High antistatic coated floor material and coated floor

A flooring material with a room-temperature-curing epoxy resin, single-walled carbon nanotubes, and high-boiling-point solvent addresses viscosity issues in low-temperature environments, ensuring excellent finish and antistatic performance without volatile solvents.

JP2024151455APending Publication Date: 2024-10-25SUMITOMO RUBBER INDUSTRIES LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023064785
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing floor coatings with single-walled carbon nanotubes face issues with increased viscosity in low-temperature environments, leading to poor workability, air bubbles, and color separation, and require highly volatile solvents that can be hazardous.

Method used

A flooring material containing a room-temperature-curing epoxy resin, single-walled carbon nanotubes, and a solvent with a boiling point of 200°C or higher, with specific viscosity ranges and additive compositions to maintain finish quality.

Benefits of technology

The solution provides a flooring material with excellent finishability and antistatic properties in low-temperature environments without using volatile solvents, preventing air bubbles and color separation while maintaining high conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151455000001
    Figure 2024151455000001
Patent Text Reader

Abstract

To provide a coated floor material to which a single-walled carbon nanotube is added, and which has excellent finish properties even in a low-temperature environment.SOLUTION: A coated floor material contains a normal temperature curing epoxy resin, single-walled carbon nanotubes, and a solvent having a boiling point of 200°C or more, wherein the content of the single-walled carbon nanotubes is not less than 0.010 mass% and not more than 0.040 mass%, and the mixing viscosity at 10°C is not less than 1800 mPa s and not more than 3500 mPa s.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a coated floor material having improved antistatic performance. The present disclosure also relates to a coated floor including a cured coating film of the coated floor material. [Background technology]

[0002] Coated floors using curable resins such as epoxy resins are often used for floors in production facilities such as factories. However, the curable resins used in coated floors are electrically insulating, so there is a problem that static electricity can cause problems when working on the coated floors. Therefore, in order to impart antistatic properties to the coated floors, conductive fillers are added to the curable resins.

[0003] Carbon black is known as a conductive filler with high conductivity-imparting capabilities. However, carbon black colors the coating film black, which limits the range of use of the coated floor from the viewpoint of aesthetics of the coated floor. On the other hand, carbon nanotubes are also known as a conductive filler with high conductivity-imparting capabilities, and coated floors using single-walled carbon nanotubes have been developed in recent years (see, for example, Patent Documents 1 to 4). Patent Documents 1 to 3 disclose that coated floors using single-walled carbon nanotubes exhibit a 10% or less electrical conductivity at an applied voltage of 25 V. 5 Ω~10 7 It is described that the film has excellent antistatic properties, as shown by an electric resistance of Ω. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2022-35461 [Patent Document 2] Patent Publication No. 2022-35462 [Patent Document 3] JP 2022-35463 A [Patent Document 4] JP 2022-53519 A Summary of the Invention [Problem to be solved by the invention]

[0005] Generally, in the low temperature environment of winter, the viscosity of the floor coating material becomes higher than that of summer, so that the workability becomes extremely poor. Therefore, in the general method of construction in winter, a highly volatile solvent is added to the floor coating material to make it less viscous so that construction becomes easier, and the added solvent is evaporated before the floor coating material hardens so that the characteristics of the floor coating do not deteriorate. However, there are concerns about the generation of odors and adverse effects on the human body with highly volatile solvents. In addition, highly volatile solvents cannot be used at construction sites where the use of solvents is regulated.

[0006] For this reason, it is desired that the coating floor material can be applied even in a low-temperature environment without adding a highly volatile solvent. In response to this, the inventors have conducted extensive research and found that the coating floor material to which single-walled carbon nanotubes are added tends to have a greater increase in viscosity in a low-temperature environment in winter than a general coating floor material. Therefore, it has been found that when the coating floor material is applied in a low-temperature environment without adding a highly volatile solvent, air bubbles tend to remain in the coating floor after curing, and color separation tends to occur in the coating floor after curing. Therefore, it has been found that there is room for improvement in the finish of the coating floor material to which single-walled carbon nanotubes are added in a low-temperature environment.

