Sterilization paper, and sterilization package

The sterile paper with a thermoplastic resin and high-melting-point wax adhesive layer maintains easy-peelability and prevents substrate tearing, addressing contamination issues in high-temperature storage.

JP2024153140APending Publication Date: 2024-10-29OJI HLDG CORP

Patent Information

Application Number
JP2023066798
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Sterile paper used in medical packaging often loses its easy-peel properties due to high-temperature storage, leading to substrate failure and re-contamination risks.

Method used

A breathable base material with a thermal adhesive layer containing a thermoplastic resin and a wax with a melting point of 60°C or higher, ensuring easy-peelability and preventing substrate destruction even after high-temperature storage.

Benefits of technology

Maintains easy-peel properties and prevents substrate tearing, reducing contamination risks in high-temperature environments, enhancing cleanliness in medical settings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153140000001_ABST
    Figure 2024153140000001_ABST
Patent Text Reader

Abstract

To provide sterilization paper and a sterilization package which can improve easy peelability and high temperature environment stability.SOLUTION: Sterilization paper includes an air permeable base material 22, and a heat adhesive layer 23 on one surface of the air permeable base material, wherein the adhesive layer contains a thermoplastic resin and a wax, a melting point of the wax is 60°C or higher, and Oken type air permeability measured according to JIS P 8121:2012 is 700 seconds or less. Preferably, 1 to 20 pts.mass of the wax is contained with respect to 100 pts.mass of the thermoplastic resin, and the wax contains one or more kinds of carnauba waxes.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to sterilization paper and sterilization packaging. [Background technology]

[0002] Instruments used in surgery, treatment, etc. are sterilized before use while being stored in a sterile package. Sterilization methods implemented in hospitals, etc. include gas sterilization, high-pressure steam sterilization, radiation sterilization, etc., after sealing the objects to be sterilized, such as scalpels and forceps, in a sterile package. In gas sterilization, the pressure in a pressure-resistant container containing the sterile package is reduced, and then ethylene oxide gas (EOG) or the like is filled in the container, thereby permeating the sterile package and sterilizing it. In high-pressure steam sterilization, the sterile package is exposed to high-temperature steam using an autoclave or the like, and sterilized by repeatedly reducing and pressurizing the pressure. In radiation sterilization, the sterile package is irradiated with radiation to sterilize it. Of these sterilization methods, high-pressure steam sterilization and gas sterilization are widely used because the cost required for sterilization is low and the work required for sterilization is simple.

[0003] On the other hand, a sterile package containing an object to be sterilized is stored until it is to be used in surgery, etc., and is opened when it is to be used in surgery, etc. Therefore, in order to make it easy for a doctor or practitioner wearing gloves to open the sterile package, two thin rectangular sheets or films are peelably bonded to each other on the front and back, or a thin sheet having an easy-to-tear property that makes it easy to tear and open is used. When opening the package, a peel-open method in which one thin sheet is peeled from the other thin sheet, or a tear-open method in which two thin sheets are torn apart is generally used.

[0004] When the adherend is peeled off from the sterilized paper in the above-mentioned peel-open sterilization packaging, paper powder and the like may scatter due to the destruction of the base material of the sterilized paper. Paper powder and dust (lint) caused by the destruction of the base material may cause recontamination of the sterilized object such as medical instruments after sterilization. Therefore, it is required that the sterilized paper has improved easy peelability, which is the property that makes it easy to peel off, and that the scattering of lint during peeling is suppressed. The demand for improved easy peelability is particularly prominent in medical settings where a high level of cleanliness is required, such as inside operating rooms and before operating rooms.

[0005] As an example of the above-mentioned sterile packaging body, for example, the configurations described in Patent Documents 1 to 8 are known. The sterile packaging body described in Patent Document 1 has a thermoplastic resin layer on one side of a base paper. The sterile packaging body described in Patent Document 2 is obtained by coating an acrylic acid-based copolymer on a base paper containing an aluminate. The sterile packaging body described in Patent Document 3 has a thermoplastic resin layer containing a hollow polymer pigment on the surface of the base paper. The sterile packaging body described in Patent Document 4 is obtained by impregnating a low-air permeability base paper of 10 seconds or less with an impregnating agent mainly composed of polyvinyl alcohol. The sterile packaging body described in Patent Document 5 has a coating layer on at least one side of a base paper, the coating layer being mainly crosslinked polyvinyl alcohol, and has a dry weight of 0.1 g / m after coating. 2 More than 6g / m 2 The sterilized packaging material described in Patent Document 6 is obtained by impregnating a base paper with low air permeability of 20 seconds or less with an impregnating agent mainly composed of an acrylic copolymer. The sterilized packaging material described in Patent Document 7 is a base paper having a thermoplastic resin layer containing a polyolefin resin, an inorganic material, and a surfactant on one side thereof. Patent Document 8 is a sterilized paper and a sterilized packaging material having a heat-sealing layer containing a thermoplastic resin and fatty acid calcium. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2001-122348 A [Patent Document 2] Japanese Patent Application Publication No. 9-290808 [Patent Document 3] JP 2010-196188 A [Patent Document 4] JP 2001-200493 A [Patent Document 5] JP 2004-84131 A [Patent Document 6] JP 2002-173900 A [Patent Document 7] JP 2008-105374 A [Patent Document 8] JP 2022-68392 A Summary of the Invention [Problem to be solved by the invention]

