Cu PILLAR JOINT AND MANUFACTURING METHOD THEREOF
The Cu pillar assembly with a porous Cu layer and solder layer addresses the inefficiencies of the SLID method by forming intermetallic compounds under low temperatures and short times, improving thermal reliability and efficiency.
Patent Information
- Application Number
- JP2023067191
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-17
AI Technical Summary
The SLID method for semiconductor device bonding requires long heating times and leaves behind excessive low-melting-point solder material, compromising thermal reliability and efficiency.
A Cu pillar assembly with a porous Cu layer and a solder layer, where the porous Cu layer has a porosity of 5-80%, allowing intermetallic compounds to form under low temperatures and short times, and optionally includes a diffusion prevention layer to prevent solder diffusion.
The method enables efficient formation of intermetallic compounds without excess low-melting-point solder, enhancing thermal reliability and production efficiency.
Smart Images

Figure 2024153356000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a Cu pillar joining method for joining a first Cu pillar and a second Cu pillar. [Background technology]
[0002] In recent years, the performance of semiconductor devices has improved, and the importance of micro-joining technology has increased. Flip-chip mounting is widely used as a mounting technique for IC chips, and as shown in Patent Document 1, for example, a method is provided in which a solder layer is formed on a protruding electrode and then the electrodes are joined by soldering.
[0003] In addition, in order to accommodate even narrower pitches, bonding technologies such as the TLP method (Transient Liquid Phase Diffusion Bonding) and the SLID method (Solid-Liquid Interdiffusion), which bond by diffusing solid and liquid phases into each other, have been proposed. In the SLID method, as shown in Patent Documents 1 and 2, a solder material is used as a material that forms a liquid phase. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-046148 A [Patent Document 2] Patent No. 6061276 [Patent Document 3] Patent No. 6369620 Summary of the Invention [Problem to be solved by the invention]
[0005] As described above, the SLID method uses solder material. However, if a large amount of low-melting-point solder material remains after joining, there is a risk that the heat resistance will be poor and that the thermal cycle reliability and thermal reliability will be insufficient. In order to diffuse the solder material and form an intermetallic compound, a long period of heating is required, which causes a problem of reduced production efficiency.
[0006] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a Cu pillar bonded structure in which an intermetallic compound can be sufficiently formed even under low temperature and short time conditions, and in which a large amount of solder layer does not remain, resulting in excellent thermal reliability, and a manufacturing method for the Cu pillar bonded structure. [Means for solving the problem]
[0007] In order to solve the above problems, the inventors conducted extensive research and discovered that by forming a porous Cu layer on the bonding surface of the Cu pillar, the surface area of the bonding surface of the Cu pillar is increased and the diffusion rate is increased, thereby promoting the generation of intermetallic compounds and making it possible to suppress the remaining low-melting point solder material from remaining in a large amount after bonding.
[0008] The present invention has been made based on the above-mentioned findings, and the Cu pillar bonded body of aspect 1 of the present invention is a Cu pillar bonded body in which a first Cu pillar and a second Cu pillar are bonded via a bonding layer, the bonding layer having a porous Cu layer formed on the first Cu pillar side, a solder layer formed on the second Cu pillar side, and an intermetallic compound layer formed between the porous Cu layer and the solder layer, and is characterized in that the porosity of the porous Cu layer is in the range of 5% or more and 80% or less.
[0009] According to the Cu pillar bonded body of aspect 1 of the present invention, the bonding layer formed between the first Cu pillar and the second Cu pillar has a porous Cu layer formed on the first Cu pillar side, a solder layer formed on the second Cu pillar side, and an intermetallic compound layer formed between the porous Cu layer and the solder layer, and the porosity of the porous Cu layer is within the range of 5% or more and 80% or less. Therefore, even under low temperature and short time conditions, the liquid phase of the molten solder layer and the solid phase of the porous Cu layer sufficiently interdiffuse to promote the generation of an intermetallic compound, and the low melting point solder material is prevented from remaining in a large amount, resulting in excellent thermal reliability.
