Sapling protector
The sapling protector with a water-repellent coating layer addresses the issue of snow-induced collapse by dispersing snow force, maintaining the protector's structure and protecting seedlings from wild animals.
Patent Information
- Application Number
- JP2023065690
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing seedling protectors collapse under the weight of accumulated snow, fail to maintain their posture, and may deform seedlings due to pressure, especially in areas with heavy snowfall, without effective measures to prevent this collapse.
A sapling protector with a cylindrical net featuring a water-repellent coating layer containing water-repellent particles and filler particles to disperse the force of snow accumulation, preventing collapse and maintaining the protector's structure.
The water-repellent coating effectively suppresses snow accumulation on the net, preventing the protector from collapsing and ensuring the seedlings are protected from wild animals and deformation.
Smart Images

Figure 2024151896000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a seedling protector for protecting seedlings from wild animals. [Background technology]
[0002] Patent Document 1 discloses a protective device for seedlings, etc., which protects seedlings of trees such as seedlings or young trees from damage caused by wild animals and promotes the growth of the seedlings, etc. The protective device has a protective net having a vertically elongated cylindrical or substantially truncated cone shape, and a support material that supports the protective net. Paragraph 0015 of Patent Document 1 describes that the protective device for seedlings, etc., has shape retention that does not put a load on the seedlings, etc., even with the weight of accumulated snow. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-161302 A Summary of the Invention [Problem to be solved by the invention]
[0004] Incidentally, when protective equipment for seedlings, etc. (hereinafter referred to as "protective equipment") is used in areas with snowfall, the protective equipment may collapse under the weight of accumulated snow, and the protective equipment may not be able to maintain a normal posture due to the accumulation of snow. In such cases, the purpose of the protective equipment, which is to protect seedlings, etc. from damage caused by wild animals eating them, cannot be achieved. In particular, in areas with heavy snowfall, it has been reported that protective equipment breaks and collapses due to the weight of snow and the shift of accumulated snow when it melts. In addition, damage has been reported in which seedlings do not grow straight and become deformed due to the pressure of collapsed protective equipment. As a countermeasure, attempts have been made to strengthen the support poles of the protective equipment and to make the support poles flexible by using FRP materials, but a measure that can efficiently suppress and prevent the collapse of protective equipment due to snow accumulation has not yet been found.
[0005] The present invention has been made in view of the above-mentioned points. That is, an object of the present invention is to prevent the collapse of protective equipment due to snow accumulation. [Means for solving the problem]
[0006] The present invention relates to a seedling protector having a tubular net for surrounding a seedling, the net having a water-repellent coating layer on its surface. Effect of the Invention
[0007] According to the present invention, the net has a water-repellent coating layer on the surface thereof, and the water-repellent coating layer contains water-repellent particles, which effectively prevents snow from accumulating and disperses the force of the snow, thereby deflecting the force that would cause the protective equipment to collapse. As a result, the collapse of the protective equipment due to snow accumulation can be prevented. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a perspective view showing a protective device according to an embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the surface of the net of the protective equipment. [Diagram 3] Photographs showing the results of Example 1 and Comparative Example 1. [Figure 4] Photographs showing the results of Example 2 and Comparative Example 2. [Diagram 5] 6 is a photograph showing the results of Examples 3 to 6 and Comparative Example 3. [Figure 6] Photographs showing the state of Examples 7 to 9 and Comparative Example 4 on December 26, 2022. [Figure 7] Photographs showing the state of Examples 7 to 9 and Comparative Example 4 on January 3, 2023. [Figure 8] Photographs showing the state of Examples 7 to 9 and Comparative Example 4 on January 28, 2023. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] (Embodiment) The embodiments will be described in detail below.
[0010] --Protective equipment-- Fig. 1 shows a seedling protector 1 (hereinafter referred to as "protector") according to an embodiment. The protector 1 is for protecting a seedling T from being eaten by wild animals, and Fig. 1 shows a case in which a seedling T having a height of about 30 to 50 cm is protected. The protector 1 includes a net 2 formed into a cylindrical shape so as to surround the seedling T, at least one support pole 3 that supports the net 2, and a bamboo stake 4 that fixes the net 2 to the ground G.
[0011] The net 2 is not limited as long as it can surround the seedlings T to protect them from damage by wild animals, but the net 2 according to this embodiment is specifically as follows. The net 2 is formed in a cylindrical shape with a tubular axis direction along the extension direction (vertical direction) of the seedlings T. The dimensions of the net 2 are not limited, but the length in the tubular axis direction is about 140 to 200 cm, and the diameter of the tube is about 50 cm.