[0007] The above-mentioned easy peel property may deteriorate depending on the storage conditions of the sterilized paper before heat sealing. In particular, storage of the sterilized paper under high temperature conditions may increase the peel strength and cause the substrate to break. The present invention provides a sterilized paper and a sterilized package that can maintain the easy peel property even after high temperature storage. [Means for solving the problem]

[0008] The present invention, which solves the above problems, has the following configuration. (1) A sterilized paper comprising a breathable substrate and a thermal adhesive layer on one side of the breathable substrate, the adhesive layer containing a thermoplastic resin and a wax, the melting point of the wax being 60°C or higher, and the Oken air permeability measured in accordance with JIS P 8121:2012 being 700 seconds or less. (2) The sterilized paper according to (1), wherein the wax is contained in an amount of 1 to 20 parts by mass per 100 parts by mass of the thermoplastic resin. (3) The sterilized paper according to (1) or (2), wherein the wax comprises one or more types of carnauba wax. (4) The sterilized paper according to any one of (1) to (3), wherein the thermoplastic resin has a polyolefin structure in its molecule. (5) The sterilized paper according to any one of (1) to (4), wherein the 180° peel strength when the thermal adhesive layer and a polyvinyl chloride film are thermocompression-bonded under conditions of 150°C, 0.1 MPa, and 1 second, and peeled at a peel speed of 300 mm / min in accordance with JIS P 8113:2006, is 0.5 N / 15 mm or more. (6) The sterilized paper according to any one of (1) to (5), wherein the breathable substrate contains a polyacrylamide resin. (7) The sterilized paper according to any one of claims 1 to 6, which is adhered to a plastic material or a plastic material surface of a plastic-laminated paper by the thermal adhesive layer. (8) A sterilization package having, at least as a part thereof, the sterilization paper according to any one of (1) to (7). (9) A sterilization package having a thermally sealed portion formed by overlapping and thermocompressing at least a portion of the thermal adhesive layer of the sterilization paper according to any one of (1) to (7) with at least a portion of another substrate. (10) The sterilization package according to (9), wherein the heat-sealed portion has a 180° peel strength of 0.5 to 15 N / 15 mm when peeled at a peel speed of 300 mm / min in accordance with JIS P 8113:2006. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a cross-sectional view showing a cross-sectional structure of one embodiment of a sterilization package. [Explanation of symbols]

[0010] S... Space, 11... Sterilized package, 11E... Heat bonding part, 21... Sterile paper, 22... Breathable base material, 23... Heat adhesive layer, 31... Adherent, 31E... One end. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the sterilization paper and the sterilization packaging body will be described with reference to FIG. [Sterile packaging 11] The sterilization package 11 comprises a sterilization paper 21 and an adherend 31. The sterilization paper 21 comprises an air-permeable substrate 22 and a thermal adhesive layer 23 located on one side of the air-permeable substrate 22.

[0012] The adherend 31 is, for example, a wrapping paper, a laminated paper, a film, a molded container for sterilization, or the like. The material constituting the adherend 31 is at least one resin selected from the group consisting of polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate, polyvinyl chloride, polyvinylidene chloride, polystyrene, ethylene-vinyl acetate copolymer resins, and ethylene-acrylic copolymer resins. The adherend 31 may also be made of a composite material in which these resins are laminated with other materials. The material constituting the adherend 31 may be a mixture of two or more different resins. The adherend 31 can also be embodied as a laminate in which two or more different resins form separate layers.

[0013] The sterilization package 11 has a heat sealed portion 11E. The thermally bonded portion 11E has a ring shape in which the sterilization paper 21 and the adherend 31 are thermally bonded to each other.

[0014] The sterilization package 11 has a space S surrounded by the thermally bonded portion 11E between the sterilization paper 21 and the adherend 31. The space S of the sterilization package 11 is a space for accommodating an object to be sterilized, such as a medical instrument. For example, the sterilization package 11 accommodates an object to be sterilized in the space S, and in this state, is subjected to a sterilization process such as autoclaving, ethylene oxide gas (EOG) sterilization, electron beam sterilization, or gamma ray sterilization. When the sterilized object to be sterilized is used, one end 31E of the adherend 31 separated from the sterilization paper 21 is pulled up toward the breathable substrate 22, and the adherend 31 is peeled off from the sterilization paper 21. Then, the space S is released, and the object to be sterilized is exposed to the space where the sterilization package 11 is located. The thermally bonded layer 23 can be formed on one side of the breathable substrate 22 where the adherend 31 is located, and on the opposite side.

[0015] [Thermal adhesive layer 23] The thermal adhesive layer 23 contains at least a thermoplastic resin and a wax having a melting point of 60° C. or higher. The thermoplastic resin preferably contains a polyolefin structure. Examples of the polyolefin structure include polyethylene and polypropylene. Examples of commercially available thermoplastic resins that can be used in the present invention include the DIC Seal E series manufactured by DIC Graphics and the Chemipearl series manufactured by Mitsui Chemicals.