[0010] A Cu pillar bonded body according to a second aspect of the present invention is characterized in that, in the Cu pillar bonding method according to the first aspect, a diffusion prevention layer is formed between the second Cu pillar and the solder layer. According to the Cu pillar bonded body of aspect 2 of the present invention, a diffusion prevention layer is formed between the second Cu pillar and the solder layer, thereby preventing the metal elements constituting the solder layer from diffusing into the second Cu pillar, and allowing sufficient interdiffusion between the liquid phase of the molten solder layer and the solid phase of the porous Cu layer, thereby ensuring reliable bonding of the first Cu pillar and the second Cu pillar.
[0011] A Cu pillar bonded body of aspect 3 of the present invention is characterized in that in the Cu pillar bonded body of aspect 1 or aspect 2, a second porous Cu layer is formed between the second Cu pillar and the solder layer. According to the Cu pillar bonded body of aspect 3 of the present invention, a second porous Cu layer is formed between the second Cu pillar and the solder layer, so that the generation of intermetallic compounds can be promoted also on the second porous Cu layer side, and the residual low-melting point solder material is further suppressed, so that a pillar bonded body with excellent thermal reliability can be produced.
[0012] A Cu pillar bonded structure according to a fourth aspect of the present invention is characterized in that in the Cu pillar bonded structure according to any one of the first to third aspects, the solder layer is made of In or an In alloy. According to the Cu pillar bonded structure of the fourth aspect of the present invention, the solder layer is made of In or an In alloy, so that bonding can be performed under low temperature conditions of 200° C. or less.
[0013] The manufacturing method of a Cu pillar bonded body of aspect 5 of the present invention is a manufacturing method of a Cu pillar bonded body in which a first Cu pillar and a second Cu pillar are bonded, and is characterized by comprising a porous Cu layer formation process of forming a porous Cu layer having a porosity in the range of 5% or more and 80% or less on the bonding surface of the first Cu pillar, a solder layer formation process of forming a solder layer on the bonding surface of the second Cu pillar, a stacking process of stacking the first Cu pillar on which the porous Cu layer is formed and the second Cu pillar on which the solder layer is formed, and a bonding process of heat-treating the stacked first Cu pillar and second Cu pillar at a temperature of 120°C or more and 200°C or less to generate an intermetallic compound between the porous Cu layer and the solder layer, and bonding the first Cu pillar and the second Cu pillar.
[0014] According to the manufacturing method of the Cu pillar joint body of aspect 5 of the present invention, a porous Cu layer having a porosity in the range of 5% or more and 80% or less is formed on the joint surface of the first Cu pillar, the first Cu pillar and the second Cu pillar are laminated via a solder material, and a heat treatment is performed at a temperature of 120°C or more and 200°C or less. Therefore, the liquid phase of the molten solder layer and the solid phase of the porous Cu layer are sufficiently interdiffused to promote the generation of an intermetallic compound, and the low-melting point solder material is prevented from remaining in a large amount, making it possible to produce a pillar joint body with excellent thermal reliability.
[0015] The manufacturing method of a Cu pillar bonded body of aspect 6 of the present invention is characterized in that, in the manufacturing method of a Cu pillar bonded body of aspect 5, it further includes a diffusion prevention layer formation step of forming a diffusion prevention layer on the bonding surface of the second Cu pillar, and in the solder layer formation step, the solder layer is formed on the diffusion prevention layer. According to the manufacturing method of the Cu pillar joint body of aspect 6 of the present invention, a diffusion prevention layer formation process is included in which a diffusion prevention layer is formed on the joint surface of the second Cu pillar. This makes it possible to suppress the diffusion of metal elements constituting the solder layer into the second Cu pillar, and allows sufficient interdiffusion between the liquid phase of the molten solder layer and the solid phase of the porous Cu layer, thereby enabling reliable joining of the first Cu pillar and the second Cu pillar.
[0016] The manufacturing method of a Cu pillar bonded body of aspect 7 of the present invention is characterized in that, in the manufacturing method of a Cu pillar bonded body of aspect 5 or aspect 6, it includes a second porous Cu layer formation step of forming a second porous Cu layer on the bonding surface of the second Cu pillar, and in the solder layer formation step, the solder layer is formed on the second porous Cu layer. According to the manufacturing method of the Cu pillar bonded body of aspect 7 of the present invention, a second porous Cu layer formation process is included in which a second porous Cu layer is formed on the bonding surface of the second Cu pillar. This makes it possible to promote the generation of an intermetallic compound even on the second porous Cu layer side formed on the bonding surface of the second Cu pillar, and thus makes it possible to fabricate a pillar bonded body with excellent thermal reliability.
