Surface-modified polyimide porous membrane, and method for producing surface-modified polyimide

A surface-modified polyimide porous membrane with a graft chain and specific surface properties achieves effective metal ion capture by addressing the limitations of existing methods, ensuring good metal removability and minimizing surface damage.

JP2024151472APending Publication Date: 2024-10-25TOKYO OHKA KOGYO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023064824
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing methods for imparting metal removability to porous materials, such as those described in Patent Document 1, are insufficient as they fail to effectively reach the surface of the pores due to viscosity and wettability issues, leading to inadequate metal adsorption properties.

Method used

A surface-modified polyimide porous membrane is developed with a graft chain having a metal-adsorbing functional group, a contact angle of 20° or less, and a surface roughness Rz of 500 nm or less, achieved through plasma graft polymerization using gases with lower molecular weights than argon, followed by contact with a monomer having a metal-adsorbing functional group.

Benefits of technology

The surface-modified polyimide porous membrane exhibits excellent metal removability, effectively capturing a wide range of metal ions while minimizing surface damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151472000005
    Figure 2024151472000005
  • Figure 2024151472000006
    Figure 2024151472000006
  • Figure 2024151472000007
    Figure 2024151472000007
Patent Text Reader

Abstract

To provide a surface-modified polyimide porous membrane exhibiting excellent metal removability, and a method for producing the surface-modified polyimide.SOLUTION: A surface-modified polyimide porous membrane having a graft chain having a metal adsorbing functional group on a surface and having a contact angle of 20° or less and a surface roughness Rz of 500 nm or less is used. Further, a surface-modified polyimide is produced by a method comprising (a) a step of performing plasma treatment on at least a part of the surface of the polyimide using a gas of a molecule having a lower molecular weight than argon, and (b) a step of contacting plasma-treated polyimide with a monomer having a metal adsorbing functional group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface-modified polyimide porous film and a method for producing a surface-modified polyimide. [Background technology]

[0002] Conventionally, various materials have been studied for removing metal ions from liquids containing metal ions. For example, Patent Document 1 proposes a metal ion adsorbent in which a resin having a specific functional group is physically attached to the surface of a substrate. It has also been confirmed that nylon has a certain degree of metal adsorption. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-159039 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in Patent Document 1, the substrate surface is treated with a resin solution to impart metal-removing properties to the substrate. However, when the substrate is a porous material, the method described in Patent Document 1 makes it difficult to impart sufficient metal-removing properties to the surfaces of the pores of the substrate, depending on the viscosity of the resin solution and the wettability of the resin solution with the substrate. Therefore, the present inventors have investigated the possibility of performing plasma graft polymerization on polyimide to chemically bond molecules having metal-adsorbing functional groups. This is because plasma gas and graft monomers or solutions of graft monomers, which generally have low viscosity, tend to easily penetrate into the pores of porous materials. However, this method also has the problem that it is difficult to obtain polyimide with excellent metal adsorption.

[0005] The present invention has been made in view of the above problems, and has an object to provide a surface-modified polyimide porous film that exhibits good metal removability, and a method for producing a surface-modified polyimide. [Means for solving the problem]

[0006] In order to solve the above problems, the present inventors conducted extensive research and found that the above problems can be solved by a surface-modified polyimide porous film having graft chains with metal-adsorbing functional groups on its surface and having a predetermined contact angle and a predetermined surface roughness Rz, thereby completing the present invention. Specifically, the present invention provides the following.

[0007] [1] A surface-modified polyimide porous film comprising a porous polyimide and a graft chain formed on at least a part of a surface of the porous polyimide, the graft chain has a metal-adsorbing functional group, the contact angle of the surface of the polyimide porous film is 20° or less; The surface-modified polyimide porous film has a surface roughness Rz of 500 nm or less.

[0008] [2] The metal-adsorbing functional group is a sulfo group, -NR 1 R 2 (R 1 and R 2 each independently represents a hydrogen atom or an alkyl group), a hydroxy group, a carboxy group, -N + R 3 R 4 R 5 (R 3 , R 4 , and R 5 each independently represents a hydrogen atom or an alkyl group), and a phosphoryl group.

[0009] [3] The surface-modified polyimide porous film according to [1] or [2], having a sulfur element ratio of 1 atm % or more as determined by X-ray photoelectron spectroscopy.

[0010] [4] (a) performing a plasma treatment on at least a portion of a surface of the polyimide using a gas having a molecular weight lower than that of argon; (b) contacting the plasma-treated polyimide with a monomer having a metal-adsorbing functional group.

[0011] [5] The method according to [4], wherein the polyimide is a porous polyimide.

[0012] [6] The manufacturing method according to [4] or [5], wherein the gas comprises at least one selected from the group consisting of helium gas, oxygen gas, and nitrogen gas.

[0013] [7] The method according to any one of [4] to [6], wherein the RF power of the plasma treatment is 100 W or more. Effect of the Invention

[0014] According to the present invention, it is possible to provide a surface-modified polyimide porous film exhibiting good metal removability, and a method for producing a surface-modified polyimide. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a SEM image of the porous membrane obtained in Example 1. [Diagram 2] FIG. 2 is a SEM image of the porous membrane obtained in Comparative Example 1. [Diagram 3] FIG. 1 is a SEM image of the porous membrane obtained in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The following describes in detail the embodiments of the present invention. However, the present invention is not limited to the following embodiments and can be implemented with appropriate modifications within the scope of the object of the present invention.

