Vehicle interior material and method for manufacturing the same
The vehicle interior material maintains fabric texture and flexibility by using design rolls to create a fine uneven pattern on automotive fabrics, addressing the issue of impaired feel and flexibility in conventional methods.
Patent Information
- Application Number
- JP2023065549
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional methods for forming uneven patterns on automotive fabrics using thermoplastic resins impair the original feel and flexibility of the fabric, reducing its commercial value.
A vehicle interior material with a first design part derived from the woven or knitted fabric structure and a second design part featuring a fine uneven pattern formed on the backside recesses by embossing, using design rolls with specific dimensions and temperatures to create a fabric with enhanced commercial value.
The solution maintains the fabric's texture and flexibility while allowing a visually distinct fine uneven pattern, preventing collapse and maintaining flexibility, thus enhancing the fabric's commercial value.
Smart Images

Figure 2024151824000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an interior material for a vehicle. [Background technology]
[0002] In recent years, there has been a demand for fabrics for vehicle interiors that are more differentiated and have higher commercial value than ever before. On the other hand, various fabric processing methods have been used to improve the design of fabrics, not only for automobiles.
[0003] For example, Patent Document 1 discloses a method in which a pattern roll having an uneven pattern on its surface and a hot roll having a smooth peripheral surface are arranged in parallel with a gap narrower than the thickness of the fabric, the back side of the fabric is pressed against the pattern roll while passing through the gap between the two rolls, and the hot roll is brought into contact with the fabric surface protruding from the convex parts of the pattern roll to smoothly deform the contact area, thereby forming a glossy pattern on the fabric surface. This is said to be a method that can inexpensively form a glossy pattern only on the fabric surface without impairing the texture. However, since the hot roll is brought into contact to smoothly deform the contact area, the texture is not impaired except for the contact area, but the smoothly deformed contact area inevitably reduces the luxurious feel.
[0004] Patent Document 2 also discloses a method for imparting a special uneven pattern to a fabric, in which a fabric made of thermoplastic synthetic fibers is embossed and calendered so that the height difference between the concave and convex parts is 1 mm or more, and then the convex surface of the fabric is placed against a mirror roll surface heated to 100° C. or more to perform friction calendering. This is said to produce a fabric with durable special unevenness and strong gloss. However, this requires two steps, embossed calendering and friction calendering.
[0005] In addition, as a processing method that does not cause gloss in the recesses of the uneven pattern and does not impair the design and texture, Patent Document 3 discloses an embossing method in which a water-soluble polymer compound is attached to a fabric, the fabric is dried, and then a heated embossing mold is pressed against the fabric to impart an uneven pattern, and then the fabric is washed to remove the water-soluble polymer compound. This is said to be able to impart a durable uneven pattern to the fabric without impairing the design and texture. However, not only is a water-soluble polymer compound necessary, but the process of attaching the water-soluble polymer compound to the fabric, washing, and removing it are also necessary, which leads to an increase in the number of processing steps. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 7-145553 [Patent Document 2] Japanese Patent Application Publication No. 55-107574 [Patent Document 3] JP 2010-7211 A Summary of the Invention [Problem to be solved by the invention]
[0007] Meanwhile, since thermoplastic resins such as polyester are mainly used as raw materials for automotive fabrics, in order to form and maintain a concave-convex pattern on the fabric, it is necessary to perform embossing using a heated plate or a heated roll. The embossed fabric has recesses formed therein, and these recesses are given a strong gloss due to the hardening of the fabric. Therefore, when the conventional technology is applied, although it is possible to form a concave-convex pattern on the fabric, there is a problem that the original tactile feel of the fabric is deteriorated and the flexibility is impaired, i.e., the commercial value is reduced.
[0008] The present invention has been made in consideration of the above technical background, and aims to provide a vehicle interior material with high commercial value that suppresses deterioration of the texture, such as the feel and flexibility, of the fabric, and a method for manufacturing the vehicle interior material. [Means for solving the problem]
[0009] In order to achieve the above object, the present invention provides the following means.