[0012] The net 2 is formed by intersecting a plurality of wire members extending in the vertical direction and a plurality of wire members extending in the horizontal direction. The mesh (holes) of the net 2 are approximately rectangular, and the size of the mesh (length of one side) is preferably 0.2 mm or more and 1.0 mm or less.
[0013] The wire members of the net 2 are preferably made of a fabric such as a woven fabric, a split cloth, or a nonwoven fabric. Examples of the fibers constituting the wire members of the net 2 include chemical fibers and biodegradable fibers. Examples of chemical fibers include regenerated fibers, semi-synthetic fibers, and synthetic fibers, and examples of synthetic fibers include polypropylene and polyester. Examples of biodegradable fibers include polylactic acid.
[0014] The net 2 may be made by bending an originally rectangular shape into a cylindrical shape so that the long sides overlap, or may be made from a net originally formed into a cylindrical shape. When the protective equipment 1 is installed, the shape of the net 2 may be an inverted cone shape with a narrowed diameter at the bottom to make it difficult for wild animals to insert their noses into it.
[0015] The posts 3 are formed in the shape of rods extending vertically, with their lower portions driven into the ground G. The posts 3 are fixed to the net 2 at one or more points by fixing members 5 made of wire, clips, etc. In this way, the net 2 is supported by the posts 3, and can maintain a state in which it surrounds the seedlings T.
[0016] -Water-repellent coating layer- As shown in Fig. 2, the net 2 has a water-repellent coating layer 6 on its surface. Therefore, the surface of the net 2 is water-repellent. From the viewpoint of particularly effectively suppressing accumulation of snow on the net 2, the contact angle of water with the surface of the net 2 is preferably 130° or more. This contact angle is measured by a tangential method by dropping droplets of ion-exchanged water onto the surface of the net 2 according to the embodiment under conditions of a temperature of 25±5°C and a humidity of 50±10%.
[0017] The water-repellent coating layer 6 contains water-repellent particles 61 and filling particles 62 having a larger average particle diameter than the water-repellent particles 61. The water-repellent coating layer 6 can obtain very high water-repellent performance by containing the water-repellent particles 61 and the filling particles 62 having a larger average particle diameter than the water-repellent particles 61. This is presumably because the water-repellent particles 61 get into between the filling particles 62, and the surface area in which the water-repellent particles 61 can exist is expanded due to the surface irregularities formed by the filling particles 62, and many water-repellent particles 61 are distributed along the surface, thereby enhancing the water-repellent performance of the water-repellent particles 61. In particular, it is preferable that the average particle diameter of the filling particles 62 is 20 times or more larger than that of the water-repellent particles 61.
[0018] -Water-repellent particles- Examples of the water-repellent particles 61 include nanosilica, ungranulated carbon black, and fluoropolymers. The water-repellent particles 61 preferably contain one or both of nanosilica and ungranulated carbon black, and more preferably contain nanosilica from the viewpoint of obtaining a non-black, extremely high water-repellent performance.
[0019] In the present application, "nanosilica" refers to silica particles having an average particle size (primary particle size) of less than 1 μm. Examples of nanosilica include fumed silica, precipitated silica, gel silica, and colloidal silica. Nanosilica preferably contains one or more of these, and more preferably contains fumed silica from the viewpoint of obtaining very high water repellency. Examples of commercially available fumed silica include the Aerosil series manufactured by Nippon Aerosil Co., Ltd.
[0020] Fumed silica includes hydrophilic fumed silica that has not been surface-treated, and hydrophobic fumed silica whose silanol group portion has been chemically surface-treated with silane and / or siloxane. Nanosilica preferably contains one or both of these hydrophilic fumed silica and hydrophobic fumed silica, and more preferably contains hydrophobic fumed silica from the viewpoint of obtaining very high water repellency.
[0021] In the present application, "ungranulated carbon black" refers to carbon black that does not form granules in which primary particles are aggregated. Therefore, in the present application, "ungranulated carbon black" includes finely powdered carbon black that does not contain a granulating agent, finely powdered carbon black that has not been surface-treated for granulation, and finely powdered carbon black that is intentionally free of functional groups containing oxygen and / or hydrogen that contribute to granulation and is substantially free of such functional groups.