[0017] <Surface-modified polyimide porous film> The surface-modified polyimide porous film includes a porous polyimide and a graft chain formed on at least a part of the surface of the porous polyimide. The graft chain has a metal-adsorbing functional group. The surface of the surface-modified polyimide porous film has a contact angle of 20° or less and a surface roughness Rz of 500 nm or less. Hereinafter, the surface-modified polyimide porous film is also simply referred to as a "porous film." Such a surface-modified polyimide porous film exhibits good metal removal properties.

[0018] The type, valence, etc. of metal ions that can be removed by the surface-modified polyimide porous film are not particularly limited. Examples of metal ions include lithium ions, sodium ions, magnesium ions, aluminum ions, potassium ions, calcium ions, titanium ions, vanadium ions, chromium ions, manganese ions, iron ions, cobalt ions, nickel ions, copper ions, zinc ions, silver ions, arsenic ions, strontium ions, zirconium ions, cadmium ions, tin ions, barium ions, and lead ions.

[0019] The contact angle of the surface of the porous film is 20° or less, and preferably 10° or less. There is no particular lower limit to the contact angle. By making the contact angle 20° or less, excellent metal removal properties are easily obtained. In this specification, the contact angle is a value measured by the method described in the Examples section below.

[0020] The surface roughness Rz (maximum height roughness) of the porous film is 500 nm or less, preferably 400 nm or less, more preferably 300 nm or less. The lower limit of the surface roughness Rz is not particularly limited, but is, for example, 50 nm or more. By being 500 nm or less, the metal removal property of the porous film is good. The surface roughness Ra of the porous film is preferably 200 nm or less, more preferably 100 nm or less, and even more preferably 50 nm or less. The lower limit of the surface roughness Ra is not particularly limited, but is, for example, 10 nm or more. When it is 200 nm or less, the metal removal property of the porous film is good. In this specification, the surface roughnesses Rz and Ra are values ​​measured by the method described in the Examples section below.

[0021] The sulfur element ratio on the surface of the porous film determined by X-ray photoelectron spectroscopy (XPS) is preferably 0.5 atm% or more, more preferably 1 atm% or more. The upper limit of the sulfur element ratio is not particularly limited, but is, for example, 0.25 atm% or less. When it is 0.5 atm% or more, excellent metal removal properties are easily obtained. In this specification, the sulfur element ratio is a value measured by the method described in the Examples below.

[0022] The thickness of the porous membrane is not particularly limited and is appropriately determined depending on the application. Typically, the thickness of the porous membrane is preferably 20 μm or more, more preferably 20 μm or more and 200 μm or less, and even more preferably 30 μm or more and 100 μm or less.

[0023] <Porous polyimide> The porous polyimide is a porous material made of a polyimide resin or a polyimide resin composition containing a polyimide resin. The shape of the pores in the porous material is not particularly limited as long as the porous membrane allows fluid to flow from one main surface to the other main surface. The porous materials constituting the porous polyimide each have a desired porosity, and as described below, preferably have a structure in which spherical pores are interconnected (hereinafter, abbreviated as interconnected pores). The spherical shape of the hole includes a perfect sphere, but is not limited to a perfect sphere. The spherical shape may be substantially a perfect sphere, and includes a shape that can be recognized as a nearly perfect sphere when a magnified image of the hole is visually observed. Specifically, in the case of a spherical hole, the surface that defines the hole portion is a curved surface, and the curved surface may define a hole that is perfectly spherical or approximately perfectly spherical.

[0024] For example, in the case of porous polyimide, the individual spherical pores are typically formed by removing individual particles present in the polyimide resin-particle composite film described below in a subsequent process. In the method for producing a porous polyimide, the communicating pores are formed by removing a plurality of particles that are in contact with each other in the polyimide resin-particle composite film in a later step. The points where the spherical pores communicate with each other in the communicating pores are derived from the points where the plurality of particles before being removed contact each other.

[0025] The diameter of the openings of the porous polyimide is preferably 50 nm or more and 3000 nm or less, more preferably 100 nm or more and 2000 nm or less, and even more preferably 200 nm or more and 1000 nm or less, in terms of achieving both an excellent fluid passage speed and the strength of the porous polyimide. The diameter of the opening is equal to or approximately equal to the diameter of the spherical hole that constitutes the communicating hole. The porous polyimide has internal communicating pores that pass through the porous film in the thickness direction and serve as fluid flow paths, allowing the fluid to permeate from one main surface of the porous film to the other main surface. In addition, when the porous membrane is used as a filter, the fluid passes through the inside of the porous membrane while contacting the curved surface that defines each spherical hole. The contact area of ​​the fluid inside the porous membrane is quite large due to the presence of communicating holes made of spherical holes. Therefore, when the fluid passes through a laminate including the porous membrane, it is considered that minute substances present in the fluid are easily adsorbed by the spherical holes in the porous membrane.

[0026] The porosity of the porous polyimide is preferably 60% or more, more preferably 65% ​​or more and 85% or less, and even more preferably 70% or more and 80% or less, from the viewpoint of excellent fluid passage speed.

[0027] The porosity indicates, for example, the ratio of voids per unit volume of a porous polyimide, and can be calculated by the following formula (A). Porosity (%) = {volume of specimen (cm 3 )-[Weight of test piece (g) / Specific gravity of polyimide resin or polyimide resin composition (g / cm3 )]} / volume of test piece (cm 3 )×100···(A) As will be described later, the porosity can be adjusted to a desired value by appropriately adjusting the particle size and content of the fine particles used in producing the porous polyimide.