[0007] In view of the above circumstances, an object of the present disclosure is to provide a coated floor material containing added single-walled carbon nanotubes, which has excellent finish even in low-temperature environments. [Means for solving the problem]

[0008] The present disclosure relates to a coated floor material containing a room temperature curing epoxy resin, single-walled carbon nanotubes, and a solvent having a boiling point of 200°C or higher, wherein the content of the single-walled carbon nanotubes is 0.010% by mass or more and 0.040% by mass or less, and the mixed viscosity at 10°C is 1800 mPa·s or more and 3500 mPa·s or less. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a coated floor material to which single-walled carbon nanotubes have been added, which has excellent finish even in low-temperature environments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The coated floor material of the present disclosure contains a room temperature curing epoxy resin, single-walled carbon nanotubes, and a solvent with a boiling point of 200°C or higher. The content of the single-walled carbon nanotubes in the coated floor material of the present disclosure is 0.010% by mass or more and 0.040% by mass or less. The mixed viscosity of the coated floor material of the present disclosure at 10°C is 1800 mPa·s or more and 3500 mPa·s or less. In this specification, the classification of various additives follows the usual classification in the paint field (particularly the field of paints for coated floors).

[0011] [Room temperature curing epoxy resin] The room temperature curing epoxy resin is an epoxy resin that can be cured at room temperature (for example, 0° C. to 40° C., particularly 5° C. to 35° C.), which is the temperature of the application environment. As the epoxy resin, any known epoxy resin for floor coating applications can be used, and a two-component curing type that is liquid at room temperature and cures by the reaction of an epoxy resin component with a curing agent component is preferred.

[0012] Examples of the epoxy resin component include alicyclic epoxy resins such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate; glycidyl ester type epoxy resins such as hexahydrophthalic acid diglycidyl ester; bisphenol type epoxy resins derived from bisphenols such as bisphenol A and bisphenol F and epihalohydrins; epoxidized novolac resins such as phenol novolac resin, cresol novolac resin, bisphenol A novolac resin, naphthol novolac resin, and biphenyl novolac resin; glycidyl ether type epoxy resins derived from dihydric alcohols such as hydrogenated bisphenol F, hydrogenated bisphenol A, 1,4-cyclohexanedimethanol, and alkylene oxide adducts of bisphenol A and epihalohydrins; and epoxy resins derived from polyhydric phenols such as hydroquinone and catechol and epihalohydrins. Among these, bisphenol type epoxy resins (particularly bisphenol A type epoxy resins) are preferred. These can be used alone or in combination of two or more.

[0013] As the hardener component, those known in the application of floor coating materials can be used. Specific examples thereof include aliphatic amines such as diethylenetriamine, triethylenetetramine, pentaethylenehexamine, etc., or modified products thereof; aromatic amines such as m-phenylenediamine, m-xylylenediamine, diaminodiphenylmethane, etc., or modified products thereof; alicyclic amines such as 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, etc., or modified products thereof; acid anhydrides such as phthalic anhydride, hexahydrophthalic anhydride, pyromellitic anhydride, etc.; polysulfides; acid amides; thiokol, etc. Among them, alicyclic amines, aromatic amines, and modified products thereof are preferred. Modified products include Mannich modified products, adduct modified products, etc. These can be used alone or in combination of two or more.

[0014] The mixing amount of the epoxy resin component and the curing agent component may be set so that the molar amount of the epoxy groups contained in the epoxy resin component and the molar amount of the active hydrogen contained in the curing agent component are approximately equal, as in the conventional method. When a reactive diluent is used, which will be described later, the total molar amount of the epoxy groups contained in the epoxy resin component and the epoxy groups contained in the reactive diluent may be set so that the molar amount of the active hydrogen contained in the curing agent component is approximately equal.