[0022] On the other hand, the "ungranulated carbon black" in the present application does not include granular carbon black containing a granulating agent, granular carbon black that has been surface-treated for granulation, or granular carbon black into which functional groups containing oxygen and / or hydrogen that contribute to granulation have been intentionally introduced. However, these granular carbon blacks that have been subjected to a baking treatment or the like to lose their granular form and become fine powder are also included in the "ungranulated carbon black" in the present application. In addition, the ungranulated carbon black in the present application also includes ungranulated carbon nanotubes and ungranulated carbon graphite.
[0023] The ungranulated carbon black is preferably such that no peaks of intensity of HO (-OH), CO (CHO, >CO), or CO (-COOH) are detected when analyzed by gas chromatography mass spectrometry (GCMS analysis) in the analysis temperature range of 50° C. to 800° C. The ungranulated carbon black has an oxygen content due to functional groups of preferably 0.03% by mass or less, more preferably 0.02% by mass or less, and even more preferably 0.01% by mass or less.
[0024] Examples of ungranulated carbon black include acetylene black, channel black, furnace black such as SAF, ISAF, N339, HAF, MAF, FEF, SRF, GPF, ECF, and N234, and thermal black such as FT and MT. The ungranulated carbon black preferably contains one or more of these. From the viewpoint of obtaining very high water repellency, the ungranulated carbon black preferably contains acetylene black. Examples of commercially available ungranulated acetylene black include a powder product manufactured by Denka Co., Ltd. under the trade name Denka Black.
[0025] From the viewpoint of obtaining extremely high water repellency, the average particle diameter (primary particle diameter) of the water repellent particles 61 is preferably 5 nm or more and 100 nm or less, more preferably 10 nm or more and 70 nm or less, and further preferably 15 nm or more and 50 nm or less. The average particle diameter of the water repellent particles 61 is calculated based on measurements by observation with an electron microscope.
[0026] The BET specific surface area of the water-repellent particles 61 is preferably 10 mm 2 / g or more 300mm 2 / g or less, more preferably 20 mm 2 / g or more 200mm 2 / g or less, more preferably 35 mm 2 / g or more 130mm 2 The BET specific surface area of the water-repellent particles 61 is measured based on JIS Z8830:2013.
[0027] -Filled particles- Examples of the filling particles 62 include inorganic particles such as silica particles having an average particle size of 1 μm or more (hereinafter referred to as "large particle size silica"), calcium particles, montmorillonite particles, mica particles, and talc particles; and organic particles such as acrylic resin particles and polyethylene resin particles. The filling particles 62 preferably contain one or more of these, and from the viewpoint of obtaining very high water repellency, it is more preferable that the filling particles 62 contain large particle size silica.
[0028] The large-sized silica includes hydrophilic large-sized silica that has not been surface-treated, and hydrophobic large-sized silica whose silanol group portion has been chemically surface-treated with silane and / or siloxane. The large-sized silica preferably contains one or both of these hydrophilic large-sized silica and hydrophobic large-sized silica, and more preferably contains hydrophilic large-sized silica from the viewpoint of obtaining very high water repellency.
[0029] The average particle diameter of the filling particles 62 is preferably 100 μm or less. In particular, from the viewpoint of obtaining extremely high water repellency, the average particle diameter of the filling particles 62 is preferably 1 μm or more and 50 μm or less, more preferably 2 μm or more and 50 μm or less, and even more preferably 3 μm or more and 5 μm or less. The average particle diameter of the filling particles 62 is measured by a laser diffraction scattering method.
[0030] The filling particles 62 have a larger average particle diameter than the water-repellent particles 61. From the viewpoint of obtaining extremely high water-repellent performance, the average particle diameter of the filling particles 62 is preferably 20 to 250 times, more preferably 30 to 200 times, even more preferably 40 to 100 times, and still more preferably 50 to 70 times the average particle diameter of the water-repellent particles 61.
[0031] The filling particles 62 are preferably porous. From the viewpoint of obtaining a very high water repellency, the BET specific surface area of the filling particles 62 is preferably 150 mm 2 / g or more 700mm 2 / g or less, more preferably 200 mm 2 / g or more 400mm 2 / g or less, more preferably 250 mm 2 / g or more 350mm 2 / g or less. The BET specific surface area of the filling particles 62 is also measured in the same manner as the water-repellent particles 61, based on JIS Z8830:2013.
[0032] From the viewpoint of obtaining extremely high water repellency, the ratio of the BET specific surface area of the filling particles 62 to the BET specific surface area of the water repellent particles 61 is preferably from 2 to 20, more preferably from 3 to 15, and even more preferably from 4 to 10. From the viewpoint of obtaining extremely high water repellency, the BET specific surface area of the filling particles 62 is preferably larger than the BET specific surface area of the water repellent particles 61.