[0010] [1] A fabric made of a woven or knitted thermoplastic resin, The fabric has a first design portion and a second design portion on a surface thereof, The unique design portion is a design including a pattern based on a structure derived from the woven or knitted fabric, The second design portion is characterized in that it is a design including a fine uneven pattern formed on the front side of a recess formed on the back side of the fabric by embossing.
[0011] [2] The vehicle interior material according to paragraph 1, wherein the thickness of the fabric of the first design portion is greater than the thickness of the fabric of the second design portion.
[0012] [3] A method for producing a vehicle interior material according to the preceding paragraph 1 or 2, The method includes a step of heating and pressing a fabric made of a woven or knitted fabric made of a thermoplastic resin between a design roll A and a design roll B, The design roll A has a top portion having an uneven height on the roll surface and a deep portion having an uneven depth, The average distance from the apex to the deep portion is in the range of 5 μm to 500 μm; The design roll B has a diameter of 200 mm or more, The roll has a protruding portion on the surface thereof and is disposed on the back surface side of the fabric, A method for producing a vehicle interior material, characterized in that the surface temperature is 120°C or higher.
[0013] [4] The method for producing an interior material for a vehicle according to item 3 above, wherein the height of the protrusions is in the range of 1 mm to 10 mm.
[0014] [5] The ratio of the diameter of the design roll A to the diameter of the design roll B is in the range of 1 / 1 to 1 / 1.8, and 5. The method for producing an interior material for a vehicle according to item 3 or 4 above, wherein the diameter of the designed roll B is in the range of 200 mm to 400 mm.
[0015] [6] The method for producing a vehicle interior material according to any one of items 3 to 5, wherein the fabric is a woven or knitted fabric made of polyester, and in the heating and pressing step, the surface temperature of the design roll B is heated to a range of 120°C to 230°C. Effect of the Invention
[0016] In the invention [1], a first design portion and a second design portion are provided on the surface of a fabric made of a woven or knitted thermoplastic resin, the first design portion being a design including a pattern derived from the texture of the woven or knitted fabric, and the second design portion being a design including a fine uneven pattern formed on the surface side of a recess formed on the back side of the fabric by embossing, so that the fine uneven pattern can be seen from any direction on the surface of the fabric, and a vehicle interior material with high commercial value in which deterioration of the texture of the fabric is suppressed can be provided.
[0017] In the invention [2], the thickness of the fabric of the first design portion is thicker than the thickness of the fabric of the second design portion, so that the second design portion has a unique texture that sinks in when touched. When the vehicle interior material is used as a seat covering material and a person sits in the seat, friction and body pressure are distributed to the back side of the second design portion, so that a vehicle interior material can be provided in which there is little risk of the design of the second design portion collapsing or disappearing.
[0018] The invention of [3] includes a process of heating and pressing a fabric made of a woven or knitted thermoplastic resin between a design roll A and a design roll B, the design roll A has a peak with a non-uniform height on the roll surface and a non-uniform depth, and the average distance from the peak to the non-uniform depth is in the range of 5 μm to 500 μm, and the design roll B has a diameter of 200 mm or more, has a protruding portion on the roll surface, is arranged on the back side of the fabric, and has a surface temperature of 120° C. or more, so that a vehicle interior material with high commercial value in which the deterioration of the texture of the fabric is suppressed can be manufactured. More specifically, the protruding portion on the roll surface of the design roll B forms a recess on the back side of the fabric, and the peak with a non-uniform height and the non-uniform depth on the roll surface of the design roll A form a fine uneven pattern on the surface layer on the front side of the fabric, that is, the second design portion can be formed. By setting the average distance from the top to the deepest part of the roll surface of the design roll A in the range of 5 μm to 500 μm, the glossiness of the fine uneven pattern can be adjusted without reducing the feel of the second design portion.
[0019] In the invention [4], the height of the convex portions is in the range of 1 mm to 10 mm. Therefore, no part of the back surface of the fabric is heated and pressed except for the part where the concave portions are formed. This makes it possible to suppress any deterioration in the feel of the fabric and any deterioration in its flexibility and elongation.