[0028] [Method of manufacturing porous polyimide] A preferred porous polyimide having therein communicating pores in which spherical pores communicate with each other can be produced, for example, by the following method.

[0029] in particular, a step of forming an unsintered composite film on a substrate using the composition for producing a porous polyimide; a firing step of firing the unfired composite film to obtain a polyimide resin-particle composite film; and a particle removing step of removing the particles from the polyimide resin-particle composite film.

[0030] The composition for producing a porous polyimide will be described in detail below.

[0031] [Composition for producing porous polyimide] The composition for producing a porous polyimide contains a compound capable of producing a polyimide resin. The compound capable of producing a polyimide resin may be a monomer for forming a polyimide resin, or may be a polyamic acid which is a precursor of a polyimide resin. The compound capable of producing a polyimide resin is preferably a polyamic acid.

[0032] The essential and optional components contained in the composition for producing a porous polyimide will be described below.

[0033] (Polyamic acid) As the polyamic acid, a resin obtained by polymerizing any tetracarboxylic dianhydride and diamine can be used without any particular limitation. The amount of the tetracarboxylic dianhydride and the diamine used is not particularly limited. The amount of the diamine used per mole of the tetracarboxylic dianhydride is preferably 0.50 moles or more and 1.50 moles or less, more preferably 0.60 moles or more and 1.30 moles or less, and particularly preferably 0.70 moles or more and 1.20 moles or less.

[0034] The tetracarboxylic dianhydride can be appropriately selected from tetracarboxylic dianhydrides that have been used as a synthetic raw material for polyamic acid. The tetracarboxylic dianhydride may be an aromatic tetracarboxylic dianhydride or an aliphatic tetracarboxylic dianhydride. From the viewpoint of the heat resistance of the resulting polyimide resin, it is preferable to use an aromatic tetracarboxylic dianhydride. The tetracarboxylic dianhydride may be used alone or in combination of two or more.

[0035] Specific examples of suitable aromatic tetracarboxylic dianhydrides include pyromellitic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 2,3,3',4'-biphenyl tetracarboxylic dianhydride, 2,2,6,6-biphenyl tetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, phenyl) ether dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 4,4-(p-phenylenedioxy) diphthalic dianhydride, 4,4-(m-phenylenedioxy) diphthalic dianhydride, 1,2,5,6-naphthalene tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 1,2,3,4-benzene tetracarboxylic dianhydride, 3,4,9,10-perylene tetracarboxylic dianhydride, 2,3,6,7-anthracene tetracarboxylic dianhydride, 1,2,7,8-phenanthrene tetracarboxylic dianhydride, 9,9-bisphthalic anhydride fluorene, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, and the like. Examples of the aliphatic tetracarboxylic dianhydride include ethylene tetracarboxylic dianhydride, butane tetracarboxylic dianhydride, cyclopentane tetracarboxylic dianhydride, cyclohexane tetracarboxylic dianhydride, 1,2,4,5-cyclohexane tetracarboxylic dianhydride, and 1,2,3,4-cyclohexane tetracarboxylic dianhydride. Among these, 3,3',4,4'-biphenyl tetracarboxylic dianhydride and pyromellitic dianhydride are preferred in terms of price, availability, and the like. These tetracarboxylic dianhydrides can be used alone or in combination of two or more.

[0036] The diamine can be appropriately selected from diamines that have been used as a synthetic raw material for polyamic acid. The diamine can be an aromatic diamine or an aliphatic diamine, but from the viewpoint of the heat resistance of the resulting polyimide resin, an aromatic diamine is preferable. These diamines can be used alone or in combination of two or more.

[0037] Examples of aromatic diamines include diamino compounds having one or 2 to 10 phenyl groups bonded thereto, specifically phenylenediamine and its derivatives, diaminobiphenyl compounds and their derivatives, diaminodiphenyl compounds and their derivatives, diaminotriphenyl compounds and their derivatives, diaminonaphthalene and its derivatives, aminophenylaminoindan and its derivatives, diaminotetraphenyl compounds and their derivatives, diaminohexaphenyl compounds and their derivatives, and cardo-type fluorenediamine derivatives.

[0038] The phenylenediamines include m-phenylenediamine, p-phenylenediamine, etc., and the phenylenediamine derivatives include diamines to which an alkyl group such as a methyl group or an ethyl group is bonded, such as 2,4-diaminotoluene and 2,4-triphenylenediamine.

[0039] Diaminobiphenyl compounds have two aminophenyl groups bonded together, such as 4,4'-diaminobiphenyl.

[0040] A diaminodiphenyl compound is a compound in which two aminophenyl groups are bonded to each other via another group. The bond may be an ether bond, a sulfonyl bond, a thioether bond, a bond by an alkylene or its derivative group, an imino bond, an azo bond, a phosphine oxide bond, an amide bond, a ureylene bond, or the like. The number of carbon atoms in the alkylene bond is about 1 to 6, and the derivative group of the alkylene group is an alkylene group substituted with one or more halogen atoms, or the like.