[0015] [Single-walled carbon nanotubes] In the present disclosure, single-walled carbon nanotubes (SWNTs) are used as the conductive filler. SWNTs have a structure in which one graphene sheet is rolled into a cylindrical shape. The single-walled carbon nanotubes may be of any of the armchair type, zigzag type, and chiral type. Since they can be easily dispersed in the floor coating material, it is preferable to use pre-dispersed single-walled carbon nanotubes, and in particular, it is preferable to use pre-dispersed single-walled carbon nanotubes in a diluent that is reactive with a room temperature curing epoxy resin. Single-walled carbon nanotubes can be synthesized according to a known method, and are also available as commercial products. A suitable example of pre-dispersed single-walled carbon nanotubes is "TUBALL MATRIX201" manufactured by OCSiAL. This "TUBALL MATRIX201" contains a fatty acid glycidyl ester as a reactive diluent. Therefore, this fatty acid glycidyl ester can react with the curing agent component together with the room temperature curing epoxy resin component.

[0016] The content of single-walled carbon nanotubes in the coating floor material is not particularly limited, but if it is too small, the conductivity will be insufficient. Therefore, the content of single-walled carbon nanotubes in the coating floor material (i.e., relative to the total mass of the coating floor material; in the case of a two-component epoxy resin that cures at room temperature, relative to the total mass of the coating floor material including the mass of the curing agent component) is 0.010% by mass or more, preferably 0.015% by mass or more, and more preferably 0.020% by mass or more. On the other hand, if the content of single-walled carbon nanotubes in the coating floor material is too high, the coating floor material will thicken and the finish will be impaired. Therefore, the content of single-walled carbon nanotubes in the coating floor material is 0.040% by mass or less, preferably 0.035% by mass or less, and more preferably 0.030% by mass or less.

[0017] [Solvents with a boiling point of 200°C or higher] As a result of intensive research, the inventors came up with the idea of ​​adding a solvent with a high boiling point to the coated floor material to adjust the viscosity of the coated floor material in order to provide a coated floor material that can be applied with good finish without adding a highly volatile solvent in low temperature environments such as winter. Therefore, the coated floor material of the present disclosure contains a solvent with a boiling point of 200°C or higher (hereinafter also referred to as a "high boiling point solvent"). The coated floor material of the present disclosure has the effect of adjusting the mixed viscosity of the coated floor material at 10°C to 1800mPa·s to 3500mPa·s.

[0018] By setting the boiling point of the high-boiling solvent to 200°C or higher, it is possible to suppress the deterioration of the finish caused by the evaporation of the solvent during the hardening of the applied floor coating material, and it is also possible to suppress the generation of an organic solvent odor.

[0019] The type and amount of the high boiling point solvent are not particularly limited as long as the mixed viscosity of the floor coating material at 10°C can be adjusted to 1800 mPa·s to 3500 mPa·s. The high boiling point solvent preferably does not have an epoxy group, and therefore functions as a non-reactive diluent. Due to its high viscosity adjustment ability, the high boiling point solvent is preferably a phenyl alkyl alcohol-based non-reactive diluent (e.g., benzyl alcohol (boiling point: 205°C), 2-phenethyl alcohol (boiling point: 220°C), etc.); phenyl xylyl ethane (boiling point: 210°C), and more preferably benzyl alcohol.

[0020] The viscosity of the high boiling point solvent at 25° C. is preferably 1.0 mPa·s or more and less than 10.0 mPa·s, and more preferably 3.0 mPa·s or more and 8.0 mPa·s or less. The viscosity can be measured using a rotational viscometer according to a known method.

[0021] If the content of the high boiling point solvent in the coating floor material is too low, the viscosity of the coating floor material will be too high, and after the coating floor material hardens, many bubbles will remain on the surface of the coating floor, which may cause the finish to be poor and the aesthetics to be impaired. On the other hand, if the content of the high boiling point solvent in the coating floor material is too high, the viscosity of the coating floor material will be too low, and after the coating floor material hardens, the coating floor may become discolored, which may cause the finish to be poor and the aesthetics to be impaired. Therefore, the content of the high boiling point solvent in the coating floor material is preferably 8.0% by mass to 12.0% by mass, more preferably 8.2% by mass to 11.5% by mass.