[0017] The manufacturing method of a Cu pillar bonded body of aspect 8 of the present invention is characterized in that, in the manufacturing method of a Cu pillar bonded body of any one of aspects 5 to 7, the solder layer formation step forms a solder layer composed of In or an In alloy. According to the method for producing a Cu pillar bonded body of aspect 8 of the present invention, since the solder layer made of In or an In alloy is formed in the solder layer formation step, bonding can be performed under low temperature conditions of 200° C. or less. Effect of the Invention
[0018] According to the present invention, it is possible to provide a Cu pillar bonded structure in which an intermetallic compound can be sufficiently formed even under low temperature and short time conditions and a large amount of solder layer does not remain, resulting in excellent thermal reliability, and a manufacturing method for the Cu pillar bonded structure. [Brief description of the drawings]
[0019] [Figure 1] FIG. 2 is an explanatory diagram of a Cu pillar bonded body according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a flow diagram of a method for producing a Cu pillar bonded body according to one embodiment of the present invention. [Diagram 3] 1A to 1C are explanatory diagrams of a Cu pillar bonding method (a method for manufacturing a Cu pillar bonded body) according to one embodiment of the present invention. [Figure 4] FIG. 2 is an explanatory diagram of a Cu pillar bonded body according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, a Cu pillar bonded body and a method for manufacturing the Cu pillar bonded body according to embodiments of the present invention will be described with reference to the drawings.
[0021] The Cu pillar bonded body 1 according to this embodiment is, for example, a semiconductor device in which protruding electrodes (Cu pillars) formed on a semiconductor chip are bonded to each other. As shown in FIG. 1, the Cu pillar bonding body 1 in this embodiment has a structure in which a first Cu pillar 11 formed on a first wafer 10 and a second Cu pillar 21 formed on a second wafer 20 are bonded via a bonding layer 30.
[0022] The bonding layer 30 includes a porous Cu layer 31 formed on the first Cu pillar 11 side, a solder layer 32 formed on the second Cu pillar 21 side, and an intermetallic compound layer 33 formed between the porous Cu layer 31 and the solder layer 32.
[0023] The porous Cu layer 31 formed on the first Cu pillar 11 side has nano-sized pores. Here, in the porous Cu layer 31, its average porosity P ave is set to be within the range of 5% to 80%. Average porosity P aveis the average value of the porosity P calculated as follows. In this embodiment, the porosity P is calculated at three locations, and the average porosity P is taken as the average value of the porosity P. ave The following is calculated. The porosity P is calculated by determining the total area S1 of the porous Cu layer 31 and the area S2 of the pores in the porous Cu layer 31 through image analysis of the cross section of the porous Cu layer 31 using a scanning electron microscope, and then calculating the porosity P using the following formula. Porosity P(%)=(S2 / S1)×100
[0024] On the other hand, in this embodiment, a diffusion prevention layer 22 is formed between the second Cu pillar 21 and the solder layer 32 formed on the second Cu pillar 21 side.
[0025] The diffusion prevention layer 22 prevents the metal elements constituting the solder layer 23 from diffusing toward the second Cu pillar 21. In this embodiment, the diffusion prevention layer 22 is made of Ni. Here, the thickness of the diffusion prevention layer 22 is preferably within the range of 0.5 μm to 3 μm.
[0026] The solder layer 32 is made of a solder material made of a metal having a low melting temperature, and the melting temperature is preferably 200° C. or lower. In this embodiment, the solder layer 32 is made of In or an In alloy, and specifically, the solder layer 32 is an In--Sn alloy (Sn concentration is 0 mass % or more and 75 mass % or less). Furthermore, the solder material constituting the solder layer 32 is preferably a low alpha ray material that generates a small amount of alpha rays.