[0020] In the invention [5], the ratio of the diameter of the design roll A to the diameter of the design roll B is in the range of 1 / 1 to 1 / 1.8, and the diameter of the design roll B is in the range of 200 mm to 400 mm. Therefore, when the vehicle interior material is used as, for example, a seat covering material, a design with a larger repeat size can be made, and the protruding parts on the roll surface of the design roll B can be more effectively prevented from suddenly hitting the fabric. Therefore, there is no risk of a large step being created at the boundary between the first design part and the second design part, and vehicle interior materials can be manufactured without risking interference with the formation of a fine uneven pattern.
[0021] In the invention [6], the fabric is made of a polyester woven or knitted fabric, and in the heat pressing process, the surface temperature of the design roll B is heated to a range of 120°C to 230°C, thereby allowing sufficient recesses to be formed on the back surface of the fabric, and the polyester woven or knitted fabric does not melt, further preventing a decrease in the feel of the fabric.In addition, since the recesses are partial on the back surface of the fabric, a decrease in the flexibility of the fabric can also be prevented. [Brief description of the drawings]
[0022] [Figure 1] 1 is an explanatory diagram (plan view) of a vehicle interior material according to one embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view taken along line aa in FIG. 1. [Diagram 3] FIG. 13 is an explanatory diagram of a hot pressing step. [Figure 4] FIG. 2 is an example of a partially enlarged cross-sectional view of the design roll A in a heating and pressing process. [Diagram 5] FIG. 2 is an example of a partially enlarged cross-sectional view of the design roll B in a heating and pressing process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Next, an embodiment of a vehicle interior material according to the present invention will be described with reference to Figs.
[0024] In Fig. 1, the vehicle interior material 1 is a fabric 2 made of a woven or knitted fabric made of a thermoplastic resin, and has a first design part 3 and a second design part 4 on the surface of the fabric 2, the first design part 3 being a design including a pattern due to the texture of the woven or knitted fabric, and the second design part 4 being a design including a fine uneven pattern formed on the surface side of the recessed part 5 formed on the back side of the fabric 2 by embossing. By adopting such a configuration, more specifically, the fine uneven pattern can be visually recognized from any direction on the surface of the fabric 2, and a vehicle interior material 1 with high commercial value in which the deterioration of the texture of the fabric 2 is suppressed can be provided. In addition, there is no large step at the boundary between the first design part 3 and the second design part 4 as in the conventional embossing process, and the material has a smooth feel and a delicate gloss.
[0025] The fabric 2 is a woven or knitted fabric made of a thermoplastic resin, that is, a woven or knitted fabric. The thermoplastic resin is not particularly limited, and one or more conventionally known thermoplastic resins may be used. To use a plurality of thermoplastic resins, a method of using a mixture of fibers made of a thermoplastic resin as threads constituting a woven or knitted fabric, or a method of interweaving or interweaving can be mentioned. As the thermoplastic resin applied to the fabric 2 for vehicle interiors, a polyester-based resin is preferable from the viewpoint of durability, heat resistance, etc. In addition, the structure of the woven or knitted fabric, that is, the type of the woven or knitted structure is not particularly limited, and a conventionally known structure can be used. Examples of the weaving structure include dobby fabric and jacquard fabric. Examples of the knitting structure include warp knitting, weft knitting, circular knitting, etc.
[0026] The surface of the fabric 2 has a first design part 3 and a second design part 4. The first design part 3 is a design (omitted in FIG. 1) including a pattern due to the structure derived from the woven or knitted fabric described above. Here, the pattern due to the structure derived from the woven or knitted fabric includes fine unevenness due to the combination of thread thicknesses that appear on the surface of the fabric 2, the frequency of appearance, and the degree of continuity. The second design part 4 is a design including a fine uneven pattern formed on the surface layer part of the surface side of the fabric 2 by heating and pressing with the convex parts 9 protruding from the roll surface 8 of the design roll B by embossing, i.e., the heating and pressing step in the manufacturing method described later, and the surface of the fabric 2 comes into contact with the design roll A having peaks with variable heights and deep parts with variable depths. 1 shows an example of multiple diamonds in plan view as the second design portion 4, but it is not limited to diamonds and can be any shape such as a circle, a triangle, a square, a polygon, a geometric shape, a straight line, a curve, or a combination of these. This is due to the shape of the top surface 10 of the convex portion 9 of the design roll B.