[0033] From the viewpoint of obtaining extremely high water repellency, the mass content of the filling particles 62 in the water repellent coating layer 6 according to the embodiment is preferably greater than the mass content of the water repellent particles 61. The mass ratio of the content of the filling particles 62 to the content of the water repellent particles 61 in the water repellent coating layer 6 according to the embodiment is preferably 1 or more and 18 or less, more preferably 2 or more and 15 or less, and even more preferably 3 or more and 12 or less.
[0034] - Binder resin - The water-repellent coating layer 6 may be composed of only the water-repellent particles 61 and the filling particles 62, but from the viewpoint of enhancing their fixation to the net 2, it is preferable that the water-repellent coating layer 6 further contains a binder resin 63.
[0035] Examples of the binder resin 63 include thermosetting resin, thermoplastic resin, and photocurable resin. Examples of the thermosetting resin include silicone resin, epoxy resin, phenol resin, urea resin, and melamine resin. Examples of the thermoplastic resin include fluororesin, polyethylene resin, polypropylene resin, polyamide resin, polyester resin, and polyurethane resin. Examples of the photocurable resin include epoxy compounds and urethane compounds to which acrylic acid is added. Of these, the binder resin preferably contains at least one of silicone resin and fluororesin, and more preferably contains both of them.
[0036] From the viewpoint of improving the fixation of the water-repellent particles 61 and the filling particles 62 to the net 2 and obtaining high water-repellent performance, it is preferable that the binder resin 63 contains a silicone resin. Examples of the silicone resin include polyalkoxysiloxane, polyalkylsiloxane, polyalkylalkoxysiloxane, polyarylsiloxane, polyarylalkylsiloxane, polyethersiloxane, and the like.
[0037] As the preferable binder resin 63, in addition to the above, an acrylic resin can be mentioned.
[0038] In order to obtain extremely high water repellency, the content of the binder resin 63 in the water-repellent coating layer 6 is preferably 5% by mass or more and 30% by mass or less, more preferably 10% by mass or more and 25% by mass or less, and even more preferably 15% by mass or more and 20% by mass or less.
[0039] Further, the total content of the water-repellent particles 61 and the filling particles 62 relative to 100 parts by mass of the binder resin 63 is preferably 10 parts by mass or more and 40 parts by mass or less, more preferably 15 parts by mass or more and 35 parts by mass or less, and even more preferably 20 parts by mass or more and 30 parts by mass or less, from the viewpoint of increasing their fixation to the net 2 and obtaining very high water repellency. From the same viewpoint, the content of the water-repellent particles 61 relative to 100 parts by mass of the binder resin 63 is preferably 1 part by mass or more and 20 parts by mass or less, more preferably 2 parts by mass or more and 10 parts by mass or less, and even more preferably 3 parts by mass or more and 6 parts by mass or less. From the same viewpoint, the content of the filling particles 62 relative to 100 parts by mass of the binder resin 63 is preferably 5 parts by mass or more and 35 parts by mass or less, more preferably 10 parts by mass or more and 30 parts by mass or less, and even more preferably 15 parts by mass or more and 25 parts by mass or less.
[0040] -wax- From the viewpoint of obtaining extremely high water repellency, the water repellent coating layer 6 preferably contains a wax. As the wax, it is preferable that at least one of a polyolefin wax and an oxidized polyolefin wax is further contained.
[0041] Polyolefin wax is generally a low molecular weight polyolefin having a molecular weight of not more than 10000. Examples of polyolefin wax include polyethylene wax, polypropylene wax, and high density polymerization types and low density polymerization types thereof.
[0042] The oxidized polyolefin wax is a wax obtained by oxidizing a polyolefin wax and introducing polar groups such as carboxyl groups and hydroxyl groups. This oxidized polyolefin wax is generally known as oxidized polyolefin wax and is commercially available. Examples of the oxidized polyolefin wax include ethylene-acrylic acid copolymer wax, ethylene-vinyl acetate copolymer wax, ethylene oxide-vinyl acetate copolymer wax, ethylene-maleic anhydride copolymer wax, propylene-maleic anhydride copolymer wax, and high-density oxidized polyethylene wax. The oxidized polyolefin wax preferably contains one or more of these.
[0043] - Method for forming water-repellent coating layer - The method for forming the water-repellent coating layer 6 according to the above embodiment is, for example, as follows: A water-repellent coating agent containing water-repellent particles 61, filler particles 62, and uncured binder resin 63 is applied to the surface of the net 2 to form the water-repellent coating layer 6 on the surface of the net 2.