[0027] The intermetallic compound layer 33 formed between the solder layer 32 and the porous Cu layer 31 is formed by mutual diffusion between the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31. Here, the thickness of the bonding layer 30 (the total thickness of the porous Cu layer 31, the solder layer 32 and the intermetallic compound layer 33) is preferably within a range of 3 μm to 20 μm. Moreover, the area ratio of the intermetallic compound layer 33 in the bonding layer 30 is preferably 50% or more, more preferably 70% or more, and even more preferably 90% or more.
[0028] Next, the manufacturing method of the Cu pillar bonded body 1 of this embodiment includes a pillar forming process S01, a porous Cu layer forming process S02, a diffusion prevention layer forming process S03, a solder material disposing process S04, a stacking process S05, and a bonding process S06, as shown in FIG. 2.
[0029] <Pillar formation process S01> 3, resist layers 41, 51 are formed on one surface of the first wafer 10 and the second wafer 20. With the resist layers 41, 51 formed, Cu plating is performed to form the first Cu pillar 11 and the second Cu pillar 21. Before the first Cu pillar 11 and the second Cu pillar 21 are formed, an adhesion layer (for example, a Ti layer) and a seed layer (Cu layer) may be formed on one surface of the first wafer 10 and the second wafer 20.
[0030] <Porous Cu layer formation process S02> 3, a porous Cu layer 31 is formed on the bonding surface of the first Cu pillar 11. In this embodiment, with the resist layer 41 formed, plating is performed as follows to form the porous Cu layer forming step S02. Here, a description will be given of a method for forming the porous Cu layer 31. Methods for forming the porous Cu layer 31 include, for example, a dealloying method and a direct plating method.
[0031] (Dealloying method) In the dealloying method, copper and a metal species that is electrochemically less noble than copper are co-deposited on the bonding surface of the first Cu pillar 11 by electrolytic plating to form a copper alloy plating film, and then the less noble metal species in the copper alloy plating film is dealloyed to form a porous Cu layer 12. In this dealloying method, the precipitation ratio and precipitation form of copper and metal species less noble than copper are controlled, respectively, so that a porous Cu layer 31 having a desired porosity and shape can be formed.
[0032] The copper alloy plating is formed using a copper-zinc alloy plating solution containing, for example, copper salt, zinc salt, additives for controlling the deposition of copper and zinc, and a solvent. This copper alloy plating can be performed by electroless plating or electrolytic plating. Metal species that are electrochemically less noble than copper (e.g., Fe, Mn, etc.) can also be selected as alloy species.
[0033] In copper-zinc alloy plating, the metal salt may be copper sulfate, zinc sulfate, zinc pyrophosphate, zinc phosphate, or the like. The copper ions and zinc ions in the copper-zinc alloy plating solution are each preferably 0.001 to 1.0 moles, and the molar ratio of copper ions to zinc ions is preferably within the range of Cu:Zn=1:1 to 1:1000. The zinc ion concentration is made higher than the copper ion concentration because copper is preferentially deposited compared to zinc due to the difference in standard oxidation-reduction potential.
[0034] Furthermore, citric acid and pyrophosphoric acid may be added as supporting salts (complexing agents). Examples of the gloss agent include surfactants such as alkanolamines, glycine, serine, alanine, tyrosine, aspartic acid, glutamic acid, histidine, and salts thereof. The pH of the plating solution should be 2.5 or higher to adjust the balance of copper and zinc deposition. The cathode current density should be 0.3 A / dm 2 More than 0.8A / dm 2 Set within the following range.
[0035] After the copper-zinc alloy plating film is formed, the resist layer 41 is removed using a resist stripper, and then a dealloying process is carried out. Examples of dealloying treatment of the formed copper-zinc alloy plating film include an etching reaction using a chemical solution and a method of electrochemically progressing an anode reaction. In this embodiment, dealloying is performed using an acid, and the copper alloy film is immersed in and stirred in a solution containing hydrochloric acid with a concentration of 0.002 mol / L to 0.5 mol / L at a temperature of 20°C to 35°C for 30 minutes or more (depending on the thickness of the plating film) to remove zinc from the copper-zinc alloy plating film. This forms a porous Cu layer 31 on the bonding surface of the first Cu pillar 11.