[0027] As shown in FIG. 2, the first design portion 3 and the second design portion 4 are present on the surface of the fabric 2, and it is preferable that the thickness of the fabric 2 in the first design portion 3 is thicker than the thickness of the fabric 2 in the second design portion 4. By adopting such a configuration, the thickness of the first design portion 3 and the thickness of the second design portion 4 are different, and the thickness of the fabric in the first design portion 3 is thicker than the thickness of the fabric in the second design portion 4, so that the second design portion 4 sinks in when touched, creating a unique texture. When the vehicle interior material 1 is used as a seat covering material and a person sits on the seat, friction and body pressure are distributed to the back side in the second design portion 4, so that a vehicle interior material 1 can be provided that is unlikely to collapse or disappear. In addition, the first design portion 3 does not lose its touch or flexibility due to heating or pressure. Although not shown in FIG. 2, the recessed portion 5 may have a fine uneven pattern at the bottom in order to be more three-dimensional. In this case, it is preferable to provide unevenness on the top surface 10 of the convex portion 9 of the design roll B in the manufacturing method described later. Note that the fine uneven pattern on the bottom of the concave portion 5 does not correspond to the pattern due to the structure of the woven or knitted fabric of the first design portion 3.
[0028] Next, a manufacturing method of the vehicle interior material 1 will be described. The manufacturing method of the vehicle interior material 1 includes a step of heating and pressing the fabric 2 made of a woven or knitted fabric made of a thermoplastic resin between a design roll A and a design roll B. The design roll A has a peak 6 on the roll surface that has a non-uniform height, and a deep portion 7 that has a non-uniform depth. The average distance d from the peak 6 to the deep portion 7 is in the range of 5 μm to 500 μm. The design roll B has a diameter of 200 mm or more, has a protruding portion 9 protruding from the roll surface 8, is disposed on the back side of the fabric 2, and has a surface temperature of 120° C. or more. The height h of the protruding portion 9 is preferably in the range of 1 mm to 10 mm, and the second design portion 4 can be provided without unnecessarily heating and compressing the surrounding fabric 2 that is heated and pressed by the protruding portion 9.
[0029] In the heat pressing process, the fabric 2 is heated and pressed between the design roll A and the design roll B to form a recess 5 on the back surface of the fabric 2 and a second design portion 4 on the front surface of the fabric 2. That is, the second design portion 4 is a design including a fine uneven pattern formed on the surface layer of the front surface side of the fabric 2 by the front surface of the fabric 2 coming into contact with the design roll A having a peak portion with a variable height and a deep portion with a variable depth when the recess 5 is formed on the back surface of the fabric 2 by heating and pressing with the protrusion 9 protruding from the roll surface 8 of the design roll B, which is arranged on the back surface side of the fabric 2 and has a surface temperature of 120°C or more. The first design portion 3 is a design on the surface of the fabric 2 in the portion where the recess 5 is not formed on the back surface of the fabric 2. The surface of the fabric 2 contacts the design roll A, but the first design part 3 is not heated and pressed from the back by the protruding parts 9 protruding from the roll surface 8 of the design roll B, so the pattern due to the texture derived from the woven or knitted fabric is maintained. In this way, the surface of the fabric 2 has the first design part 3 with a design including a pattern due to the texture derived from the woven or knitted fabric, and the second design part 4 with a fine uneven pattern on the surface layer, and a high-value vehicle interior material 1 can be manufactured in which the deterioration of the texture of the fabric 2 is suppressed. More specifically, the protruding parts 9 protruding from the roll surface 8 of the design roll B form the recesses 5 on the back side of the fabric 2, and the top parts 6 with non-uniform heights and deep parts 7 with non-uniform depths on the roll surface 8 of the design roll A form a fine uneven pattern on the surface layer on the front side of the fabric 2, that is, the second design part 4 can be formed. Moreover, there is no increase in the number of processing steps.