[0016] Examples of the wax include paraffin wax, natural oil-based waxes derived from animals and plants such as carnauba wax, and synthetic waxes such as polyethylene wax. The wax may be used alone or in combination of two or more kinds. Among these, carnauba wax is preferably used. The wax has a melting point of 60° C. or higher, more preferably 70° C. or higher, and even more preferably 80° C. or higher.

[0017] The wax is preferably 1 to 20 parts by mass, more preferably 3 to 15 parts by mass, and even more preferably 5 to 50 parts by mass, based on 100 parts by mass of the thermoplastic resin. If it is more than 20 parts by mass, the peel strength decreases and the adhesiveness is affected. If it is less than 1 part by mass, the effect is difficult to obtain.

[0018] The thermal adhesive layer may contain other materials within the scope of the invention, such as dispersants, water retention agents, defoaming agents, and other auxiliary agents, various inorganic pigments, and organic pigments.

[0019] The thermal adhesive layer 23 is obtained, for example, by applying a thermal adhesive layer paint to one surface (the upper surface in the figure) of the breathable substrate 22 and drying the applied thermal adhesive layer paint. The thermal adhesive layer paint heat sealant contains a heat sealant, wax, other materials and a liquid medium. In addition to the one surface of the breathable substrate 22, the thermal adhesive layer may also have another thermal adhesive layer 23 on the opposite surface. The thermal adhesive layer paint may be a water-based paint or a solvent-based paint.

[0020] The coating method of the thermal adhesive layer can be any of various known wet coating methods. For example, an on-machine size press device of a papermaking machine, a transfer roll coater (such as a shim sizer or gate roll coater), or a spray device can be used. In addition, in the off-machine type device, a general coating device such as a blade coater, an air knife coater, a roll coater, a reverse roll coater, a shim sizer, a gate roll coater, a bar coater, a curtain coater, a slot die coater, a gravure coater, a champlex coater, a brush coater, a two-roll coater, a bill blade coater, or a short dwell coater can be used. From the viewpoint of reliably suppressing contamination of the equipment, it is preferable to use an air dryer or an infrared heater that does not come into contact with the coating surface as the drying equipment for the thermal adhesive layer paint. In addition, it is also possible to use a direct contact method of the coating surface using a cylinder dryer as the drying equipment for the thermal adhesive layer paint.

[0021] The amount of the thermal adhesive layer coating applied is, for example, 0.1 g / m 2 More than 20g / m 2 Less than 0.5 g / m 2 More than 12g / m 2 More preferably, 1.0 g / m or less 2 More than 7.0g / m 2 The coating weight of the thermal adhesive layer paint is adjusted to the following range: 0.1 g / m 2 When the coating amount is 20 g / m or more, it is possible to ensure the adhesive strength required for the thermal adhesive layer 23. 2 If it is equal to or less than this, the breathability required for the sterilization treatment of the sterilization package is ensured.

[0022] The inclusion of a thermoplastic resin and a wax in the thermal adhesive layer provides sufficient adhesive strength to the adherend and allows easy peeling between the breathable substrate 22 and the thermal adhesive layer 23, improving the easy peelability when opening the sterilized package 11. After peeling, the thermal adhesive layer 23 transfers to the adherend 31, making it easy to visually confirm that the thermal adhesive layer 23 is located on the adherend 31, and therefore that the adherend 31 has been peeled off from the sterilized paper 21.

[0023] [Breathable substrate 22] The breathable substrate 22 includes, for example, a paper substrate and an undercoat layer that is provided as necessary. The paper substrate is obtained by papermaking of a papermaking raw material that includes a pulp slurry. The pulp used in the pulp slurry is, for example, wood pulp or non-wood pulp. The wood pulp is, for example, at least one type selected from the group consisting of softwood pulp and hardwood pulp. The cooking method and bleaching method of the wood pulp are not particularly limited. The non-wood pulp is, for example, at least one type selected from the group consisting of hemp pulp, kenaf pulp, and bamboo pulp. The pulp slurry can include materials other than pulp fibers as secondary materials, such as rayon fibers, nylon fibers, and other heat-sealing fibers.

[0024] The pulp slurry is obtained by beating the pulp in the presence of water. As the method for beating the pulp and the beating device used therein, for example, a double disk refiner (DDR) having high beating efficiency is preferably used. The beating of the pulp is carried out so that the freeness of the pulp measured in accordance with JIS P 8121-2:2012 (hereinafter also referred to as "standard freeness") is 250 mL or more and 700 mL or less, more preferably 250 mL or more and 600 mL or less, and even more preferably 300 mL or more and 500 mL or less. When the standard freeness of the pulp is 250 mL or more, it is possible to ensure the air permeability of the paper. Also, when the standard freeness of the pulp is 250 mL or less, it is possible to improve the strength of the paper and improve the easy peel property.

[0025] Generally, the relationship between pulp beating and paper strength is that if the beating is not advanced enough, the paper strength is difficult to obtain, and this is thought to be because the pulp fibers are weakly entangled and there are few points of interfiber bonding (hydrogen bonds), and the paper strength improves by advancing the beating to a certain extent. On the other hand, if the beating is advanced, the pulp fibers become more entangled and the number of points of interfiber bonding increases, so that the paper strength is obtained but the voids in the fibers decrease and the air permeability of the paper base material decreases. In this regard, if the standard freeness of the pulp is in the range of 250 mL to 700 mL, it is possible to sufficiently increase the paper strength while maintaining the air permeability of the paper base material and thus the breathable base material 22, and as a result, it is possible to further improve the easy peel suitability of the sterilized paper 21.