[0036] Next, the formed porous Cu layer 31 is washed with a washing solvent such as ethanol, water, or acetone, and dried in the atmosphere using dry air. In order to prevent surface oxidation, it is preferable to immerse the plate in a rust inhibitor containing benzotriazole and a surfactant as main components for a predetermined period of time.
[0037] (Direct plating method) In the direct plating method, a Cu plating solution containing an azole-based additive, which is a copper ion electrodeposition inhibitor, is used to perform electrolytic plating on the bonding surface of the first Cu pillar 11 to form a porous Cu layer 31 having a porous structure. After the porous Cu layer 31 is formed, the resist layer 41 is removed using a resist stripper. In this direct plating method, it is possible to form a porous Cu layer 31 having a desired porosity and shape by controlling the type and content of additives contained in the Cu plating solution and the plating conditions.
[0038] The Cu plating solution used is an acidic electrolytic copper plating solution containing a soluble copper salt, an azole compound having 2 to 3 nitrogen atoms in a five-membered ring as a copper ion electrodeposition inhibitor, an acid, and water. If necessary, a brightener, a surfactant, an antioxidant, etc. can also be added. The Cu plating solution used has a copper concentration of 0.1 mol / L or more, an azole compound concentration of 10 mmol / L or more and 50 mmol / L or less, and a chlorine chloride ion concentration of 10 ppm or less.
[0039] Specific examples of soluble copper salts include copper sulfate, copper oxide, copper carbonate, copper alkanesulfonates such as copper methanesulfonate and copper propanoate, copper alkanolsulfonates such as copper isethionate and copper propanolsulfonate, and copper organic acids such as copper acetate, copper citrate, and copper tartrate. These can be used alone or in combination of two or more.
[0040] Further, the acid may be an organic acid or an inorganic acid. Examples of the acid include sulfuric acid; alkanesulfonic acids such as methanesulfonic acid and propanesulfonic acid; alkanolsulfonic acids such as isethionic acid and propanolsulfonic acid; and organic acids such as citric acid and tartaric acid. These may be used alone or in combination of two or more. The water may be pure water such as ion-exchanged water and distilled water.
[0041] The plating conditions are, for example, a DC power source and a current density of 0.1 A / dm 2 ~5A / dm 2 Approximately, preferably 0.4A / dm 2 ~1.0A / dm 2 Then, a plating time is selected that allows the desired porous Cu layer 12 to be formed. When Cu plating is performed under the above conditions, the azole compound, which is a copper ion electrodeposition inhibitor, as well as the copper ions are adsorbed on the cathode surface, which is the bonding surface of the first Cu pillar 11. The presence of the azole compound strongly inhibits the electrodeposition of copper ions, giving priority to copper nucleation, and a porous Cu layer 31 is formed on the cathode surface as a copper plating film.
[0042] <Diffusion prevention layer forming process S03> The diffusion prevention layer 22 is formed on the bonding surface of the second Cu pillar 21. In this embodiment, with the resist layer 51 formed, Ni plating is performed to form the diffusion prevention layer 22 made of Ni.
[0043] <Solder layer formation process S04> Next, a solder material is disposed so as to be laminated on the diffusion prevention layer 22 formed on the bonding surface of the second Cu pillar 21, thereby forming the solder layer 32. In this embodiment, the solder material is plated in a state in which the resist layer 51 is formed, thereby forming the solder layer 32. After the solder layer 32 is formed, the resist layer 51 is removed using a resist remover. Here, the thickness of the solder layer 32 is preferably within the range of 1 μm to 10 μm. The solder material is made of In or an In alloy. Specifically, the solder layer 32 is made of an In--Sn alloy (Sn concentration is 0 mass % or more and 75 mass % or less). The solder material constituting the solder layer 32 is preferably a low alpha ray material that generates a small amount of alpha rays.
[0044] <Lamination process S05> Next, as shown in FIG. 3, a first Cu pillar 11 having a porous Cu layer 31 formed on its joining surface and a second Cu pillar 21 having a diffusion barrier layer 22 and a solder layer 32 formed on its joining surface are laminated.