[0044] In order to form a uniform water-repellent coating layer 6 that exhibits extremely high water-repellent performance, it is preferable that the water-repellent coating agent further contains an organic solvent that disperses the water-repellent particles 61 and the filling particles 62 and dissolves the uncured binder resin 63.
[0045] Examples of such organic solvents include aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, alcohol solvents, ketone solvents, ester solvents, etc. Examples of aromatic hydrocarbon solvents include benzene, toluene, xylene, etc. Examples of aliphatic hydrocarbon solvents include n-hexane, isohexane, cyclohexane, n-octane, isooctane, decane, dodecane, etc. Examples of alcohol solvents include methanol, ethanol, isopropanol, etc. Examples of ketone solvents include methyl ethyl ketone, methyl isobutyl ketone, etc. Examples of ester solvents include ethyl acetate, isobutyl acetate, etc. It is preferable that the organic solvent contains one or more of these, and from the viewpoint of forming a uniform water-repellent coating layer 6 that exhibits very high water-repellent performance, it is preferable that the organic solvent contains an aromatic hydrocarbon solvent, and more preferably contains toluene and / or hexane.
[0046] Examples of the means for applying the water-repellent coating agent to the surface of the net 2 include spray coating, roller coating, gravure coater coating, die coater coating, lip coater coating, comma coater coating, knife coater coating, reverse coater coating, dip coating, brush coating, etc. Among these, spray coating or dip coating is preferred from the viewpoint of good workability. In addition, when a nonwoven fabric is used as the net 2, dip coating is preferred from the viewpoint of obtaining very high water-repellent performance and excellent abrasion resistance.
[0047] Furthermore, the water-repellent coating layer 6 according to the embodiment can also be obtained, for example, by spray-coating an adhesive onto the surface of the net 2 in advance, and then spray-coating the water-repellent particles 61 and the filling particles 62 on top of that.
[0048] --Action and Effects-- According to this embodiment, the net 2 has a water-repellent coating layer 6 containing water-repellent particles 61 on the surface, and therefore snow can be prevented from adhering to the net 2. As a result, snow can be effectively prevented from accumulating on the net 2, and the protective equipment 1 can be prevented from collapsing. In particular, when the contact angle of water with respect to the surface of the net 2 is 130° or more, the effect of preventing snow from accumulating on the net 2 is further enhanced.
[0049] The reason why the water-repellent coating layer 6 can effectively prevent snow from accumulating on the net 2 is presumed to be as follows. Snow particles or water and snow tend to adhere to each other, so when a small amount of snow or moisture derived from a small amount of snow adheres to the surface of the net 2, more snow tends to adhere to that small amount of snow or moisture. For this reason, it is believed that once a small amount of snow or moisture adheres to the surface of the net 2, snow accumulation is rapidly promoted. In other words, if the water-repellent coating layer 6 can prevent the initial small amount of snow or moisture from adhering to the surface of the net 2, it can also prevent further snow from adhering, and as a result, snow from accumulating on the net 2 can be prevented.
[0050] Furthermore, as will be suggested by the results of the examples described later, when the water-repellent coating layer 6 contains the water-repellent particles 61, accumulation of snow on the net 2 can be extremely effectively suppressed.
[0051] (Other embodiments) In the above embodiment, the water-repellent coating layer 6 contains the water-repellent particles 61 and the filling particles 62, but the present invention is not limited thereto. The water-repellent coating layer 6 only needs to have water repellency. For example, the water-repellent coating layer 6 may contain neither the water-repellent particles 61 nor the filling particles 62, but a fluororesin, silicone resin, acrylic resin, or the like, for imparting water repellency. EXAMPLES
[0052] --Example 1, Comparative Example 1-- In Example 1 and Comparative Example 1, the protective equipment according to the present invention was examined for its effect of suppressing collapse due to accumulation of snow.
[0053] Specifically, in Example 1, the protective equipment according to the present invention was installed on 20 seedlings planted on a mountain with a large amount of snowfall in Tomata-gun, Okayama Prefecture, and each seedling was surrounded by the net of the protective equipment. The water-repellent coating layer of the net was formed as follows. First, a water-repellent coating agent was prepared, which contains toluene as a solvent, 5% by mass of nanosilica (primary particle diameter 30 nm) as water-repellent particles, 5% by mass of large-particle silica (average particle diameter 3 μm) as filling particles, 10% by mass of silicone resin as a binder resin, 0.5% by mass of fluorine resin as a binder resin, and 0.5% by mass of polyolefin wax. Next, the net of each protective equipment was dip-coated with the water-repellent coating agent to perform a water-repellent treatment.