[0030] As an example of an apparatus used in the hot pressing step, as shown in Fig. 3, rolls 11 and 12 are rotatably arranged opposite each other, and although not shown, rolls 11 and 12 are each equipped with a heating means. Design roll A is arranged as roll 11, and design roll B is arranged as roll 12, and the fabric 2 is passed between the heated rolls 11 and 12 with the front side of the fabric 2 facing up (the roll 11 side in Fig. 3) to be hot pressed. In Fig. 3, the fabric 2 is placed along about one-quarter of the circumference of the roll 12 and then hot pressed. The fabric 2 may be passed in the horizontal direction in Fig. 3, but this is preferred because the back side of the fabric 2 can be preheated.
[0031] In Figure 3, the peak 6 and deep portion 7 of the surface of design roll A arranged as roll 11, and the convex portion 9 of design roll B arranged as roll 12 are not shown, but Figure 4 shows an example of a partially enlarged cross-sectional view of design roll A, and Figure 5 shows an example of a partially enlarged cross-sectional view of design roll B.
[0032] As shown in FIG. 4, the outer peripheral surface of the design roll A has a plurality of peaks 6 with varying heights on the roll surface, as well as deep parts 7 with varying depths. Although neither is constant, they may be roughly uniform, and the average distance d from the peaks 6 to the deep parts 7 is in the range of 5 μm to 500 μm. By setting it in this range, the glossiness of the fine uneven pattern can be adjusted without degrading the tactile feel of the second design part 4. If the average distance d is less than 5 μm, the pattern will not be finely uneven, but will be flat, resulting in shininess, and if it exceeds 500 μm, the unevenness will become too large, which will hinder the tactile feel.
[0033] As shown in FIG. 5, the protrusions 9 are formed on the roll surface 8 of the design roll B. The height h of the protrusions 9 is preferably in the range of 1 mm to 10 mm. If the height h is less than 1 mm, the entire surface of the fabric 2 is pressed, which may reduce the texture and elongation of the fabric 2, such as the feel and flexibility, and if it exceeds 10 mm, the manufacturing cost of the roll increases and the thickness of the roll becomes thin, resulting in a decrease in strength. The height h may be set to be equal to or greater than the thickness of the fabric 2 within the above range. The shape of the top surface 10 of the protrusions 9 of the design roll B is not particularly limited, and may be set to any shape, such as a circle, a triangle, a square, a polygon, a geometric shape, a straight line, a curve, or a combination of these. In addition, in the design roll B, a plurality of protrusions 9 are provided, and it is preferable that the height h of each protrusion 9 is uniform, but in order to add contrast to the fine uneven pattern of the surface layer on the front side of the fabric 2, protrusions 9 of appropriately different heights h may be provided within a range that allows the formation of depressions 5 on the back side of the fabric 2. In addition, since the protrusions 9 of the design roll B do not heat and press any areas other than the areas where the depressions 5 are formed on the back side of the fabric 2, deterioration of the texture of the fabric 2 can be suppressed.
[0034] The surfaces of the design rolls A and B are made of metal, and the material is preferably carbon steel S25C or S45C because of its good thermal conductivity.
[0035] It is preferable that the ratio of the diameter of the design roll A to the diameter of the design roll B is in the range of 1 / 1 to 1 / 1.8, and the diameter of the design roll B is in the range of 200 mm to 400 mm. By adopting such a configuration, when the vehicle interior material 1 is used as, for example, a seat covering material, a design with a larger repeat size can be obtained, and the convex portion 9 protruding from the roll surface 8 of the design roll B can be more suppressed from suddenly hitting the fabric 2, so that the vehicle interior material 1 can be manufactured without the risk of a large step being generated at the boundary between the first design portion 3 and the second design portion 4 and without the risk of interfering with the formation of a fine uneven pattern. Note that if the diameter of the design roll B exceeds 400 mm, the weight of the roll increases and the cost increases, so the range of 200 mm to 350 mm is more preferable, and the diameter of the design roll A is even more preferable in the range of 200 mm to 250 mm within the range where the above-mentioned relationship is satisfied.
