coils is 2 or more and 5 or less.
9. 9. The high temperature superconducting tape sheet for a multi-turn coil according to claim 1, wherein the shape of the plurality of planar coil portions is at least one selected from the group consisting of a circle, an ellipse, and a polygon.
10. The superconducting layer of the high temperature superconducting tape sheet is a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O) containing the general formula REBa a Cu 3 O b wherein RE is at least one element selected from the group consisting of yttrium (Y), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), and ytterbium (Yb), a satisfies 0<a≦2, and b satisfies 6.2≦b≦7. The high temperature superconducting tape sheet for multi-winding coils according to any one of claims 1 to 9.
11. A multi-turn coil made of high temperature superconducting tape, A multi-turn coil, wherein the high-temperature superconducting tape is the high-temperature superconducting tape sheet for a multi-turn coil according to any one of claims 1 to 10.
12. 12. The multi-turn coil according to claim 11, wherein in the high temperature superconducting tape sheet, at least some of the planar coil sections are overlapped so that the direction of current flow is the same.
13. A superconducting flux transformer comprising the multi-turn coil according to claim 11 or 12.
14. A superconducting flux transformer according to claim 13; One or more magnetic sensors selected from the group consisting of a high-temperature superconducting SQUID, an MR element including an AMR element, a TMR element, and a GMR element, an MI element, a fluxgate, and a Hall element; A superconducting magnetometer comprising:
Citation Information
Patent Citations
Magnetic flux transformer and coaxial three-diomensiona gradiometer
JP2011181559A
Annular line structure using high-temperature superconducting flat tape line material, and method of manufacturing the same
JP2013175577A