[0045] <Joining process S06> 3, the stacked first Cu pillar 11 and second Cu pillar 21 are heated while being pressurized in the stacking direction to bond the first Cu pillar 11 and the second Cu pillar 21. In this way, a pillar bonded body 1 in which the first Cu pillar 11 and the second Cu pillar 21 are bonded is manufactured.
[0046] In this embodiment, the first Cu pillar 11 and the second Cu pillar 21 are joined by the SLID method in which the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31 diffuse into each other to form a bond. That is, the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31 diffuse into each other, forming an intermetallic compound layer 33, and the first Cu pillar 11 and the second Cu pillar 21 are joined together.
[0047] In this embodiment, the pressure load in the joining step S06 is preferably within a range of 0.1 MPa to 20 MPa. In this embodiment, the bonding temperature in the bonding step S06 is preferably within the range of 120° C. or higher and 200° C. or lower. Furthermore, in this embodiment, the holding time at the bonding temperature in the bonding step S06 is preferably within a range of 10 seconds to 3 minutes.
[0048] According to the Cu pillar bonded body 1 of this embodiment configured as described above, the bonding layer 30 formed between the first Cu pillar 11 and the second Cu pillar 21 has a porous Cu layer 31 formed on the first Cu pillar 11 side, a solder layer 32 formed on the second Cu pillar 21 side, and an intermetallic compound layer 33 formed between the porous Cu layer 31 and the solder layer 32. The porosity of the porous Cu layer 31 is within the range of 5% or more and 80% or less. Therefore, even under low temperature and short time conditions, the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31 sufficiently interdiffuse with each other to promote the generation of an intermetallic compound, thereby preventing a large amount of low-melting point solder material from remaining, and providing excellent thermal reliability.
[0049] In the Cu pillar joint body 1 of this embodiment, when a diffusion prevention layer 22 is formed on the joint surface of the second Cu pillar 21, the metal elements constituting the solder layer 13 can be suppressed from diffusing toward the second Cu pillar 21, and the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31 can be sufficiently interdiffused to promote the generation of an intermetallic compound, thereby ensuring reliable joining of the first Cu pillar 11 and the second Cu pillar 12.
[0050] In the Cu pillar bonding body 1 of this embodiment, when the solder layer 32 is composed of In or an In alloy, a liquid phase can be generated even at low temperature conditions of 200°C or less, and the first Cu pillar 11 and the second Cu pillar 12 can be reliably bonded by the SLID method.
[0051] According to the manufacturing method of the Cu pillar joint body 1 of this embodiment, a porous Cu layer 31 having a porosity in the range of 5% or more and 80% or less is formed on the joint surface of the first Cu pillar 11, the first Cu pillar 11 and the second Cu pillar 12 are laminated via the solder layer 32, and a heat treatment is performed at a temperature of 120°C or more and 200°C or less. Therefore, the liquid phase of the molten solder layer 32 and the solid phase of the porous Cu layer 31 are sufficiently interdiffused to promote the generation of an intermetallic compound, and a large amount of low-melting point solder material is prevented from remaining, making it possible to produce a pillar joint body 1 with excellent thermal reliability.
[0052] In the manufacturing method of the Cu pillar joint body 1 of this embodiment, when a diffusion prevention layer formation process S03 for forming a diffusion prevention layer 22 on the joint surface of the second Cu pillar 21 is included, the metal elements constituting the solder layer 32 can be prevented from diffusing into the second Cu pillar 21, and the first Cu pillar 11 and the second Cu pillar 21 can be reliably joined.
[0053] In addition, in this embodiment, when a low alpha ray material that generates a small amount of alpha rays is used as the solder material constituting the solder layer 32, the occurrence of soft errors in a semiconductor device including the pillar bonding body 1 of this embodiment can be suppressed, and a semiconductor device that can be used stably can be configured.
[0054] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. For example, in the present embodiment, the diffusion prevention layer 22 made of Ni is formed, but the present invention is not limited to this, and the diffusion prevention layer may not be formed.
[0055] In addition, in the present embodiment, the porous Cu layer is formed on the first Cu pillar side, but the present invention is not limited to this. As in the pillar bonded body 101 shown in FIG. 4, the second porous Cu layer 34 may be formed on the second Cu pillar 21 side, and the solder layer 31 may be formed so as to contact the second porous Cu layer 34. In this case, the second intermetallic compound layer 35 is formed between the solder layer 31 and the porous Cu layer 34. EXAMPLES
[0056] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.