[0022] [Pigments] The coated floor material of the present disclosure usually contains a pigment for the purpose of adjusting the color tone, etc. However, the coated floor material may be in a form in which the product does not contain a pigment, and the pigment is added to the product at the time of use. Therefore, the coated floor material of the present disclosure may or may not contain a pigment.

[0023] As the pigment, a known pigment used in a coating floor material may be used. The pigment may be used in the form of a toner. The content of the pigment may be appropriately set according to the type of pigment and the desired color tone.

[0024] [Wetting and dispersing agent] The floor coating material of the present disclosure may contain a wetting dispersant for the purpose of improving the dispersion state of the carbon nanotubes and further improving the finish, etc. In the field of paints, the wetting dispersant is an additive that acts as a surfactant and has both the function of a wetting agent that improves the wettability of the coating film and the function of a dispersant that prevents particle aggregation by the action mechanism of electrical repulsion, steric hindrance, etc.

[0025] The wetting and dispersing agent is preferably a polymer salt containing an acid group and an amino group. By using such a wetting and dispersing agent, it is possible to more effectively prevent the aggregation of single-walled carbon nanotubes in the floor coating material, and to more effectively suppress the deterioration of the finish due to the thickening.

[0026] The acidic group is preferably an acidic phosphate group. The polymer of the polymer salt may be a homopolymer or a copolymer. The polymer is preferably a graft copolymer in which one or more side chains (e.g., polyester chains) are introduced into a main chain (e.g., polyurethane chain). In this case, the dispersibility of the single-walled carbon nanotubes is improved due to the steric hindrance of the polymer chain. As the polymer salt, alkyl ammonium salts and phosphate salts are preferred, and alkyl ammonium salts are more preferred.

[0027] The wetting dispersant preferably has an acid value and an amine value of 10 mgKOH / g or more. From the viewpoint of storage stability, the acid value and the amine value of the wetting dispersant are more preferably 30 mgKOH / g or more, and even more preferably 35 mgKOH / g or more. The acid value refers to the acid value per 1 g of polymer dispersant solid content, and can be determined, for example, by potentiometric titration in accordance with JIS K0070. The amine value refers to the amine value per 1 g of polymer dispersant solid content, and can be determined, for example, by using a 0.1 N hydrochloric acid aqueous solution and converting the value determined by potentiometric titration into the equivalent amount of potassium hydroxide.

[0028] Examples of wetting and dispersing agents that are polymer salts containing an acidic group and an amino group include "BYK-9076" and "DISPERBYK-142" manufactured by BYK Japan Co., Ltd.; and "Disparlon DA-325" manufactured by Kusumoto Chemical Industries, Ltd., with "BYK-9076" and "DISPERBYK-142" being preferred. Wetting and dispersing agents can be used alone or in combination of two or more.

[0029] The content of the wetting dispersant in the coating floor material is not particularly limited, but if it is too small, sufficient conductivity may not be obtained. In addition, the higher the content of the wetting dispersant, the higher the storage stability tends to be. Therefore, the content of the wetting dispersant in the coating floor material is preferably 0.04 mass% or more, more preferably 0.10 mass% or more. On the other hand, if the content of the wetting dispersant in the coating floor material is too high, the conductivity may decrease. Therefore, the content of the wetting dispersant in the coating floor material is preferably 0.40 mass% or less, more preferably 0.32 mass% or less, and even more preferably 0.25 mass% or less.

[0030] [Leveling Agent] The floor coating material of the present disclosure may contain a leveling agent for the purpose of further improving the finish, etc. The leveling agent may typically be compatible or oil-drop shaped in the paint, but becomes oil-drop shaped during the coating film formation process and is oriented on the coating film surface, making the evaporation of the solvent from the coating film surface uniform, preventing the formation of Benard cells, and reducing the change in surface tension to smooth the surface.