[0026] The pulp slurry obtained by beating can be used as a papermaking raw material prepared by adding various internal additives for papermaking. The internal additives include, for example, sizing agents, paper strength agents, wet strength agents, aluminum sulfate, cationic starch, and other fixing agents. In addition to these, retention aids, defoamers, fillers, colorants, and other internal additives can be arbitrarily added to the papermaking raw material.

[0027] The paper strength enhancer includes at least one selected from, for example, polyacrylamide resin, cationic starch, and polyvinyl alcohol. Among these paper strength enhancers, by adding a polyacrylamide resin-based paper strength enhancer, it is possible to more effectively improve the strength of the breathable base material and further increase the easy peel property. In order to exhibit the paper strength enhancing effect after the addition of the paper strength enhancer, the mass average molecular weight is preferably 2 million (Mw) or more. In addition, in terms of the operation of adding the paper strength enhancer, a suitable viscosity is obtained and addition is easy, so the mass average molecular weight is preferably 10 million (Mw) or less. The mass average molecular weight of the polyacrylamide resin is a polyethylene oxide equivalent value measured by gel permeation chromatography (GPC). In addition, the polyacrylamide resin as the paper strength enhancer can be, for example, anionic, cationic, amphoteric, or nonionic polyacrylic resin, and among these, it is particularly preferable to use an amphoteric polyacrylamide resin. The sizing agent includes at least one selected from the group consisting of, for example, alkenyl succinic acid, alkyl ketene dimer, and rosin, and the wet strength agent includes at least one selected from the group consisting of, for example, epichlor resin and melamine resin.

[0028] It is also possible to apply a primer, which is a coating liquid containing a polyacrylamide resin, to at least one surface of the breathable substrate. By applying the primer, it is possible to further improve the easy peeling property. When the primer is applied to only one surface of the breathable substrate, the primer is applied to the surface of the breathable substrate on which the thermal adhesive layer 23 is provided. The primer may be applied to both one surface of the breathable substrate and the opposite surface.

[0029] The paper base material of the breathable substrate 22 is obtained, for example, by making a prepared papermaking raw material by a standard method. The basis weight of the breathable substrate 22 can be appropriately set according to the basis weight of the paper base material and the amount of the undercoat applied.

[0030] The undercoat agent includes a polyacrylamide resin. The polyacrylamide resin is a polymer in which (meth)acrylamide units are repeated. (Meth)acrylamide is a general term for acrylamide and methacrylamide. The polyacrylamide resin may have either an acrylamide unit or a methacrylamide unit, or may have both. The polyacrylamide resin may have units other than (meth)acrylamide units.

[0031] The polyacrylamide resin contained in the undercoat agent is, for example, anionic polyacrylamide resin, cationic polyacrylamide resin, amphoteric polyacrylamide resin, nonionic polyacrylamide resin. These undercoat agents are used as paper strength agents in the papermaking field. The polyacrylamide resin may be used alone or in combination of two or more. In terms of availability, anionic polyacrylamide resin is preferred.

[0032] The anionic polyacrylamide resin contains an anionic functional group such as a carboxy group, a sulfonic acid group, a phosphoric acid group, or a salt thereof, etc. The anionic polyacrylamide resin is, for example, a copolymer of (meth)acrylamide and an anionic functional group-containing monomer such as acrylic acid, or a partial hydrolyzate of poly(meth)acrylamide.

[0033] The mass average molecular weight (Mw) of the polyacrylamide resin contained in the undercoat agent is preferably 50,000 or more and 2,000,000 or less, more preferably 50,000 or more and 500,000 or less, and even more preferably 50,000 or more and 300,000 or less. If the mass average molecular weight of the polyacrylamide resin contained in the undercoat layer is 50,000 or more and 2,000,000 or less, the effect of suppressing fuzzing on the surface of the breathable substrate 22 due to peeling of the adherend 31 is more excellent. If the mass average molecular weight is 50,000 or more, the effect of suppressing fuzzing on the surface of the breathable substrate 22 when the thermal adhesive layer 23 is peeled off is easily obtained. If the mass average molecular weight is 2,000,000 or less, the low viscosity required for application of the undercoat agent can be sufficiently obtained, and the preparation and application of the undercoat agent are easy. In addition, the concentration of the polyacrylamide resin contained in the undercoat agent can be increased within the desired viscosity range, and the desired application amount is easily obtained. The mass average molecular weight of the polyacrylamide resin is a polyethylene oxide equivalent value measured by gel permeation chromatography (GPC).