[0057] First, a silicon wafer (thickness: 0.8 mm) with a seed layer formed on the wafer surface was used. The seed layer was formed by sputtering a titanium layer (thickness: 100 nm) on the wafer surface and a copper layer (thickness: 500 nm) on the titanium layer. The surface of this Si wafer was patterned with photoresist to have a 75 μm diameter bump pattern (total number of bumps: 625), forming a resist layer with openings on the seed layer.
[0058] In Inventive Examples 1 to 12, the above-mentioned wafer was used as the first wafer, and a first Cu pillar and a porous Cu layer were formed on one surface of this first wafer. Note that in Comparative Example 1, no porous Cu layer was formed.
[0059] In Inventive Examples 1 to 6 and Comparative Example 2, the porous Cu layer was formed by a dealloying method. Copper-zinc alloy electroplating was carried out using a copper-zinc alloy electroplating solution. Table 1 shows the plating conditions for the dealloying method of invention examples 1 to 7. After forming the copper-zinc alloy plating layer, the resist layer was dissolved and removed using a resist stripper for dry films. Next, the seed layer was removed from the portion where the copper-zinc alloy plating layer was not formed using an etching solution. Next, the copper-zinc alloy plating layer was immersed in a solution containing hydrochloric acid with a concentration of 1.00 mol / L at 27°C, and the solution was stirred for 70 minutes to remove zinc from the copper-zinc alloy plating layer and dealloy it.
[0060] [Table 1]
[0061] In Inventive Examples 7 to 12 and Comparative Example 3, the porous Cu layer was formed by a direct plating method. Copper plating was carried out using a copper plating bath. Table 2 shows the plating conditions for the direct plating method in Inventive Examples 7 to 12 and Comparative Example 3. In the direct plating method, after performing porous copper plating, the resist layer was dissolved and removed using a resist stripper for dry films, and the seed layer was etched.
[0062] [Table 2]
[0063] The above-mentioned wafer was used as a second wafer, and a second Cu pillar, a diffusion prevention layer made of Ni, and a solder layer were formed on one surface of the second wafer by plating. The thicknesses of each were as shown in Table 3.
[0064] Then, the first Cu pillar and the second Cu pillar shown in Table 3 were stacked and aligned using a Treky high-precision flip chip bonder T-300-PRO. After that, the first Cu pillar and the second Cu pillar were pressed at a pressure of 0.1 MPa in a nitrogen atmosphere and heat-treated at the bonding temperature shown in Table 3 for 1 minute to bond the first Cu pillar and the second Cu pillar to obtain a pillar bonded body.
[0065] Here, the average porosity Pave was calculated as follows: The cross section of the porous Cu layer was subjected to image analysis using a scanning electron microscope to determine the total area S1 of the porous Cu layer and the area S2 of the pores in the porous Cu layer, and the porosity P was calculated using the following formula. Porosity P(%)=(S2 / S1)×100 Then, the porosity P was calculated at three locations, and the average porosity P was calculated as the average porosity P ave The evaluation results are shown in Table 3.
[0066] In addition, the cross-section of the joint of the pillar joint was observed to evaluate the formation of metal compounds (IMC) at the joint. The cross section of the joint layer of the pillar joint was processed by CP to obtain SEM images and EDS maps of Cu and solder metals (In, Sn). The overlapping areas of the solder metals (In, Sn) and Cu EDS maps were determined to be intermetallic compounds. The area ratio of the metal compounds in the joint (IMC ratio) was calculated using the following formula. IMC rate (%) = (EDS overlap area of solder material (In, Sn) and Cu) / (EDS area of solder material (In, Sn)) x 100
[0067] The above-mentioned IMC ratio (%) of 90% or more was evaluated as "good", the IMC ratio (%) of 50% to less than 90% was evaluated as "passable", and the IMC ratio (%) of less than 50% was evaluated as "unacceptable". The evaluation results are shown in Table 3.