[0041] Examples of the diaminodiphenyl compound include 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl methane, 3,4'-diaminodiphenyl methane, 4,4'-diaminodiphenyl methane, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl ketone, 3,4'-diaminodiphenyl ketone, 2,2-bis(p-aminophenyl)propane, 4-methyl-2,4-bis(p-aminophenyl)-1-pentene, 4-methyl-2,4-bis(p-aminophenyl)propane ... p-aminophenyl)-2-pentene, iminodianiline, 4-methyl-2,4-bis(p-aminophenyl)pentane, bis(p-aminophenyl)phosphine oxide, 4,4'-diaminoazobenzene, 4,4'-diaminodiphenylurea, 4,4'-diaminodiphenylamide, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and the like.

[0042] Among these, p-phenylenediamine, m-phenylenediamine, 2,4-diaminotoluene, and 4,4'-diaminodiphenyl ether are preferred in view of cost, availability, and the like.

[0043] A diaminotriphenyl compound is a compound in which two aminophenyl groups and one phenylene group are bonded via other groups. The other groups are selected from the same groups as those of the diaminodiphenyl compound. Examples of the diaminotriphenyl compound include 1,3-bis(m-aminophenoxy)benzene, 1,3-bis(p-aminophenoxy)benzene, and 1,4-bis(p-aminophenoxy)benzene.

[0044] Examples of diaminonaphthalenes include 1,5-diaminonaphthalene and 2,6-diaminonaphthalene.

[0045] Examples of aminophenylaminoindanes include 5 or 6-amino-1-(p-aminophenyl)-1,3,3-trimethylindan.

[0046] Examples of diaminotetraphenyl compounds include 4,4'-bis(p-aminophenoxy)biphenyl, 2,2'-bis[p-(p'-aminophenoxy)phenyl]propane, 2,2'-bis[p-(p'-aminophenoxy)biphenyl]propane, and 2,2'-bis[p-(m-aminophenoxy)phenyl]benzophenone.

[0047] Examples of the cardo-type fluorenediamine derivatives include 9,9-bisanilinefluorene.

[0048] The number of carbon atoms of the aliphatic diamine is, for example, about 2 to 15. Specific examples of the aliphatic diamine include pentamethylene diamine, hexamethylene diamine, and heptamethylene diamine.

[0049] The diamine may be a compound in which a hydrogen atom of the diamine is substituted with at least one substituent selected from the group consisting of a halogen atom, a methyl group, a methoxy group, a cyano group, a phenyl group, and the like.

[0050] There is no particular limitation on the means for producing the polyamic acid, and for example, a known method such as a method of reacting an acid and a diamine component in a solvent can be used.

[0051] The reaction between the tetracarboxylic dianhydride and the diamine is usually carried out in a solvent. The solvent used in the reaction between the tetracarboxylic dianhydride and the diamine is not particularly limited as long as it can dissolve the tetracarboxylic dianhydride and the diamine and does not react with the tetracarboxylic dianhydride and the diamine. The solvent may be used alone or in combination of two or more.

[0052] Examples of the solvent used in the reaction between the tetracarboxylic dianhydride and the diamine include nitrogen-containing polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dimethylformamide, N,N-diethylformamide, N-methylcaprolactam, and N,N,N',N'-tetramethylurea; lactone-based polar solvents such as β-propiolactone, γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, and ε-caprolactone; dimethyl sulfoxide; acetonitrile; fatty acid esters such as ethyl lactate and butyl lactate; ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dioxane, tetrahydrofuran, methyl cellosolve acetate, and ethyl cellosolve acetate; and phenol-based solvents such as cresols and xylene-based mixed solvents. These solvents may be used alone or in combination of two or more. There is no particular restriction on the amount of the solvent used, but it is desirable that the content of the produced polyamic acid be 5 to 50 mass %.

[0053] Among these solvents, nitrogen-containing polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-diethylacetamide, N,N-dimethylformamide, N,N-diethylformamide, N-methylcaprolactam, and N,N,N',N'-tetramethylurea are preferred from the viewpoint of the solubility of the produced polyamic acid.

[0054] The polymerization temperature is generally from −10° C. to 120° C., preferably from 5° C. to 30° C. The polymerization time varies depending on the composition of the raw materials used, but is usually from 3 hours to 24 hours. The polyamic acid may be used alone or in combination of two or more kinds.

[0055] (Polyimide resin) The polyimide resin is not limited in structure or molecular weight, and any known polyimide resin can be used. The polyimide may have a condensable functional group such as a carboxyl group or a functional group that promotes a crosslinking reaction during baking in the side chain. In addition, when the composition for producing a porous polyimide contains a solvent, a soluble polyimide that can be dissolved in the solvent used is preferable.

[0056] In order to make the polyimide resin soluble in a solvent, it is effective to use a monomer for introducing a flexible, bent structure into the main chain, for example, an aliphatic diamine such as ethylenediamine, hexamethylenediamine, 1,4-diaminocyclohexane, 1,3-diaminocyclohexane, or 4,4'-diaminodicyclohexylmethane; an aromatic diamine such as 2-methyl-1,4-phenylenediamine, o-tolidine, m-tolidine, 3,3'-dimethoxybenzidine, or 4,4'-diaminobenzanilide; a polyoxyalkylene diamine such as polyoxyethylenediamine, polyoxypropylenediamine, or polyoxybutylenediamine; a polysiloxane diamine; 2,3,3',4'-oxydiphthalic anhydride, 3,4,3',4'-oxydiphthalic anhydride, or 2,2-bis(4-hydroxyphenyl)propanedibenzoate-3,3',4,4'-tetracarboxylic dianhydride; or the like. Furthermore, in addition to the monomer for improving the solubility of the polyimide resin, the same monomer as the monomer described in the polyamic acid column above can also be used in combination, provided that the solubility is not impaired. The polyimide resin and the monomer thereof may each be used alone or in combination of two or more kinds.

