Inorganic molded body, and method of producing the same

By using granulated blast furnace slag and fly ash with cement and hydrothermal treatment, the production of inorganic molded bodies achieves desired properties at lower temperatures, overcoming density, strength, and stability issues, and reducing environmental impact.

JP2024151842APending Publication Date: 2024-10-25A & A MATERIAL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023065582
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing inorganic molded bodies using natural products like quicklime and silica stone face challenges in achieving low bulk density, high bending strength, and dimensional stability due to high curing temperatures and the use of gypsum, which generates negative reaction products.

Method used

Utilizing granulated blast furnace slag and fly ash as industrial by-products, combined with cement and hydrothermal treatment, to produce an inorganic molded body with specific component ratios and low-temperature curing, incorporating reinforcing fibers and lightweight materials like tobermorite slurry.

Benefits of technology

The solution results in a product with a bulk density of 0.90 to 1.10 g/cm³, bending strength of 10.0 N/mm², and a length change rate of 0.15% or less, addressing the limitations of existing technologies while reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151842000001
    Figure 2024151842000001
  • Figure 2024151842000002
    Figure 2024151842000002
Patent Text Reader

Abstract

To provide an inorganic molded body made from an industrial byproduct instead of a natural product by way of a reaction at a low temperature, satisfying required characteristics, i.e., a product bulk density of from 0.90 to 1.10 g / cm3, flexural strength of 10.0 N / mm2 or more, and a length change rate of 0.15% or less.SOLUTION: The inorganic molded body contains blast furnace water-granulated slug (a), cement (b), and fly-ash (c) in an amount of 35 mass% or more and 97 mass% or less in total, a hydrothermally processed weight-saving material (d) in an amount of 3 mass% or more and 24 mass% or less, and a reinforcement fiber (e) in an amount of 3 mass% or more and 10 mass% or less relative to the whole solid components, with the mass ratio of the components (a), (b), and (c) contained therein being as follows: ((a)+(b)) / (c))=80 / 20 to 30 / 70, and (a) / (b)=100 / 10 to 100 / 50.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an inorganic molded body and a method for producing the same. [Background technology]

[0002] Inorganic molded bodies such as calcium silicate boards are non-flammable and have excellent durability, and are therefore widely used as building materials for interior materials, etc. These calcium silicate boards are usually produced by wet molding a slurry containing a calcareous raw material such as quicklime, a siliceous raw material such as silica stone, cement, reinforcing fibers, and an inorganic lightweight material, followed by autoclaving at a temperature of about 180°C (Patent Documents 1 to 3). Natural products such as quicklime and silica stone are widely used as the raw materials for calcium silicate of these inorganic moldings, but in consideration of reducing the burden on the global environment, it is desirable to use some industrial by-products. Furthermore, when natural products such as quicklime and silica stone are used, a curing and hardening process at a high temperature of about 180°C is required due to the hardening reaction of the product.

[0003] On the other hand, Patent Documents 4 to 6 have been reported as techniques for producing inorganic molded bodies without using quicklime or silica stone, which use blast furnace slag or fly ash as raw materials. However, the inorganic molded bodies described in Patent Documents 4 and 5 do not use cement, and therefore do not meet the required characteristics of low product bulk density and high bending strength due to insufficient hardening. In addition, the inorganic molded body described in Patent Document 6 uses 2 to 5 mass% gypsum, which generates reaction products containing gypsum components that are thought to have an adverse effect on the length change rate, and as a result, it does not meet the required characteristics of a small length change rate, i.e., excellent dimensional stability. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 52-135330 [Patent Document 2] JP 2013-203566 A [Patent Document 3] JP 2019-43783 A [Patent Document 4] JP 58-125656 A [Patent Document 5] Japanese Patent Application Publication No. 10-259052 [Patent Document 6] JP 2013-216534 A Summary of the Invention [Problem to be solved by the invention]