[0031] The leveling agent may be a known one used in floor coating materials. Examples of the leveling agent include acrylic polymers. The leveling agent may be the "Polyflow" series manufactured by Kyoeisha Chemical Co., Ltd. The leveling agent may be used alone or in combination of two or more types.

[0032] The content of the leveling agent in the coating floor material is not particularly limited, but if it is too small, the finish may be deteriorated. Therefore, the content of the leveling agent in the coating floor material is preferably 0.04 mass% or more, more preferably 0.06 mass% or more, and even more preferably 0.07 mass% or more. On the other hand, if the content of the leveling agent in the coating floor material is too high, the conductivity may be insufficient. Therefore, the content of the leveling agent in the coating floor material is preferably 0.21 mass% or less, more preferably 0.18 mass% or less, and even more preferably 0.15 mass% or less.

[0033] [Antifoaming agent] The coated floor material of the present disclosure may contain an antifoaming agent for the purpose of further improving the finish. The antifoaming agent may be a known agent used in coated floor materials. Examples of the antifoaming agent include acrylic polymers, vinyl ether polymers, and mixtures thereof. The antifoaming agent may be the "Florene" series manufactured by Kyoeisha Chemical Co., Ltd. The antifoaming agent may be used alone or in combination of two or more types.

[0034] The content of the defoaming agent in the coating floor material is not particularly limited, but if it is too small, the finish may be deteriorated. Therefore, the content of the defoaming agent in the coating floor material is preferably 0.12 mass% or more, more preferably 0.18 mass% or more, and even more preferably 0.24 mass% or more. On the other hand, if the content of the defoaming agent in the coating floor material is too high, the conductivity may be insufficient. Therefore, the content of the defoaming agent in the coating floor material is preferably 0.40 mass% or less, more preferably 0.38 mass% or less, and even more preferably 0.36 mass% or less.

[0035] [Other optional ingredients] The coated floor material of the present disclosure may contain an insulating filler for the purpose of improving strength, colorability, etc. As the insulating filler, a known one used in coated floor materials may be used. Examples thereof include calcium carbonate, magnesium carbonate, barium sulfate, calcium oxide, magnesium oxide, alumina, silica, kaolin, talc, mica, glass beads, glass microballoons, glass fiber, etc., and among them, calcium carbonate (particularly heavy calcium carbonate) is preferable. The content of the insulating filler may be appropriately set according to the desired strength, etc.

[0036] The coated floor material of the present disclosure may contain a surface conditioner such as an acrylic surface conditioner. In particular, when an acrylic surface conditioner that increases the surface free energy of a cured coating film is added to the coated floor material in an amount of, for example, 0.1% by mass to 3.0% by mass, the aggregation of pigments can be suppressed, and the occurrence of color separation can be further suppressed. Examples of the acrylic surface conditioner include acrylic surface conditioners in which a highly polar side chain is grafted to a low polar acrylic main chain. Specific examples of such surface conditioners include Disparlon SEI-W01 and Disparlon SEI-W02 manufactured by Kusumoto Chemical Industry Co., Ltd., and among them, Disparlon SEI-W01 is preferred.

[0037] Alternatively, when a silicone-free nonionic acrylic surface conditioner of the type that improves wettability with the object to be coated is added to the floor coating material in an amount of, for example, 0.1% by mass to 3.0% by mass, the aggregation of the pigment can be suppressed, and the occurrence of color separation can be further reduced. Examples of the acrylic surface conditioner include the "L-1980N" series (e.g., L-1980N, L-1982N, L-1983N, L-1984N) manufactured by Kusumoto Chemical Co., Ltd., and among them, L-1982N and L-1983N are preferred.

[0038] The coated floor material of the present disclosure may contain a reactive diluent, etc. As the reactive diluent, for example, a compound having an epoxy group such as neopentyl glycol diglycidyl ether or tolyl glycidyl ether can be used.