[0057] There is no particular limitation on the means for producing the polyimide resin, and for example, known methods such as chemical imidization or thermal imidization of polyamic acid can be used. Examples of such polyimide resins include aliphatic polyimide resins (all aliphatic polyimide resins) and aromatic polyimide resins, and aromatic polyimide resins are preferred. Examples of aromatic polyimide resins include polyimides obtained by subjecting polyamic acid having a repeating unit represented by formula (1) to a ring-closing reaction by thermal or chemical means, or polyimides having a repeating unit represented by formula (2). In the formula, Ar represents an aryl group. When the composition for producing porous polyimide contains a solvent, these polyimide resins are then preferably dissolved in the solvent used. [ka] [ka]

[0058] (fine particles) The material of the microparticles is not particularly limited and any known material can be used as long as it is insoluble in the solvent contained in the porous polyimide manufacturing composition and can be removed from the polyimide resin-microparticle composite film later. For example, inorganic materials include metal oxides such as silica (silicon dioxide), titanium oxide, and alumina (Al2O3), and organic materials include organic polymer microparticles such as high molecular weight olefins (polypropylene, polyethylene, etc.), polystyrene, epoxy resins, cellulose, polyvinyl alcohol, polyvinyl butyral, polyester, and polyether.

[0059] Specifically, the fine particles include, for example, colloidal silica. Among them, it is preferable to select monodispersed spherical silica particles because they can form uniform pores.

[0060] In addition, it is preferable that the fine particles have a high sphericity and a small particle size distribution index. Fine particles that satisfy these conditions have excellent dispersibility in the composition for producing porous polyimide and can be used in a state where they do not aggregate with each other. The average particle size of the fine particles used is appropriately selected taking into consideration the opening size on the surface of the porous polyimide and the film thickness of the porous film. The average particle size of the fine particles is, for example, preferably 50 nm or more, more preferably 100 nm or more and 2000 nm or less, and even more preferably 200 nm or more and 1000 nm or less. By satisfying these conditions, the pore size of the porous polyimide obtained by removing the fine particles can be made uniform. The fine particles may be used alone or in combination of two or more kinds.

[0061] (solvent) The solvent is not particularly limited as long as it dissolves polyamic acid and / or polyimide resin and does not dissolve fine particles. Suitable examples of the solvent include the solvents exemplified for the reaction between tetracarboxylic dianhydride and diamine. The solvent may be used alone or in combination of two or more.

[0062] (Dispersant) In order to uniformly disperse the fine particles in the porous polyimide producing composition, a dispersant may be added together with the fine particles. By adding a dispersant, the fine particles can be mixed more uniformly in the porous polyimide producing composition, and the fine particles can be uniformly distributed in the film formed from the porous polyimide producing composition. As a result, dense openings can be provided on the surface of the finally obtained porous polyimide, and the front and back surfaces can be efficiently connected, improving the air permeability of the porous film. Furthermore, by adding a dispersant, the drying property of the porous polyimide producing composition is easily improved, and the peelability of the formed unfired composite film from the substrate or the like is easily improved.

[0063] The dispersant is not particularly limited, and known dispersants can be used. For example, anionic surfactants such as coconut fatty acid salts, castor sulfate oil salts, lauryl sulfate salts, polyoxyalkylene allyl phenyl ether sulfate salts, alkylbenzene sulfonic acid, alkylbenzene sulfonate salts, alkyl diphenyl ether disulfonate salts, alkyl naphthalene sulfonate salts, dialkyl sulfosuccinate salts, isopropyl phosphate, polyoxyethylene alkyl ether phosphate salts, and polyoxyethylene allyl phenyl ether phosphate salts; cationic surfactants such as oleylamine acetate, lauryl pyridinium chloride, cetyl pyridinium chloride, lauryl trimethyl ammonium chloride, stearyl trimethyl ammonium chloride, behenyl trimethyl ammonium chloride, and didecyl dimethyl ammonium chloride; amphoteric surfactants such as coconut alkyl dimethyl amine oxide, fatty acid amidopropyl dimethyl amine oxide, alkyl polyaminoethyl glycine hydrochloride, amido betaine type surfactants, alanine type surfactants, and lauryl imino dipropionic acid; Nonionic surfactants of polyoxyalkylene primary alkyl ethers or polyoxyalkylene secondary alkyl ethers, such as ethylene octyl ether, polyoxyethylene decyl ether, polyoxyethylene lauryl ether, polyoxyethylene laurylamine, polyoxyethylene oleylamine, polyoxyethylene polystyrylphenyl ether, and polyoxyalkylene polystyrylphenyl ether; other polyoxyalkylene-based nonionic surfactants, such as polyoxyethylene dilaurate, polyoxyethylene laurate, polyoxyethylenated castor oil, polyoxyethylenated hydrogenated castor oil, sorbitan laurate, polyoxyethylene sorbitan laurate, and fatty acid diethanolamide; fatty acid alkyl esters, such as octyl stearate and trimethylolpropane tridecanoate; and polyether polyols, such as polyoxyalkylene butyl ether, polyoxyalkylene oleyl ether, and trimethylolpropane tris(polyoxyalkylene)ether, but are not limited to these.The above dispersants can also be used in combination of two or more.