[0054] Comparative Example 1 is the same as Example 1, except that the nets of each protective equipment are not dip-coated with the water-repellent coating agent, i.e., water-repellent treatment is not performed. The installation locations of each protective equipment in Comparative Example 1 are about 10 to 20 m away from the installation locations of each protective equipment in Example 1, but the amount of snowfall at both installation locations is the same.
[0055] The protective equipment of Example 1 and Comparative Example 1 was installed in November 2020. Next, the condition of each seedling and protective equipment was confirmed at each time point in June 2021 and June 2022. Photographs of each seedling and protective equipment taken in June 2022 are shown in FIG.
[0056] The results are shown in Table 1, but are specifically as follows. As of June 2021, only one of the 20 seedlings that had protective equipment installed had collapsed along with the equipment, but the remaining 19 seedlings had not collapsed, and each protective equipment was surrounding each seedling in the same position as when it was first installed, and the purpose of each protective equipment was being achieved, which was to protect the seedling from damage by wild animals. As for the one seedling that collapsed along with the protective equipment, part of the seedling was outside the protective equipment net due to the collapse, and it was in a state where it could not be protected from damage by wild animals. The reason why one seedling collapsed along with the protective equipment was due to the weight of snow that had accumulated on the protective equipment net in winter. As of June 2022, only one more seedling had collapsed along with the protective equipment, and as shown in Figure 3, 18 seedlings and protective equipment had not collapsed.
[0057] [Table 1]
[0058] For Comparative Example 1, the condition of each seedling and protective equipment was confirmed in the same manner as in Example 1. As of June 2021, of the 20 seedlings on which protective equipment was installed, 6 seedlings had collapsed together with the protective equipment, and as of June 2022, all 20 seedlings had collapsed together with the protective equipment, as shown in FIG. 3. At each time point, for the seedlings that had collapsed together with the protective equipment, some of the seedlings were outside the net of the protective equipment due to the collapse, and were in a state where they could not be protected from damage by wild animals.
[0059] From the results of Example 1, it can be seen that the protective gear according to the present invention, in which the net is treated to be water repellent and the surface of the net has a water repellent coating layer containing water repellent particles, is able to suppress the accumulation of snow on the net compared to protective gear in which the net is not treated to be water repellent.
[0060] --Example 2, Comparative Example 2-- In Example 2 and Comparative Example 2, the ease / difficulty of snow adhering to the net was examined. Specifically, in Example 2, a net made of polypropylene and having a mesh and a roughly rectangular shape measuring 250 mm x 500 mm as shown in Fig. 4 was subjected to a water-repellent treatment in the same manner as in Example 1. The net in Comparative Example 2 was the same as the net in Example 2, except that it was not subjected to a water-repellent treatment.
[0061] Each net of Example 2 and Comparative Example 2 was immersed in water, then buried in snow, and pressed from above the snow to facilitate adhesion of the snow to each net. Next, each net was taken out of the snow and spread out in the approximately vertical direction as shown in FIG.
[0062] 4, almost no snow adhered to the net of Example 2, whereas a relatively large amount of snow adhered to the net of Comparative Example 2. As described above, it is understood that the protective equipment according to the present invention is resistant to snow adhesion because the net is treated to be water repellent and the surface of the net has a water repellent coating layer containing water repellent particles.
[0063] --Examples 3 to 6, Comparative Example 3-- In Examples 3 to 6 and Comparative Example 3, the ease / difficulty of snow adhesion due to the water-repellent coating layer was examined when a water-repellent coating layer was formed on an acrylic plate. The acrylic plates of Examples 3 to 6 had a water-repellent coating layer formed on their surfaces due to the water-repellent treatment. On the other hand, the acrylic plate of Comparative Example 3 had not been subjected to the water-repellent treatment and therefore did not have a water-repellent coating layer formed.