[0034] The liquid medium contained in the undercoat agent is preferably one that dissolves the polyacrylamide resin, for example, water. The undercoat agent can also contain other components other than the polyacrylamide resin, as long as the easy peeling property is not impaired. The other components are, for example, water-soluble polymer compounds, aqueous polymer compounds, release agents, defoamers, dispersants, wetting agents, colored dyes, colored pigments, and white pigments, and any one of these may be used alone or in combination of two or more. Examples of water-soluble polymer compounds are starch, modified starch, polyvinyl alcohol, modified polyvinyl alcohol, hydroxyethyl cellulose, methyl cellulose, carboxymethyl cellulose, gelatin, casein, gum arabic, diisobutylene-maleic anhydride copolymer salt, and styrene-maleic anhydride copolymer salt. Examples of aqueous polymer compounds are styrene-butadiene copolymer emulsion, acrylic acid ester copolymer emulsion, urethane resin, urea resin, styrene-acrylic resin emulsion, and ethylene-acrylic resin emulsion.

[0035] The content (concentration) of polyacrylamide resin contained in the primer is preferably 50% by mass or more and 100% by mass or less, and more preferably 80% by mass or more and 100% by mass or less, based on the total solids content (100% by mass) in the primer. If the polyacrylamide resin content is 50% by mass or more, the easy peel suitability of the sterilized paper 21 can be further improved. The total solids content is the total amount excluding the liquid medium from the primer, and if other components other than the polyacrylamide resin are contained, it is the sum of the polyacrylamide resin and the other components.

[0036] The amount of the undercoat applied to the breathable substrate is appropriately set according to the content of polyacrylamide resin contained in the undercoat. The amount of the undercoat applied to the surface of the breathable substrate on which the thermal adhesive layer 23 is located is 0.05 g / m2, calculated as the amount of polyacrylamide resin. 2 More than 20g / m 2 It is preferable that the content is 0.1 g / m or less. 2 More than 15g / m 2 More preferably, it is 0.2 g / m or less. 2 More than 10g / m 2 It is more preferable that the coating amount of the polyacrylamide resin is 0.05 g / m or less. 2 If the amount of polyacrylamide resin applied is more than 20 g / m, the breathable substrate 22 and the thermal adhesive layer 23 are easily peeled off when the adherend 31 is peeled off from the sterilized paper 21, and the surface of the breathable substrate 22 is not easily frayed or the breathable substrate 22 is not easily damaged due to the peeling. 2 If the thickness is less than this, uneven adhesion can be suppressed when heat sealing the sterilization paper 21, and for example, the undercoat agent can be applied approximately uniformly to the entire surface of the breathable substrate on which the thermal adhesive layer 23 is located. On the other hand, the undercoat agent may be applied in a predetermined pattern to the surface of the breathable substrate on which the thermal adhesive layer 23 is provided, for example.

[0037] The components of the undercoat layer may contain other components besides polyacrylamide resin. The other components are, for example, at least one selected from the group consisting of starch, resins such as polyvinyl alcohol and styrene-butadiene resin, and pigments such as kaolin, talc, calcium carbonate, and white carbon. The polyacrylamide resin contained in the undercoat applied to one side may be, for example, the same as the polyacrylamide resin contained in the undercoat applied to the other side, or may be different from each other. When the undercoat is applied to the other side of the paper substrate, the amount of the undercoat applied is, for example, 0.01 g / m2 converted into the solid content. 2 More than 20g / m 2 Less than or equal to 0.01 g / m 2 More than 5g / m 2 It is preferable that the content is 0.01 g / m or less. 2 More than 3g / m 2 More preferably, it is 0.1 g / m or less. 2 More than 2g / m 2 It is more preferable that the coating amount of the primer is 20 g / m or less. 2 If the amount is less than this, the air permeability of the sterilized paper 21 can be maintained at a good level. In addition, by adjusting the amount of the undercoat applied on the other side of the paper substrate in this manner, it becomes easy to appropriately adjust the concentration of the polyacrylamide resin on one side, the other side, and the intermediate between the one side and the other side of the paper substrate. When applying the undercoat to each of the one side and the other side of the paper substrate, for example, it is preferable to set the ratio of the amount applied on the one side to the amount applied on the other side to 3:7 to 7:3. This ratio of the amount applied makes it easier to make the concentration of the polyacrylamide resin in the breathable substrate higher on the one side and the other side of the breathable substrate than the intermediate between them. In addition, from the viewpoint of reducing the manufacturing cost of the sterilized paper 21, a case in which the undercoat is not applied to the other side of the paper substrate can be adopted as an example of a preferred embodiment.

[0038] The undercoat agent can be applied by various known wet coating methods. The undercoat agent can be applied by, for example, an on-machine size press device of a papermaking machine, a transfer roll coater (such as a shim sizer or a gate roll coater), a spray device, or the like. In addition, in the off-machine type device, a general coating device, such as a blade coater, an air knife coater, a roll coater, a reverse roll coater, a shim sizer, a gate roll coater, a bar coater, a curtain coater, a slot die coater, a gravure coater, a champlex coater, a brush coater, a two-roll coater, a bill blade coater, a short dwell coater, or the like, can be used. From the viewpoint of improving operability and productivity, it is preferable to use an on-machine type for applying and drying the undercoat agent. The type of the papermaking machine for making the paper substrate is preferably one equipped with an on-machine coater, such as a fourdrinier papermaking machine, a short wire papermaking machine, or a cylinder papermaking machine. The content of the polyacrylamide resin in the breathable substrate 22 is, for example, not less than 1.0% by mass and not more than 30% by mass.