[0064] In the composition for producing a porous polyimide, the content of the dispersant is, for example, from the viewpoint of film-forming properties, preferably from 0.01% by mass to 5% by mass, more preferably from 0.05% by mass to 1% by mass, and even more preferably from 0.1% by mass to 0.5% by mass, relative to the mass of the microparticles.

[0065] <Graft chain> The graft chains are formed on at least a part of the surface of the porous polyimide. In other words, molecules different from the porous polyimide are chemically bonded to at least a part of the surface. The surface of the porous polyimide includes the surfaces of the pores.

[0066] The grafted chains have metal-adsorbing functional groups. The metal-adsorbing functional group is not particularly limited as long as it is a functional group that has been conventionally known to exhibit metal adsorption, and examples of such functional groups include sulfo groups, -NR 1 R 2 (R 1 and R 2 each independently represents a hydrogen atom or an alkyl group), a hydroxy group, a carboxy group, -N + R 3 R 4 R 5 (R 3 , R 4 , and R 5 each independently represents a hydrogen atom or an alkyl group), a phosphoryl group, a boronyl group, an imidazolium group, a pyridinyl group, a thiol group, a nitrile group, and other ion exchange groups. Among these, sulfo groups, -NR 1 R 2 Groups represented by the formula: hydroxyl group, carboxyl group, -N + R 3 R 4 R 5 and a phosphoryl group, and a sulfo group is more preferable.

[0067] R 1 ~R 5 In the formula, the alkyl group may be linear or branched, but is preferably a linear alkyl group. The number of carbon atoms in the alkyl group is preferably 1 to 10, more preferably 1 to 4. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a sec-pentyl group, a tert-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group.

[0068] Examples of monomers capable of forming graft chains having a metal-adsorbing functional group include monomers having a radical polymerizable group and a metal-adsorbing functional group. The radical polymerizable group typically includes an ethylenically unsaturated double bond group, preferably a vinyl group or an alkenyl group such as an allyl group, more preferably a (meth)acryloyl group. Specific examples of the monomer include sulfo group-containing monomers such as 2-(meth)acrylamido-2-methylpropanesulfonic acid, styrenesulfonic acid, 2-methyl-2-propene-1-sulfonic acid, vinylsulfonic acid, and 3-((meth)acryloyloxy)propane-1-sulfonic acid; -NR monomers such as (meth)acrylamide, 2-(dimethylamino)ethyl (meth)acrylate, 2-aminoethyl (meth)acrylate, N-(2-aminoethyl)(meth)acrylamide, and N-(3-aminopropyl)(meth)acrylamide; 1 R 2hydroxyl group-containing monomers such as N-(2-hydroxyethyl)(meth)acrylamide, N-(hydroxymethyl)(meth)acrylamide, and dopamine(meth)acrylamide; carboxyl group-containing monomers such as 6-(meth)acrylamidohexanoic acid, (meth)acrylic acid, and 2-carboxyethyl (meth)acrylate; -N group-containing monomers such as 3-((meth)acrylamidopropyl)trimethylammonium chloride, [2-((meth)acryloyloxy)ethyl]trimethylammonium chloride, and (vinylbenzyl)trimethylammonium chloride. + R 3 R 4 R 5 Examples of the monomer include a monomer containing a group represented by the following formula: embedded image phosphoryl group-containing monomers such as 11-phosphonoundecyl(meth)acrylate and vinylphosphonic acid; and salts thereof.

[0069] The graft chain may contain a structural unit derived from a monomer other than the monomer having a radical polymerizable group and a metal-adsorbing functional group.

[0070] The grafting method may be, for example, the method described in the below-mentioned method for producing a surface-modified polyimide.

[0071] <Application> The porous membrane can be processed into various filters and can be applied to, for example, the adsorption and recovery of metal ions dissolved in liquids. Specifically, for example, various metal ions contained in pure water used in semiconductor manufacturing are captured by the porous membrane.

[0072] <Method for producing surface-modified polyimide> The method for producing a surface-modified polyimide includes the steps of (a) performing a plasma treatment on at least a portion of a surface of the polyimide using a gas having a molecular weight lower than that of argon, and (b) contacting the plasma-treated polyimide with a monomer having a metal-adsorbing functional group.

[0073] <Process (a)> In step (a), a plasma treatment is performed on at least a part of the surface of the polyimide using a gas with a molecular weight lower than that of argon, which generates radicals on the surface of the polyimide, allowing graft polymerization to proceed in the next step (b). Furthermore, by carrying out the plasma treatment in this manner, damage to the surface of the polyimide is suppressed.

[0074] As the polyimide, particles such as powder, beads, and pellets, composite fibers such as tubes, monofilaments, and twisted yarns, and porous materials are preferred, and porous materials (porous polyimide) are more preferred. When used as a material having metal removal properties, a membrane made of a porous material (polyimide porous membrane) is even more preferred because it is easy to handle and has a large contact area with a liquid containing metal ions.

[0075] The plasma treatment can be carried out by a conventional method, except that a gas having a molecular weight lower than that of argon is used. When the polyimide is in the form of a film, both sides of the polyimide film may be plasma-treated, or only one side of the polyimide film may be plasma-treated.