[0005] The object of the present invention is to use industrial by-products instead of natural products, and to produce a product with a bulk density of 0.90 to 1.10 g / cm3 at a low temperature. 3 , bending strength 10.0N / mm 2 The object of the present invention is to provide an inorganic molded article that satisfies the required characteristic of a length change rate of 0.15% or less, and a method for producing the same. [Means for solving the problem]

[0006] The inventors therefore discovered that by using industrial by-products, granulated blast furnace slag and fly ash, as the calcareous and siliceous raw materials, and mixing these with cement in a specific range, and by using certain amounts of hydrothermal treatment lightweight material and reinforcing fibers, an inorganic molded body having the required characteristics can be obtained by heat treatment at a lower temperature, and thus completed the present invention.

[0007] That is, the present invention provides the following inventions [1] to [5]. [1] An inorganic molded body containing, relative to the total solid content, 35% by mass or more and 97% by mass or less of granulated blast furnace slag (a), cement (b) and fly ash (c), 3% by mass or more and 24% by mass or less of a hydrothermal treatment lightweight material (d), and 3% by mass or more and 10% by mass or less of a reinforcing fiber (e), wherein the mass ratios of the components (a), (b) and (c) are ((a)+(b)) / (c))=80 / 20-30 / 70 and (a) / (b)=100 / 10-100 / 50. [2] The inorganic molded body according to [1], wherein the hydrothermal treated lightweight material (d) is a lightweight material containing one or more selected from a tobermorite slurry, a xonotlite slurry, a low-crystalline calcium silicate hydrate slurry, and a calcium aluminate hydrate slurry. [3] The inorganic molded body according to [1] or [2], further comprising a filler. [4] Product bulk density: 0.90-1.10g / cm 3 , bending strength 10.0N / mm 2 The inorganic molded product according to any one of [1] to [3], wherein the rate of change in length is 0.15% or less. [5] A method for producing an inorganic molded body, comprising wet molding a slurry containing granulated blast furnace slag (a), cement (b), fly ash (c), hydrothermal treatment lightweight material (d), and reinforcing fiber (e), followed by curing and hardening at a temperature of 80 to 160°C. The inorganic molded body contains granulated blast furnace slag (a), cement (b), and fly ash (c) in a total amount of 35% by mass to 97% by mass, hydrothermal treatment lightweight material (d) in an amount of 3% by mass to 24% by mass, and reinforcing fiber (e) in an amount of 3% by mass to 10% by mass, based on the total solid content, and the mass ratio of the components (a), (b), and (c) is ((a)+(b)) / (c))=80 / 20 to 30 / 70, (a) / (b)=100 / 10 to 100 / 50. Effect of the Invention

[0008] The inorganic molded body of the present invention uses a large amount of industrial by-products instead of natural products as raw materials, and by low-temperature heat treatment, the product has a bulk density of 0.90 to 1.10 g / cm. 3 , bending strength 10.0N / mm 2 As described above, an inorganic molded article that satisfies the required characteristic of a length change rate of 0.15% or less can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] One aspect of the present invention is an inorganic molded body containing, relative to the total solid content, 35% by mass or more and 97% by mass or less of granulated blast furnace slag (a), cement (b) and fly ash (c), 3% by mass or more and 24% by mass or less of a hydrothermal treatment lightweight material (d), and 3% by mass or more and 10% by mass or less of a reinforcing fiber (e), wherein the mass ratios of the components (a), (b) and (c) are ((a)+(b)) / (c))=80 / 20 to 30 / 70 and (a) / (b)=100 / 10 to 100 / 50.