[0039] The basis weight of the breathable substrate 22 is, for example, 30 g / m 2 It is preferable that the thickness is 40 g / m or more. 2 More preferably, it is 45 g / m or more. 2 It is more preferable that the basis weight of the breathable substrate 22 is 30 g / m or more. 2 If the thickness is more than this, the breathable substrate 22 is likely to have a strength that can withstand peeling of the adherend 31 from the breathable substrate 22, and the breathable substrate 22 is less likely to break during peeling. In addition, the occurrence of pinholes is also suppressed, which is preferable from the viewpoint of bacterial barrier properties.

[0040] The upper limit of the basis weight of the breathable base material 22 is not particularly limited, but from the viewpoint of obtaining breathability during sterilization treatment, it is set to 300 g / m 2 It is preferable that the thickness is less than 250 g / m 2 Less than 200 g / m is more preferable. 2 The following is even more preferable: The basis weight of the breathable substrate 22 and the paper substrate is measured in accordance with, for example, JIS P 8124:2011.

[0041] The density of the breathable substrate 22 is, for example, 0.60 g / cm 3 More than 1.20g / cm 3 It is preferable that the density is 0.70 g / cm or less. 3 More than 1.10g / cm 3 It is more preferable that the density of the breathable substrate 22 is 0.60 g / cm or less. 3 If the density of the breathable substrate 22 is 1.20 g / cm or more, it is easy to obtain a strength that can withstand easy peeling, and the breathable substrate 22 is less likely to break during peeling. 3 The density of the breathable substrate 22 can be calculated from the measured thickness and basis weight by measuring the thickness in accordance with, for example, JIS P 8118:1998.

[0042] [Sterile paper 21] The sterilized paper 21 preferably has an Oken air permeability of, for example, 700 seconds or less, more preferably 500 seconds or less, and particularly preferably 300 seconds or less, as measured in accordance with JIS P 8117:2009. If the sterilized paper 21 has an Oken air permeability in this range, the air permeability of the sterilized paper 21 can be effectively improved. On the other hand, the lower limit of the Oken air permeability can be set to, for example, 5 seconds. The Oken air permeability of the sterilized paper 21 can be adjusted by appropriately selecting, for example, the freeness of the pulp, the basis weight of the breathable base material 22, the amount of application of the undercoat agent, and the like.

[0043] The thermal adhesive surface of the sterilized paper 21, which is the surface of the thermal adhesive layer 23, is preferably, for example, 50 seconds or more in terms of Oken smoothness measured in accordance with JIS P 8155: 2010, since this reduces the variation in seal strength and allows for short-term heating. The smoothness of the thermal adhesive surface can be adjusted by subjecting the breathable substrate 22 to a smoothing treatment by any of various known methods, or by forming the thermal adhesive layer 23 and then subjecting it to a smoothing treatment.

[0044] The sterilized package 11 obtained by thermally bonding the sterilized paper 21 and the adherend 31 is preferably adjusted to have a peel strength of, for example, 0.5 N / 15 mm or more and 15 N / 15 mm or less when the adherend 31 is peeled at 180° at a peel speed of 300 mm / min in accordance with JIS P 8113:2006. If the sterilized paper 21 has a peel strength in this range, a sterilized package 11 with an excellent balance between easy peelability and thermal adhesive strength can be obtained. In addition, from the viewpoint of more effectively improving the balance between easy peelability and thermal adhesive strength, the peel strength is more preferably 0.5 N / 15 mm or more and 7.0 N / 15 mm or less, and even more preferably 1.0 N / 15 mm or more and 4.0 N / 15 mm or less. The peel strength can be appropriately adjusted, for example, by selecting the type and amount of application of the thermal adhesive layer 23.

[0045] [Function] The sterilized paper 21 has excellent easy peeling properties and temperature stability by containing a specific ratio of thermoplastic resin and wax in the thermal adhesive layer 23. For example, after the sterilized paper 21 is thermally adhered to the film-like adherend 31, when the sterilized paper 21 is peeled off from the adherend 31, the thermal adhesive layer 23 is easily peeled off from the interface with the breathable substrate 22 while remaining attached to the adherend 31, and the breathable substrate 22 is not easily torn. Furthermore, since the thermal adhesive layer 23 can be visually confirmed on the adherend 31, it is easy to confirm that the adherend was uniformly attached before peeling. Furthermore, the sterilized paper 21 maintains its easy peeling properties even when stored in a high-temperature environment. For example, the breathable substrate 22 is not easily torn even after storage at 60°C or 80°C. Furthermore, the stabilization of the easy peeling properties stably suppresses fluffing and peeling of paper pieces, so that it is possible to prevent lint that has fallen off from the fluffed part and peeled paper pieces from adhering to the adherend 31 or the contents. As a result, it is possible to provide a sterile paper 21 that is less likely to fluff when peeled off and can be used in highly clean operating rooms.

[0046] Sterilization methods for the sterilized package 11 include several sterilization methods such as autoclaving, ethylene oxide gas (EOG) sterilization, and gamma ray sterilization, but EOG sterilization in particular requires gas replacement after sterilization. The sterilized paper 21 can also have excellent air permeability depending on the freeness of the pulp used to manufacture the breathable base material 22 and the basis weight of the breathable base material 22. By increasing the air permeability of the sterilized paper 21, the time required to replace the sterilization gas with air after sterilization can be shortened. This makes it possible to realize a sterilized paper 21 that is particularly suitable for EOG sterilization. As such, the sterilized paper 21 has an excellent balance between easy peelability and air permeability and is extremely useful in practice.