[0036] The fabric 2 is made of a woven or knitted polyester fabric, and in the heat pressing step, it is preferable to heat the surface temperature of the design roll B to a range of 120° C. to 230° C. By adopting such a configuration, the recesses 9 can be sufficiently formed on the back surface of the fabric 2, the polyester woven or knitted fabric does not melt, and deterioration in texture is further suppressed, and since the recesses 5 are partial on the back surface of the fabric 2, deterioration in the flexibility of the fabric 2 can also be suppressed.
[0037] The temperature of the design roll A and the temperature of the design roll B can be appropriately set depending on the type of thermoplastic resin. The temperature is higher than the glass transition temperature of the thermoplastic resin. For example, when the fabric 1 is a polyester resin, the temperature is preferably in the range of 140°C to 210°C, and more preferably in the range of 160°C to 190°C. The temperature of the design roll B is preferably about 10°C to 20°C higher than the temperature of the design roll A.
[0038] Moreover, the pressing pressure between the design roll A and the design roll B is preferably set within a range of conditions of, for example, about 20 to 60 kg / cm, and the processing speed is preferably set to about 0.1 to 5 m / min in terms of the passing speed of the fabric 2. By setting the speed within this range, a fine uneven pattern can be stably formed on the surface layer portion of the surface of the fabric 2, and deterioration of the texture of the fabric 2 can be suppressed, which is preferable.
[0039] In the above embodiment, the fabric 2 is a fabric made of a woven or knitted fabric made of thermoplastic resin, but within the scope of the technical concept of the present invention, a cushion layer may be laminated on a woven or knitted fabric made of thermoplastic resin. Examples of the cushion layer include polyurethane foam, fiber cushioning material, and nonwoven fabric, and the thickness is preferably about 1 mm to 12 mm. EXAMPLES
[0040] Next, specific examples of the present invention will be described, but the present invention is not particularly limited to these examples. Table 1 shows the details of each example and comparative example, and the evaluation results.
[0041] <Example 1> Fabric 2 is a woven fabric made of polyester fiber yarn (weight 400 g / m 2A design roll A (diameter 203 mm) with a leather grain pattern was prepared, in which the average distance d from the top 6 to the deep part 7 of the multiple peaks 6 and deep parts 7 formed on the roll surface as shown in FIG. 4 is 6.3 μm. In addition, a design roll B (diameter 203 mm) with a square dot pattern consisting of multiple protrusions 9 (top surface is square, height h is 1.5 mm) was prepared as a roll facing the design roll A. Using an apparatus as shown in FIG. 3, the design roll A was placed on the front side of the fabric as roll 11, and the design roll B was placed on the back side of the fabric as roll 12, and the surface of the design roll A was heated to a temperature of 190° C. and the surface of the design roll B was heated to a temperature of 210° C., and the two rolls were passed at a speed of 2 m / min. The contact pressure applied to the fabric between the design roll A and the design roll B was set to 50 kg / cm. In this way, a vehicle interior material with a leather grain pattern partially on the surface layer of the fabric was obtained. The resulting vehicle interior material was evaluated as having a grade 3 for abrasion resistance, an excellent rating for touch, and an excellent rating for flexibility.
[0042] <Example 2> A vehicle interior material was obtained in the same manner as in Example 1, except that a design roll A (diameter 203 mm) with a cross diamond pattern with an average distance d of 450 μm was used instead of the design roll A with a leather grain pattern with an average distance d of 6.3 μm, and a design roll B with a diameter of 350 mm was used instead of the design roll B with a square dot pattern. The evaluation of the obtained vehicle interior material was grade 4 for abrasion, "excellent" for touch, and "good" for flexibility.
[0043] <Example 3> In Example 1, a knitted fabric (polyester fiber, basis weight 350 g / m) was used instead of a woven fabric as the fabric 2. 2 A vehicle interior material was obtained in the same manner as in Example 1, except that a design roll A (diameter 203 mm) with a cross diamond pattern was used instead of design roll A with a leather grain pattern and an average distance d of 6.3 μm, and a design roll B with a square dot pattern and ...