[0010] The inorganic molded body of the present invention contains 35 mass% or more and 97 mass% or less of granulated blast furnace slag (a), cement (b) and fly ash (c) in total relative to the total solid content, and the mass ratios of the components (a), (b) and (c) are ((a)+(b)) / (c))=80 / 20 to 30 / 70 and (a) / (b)=100 / 10 to 100 / 50. The inorganic molded body of the present invention contains granulated blast furnace slag and fly ash as matrix forming raw materials in addition to cement, and does not substantially use quicklime or silica stone which have been conventionally used. Granulated blast furnace slag (a) is a by-product produced when pig iron is produced in a blast furnace of a steelworks, and is mainly composed of CaO, SiO2, and Al2O3. In the present invention, it functions as a calcareous raw material and a siliceous raw material, leading to the effective use of industrial waste. The preferred ranges of the contents of these components are CaO: 30-50 mass%, more preferably 40-44 mass%, SiO2: 25-40 mass%, more preferably 30-35 mass%, and Al2O3: 10-20 mass%, more preferably 12-16 mass%. When the contents of CaO and SiO2 are as described above, the balance of the contents of the calcareous raw material and the siliceous raw material is good, and the hardening property is good, so this is preferable. In addition, the specific surface area of ​​the blast furnace slag is preferably 1000-15000, more preferably 3000-11000. The specific surface area in the above range is preferable because it provides good curability, prevents process problems such as clogging, prevents high costs, and ensures necessary physical properties. Here, the specific surface area is a value measured by the test method specified in JIS A 6206. As the cement (b), ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement (JIS R 5210), etc. can be used. Fly ash (c) is a by-product generated in coal-fired power plants, and is formed when pulverized coal is burned and the ash melts and cools to form a globular shape. It is mainly composed of SiO2 and Al2O3. Therefore, in the present invention, it functions as a siliceous raw material. The content of the SiO2 component is preferably in the range of 35 to 80 mass%, more preferably 40 to 75 mass%. When the content of SiO2 is in the above range, the content as a siliceous raw material is good, and the hardening property is also good, which is preferable.

[0011] In the present invention, the total content of granulated blast furnace slag (a), cement (b) and fly ash (c) is preferably 35% by mass or more and 97% by mass or less based on the total solid content. By including the amounts in this range, particularly 35% by mass or more, an inorganic molded product having good properties can be obtained without substantially using natural products such as quicklime and silica stone. The total content of these three components is more preferably 40% by mass or more and 96% by mass or less, and even more preferably 45% by mass or more and 95% by mass or less. When a lightweight material containing as its main components a tobermorite slurry, a xonotlite slurry, and a low-crystalline calcium silicate hydrate slurry is used as the hydrothermal treatment lightweight material (d), the total amount of these three components is preferably 35% by mass or more and 94% by mass or less, more preferably 40% by mass or more and 93% by mass or less, and even more preferably 45% by mass or more and 92% by mass or less. Furthermore, when a lightweight material containing calcium aluminate hydrate slurry as a main component (e.g., swollen slag slurry) is used as the hydrothermal treatment lightweight material (d), the content is preferably 50% by mass or more and 97% by mass or less, more preferably 55% by mass or more and 93% by mass or less, and even more preferably 60% by mass or more and 92% by mass or less. The mass ratio of the three components (a), (b) and (c) is preferably ((a)+(b)) / (c)=80 / 20 to 30 / 70, (a) / (b)=100 / 10 to 100 / 50, in order to obtain an inorganic molded product having good properties by low-temperature heat treatment. Moreover, ((a)+(b)) / (c)) is more preferably 70 / 30 to 40 / 60. (a) / (b) is more preferably 100 / 15 to 100 / 45.