[0039] The coated floor material of the present disclosure may further contain components other than those described above, provided that the effects of the present disclosure are not significantly impaired.

[0040] [Mix viscosity] The mixed viscosity of the floor coating material of the present disclosure at 10°C is 1800mPa·s to 3500mPa·s. If the mixed viscosity is less than 1800mPa·s, color separation occurs on the coated floor after the coated floor material hardens, resulting in poor finish and impaired aesthetics. The viscosity is preferably 1900mPa·s or more, more preferably 2000mPa·s or more. On the other hand, if the mixed viscosity exceeds 3500mPa·s, many bubbles remain on the coated floor surface after the coated floor material hardens, resulting in poor finish and impaired aesthetics. The viscosity is preferably 3200mPa·s or less, more preferably 3000mPa·s or less.

[0041] The mixed viscosity is the viscosity when the floor coating material of the present disclosure is mixed, and can be measured using a B-type viscometer according to a known method. Specifically, for example, the mixed viscosity of the floor coating material at 10°C can be measured using a BH viscometer manufactured by Toki Sangyo Co., Ltd. under conditions of a temperature of 10°C and a rotation speed of 2rm. This measurement is started within 2 minutes after the completion of mixing all the components of the floor coating material, including the hardener.

[0042] The method of preparing the coated floor material of the present disclosure is not particularly limited, and it can be prepared according to a known method. For example, each component of the coated floor material of the present disclosure may be mixed at once at the construction site or the like to prepare it. For example, the coated floor material of the present disclosure may be prepared as a two-liquid type divided into a main agent containing components other than the hardener and a hardener, and the main agent and hardener are mixed and used at the construction site or the like. For example, it may be prepared as a two-liquid type, and the main agent component may be prepared without mixing an insulating filler or with a small amount of insulating filler, and the insulating filler may be added to the main agent so that the mixing amount is determined in consideration of the condition of the base and the characteristics required for the coated floor, for example, at the construction site or the like. For example, it may be prepared as a two-liquid type, and the main agent component may be prepared without mixing a colorant, and the colorant may be added to the main agent according to the color tone required for the coated floor, for example, at the construction site or the like.

[0043] The coated floor material of the present disclosure can be applied and used according to a known method. For example, the coated floor material of the present disclosure can be applied to the floor to be applied by a pouring method, and then left to stand for a predetermined time to dry and harden the epoxy resin, thereby forming a coated floor. The applied coated floor may be a single layer of the layer formed by the coated floor material of the present disclosure (i.e., a layer of the cured coating film of the coated floor material of the present disclosure), or may be a multi-layer structure combining a layer formed by the coated floor material of the present disclosure and a primer layer.

[0044] Furthermore, with the coated floor material of the present disclosure, there is no need to add highly volatile solvents, even when construction is carried out in a low-temperature environment such as winter (for example, around 10°C), and it is not necessary to add highly volatile solvents. Therefore, there is no concern about odor generation or adverse effects on the human body due to highly volatile solvents. In addition, with the coated floor material of the present disclosure, even when construction is carried out in a low-temperature environment, air bubbles are unlikely to remain in the coated floor after curing, and color separation is also unlikely to occur. The coated floor material of the present disclosure has excellent finish even in a low-temperature environment. Furthermore, the cured coating film of the coated floor material of the present disclosure exhibits high conductivity even at 25 V. In particular, the resistance at 25 V is 10 5It is also possible to achieve a conductivity of the order of Ω. Therefore, the coated floor material of the present disclosure has excellent antistatic performance (hence, it can be called a "highly antistatic coated floor material"). Therefore, the coated floor material of the present disclosure can prevent not only normal static electricity prevention, but also static electricity damage such as the destruction of electronic components (e.g., semiconductor elements) at low voltage.

[0045] Therefore, from another viewpoint, the present disclosure is a coated floor having a cured coating film of the above-mentioned coated floor material. The thickness of the cured coating film of the above-mentioned coated floor material is not particularly limited, but is, for example, 1.0 mm or more and 3.0 mm or less, preferably 1.0 mm or more and 2.0 mm or less. The coated floor may have other layers such as a primer layer.