[0064] Specifically, in Example 3, a rectangular acrylic plate with a length of 30 cm, a width of 10 cm, and a thickness of 0.3 cm was prepared. In Example 3, a water-repellent coating agent was prepared, which contains toluene as a solvent, 5% by mass of nanosilica (primary particle diameter 30 nm) as water-repellent particles, 5% by mass of large-diameter silica (average particle diameter 3 μm) as filling particles, 10% by mass of silicone resin as a binder resin, 0.5% by mass of fluorine resin as a binder resin, and 0.5% by mass of polyolefin wax. Next, the prepared water-repellent coating agent was applied to the acrylic plate by spray coating and dried. As a result, the surface of the acrylic plate was treated to be water-repellent. The contact angle of water with respect to the surface of the acrylic plate was 140° or more and 150° or less. This contact angle was measured by a tangential method by dropping droplets of ion-exchanged water under conditions of a temperature of 25±5°C and a humidity of 50±10%.
[0065] Next, in Mikata-gun, Hyogo Prefecture, the prepared acrylic plate thus obtained, which had been treated for water repellency, was placed in an environment with snowfall (time: end of December, temperature: about 10°C, snow quality: wet snow (1°C or higher)) with its width oriented horizontally and its length tilted at an angle of 45° from the horizontal. Wet snow was passed through a sieve with 1cm openings directly above the acrylic plate and allowed to fall onto the acrylic plate for 1 minute. The components of the water repellent coating agent are also shown in Table 2.
[0066] [Table 2]
[0067] In Example 4, a water-repellent coating agent was prepared in the same manner as in Example 3, except that in addition to 10% by mass of silicone resin and 0.5% by mass of fluororesin, 6% by mass of acrylic resin was also contained as the binder resin, and no polyolefin wax was contained. The prepared water-repellent coating agent was applied to the surface of an acrylic plate by spray coating and dried. As a result, the surface of the acrylic plate was treated to be water-repellent, and the contact angle measured by the same method as in Example 3 was 130° or more and 140° or less. Next, wet snow was removed from the water-repellent treated acrylic plate obtained in this manner under the same conditions as in Example 3.
[0068] In Example 5, a water-repellent coating agent was prepared containing toluene as a solvent, 5 mass% fluoropolymer particles as water-repellent particles, 10 mass% silicone resin as a binder resin, 0.5 mass% fluororesin as a binder resin, and 0.5 mass% polyolefin wax. Next, the prepared water-repellent coating agent was spray-coated and dried on an acrylic plate having the same configuration as in Example 3. As a result, the surface of the acrylic plate was treated to be water-repellent, and the contact angle measured by the same method as in Example 3 was 135° or more and 154° or less. Next, wet snow was removed from the water-repellent acrylic plate obtained in this way under the same conditions as in Example 3.
[0069] In Example 6, a water-repellent coating agent was prepared that was composed of 70% by mass of water as a solvent and 30% by mass of fluororesin. The water-repellent coating agent of Example 6 did not contain water-repellent particles, unlike Examples 3 to 5. The prepared water-repellent coating agent was applied by spray coating to an acrylic plate having the same configuration as Example 3, and then dried. As a result, the surface of the acrylic plate was treated to be water-repellent, and the contact angle measured by the same method as Example 3 was 120° or more and 130° or less. Next, wet snow was removed from the water-repellent acrylic plate obtained in this manner under the same conditions as Example 3.
[0070] In Comparative Example 3, wet snow was removed from an acrylic plate that had not been subjected to a water-repellent treatment under the same conditions as in Example 3. The contact angle of water with respect to the surface of the acrylic plate in Comparative Example 3 was less than 90°.
[0071] FIG. 5 is a photograph of the acrylic plates of Examples 3 to 6 and Comparative Example 3 after the snow was removed as described above. For each acrylic plate, those with no snow or very little snow on the surface were rated as ◯, and those with a lot of snow on the surface were rated as ×. As can be seen from FIG. 5, the acrylic plates of Examples 3 to 5 had almost no snow on the surface (rated ◯), whereas the acrylic plates of Example 6 and Comparative Example 3 had so much snow that it covered most of the surface (rated ×). Although snow was accumulated on the acrylic plate of Example 6, there were some parts of the surface that were not covered with snow, and the amount of snow that had accumulated was less than that of the acrylic plate of Comparative Example 3.
[0072] What is noteworthy about the results of Examples 3 to 6 and Comparative Example 3 is that when the water-repellent coating agent contains water-repellent particles and the contact angle is 130° or more, as in Examples 3 to 5, accumulation of snow on the acrylic plate surface can be suppressed extremely effectively. In Example 6, although the acrylic plate surface was treated to be water-repellent, the effect of suppressing snow accumulation was significantly smaller than in Examples 3 to 5.