[0012] In the present invention, it is preferable to use the hydrothermal treatment lightweight material (d) as the lightweight material from the viewpoints of ensuring a good appearance, reducing the production cost, and obtaining an inorganic molded product with good dimensional stability. The hydrothermally treated lightweight material (d) may be one or more selected from the group consisting of tobermorite slurry, xonotlite slurry, low-crystalline calcium silicate hydrate slurry, and calcium aluminate hydrate slurry. These hydrothermally treated lightweight materials are obtained by hydrothermally treating a slurry containing a siliceous raw material and a calcareous raw material or a slurry containing granulated blast furnace slag. A slurry containing tobermorite as a main component and a small amount of low-crystalline calcium silicate hydrate, or a slurry containing low-crystalline calcium silicate hydrate as a main component and optionally containing a small amount of tobermorite, is a tobermorite-based slurry, which is obtained by producing a slurry of a calcareous raw material and a siliceous raw material in a blending ratio of 0.3 to 1.5 in terms of Ca / Si molar ratio, and holding the slurry at 150°C to 220°C for 0.5 to 24 hours when tobermorite is the main component, or by holding the slurry at 100°C or higher but lower than 150°C for 0 to 12 hours when low-crystalline calcium silicate hydrate is the main component (bulk density: 0.12 to 0.17 g / cm 3 , wet volume: 50~150ml). A slurry containing xonotlite as a main component and a small amount of low-crystalline calcium silicate hydrate, or a slurry containing low-crystalline calcium silicate hydrate as a main component and optionally containing a small amount of xonotlite, is a xonotlite-based slurry, which is obtained by producing a slurry from a calcareous raw material and a siliceous raw material in a blending ratio of 0.8 to 1.2 in terms of Ca / Si molar ratio, and holding the slurry at 190°C to 220°C for 5 to 20 hours when xonotlite is the main component, or by holding the slurry at 190°C to 220°C for 1 hour or more but less than 5 hours when low-crystalline calcium silicate hydrate is the main component (bulk density: 0.07 to 0.15 g / cm 3 , wet volume: 100~300ml). The lightweight material consisting essentially of low-crystalline calcium silicate hydrate slurry is obtained by producing a slurry of a calcareous raw material and a siliceous raw material in a blending ratio of 0.2 to 4.0 in terms of Ca / Si molar ratio, and keeping the slurry at 80°C to less than 100°C for 1 to 6 hours (bulk density: 0.08 to 0.16 g / cm 3 , wet volume: 120~400ml). The lightweight material made of calcium aluminate hydrate slurry is obtained by making a slurry of raw materials containing calcium and aluminum, such as granulated blast furnace slag, and keeping it at 80°C to less than 100°C for 0.5 to 6 hours (bulk density: 0.18 to 0.24 g / cm 3 , wet volume: 20~60ml). The bulk density and wet volume of each of the slurries were measured as follows. ·Bulk density of slurry Internal volume 91.5cm 3 The slurry is poured into a Buchner funnel and suction filtered. After filtration, the slurry is dried at 105°C and the weight W is measured and calculated using the following formula. Bulk density = W / 91.5 (g / cm 3 ) Wet volume of slurry 10 g of the slurry solids are placed in a 500 ml graduated cylinder, then water is added to make the total volume 500 ml, the mixture is stirred by inversion 10 times, and the settled volume is read after leaving it to stand for 60 minutes. Examples of the calcareous raw materials used in the production of these hydrothermal treated lightweight materials include quicklime and slaked lime, and examples of the siliceous raw materials include silica stone and silica sand. Other siliceous raw materials that can be used include silica fume, diatomaceous earth, fly ash, and synthetic amorphous silica. The content of the hydrothermal treated lightweight material (d) in the inorganic molded body is preferably 3% by mass or more and 24% by mass or less, more preferably 4% by mass or more and 22% by mass or less, and even more preferably 5% by mass or more and 20% by mass or less, based on the total solids content, from the viewpoints of obtaining an inorganic molded body having good properties by hydrothermal treatment at a lower temperature, ensuring a good appearance, and reducing production costs. When using a lightweight material whose main component is a tobermorite slurry, a xonotlite slurry, or a low-crystalline calcium silicate hydrate slurry, it is more preferable for the content to be 3% by mass or more and 15% by mass or less, even more preferable for the content to be 4% by mass or more and 14% by mass or less, and even more preferable for the content to be 5% by mass or more and 13% by mass or less. Furthermore, when using a lightweight material containing calcium aluminate hydrate slurry as a main component (e.g., swollen slag slurry), the content is preferably 8% by mass or more and 24% by mass or less, more preferably 8.5% by mass or more and 22% by mass or less, and even more preferably 9% by mass or more and 20% by mass or less.