[0076] Examples of gases having molecules with lower molecular weights than argon include helium gas, oxygen gas, nitrogen gas, neon gas, hydrogen gas, etc. Among these, helium, oxygen, and nitrogen are preferred, and helium is more preferred, since they tend to exhibit particularly good metal adsorption properties and damage suppression.

[0077] The time for plasma irradiation of polyimide is not particularly limited as long as the desired performance is obtained, but is preferably 10 seconds or more, more preferably 30 seconds or more, and also preferably 20 minutes or less, more preferably 10 minutes or less. The RF power is preferably 100 W or more, more preferably 300 W or more, and even more preferably 400 W or more, and is preferably 2000 W or less, more preferably 1000 W or less, and even more preferably 600 W or less, from the viewpoint that the effect of the present invention is easily exerted since damage is easily caused. The pressure in the processing chamber is preferably 1 Pa or more, and preferably 15 Pa or less.

[0078] <Process (b)> In step (b), the plasma-treated polyimide is brought into contact with a monomer having a metal-adsorbing functional group, which causes graft polymerization to proceed, producing a polyimide having graft chains formed on at least a portion of its surface.

[0079] As the monomer having a metal-adsorbing functional group, the compounds exemplified as the monomer capable of forming a graft chain having a metal-adsorbing functional group in the above-mentioned surface-modified polyimide porous film can be used.

[0080] The contact method is not particularly limited, and examples thereof include immersion, spin coating, spraying, roller coating, etc. Among these, the immersion method is preferred in the case of a porous polyimide, since it is easy to treat the polyimide uniformly.

[0081] The graft polymerization conditions after contact vary depending on the reactivity of the monomer, but for example, it is preferable to heat the mixture to 40° C. or higher and 100° C. or lower. It is also preferable to bubble the monomer solution with nitrogen or the like during the graft polymerization. This makes it easier for the graft polymerization to proceed smoothly.

[0082] After step (b), post-treatment such as washing and drying can be carried out. By washing, unreacted monomers and other unnecessary components can be removed from the obtained surface-modified polyimide. The washing method is not particularly limited, but it is sufficient to penetrate the surface-modified polyimide with a washing solvent by immersion or pressing, and then remove it. Examples of the washing solvent include water, alcohols such as methanol, ethanol, 1-propanol, and 2-propanol, ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, ethers such as tetrahydrofuran and dioxane, ethyl acetate, chloroform, and mixed solvents of two or more of these. The drying means includes heating, wind, reduced pressure, etc., and is not particularly limited, but wind drying and heating drying are preferred from the viewpoint of simplicity of the production process, and wind drying is more preferred. Drying may be achieved by simply leaving it to stand. EXAMPLES

[0083] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0084] Example 1 A porous polyimide film having a structural unit represented by the following formula was cut to a size of 100 mm x 100 mm. [ka] The cut porous polyimide film was placed in a treatment chamber of a plasma treatment device (TCE-4802, manufactured by Tokyo Ohka Kogyo Co., Ltd.) and subjected to plasma treatment under the following conditions. Gas: Helium (100cc) ·RF power: 500W (13.56MHz) ·Processing chamber pressure: 2~3Pa Processing time: 1 minute ·Double-sided processing

[0085] 2-acrylamido-2-methylpropanesulfonic acid (AMPS), ethanol, and deionized water were mixed in a mass ratio of 10:20:70. Nitrogen was bubbled through the mixture at room temperature for about 3 to 5 hours without generating bubbles, to prepare a monomer solution. The porous polyimide film immediately after plasma treatment was immersed in the monomer solution and reacted for 3.5 hours at 60°C while bubbling with nitrogen to carry out graft polymerization. The porous polyimide membrane taken out from the monomer solution was washed with water, ethanol, and water in this order, and then dried with an air blower to obtain a surface-modified porous polyimide membrane.

[0086] Example 2 A surface-modified polyimide porous film was obtained in the same manner as in Example 1, except that oxygen gas was used instead of helium gas as the gas in the plasma treatment.

[0087] Example 3 A surface-modified polyimide porous film was obtained in the same manner as in Example 1, except that nitrogen gas was used instead of helium gas as the gas in the plasma treatment.

[0088] Example 4 A surface-modified polyimide porous film was obtained in the same manner as in Example 1, except that acrylamide was used instead of AMPS as the monomer.

[0089] Example 5 A surface-modified polyimide porous film was obtained in the same manner as in Example 1, except that N-(2-hydroxyethyl)acrylamide was used as the monomer instead of AMPS.

[0090] Example 6 A surface-modified polyimide porous film was obtained in the same manner as in Example 1, except that 6-acrylamide hexanoic acid was used as the monomer instead of AMPS.

[0091] Example 7 A surface-modified polyimide porous film was obtained in the same manner as in Example 1, except that (3-acrylamidopropyl)trimethylammonium chloride was used as the monomer instead of AMPS.

[0092] Example 8 A surface-modified polyimide porous film was obtained in the same manner as in Example 1, except that dopamine methacrylamide was used as the monomer instead of AMPS.

[0093] Comparative Example 1 A surface-modified polyimide porous film was obtained in the same manner as in Example 1, except that the plasma treatment was not performed and an untreated porous polyimide film was immersed in the monomer solution.

[0094] Comparative Example 2 A surface-modified polyimide porous film was obtained in the same manner as in Example 1, except that argon gas was used instead of helium gas as the gas in the plasma treatment.