[0047] As described above, the sterilized paper 21 is not limited to the above embodiment. Each configuration and their combinations in the above embodiment are examples, and addition, omission, substitution, and other modifications of the configuration are possible within the scope of the present invention. For example, the sterilized paper 21 may have another layer between the breathable base material 22 and the thermal adhesive layer 23. Examples of the other layer include a water vapor barrier layer, an oxygen barrier layer, a printing layer, a printability improving layer, an overprint layer, and a light-shielding layer. The other layer located between the breathable base material 22 and the thermal adhesive layer 23 may be one layer, or two or more layers. In addition, the breathable base material 22 may have a printing layer on both sides as long as the air permeability and peel strength are within the scope of the present invention. An overprint layer may be further provided on the printing layer. EXAMPLES

[0048] An example of the above-described embodiment will be described below. <Example 1> [Production of breathable substrate 22] Hardwood bleached kraft pulp (LBKP) was beaten by a double disc refiner (DDR) to obtain a pulp slurry having a Canadian standard freeness (freeness) of 400 mL as described in JIS P 8121-2:2012. Next, an internal additive was added to the pulp slurry to obtain a papermaking raw material. The internal chemicals, in terms of the amount added on an absolute dry basis relative to the mass of pulp, were 0.5% aluminum sulfate, 0.05% alkenyl succinic acid sizing agent (Fibran 81K, National Starch) previously dispersed with cationic starch (Pillar 3YK, Pillar Starch), 0.7% amphoteric polyacrylamide resin paper strength enhancer (PAM) (product name: Polystron OFT-3, Arakawa Chemical Industries, mass average molecular weight 3 million), and 0.4% polyamine-polyamide epichlorohydrin resin wet strength enhancer (WS4024, Seiko PMC). Next, the raw paper was made into base paper on a Fourdrinier papermaking machine, and then the following paint A was applied to both sides at 29 mL / m using a size press coater attached to the papermaking machine. 2 After coating and drying, the Oken smoothness of the base paper surface, measured in accordance with JIS P 8155:2010 using an on-machine calendar attached to the papermaking machine, is adjusted to 100 seconds, and the basis weight is 60 g / m 2 and its density is 0.8g / cm 3 Thus, the breathable substrate 22 of Example 1 was obtained. [Paint A] An aqueous solution of anionic polyacrylamide resin (mass average molecular weight 200,000) (Polymerset (registered trademark) 512 manufactured by Arakawa Chemical Industries, Ltd. was diluted with water to adjust the anionic polyacrylamide resin concentration to 7 mass %).

[0049] [Production of sterilized paper] 100 parts by mass of olefin-based water-based emulsion (manufactured by Mitsui Chemicals) and 10 parts by mass of carnauba wax (manufactured by Michaelman, ML160RPH, melting point 80-85°C) were adjusted to a solid content concentration of 30%, to obtain a heat seal layer coating material. Next, a coating amount of 3.0 g / m2 after drying was applied to one side of the breathable substrate of Example 1 using a bar coater. 2The heat seal layer paint was applied and dried so as to form the thermal adhesive layer 23 of Example 1. In this way, a sterilized paper having the breathable substrate of Example 1 and the thermal adhesive layer of Example 1 was obtained.

[0050] Example 2 The sterilized paper of Example 2 was produced in the same manner as in Example 1, except that the amount of carnauba wax was changed to 5 parts by mass.

[0051] <Example 3> The sterilized paper of Example 3 was produced in the same manner as in Example 1, except that in the production of the sterilized paper of Example 1, the amount of carnauba wax was 20 parts by mass and the coating amount was 4.5 g / m2.

[0052] Comparative Example 1 The sterilized paper of Comparative Example 1 was produced in the same manner as in Example 1, except that no carnauba wax was added.

[0053] <Comparative Example 2> The sterilized paper of Comparative Example 2 was produced in the same manner as in Example 1, except that the carnauba wax was changed to paraffin wax (Digit S8, manufactured by GOO Chemical Co., Ltd., melting point 50-55°C).

[0054] <Evaluation> The following evaluations were carried out for each of the sterilized papers of Examples 1 to 3 and Comparative Examples 1 and 2. The evaluation results for each sterilized paper are shown in Table 1.

[0055] [Oken air permeability measurement] The Oken air permeability of each sterilized paper was measured according to JIS P 8117: 2009. If the Oken air permeability is 300 seconds or less, it can be said to be suitable as a sterilization packaging material.

[0056] [Adhesion to Adherend] A polyvinyl chloride film (Mitsubishi Chemical Corporation, C-1436) was used as the adherend 31. The sterilized paper 21 was placed on the film so that the thermal adhesive layer side of the sterilized paper 21 was in contact with the film, and the film was subjected to heat-pressing under heat-adhesion conditions of 150°C, 0.2 MPa, and 1.0 second using a heat press tester, thereby obtaining each heat-adhesive sample. In addition, in order to secure a portion that could be chucked by a tensile tester in the "peel strength measurement" described below, a portion where the adherend and the sterilized paper were not thermally bonded was left at the end of the heat-bonded sample.