[0013] Examples of the reinforcing fiber (e) include plant fibers such as wood pulp, recycled pulp, and various hemp fibers; synthetic fibers such as polyvinyl alcohol, polypropylene, polyethylene, polyester, acrylic, and rayon; glass wool, rock wool, ceramic wool, and carbon fibers; and these can be used alone or in combination of two or more. The content of these reinforcing fibers (e) in the inorganic molded body is preferably 3 mass% or more and 10 mass% or less, more preferably 3.5 mass% or more and 9 mass% or less, and even more preferably 4 mass% or more and 8 mass% or less, in order to impart excellent impact resistance and bending strength to the inorganic molded body.

[0014] The inorganic molded body of the present invention may further contain various fillers for the purpose of improving bending strength, controlling the rate of change in length, etc. Examples of fillers include mica powder, wollastonite powder, calcium carbonate, talc, and bentonite. From the viewpoint of improving the above-mentioned functions, the content of the filler is preferably from 0 to 40% by mass, more preferably from 0 to 30% by mass, and even more preferably from 0 to 25% by mass.

[0015] The inorganic molded body of the present invention can be produced by wet molding a slurry containing granulated blast furnace slag (a), cement (b), fly ash (c), hydrothermal treatment lightweight material (d), and reinforcing fibers (e), followed by curing and hardening at a temperature of 80 to 160°C. More specifically, a slurry containing granulated blast furnace slag (a), cement (b), fly ash (c), hydrothermal treatment lightweight material (d), and reinforcing fibers (e) is prepared, the slurry is wet-molded to obtain a green sheet, one or more of the obtained green sheets are laminated and pressure-molded, and then cured at a temperature of 80 to 160°C to obtain the composite material. In the conventional manufacturing method of calcium silicate board, a heating temperature of about 180°C is required for curing and hardening. In the present invention, however, a heating temperature of 80 to 160°C is required, and the product has a bulk density of 0.90 to 1.10 g / cm. 3 , bending strength 10.0N / mm 2 Thus, an inorganic molded article having a length change rate of 0.15% or less can be obtained.

[0016] According to the present invention, by using granulated blast furnace slag and fly ash, which are industrial by-products, as the main raw materials, adding a hydrothermal treatment lightweight material, and mixing each raw material in an appropriate ratio, it is possible to obtain sufficient performance as an interior material at a low curing and hardening temperature. In other words, the present invention makes it possible to manufacture environmentally friendly products, which can lead to the suppression of global warming. EXAMPLES

[0017] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0018] Examples 1 to 8 and Comparative Examples 1 to 12 The raw materials used in each example are as follows: Tobermorite slurry Quicklime (CaO content 97.2% by mass) 33% by mass, Blaine value 10300 cm 2 A raw material slurry was obtained by adding 1,000 parts by mass of water to 100 parts by mass of a mixture consisting of 67% by mass of silica powder (SiO2 content 94.7% by mass, Al2O3 content 1.6% by mass, Ca / (Al+Si) molar ratio = 0.54) with a Ca content of 94.7% by mass and an Al content of 1.6% by mass, and mixing and dispersing the mixture. This raw material slurry was subjected to hydrothermal synthesis in an autoclave at 190°C for 2 hours to obtain a synthetic tobermorite slurry (solid content: 10.1% by mass, average particle size: 109 μm). (Bulk density: 0.136g / cm 3 , wet volume: 80ml) · Swollen slag slurry (calcium aluminate hydrate slurry) Blaine value 4500cm 2 A raw material slurry was obtained by adding 1,000 parts by mass of water to 100 parts by mass of a mixture consisting of 77% by mass of granulated blast furnace slag having a molecular weight of 1.01 g / g and 23% by mass of ordinary Portland cement, and mixing and dispersing the mixture. This raw material slurry was subjected to hydrothermal treatment in an autoclave at 95°C for 2 hours to obtain a swollen slag slurry (calcium aluminate hydrate slurry, solid content: 9.8% by mass, average particle size: 62 μm). (Bulk density: 0.211g / cm 3 , wet volume: 40ml) Granulated blast furnace slag (JIS A 6206) Blaine value 4500cm 2 / g, CaO content 42% by mass, SiO2 content 33% by mass, Al2O3 content 14% by mass ·cement Ordinary Portland cement (JIS R 5210) CaO content 65% by mass, SiO2 content 22% by mass, Al2O3 content 5% by mass Fly ash Blaine value 5700cm 2 / g, SiO2 content 60% by mass Reinforcement fibers Wood pulp Canadian Freeness 320cc ·Filling material Calcium carbonate Blaine value 5500cm 2 / g