[0046] For example, when the coated floor of the present disclosure is an antistatic floor, the coated floor may include three layers: a primer layer, a conductive primer layer, and a base coat layer. The primer layer is a layer for ensuring adhesion to the surface of a base such as concrete, and may have the same configuration as a known primer layer. The primer layer can be formed, for example, using a known epoxy resin coated floor paint for primers (e.g., "C355" (base agent) and "H355" (hardener) manufactured by Sumitomo Rubber Industries, Ltd.).

[0047] The conductive primer layer may have the same structure as a known conductive primer layer. Typically, the conductive primer layer has a thickness of, for example, 10 3 It is configured to have a conductivity of about Ω. The conductive primer layer can be formed, for example, by using a known conductive primer floor coating paint (e.g., "SL333A" (base agent) and "SL333B" (hardener) manufactured by Sumitomo Rubber Industries, Ltd.) in which carbon black is blended with epoxy resin to impart conductivity.

[0048] The base coat layer is constituted by the cured coating film of the above-mentioned floor coating material.

[0049] The coated floor of the present disclosure has a good finish even in a low-temperature environment and exhibits high conductivity even at 25 V. Therefore, electrostatic damage such as the destruction of electronic components at low voltage is prevented. The coated floor of the present disclosure can be used in various buildings, and is particularly suitable for research facilities and production facilities for electronic components (e.g., semiconductor devices). EXAMPLES

[0050] Examples of the present disclosure will be described below, but it is not intended that the present disclosure be limited to those shown in these examples.

[0051] [Examples and Comparative Examples] In an environment of 10±1°C temperature and 55±1% relative humidity, the components shown in Table 1 were mixed for 10 minutes at 1300 rpm using a stirrer to prepare the base agent (the values ​​in the table indicate parts by mass). 20 parts by mass of the curing agent shown in Table 1 were blended with 100 parts by mass of the prepared base agent, and mixed for 1 minute at 1300 rpm using a stirrer to prepare the coated floor materials of each Example and Comparative Example.

[0052] [Mix viscosity] Within 2 minutes of completing the mixing of the base agent and hardener in a 10°C environment, the floor coating materials of each Example and Comparative Example were set in a BH viscometer (manufactured by Toki Sangyo Co., Ltd.) and the viscosity (mPa s) was measured by rotating the rotor at a rotation speed of 2 rpm for 1 minute. The results are shown in Table 1.

[0053] [Evaluation of Finished State] The floor coating materials of each of the above-prepared Examples and Comparative Examples were applied to a 30 cm square flat plate in an environment of 10±1°C temperature and 55±1% relative humidity. This was left to stand in that environment for 7 days to harden, and a test sample was prepared. Fluorescent light was applied to the surface of the test sample to check the state of remaining bubbles and the occurrence of color separation. The defoaming property was evaluated according to the following criteria, with ◯ being a pass. The occurrence of color separation was also evaluated according to the following criteria, with ◯ being a pass. The evaluation results are shown in Table 1. (defoaming) ×: A lot of foam remains 〇: Almost no foam remaining (Color-coded) ×: Many color separations 〇: Almost no color separation

[0054] [Conductivity evaluation] A primer layer was formed on the substrate using epoxy primer (Sumitomo Rubber Industries, Ltd.'s C355 (base) / H355 (hardener)) in a temperature environment of 23°C. Furthermore, a conductive primer layer was formed on this primer layer using conductive primer (Sumitomo Rubber Industries, Ltd.'s SL333A (base) / SL333B (hardener)). In a temperature environment of 10°C, the floor coating materials of each of the examples and comparative examples prepared above were applied on this conductive primer layer, and cured to form a base coat layer. In this way, a test sample was prepared. The resistance of this test sample was measured using an insulation resistance meter when an applied voltage of 25V was set in accordance with the NFPA method and JIS A1454:2016. In addition, 2.25 kg iron cylinders were used as electrodes, and the distance between the electrodes was 3 feet (about 91 cm). The measurement results are shown in Table 1.