[0044] <Example 4> In Example 1, instead of design roll A with an average distance d of 6.3 μm for the leather grain pattern, design roll A (diameter 203 mm) with a leather grain pattern with an average distance d of 350 μm was used, and instead of design roll B with a height h of 1.5 mm for the convex parts 9 of the square dot pattern, design roll B with a height h of 2.5 mm and a diameter of 270 mm was used, and a vehicle interior material was obtained in the same manner as in Example 1. The evaluation of the obtained vehicle interior material was grade 4 for abrasion, grade "○" for touch, and grade "○" for flexibility.
[0045] <Comparative Example 1> A fabric was obtained in the same manner as in Example 1, except that a roll (diameter 203 mm) having a mirror surface without a pattern on the roll surface was used instead of the design roll A having an average distance d of 6.3 μm for the leather grain pattern in Example 1. The evaluation of the obtained fabric was grade 2 for abrasion, "excellent" for touch, and "x" for flexibility.
[0046] <Comparative Example 2> In Example 1, the two rolls placed in the device were interchanged. That is, the design roll B was placed on the front side of the fabric as roll 11, and the design roll A was placed on the back side of the fabric as roll 12, and the surface of the design roll B was heated to a temperature of 190° C., and the surface of the design roll A was heated to a temperature of 210° C. A fabric was obtained in the same manner as in Example 1. The evaluation of the obtained fabric was grade 5 for abrasion, grade "x" for touch, and grade "good" for flexibility.
[0047] <Comparative Example 3> A fabric was obtained in the same manner as in Example 1, except that a leather grain pattern roll (diameter 203 mm) with an average distance d of 650 μm was used instead of the design roll A with an average distance d of 6.3 μm in the leather grain pattern in Example 1. The evaluation of the obtained fabric was grade 4 for abrasion, grade "x" for touch, and grade "good" for flexibility.
[0048] <Comparative Example 4> A fabric was obtained in the same manner as in Example 1, except that the surface temperature of the design roll B was heated to 100° C. instead of 210° C. The evaluation of the obtained vehicle interior material was grade 2 in abrasion resistance, grade "A" in touch, and grade "O" in flexibility.
[0049] <Comparative Example 5> A fabric was obtained in the same manner as in Example 1, except that a roll with a diameter of 100 mm was used instead of the square dot pattern design roll B (diameter 203 mm) in Example 1. The obtained vehicle interior material was evaluated as having abrasion of grade 4, a touch of "x", and a flexibility of "good".
[0050] [Table 1]
[0051] The vehicle interior materials of Examples 1 to 4 were flexible and had a high-quality feel with high commercial value, with the deterioration of the texture of the fabric suppressed. That is, the vehicle interior material of Example 1 was flexible, had a fine uneven pattern partially on the surface, and had a smooth texture without feeling a large concave on the surface layer at the edge of the pattern. In addition, the vehicle interior material of Example 2 had a large diameter of the design roll B, so the contact of the roll convex part during processing was mild, and the step at the edge of the pattern was smooth. The vehicle interior materials of Examples 2 and 4 had clear cross diamond patterns and leather grain patterns, respectively, after the wear test. In addition, the vehicle interior material of Example 3 had a high-quality feel like Example 1. On the other hand, the fabrics of Comparative Examples 1 to 5 did not simultaneously satisfy all of the wear resistance, texture, and flexibility.
[0052] <Wear resistance evaluation> The test was carried out under the following conditions using a Taber tester specified in ASTM D38846.1, and the degree of loss of the design (pattern) due to wear on the test piece surface was examined and evaluated. That is, the test piece was placed on a desk with the surface facing up, and visually observed from an angle of 45 to 60 degrees, and evaluated based on the following criteria. Grade 3 or higher was considered to be a pass. (Test conditions) Wear wheel No.: CS#10, Load: 4.9N, Test rotation speed: 1,000 times, Rotational friction speed: 60rpm / min (Judgment criteria) Grade 5: No change in design is observed. Grade 4: Wear marks are visible on the design. Grade 3: The design is faded. Class 2: It is recognized that part of the design has disappeared. Class 1: The entire design is deemed to have disappeared.