[0019] The raw materials were mixed in the proportions shown in Tables 1 and 2 to prepare a mixture, and 100 parts by mass of water was added to 100 parts by mass of the solid content of the raw material mixture and mixed to obtain a raw material slurry. Next, the raw material slurry was press-molded at a press pressure of 1.6 MPa in a table test simulating a papermaking method to obtain a green sheet with a width of 150 mm, a length of 200 mm, and a thickness of about 10 mm. This green sheet was cured by curing under saturated steam pressure at the temperature and holding time shown in the table to prepare a test specimen. After drying the test specimen, the following tests were performed.

[0020] -Bulk density of specimen Measured according to JIS A 5430 8.5 Bulk Density Test (Calcium Silicate Board (Type 2)). -Bending strength of specimen After drying at 40°C for 24 hours, a three-point bending test was carried out on specimens measuring 150 mm x 200 mm with a span of 15 cm and a crosshead speed of 1 mm / min. - Length change rate due to water absorption of specimen (%) Measured using JIS A 5430 8.7 Length change rate due to water absorption test (calcium silicate board (type 2)).

[0021] [Table 1]

[0022] [Table 2]

Claims

1. The inorganic molded body contains, relative to the total solid content, 35% by mass or more and 97% by mass or less of granulated blast furnace slag (a), cement (b) and fly ash (c), 3% by mass or more and 24% by mass or less of a hydrothermal treatment lightweight material (d), and 3% by mass or more and 10% by mass or less of reinforcing fibers (e), wherein the mass ratios of the components (a), (b) and (c) are ((a)+(b)) / (c))=80 / 20 to 30 / 70 and (a) / (b)=100 / 10 to 100 / 50.

2. 2. The inorganic formed article according to claim 1, wherein the hydrothermal treatment lightweight material (d) is a lightweight material containing at least one material selected from the group consisting of a tobermorite slurry, a xonotlite slurry, a low-crystalline calcium silicate hydrate slurry, and a calcium aluminate hydrate slurry.

3. 2. The inorganic molded article according to claim 1, further comprising a filler.

4. Product bulk density 0.90-1.10g / cm 3 , bending strength 10.0 N / mm 2 2. The inorganic molded article according to claim 1, wherein the rate of change in length is 0.15% or less.

5. A method for producing an inorganic molded body, comprising wet molding a slurry containing granulated blast furnace slag (a), cement (b), fly ash (c), a hydrothermal treatment lightweight material (d), and reinforcing fibers (e), followed by curing and hardening at a temperature of 80 to 160°C, the inorganic molded body containing granulated blast furnace slag (a), cement (b), and fly ash (c) in total at 35% by mass to 97% by mass, 3% by mass to 24% by mass of the hydrothermal treatment lightweight material (d), and 3% by mass to 10% by mass of the reinforcing fibers (e) relative to the total solid content, the mass ratio of the components (a), (b), and (c) being ((a)+(b)) / (c))=80 / 20 to 30 / 70, and (a) / (b)=100 / 10 to 100 / 50.

Citation Information

Patent Citations

  • Production of calcium silicate boad free from asbestos

    JP1977135330A

  • Manufacture of inorganic board

    JP1983125656A

  • Production of inorganic hardened body

    JP1998259052A

  • Calcium silicate compact, and method for producing the same

    JP2013203566A

  • Inorganic board

    JP2013216534A