[0095] Comparative Example 3 Except for using a polypropylene film instead of a porous polyimide film, the plasma treatment was carried out in the same manner as in Comparative Example 2. Since damage occurred due to the heat of the plasma treatment, immersion in a monomer solution was not carried out. No metal removal properties were observed.

[0096] Comparative Example 4 Except for using a nylon film instead of the porous polyimide film, the plasma treatment was carried out in the same manner as in Comparative Example 2. Since damage occurred due to the heat of the plasma treatment, immersion in a monomer solution was not carried out.

[0097] <Contact angle> A droplet of pure water (2.0 μL) was dropped onto the surface of the surface-modified polyimide porous film using a Dropmaster 700 (manufactured by Kyowa Interface Science Co., Ltd.), and the contact angle was measured 2 seconds after the drop. The results are shown in Table 1.

[0098] <Surface roughness Rz and Ra> The obtained surface-modified polyimide porous film was spread on a flat glass substrate. At that time, a PET film was used to remove the air between the glass substrate and the porous film, thereby smoothing out any wrinkles that had formed in the porous film. Then, the surface roughness Rz and Ra were measured using a wide-range AFM AS-7B-μX manufactured by Takano Corporation under the following conditions. The results are shown in Table 1. Measurement range: 10μm×10μm

[0099] <Sulfur element ratio> The sulfur element ratio on the surface of the obtained surface-modified polyimide porous film was measured using a K-Alpha (registered trademark) XPS system (manufactured by Thermo Fisher Scientific Co., Ltd.) The results are shown in Table 1.

[0100] <Metal removability> As the test liquid, 30 mL of isopropyl alcohol (IPA) to which metal standard liquid XSTC-622B (manufactured by SPEX) was added so that each metal element had a concentration of 20 ppb by mass was used. The resulting surface-modified polyimide porous membrane was immersed in the test solution at room temperature for 6 hours and then removed, and the remaining test solution was used as a sample for measuring the metal ion concentration. The amount of 28 metal ions C (mass ppb) in the samples was measured using an inductively coupled plasma mass spectrometer (ICP-MS). Using the obtained value of the amount of metal ions C, the following formula: Metal ion removal rate (%) = 100-C (mass ppb) / 20 (mass ppb) x 100 The metal ion removal rate (%) was calculated according to the following. The arithmetic mean values ​​of the metal ion removal rates of chromium ions, manganese ions, iron ions, cobalt ions, and nickel ions related to stainless steel (SUS) components were evaluated according to the following criteria. The results are shown in Table 1. 〇: Higher removal rate than untreated nylon △: Metal removal is possible, but the removal rate is lower than that of untreated nylon. ×: No metal removal ability

[0101] <Damage> The surface of the obtained surface-modified polyimide porous membrane was observed with a scanning electron microscope (SEM) and evaluated according to the following criteria. The results are shown in Table 1. SEM images of Example 1 and Comparative Examples 1 and 2 are shown in Figures 1 to 3, respectively. ○: No change in appearance ×: There is a change in appearance such as surface roughness

[0102] [Table 1]

[0103] A comparison between the Examples and Comparative Examples reveals that a surface-modified polyimide porous film obtained by plasma treatment using a gas with a molecular weight lower than that of argon, which contains graft chains having metal-adsorbing functional groups, has a contact angle of 20° or less, and a surface roughness Rz of 500 nm or less, exhibits excellent metal removal properties and suppresses damage. According to Comparative Example 1, it is clear that the polyimide porous film obtained by reacting a monomer without carrying out a plasma treatment does not contain graft chains having metal-adsorbing functional groups and is poor in metal removal properties. According to Comparative Example 2, the contact angle and surface roughness Rz are outside the above numerical ranges, and it is found that the surface-modified polyimide porous film obtained by plasma treatment using argon gas has poor metal removal properties and is damaged.

Claims

1. A surface-modified polyimide porous film comprising a porous polyimide and a graft chain formed on at least a part of a surface of the porous polyimide, the graft chain has a metal-adsorbing functional group, the contact angle of the surface of the polyimide porous film is 20° or less; The surface-modified polyimide porous film has a surface roughness Rz of 500 nm or less.

2. The metal-adsorbing functional group is a sulfo group, -NR 1 R 2 (R 1 and R 2 each independently represents a hydrogen atom or an alkyl group), a hydroxy group, a carboxy group, -N + R 3 R 4 R 5 (R 3 , R 4 , and R 5 The surface-modified polyimide porous film according to claim 1 , comprising at least one selected from the group consisting of a group represented by the formula (III) (wherein each independently represents a hydrogen atom or an alkyl group) and a phosphoryl group.

3. 3. The surface-modified polyimide porous film according to claim 1, wherein the sulfur element ratio determined by X-ray photoelectron spectroscopy is 1 atm % or more.

4. (a) performing a plasma treatment on at least a portion of a surface of the polyimide using a gas having a molecular weight lower than that of argon; (b) contacting the plasma-treated polyimide with a monomer having a metal-adsorbing functional group.

5. The method according to claim 4 , wherein the polyimide is a porous polyimide.

6. The method according to claim 4 or 5, wherein the gas comprises at least one selected from the group consisting of helium gas, oxygen gas, and nitrogen gas.

7. The method according to claim 4 or 5, wherein the RF power of the plasma treatment is 100 W or more.

Citation Information

Patent Citations

  • Surface treatment liquid, surface treatment method, cation adsorbent, cation removing device, and cation removing method

    JP2018159039A