[0073] --Examples 7 to 9, Comparative Example 4-- In Examples 7 to 9 and Comparative Example 4, the tendency of the protective equipment according to the present invention to tip over when snow accumulates was examined. Specifically, in Example 7, a water-repellent coating agent similar to that in Example 3 was first prepared. Next, the prepared water-repellent coating agent was dip-coated onto the net of the protective equipment to make the net water-repellent. The wire members of the net were made of polypropylene.
[0074] Example 8 was the same as Example 7, except that the net of the protective equipment was spray-coated with a water-repellent coating agent prepared in the same manner as in Example 3 to make the net water-repellent.
[0075] Example 9 was the same as Example 7, except that the net of the protective equipment was dip-coated with a water-repellent coating agent prepared in the same manner as in Example 6 to make the net water-repellent.
[0076] Comparative Example 4 is the same as Example 7, except that the net of the protective equipment was not subjected to a water repellent treatment.
[0077] The contact angles of water on the net surfaces of the protective gears according to Examples 7 to 9 and Comparative Example 4 were 137°, 141°, 120°, and less than 88°, respectively, as shown in Table 3. The contact angles were measured by the tangential method using droplets of ion-exchanged water dropped under conditions of a temperature of 25±5°C and a humidity of 50±10%.
[0078] [Table 3]
[0079] The obtained protective equipment according to Examples 7 to 9 and Comparative Example 4 was installed on a plateau with a lot of snowfall in Yabu City, Hyogo Prefecture on December 26, 2022. There were five protective equipment according to Example 7, Example 9, and Comparative Example 4, and four protective equipment according to Example 8. The state of each installed protective equipment was confirmed at each point in time on January 3, 2023 and January 28, 2023. Photographs of the protective equipment taken at each point in time are shown in Figures 6 to 8. In Figures 6 to 8, the five protective equipment according to Example 7 are distinguished and displayed using the alphabets a to e, such as "Example 7a", "Example 7b", ..., "Example 7e", and the multiple protective equipment according to Examples 8 to 9 and Comparative Example 4 are also displayed using the alphabets a to e in the same manner.
[0080] As shown in Figure 6, each piece of protective equipment was upright as of December 26, 2022. As shown in Figures 7 and 8, snow accumulated on each piece of protective equipment over time. Specifically, the following is true:
[0081] First, focusing on the protective equipment according to Comparative Examples 4a to 4e, in which the net was not treated with a water repellent treatment, as shown in Figure 7, as of January 3, 2023, each protective equipment was upright, but a lot of snow had already accumulated. As shown in Figure 8, as of January 28, 2023, the protective equipment according to Comparative Examples 4a to 4d was buried in snow accumulated on the ground as a result of being significantly tilted by the weight of the snow.
[0082] Next, when focusing on the protective equipment according to Examples 7a to 7e, Examples 8a to 8d, and Examples 9a to 9e in which the net was treated for water repellency, the amount of snow accumulated on these protective equipment was relatively small even after the passage of time. However, the protective equipment according to Examples 9a to 9e in which the water repellent coating layer did not contain water repellent particles had a larger amount of accumulated snow than the protective equipment according to Examples 7a to 7e and Examples 8a to 8d in which the water repellent coating layer contained water repellent particles. As a result, as shown in FIG. 8, the protective equipment according to Examples 9a, 9b, and 9c had a large inclination due to the weight of snow and was buried in the snow accumulated on the ground.
[0083] From the above, it can be seen that by treating the net to be water-repellent and having a water-repellent coating layer, it is possible to prevent the protective equipment from collapsing due to snow accumulation, and that this effect is particularly high when the water-repellent coating layer contains water-repellent particles. [Industrial Applicability]
[0084] The present invention is useful as a protection device for protecting seedlings from wild animals. [Explanation of symbols]
[0085] T sapling G ground 1 Seedling protection equipment 2. Internet 3 pillars 4 stakes 5 Fixing material 6 Water-repellent coating layer 61 Water-repellent particles 62 Filled particles 63 Binder Resin
Claims
1. A seedling protector comprising a tubular net surrounding a seedling, the net having a water-repellent coating layer on its surface.
2. The seedling protector according to claim 1, The water-repellent coating layer comprises water-repellent particles.
3. The seedling protector according to claim 2, The water-repellent coating layer further contains filling particles having an average particle diameter at least 20 times larger than that of the water-repellent particles.
4. The seedling protector according to any one of claims 1 to 3, A seedling protector, wherein the contact angle of water with the surface of the net is 130° or more.
5. The seedling protector according to claim 1, The water-repellent coating layer comprises a wax.
Citation Information
Patent Citations
Protective device for young plant etc