[0055] [Table 1]

[0056] Polyflow No. 85: Kyoeisha Chemical Co., Ltd.'s leveling agent "Polyflow No. 85" FLORON AC324: Defoamer "FLORON AC324" manufactured by Kyoeisha Chemical Co., Ltd. MATRIX201: OCSiAL's "TUBALL MATRIX201" (contains single-walled carbon nanotubes: fatty acid glycidyl ester (reactive diluent) in a mass ratio of 1:9) BYK-9076: Wetting and dispersing agent "BYK-9076" manufactured by BYK Japan (alkyl ammonium salt of a polymer in which a polyester chain is grafted onto a polyurethane main chain; acid value = 38 mg KOH / g, amine value = 44 mg KOH / g) H506WA: Modified polyamine-based hardener "H506WA" from Sumitomo Rubber Industries

[0057] In the coated floor materials of Examples 1 to 3, in which the mixed viscosity at 10°C was adjusted to within the range of 1800 mPa·s to 3500 mPa·s using benzyl alcohol, a solvent with a boiling point of 200°C or higher, good results were obtained in both the defoaming evaluation and the color separation evaluation. 5 High electrical conductivity on the order of Ω was obtained.

[0058] On the other hand, in Comparative Examples 1 and 2, where the mixed viscosity exceeded 3500 mPa s, a lot of residual bubbles were observed and the finish was poor. Also, in Comparative Example 3, where the mixed viscosity was less than 1800 mPa s, a lot of color separation was observed and the finish was poor.

[0059] From the above results, it can be seen that the coated floor material of the present disclosure is a coated floor material to which single-walled carbon nanotubes have been added, and can provide a coated floor material that has excellent finish even in low-temperature environments.

[0060] As described above, the present disclosure (1) is a coated floor material containing a room temperature curing epoxy resin, single-walled carbon nanotubes, and a solvent having a boiling point of 200°C or higher, wherein the content of the single-walled carbon nanotubes is 0.010% by mass or more and 0.040% by mass or less, and the mixed viscosity at 10°C is 1800 mPa·s or more and 3500 mPa·s or less.

[0061] The present disclosure (2) is the floor coating material according to the present disclosure (1), in which the content of the solvent is 8.0% by mass or more and 12.0% by mass or less.

[0062] The present disclosure (3) is the floor coating material according to the present disclosure (1) or (2), in which the solvent is a phenylalkyl alcohol-based non-reactive diluent.

[0063] The present disclosure (4) is the floor coating material according to the present disclosure (3), wherein the solvent is benzyl alcohol.

[0064] The present disclosure (5) is a coated floor having a cured coating film of the coated floor material according to any one of the present disclosures (1) to (4).

Claims

1. A floor coating material containing a room temperature curing epoxy resin, single-walled carbon nanotubes, and a solvent having a boiling point of 200°C or higher, The content of the single-walled carbon nanotubes is 0.010% by mass or more and 0.040% by mass or less, The mixed viscosity at 10°C is 1800 mPa·s or more and 3500 mPa·s or less. Painted flooring.

2. The floor coating material according to claim 1, wherein the content of the solvent is 8.0% by mass or more and 12.0% by mass or less.

3. The floor coating material according to claim 1, wherein the solvent is a phenyl alkyl alcohol-based non-reactive diluent.

4. The floor coating material according to claim 3, wherein the solvent is benzyl alcohol.

5. A coated floor comprising a cured coating film of the coated floor material according to claim 1.

Citation Information

Patent Citations

  • Highly antistatic coated flooring and coated floor

    JP2022035461A

  • Method of constructing antistatic non-slip floor

    JP2022035462A

  • Highly antistatic coated flooring and coated floor

    JP2022035463A

  • Conductive floor coating material composition, construction method thereof, and conductive coated floor

    JP2022053519A