[0057] [Measurement of peel strength, evaluation of destruction state of breathable substrate] Each sterilized package was cut to correspond to a measurement clearance of 15 mm in width and 100 mm in length to prepare a sample for measuring peel strength. The peel strength (N / 15 mm) of each sample for measuring peel strength was measured in accordance with JIS P 8113:2006. At this time, a tensile tester (model: Tensilon RTC-1250A, manufactured by Orientec Co., Ltd.) was used to chuck one end 31E of the adherend and one end of the sterilized paper, and the peel strength was measured at a peel speed of 300 mm / min by the 180-degree peel method. In addition, when the peel strength was measured, if the thermal adhesive layer or the interface between the thermal adhesive layer and the adherend did not peel off and the substrate was destroyed, it was recorded as "substrate destruction" instead of the measured value. A peel strength of 0.5 N / 15 mm or more is acceptable for practical use as a sterilization package, and a peel strength of 4.0 N / 15 mm or less is suitable for easy peeling.

[0058] [Measurement of temperature stability] The sterilized papers of Examples 1 to 3 and Comparative Examples 1 and 2 were stored under the following two conditions, and then measurements were made using the method described above in "Measurement of peel strength." (Condition 1) Store in a dryer at 80°C for one day. (Condition 2) Store in a dryer at 60°C for 7 days. If the peel strength after storage under condition 1 and the peel strength after storage under condition 2 are both maintained within the range of 0.5N to 4N / 15mm, it can be said that the quality stability in a high humidity environment is excellent.

[0059] [Table 1]

[0060] As shown in Table 1, the sterilized papers of Examples 1 to 3 maintained peel strengths in the range of 0.5 to 4.0 N / 15 mm both before and after storage in a high-temperature environment, confirming that they have excellent easy-peel properties and stability of the easy-peel properties in a high-temperature environment. On the other hand, the sterilized paper of Comparative Example 1 did not have easy-peel properties immediately after production. Moreover, the sterilized paper of Comparative Example 2 had easy-peel properties immediately after production, but lost the easy-peel properties after storage in a high-temperature environment.

[0061] As described above, according to the above embodiment, the following effects can be obtained. The sterilized paper of the present invention contains a thermoplastic resin and a wax having a melting point of 60°C or higher in the thermal adhesive layer, so that sufficient seal strength can be obtained when the sterilized paper and the adherend are heat-sealed, and when peeling, the breathable substrate and the thermal adhesive layer can be easily peeled from one side to the other with a moderate force (easy peel property). Furthermore, the easy peel property can be maintained even if the sterilized paper before heat bonding is stored in a high temperature environment and then the heat seal sheet and the adherend are heat-sealed. [Industrial Applicability]

[0062] The present invention provides an excellent sterilized paper that has good heat sealability and easy peelability, and that can maintain the easy peelability even when the heat sealable sheet is stored in a high temperature environment before thermal bonding and then the heat sealable sheet is heat sealed to an adherend.

Claims

1. A sterilized paper comprising a breathable substrate and a thermal adhesive layer on one side of the breathable substrate, the adhesive layer containing a thermoplastic resin and a wax, the wax having a melting point of 60°C or higher, and an Oken air permeability of 700 seconds or less as measured in accordance with JIS P 8121:2012.

2. 2. The sterilized paper according to claim 1, wherein the wax is contained in an amount of 1 to 20 parts by weight per 100 parts by weight of the thermoplastic resin.

3. The sterilized paper according to any one of claims 1 to 2, wherein the wax comprises one or more carnauba waxes.

4. The sterilization paper according to any one of claims 1 to 3, wherein the thermoplastic resin has a polyolefin structure in its molecule.

5. The sterilized paper according to any one of claims 1 to 4, wherein the 180° peel strength when the thermal adhesive layer and the polyvinyl chloride film are thermocompression bonded under conditions of 150°C, 0.1 MPa, and 1 second, and peeled at a peel speed of 300 mm / min in accordance with JIS P 8113:2006, is 0.5 N / 15 mm or more.

6. The sterilized paper according to any one of claims 1 to 5, wherein the breathable substrate comprises a polyacrylamide resin.

7. The sterilized paper according to any one of claims 1 to 6, which is adhered to a plastic material or a plastic material surface of a plastic-laminated paper by the thermal adhesive layer.

8. A sterilization package having at least a part thereof the sterilization paper according to any one of claims 1 to 7.

9. A sterilization package having a thermally sealed portion formed by overlapping and thermocompressing at least a portion of the thermal adhesive layer of the sterilization paper according to any one of claims 1 to 7 with at least a portion of another substrate.

10. The sterilization package according to claim 9, wherein the thermally sealed portion has a 180° peel strength of 0.5 to 15 N / 15 mm when peeled at a peel speed of 300 mm / min in accordance with JIS P 8113:2006.

Citation Information

Patent Citations

  • Heat seal sheet, manufacturing method therefor, and sterilized package

    WO2019107025A1

  • Laminate body, and package using laminate

    WO2022185932A1

  • Paper for sterilized bag

    JP1997290808A

  • Sterilized bag paper

    JP2001122348A

  • Sterilized paper

    JP2001200493A