[0068] [Table 3]
[0069] In Comparative Example 1 in which no porous Cu layer was formed, under conditions of 200° C. and 1 minute, intermetallic compounds were not sufficiently generated, and a large amount of the low-melting-point solder layer remained. In Comparative Example 2, in which the porosity of the porous Cu layer was 85%, intermetallic compounds were not sufficiently generated under conditions of 150° C. and 1 minute, and a large amount of the low-melting-point solder layer remained. In Comparative Example 3, in which the porosity of the porous Cu layer was 3%, intermetallic compounds were not sufficiently generated under conditions of 200° C. and 1 minute, and a large amount of the low-melting-point solder layer remained.
[0070] In contrast, in Examples 1 to 12 of the present invention, in which a porous Cu layer with a porosity in the range of 5% or more and 80% or less was formed, intermetallic compounds were sufficiently generated, and the residue of the low-melting point solder layer was suppressed.
[0071] From the results of the above confirmatory experiments, it was confirmed that according to the present invention, it is possible to provide a Cu pillar bonded structure that can sufficiently form an intermetallic compound even under low temperature and short time conditions and has excellent thermal reliability without leaving a large amount of solder layer, and a manufacturing method for the Cu pillar bonded structure. [Explanation of symbols]
[0072] 1,101 Cu pillar joint 11 First Cu pillar 21 Second Cu pillar 30 Bonding layer 31 Porous Cu layer 32 Solder layer 33 Intermetallic compound layer
Claims
1. A Cu pillar bonded body in which a first Cu pillar and a second Cu pillar are bonded via a bonding layer, The bonding layer has a porous Cu layer formed on the first Cu pillar side, a solder layer formed on the second Cu pillar side, and an intermetallic compound layer formed between the porous Cu layer and the solder layer, A Cu pillar bonded body, characterized in that the porosity of the porous Cu layer is within the range of 5% or more and 80% or less.
2. The Cu pillar bonded body according to claim 1 , further comprising a diffusion barrier layer formed between the second Cu pillar and the solder layer.
3. The Cu pillar bonded body according to claim 1 , further comprising a second porous Cu layer formed between the second Cu pillar and the solder layer.
4. 2. The Cu pillar bonded structure according to claim 1, wherein the solder layer is made of In or an In alloy.
5. A method for manufacturing a Cu pillar bonded body in which a first Cu pillar and a second Cu pillar are bonded, comprising the steps of: A porous Cu layer forming step of forming a porous Cu layer having a porosity in the range of 5% to 80% on a bonding surface of the first Cu pillar; a solder layer forming step of forming a solder layer on a bonding surface of the second Cu pillar; a lamination step of laminating the first Cu pillar on which the porous Cu layer is formed and the second Cu pillar on which the solder layer is formed; a bonding process in which the stacked first Cu pillar and the second Cu pillar are heat-treated at a temperature of 120° C. or more and 200° C. or less to generate an intermetallic compound between the porous Cu layer and the solder layer, thereby bonding the first Cu pillar and the second Cu pillar; A method for manufacturing a Cu pillar bonded body, comprising the steps of:
6. 6. The method for manufacturing a Cu pillar joint body according to claim 5, further comprising a diffusion prevention layer forming step of forming a diffusion prevention layer on the joint surface of the second Cu pillar, and in the solder layer forming step, the solder layer is formed on the diffusion prevention layer.
7. The method for manufacturing a Cu pillar joint body described in claim 5, characterized in that it includes a second porous Cu layer formation process for forming a second porous Cu layer on the joint surface of the second Cu pillar, and in the solder layer formation process, the solder layer is formed on the second porous Cu layer.
8. 6. The method for manufacturing a Cu pillar bonded structure according to claim 5, wherein the solder layer forming step forms a solder layer made of In or an In alloy.
Citation Information
Patent Citations
Metal pillar with cushioned tip
US20170278815A1
Metallic Interconnect, a Method of Manufacturing a Metallic Interconnect, a Semiconductor Arrangement and a Method of Manufacturing a Semiconductor Arrangement
US20190103378A1
Substrate joining method
WO2015079582A1
Conductive pillar and method for manufacturing same, and method for manufacturing bonded structure
WO2021145129A1
printer