[0053] <Evaluation of texture> The surface of the test piece was evaluated by touching it with a finger to see whether the unevenness of the pattern edge of the test piece was felt. That is, the test piece was placed on a desk with the surface facing up and touched with a finger, and evaluated based on the following criteria. A rating of "◯" or higher was considered to be a pass. (Judgment criteria) ◎: No unevenness felt at the edge of the pattern. ○: There is slight unevenness at the edge of the pattern. ×: There are unevenness around the edge of the pattern.
[0054] <Flexibility assessment> JIS L1096 2010 8.21 Bending resistance Measured using Method A (45° cantilever method). The average value of the vertical and horizontal directions is 60mm or less, which is considered to be "good", and over 60mm is considered to be "bad". Method A (45° cantilever method) is as follows. a) Procedure A involves taking five test pieces, each 20 mm x 150 mm in length and width or wale and course, from the sample prepared in accordance with Clause 6, and placing the short side of the test piece on a smooth horizontal table with a 45° slope at one end, aligning it with the scale baseline. Next, gently slide the test piece in the direction of the slope by an appropriate method, and when the center point of one end of the test piece comes into contact with slope A, read the position of the other end on the scale. The bending resistance is indicated by the length (mm) traveled by the test piece, and measurements are taken on the front and back of each of the five pieces. b) The calculation shall be made by calculating the average value in each of the warp and weft directions or the wale and course directions, and rounding off to the nearest integer. [Industrial Applicability]
[0055] The vehicle interior material according to the present invention is suitably used in vehicles such as trains, buses, and automobiles, which require high merchantability. [Explanation of symbols]
[0056] 1. Vehicle interior materials 2...Fabric 3. Design Department 4. Second Design Department 5. Recess 6...Top 7...Deep part 8. Roll surface 9. Convex part 10...Top surface 11. Roll 12 rolls d distance h height
Claims
1. A fabric made of a woven or knitted thermoplastic resin, The fabric has a first design portion and a second design portion on a surface thereof, The unique design portion is a design including a pattern based on a structure derived from the woven or knitted fabric, The second design portion is characterized in that it is a design including a fine uneven pattern formed on the front side of a recess formed on the back side of the fabric by embossing.
2. The vehicle interior material according to claim 1 , wherein a thickness of the fabric of the first design portion is greater than a thickness of the fabric of the second design portion.
3. A method for producing the vehicle interior material according to claim 1 or 2, The method includes a step of heating and pressing a fabric made of a woven or knitted fabric made of a thermoplastic resin between a design roll A and a design roll B, The design roll A has a top portion having a non-uniform height on the roll surface and a deep portion having a non-uniform depth, The average distance from the apex to the depth is in the range of 5 μm to 500 μm; The design roll B has a diameter of 200 mm or more, The roll has a protruding portion on the surface thereof and is disposed on the back surface side of the fabric, A method for producing an interior material for a vehicle, characterized in that the surface temperature is 120°C or higher.
4. The method for producing an interior material for a vehicle according to claim 3, wherein the height of the protrusions is in the range of 1 mm to 10 mm.
5. The ratio of the diameter of the design roll A to the diameter of the design roll B is in the range of 1 / 1 to 1 / 1.8, and The method for producing an interior material for a vehicle according to claim 3 or 4, wherein the diameter of the design roll B is in the range of 200 mm to 400 mm.
6. The fabric is made of a polyester woven or knitted fabric, The method for manufacturing a vehicle interior material according to any one of claims 3 to 5, wherein in the heat pressing step, the surface temperature of the design roll B is heated to a range of 120°C to 230°C.
Citation Information
Patent Citations
Fabric modifying method
JP1980107574A
Method for forming glossy pattern on surface of cloth and apparatus therefor
JP1995145553A
Method for embossing finish of fabric
JP2010007211A